Additive manufacturing process for an object comprising at least one thin wall.
The selective consolidation of thin walls using continuous laser paths in multiple layers addresses the inefficiencies of core/contour strategies, enhancing productivity and quality in additive manufacturing of thin walls.
Patent Information
- Application Number
- FR2022005337
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-06-02
AI Technical Summary
Existing additive manufacturing processes for objects with numerous thin walls face challenges such as increased calculation times, reduced productivity, and fusion defects due to the core/contour selective consolidation strategy, especially when dealing with thin walls less than 0.5 mm thick.
A selective consolidation strategy using continuous laser beam paths in multiple layers to consolidate thin walls, reducing the number of paths and jumps, and ensuring overlap between adjacent paths for improved cohesion.
This approach reduces calculation times, enhances productivity, and produces thinner, higher-quality thin walls with improved metallurgical structure, while maintaining dimensional accuracy.
Smart Images

Figure 00000013_0000 
Figure 00000013_0001 
Figure 00000014_0000
Abstract
Description
Title of the invention: Method for additive manufacturing of an object comprising at least one thin wall.
[0001] The present invention relates to the additive manufacturing of an object comprising at least one thin wall. The additive manufacturing method according to the invention is particularly advantageous when it is used to manufacture an object comprising numerous thin walls which may or may not intersect with each other. By thin walls is meant walls whose thickness is less than 0.5 mm.
[0002] More specifically, the invention relates to a method of additive manufacturing by powder bed deposition and selective fusion. According to this method, the object is manufactured by the selective consolidation of different layers of powder superimposed on each other. For example, the selective consolidation of each layer of powder is carried out using a laser beam.
[0003] To achieve the selective consolidation of each layer of powder, the laser beam spot travels a continuous or discontinuous trajectory on each layer of powder. This trajectory is determined, for each layer of powder, before the implementation of additive manufacturing via software, called slicing, dedicated to this operation.
[0004] As illustrated in [Fig.l], to manufacture a part 10 comprising walls 12 which intersect, it is possible to use a selective consolidation strategy called core / contour in which a wall 12 is selectively consolidated in each layer of powder with at least one contour path 14 of the laser beam spot which extends along the length of said wall and which is located at the outer edge of said wall, and with a plurality of hatching paths 16 of the laser beam spot which are juxtaposed across the length of said wall and which are located inside the contour path(s) 14, i.e. at the heart of the manufactured part 10.
[0005] In the case of the manufacture of parts 10 with numerous walls 12, this selective consolidation strategy called core / contour has several drawbacks.
[0006] On the one hand, the large number of walls 12 of the part will result in a very large number of hatching paths 16, which considerably increases the calculation times of the trajectories of the laser beam spot for all the layers of powders by the slicing software.
[0007] In addition, the large number of hatching paths 16 results in a large number of jumps of the laser beam spot between two adjacent hatching paths, and this large number of jumps increases the selective consolidation times of each layer of powder and therefore penalizes the productivity of the manufacturing process and the manufacturing machine on which it is implemented.
[0008] Finally, when the walls 12 of the part 10 are thin walls of only a few millimeters in thickness, the selective consolidation strategy called core / contour may lead to defects in the fusion of the powder, and therefore to problems of sealing of the manufactured part, or may not allow the requested dimensions to be respected, resulting in the manufacture of walls 12 that are thicker than what was requested.
[0009] The present invention aims to provide a solution to the drawbacks of the so-called core / contour selective consolidation strategy.
[0010] For this purpose, the subject of the invention is a method for additive manufacturing of an object comprising at least one thin wall, a thin wall being a wall whose thickness is less than 0.5 millimeters, the object being manufactured by the selective consolidation of different superimposed layers of powder, the selective consolidation of each layer of powder being carried out using at least one laser beam, the spot of the laser beam traveling a continuous or discontinuous trajectory on each layer of powder to carry out the selective consolidation of this layer of powder, the trajectory of the spot of the laser beam on each layer of powder comprising at least one continuous path.
[0011] According to the invention, at least one thin wall of the object is selectively consolidated in several layers of powder useful for its manufacture with a single continuous path of the laser beam spot in each of these layers of powder or only with a plurality of continuous paths of the laser beam spot juxtaposed in each of these layers of powder, the continuous path(s) constituting a thin wall in a layer of powder extending along the entire length of said thin wall in this layer of powder.
