FOAMED PET COMPOSITE BOARD AND MANUFACTURING METHOD THEREOF

DE602022006790T2Active Publication Date: 2024-10-16ZHEJIANG TIANZHEN BAMBOO & WOOD DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602022006790
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2022-05-17
Publication Date
2024-10-16
Estimated Expiration
2042-05-17
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to the technical field of boards, and in particular to a foamed PET composite board and a preparation method thereof.BACKGROUND ART

[0002] Polyethylene terephthalate (PET) has a chemical formula of (C 10 H 8 O 4 ) n and is prepared by the transesterification of dimethyl terephthalate with ethylene glycol or by the esterification of terephthalic acid with ethylene glycol to synthesize dihydroxyethyl terephthalate, followed by polycondensation. PET is crystalline saturated polyester. It is a milk-white or light yellow, highly crystalline polymer with a smooth and glossy surface, and is a quite common resin in life. PET has excellent physical and mechanical properties in a wide temperature range. Its long-term service temperature may be up to 120°C. PET has excellent electrical insulation and still good electrical properties even at high temperatures and high frequencies with relatively poor corona resistance. PET also shows desirable creep resistance, fatigue resistance, abrasion resistance and dimensional stability.

[0003] PET is mainly used in electronic appliances, such as electrical socket, electronic connector, rice cooker handle, TV deflection yoke, terminal block, interrupter casing, switch, motor fan casing, instrument mechanical parts, currency count machine parts, electric iron and fittings for electromagnetic stove; in automobile industry, such as flow control valve, carburetor cover, car window controller, pedal transmission and distribution board cover; in machinery industry, such as gear, vane, belt pulley and pump parts as well as body and wheels of wheelchair, lamp housing, illuminator housing, drainage fitting, zipper, clock parts and sprayer parts. PET may be spun into polyester fibers, namely terylene. PET may be made into thin films to be used in substrates of tape, video and filmstrip, insulating films and product packaging. As plastic, PET may be blown into various bottles, such as coke bottle and mineral water bottle. PET may also be used as electronic appliance parts, bearings, gears and the like.

[0004] In the prior art, the extensive use of PET leads to a waste of PET, failing to realize the resource utilization of PET.

[0005] WO2020118986A1 discloses a thermoplastic polyester extrusion foam molding method, comprising melting a thermoplastic polyester, a lubricant and a foaming aid in a twin-screw extruder, the exit pressure of the twin-screw extruder being 3 MPa to 10 MPa; supplying extruder, the inlet pressure of the single screw extruder being 15 MPa to 25 MPa; and lowering the temperature of the thermoplastic polyester melt comprising the phy sical foaming agent by means of the single screw extruder, subjecting the thermoplastic polyester melt to extrusion foaming through a die, and cooling and forming the extrudate to obtain a thermoplastic ester foamed product.

[0006] US5391582 discloses that blends of branched polyethylene terephthalate) ("PET") polymer and recycled plastics can be foamed to produce closed cell structures with advantageous densities, cell sizes, cell size distributions, mechanical properties and thermal properties.SUMMARY

[0007] In view of this, an objective of the present disclosure is to provide a foamed PET composite board and a preparation method thereof. In the present disclosure, recycled PET is used to prepare a board, which realizes the resource utilization of PET.

[0008] To achieve the above objective, the present disclosure provides the following technical solutions: The present disclosure provides a foamed PET composite board, prepared from a raw material including the following components in parts by mass: 100 parts of PET, 10-20 parts of a regulator, 100-200 parts of an inorganic filler, 1-2 parts of a blowing agent, and 1-4 parts of PE wax, wherein the PET is recycled PET; wherein the inorganic filler is calcium carbonate and talc powder, a mass ratio of calcium carbonate to talc powder is in a range of (1-9):(9-1); the blowing agent is azodicarbonamide (AC) blowing agent; and the regulator is a compound acrylic ester copolymer (ACR) foaming regulator.

[0009] In some embodiments, the foamed PET composite board is prepared from a raw material including the following components in parts by mass: 100 parts of the PET, 14-16 parts of the regulator, 140-160 parts of the inorganic filler, 1-2 parts of the blowing agent, and 2-3 parts of the PE wax.

[0010] In some embodiments, the foamed PET composite board is prepared from a raw material including the following components in parts by mass: 100 parts of the PET, 15 parts of the regulator, 150 parts of the inorganic filler, 2 parts of the blowing agent, and 3 parts of the PE wax.

