FIBROUS PREFORM AND ITS MANUFACTURING PROCESS FOR PRODUCING A PART IN CERAMIC MATRIX COMPOSITE MATERIAL

A sacrificial silicon carbide layer with fine grains addresses the corrosion issue in CMC material production, ensuring the pre-densified layer's integrity and improving mechanical properties.

FR3141164B1Active Publication Date: 2024-10-04SAFRAN CERAMICS SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022010914
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-10-04
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Existing CMC material manufacturing processes face issues with corrosion of the pre-densified layer by liquid silicon during melt infiltration, leading to crack formation and degradation of mechanical properties due to random corrosion at grain boundaries.

Method used

Incorporation of a sacrificial silicon carbide layer with finer grains and increased grain boundary surface area to block the degradation of the pre-densified layer by liquid silicon, forming a tortuous path to limit infiltration and propagation.

Benefits of technology

The sacrificial layer effectively protects the pre-densified layer and interphase layer from liquid silicon attack, enhancing the mechanical performance and durability of the CMC material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000016_0000
    Figure 00000016_0000
  • Figure 00000016_0001
    Figure 00000016_0001
  • Figure 00000016_0002
    Figure 00000016_0002
Patent Text Reader

Abstract

The invention relates to a fibrous preform (1) for the production of a part (10) in ceramic matrix composite material, the fibrous preform comprising: - a fibrous reinforcement (2) comprising silicon carbide-based fibers (20), - an interphase layer (3) extending around a surface of each of said silicon carbide-based fibers (20), preferably the interphase layer (3) being boron nitride-based, - a pre-densified layer (4) comprising silicon carbide, located on the interphase layer and having a columnar microstructure, said pre-densified layer having a thickness of between 3 µm and 20 µm, and - a sacrificial layer (7) located on said pre-densified layer, said sacrificial layer comprising silicon carbide having grains of an average size of between 0.1 µm and 0.5 µm. Figure for the abbreviation: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: FIBROUS PREFORM AND ITS MANUFACTURING METHOD FOR PRODUCING A PART MADE OF CERAMIC MATRIX COMPOSITE MATERIAL Technical field

[0001] The invention relates to the general field of manufacturing parts made of ceramic matrix composite material, in particular based on silicon carbide. More particularly, the invention relates to a fiber preform for producing a part made of ceramic matrix composite material. The invention also relates to a method for manufacturing such a fiber preform and such a part made of ceramic matrix composite material. Technical background

[0002] Ceramic matrix composite (CMC) materials have good thermo-structural properties, i.e. high mechanical properties which make them suitable for forming structural parts and the ability to retain these properties at high temperatures (in particular up to 1200°C and even beyond) and in an oxidizing environment.

[0003] The use of CMC materials instead of metallic materials is advantageous in the aeronautical field, such as in aircraft turbomachines. Indeed, these CMC materials are relatively light compared to metallic materials and are suitable for use at higher temperatures than the latter.

[0004] Generally, a CMC material is a ceramic matrix into which ceramic fibers (or filaments) are incorporated. The CMC material may be carbide-based, such as silicon carbide (SiC) fibers or carbon (C) fibers which may be reinforced with a silicon carbide matrix, or any other non-oxide ceramic fibrous reinforcement with a non-oxide ceramic matrix.

[0005] A method for manufacturing CMC materials, in particular reinforced with silicon carbide fibers, comprises the production of a fiber preform whose shape is close to that of the part to be manufactured, followed by the densification of this fiber preform by a matrix.

[0006] [Fig. 1] represents an example of a process for producing a part from CMC material. For this, the process comprises the following steps: (a) production of a fibrous reinforcement 2 comprising silicon carbide fibers 20, (b) coating the fibers 20 of the fibrous reinforcement with an interphase layer 3, (c) formation of a so-called pre-densified layer 4 of silicon carbide on the interphase layer 3 by chemical vapor infiltration (also designated by the English term "Chemical Vapor Infiltration" CVI) to form a fibrous preform 1, (e) incorporation of a silicon carbide powder into the porosity of the fiber preform 1, (f) densification of the fiber preform 1 obtained in step (e) by infiltration in the molten state of a ceramic matrix 6 (also designated by the English term “Melt Infiltration” MI), in particular with liquid silicon, to form the part in CMC material.

