High-temperature treatment process for barrel staves

A controlled heat treatment process uniformly transforms barrel staves, addressing issues of appearance, aroma transfer, and durability, resulting in improved wine barrels with extended lifespan and reduced maintenance.

FR3135643B1Active Publication Date: 2024-10-11OPR
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022004738
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-18
Publication Date
2024-10-11
Estimated Expiration
2042-05-18

AI Technical Summary

Technical Problem

Current barrel manufacturing processes face issues such as non-standardized external appearance, reduced aroma transfer due to uneven heating, mold development, high oxidation, dimensional instability, and frequent maintenance needs, leading to a short barrel lifespan and handling difficulties.

Method used

A controlled heat treatment process for barrel staves involving temperature increase, maintenance, and rehumidification within a sealed enclosure to transform the wood uniformly, reducing micro-oxygenation and fungal resistance, while maintaining aroma transfer and enhancing durability.

Benefits of technology

The process results in visibly transformed staves with improved aroma transfer, reduced oxidation, enhanced durability, and dimensional stability, extending barrel lifespan and reducing maintenance, with lighter weight for easier handling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000012_0000
    Figure 00000012_0000
  • Figure 00000012_0001
    Figure 00000012_0001
  • Figure 00000013_0000
    Figure 00000013_0000
Patent Text Reader

Abstract

The invention relates to a heat treatment process for barrel staves (2) (1) comprising the following successive steps, carried out in a sealed chamber (10) where the atmosphere is controlled: - increasing the treatment temperature to a predetermined target temperature Tc, - maintaining the target treatment temperature Tc for a predetermined duration D1, - cooling and rehumidifying the treated staves to a predetermined humidification level H1. Figure 3 (for the abstract)
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Method for treating barrel staves at high temperatures

[0001] The invention relates to the field of cooperage and more precisely to the treatment of staves intended to be assembled with each other to design barrels.

[0002] Processes for manufacturing barrels (also called "casks" or "barrels") intended to hold liquids, such as wine, beer or vinegar, are already known in the state of the art. More specifically, with regard to wine, such barrels have been used for centuries and allow, in particular, the stage known as "aging the wine".

[0003] The methods of manufacturing such barrels comprise, in a known manner, the following steps ([Fig.l]): a. cutting and selection of trunks, b. splitting the logs into quarters c. flow of staves d. drying of staves e. machining of staves f. pink setting g. bending h. heating i. installation of bases, strapping and drilling j. finishing (sanding and cleaning)

[0004] The heating stage of the curved staves is particularly important since its purpose is to allow the wood fiber to keep its shape, due to its thermoelastic properties, but also to develop the aromas that will be transmitted to the wine during its storage (hazelnut, buttery, vanilla, even smoky flavors, which will match the wines). This heating allows the staves to be "cooked" on the surface.

[0005] However, this step of heating the staves has many disadvantages. A first disadvantage is the lack of uniformity in the external appearance of the barrels obtained. Indeed, the degree of heating carried out during the manufacture of the barrel, which defines the aromas transmitted to the wine, and consequently the specific characteristics of the barrel, are not visible from the outside of the barrel, because the heating is carried out only on the internal wall of the curved staves forming the barrel. A second disadvantage, also linked to this heating step carried out only on the internal wall of the barrel, is that it needs to be carried out before the installation of the bottoms which are therefore not heated with the internal wall. As a result, the exchange surface between the wine and the heated wood of the barrel is reduced, thus reducing the transfer of aroma between the wood of the barrel and the wine. In addition, the ability of barrels, produced according to current techniques, to transmit aromas to the wine generally fades after three years, which implies a very short barrel renewal cycle. A third disadvantage, still linked to the heating stage of the staves, is that the latter are subject to a strong development of mold on the surface of the barrels, especially in humid cellars. Indeed, on the external face, the wood is not heat treated. It is therefore left raw. However, wood, by nature, in a humid environment, absorbs water like a sponge and therefore becomes a very favorable environment for the development of fungi.Indeed, for certain fungi (wood-eating fungi), wood is edible and their growth is facilitated by humidity.