[0011] The present disclosure further provides a preparation method of the foamed PET composite board according to the above technical solutions, including: mixing the PET, the regulator, the inorganic filler, the blowing agent and the PE wax, and then subjecting to melt extrusion, plastic fixing and calendaring molding in sequence to obtain the foamed PET composite board.

[0012] In some embodiments, the melt extrusion is conducted at a temperature in a range of 200-260 °C.

[0013] The present disclosure provides a foamed PET composite board, prepared from a raw material including the following components in parts by mass: 100 parts of PET, 10-20 parts of a regulator, 100-200 parts of an inorganic filler, 1-2 parts of a blowing agent, and 1-4 parts of PE wax (polyethylene wax), wherein the PET is recycled PET, the components being as defined in claim 1.

[0014] In the present disclosure, recycled PET is used to realize the resource utilization of PET, solving the problem of PET waste present in the art.

[0015] In the present disclosure, the foamed PET composite board with properties of high strength, sound insulation and thermal insulation, and without pollution is obtained by accurately limiting the amounts of the PET, the regulator, the inorganic filler, the blowing agent and the PE wax.

[0016] The present disclosure further provides a preparation method of the foamed PET composite board according to the above technical solutions. The preparation method is simple and fast, with fewer steps, and is beneficial to realize industrial production.BRIEF DESCRIPTION OF THE DRAWINGS

[0017] FIG. 1 is a physical photo of the foamed PET composite board prepared according to Example 1. FIG. 2 is a physical photo of the foamed PET composite board prepared according to Example 2. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0018] The present disclosure provides a foamed PET composite board, which is prepared from a raw material including the following components in parts by mass: 100 parts of PET, 10-20 parts of a regulator, 100-200 parts of an inorganic filler, 1-2 parts of a blowing agent, and 1-4 parts of PE wax, wherein the PET is recycled PET.

[0019] In the present disclosure, unless otherwise specified, all the raw materials used are commercially available products in the art.

[0020] In the present disclosure, the PET may preferably be recycled PET, and more preferably PET recycled from PET bottle chips.

[0021] In the present disclosure, in some embodiments, the recycling process of the PET bottle chips may include: separating a body of a PET bottle from a cap and a label, and then crushing, cleaning and drying successively.

[0022] In some specific embodiments, the steps are performed as follows: step 1, picking and sorting various PET bottle chips and tearing off labels on the outside, most of which are OPP (o-phenylphenol) and some are PVC (polyvinyl chloride) shrink films and have to be stripped away firstly; step 2, conducting a crushing process, during which rinsing is carried out with water to remove dirt from the various PET bottle chips; step 3, placing obtained chips in a steam treatment device and adding sodium hydroxide (caustic soda flakes) to remove greases and other stubborn impurities; step 4, washing with clean water, spin-drying to remove the remaining water and bagging, and then drying in a vacuum oven; and step 5, smashing into pieces.

[0023] Based on the parts by mass of the PET, the foamed PET composite board includes 1-2 parts of the blowing agent, and more preferably 2 parts

[0024] In the present disclosure, the blowing agent is azodicarbonamide AC blowing agent.

[0025] Based on the parts by mass of the PET, the foamed PET composite board may preferably include 14-16 parts of the regulator, and more preferably 15 parts.

[0026] In the present disclosure, the regulator is a compound acrylic ester copolymer ACR foaming regulator that has an effect of increasing solution strength.

[0027] Based on the parts by mass of the PET, the foamed PET composite board may preferably include 140-160 parts of the inorganic filler, and more preferably 150 parts.

[0028] In the present disclosure, the inorganic filler is calcium carbonate and talc powder.

[0029] In the present disclosure, a mass ratio of calcium carbonate to talc powder is in a range of (1-9): (9-1), and more preferably 1:1.

[0030] In the present disclosure, in some embodiments, the inorganic filler may have a particle size of 37-74 µm (200-400 mesh) Based on the parts by mass of the PET, the foamed PET composite board may preferably include 2-3 parts of PE wax, and more preferably 3 parts.

[0031] In some specific embodiments, the foamed PET composite board may be prepared from a raw material including the following components in parts by mass: 100 parts of the PET, 15 parts of the regulator, 150 parts of the inorganic filler, 2 parts of the blowing agent, and 3 parts of the PE wax.

[0032] The present disclosure further provides a method for preparing the foamed PET composite board according to the above technical solutions, including the following steps: mixing PET, the regulator, the inorganic filler, the blowing agent and PE wax, and subjecting to melt extrusion, plastic fixing and calendaring molding in sequence to obtain the foamed PET composite board.