[0007] The fiber preform 1 formed in step (c) therefore comprises: - the fibrous reinforcement 2 comprising fibers 20 based on silicon carbide, - the interphase layer 3 surrounding a surface 22 of the fiber 20, - the pre-densified layer 4 at least partially coating the interphase layer 3.

[0008] The interphase layer 3 may be based on boron nitride (BN). The interphase layer 3 coating the fibers 20 makes it possible to optimize the bond between the fibers 20 and the matrix 6 of the CMC material part. Indeed, this interphase layer 3 makes it possible to have a sufficient bond to ensure transfer to the fiber reinforcement of the mechanical stresses to which the CMC material part is subjected. The interphase layer 3 thus makes it possible to deflect the cracks generated within the matrix 6.

[0009] The silicon carbide of the pre-densified layer 4 has a microstructure composed of grains which grow in a preferred direction during the CVI deposition until they form a columnar microstructure of silicon carbide. In such a columnar microstructure, the largest dimension of the grains is their radial dimension, that is to say that extending between the fiber 20 and the external surface of the pre-densified layer 4. This pre-densified layer 4 also makes it possible to protect the fibers 20 and the interphase layer 3 by consolidating them in a predefined shape by a first level of densification.

[0010] The incorporation of the silicon carbide powder 5 makes it possible to limit the reactivity of the liquid silicon on the pre-densified layer 4 during step (f). The powder mixture 5 also makes it possible to fractionate the porosity of the fibrous preform 1 to facilitate the capillary rise of the liquid silicon in this fibrous preform 1 during step (f).

[0011] Finally, the melt infiltration technique provides a second level of densification to plug the porosity of the fiber preform 1. Step (f) makes it possible to densify and form the part in CMC material, while also protecting the fibers 20 and the matrix 6.

[0012] Although the chemical interaction between the liquid silicon and the pre-densified layer 4 is limited (in particular by steps (c) and (e)), the method described above is not fully satisfactory. Indeed, even in the presence of the carbide powder 5 silicon, corrosion of the pre-densified layer 4 by liquid silicon can be observed randomly on the pre-densified layer. This corrosion is mainly observed at the grain boundaries of the pre-densified layer and propagates along them. Due to the columnar microstructure of the pre-densified layer, and the preferential propagation along the grain boundaries, the corrosion can lead to the formation of crevices extending in the radial direction of the fiber, i.e. from the free surface of the pre-densified layer to the fiber of the fiber reinforcement. The presence of such crevices can alter the mechanical properties and the service life of the CMC material part.

[0013] These crevices are designated by arrows in [Fig.2]. They explain a deep degradation on the pre-densified layer up to the interphase layer. Liquid silicon can infiltrate between the columns of the pre-densified layer. Therefore, the deposition of the pre-densified layer on the interphase layer may have limited effectiveness in protecting this interphase layer during infiltration by liquid or molten silicon.

[0014] There is therefore a need to optimize the manufacture of parts made of CMC material by limiting the reactivity of liquid silicon with respect to silicon carbide deposited by CVI prior to the densification operation by ML. Summary of the invention

[0015] The present invention provides a simple, effective and economical solution to the aforementioned drawbacks of the prior art.

[0016] To this end, the invention relates to a fiber preform for producing a part from a ceramic matrix composite material, the fiber preform comprising: - a fibrous reinforcement comprising silicon carbide-based fibers, - an interphase layer extending around a surface of each of said silicon carbide-based fibers, preferably the interphase layer being boron nitride-based, - a pre-densified layer comprising silicon carbide, located on the interphase layer and having a columnar microstructure, said pre-densified layer having a thickness of between 3 pm and 20 pm.

