Enzyme-based multilayer article with water barrier properties

A multilayer biodegradable plastic article with specific polymer and enzyme compositions addresses the challenge of water barrier properties in biodegradable plastics, ensuring effective food packaging without compromising biodegradability.

FR3139500B1Active Publication Date: 2024-09-27CARBIOLICE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022009254
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-09-14
Publication Date
2024-09-27
Estimated Expiration
2042-09-14

AI Technical Summary

Technical Problem

Existing biodegradable plastic articles lack effective water barrier properties without compromising the biodegradability and enzyme activity, making it difficult to enhance their functionality for food packaging applications.

Method used

A biodegradable multilayer article composed of layers containing PHA, PLA, and thermoplastic polymers, with enzymes capable of degrading PLA, is developed to improve water barrier properties while maintaining biodegradability and enzyme activity.

Benefits of technology

The multilayer article achieves enhanced water barrier properties and maintains biodegradability, suitable for various packaging applications, including food packaging, without adversely affecting enzyme activity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a biodegradable, enzyme-enriched, multilayer article exhibiting water barrier properties.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: ENZYMED MULTILAYER ARTICLE having water barrier properties FIELD OF THE INVENTION.

[0001] The present invention relates to a biodegradable multi-layer plastic article having water barrier properties, in which at least one of the layers contains PLA as a biodegradable polymer and enzymes capable of degrading it. BACKGROUND OF THE INVENTION.

[0002] Bio-sourced and biodegradable articles are known, in particular single-layer or multi-layer articles, used in the field of bagging, and in particular for the manufacture of plastic bags. These bags are used in particular for the packaging of food products, in particular fruits and vegetables.

[0003] Mention may be made in particular of the articles described in patents and patent applications WO 2020 / 193770, WO 2007 / 118828, WO 2002 / 059202A1, WO 2002 / 059199, WO 2002 / 059198, WO 2004 / 052646, WO 2018 / 233888, US 6,841,597, US 8,751,816, US 5,436,078, US 9,096,758, US 2009 / 324917 and CN 106881929. However, these articles do not have water barrier properties for food packaging applications.

[0004] The method for producing an article comprising enzymes capable of degrading the polymers which constitute it must both allow the enzymes to be preserved during the preparation of said article, for example via mixtures with polymers which melt at temperatures which do not degrade said enzymes, and comply with the physical property constraints.

[0005] Improving, in a simple and economical manner, the water barrier property of an enzymatic biodegradable article is all the more difficult to obtain, as this must not be done to the detriment of the activity of the enzymes on the degradation of the degradable polyester.

[0006] Consequently, it is necessary to propose solutions making it possible to improve the water barrier properties of a plastic article without harming its biodegradability, and to do so in a simple, economical and efficient manner.

[0007] This objective, among others, is achieved by the new composition of the biodegradable multilayer article according to the invention which offers numerous advantages, in particular of having water barrier properties.

[0008] Indeed, the inventors have discovered that a particular mixture of polymers makes it possible to improve the water barrier properties of a multi-layer article made of biodegradable plastic including enzymes and to respect the physical property constraints of articles shaped with this mixture. BRIEF DESCRIPTION OF THE INVENTION.

[0009] The invention relates to a biodegradable multilayer article of type AB, AB A, ABC, BAB, BAC, ABCA BACB, BCACB or ACBCA, in which - layer A comprises at least PHA (polyhydroxyalkanoate) in an amount of less than 60% and PLA (polylactic acid); - layer B comprises at least one thermoplastic polymer; and - layer A and / or layer B comprises at least 0.001% enzymes capable of degrading said PLA, the percentage being given by weight relative to the total weight of the composition of each layer.

[0010] According to one embodiment of the invention, the polymer constituting layer B comprises at least one polyester chosen from polyesters such as PLA (polylactic acid), PBAT (polybutylene adipate terephthalate), PHA (polyhydroxyalkanoate), PBS (polybutylene succinate), PCL (polycaprolactone), PBSA (polybutylene succinate adipate) and mixtures thereof in all proportions, preferably a mixture of PLA, PHA and PBAT.

[0011] The article according to the invention relates to a flexible article made of plastic material, in particular a plastic film or a rigid article made of plastic material, in particular a sheet.

[0012] The flexible article according to the invention preferably has a thickness ranging from 20 to 100 μm, preferably from 25 to 80 μm, more preferably from 30 to 60 μm, even more preferably around 50 μm.

[0013] The rigid article according to the invention has a thickness of between 150 and 5000 μm, preferably between 400 and 500 μm, more preferably equal to approximately 450 μm.

[0014] The invention also relates to a film comprising a multilayer article according to the invention, preferably a flexible multilayer article according to the invention.

[0015] The invention also relates to a sheet comprising a multilayer article according to the invention, preferably a rigid multilayer article according to the invention.

[0016] The multilayer article according to the invention can be used for the preparation of a package, a lid, a cup, a plate, a beverage capsule, a tray or a packaging blister. DETAILED DESCRIPTION OF THE INVENTION.

[0017] Definitions

[0018] This description will be better understood with reference to the following definitions.

[0019] By multilayer thermoplastic article of type AB, AB A, ABC, BAB, BAC, ABCA, BACB, BCACB or ACBCA, is meant according to the invention an article whose layers are bonded together and not simply associated by simple juxtaposition. In particular and preferably, the layers are bonded by coextrusion. For example, by article of type ABA is meant an article comprising a central layer B framed by two adjacent layers A. The two layers A preferably have the same composition. According to certain embodiments of the invention, the multilayer article may comprise one or two layers C between layers A and B to provide particular properties to the articles according to the invention, more particularly to provide barrier properties to gases and in particular to oxygen. By way of example, the article ABCA or ACBCA comprises a layer C between the external layer A and the central layer B.