[0006] An additional disadvantage, also linked to the heating step, is that the latter generally confers a strong micro-oxygenation power to the staves leading to a very high oxidation of the wine, which can be detrimental for certain types of wine where such oxidation is not desirable. Another disadvantage resulting from current manufacturing processes is that the barrels obtained suffer from a loss of tightness between winemaking seasons. Indeed, the wood currently used is subject to strong dimensional variations when the hydrometric conditions vary (barrel full of liquid or empty barrel), which implies regular and significant maintenance to avoid these deformations. Finally, current barrels are generally extremely heavy, which complicates both their transport and the numerous handling operations required during their manufacture by the cooper.

[0007] The invention aims to overcome all of the aforementioned drawbacks.

[0008] To this end, the invention relates to a method for heat treatment of barrel staves comprising the following successive steps, carried out in a sealed enclosure where the atmosphere is controlled:

[0009] - increasing the treatment temperature to a target temperature Te predetermined,

[0010] - maintaining the target treatment temperature Te for a duration DI predetermined,

[0011] - cooling and re-wetting of the treated staves to a rate predetermined H1 humidification.

[0012] Thus, thanks to the method of heat treatment of the staves according to the invention, it is possible to treat the wood of the staves so as to lead to a total transformation of said wood. Such a transformation is visible on the whole (in other words on both sides) of the stave, which results in a variation in the color of the wood. This is therefore visible from the outside of the barrel made from such staves. It is therefore possible to view its specific characteristics from the outside of the barrel. The transformation of the wood of the treated staves results in a tightening of the wood mesh. Micro-oxygenation is therefore reduced, which limits the oxidation undergone by the stored wine. The sulfites naturally present in the wine are also preserved for longer and thus act as an antioxidant and antiseptic. The barrels thus obtained offer better natural preservation of the wine. The wood used to form the staves can be any type of wood known to those skilled in the art. By way of non-limiting example, it can be oak, chestnut, black locust, poplar, ash, willow or even alder.

[0013] The transformation induced by the process according to the invention also makes it possible to increase the natural durability of the wood used to form the staves, since they are more resistant to fungal attacks and insects. Thus, the barrels obtained from the treated staves have a longer lifespan and ensure better sanitary conditions throughout their life. The heat treatment, by reducing the equilibrium hydrometry rate of the wood, in fact prevents the development of micro-organisms. The heat treatment of the staves according to the process of the invention gives them increased dimensional stability of the order of 30 to 50%, thus drastically reducing sealing problems as well as the related maintenance costs. The duration of aroma transfer is also extended compared to staves of the prior art. The replacement of the barrels is therefore less frequent.Finally, the staves thus treated undergo a loss of mass of the order of 5 to 10%, which ultimately makes the resulting barrel lighter and therefore easier to handle and transport.

[0014] According to other optional characteristics of the method of heat treatment of staves of a barrel according to the invention taken alone or in combination:

[0015] - the temperature increase step is broken down as follows:

[0016] - a first linear increase in the treatment temperature up to a first predetermined temperature Tl,

[0017] - second linear increase in the processing temperature up to a second predetermined temperature T2,

[0018] - third linear increase in processing temperature up to the predetermined target temperature Te;

[0019] - the target temperature Te is between 140 and 240°C;

[0020] - the duration DI is between 2 and 3 hours;

[0021] - the humidification rate H1 is between 4 and 7%;

[0022] - the first linear increase in processing temperature is faster than the second linear increase in processing temperature; and

[0023] - the controlled atmosphere is composed of air and a pyrolysis regulating agent, the pyrolysis regulating agent preferably being pressurized water vapor.

[0024] The invention also relates to a method of manufacturing a barrel comprising a step of heat treatment of the staves according to the heat treatment method according to the invention.

[0025] According to other optional characteristics of the barrel manufacturing process taken alone or in combination:

[0026] - the manufacturing process includes a step of laying the bottoms, strapping and drilling of the barrel after the heat treatment stage of the staves; and

[0027] - the manufacturing process comprises a first step of machining the staves prior to the heat treatment step of the staves and a second step of machining the staves after the heat treatment step of the staves.

[0028] The invention also relates to a method for restoring an existing barrel comprising a step of heat treatment of the staves according to a heat treatment method according to the invention.