[0017] According to the invention, the fiber preform further comprises a sacrificial layer located on said pre-densified layer, said sacrificial layer comprising silicon carbide having grains with an average size of between 0.1 μm and 0.5 μm.

[0018] A fiber preform is understood to mean an intermediate part for producing a part made of CMC material. This fiber preform can be said to be “pre-densified” since it has a first level of densification. Indeed, the fiber preform comprises a layer pre-densified by a silicon carbide pre-densification phase deposited by CVI.

[0019] The main advantage of the fiber preform according to the invention is that it significantly reinforces the protection of the pre-densified layer, the interphase layer and the fiber reinforcement against attack by liquid silicon during the production of this fiber preform.

[0020] For this, the fiber preform comprises a sacrificial layer of silicon carbide on the pre-densified layer so that this sacrificial layer, forming an external surface of the fiber preform, blocks the degradation of the pre-densified layer (and the interphase layer and the fiber) by the liquid silicon.

[0021] By the term "sacrificial" is meant a portion (or an area) of this sacrificial layer which is non-functional and therefore configured to be degraded first by the liquid silicon.

[0022] In particular, the sacrificial layer has a silicon carbide grain size smaller than the size of the columnar microstructure of the pre-densified layer. This makes it possible to form a fine-grained microstructure of the sacrificial layer compared to the columnar microstructure of the pre-densified layer. The sacrificial layer is therefore enriched in carbon (compared to the pre-densified layer). Indeed, the small grain size of the sacrificial layer makes it possible to increase the grain boundary surface in this sacrificial layer, the carbon of which can react with the liquid silicon and the sacrificial layer thus preserves the underlying layer (namely the pre-densified layer) from the reactivity of the liquid silicon.Furthermore, the fine grain microstructure of the silicon carbide of the sacrificial layer makes it possible to create tortuosity (i.e. a tortuous / sinuous path, in the form of a labyrinth) so as to limit the infiltration and propagation of liquid silicon towards the layers under the sacrificial layer. Consequently, the fibrous preform according to the invention has very good resistance to the chemical reactivity of liquid silicon and improves the mechanical performance of the CMC material part to be produced from this fibrous preform.

[0023] The fiber preform may comprise one or more of the following features, taken in isolation from one another or in combination with one another:

[0024] - said at least one sacrificial layer has a grain density greater than that of the pre-densified layer by a factor of between 20 and 40;

[0025] - said at least one sacrificial layer has a thickness of between 1 and 4 pm ;

[0026] - several sacrificial layers are superimposed on each other and extend on said pre-densified layer, the number of these sacrificial layers being at most five ;

[0027] — the columnar microstructure of the pre-densified layer has SiC grains in cylindrical form preferably having a height which is greater than or equal to 3 qm and / or a width between 0.2 pm and 1 qm;

[0028] — the pre-densified layer has a thickness of between 10 and 20 pm.

[0029] The invention also relates to a part made of ceramic matrix composite material comprising a fiber preform according to any one of the preceding claims, and a densified ceramic matrix, said ceramic matrix preferably being based on silicon carbide.

[0030] The part made of CMC material may be a part of a turbomachine, in particular an aircraft part. For example, this turbomachine part is a blade of a turbine or a compressor of the turbomachine, an annular wall of a combustion chamber of the turbomachine, etc.

[0031] The invention also relates to a method for manufacturing a fiber preform according to one of the features of the invention. This fiber preform is intended to produce a part made of ceramic matrix composite material according to the invention. This method comprises the steps consisting of: (a) obtaining the fibrous reinforcement comprising silicon carbide-based fibers, (b) forming the interphase layer on each of the surfaces of the silicon carbide-based fibers, (c) forming the pre-densified layer on said interphase layer by chemical vapor infiltration (CVI), to obtain said fibrous preform, and (d) depositing at least one sacrificial layer based on silicon carbide on said pre-densified layer obtained in step (c) by chemical vapor infiltration (CVI).