[0012] By using this selective consolidation strategy, hatching paths that increase the calculation times of the laser beam spot trajectories for all the powder layers by the slicing software are avoided and the size of the production files generated by the slicing software is reduced by reducing the number of distinct paths of the laser beam spot on each powder layer. In addition, by avoiding the use of hatching paths, the multiplication of jumps of the laser beam spot is avoided, which improves the productivity of the manufacturing process and the manufacturing machine on which it is implemented. Finally, the selective consolidation strategy according to the invention makes it possible to obtain thinner walls of better quality than the core / contour strategy.
[0013] Advantageously but not necessarily, the invention also consists of an additive manufacturing process in which: - at least one thin wall of the object is selectively consolidated in several layers of powder useful for its manufacture only with two to twelve continuous paths of the laser beam spot juxtaposed in each of these layers of powder, - at least one thin wall of the object is selectively consolidated in several layers of powder useful for its manufacture only with two continuous paths of the laser beam spot juxtaposed in each of these layers of powder, - when a thin wall of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths of the laser beam spot juxtaposed in each of these layers of powder, the juxtaposed continuous paths are arranged at a regular interval, also called intervector space, from each other, - when a thin wall of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths of the laser beam spot juxtaposed in each of these layers of powder, two adjacent continuous paths taken from this plurality of juxtaposed continuous paths are traveled in opposite directions by the spot of the laser beam, - when a thin wall of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths of the laser beam spot juxtaposed in each of these layers of powder, and each continuous path traveled by the laser beam spot in a layer of powder results in the creation of a bead of solid material of non-zero thickness and non-zero depth, an overlap is provided between two adjacent beads of solid material resulting from the path of the laser beam spot along two continuous juxtaposed and adjacent paths, - the overlap between two adjacent cords of solid material which are solidified in the same layer of powder to produce the same thin wall is between 20% and 60%, preferably between 30% and 40%, of the thickness of one of the two cords, - when the manufactured object comprises a first thin wall that intersects a second thin wall, the continuous path(s) of the laser beam spot used to consolidate the first thin wall in a layer of powder intersect with the continuous path(s) of the laser beam spot used to consolidate the second thin wall in this same layer of powder, and the continuous path(s) of the laser beam spot used to consolidate the first thin wall in this layer of powder extend on either side of their intersection with the continuous path(s) of the laser beam spot used to consolidate the second thin wall in this same layer of powder, - the manufactured object being made up of one or more thin walls with a thickness of less than 0.5 mm and a thick portion with a thickness of greater than 0.5 mm, the thick portion is selectively consolidated in a plurality of layers of powder according to a core / contour strategy with at least one contour path of the laser beam spot in each powder layer of this plurality of powder layers which extends along the length of said thick portion in this powder layer and which lies on the outer edges of said thick portion, and with a plurality of hatching paths of the laser beam spot in each powder layer of this plurality of powder layers, the hatching paths being juxtaposed across the length of said thick portion in this powder layer and lying inside the at least one contour path, - the powder layers are superimposed in a vertical superposition direction, and in which a thin wall rises in height in this vertical superposition direction.
[0014] The invention also relates to an object manufactured additively with the additive manufacturing method according to the invention, knowing that the metallurgical structure of the object in its thin wall(s) being specific to the additive manufacturing method according to the invention and differing from the metallurgical structure of the thin wall(s) of an object manufactured with a selective core / contour consolidation strategy.
[0015] Finally, the invention also relates to an object manufactured additively with the additive manufacturing method according to the invention, and in which the thin wall(s) with a thickness of less than 0.5 are connected to a thick part with a thickness greater than 0.5 mm.
[0016] Other characteristics and advantages of the invention will appear in the description which follows. This description, given by way of example and not as a limitation, refers to the attached drawings in which: [Fig.l] is a schematic representation of a selective consolidation strategy, called core / contour, of an additive manufacturing process, [Fig.2] schematically illustrates a first variant of the production of a thin wall manufactured using the additive manufacturing method according to the invention, [Fig.3] schematically illustrates a second variant of the production of a thin wall manufactured using the additive manufacturing method according to the invention, [Fig.4] schematically illustrates an alternative embodiment of the intersection of two thin walls manufactured using the additive manufacturing method according to the invention, [Fig.5] schematically represents the overlap between two cords of solid material constituting a thin wall manufactured using the additive manufacturing process according to the invention, [Fig.6] schematically represents an object comprising thin walls manufactured with the additive manufacturing method according to the invention and connected to a thick part manufactured with a core / contour strategy.
[0017] The invention relates to a method for additive manufacturing of an object 20 comprising at least one thin wall 22.
[0018] By thin wall is meant a wall 22 whose thickness E22 is less than 0.5 millimeters. The thickness E22 of a thin wall 22 is measured in a plane corresponding to one of the layers of powder which has been selectively consolidated for the manufacture of the object comprising this thin wall.