[0020] By "plastic article" according to the invention is meant any article made from at least one polymer, such as a sheet, film, tube, rod, profile, shape, solid block, fiber, etc. made of plastic.

[0021] The term "plastic film" or "plastic film" refers to a flexible plastic film (i.e., capable of being bent without breaking) with a thickness of less than 250 μm. Thin films are considered to have a thickness of less than 100 μm and are preferably produced by blown film extrusion while thick films have a thickness greater than 100 μm and are preferably produced by cast film extrusion.

[0022] According to the invention, the term “rigid article” or “rigid plastic article” refers to a plastic article which is not a film. These articles are preferably produced by injection, thermoforming, blow molding or even by rotational molding or 3D printing.

[0023] As used herein, the term "masterbatch" refers to a concentrated mixture of selected ingredients (e.g., enzymes, additives, etc.) and a carrier polymer that can be used to introduce said ingredients into plastic articles to impart desired properties. The masterbatch compositions enable the process to economically introduce selected ingredients during the plastic manufacturing process. Advantageously, the masterbatch is composed of a carrier polymer into which the selected ingredients are incorporated at a high concentration. Generally, the masterbatch is intended to be blended with one or more polymers or a polymer-based matrix to produce a final plastic article containing a desired amount of selected ingredients. The masterbatch may further include inorganic or organic fillers.

[0024] Unless otherwise indicated, percentages and relative ratios are expressed by mass. relative to the total mass of the composition of the article.

[0025] It is specified that the expressions “from... to...” and “between... and...” used in the present description must be understood as including the limits mentioned.

[0026] In the context of the invention, the term "approximately" refers to a margin of + / -5%, preferably + / -1%, or within the tolerance of a suitable measuring device or instrument.

[0027] Composition of the Articles

[0028] The article according to the invention is a multilayer thermoplastic article of biodegradable plastic material of type AB, ABA, ABC, BAB, BAC, ABCA, BACB, BCACB or ACBCA, in which: - layer A comprises at least PHA (polyhydroxyalkanoate) in an amount of less than 60% and PLA (polylactic acid); - layer B comprises at least one thermoplastic polymer, preferably a polyester; and - layer A and / or layer B comprises at least 0.001% of enzymes capable of degrading said PLA; the percentage being given by weight relative to the total weight of the composition of each layer.

[0029] Without being bound by any theory, it appears that the PHA, present in the composition in an amount of less than 60% with PLA and at least one thermoplastic polymer, exerts in an enzymatic multilayer article, an exacerbated function of water barrier.

[0030] Composition of layer A:

[0031] According to the invention, PHA (polyhydroxyalkanoate) polymers are biodegradable polymers and many of them are produced on an industrial scale by bacterial fermentation processes or isolated from plant materials such as corn, sweet potatoes, etc. PHA polymers can also be polycondensates of one or more hydroxyalkanoic acids.Examples of such hydroxyalkanoic acids that may be included in the PHA polymer are glycolic acid, hydroxypropanoic acid (also known as lactic acid), hydroxybutyric acid, hydroxyisobutanoic acid, hydroxypentanoic acid (also known as hydroxyvaleric acid), hydroxyhexanoic acid (also known as polycaprolactone, PCL), hydroxyheptanoic acid, hydroxyoctanoic acid, hydroxydecanoic acid, hydroxydodecanoic acid, hydroxytetradecanoic acid, or combinations of two or more thereof.

[0032] Examples include PHAs such as PHBV (poly(3-hydroxybutyrate-co-3-hydroxyvalerate), PHBH (poly3-hydroxybutyrate-co-3-hydroxyhexanoate), PHB (poly-[3-hydroxybutyrate), PHH (polyhydroxyhexanoate), P3HP (poly 3-hydroxypropionate), P3HB (poly 3-hydroxybutyrate), P4HB (poly 4-hydroxybutyrate), P4HV (poly 4-hydroxyvalerate), P5HV (poly 5- hydroxyvalerate), PHB3HP (poly 3-hydroxybutyrate-co-3-hydroxypropionate), P3HB4HB (poly 3-hydroxybutyrate-co-4-hydroxybutyrate), PHB4HV (poly 3-hydroxybutyrate-co-4-hydroxyvalerate), PHB3HV (poly 3 -hydro xybutyrate-co-3 -hydro xyvalerate), the PHB3HH (poly 3-hydroxybutyrate-co-3-hydroxyhexanoate), PHB5HV (poly 3-hydroxybutyrate-co-5-hydroxyvalerate and mixtures thereof in any proportion. Preferably, the PHA is chosen from PHBV or PHBH.

[0033] Advantageously, the PHA content in layer A is between 5% and 50%, preferably between 10% and 45%, more preferably between 20% and 40%, even more preferably between 20% and 35% by weight. According to certain embodiments of the invention, the PHA content in layer A is equal to approximately 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% and 50%.

[0034] According to a preferred embodiment, the PHA content in layer A is equal to approximately 25%.

[0035] Advantageously, the PLA content in layer A is between 2% and 90% by weight, preferably between 3% and 80%, between 4% and 70%, between 5% and 60%, more preferably between 5% and 40%, even more preferably between 10% and 40% by weight.

[0036] Layer A may comprise, in addition to PHA and PLA, complementary polyesters which are biodegradable polyesters well known to those skilled in the art. These “complementary polyesters” are in particular chosen from PB AT (polybutylene adipate terephthalate), PBS (polybutylene succinate), PCL (polycaprolactone), and PBSA (polybutylene succinate adipate), plasticized starch and their mixtures in all proportions.

[0037] Preferably, the content of complementary polyesters in layer A is between 10% and 90%, preferably between 20% and 80%, more preferably between 30 and 75%, even more preferably 40% and 70%.