[0032] As mentioned previously, the sacrificial layer coating the pre-densified layer of the fiber preform makes it possible to block the degradation of the pre-densified layer by the liquid silicon. For this, one or more parameters of the CVI deposition of the silicon carbide can be modified to move from a columnar microstructure of the silicon carbide grains of the pre-densified layer to a crystallized microstructure of the silicon carbide grains of the sacrificial layer. The method for obtaining the fiber preform of the invention thus makes it possible to achieve the objective mentioned above by modifying the parameters of an existing CVI deposition step of the method for manufacturing a part made of CMC material.

[0033] At the end of step (c) and step (d), the fiber preform is said to be “pre-densified” because a first level of densification or pre-densification in silicon carbide deposited by CVI is carried out.

[0034] The method of manufacturing the fiber preform may comprise one or more of the following characteristics, taken in isolation from each other or in combination with each other:

[0035] - the chemical vapor infiltration of step (c) is carried out by a first gas mixture comprising methyltrichlorosilane (MTS) and dihydrogen (H2), in a volume ratio of dihydrogen to methyltrichlorosilane of between 5 and 15, at a first pressure of between 70 mbar and 150 mbar and a first duration of between 10 hours and 30 hours, and the chemical vapor infiltration of step (d) is carried out by a second gas mixture comprising methyltrichlorosilane (MTS) and dihydrogen (H2) at a second pressure identical to the first pressure and a second duration of between 30 minutes and 3 hours;

[0036] - step (d) comprises at least two successive cycles, preferably between two and ten cycles, each cycle lasting between 3 and 18 minutes, and wherein the second gas mixture has the same 50 / 50 volume ratio of methyltrichlorosilane (MTS) to dihydrogen (H2) as the first gas mixture, and the first and second pressures are the same;

[0037] - in step (d), the second gas mixture comprises a proportion of methyltrichloroethane rosilane (MTS) higher than that of dihydrogen (H2), preferably the proportion of methyltrichlorosilane (CH3Cl3Si) and dihydrogen (H2) is between 70 / 30 and 85 / 15 by volume, and wherein the first and second predetermined pressures are identical;

[0038] - the method comprises a step (e) of incorporating a mixture of powders ramic, preferably silicon carbide, in said fibrous preform obtained in step (d).

[0039] The invention also relates to a method for manufacturing a part made of ceramic matrix composite material according to the invention. This method comprises steps (a) to (e) of the method for manufacturing a fiber preform described above, and a step (f) of densifying said fiber preform obtained in step (e) by infiltration of a molten ceramic matrix to form said part made of ceramic matrix composite material.

[0040] Preferably, the ceramic matrix is ​​based on liquid silicon.

[0041] At the end of step (f), the fiber preform is said to be “densified” by the matrix. ceramic because a second level of densification with silicon is achieved by MI infiltration. Brief description of the figures

[0042] The present invention will be better understood and other details, features and advantages of the present invention will become more apparent upon reading the following description of a non-limiting example which follows, with reference to the attached drawings in which:

[0043] [Fig.l] schematically represents a method of manufacturing a CMC material according to the prior art,

[0044] [Fig.2] represents the reactivity of liquid silicon on a pre-densified layer of silicon carbide of the CMC material obtained by the process of [Fig.l],

[0045] [Fig. 3] is a partial schematic representation of a predensified fiber preform according to the invention,

[0046] [Fig.4] is an enlarged view of [Fig.3],

[0047] [Fig.5] represents the reactivity of liquid silicon on a sacrificial layer of the pre-densified fiber preform of [Fig.3],

[0048] [Fig.6] schematically represents in blocks the steps of a method of manufacturing a part made of CMC material according to the invention.

[0049] Elements having the same functions in different implementations have the same references in the figures. Detailed description of the invention

[0050] Figures 1 and 2 have been described in the technical background of the present invention and illustrate a fiber preform for producing a part from ceramic matrix composite (CMC) material, in particular reinforced with silicon carbide (SiC), and its manufacturing method according to the prior art.