[0019] Indeed, the invention relates to an additive manufacturing method by powder bed deposition and selective fusion. According to this additive manufacturing method, the object is manufactured by the selective consolidation of different layers of powder superimposed on each other. Preferably, in the additive manufacturing method according to the invention, the selective consolidation of each layer of powder is carried out using at least one laser beam.
[0020] To achieve the selective consolidation of each layer of powder, the spot of the laser beam travels a continuous or discontinuous trajectory 24 on each layer of powder. This trajectory is determined, for each layer of powder, before the implementation of additive manufacturing via software, called slicing, dedicated to this operation.
[0021] According to the invention, the trajectory 24 of the spot of the laser beam on each layer of powder comprises at least one continuous path 26. For example, an object 20 may consist solely of a thin wall 22. By trajectory or path of the spot of the laser beam, it is meant a trajectory or a path of the center of the spot of the laser beam on the layer of powder. In the various figures, a trajectory or a path of the spot of the laser beam is therefore represented by a line illustrating the trajectory or the path of the center of the spot of the laser beam.
[0022] In a first variant embodiment of a thin wall illustrated in [Fig.2], at least one thin wall 22 of the object 20 is selectively consolidated in several layers of powder useful for its manufacture with a single continuous path 26 of the laser beam spot in each of these layers of powder. In this case, a thin wall 22 has for example a thickness E22 of between 80 micrometers and 200 micrometers.
[0023] In a second variant embodiment of a thin wall illustrated in [Fig.3], at least one thin wall 22 of the object 20 is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths 26 of the laser beam spot juxtaposed in each of these layers of powder.
[0024] By continuous juxtaposed paths 26 is meant paths of the laser beam spot arranged next to each other in a layer of powder and which do not intersect.
[0025] In either of these alternative embodiments, the continuous path(s) 26 constituting a thin wall 22 in a layer of powder extend over the entire length L22 of said thin wall in this layer of powder. The length L22 of a thin wall is the longest dimension of this thin wall in a layer of powder in which this thin wall is consolidated and therefore manufactured.
[0026] For example, a thin wall 22 of the object 20 is selectively consolidated in each of the layers of powder useful for its manufacture with a single continuous path 26 of the laser beam spot in each of these layers of powder.
[0027] For example, a thin wall 22 of the object 20 is selectively consolidated in each of the layers of powder useful for its manufacture only with a plurality of continuous paths 26 of the laser beam spot juxtaposed in each of these layers of powder.
[0028] As a thin wall has a thickness E22 of less than 0.5 mm and the spot of a laser beam used for the selective consolidation measurement has a diameter or a maximum dimension of between 80 and 200 micrometers, the method according to the invention provides that at least one thin wall 22 of the object is selectively consolidated in several layers of powder useful for its manufacture only with two to twelve continuous paths 26 of the spot of the laser beam juxtaposed in each of these layers of powder.
[0029] For example, a thin wall 22 of the object 20 is selectively consolidated in all the layers of powder useful for its manufacture with the same number of continuous paths 26 of the laser beam spot juxtaposed in each of these layers of powder.
[0030] For example, a thin wall 22 of the object is selectively consolidated in each of the layers of powder useful for its manufacture only with a number of continuous and juxtaposed paths 26 of between two and twelve.
[0031] For example, at least one thin wall 22 of the object is selectively consolidated in several layers of powder useful for its manufacture only with two continuous paths 26 of the laser beam spot juxtaposed in each of these layers of powder.
[0032] For example, at least one thin wall 22 of the object is selectively consolidated in all the layers of powder useful for its manufacture only with two continuous paths 26 of the laser beam spot juxtaposed in each of these layers of powder.
[0033] In the case where a thin wall 22 of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths 26 of the laser beam spot juxtaposed in each of these layers of powder, the juxtaposed continuous paths 26 are for example arranged at a regular interval 126, also called inter-vector space, from each other. For example, the regular interval 126 between two juxtaposed continuous paths is between 40 micrometers and 250 micrometers.
[0034] To further improve productivity and as illustrated in Figures 3 and 4, when a thin wall 22 of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths 26 of the laser beam spot juxtaposed in each of these layers of powder, two adjacent continuous paths 26A, 26B taken from this plurality of juxtaposed continuous paths are traveled in opposite directions S1, S2 by the laser beam spot. Thus, the thin wall 22 is consolidated by back and forth(s) of the laser beam in the layer of powder, which limits the number of jumps and the jump distance of the laser beam between two continuous paths.