[0033] In the present disclosure, the melt extrusion may preferably be conducted at a temperature in a range of 200-260°C, and more preferably 240°C.

[0034] There are no special limits to the specific processes of the plastic fixing and calendaring molding in the present disclosure, and the processes well known to those skilled in the art may be used.

[0035] To further describe the present disclosure, hereinafter, the foamed PET composite board and the preparation method thereof provided in the present disclosure will be described in detail with reference to examples, which should not be construed as limiting the protection scope of the present disclosure.

[0036] Raw materials for preparing the foamed PET composite boards according to Examples 1 to 5 are shown in Table 1. Table 1 Raw materials for preparing foamed PET composite boards according to Examples 1 to 5 (part by mass)Recycled PETRegulatorCalcium carbonateTalc powderAC blowing agentPE waxExample 110010406011Example 210014707022Example 310015757523Example 410016907013Example 510010505024

[0037] A preparation method of the foamed PET composite boards according to Examples 1 to 5 was performed as follows:

[0038] Recycling PET from PET bottle chips: step 1, various PET bottle chips were picked and sorted, and labels on the outside were torn off, wherein most of the labels were OPP and some were PVC shrink films that had to be stripped away firstly; step 2, a crushing process was conducted, during which rinsing was performed with water to remove dirt from the various PET bottle chips obtained from step 1; step 3, the chips obtained from step 2 were placed in a steam treatment device, and sodium hydroxide (caustic soda flakes) was added to remove greases and other stubborn impurities; step 4, the chips obtained from step 3 were washed with clean water, spin-dried to remove the remaining water and bagged, and then were dried in a vacuum oven; and step 5, the chips obtained from step 4 were smashed into pieces.

[0039] The recycled PET, the regulator, the inorganic filler, the blowing agent and PE wax were mixed, and then subjected to melt extrusion (conducted at 240°C), plastic fixing and calendaring molding successively, obtaining a foamed PET composite board.

[0040] FIG. 1 is a physical photo of the foamed PET composite board prepared according to Example 1; FIG. 2 is a physical photo of the foamed PET composite board prepared according to Example 2.

[0041] The foaming ratios of the raw materials of Examples 1 to 5 during the melt extrusion were 0.8-, 0.86-, 1.0-, 0.9-, and 0.94-times, respectively.

[0042] The hardness, static load, bending strength and noise reduction coefficient were tested for the foamed PET composites prepared according to Examples 1 to 5. Herein, the noise reduction coefficient refers to GBJ47-1983. Results are shown in Table 2. Table 2 The performance testing results of the foamed PET composites prepared according to Examples 1 to 5Hardness / DStatic load / mmBending strength / MPaNoise reduction coefficientExample 1530.151850.96Example 2470.161670.93Example 3450.181580.89Example 4510.142030.95Example 5430.191690.94

Claims

1. A foamed PET composite board, prepared from a raw material including the following components in parts by mass: 100 parts of PET, 10-20 parts of a regulator, 100-200 parts of an inorganic filler, 1-2 parts of a blowing agent, and 1-4 parts of PE wax, wherein the PET is recycled PET; wherein the inorganic filler is calcium carbonate and talc powder, a mass ratio of calcium carbonate to talc powder is in a range of (1-9):(9-1); the blowing agent is azodicarbonamide (AC) blowing agent; and the regulator is a compound acrylic ester copolymer (ACR) foaming regulator.

2. The foamed PET composite board according to claim 1, wherein the foamed PET composite board is prepared from a raw material including the following components in parts by mass: 100 parts of the PET, 14-16 parts of the regulator, 140-160 parts of the inorganic filler, 1-2 parts of the blowing agent, and 2-3 parts of the PE wax.

3. The foamed PET composite board according to claim 1 or 2, wherein the foamed PET composite board is prepared from a raw material including the following components in parts by mass: 100 parts of the PET, 15 parts of the regulator, 150 parts of the inorganic filler, 2 parts of the blowing agent, and 3 parts of the PE wax.

4. A method for preparing the foamed PET composite board according to any one of claims 1 to 3, including: mixing the PET, the regulator, the inorganic filler, the blowing agent and the PE wax, and then subjecting to melt extrusion, plastic fixing and calendaring molding in sequence to obtain the foamed PET composite board.

5. The method according to claim 4, wherein the melt extrusion is conducted at a temperature in a range of 200-260°C.