[0051] Reference is made to Figures 3 and 4 which illustrate a fiber preform 1 for producing a part from CMC material 10.

[0052] The fiber preform 1 according to the invention comprises: - a fibrous reinforcement 2, - at least one interphase layer 3, - at least one pre-densified layer 4, and - at least one sacrificial layer 7.

[0053] The fibrous reinforcement 2 may comprise ceramic fibers 20. For example, the fibers 20 may comprise mainly silicon carbide (hereinafter referred to as SiC) or non-oxide ceramic fibers. SiC fibers marketed under the name “Hi-Nicalon S” may be used. Alternatively, it is possible to use carbon fibers.

[0054] The fibrous reinforcement 2 may be in the form of a unidirectional (1D) texture such as a yarn or a roving, or a bidirectional (2D) texture such as a unidirectional or multidirectional fabric or sheet, or in the form of a three-dimensional (3D) texture such as a felt, a fabric or a knit; or even a 3D texture formed by winding or draping 1D or 2D textures. Preferably, the reinforcement fibrous has a deformable structure.

[0055] The interphase layer 3 extends around a surface 22 of each of the fibers 20. In other words, the interphase layer 3 coats each fiber 20 of the fiber reinforcement. As mentioned previously, this interphase layer makes it possible to optimize the bond between the fibers 20 and a matrix 6 of the part made of CMC material and to deflect cracks (which may be generated within the matrix 6) which would propagate towards the fibers 20.

[0056] Preferably, the interphase layer 3 is based on boron nitride (BN). Boron nitride provides good resistance to oxidation and can be easily implemented.

[0057] Advantageously, the interphase layer 3 has a thickness of between 100 nm and 700 nm, preferably between 250 nm and 500 nm.

[0058] The pre-densified layer 4 extends over the interphase layer 3. Thus, the interphase layer 3 is interposed between the fiber 20 and the pre-densified layer 4. The pre-densified layer 4 may be made of ceramic, such as SiC, in particular when the fibers 20 are made of SiC or carbon.

[0059] This pre-densified layer 4 has a columnar microstructure composed in particular of SiC grains.

[0060] The columnar microstructure is understood, in the usual sense of the crystallographic field, as a microstructure in which the grains have a cylindrical shape, that is to say one direction of which is greater than the other two. In the present application, the largest direction of the grains of the columnar microstructure extends in a radial direction from the fiber 20 towards the pre-densified layer 4.

[0061] Such a columnar microstructure may be the result of a CVI process which will be described below, and in particular of the growth of the grains in a preferred crystallographic direction.

[0062] To ensure that the microstructure can be columnar, it is preferable that the pre-densified layer 4 has a thickness greater than or equal to 3 pm.

[0063] Thus, the cylindrical SiC grains of the pre-densified layer 4 may have a height (in the radial direction) greater than or equal to 3 pm. These cylindrical SiC grains may have a width of between 0.2 pm and 1 pm.

[0064] Advantageously, the pre-densified layer 4 has a thickness of between 3 μm and 20 μm. This range of values ​​makes it possible to obtain a pre-densified layer with a columnar microstructure. Preferably, the thickness of the pre-densified layer is between 10 μm and 20 μm.

[0065] The sacrificial layer 7 is located on the pre-densified layer 4 and is preferably in direct contact with it. The sacrificial layer 7 may be made of ceramic, such as than SiC, especially when the pre-densified layer 4 is made of SiC.

[0066] The sacrificial layer 7 comprising SiC has grains with an average size of between 0.1 qm and 0.5 qm.

[0067] The sacrificial layer 7 may have a grain density (SiC) which is greater than a grain density (SiC) of the pre-densified layer 4. For example, the grain density of the sacrificial layer 7 is greater by a factor of between 20 and 40 compared to that of the pre-densified layer 4. This makes it possible in particular to obtain a fine-grained microstructure of the sacrificial layer 7 compared to the columnar microstructure of the pre-densified layer 4.