[0029] The restoration method preferably comprises a step of machining the staves of the existing barrel, said machining step being subsequent to the step of heat treatment of the staves.

[0030] The invention also relates to a barrel comprising staves obtained by the heat treatment process according to any one of the variants mentioned above. Brief description of the figures

[0031] The invention will be better understood on reading the following description given solely by way of example and with reference to the appended drawings in which:

[0032] [Fig-1] [Fig.l] illustrates a method of manufacturing barrels according to the prior art

[0033] [Fig.2] [Fig.2] is a graph illustrating the method of heat treatment of staves of a barrel according to a first embodiment of the invention;

[0034] [Fig.3] [Fig.3] is a graph illustrating the method of heat treatment of staves of a barrel according to a second embodiment of the invention;

[0035] [Fig.4] [Fig.4] illustrates a method of manufacturing barrels according to a first embodiment of the invention,

[0036] [Fig.5] [Fig.5] illustrates a method of restoring an existing barrel according to a first embodiment of the invention. Detailed description

[0037] Figures 1, 4 and 5 show a barrel, designated by the general reference 1. Whether it is a new or restored barrel 1, the latter comprises a plurality of staves 2 treated in accordance with the heat treatment method of the invention a first mode of which is illustrated in [Fig.2]. This method of heat treatment of staves 2 of a barrel 1 successively comprises the following steps, carried out in a sealed enclosure 10 where the atmosphere is controlled:

[0038] - increasing the treatment temperature to a target temperature Te predetermined,

[0039] - maintaining the target treatment temperature for a predetermined duration DI,

[0040] - cooling and re-wetting of the treated staves to a rate predetermined H1 humidification.

[0041] The enclosure 10 is an airtight space within which the atmosphere can be controlled so as to adapt the heating applied to the stored stave. By "controlled atmosphere" is meant an ambient atmosphere within which the evolution of the physicochemical components are measured and regulated. In a non-exhaustive manner, this control can involve the regulation of the ambient gases (oxygen, nitrogen, dioxygen) and / or the maintenance of a minimum hydrometry rate. Advantageously and in order to best control the cooking of the staves 2, a pyrolysis regulating agent partially composes the controlled atmosphere. Advantageously, such a regulating agent is pressurized water vapor. Alternatively, it can be any pyrolysis regulating agent known to those skilled in the art, for example, nitrogen or gases emitted during at least one of the linear increases P1, P2 and / or P3 of the treatment temperature of the staves 2.

[0042] The increase in the processing temperature may be linear until the target processing temperature Te is obtained. Alternatively, it may be an increase in stages (as described in the second embodiment).

[0043] The method of heat treatment of staves 2 of a barrel 1 according to the first embodiment operates as follows.

[0044] After placing the staves 2 in the sealed enclosure 10, the enclosure is heated to obtain an increase in the treatment temperature up to a predetermined target temperature Te. For example, for this step, the staves 2 are gradually heated, for example between 36 and 48 hours, until the target temperature TC is obtained, advantageously between 140°C and 240°C. In order to ensure very good transformation of the wood of the staves 2, this target temperature Te is then maintained for the duration D1, advantageously between 2 and 3 hours. This step is similar to a step of cooking the wood of the staves 2.

[0045] Finally, the temperature within the enclosure 10 is gradually lowered until it returns to the initial temperature, while re-wetting the wood of the staves 2 by spraying water so as to obtain a humidification rate H1 of the staves 2. Advantageously, and to obtain good mechanical properties of the staves 2 treated, the H1 humidification rate is between 4% and 7%. This last stage lasts between 5 and 15 hours.

[0046] Such a heat treatment process for the staves 2 of the barrel 1 results in a more hydrophilic structure of the wood forming the staves 2 due to the degradation of the hemicelluloses, this degradation making it possible to limit moisture uptake, which gives the treated wood improved dimensional stability and durability, compared to the original wood. This heat treatment process also makes it possible to promote the crosslinking of the lignins in the wood of the staves 2, which results in a hardening of the latter. Finally, the heat treatment process causes the transformation of the crystalline structure of the cellulose in the wood of the staves 2. This results in increased rigidity of the wood fiber.In other words, the staves 2 thus treated by the heat treatment process described exhibit an increase in the natural durability of the wood (enabling them to resist fungal and insect attacks), better dimensional stability, a modification to the core of the wood (involving a change in the color and odor of the wood) and a loss of mass.

