Metal powder for a powder bed additive manufacturing process
A nickel-based alloy powder with tailored composition and particle size, combined with laser fusion and heat treatments, addresses the limitations of existing powders by producing a high-temperature-resistant material for turbomachines.
Patent Information
- Application Number
- FR2021013048
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-12-07
AI Technical Summary
Existing metal powders for additive manufacturing processes do not produce materials suitable for turbomachines due to insufficient resistance to temperatures above 650°C, lacking tensile strength, and susceptibility to oxidation and corrosion.
A nickel-based alloy powder with specific elemental composition and particle size distribution, combined with a laser fusion process and heat treatments, to produce a material resistant to temperatures up to 850°C or 1000°C, maintaining tensile strength and weldability.
The process yields a material with enhanced mechanical properties, including resistance to high temperatures, oxidation, and corrosion, suitable for turbomachine parts, with minimal porosity and improved structural integrity.
Smart Images

Figure 00000012_0000
Abstract
Description
Title of the invention: Metal powder for a powder bed additive manufacturing process FIELD OF THE INVENTION
[0001] The present invention relates to the field of additive manufacturing and more particularly to alloys for implementing an additive manufacturing process on a powder bed. STATE OF THE ART
[0002] Many alloys are known for the implementation of powder bed additive manufacturing (PBM) processes. It is specified that by alloy for the implementation of a powder bed additive manufacturing process, it is understood a powder comprising a metal alloy. The powder being intended to be melted then solidified during the implementation of a powder bed additive manufacturing process, to form a part.
[0003] Currently, many powders exist. However, most existing powders do not allow obtaining - after fusion by a laser beam - a material suitable for use in a turbomachine. In particular, many powders do not allow obtaining a material resistant to a temperature of more than 650°C. However, a maximum resistance temperature of 650°C is much too low for use in a turbomachine.
[0004] In this context, it is necessary to provide a powder comprising a metal alloy for a powder bed additive manufacturing process, which makes it possible to obtain a material retaining its characteristics of tensile strength, fining and resistance to oxidation and corrosion, at least up to a temperature of 850°C, or even 1000°C, and which is weldable. Statement of the invention
[0005] According to a first aspect, the invention provides a metal powder for an additive manufacturing process, the metal powder comprising a nickel-based alloy comprising between 0.02% and 0.04% carbon, between 18% and 22% chromium, between 11% and 13% cobalt, between 5% and 5.5% niobium, between 3% and 3.5% tantalum, between 3% and 3.4% molybdenum, between 0.9% and 1.1% titanium, between 0.4% and 0.6% aluminum, between 0.003% and 0.005% boron, at most 0.5% iron, at most 0.1% copper, at most 0.1% silicon, at most 0.05% manganese, at most 0.01% phosphorus, at most 0.01% zirconium, at most 0.004% magnesium, maximum 0.003% sulfur, maximum 0.025% oxygen, maximum 0.018% nitrogen and maximum 0.003% hydrogen.
[0006] According to other advantageous and non-limiting characteristics:
[0007] The metal powder comprises a plurality of grains having a particle size distribution in which at least 10% of the grains have a diameter of between 8 pm and 28 pm.
[0008] The metal powder comprises a plurality of grains having a particle size distribution in which at least 50% of the grains have a diameter of between 10 μm and 45 μm.
[0009] The metal powder comprises a plurality of grains having a particle size distribution in which at least 90% of the grains have a diameter of between 25 pm and 75 pm.
[0010] According to a second aspect, the invention proposes a method of additive manufacturing on a powder bed by laser fusion of a powder according to the first aspect, the method making it possible to manufacture a part in a material obtained by laser fusion of said powder.
[0011] According to other advantageous and non-limiting characteristics:
[0012] The laser emits a beam with a power of between 150W and 350W.
[0013] The laser is moved at a speed between 900mm / s and 2500mm / s.
[0014] The laser emits a beam having a diameter between 50pm and 200pm.
[0015] The laser fuses the powder in bands, each band having a width of between 2mm and 15mm.
[0016] Each merged band overlaps at least one other band, over a width of between 0.05mm and 0.15mm.
[0017] The laser fuses layers of powder, each layer of fused powder has a thickness between 20pm and 60pm.