[0068] In addition, the density of SiC grains of the sacrificial layer 7 which is greater than that of the pre-densified layer 4, can make it possible to form micro-structured SiC grains 70 of the sacrificial layer 7 in comparison with the columnar SiC grains 42 of the pre-densified layer 4, as illustrated schematically in [Fig. 4]. The sacrificial layer 7 thus has a larger fine grain boundary surface compared to that of the pre-densified layer, so that the liquid silicon reacts preferentially with the sacrificial layer 7 and the pre-densified layer 4 is therefore preserved from attack by the liquid silicon.

[0069] The sacrificial layer 7 may have a thickness representing between 5% and 20% of the thickness of the pre-densified layer 4.

[0070] Advantageously, the thickness of the sacrificial layer 7 is between 1 qm and 4 qm. Preferably, the thickness of the sacrificial layer is between 1 qm and 2 qm. This makes it possible to reinforce a fine grain boundary surface so that the liquid silicon reacts with the carbon of the sacrificial layer 7.

[0071] The fiber preform 1 may comprise several sacrificial layers 7 superimposed on each other and extending over the pre-densified layer 4. The number of these sacrificial layers 7 may be at most five. This makes it possible to increase the surface area of ​​the sacrificial layer and further block the attack of the liquid silicon on the pre-densified layer. In the example of FIGS. 3 and 4, a single sacrificial layer 7 coats the pre-densified layer 4.

[0072] [Fig. 5] illustrates an example of the fiber preform 1 according to the invention, in which degradation of the sacrificial layer 7 can be observed while the pre-densified layer 4 (as well as the interphase layer 4 and the fibers 20) remain intact. The attack of this sacrificial layer 7 by the liquid silicon is indicated by arrows in [Fig. 5]. Since [Fig. 5] illustrates that no crack propagates in the pre-densified layer 4, unlike those of the prior art ([Fig. 2]), it can be concluded that a sacrificial layer 7 makes it possible to protect the pre-densified layer 4 from an attack by the liquid silicon during the process of producing the part in CMC material.

[0073] The invention also relates to a part made of CMC material 10 comprising the fiber preform 1 described above with reference to FIGS. 3 to 5, and a densified ceramic matrix 6.

[0074] The part 10 may be a part of a turbomachine, in particular an aircraft part. For example, this turbomachine part is a blade of a turbine or a compressor of the turbomachine, an annular wall of a combustion chamber of the turbomachine, etc.

[0075] Advantageously, the matrix 6 is based on silicon carbide, in particular when the fibers 20 are made of SiC or carbon.

[0076] With reference to [Fig. 6], the present application will now describe an example of a method for manufacturing the fiber preform 1 and also the part made of CMC material 10.

[0077] The method for manufacturing the fiber preform 1 comprises the steps of: (a) obtaining the fibrous reinforcement 2 comprising SiC-based fibers 20, (b) forming the interphase layer 3 on each of the surfaces 22 of the SiC-based fibers 20, (c) forming the pre-densified SiC-based layer 4 on the interphase layer 3 by chemical vapor infiltration (CVI), and (d) depositing at least one sacrificial layer 7 based on SiC on the pre-densified layer 4 of step (c) by chemical vapor infiltration (CVI), to obtain the fiber preform 1 in particular which is partially pre-densified.

[0078] The fibrous reinforcement 2 in step (a) may have a shape similar to that of the part to be manufactured. As described above, the fibrous reinforcement 2 may be obtained by multi-layer or 3D weaving from threads or strands. It is also possible to start from a 2D texture, such as a fabric or a sheet of threads or strands, to form layers which will then be draped over a form and possibly linked together, for example by sewing or implantation of threads.

[0079] For example, the interphase layer 3 can also be deposited by chemical vapor infiltration (CVI).

[0080] The CVI deposition technique is well known. Reference may be made, for example, to document FR-A1-2 742 433.