[0047] The staves 2 thus treated using the heat treatment process of the invention allow the manufacture of new barrels, in the case of staves from new staves, or the restoration of existing barrels 1, if the staves 2 come from a barrel 1 manufactured using a prior art process.

[0048] Advantageously, according to the second embodiment of the method of the invention ([Fig.3]), the temperature increase step is broken down as follows:

[0049] - first linear increase PI of the treatment temperature up to a first predetermined temperature Tl,

[0050] - second linear increase P2 of the treatment temperature up to a second predetermined temperature T2,

[0051] - third linear increase P3 of the treatment temperature up to the predetermined target temperature Te.

[0052] After placing the staves 2 in the sealed enclosure 10, the enclosure is heated to obtain a first linear increase PI in the treatment temperature. For example, for this first step, the staves 2 are heated gradually and for 2 to 6 hours until a first temperature Tl of between 80°C and 120°C, preferably 100°C, is obtained. This first step is similar to a step of rapid increase in temperature of the wood of the staves 2.

[0053] Then, the heating is increased so as to obtain a second linear increase P2 of the treatment temperature. For example, for this second step, the staves 2 are heated gradually and for 10 to 18 hours until a second temperature T2 is obtained, between 110°C and 150°C, preferably 130 °C. This step is similar to a drying step for the wood of staves 2. Advantageously, the first linear increase PI in treatment temperature is faster than the second linear increase P2 in treatment temperature. At the end of these first two steps, the moisture content of the wood forming staves 2 tends towards 0%.

[0054] Then, the enclosure 10 is heated very strongly to obtain a third linear increase P3 of the treatment temperature. For example, for this third step, the staves 2 are gradually heated for a duration DI until the target temperature Te, between 140°C and 240°C, is obtained. In order to ensure very good transformation of the wood of the staves 2, the duration DI for maintaining the target temperature Te is between 2 and 3 hours. This step is similar to a step of cooking the wood of the staves 2. The last step of this second mode of implementation is similar to that of the first mode of implementation and will therefore not be repeated.The gradual rise in temperature of this method of implementation, in addition to all the advantages cited in the context of the first method of implementation, allows better control of the integrity of the wood forming the staves 2 which allows better conditioning of the latter with a view to their cooking at the target temperature Te.

[0055] A method of manufacturing a barrel 1 according to the invention comprises as a step the method of heat treatment of staves according to the invention. Such a method comprises as a step, a step of heating the staves 2 according to the method of heat treatment of staves 2 as described in the embodiment of [Fig.2]. According to a particular embodiment of the method of manufacturing barrel 1, illustrated in [Fig.3], the following steps are included:

[0056] (a) cutting and selection of trunks,

[0057] (b) splitting the logs into quarters

[0058] (c) flow of staves

[0059] (d) drying the staves

[0060] (e) machining of staves 2

[0061] (f) pinking

[0062] (g) bending

[0063] (h') heat treatment of the staves 2 according to the method of the invention

[0064] (i) installation of the bottoms, strapping and drilling

[0065] (j) finishing (sanding and cleaning)

[0066] It is thus possible to dispense with the conventional heating step (h) of the curved barrels while resulting in a barrel 1 formed from staves 2 treated according to the heat treatment method of the invention with all the advantages relating thereto previously mentioned. Nevertheless, it is also possible according to the invention to carry out the heat treatment step (h') of the staves 2 according to the method of the invention in addition to and subsequently to a conventional heating step (h) of the curved barrel. Such an alternative may, for example, prove advantageous in the context of a treatment of staves 2 of pre-existing barrels.

[0067] In an embodiment not shown of the method for manufacturing barrel 1, the staves 2 can be re-machined after the heating step (h') of the staves 2. Thus, it is possible to rework the staves 2 in order to guarantee the final sealing of the manufactured barrel 1 when the heat treatment step (h') deforms the surface condition of the treated staves 2. Advantageously, this re-machining of the staves 2 takes place on the edge of the staves 2, in order to make them more closely fitted to each other.