[0038] According to a particular embodiment, the complementary polyester is PB AT.

[0039] According to a preferred embodiment, layer A comprises a mixture comprising PHA, PB AT, PB AT being the complementary polymer and PLA.

[0040] Composition of layer B:

[0041] Layer B comprises one or more thermoplastic polymer(s) constituting this layer. According to a preferred embodiment of the invention, this (these) constituting polymer(s) is one or more polyester(s) chosen from polyesters such as PLA (polylactic acid), PB AT (polybutylene adipate terephthalate), PHA (polyhydroxyalkanoate), PBS (polybutylene succinate), PCL (polycaprolactone), PBSA (polybutylene succinate adipate) and their mixtures in all proportions.

[0042] The constituent polymer(s) of layer B may also be chosen from barrier materials such as PVOH (polyvinyl alcohol), PVCD (polyvinyl chloride), PGA (polyglycolic acid), cellulose and its derivatives, or polysaccharides and their mixtures, used alone or in mixtures with the aforementioned polyesters.

[0043] According to a particular embodiment of the invention, the polymer constituting layer B according to the invention is chosen from PLA, PHA, and PB AT and their mixtures in all proportions.

[0044] According to a preferred embodiment, the polymers constituting layer B are a mixture of PLA, PB AT and PHA.

[0045] According to another preferred embodiment, the polymers constituting layer B are a mixture of PLA and PB AT.

[0046] Advantageously, the PHA content, when it is present alone or in a mixture with one or more other aforementioned polyesters in layer B, is as defined above for layer A. Preferably, the PHA content in layer B is equal to 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% and 55%.

[0047] In a particular embodiment, the PHA content in layer B is equal to 100%.

[0048] Advantageously, the PLA content, when present alone or in a mixture with a or several other aforementioned polyesters in layer B, is as defined above for layer A.

[0049] Advantageously, the content of PB AT, when present alone or in a mixture with one or more other aforementioned polyesters in layer B, is between 5% and 95%, preferably between 20% and 80%, more preferably 40% and 75% by weight.

[0050] Layer A and / or layer B

[0051] According to the invention, layer A and / or layer B comprises at least 0.001% of enzymes capable of degrading the PLA of layer A and where appropriate of layer B, whether they are adjacent or separated by a layer C.

[0052] The enzymes capable of degrading PLA used in the context of the present invention are well known to those skilled in the art. In particular, mention will be made of enzymes capable of degrading PLA so as to improve the biodegradability of the article according to the invention. Such enzymes and their method of incorporation into thermoplastic articles are known to those skilled in the art, in particular described in patent applications WO 2013 / 093355, WO 2016 / 198652, WO 2016 / 198650, WO 2016 / 146540 and WO 2016 / 062695. Preferably, these enzymes are chosen from proteases and serine proteases. In a particular embodiment, the serine proteases are chosen from Proteinase K of Tritirachium album, or enzymes degrading PLA from Amycolatopsis sp., Actinomadura keratinilytica, Laceyella sacchari LP 175, Thermus sp., or Bacillus licheniformis or from reformulated commercial enzymes known to degrade PLA such as Savinase®, Esperase®, Everlase® or any enzyme of the subtilisin family CAS 9014-01-1 or any functional variant.

[0053] A person skilled in the art will adapt the enzyme content in layer A and / or layer B according to his objectives of degrading the PLA of layer A and / or B which surround it.

[0054] Advantageously, the enzyme content in layer A and / or layer B will be at least 0.002%, more advantageously at least 0.05%. These contents can be up to 10%, or even more. Although it is possible to formulate compositions comprising more than 10% of enzymes, it is nevertheless rare that such contents are exceeded for the most frequent uses of the plastic articles according to the invention. Advantageously, the enzyme content in the composition of layer A and / or layer B is from 0.01 to 7%, preferably from 0.02 to 5%.

[0055] According to a particular embodiment of the invention, the multilayer article comprises, by weight relative to the total weight of the composition of the article: - 10% to 35% of PHA, preferably between 12.5 and 25% - 10% to 50% PLA, preferably between 15 and 30% - 50% to 60% PBAT, preferably between 52 and 56% - at least 0.001% of enzymes capable of degrading said PLA and - optionally, 0.8% to 8% of a support polymer such as PCL, preferably 4%.

[0056] According to a particular preferred embodiment of the invention, the article comprises, by weight relative to the total weight of the composition of the article: - 10% to 35% of PHA, preferably between 12.5 and 25% - 10% to 50% PLA, preferably between 15 and 30% - 50% to 60% PBAT, preferably between 52 and 56% - 0.8% to 8% PCL, preferably 4% - at least 0.001% of enzymes capable of degrading said PLA.

[0057] According to the invention, layer A and / or layer B may further comprise usual additives used in the preparation of plastic articles, such as slip agents, plasticizers, nucleating agents, compatibilizers, manufacturing aids, UV radiation stabilizers, anti-shock agents, mineral or vegetable fillers, etc. According to a preferred embodiment, the usual additives are used in layer A of the article.

[0058] Advantageously, the content of usual additives in the multilayer article according to the invention is at least 0.2%, in particular between 0.2 and 5% by weight, of preferably from 1 to 5%, more preferably from 2 to 4%, advantageously about 2% by weight.

[0059] According to a preferred embodiment, layer A and / or layer B of the multilayer article further comprises one or more slip agents, such as oleamide, erucamide, stearamide, behenamide, oleyl palmitamide, stearyl erucamide, ethylene bis-oleamide, EBS or a mixture thereof. Preferably, the slip agent is oleamide.

[0060] The article may also comprise plasticizers. The plasticizers used in the degradable plastic article are well known to those skilled in the art. They are in particular chosen from polyols and amides, lactic acid oligomers (OLAs) and citrate esters.