[0081] The CVI deposition of step (c) can be carried out from a first gas mixture comprising methyltrichlorosilane (MTS) and dihydrogen (H2) as reactive species. The volume ratio of dihydrogen to methyltrichlorosilane can be between 5 and 15. To carry out the CVI deposition of the pre-densified layer 4, at least one of the parameters below can be chosen: - a first pressure between 70 mbar and 150 mbar, - a first temperature between 900°C and 1100°C, and - a first duration between 10 hours and 30 hours.

[0082] The CVI deposition of step (d) can be carried out from a second gas mixture comprising methyltrichlorosilane (MTS) and dihydrogen (H2).

[0083] For the CVI deposition of the sacrificial layer or layers 7, at least one of the parameters below may be: - a second pressure between 70 mbar and 150 mbar, - a second temperature between 900°C and 1100°C, and - a second duration between 30 minutes and 3 hours.

[0084] According to a first embodiment, the CVI deposition of step (d) is carried out in conventional mode. For this, the CVI deposition can be carried out by a voluntary stopping of the supply of reactive gas flow (namely the MTS), then a new sending of the reactive gas for example for a duration of between 30 minutes and 3 hours.

[0085] The second gas mixture comprises a proportion of methyltrichlorosilane greater than that of dihydrogen. Preferably, the proportion of methyltrichlorosilane and dihydrogen is between 70 / 30 and 85 / 15 by volume. This proportion makes it possible in particular to obtain the aforementioned size and / or density of SiC grains of the sacrificial layer 7. These proportions advantageously make it possible to generate an excess of carbon in the sacrificial layer.

[0086] The first and second pressures may be identical.

[0087] According to a second embodiment, the CVI deposition of step (d) is carried out in pulsed mode. The pulsed mode can be carried out by multiple stops and returns of reagent gas over a predetermined duration interval (such as 30 minutes to 3 hours) to produce the sacrificial layer. This pulsed mode makes it possible in particular to increase the concentration of microstructure of fine SiC grains in the sacrificial layer 7. In addition, the pulsed mode makes it possible to precisely control the microstructure of the deposits of sacrificial layers formed. For this purpose and in a non-limiting manner, the fibrous reinforcement 1 is placed in an enclosure (not illustrated in the figures) where the aforementioned temperature and pressure conditions are established.A volume of the reaction gas phase giving the deposit of the sacrificial layer 7 is admitted into the enclosure and remains there for the aforementioned duration, before evacuation of the gaseous species from the enclosure and introduction of a new volume of gas phase. The cycle comprising the introduction of the gas phase into the enclosure, the residence of the gas phase inside the enclosure and the evacuation of the gaseous species from the enclosure is repeated the number of times necessary to achieve the desired thickness of the sacrificial layer deposition.

[0088] Step (d) may comprise at least two successive cycles, preferably between two and ten cycles. Each of the cycles may have a duration of between 3 and 18 minutes.

[0089] The second gas mixture may have the same 50 / 50 proportion by volume of methyltrichlorosilane and dihydrogen as the first gas mixture.

[0090] The first and second pressures may be identical.

[0091] With reference to [Fig.6], the method may comprise a step (e) of incorporating a powder 5 into the fiber preform 1 obtained in step (d). Preferably, the powder 5 may be a silicon carbide SiC powder.

[0092] The partially densified and porous fiber preform 1, resulting from step (d) or step (e), can continue the densification by an MI type process. For this, a step (f) of densification of this consolidated fiber preform 1 can be carried out by impregnating it with a liquid or molten ceramic matrix 6 to thus form the part made of CMC material 10. Preferably, the matrix 6 is based on silicon carbide.