[0018] The method comprises a step of improving the structure of the material obtained by laser melting of said powder, the step of improving the structure of the material comprising at least the following phases: (b) first heat treatment at a temperature between 1155°C and 1175°C, for approximately 3 to 5 hours, followed by cooling to 595°C in less than 23 minutes; (c) second heat treatment, comprising: - maintaining at a temperature between 890°C and 910°C for approximately 4 hours, followed by cooling to 775°C at a rate of at least 55°C per hour; - maintaining at a temperature between 765°C and 785°C for approximately 4 hours, followed by cooling to 705°C at a rate of at least 55°C per hour; - maintaining at a temperature between 695°C and 715°C, for approximately 8 hours.
[0019] The step of improving the structure of the material further comprises a preliminary phase (a) of stress relief at a temperature between 945°C and 965°C, for approximately 2 hours.
[0020] The step of improving the structure of the material further comprises the following phases: (d) third heat treatment at a temperature between 945°C and 965°C, for approximately 1 hour, followed by cooling to 650°C in less than 23 minutes; (e) fourth heat treatment, comprising: - maintaining at a temperature between 750°C and 770°C for approximately 5 hours, followed by cooling to 700°C at a rate of at least 55°C per hour; - maintaining at a temperature between 690°C and 710°C, for approximately 8 hours; - maintaining at a temperature between 640°C and 660°C, for approximately 1 hour.
[0021] According to a third aspect, the invention provides a material obtained according to the method according to the second aspect, comprising a nickel-based alloy comprising between 0.02% and 0.04% of carbon, between 18% and 22% of chromium, between 11% and 13% of cobalt, between 5% and 5.5% of niobium, between 3% and 3.5% of tantalum, between 3% and 3.4% of molybdenum, between 0.9% and 1.1% of titanium, between 0.4% and 0.6% of aluminum, between 0.003% and 0.005% of boron, at most 0.5% of iron, at most 0.1% of copper, at most 0.1% of silicon, at most 0.05% of manganese, at most 0.01% of phosphorus, at most 0.01% of zirconium, maximum 0.004% magnesium, maximum 0.003% sulfur, maximum 0.027% oxygen, maximum 0.018% nitrogen and maximum 0.003% hydrogen.
[0022] According to a fourth aspect, the invention proposes a turbomachine part made of the material according to the third aspect.
[0023] According to a fifth aspect, the invention proposes a turbomachine comprising at least one part according to the fourth aspect. DESCRIPTION OF FIGURES
[0024] Other characteristics, aims and advantages of the invention will emerge from the following description, which is purely illustrative and non-limiting, and which must be read in conjunction with the appended drawings in which:
[0025] [Fig. 1] is a table detailing the preferred composition of the powder which is the subject of the invention.
[0026] [Fig.2] schematically represents a step of improvement of the structure of the material of a preferred embodiment of the method according to the invention.
[0027] [Fig.3] is a table detailing the composition of the material preferably obtained by the method according to the invention.
[0028] [Fig.4a] is a photograph of the material preferably obtained by the process according to the invention before chemical attack.
[0029] [Fig.4b] is a photograph according to a foreground of the material preferably obtained by the method according to the invention.
[0030] [Fig.4c] is a photograph according to a second plane of the material preferably obtained by the method according to the invention. DETAILED DESCRIPTION OF THE INVENTION
[0031] Metal powder
[0032] According to a first aspect, the invention provides a metal powder for a powder bed additive manufacturing process. The metal powder comprises a nickel-based alloy comprising at least carbon, chromium, cobalt, niobium, tantalum, molybdenum, titanium, aluminum, boron, iron, copper, silicon, manganese, phosphorus, zirconium, magnesium, sulfur, oxygen, nitrogen and hydrogen.
[0033] In the remainder of this description, the “rates” or “contents” will be expressed in mass terms (i.e. mass of said element over the total mass of the alloy).
[0034] According to a particular arrangement, as detailed in the table of [Fig. 1], the nickel-based alloy comprises between 0.02% and 0.04% carbon, between 18% and 22% chromium, between 11% and 13% cobalt, between 5% and 5.5% niobium, between 3% and 3.5% tantalum, between 3% and 3.4% molybdenum, between 0.9% and 1.1% titanium, between 0.4% and 0.6% aluminium, between 0.003% and 0.005% boron, maximum 0.5% iron, maximum 0.1% copper, maximum 0.1% silicon, maximum 0.05% manganese, maximum 0.01% phosphorus, maximum 0.01% zirconium, maximum 0.004% magnesium, maximum 0.003% sulphur, maximum 0.025% oxygen, maximum 0.018% nitrogen and maximum 0.003% hydrogen.