[0061] OLAs are plasticizers known to those skilled in the art, in particular as biosourced materials. They are lactic acid oligomers with a molecular weight of less than 1500 g / mol. They are preferably esters of lactic acid oligomers, their carboxylic acid end being blocked by esterification with an alcohol, in particular a linear or branched C1-C10 alcohol, advantageously a C6-C10 alcohol, or a mixture thereof. We will mention in particular the OLAs described in patent application EP 2 256 149 with their method of preparation, and the OLAs marketed by the company Condensia Quimica under the brand name Glyplast®, in particular the references Glyplast® OLA 2, which has a molecular weight of 500 to 600 g / mol and Glyplast® OLA 8 which has a molecular weight of 1000 to 1100 g / mol.According to a preferred embodiment of the invention, the OLAs have a molecular weight of at least 900 g / mol, preferably from 1000 to 1400 g / mol, more preferably from 1000 to 1100 g / mol.

[0062] Citrate esters are also plasticizers known to those skilled in the art as bio-sourced materials. Examples include triethyl citrate (TEC), triethyl acetyl citrate (TEAC), tributyl citrate (TBC), tributyl acetyl citrate (TBAC), preferably TBAC.

[0063] Compatibilizers may be included in the composition of the multilayer article according to the invention. Such PLA / Polyester compatibilizers are well known to those skilled in the art, in particular molecules having the epoxy, acrylate, anhydride, oxazoline and lactam functions which allow grafting reactions.

[0064] Among the compatibilizers, mention will be made more particularly of polyacrylates, terpolymers of ethylene, acrylic ester and glycidyl methacrylate (for example marketed under the brand name Lotader® by the company Arkema), triblock copolymers PLA-PBAT-PLA, PLA grafted with maleic anhydride (PLA-g-AM) or PBAT grafted with maleic anhydride (PBAT-g-AM).

[0065] Mineral and / or vegetable fillers can also be used in the com position of the multilayer article of the invention, the mineral fillers preferably used are calcium carbonate or talc.

[0066] The vegetable fillers preferably used are starch and wood fibers and flour.

[0067] Composition of layer C:

[0068] The barrier materials constituting the layers C are well known to those skilled in the art, and in particular PVOH (polyvinyl alcohol), EVOH (Poly(vinyl alcohol-co-ethylene)), PVCD (polyvinyl chloride), PGA (polyglycolic acid), cellulose and its derivatives, or polysaccharides and their mixtures in all proportions, cited above for those which can also be included in the composition of layer A and / or layer B.

[0069] The PVOH used as a barrier material in the preparation of the article is well known. It is polyvinyl alcohol with a degree of polymerization between 300 and 2500. Its melting point is less than 210°C and its viscosity is between 3 and 60 mPa.s.

[0070] The PVCD used as a barrier material in the preparation of the article is also well known. It is polyvinylidene chloride resulting from the copolymerization of vinylidene chloride (85%) and vinyl chloride (15%).

[0071] The PGA used as barrier material in the preparation of the article corresponds to polyglycolic acid whose melting temperature is 220°C and whose glass transition temperature is 40°C.

[0072] Among the celluloses, microfibrillated celluloses (MFC) and cellulose acetate will be mentioned more particularly.

[0073] The MFCs used as barrier material have a diameter between 4 and 10006 nm and a density between 0.51 and 1.57 g / cm3.

[0074] The polysaccharides used as barrier materials are also well known to those skilled in the art. Mention will be made more particularly of galactomannans, pectin or soluble soy polysaccharides, marine extracts such as carrageenans and alginates, and microbial or animal polysaccharides such as gellans, dextrans, xanthans, xylans or chitosan, and mixtures thereof.

[0075] Advantageously, the rate of biosourced material for producing the article according to the invention is greater than 30%, preferably greater than 40%.

[0076] As for layer A and / or layer B, layer C may also comprise additives usual in the preparation of plastic articles, as defined previously.

[0077] According to a preferred embodiment of the invention, the composition of layer C is as follows: - 90 to 100% of barrier materials as defined previously, and - 0 to 10% additives.

[0078] Preferably, layer C comprises more than 95% barrier material, even more preferably 99% or more.

[0079] PVOH is a preferred barrier material for the C layers of the articles according to the invention.

[0080] Articles

[0081] According to the invention, the plastic article is a manufactured product, such as rigid or flexible packaging, agricultural films, bags and sacks, disposable articles or the like. Preferably, the article is made of thermoplastic material. The plastic articles according to the invention may contain additional substances or additives, such as slip agents, plasticizers, mineral or organic fillers.

[0082] The multilayer article according to the invention advantageously has a thickness greater than or equal to approximately 20 μm, preferably greater than or equal to approximately 25 μm, more preferably greater than or equal to approximately 50 μm, more preferably greater than or equal to approximately 450 μm, more preferably greater than 750 μm, preferably less than 5000 μm.

[0083] According to the invention, the plastic article can be chosen from a flexible plastic article or a rigid plastic article.

[0084] According to one embodiment, the multilayer article according to the invention is a flexible article, in particular a plastic film.

[0085] The flexible multilayer article according to the invention advantageously has a thickness of less than 250 μm, preferably ranging from 20 to 100 μm, preferably from 25 to 80 μm, more preferably from 30 to 60 μm, even more preferably around 50 μm.

[0086] Examples of plastic films include agricultural films, plastic bags or sachets, films for flexible packaging, food films, lids, packaging blisters, mailing films, routing films, mulching films, liner films, grouping films (known as "multipack films"), industrial films, personal care films, nets, etc.

[0087] The multilayer article according to the invention also relates to a film comprising a flexible multilayer article, preferably a multilayer article as defined above.