Claims

Claims

1. Fibrous preform (1) for producing a part (10) made of ceramic matrix composite material, the fibrous preform (1) comprising: - a fibrous reinforcement (2) comprising silicon carbide (SiC)-based fibers (20), - an interphase layer (3) extending around a surface of each of said silicon carbide (SiC)-based fibers (20), preferably the interphase layer (3) being boron nitride (BN)-based, - a pre-densified layer (4) comprising silicon carbide (SiC), located on the interphase layer (3) and having a columnar microstructure, said pre-densified layer (4) having a thickness of between 3 μm and 20 μm, the fibrous preform (1) being characterized in that it further comprises a sacrificial layer (7) located on said pre-densified layer (4), said sacrificial layer (7) comprising silicon carbide (SiC), ... said pre of silicon having grains with an average size between 0.1 pm and 0.5 pm.

2. Fibrous preform according to claim 1, characterized in that said at least one sacrificial layer (7) has a grain density greater than that of the pre-densified layer (4) by a factor of between 20 and 40.

3. Fibrous preform according to claim 1 or 2, characterized in that said at least one sacrificial layer (7) has a thickness of between 1 and 4 μm.

4. Fibrous preform according to any one of the preceding claims, characterized in that several sacrificial layers (7) are superimposed on each other and extend over said pre-densified layer (4), the number of these sacrificial layers (7) being at most five.

5. Part made of ceramic matrix composite material comprising a fibrous preform (1) according to any one of the preceding claims, and a densified ceramic matrix (6), said ceramic matrix (6) preferably being based on silicon carbide (SiC).

6. Method for manufacturing a fiber preform (1) according to any one of claims 1 to 4, this fiber preform (1) being intended to produce a part (10) in matrix composite material ceramic according to claim 5, the method comprising the steps of: (a) obtaining the fibrous reinforcement (2) comprising silicon carbide-based fibers (20), (b) forming the interphase layer (3) on each of the surfaces (22) of the silicon carbide-based fibers (20), (c) forming the pre-densified layer (4) on said interphase layer (3) by chemical vapor infiltration (CVI), and (d) depositing at least one silicon carbide-based sacrificial layer (7) on said pre-densified layer (4) obtained in step (c) by chemical vapor infiltration (CVI), to obtain said fibrous preform (1).

7. Method according to claim 6, characterized in that the chemical vapor infiltration of step (c) is carried out by a first gas mixture comprising methyltrichlorosilane (MTS) and dihydrogen (H2), in a volume ratio of dihydrogen to methyltrichlorosilane of between 5 and 15, at a first pressure of between 70 mbar and 150 mbar and a first duration of between 10 hours and 30 hours, and the chemical vapor infiltration of step (d) is carried out by a second gas mixture comprising methyltrichlorosilane (MTS) and dihydrogen (H2) at a second pressure identical to the first pressure and a second duration of between 30 minutes and 3 hours.

8. Method according to claim 7, characterized in that step (d) comprises at least two successive cycles, preferably between two and ten cycles, each of the cycles having a duration of between 3 and 18 minutes, and in which the second gas mixture has the same 50 / 50 proportion by volume of methyltrichlorosilane (MTS) and dihydrogen (H2) as the first gas mixture, and the first and second pressures are identical.

9. Method according to claim 7, characterized in that, in step (d), the second gas mixture comprises a proportion of methyltrichlorosilane (MTS) greater than that of dihydrogen (H2), preferably the proportion of methyltrichlorosilane (CH3Cl3Si) and dihydrogen (H2) is between 70 / 30 and 85 / 15 by volume, and in which the first and second predetermined pressures are identical.

10. Method according to any one of claims 6 to 9, characterized in that it comprises a step (e) of incorporating a mixture of ceramic powders (4), preferably silicon carbide, into said fibrous preform (1) obtained in step (d).

11. Method for manufacturing a part (10) made of ceramic matrix composite material according to claim 5, the method being characterized in that it comprises steps (a) to (e) of the method for manufacturing a fiber preform (1) according to claim 10, and a step (f) of densification of said fiber preform (1) obtained in step (e) by infiltration of a molten ceramic matrix (6), preferably based on silicon, to form said part (10) made of ceramic matrix composite material.