[0035] In doing so, the powder which is the subject of the invention comprises a level of nitrogen, oxygen and sulfur suitable for use in a powder bed additive manufacturing process.
[0036] It is specified that by a suitable rate, it is understood a rate making it possible to obtain a material having the required thermomechanical characteristics after fusion by a laser beam of the powder. Indeed, we know of metal powders for foundry (or metallurgy in general) which contain roughly the same list of elements, but their particle size and their sulfur, nitrogen and oxygen levels are not suitable.
[0037] In particular, each of sulfur, nitrogen and oxygen is present in said alloy in a level lower than a maximum level for additive manufacturing, advantageously 0.025%, very advantageously even 0.003% for sulfur and 0.018% for nitrogen.
[0038] Advantageously, the powder also has a particle size suitable for use in a powder bed additive manufacturing process.
[0039] Similarly, by suitable granulometry, we mean a granulometry allowing the good deposition of a layer of powder in a bed.
[0040] Thus, according to a particular arrangement, 10% of the grains have a diameter between 8 pm and 28 pm, 50% of the grains have a diameter between 10 pm and 45 pm and 90% of the grains have a diameter between 25 pm and 75 pm.
[0041] Preferably, 10% of the grains have a diameter between 10 pm and 25 pm, 50% of the grains have a diameter between 15 pm and 40 pm and 90% of the grains have a diameter between 30 pm and 70 pm.
[0042] This specific granulometry very advantageously makes it possible to combine optimal compactness of the powder when it is used in a powder bed additive manufacturing process, while having optimal flowability and minimizing melting stresses (which reduces the risks of cracking of the material obtained by an additive manufacturing process).
[0043] It is specified that preferably, this granulometry is obtained via an atomization process, which makes it possible to ensure the morphology of each grain while limiting the risks of pollution of the powder by foreign bodies.
[0044] Additive manufacturing process
[0045] According to a second aspect, the invention relates to a method of additive manufacturing on a powder bed by laser fusion of a powder according to the invention.
[0046] In a known manner, the method uses an additive manufacturing machine, in which a system deposits a bed of powder and emits, for example, a laser beam to melt and consolidate a layer of a material being manufactured.
[0047] In more detail, a bed of powder a few tens of microns thick is deposited on a plate, generally using a scraper. Then it is melted locally.
[0048] The plate is lowered and the deposition / fusion cycle is repeated until the part is built.
[0049] In a conventional manner, the laser beam illuminates a defined surface which is usually called a “spot”.
[0050] Generally, the laser beam is enveloped in a jet of neutral gas. Preferably, in the context of the method which is the subject of the invention, argon or nitrogen will be used.
[0051] In a manner specific to the method according to the invention, the laser emits a beam with a power of between 150W and 300W.
[0052] In addition, the laser is preferably moved at a speed between 900mm / s and 2500mm / s.
[0053] Preferably, the laser emits a beam having a diameter between 50 pm and 200 pm. It is specified that by beam diameter, it is understood that the spot, the surface illuminated by the beam, has a diameter between 50 pm and 200 pm.
[0054] As previously indicated, in a known manner, the laser beam is moved by strip and by superimposed layer to consolidate the material being manufactured.
[0055] Preferably, each strip has a width of between 2mm and 15mm.
[0056] Furthermore, the merged bands may overlap by a width of between 0.05mm and 0.15mm.
[0057] In addition, each layer of fused powder may have a thickness of between 20 pm and 60 pm.
[0058] At this stage, the raw melted alloy does not yet have the expected mechanical properties (particularly with regard to resistance to fining and fatigue).
[0059] For this, according to an advantageous arrangement, at the end of the additive manufacturing, the method comprises a step of improving the structure of the material, by various heat treatments. Each heat treatment ends with air cooling (for example under argon protection).
[0060] With reference to [Fig.2], this step may include the following phases:
[0061] It begins with an optional phase (a) of stress relief, called interoperation treatment, at a temperature between 945°C and 965°C, for approximately 2 hours (to within 20%).
[0062] This treatment allows homogenization of the material and the removal of lava phases, before the main phase of the heat treatment.
[0063] This main phase, called “use state”, makes it possible to obtain the metallurgical health necessary for the use of the material for turbomachine parts, and includes a succession of heat treatments.
[0064] First, there is (b) a first heat treatment at a temperature between 1155°C and 1175°C, for approximately 3 to 5 hours (to within 20%), followed by cooling to 595°C in less than 23 minutes, then in air.