[0088] According to another embodiment, the multilayer article according to the invention is a rigid article.

[0089] Examples of rigid plastic articles are thin-walled packaging such as food and beverage packaging, boxes, trays, containers, catering items, electronic housings, cosmetic cases, outdoor gardening items such as pots, rigid packaging, containers, cups, plates, beverage caps, trays, packaging blisters, cards, cotton buds, irrigation products, pipes, etc. Some rigid plastic items may be produced by thermoforming plastic sheets with a thickness of 150 µm or more, such plastic sheets being produced by film casting or calendering.

[0090] The rigid multilayer article according to the invention advantageously has a thickness greater than 150 μm, preferably less than 5000 μm.

[0091] According to a preferred embodiment of the invention, the thickness of the multilayer article ranges from 150 to 3000 μm.

[0092] The invention also relates to a sheet comprising a multilayer article according to the invention, preferably a rigid multilayer article as defined above.

[0093] Advantageously, the thickness of the multilayer rigid article is less than 5000 μm, preferably between 400 and 800 μm, preferably between 400 and 500 μm, more preferably equal to approximately 450 μm. Alternatively, the thickness of the multilayer rigid article is equal to approximately 750 μm.

[0094] According to certain preferred embodiments, the multilayer article is of type AB A or B AB. Preferably, the multilayer article is of type AB A.

[0095] The relative thickness of each layer of the article AB, AB A, ABC, BAB, BAC, ABCA BACB, BCACB or ACBCA according to the invention may vary according to the final properties sought for the article, in particular in terms of water barrier property but also in terms of biodegradability. According to one embodiment of the invention, the thickness of layer A or B is between 10 and 725 μm, between 18 and 30 μm, preferably equal to approximately 25 μm.

[0096] Advantageously, each layer A independently represents from 5 to 30% of the total thickness of the article and the central layer B represents from 40 to 90% of the total thickness of the article. Preferably, the central layer B represents from 50 to 90% of the total thickness of the article.

[0097] In a preferred embodiment of the flexible article of the invention, the two layers A have an identical thickness, each representing from 15 to 30% of the total thickness of the article, preferably from 16 to 25%.

[0098] In a preferred embodiment of the rigid article of the invention, the two layers A have an identical thickness, each representing from 2 to 20% of the total thickness of the article, preferably from 3 to 15%.

[0099] According to certain embodiments, the flexible multilayer article is of type AB, AB A, ABC, ABCA, ACBCA and in which each layer A represents from 15 to 30% of the total thickness of the film and the central layer B represents from 40 to 70% of the total thickness of the film.

[0100] According to certain embodiments, the flexible multilayer article is of type AB, BAB, BAC, BACB, or BCACB and in which layer B represents from 15 to 30% of the total thickness of the film and the central layer A represents from 40 to 70% of the total thickness of the film.

[0101] The C layers, when present, generally have a thickness of less than 15 μm. They individually represent less than 15% of the total thickness of the article.

[0102] According to a particular embodiment of the invention, the layers C, when present, of the multilayer flexible articles have a thickness of less than 3 μm. They individually represent less than 30% of the article.

[0103] According to a particular embodiment of the invention, the layers C, when present, of the multi-layer rigid articles have a thickness of less than 20 μm. They individually represent less than 30% of the article.

[0104] The multilayer article of the invention may also be applied to a support of a different nature, such as a biodegradable film, paper or the like. For example, the multilayer article of the invention may be bonded by lamination to a biodegradable film to enhance its water barrier properties.

[0105] Preparation of the article

[0106] Another subject of the invention relates to a method for preparing a multilayer article according to the invention. The compositions of layers A, B and C are prepared by the usual techniques for preparing polymer compositions. The preparation of the articles is carried out by mixing the different constituents, then shaping the article according to the desired shape, flexible or rigid article.

[0107] According to the invention, the enzymes having PLA degradation activity are added in a suitable form to allow a homogeneous dispersion of said enzymes in the multilayer article. These enzymes can be added directly to the polymers of layer A and / or layer B during its preparation, or in the form of a concentrated premix in a low-melting point support polymer.

[0108] According to a particular embodiment of the multilayer article according to the invention, the method comprises the following steps:

[0109] a) Providing enzymes having polyester degrading activity in a form suitable for enabling homogeneous dispersion of said enzymes in the multilayer article, said form being selected from

[0110] - a liquid composition comprising enzymes having degrading activity PLA, water and optionally a polysaccharide support, or

[0111] - a masterbatch comprising enzymes having a degradation activity of PLA and a carrier polymer having a melting temperature below 140°C and / or a glass transition temperature below 70°C, and

[0112] b) Mixing the enzymes having PLA degrading activity provided in step (a) with the polymers of layer A and / or layer B, and

[0113] c) The formatting of the article.

[0114] A person skilled in the art will be able to prepare the multilayer article according to the invention, by any usual techniques which allow their bonding, such as coextrusion, co-injection, rolling. Preferably, the article is prepared by coextrusion of the layers, a person skilled in the art being able to determine the conditions for implementing the process, and in particular the mixture of the components entering into the composition of each of the layers. Advantageously, the coextrusion is carried out at a temperature below 200°C.

[0115] According to a first embodiment, the enzymes are provided in the form of a liquid composition comprising the enzymes having PLA degradation activity, water and optionally a polysaccharide support. Such liquid compositions and their use for the preparation of enzymatic polymer mixtures are described in particular in applications WO 2019 / 043145 and WO 2019 / 043134.

[0116] The content of enzymatic composition in layer A and / or B will depend in particular on the content of enzymes in the enzymatic composition and the desired enzyme content for the article. According to a particular embodiment, from 1 to 10% by weight relative to the total weight of the composition of the multi-layer article will be used.

[0117] According to a second embodiment, the enzymes are provided by a master mix.