[0068] According to a non-represented embodiment of the barrel manufacturing method, the staves 2 are dismantled after the bending step (g) so as to be heated separately during the heating step h' according to the heat treatment method of the staves 2 of the invention while already having their final shape. Thus, it is possible to reduce the space required for transport and storage between and / or on the barrel production sites.

[0069] A method of restoring an existing barrel 1 according to the invention comprises as a step of heat treatment of the staves 2 according to the method of the invention as described in the embodiment of [Fig.2]. According to a particular embodiment of the method of restoring an existing barrel 1, illustrated in [Fig.3], the following steps are included:

[0070] (k) recovery of an existing barrel,

[0071] (1) dismantling the bottom

[0072] (m) cleaning and sanding

[0073] (h') heat treatment of the staves 2 according to the method of the invention

[0074] (n) re-machining of staves 2

[0075] (o) reassembly of the staves 2

[0076] (p) strapping and finishing

[0077] The method of restoring existing barrels 1 of the invention makes it possible to give a second life to barrels already in use which have lost their ability to transmit aromas to the wine while resulting in a new barrel 1 formed from staves 2 treated according to the heat treatment method of the invention with all the advantages relating thereto previously mentioned. Advantageously, the dismantled bottom can undergo the same treatment as the staves, then be in turn re-machined so as to have the dimensions adapted to the restored barrel.

[0078] The invention is not limited to the embodiments presented and other embodiments will become clear to those skilled in the art. List of references

[0079] 1: barrel (new or restored) 2: stave

[0080] 10: enclosure

[0081] DI: duration of maintaining the target treatment temperature

[0082] H1: predetermined humidification rate of the staves

[0083] PI: first linear increase in processing temperature

[0084] P2: second linear increase in treatment temperature

[0085] P3: third linear increase in processing temperature

[0086] Tl: first predetermined temperature

[0087] T2: second predetermined temperature

[0088] Te: predetermined target temperature

Claims

Claims

1. Method for heat treatment of staves (2) of a barrel (1) comprising successively the following steps, carried out in a sealed enclosure (10) where the atmosphere is controlled: - placing the staves (2) in the sealed enclosure (10), - increasing the treatment temperature to a predetermined target temperature Te, - maintaining the target treatment temperature Te for a predetermined duration DI, - simultaneous cooling and rehumidification of the treated staves to a predetermined humidification rate H1.

2. Heat treatment method according to the preceding claim, in which the temperature increase step is broken down as follows: - a first linear increase in the treatment temperature up to a first predetermined temperature T1, - second linear increase in the treatment temperature up to a second predetermined temperature T2, - third linear increase in the treatment temperature up to the predetermined target temperature Te.

3. A heat treatment method according to any preceding claim, wherein the target temperature Te is between 140 and 240°C.

4. A heat treatment method according to any one of the preceding claims, wherein the duration DI is between 2 and 3 hours.

5. Heat treatment method according to any one of the preceding claims, in which the humidification rate H1 is between 4 and 7%.

6. A heat treatment method according to any one of claims 2 to 5, wherein the first linear increase in treatment temperature is faster than the second linear increase in treatment temperature.

7. A heat treatment method according to any preceding claim, wherein the controlled atmosphere is composed of air and a pyrolysis regulating agent, the agent pyrolysis regulator preferably being pressurized water vapor.

8. A method of manufacturing a barrel comprising a step of heat treatment of the staves according to the heat treatment method according to any one of claims 1 to 7.

9. Manufacturing method according to the preceding claim, comprising a step of laying the bottoms, strapping and drilling the barrel after the step of heat treatment of the staves.

10. Manufacturing method according to claim 8 or 9, comprising a first step of machining the staves prior to the step of heat treatment of the staves and a second step of machining the staves subsequent to the step of heat treatment of the staves.

11. A method of restoring an existing barrel comprising a step of heat treating the staves according to the heat treatment method according to any one of claims 1 to 7.

12. Restoration method according to the preceding claim, comprising a step of machining the staves of the existing barrel, said machining step being subsequent to the step of heat treatment of the staves.

13. Barrel comprising staves obtained by the heat treatment process according to any one of claims 1 to 7.