[0035] As illustrated in [Fig. 5], each continuous path 26A, 26B traveled by the spot of the laser beam in a layer of powder results in the creation of a bead 28A, 28B of solid material of non-zero thickness E28 and non-zero depth. Also, when a thin wall 22 of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths of the spot of the laser beam juxtaposed in each of these layers of powder, an overlap C is provided between two adjacent beads of solid material 28A, 28B resulting from the travel of the spot of the laser beam along two continuous paths 26A, 26B juxtaposed and adjacent.
[0036] For example, the thickness E28 of a bead of solid material is between 80 micrometers and 300 micrometers. For example, the depth of a bead of solid material is between 50 micrometers and 300 micrometers. For example, the bead(s) of solid material forming a thin wall all have substantially the same thickness.
[0037] For example, the overlap C between two adjacent cords of solid material 28A, 28B which are solidified in the same layer of powder for the production of the same thin wall 22 is between 20% and 60%, preferably between 30% and 40%, of the thickness E28 of one of the two cords. This overlap makes it possible to guarantee the cohesion and therefore the solidity of the thin wall 22.
[0038] As illustrated in [Fig. 4], when the manufactured object comprises a first thin wall 22A which intersects a second thin wall 22B, the continuous path(s) 26A, 26B of the laser beam spot used to consolidate the first thin wall 22A in a layer of powder intersect with the continuous path(s) 26C, 26D of the laser beam spot used to consolidate the second thin wall 22B in this same layer of powder, and the continuous path(s) 26A, 26B of the laser beam spot used to consolidate the first thin wall 22A in this layer of powder extend on either side of their intersection with the continuous path(s) 26C, 26D of the laser beam spot used to consolidate the second thin wall 22B in this same layer of powder. This strategy of selectively consolidating an intersection between two thin walls allows for increased productivity compared to a strategy in which the continuous paths do not intersect.Also, more . the manufactured object 20 comprises thin walls which intersect, the more the selective consolidation strategy according to the invention makes it possible to increase the productivity of the manufacturing process.
[0039] As illustrated in [Fig.6], the manufactured object 20 may consist of several thin walls 22A, 22B with a thickness E22 of less than 0.5 mm and a thick part 30 with a thickness E30 of greater than 0.5 mm.In this case, the method according to the invention provides for example that the thick part 30 is selectively consolidated in a plurality of powder layers according to a core / contour strategy with at least one contour path 32 of the laser beam spot in each powder layer of this plurality of powder layers which extends in the length L30 of said thick part in this powder layer and which is located on the outer edges 34 of said thick part, and with a plurality of hatching paths 36 of the laser beam spot in each powder layer of this plurality of powder layers, the hatching paths 36 being juxtaposed across the length L30 of said thick part in this powder layer and located inside the contour path(s) 32.The length L30 of a thick part 30 is the longest dimension of this thick part in a layer of powder in which this thick part is consolidated and therefore manufactured.
[0040] For example, the powder layers being superimposed in a vertical superposition direction DS, a thin wall 22 rises in height in this vertical superposition direction DS. In more detail, a thin wall 22 can be aligned with this vertical superposition direction over its entire length L22 or only over a portion of its length L22, or a thin wall 22 can be inclined or curved relative to this vertical superposition direction DS over its entire length L22 or only over a portion of its length L22.
[0041] Generally speaking, the selective consolidation strategy proposed by the invention makes it possible to reduce the number of continuous paths forming the trajectory of the laser beam spot on each layer of powder to manufacture an object comprising at least one thin wall. In addition, this reduction in the number of continuous paths per layer of powder also makes it possible to reduce the number of jumps between continuous paths for each layer of powder, which improves productivity. Finally, the reduction in the number of continuous paths per layer of powder simplifies the generation of the trajectories of the laser beam spot on each layer of powder by the slicing software and makes it possible to reduce the size of the files handled and generated by this slicing software.
[0042] The invention also relates to an object 20 comprising at least one thin wall 22 and manufactured with the selective consolidation strategy which has just been described. It should be noted that the metallurgical structure of the object in its thin wall(s) 22 is specific to the additive manufacturing process according to the invention and different from the metallurgical structure of a thin wall which would have been manufactured with a core / contour strategy.
[0043] For example, the invention relates to an object 20 comprising one or more thin walls 22 connected to a thick part 30 and in which the thin wall or walls are manufactured with the selective consolidation strategy which has just been described. For example, the thick part 30 surrounds the thin wall or walls 22.