[0118] The masterbatch is a concentrated premix of enzymes and a carrier polymer.

[0119] The support polymer is a polymer having a melting temperature below 140°C and / or a glass transition temperature below 70°C.

[0120] Polymers having a melting temperature below 140°C and / or a glass transition temperature below 70°C are well known to those skilled in the art. These are in particular polycaprolactone (PCL), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polyhydroxyalkanoate (PHA), polylactic acid (PLA), or their copolymers. It may also be a natural polymer such as starch or a polymer that will be described as universal, i.e. compatible with a wide range of polymers such as an EVA-type copolymer. Advantageously, the support polymer has a melting temperature below 120°C and / or a glass transition temperature below 30°C.

[0121] The support polymer is preferably chosen from PCL, PBSA, PBAT, PHA, PLA and their mixtures in all proportions, in particular PCL.

[0122] Preferably, the masterbatch also comprises a polysaccharide.

[0123] The polysaccharides are in particular chosen from starch derivatives such as amylose, amylopectin, maltodextrins, glucose syrup, dextrins and cyclodextrins, natural gums such as gum arabic, gum tragacanth, guar gum, locust beam gum, karaya gum, mesquite gum, galactomannans, pectin or soluble soy polysaccharides, marine extracts such as carrageenans and alginates, and microbial or animal polysaccharides such as gellans, dextrans, xanthans or chitosan, and mixtures thereof. A preferred polysaccharide is gum arabic.

[0124] In this case, the composition of the multilayer article according to the invention will also comprise a polysaccharide.

[0125] A preferred masterbatch composition comprises from 50 to 95% of a low melting point polymer, in particular polycaprolactone (PCL), preferably from 70 to 90%, from 0.001 to 10% of enzymes, preferably from 1 to 6%, and from 1 to 30% of gum arabic, preferably from 10 to 25%.

[0126] Such masterbatches and their preparation processes are described in particular in patent applications WO 2019 / 043134, WO 2021 / 148665 or in French patent application No. 2107809 filed on 07 / 20 / 2021.

[0127] According to a particular embodiment of the invention, the article comprises - from 80 to 99% of constituent polymer, preferably from 90 to 99% - from 0 to 40% of polysaccharide, preferably from 0.1 to 4% - from 0 to 40% of a support polymer, preferably from 3 to 6% and - from 0.005 to 10% of enzymes, preferably from 0.01 to 5%, more preferably initially from 0.01 to 3%.

[0128] According to a more particular embodiment of the invention, the enzyme content in the above composition ranges from 0.02 to 1%.

[0129] According to another embodiment, the article is prepared by shaping a premix or “compound” consisting of the composition of the article defined previously.

[0130] The premix is ​​prepared according to the method described above, with granulation for shaping step c) using standard methods.

[0131] The invention therefore also relates to a premix in the form of granules comprising - less than 60% of PHA (polyhydroxyalkanoate), PLA - at least 0.001% of enzymes capable of degrading said polyester, and - at least one complementary thermoplastic polymer, in all variant embodiments previously described for the article.

[0132] According to a particular embodiment, layer A and / or layer B comprises, in addition to the polymers which constitute it, enzymes, a support polymer and a polysaccharide as defined above.

[0133] According to a particular embodiment of the invention, layer A or layer B consists essentially of the above enzymatic composition (the support polymer is also the constituent polymer). The composition can be supplemented by usual additives described above.

[0134] According to a particular embodiment of the invention, the constituent polymer(s) of layer B according to the invention have a melting temperature lower than that of the constituent polymers of layer A.

[0135] Use of Articles

[0136] The invention also relates to various uses of the multilayer articles obtained according to the invention, in particular flexible or rigid multilayer articles.

[0137] The multilayer article according to the invention can be used for all usual uses of thermoplastic articles, and in particular for the preparation of packaging or bags, or for mulching or routing. It can also be used for the preparation of disposable tableware (plates, glasses), packaging (trays, blisters) or beverage capsules.

[0138] The various embodiments, variants, preferences and advantages described above for each of the objects of the invention apply to all of the objects of the invention and may be taken separately or in combination.

[0139] The invention is illustrated by the following examples given without limitation. EXAMPLES.

[0140] I. Preparation of a mix of support polymer and enzyme

[0141] The mix of support polymer and enzyme is prepared from polyca-prolactone (PCL) granules and the enzyme in liquid form as described in application WO 2019 / 043134.

[0142] The mix of support polymer and enzyme was manufactured with a CLEXTRAL EV25HT twin-screw extruder comprising 11 zones for which the temperature is independently controlled and regulated. The PCL is introduced into zone 1 at 16 kg / h and the enzyme solution into zone 5 at 4 kg / h using a peristaltic pump. The zones are heated according to table [1]. 20% of the enzyme solution is introduced into the PCL (% by weight relative to the total weight).

[0143] [Table 1]: Temperature profile (°C) used for the polymer support and enzyme mix Zone ZI Z2 Z3 Z4 Z5 Z6 Z7 Z8 Z9 Z10 Zll Temperature 40 65 75 75 60 60 60 60 60 60 60

[0144] II. Commercial products

[0145] In these examples, PHBV marketed under the reference ENMAT™ Y1000P by the company Helian Polymers, PHBH marketed under the reference Green PLlanet™X128 by the company KANEKA, PLA / PBAT blends marketed under the references Eco vio® F2331, Eco vio® F2332, Eco vio® F2223 and a slip agent under the reference Ecoflex® SL-05 marketed by BASF, PLA marketed under the reference Luminy® LX175 by the company Total Corbion.

[0146] III. Film production

[0147] For the preparation of multilayer films, a Eurexma three-layer coextrusion inflation line was used, width 275 - 300 mm and screw of L / D = 30. The inflation rate was approximately 3.5 - 3.9. The settings and temperatures are detailed in tables [2] to [4].