[0065] The in-use phase then comprises (c) a second heat treatment, which itself comprises three sub-parts: heating to a temperature between 890°C and 910°C, for approximately 4 hours (to the nearest 10 minutes), followed by cooling to 775° at a rate of at least 55°C per hour; then holding at a temperature between 765°C and 785°C, for approximately 4 hours (to the nearest 10 minutes), followed by cooling to 705°C again at a rate of at least 55°C per hour; and finally holding at a temperature between 695°C and 715°C, for 8 hours (to the nearest 10 minutes). There is always the final cooling in air.
[0066] After this phase of use state, a grain size of the order of 2 to 8 ASTM is obtained which allows a good compromise between the mechanical properties (in particular between the finishing and fatigue). The heat treatments make it possible to obtain an HRC hardness of between 15 and 60HRC and properties at the expected and interesting levels for the targeted parts. A slight anisotropy typical of LBM can be noted which is however not problematic for the properties of the alloy, see figures 4a, 4b and 4c which represent the grains in the material obtained respectively before chemical attack, after chemical attack along an XY plane of the turbomachine, and after chemical attack along an XZ plane of the turbomachine.
[0067] The metallurgical health obtained includes indications of less than 0.8 mm and a porosity rate of less than 2% which allow excellent mechanical properties.
[0068] In the case of welding with another alloy, for example Inconel 718, an additional post-welding phase can be applied to maintain the two materials at the best of their respective properties.
[0069] This optional phase includes (d) a third heat treatment at a temperature between 945°C and 965°C, for approximately 1 hour (to within 20%), followed by cooling to 650°C in less than 23 minutes. The final cooling in air is always carried out.
[0070] Preferably, the post-welding phase further comprises (e) a fourth heat treatment, called tempering, again comprising three sub-parts: holding at a temperature between 750°C and 770°C, for approximately 5 hours (to the nearest 10 minutes), followed by cooling to 700°C at a rate of at least 55°C per hour; then holding at a temperature between 690°C and 710°C, for approximately 8 hours (to the nearest 10 minutes) followed by air cooling, then a final maintenance at a temperature between 640°C and 660°C, for approximately 1 hour (to the nearest 10 minutes), finished by air cooling.
[0071] Note that a thermomechanical treatment phase (application of high temperature and pressure) can be carried out at the very beginning of the step of improving the structure of the material, in particular of the hot isostatic compaction (HIC) type. This treatment makes it possible to reduce any microcracks that may be present in the material at the end of additive manufacturing.
[0072] Material obtained
[0073] According to a third aspect, the invention relates to a material obtained according to the method of the invention.
[0074] According to a particular arrangement, as detailed in the table of [Fig.3], the material obtained comprises a nickel-based alloy which comprises between 0.02% and 0.04% of carbon, between 18% and 22% of chromium, between 11% and 13% of cobalt, between 5% and 5.5% of niobium, between 3% and 3.5% of tantalum, between 3% and 3.4% of molybdenum, between 0.9% and 1.1% of titanium, between 0.4% and 0.6% of aluminum, between 0.003% and 0.005% of boron, at most 0.5% of iron, at most 0.1% of copper, at most 0.1% of silicon, at most 0.05% of manganese, at most 0.01% of phosphorus, at most 0.01% of zirconium, at most 0.01% of zinc ... maximum 0.004% magnesium, maximum 0.003% sulfur, maximum 0.027% oxygen, maximum 0.018% nitrogen and maximum 0.003% hydrogen.
[0075] This time, the material may include other chemical elements in trace amounts, in particular: - Platinum and / or vanadium at a rate of up to 500 ppm; - Other elements than those listed above at a rate of maximum 50 ppm; - It being understood that the other elements than those listed before (also other than platinum and vanadium) have a total rate of at most 500 ppm.
[0076] The presence of these elements is generally due to external contamination during handling of the powder.
[0077] It is specified that the variation in the oxygen level, relative to the composition of the powder, is due to an uptake of oxygen during the execution of the additive manufacturing process.
[0078] Turbomachine part and turbomachine
[0079] According to another aspect, the invention relates to a turbomachine part manufactured according to the method of the invention, i.e. in said material as described previously.
[0080] According to another aspect, the invention relates to a turbomachine comprising at least one part according to the invention.