Claims
Claims
1. A method for additive manufacturing an object (20) comprising at least one thin wall (22), a thin wall (22) being a wall whose thickness is less than 0.5 millimeters, the object (20) being manufactured by the selective consolidation of different superimposed layers of powder, the selective consolidation of each layer of powder being carried out using at least one laser beam, the spot of the laser beam traveling a continuous or discontinuous trajectory (24) on each layer of powder to carry out the selective consolidation of this layer of powder, the trajectory of the spot of the laser beam on each layer of powder comprising at least one continuous path (26),the additive manufacturing method being characterized in that at least one thin wall (22) of the object is selectively consolidated in several layers of powder useful for its manufacture with a single continuous path (26) of the laser beam spot in each of these layers of powder or only with a plurality of continuous paths (26) of the laser beam spot juxtaposed in each of these layers of powder, the continuous path(s) (26) constituting a thin wall in a layer of powder extending along the entire length (L22) of said thin wall in this layer of powder, and in that, when the manufactured object comprises a first thin wall (22A) which intersects a second thin wall (22B), the continuous path(s) (26A, 26B) of the laser beam spot used to consolidate the first thin wall (22A) in a layer of powder intersect with the continuous path(s) (26C,26D) of the laser beam spot used to consolidate the second thin wall (22B) in this same layer of powder, and the continuous path(s) (26A, 26B) of the laser beam spot used to consolidate the first thin wall (22A) in this layer of powder extend on either side of their intersection with the continuous path(s) (26C, 26D) of the laser beam spot used to consolidate the second thin wall (22B) in this same layer of powder.,
2. Additive manufacturing method according to claim 1, in which at least one thin wall (22) of the object is selectively consolidated in several layers of powder useful for its manufacture only with two to twelve continuous paths (26) of the laser beam spot juxtaposed in each of these layers of powder.
3. An additive manufacturing method according to claim 2, wherein at at least one thin wall (22) of the object is selectively consolidated in several layers of powder useful for its manufacture only with two continuous paths (26) of the laser beam spot juxtaposed in each of these layers of powder.
4. Additive manufacturing method according to one of the preceding claims, in which, when a thin wall (22) of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths (26) of the laser beam spot juxtaposed in each of these layers of powder, the juxtaposed continuous paths are arranged at a regular interval (126), also called inter-vector space, from each other.
5. Additive manufacturing method according to one of the preceding claims, in which, when a thin wall (22) of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths (26) of the laser beam spot juxtaposed in each of these layers of powder, two adjacent continuous paths (26A, 26B) taken from this plurality of juxtaposed continuous paths are traveled in opposite directions (S 1 , S2) by the spot of the laser beam.
6. Additive manufacturing method according to one of the preceding claims, in which, when a thin wall (22) of the object is selectively consolidated in several layers of powder useful for its manufacture only with a plurality of continuous paths (26) of the laser beam spot juxtaposed in each of these layers of powder, and each continuous path (26A, 26B) traveled by the laser beam spot in a layer of powder results in the creation of a bead of solid material (28A, 28B) of non-zero thickness (E28) and non-zero depth, an overlap (C) is provided between two adjacent beads of solid material (28A, 28B) resulting from the travel of the laser beam spot along two continuous paths (26A, 26B) juxtaposed and adjacent.
7. Additive manufacturing method according to claim 6, in which the overlap (C) between two adjacent cords of solid material (28A, 28B) which are solidified in the same layer of powder for the production of the same thin wall (22) is between 20% and 60%, preferably between 30% and 40%, of the thickness (E28) of one of the two cords.
8. Additive manufacturing method according to one of the preceding claims, wherein the manufactured object consists of one or more thin walls (22A, 22B) with a thickness of less than 0.5 mm and a thick portion (30) with a thickness (E30) greater than 0.5 mm, the thick portion (30) is selectively consolidated in a plurality of powder layers according to a core / contour strategy with at least one contour path (32) of the laser beam spot in each powder layer of this plurality of powder layers which extends in the length (L30) of said thick portion in this powder layer and which is located on the outer edges (34) of said thick portion, and with a plurality of hatching paths (36) of the laser beam spot in each powder layer of this plurality of powder layers, the hatching paths (36) being juxtaposed across the length (L30) of said thick portion in this powder layer and located inside the at least one contour path (32).
9. Additive manufacturing method according to one of the preceding claims, in which the powder layers are superimposed in a vertical superposition direction (DS), and in which a thin wall (22) rises in height in this vertical superposition direction (DS).
10. Object (20) manufactured additively with the additive manufacturing method according to one of the preceding claims, the metallurgical structure of the object in its thin wall(s) (22) being specific to the additive manufacturing method according to one of the preceding claims.
11. Object according to claim 10, in which the thin wall(s) (22) of thickness less than 0.5 mm are connected to a thick part (30) of thickness greater than 0.5 mm.