[0148] [Tables 2]: Process parameters for a 50pm film with a distribution of layers A / B / A 25 / 50 / 25 Temperatures Sector ZI Z2 Z3 Z4 ZI Z2 FIL A interior Actual Setpoint 165 130 165 135 165 135 170 140 140 150 140 155 140 160 B central Actual Setpoint 175 175 170 175 140 165 140 165 A exterior Actual Setpoint 175 175 170 175 140 165 140 165

[0149] [Tables 3]: Extruder process parameters Internal screw A Central screw B External screw A Screw speed (RPM) 35 30 35 Screw motor current (A) 2.9 8 2.9 Pressure (bars) 60 80 45

[0150] [Tables 4]: Extruder process parameters Drawing speed (m / min) 2.5 Reel speed (m / min) 2.7 Ventilation (RPM) 60

[0151] IV. Method of analysis

[0152] The water barrier properties of the films were evaluated with a permeability test according to the following protocol: films of dimensions 30x8cm are folded in half lengthwise and welded on three ends to form a sachet which is then filled with 20.0g of water. The sachet is then welded on its last side to form a hermetic pocket and is laid flat for 7 days. The mass of the sachet is determined every day for one week in order to obtain an average water loss in g / d.

[0153] The evaluation of the biodegradability of the films was evaluated with a depolymerization test carried out according to the following protocol: 100 mg of each sample was introduced into a plastic vial containing 50 mL of buffer solution at pH 9.5. The depolymerization is initiated by incubating each sample at 45°C, in an incubator shaken at 150 RPM. An aliquot of 1 mL of buffer solution is taken regularly and filtered using a 0.22 pm filter syringe in order to be analyzed by high performance liquid chromatography (HPLC) with an Aminex HPX-87H column to measure the release of lactic acid (LA) and its dimer. The chromatography system used is an Ultimate 3000 UHPLC System (Thermo Fisher Scientific, Inc. Waltham, MA, USA) comprising a pump, an autosampler, a column thermostated at 50°C and a UV detector at 220nm. The eluent is 5 rnM H2 SO4. The injection is 20 pL of sample.Lactic acid is measured from standard curves prepared from commercial lactic acid.

[0154] The hydrolysis of plastic films is calculated from the lactic acid and the released lactic acid dimer. The percentage of depolymerization is calculated after 7 days with respect to the percentage of PLA in the sample.

[0155] Results

[0156] VII. Composition of films and results

[0157] The ABA type films were prepared with the support polymer and enzyme mix prepared in I, PHA, PLA, a PLA / PBAT mixture.

[0158] According to the examples below in accordance with the invention, the support polymer and enzyme mix prepared in I is present either in layers A, or in layer B or in layers A and B.

[0159] The composition of the outer A layers of films 11 to 17 further contains 2% of a slip agent of stearate type SL-05.

[0160] The thickness of the films produced is 50 μm and the relative thicknesses of each layer A / B / A are 25% / 50% / 25%.

[0161] The compositions of these different films are listed in table [5] below. below.

[0162] [Tables 5]: The compositions of these different films produced Couche A (interne et externe) Couche B (centre) Répartition couches % 25 50 Film 10 Ecovio® F2223 Ecovio® F2223 Film 11 73% Ecovio® F2331 + 25% ENMAT™ Y1000P (PHBV) 90% Ecovio® F2223 + 10% mix I Film 12 73% Ecovio® F2331 + 25% ENMAT™ Y1000P (PHBV) 65% Ecovio® F2223 + 25% ENMAT™ Y1000P (PHBV) + 10% mix I Film 13 73% Ecovio® F2331 + 25% ENMATTM Y1000P (PHBV) 65% Ecovio® F2332 + 25%ENMATTM Y1000P (PHBV) + 10% mix I Film 14 73% Ecovio® F2332 + 25% ENMATTM Y1000P (PHBV) 65% Ecovio® F2332 + 25% ENMATTM Y1000P (PHBV) + 10% mix I Film 15 63% Ecovio® F2223 + 25% ENMATTM Y1000P (PHBV) + 10% mix I 75% Ecovio® F2331 + 25% ENMATTM Y1000P (PHBV) Film 16 68% Ecovio® F2223 + 25% ENMATTM Y1000P (PHBV) + 5% mix I 70% Ecovio® F2331 + 25% ENMATTM Y1000P (PHBV) + 5% mix I Film 17 63% Ecovio® F2331 + 35% ENMATTM Y1000P (PHBV) Ecovio® F2223 + 15% ENMATTM Y1000P (PHBV) + 10% mix I Film 18 75% Ecovio® F2223 + 25% GREEN PLLANETTM X128 (PHBH) 65% Ecovio® F2223 + 25% Green PLlanet™X128 (PHBH) + 10% mix I

[0163] Compositions with a PHA content above 60% were difficult to extrude to obtain multilayer films and have a very sticky appearance of the material which destabilizes the bubble and prevents the opening of the sheaths.

[0164] Film 10 is a comparative example.

[0165] The properties of films 11 to 18 prepared above were measured according to the protocols defined above.

[0166] The results of these measurements are given in Table 6 below.

[0167] [Tables 6]: Results of the measurements carried out Film Biodegradability (%PLA depolymerized after 7 days) Water barrier properties (water loss g / d) 10 0% 1.8 11 1.5% 0.40 12 3% 0.33 13 3% 0.25 14 1% 0.27 15 30% 0.61 16 30% 0.80 17 5% 0.35 18 1% 0.60

[0168] It is thus demonstrated that the polymer blend according to the invention leads to improved water barrier properties compared to a film without PHA. PHBV makes it possible to improve the barrier properties in PLA / PHA blends more significantly than PHBH.