Claims
Claims
1. A metal powder for an additive manufacturing process, the metal powder comprising a nickel-based alloy comprising between 0.02% and 0.04% carbon, between 18% and 22% chromium, between 11% and 13% cobalt, between 5% and 5.5% niobium, between 3% and 3.5% tantalum, between 3% and 3.4% molybdenum, between 0.9% and 1.1% titanium, between 0.4% and 0.6% aluminum, between 0.003% and 0.005% boron, at most 0.5% iron, at most 0.1% copper, at most 0.1% silicon, at most 0.05% manganese, at most 0.01% phosphorus, at most 0.01% zirconium, at most 0.004% magnesium, at most 0.003% sulfur, at most 0.025% oxygen, at most 0.018% nitrogen and at most 0.003% hydrogen, the metal powder comprising a plurality of grains having a particle size distribution in which at least 10% of the grains have a diameter of between 8pm and 28pm,at least 50% of the grains have a diameter between 10pm and 45pm and at least 90% of the grains have a diameter between 25pm and 75pm.,
2. A metal powder according to claim 1 comprising a plurality of grains having a particle size distribution in which at least 10% of the grains have a diameter between 10 pm and 25 pm.
3. A metal powder according to any preceding claim comprising a plurality of grains having a particle size distribution in which at least 50% of the grains have a diameter of between 15 pm and 40 pm.
4. A metal powder according to any preceding claim comprising a plurality of grains having a particle size distribution in which at least 90% of the grains have a diameter of between 30 pm and 70 pm.
5. A method of additive manufacturing on a powder bed by laser fusion of a powder according to any one of claims 1 to 4, the method making it possible to manufacture a part in a material obtained by laser fusion of said powder.
6. Method according to claim 5, the method being characterized in that: - the laser emits a beam with a power of between 150W and 350W, - the laser is moved at a speed between 900mm / s and 2500mm / s, - the laser emits a beam having a diameter between 50pm and 200pm - the laser fuses the powder in strips, each strip having a width between 2mm and 15mm, - each fused strip overlaps at least one other strip, over a width between 0.05mm and 0.15mm, - the laser fuses layers of powder, each layer of fused powder having a thickness between 20pm and 60pm.
7. Method according to one of claims 5 and 6 comprising a step of improving the structure of the material obtained by laser melting of said powder, the step of improving the structure of the material comprising at least the following phases: (b) first heat treatment at a temperature between 1155°C and 1175°C, for 3 to 5 hours to within 20%, followed by cooling to 595°C in less than 23 minutes; (c) second heat treatment, comprising: - maintaining at a temperature between 890°C and 910°C, for 4 hours to within 10 minutes, followed by cooling to 775°C at a rate of at least 55°C per hour; - maintaining at a temperature between 765°C and 785°C for 4 hours to the nearest 10 minutes, followed by cooling to 705°C at a rate of at least 55°C per hour; - maintaining at a temperature between 695°C and 715°C for 8 hours to the nearest 10 minutes;
8. Method according to claim 7, in which the step of improving the structure of the material further comprises a preliminary phase (a) of stress relief at a temperature between 945°C and 965°C, for 2 hours to within 20%;
9. Method according to one of claims 7 and 8, in which the step of improving the structure of the material further comprises the following phases: (d) third heat treatment at a temperature between 945°C and 965°C, for 1 hour to within 20%, followed by cooling to 650°C in less than 23 minutes; (e) fourth heat treatment, comprising: - maintaining at a temperature between 750°C and 770°C for 5 hours to the nearest 10 minutes, followed by cooling to 700°C at a rate of at least 55°C per hour; - maintaining at a temperature between 690°C and 710°C for 8 hours to the nearest 10 minutes; - maintaining at a temperature between 640°C and 660°C for 1 hour to the nearest 10 minutes.
10. Material obtained according to the method according to one of claims 6 to 9, comprising a nickel-based alloy which comprises between 0.02% and 0.04% of carbon, between 18% and 22% of chromium, between 11% and 13% of cobalt, between 5% and 5.5% of niobium, between 3% and 3.5% of tantalum, between 3% and 3.4% of molybdenum, between 0.9% and 1.1% of titanium, between 0.4% and 0.6% of aluminum, between 0.003% and 0.005% of boron, at most 0.5% of iron, at most 0.1% of copper, at most 0.1% of silicon, at most 0.05% of manganese, at most 0.01% of phosphorus, at most 0.01% of zirconium, at most 0.004% magnesium, maximum 0.003% sulfur, maximum 0.027% oxygen, maximum 0.018% nitrogen and maximum 0.003% hydrogen.
11.
12. Turbomachine part made of the material according to claim 10. Turbomachine comprising at least one part according to claim 11.