Claims

Claims

1. Biodegradable multilayer article of type AB, AB A, ABC, BAB, BAC, ABCA BACB, BCACB or ACBCA, in which - layer A comprises at least PHA (polyhydroxyalkanoate) in an amount between 5 and 50% and PLA (polylactic acid); - layer B comprises at least one thermoplastic polymer; and - layer A and / or layer B comprises at least 0.001% of enzymes capable of degrading said PLA, the percentage being given by weight relative to the total weight of the composition of each layer.

2. Multilayer article according to claim 1, characterized in that the polymers of layer B are polyesters chosen from PLA (polylactic acid), PBAT (polybutylene adipate terephthalate), PHA (polyhydroxyalkanoate), PBS (polybutylene succinate), PCL (polycaprolactone), PBSA (polybutylene succinate adipate) and mixtures thereof.

3. Multilayer article according to claim 1 or 2, characterized in that the PHA content is between 10% and 45% by weight, more preferably between 20% and 40%, even more preferably between 20% and 35% by weight relative to the total weight of the composition of each layer.

4. Multilayer article according to any one of claims 1 to 3, characterized in that the PLA content is between 2% and 90% by weight, preferably between 3% and 80%, between 4% and 70%, between 5% and 60%, more preferably between 5% and 40% by weight relative to the total weight of the composition of each layer.

5. A multi-layer article according to any one of claims 1 to 4, wherein layer A further comprises complementary polyesters selected from PBAT (polybutylene adipate terephthalate), PBS (polybutylene succinate), PCL (polycaprolactone), PBSA (polybutylene succinate adipate), plasticized starch and mixtures thereof in all proportions.

6. A multi-layer article according to claim 5, wherein the content of complementary polyesters is between 10% and 90%, preferably between 20% and 80%, more preferably between 30 and 75%, even more preferably 40% and 70% by weight relative to the total weight of the composition of each layer.

7. A multi-layer article according to any one of claims 1 to 6, wherein layer A further comprises PB AT as a complementary polyester.

8. Multilayer article according to any one of claims 1 to 7, characterized in that it comprises, by weight relative to the total weight of the composition of the article: i) 10% to 35% of PHA, preferably between 12.5 and 25% ii) 10% to 50% of PLA, preferably between 15 and 30% iii) 50% to 60% of PBAT, preferably between 52 and 56% iv) 0.8% to 8% of PCL, preferably 4% v) at least 0.001% of enzymes capable of degrading said PLA.

9. Article according to the preceding claim, characterized in that it further comprises a polysaccharide.

10. A multilayer article according to any one of claims 1 to 9, wherein the PHA is selected from the group consisting of PHBV (Poly(3-hydroxybutyrate-co-3-hydroxyvalerate), PHBH (poly3-hydroxybutyrate-co-3-hydroxyhexanoate), PHB (poly-[3-hydroxybutyrate), PHH (polyhydroxyhexanoate), P3HP (poly 3-hydroxypropionate), P3HB (poly 3-hydroxybutyrate), P4HB (poly 4-hydroxybutyrate), P4HV (poly 4-hydroxyvalerate), P5HV (poly 5-hydroxyvalerate), PHB3HP (poly 3-hydroxybutyrate-co-3-hydroxypropionate), P3HB4HB (poly 3-hydroxybutyrate-co-4-hydroxybutyrate), PHB4HV (poly 3-hydroxybutyrate-co-4-hydroxyvalerate), PHB3HV (poly 3 -hydro xybutyrate-co-3 -hydro xyvalerate), PHB3HH (poly 3 -hydro xy-butyrate-co-3 -hydroxyhexanoate), PHB5HV (poly 3-hydroxybutyrate-co-5-hydroxyvalerate and mixtures thereof in all proportions.

11. Multilayer article according to any one of claims 1 to 10, characterized in that layer A and / or layer B further comprises at least one additive chosen from slip agents, plasticizers, nucleating agents, compatibilizers, manufacturing aids, UV radiation stabilizers, anti-shock agents, mineral or vegetable fillers.

12. Multilayer article according to claim 11, characterized in that the content of additive, preferably a slip agent, is between 0.2 and 5% by weight, preferably 2% by weight.

13. Multilayer article according to any one of claims 1 to 12, characterized in that layer C, when present, comprises barrier materials chosen from PVOH (polyvinyl alcohol), EVOH (Poly(vinyl alcohol-co-ethylene)), PVCD (polyvinyl chloride), PGA (polyglycolic acid), cellulose or polysaccharides and mixtures thereof in all proportions.

14. Multilayer article according to one of claims 1 to 13, characterized in that it has a thickness greater than or equal to approximately 25 pm, approximately 50 pm, approximately 450 pm, approximately 750 pm and less than or equal to 5000 pm.

15. Multilayer article according to one of claims 1 to 13, characterized in that the thickness of layer A or layer B is between 10 and 725 pm, between 18 and 30 pm, preferably equal to approximately 25 pm.

16. Sheet, characterized in that it comprises a multi-layer article according to claims 1 to 15.

17. Sheet, in particular a tray, according to claim 16, characterized in that it has a thickness of less than 5000 pm, preferably between 400 and 800 pm, more preferably equal to approximately 450 pm or equal to approximately 750 pm.

18. Film, characterized in that it comprises a multilayer article according to any one of claims 1 to 15.

19. Film according to claim 18, characterized in that it has a thickness ranging from 20 to 100 pm, preferably from 25 to 80 pm, more preferably from 30 to 60 pm, even more preferably around 50 pm.

20. Use of a multilayer article according to any one of claims 1 to 13, for the preparation of a packaging, a lid, a cup, a plate, a beverage capsule, a tray or a packaging blister.