METHOD FOR MANUFACTUREING E-GLASS FIBERS FROM A MIXTURE OF MINERAL MATERIALS COMPRISING A CALCIUM AND ALUMINUM SILICATE
By using a calcium and aluminum silicate powder with controlled particle size in the E glass fiber manufacturing process, the issues of high energy consumption and dust generation are addressed, resulting in improved homogeneity and reduced breakage rates.
Patent Information
- Application Number
- FR2022011324
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-28
AI Technical Summary
Existing E glass fiber manufacturing processes face issues with high energy consumption, generation of respirable dust, and accelerated furnace corrosion due to the use of fine raw materials, which affect homogeneity and mechanical strength.
Incorporating a calcium and aluminum silicate powder with a specific particle size distribution into the raw material mixture, along with other components, to enhance homogeneity and reduce energy consumption while maintaining mechanical strength.
The process achieves improved homogeneity and reduced breakage rates in E glass fibers, along with decreased energy consumption and dust generation, thereby enhancing the manufacturing efficiency and safety.
Smart Images

Figure 00000019_0000
Abstract
Description
Title of the invention: METHOD FOR PRODUCING E-GLASS FIBERS FROM A MIXTURE OF MATERIALS MINERALS COMPRISING A CALCIUM AND ALUMINUM SILICATE
[0001] The invention relates to the field of melting a mixture of raw materials, in particular for the manufacture of glass fibers, in particular E-glass fibers. E-glass yarn is not only used in the textile industry but also for the reinforcement of composite elements.
[0002] Its excellent electrical insulation properties, even at low thickness, combined with its mechanical strength and its behavior at different temperatures, were the basis of the first applications of E-glass yarn.
[0003] E-glass fiber thus has low thermal conductivity. The fiber can withstand temperatures of over 600°C and is incombustible. In addition, it has excellent chemical resistance. E-glass fiber products are resistant to oils, solvents, and most chemical agents. In addition, they are rot-proof. E-glass yarn is also insensitive to variations in temperature and humidity and its coefficient of expansion is low.
[0004] E-glass fiber products are also particularly resistant to abrasion and vibration, and have excellent flexibility. Glass yarn has a higher specific strength (tensile strength / volumetric mass) than steel. This characteristic now makes it possible to develop glass yarns that will reinforce high-performance composites.
[0005] Usually, E-glass is obtained by melting a bath of raw material comprising silica, lime, kaolin, a source of boron such as borax or boric acid and possibly dolomite, the basic components being judiciously chosen to provide a glass composition producing fibers combining flexibility and robustness to mechanical traction as well as to heat, to chemical agents as well as to electrical potential. To obtain the best properties, it is essential to limit as much as possible the levels of MgO and alkali oxides Na 2O and K2O or iron oxide Fe2O3 in the composition of the E-glass finally obtained. Usually, to the silica, lime, alumina or the source of alumina, a boron oxide such as borax or boric acid or colemanite is added, while any alkali oxide is excluded to obtain E-glass. This composition is heated until it melts.At 1400°C the liquid is considered homogeneous, but it is only at 1500°C that the last bubbles and impurities disappear from the glass. Once refined, the molten mass is normally perfectly transparent when it leaves the furnace. This mass passes through dies (platinum alloy plates pierced with hundreds of holes) to produce a glass thread. This thread is then sized, wound, and dried.
[0006] In particular, for E-glass, the fiber diameter is generally less than 20 microns or even less than 10 microns for electronic applications. Due to the risk of clogging of the dies by unmelted raw material particles, the particle size distribution (or PSD) of each raw material must be as low as possible from an economic point of view. In addition, a low PSD accelerates grain digestion and improves chemical homogeneity. Typically, among the raw materials mentioned above, the PSD is of the order of a hundred micrometers.
[0007] It is generally accepted that the choice of the raw materials mentioned above is necessary to obtain good quality glass, particularly after its fiberization. Among the properties considered essential, we can cite the homogeneity of the glass. Good homogeneity conditions in particular the quality of the fiberization, and more particularly the rate of breakage of the fiber and therefore the yield of the manufacture of E glass fibers.
[0008] In particular, a key parameter in the mechanical strength of glass fiber is the homogeneity of A12O3 in the glass, which mainly fixes the elastic modulus E of the fiber or, in other words, the flexibility of the fiber and the breaking strength. It can be seen in the table below that A12O3 has the highest coefficient of the oxides present in the glass for the determination of the elastic modulus E.
[0009] [Tables 1] Oxide i Factor E; [Winkelmann*] MgO 4.0 CaO 7.0 B2O3 6.0 A12O3 15.0 SiO2 7.0
[0010] * Glass, Glass Institute, 2nd edition, 1980, page 212-3 and table 28.
[0011] In the mixture of raw materials for the manufacture of E-glass, the main The currently used Al2O3 carrier (or aluminum source) is kaolin, a mineral composed of kaolinite (hydrated aluminum silicate). However, kaolin is a raw material that frequently presents significant chemical stability problems. (Al2O3 variation, alkaline and sulfurous pollution, etc.) of the raw material mixture for the manufacture of E glass.
[0012] To meet the above requirements, the glass is usually prepared by melting in a furnace raw materials comprising silica and at least one alkaline earth (to give the glass resistance to hydrolysis) in the form of limestone (calcium carbonate), an alumina carrier (such as kaolin) and a boron carrier (for example borax or boric acid or colemanite), are the two other major elements in the composition of a current bath. In order to improve the homogeneity of the glass, it is known and common in the field to reduce as much as possible the particle size distribution (or PSD) of the raw materials and in particular the median diameter D50 of the raw materials.
[0013] However, by reducing the PSD, the amount of respirable dust generated in the composition workshop increases, which requires additional means to prevent their inhalation by operators. The service life of the furnaces used for melting the mixture is also reduced, due to the increase in its residue content, accelerating the corrosion of the refractories.
[0014] Energy consumption (energy required to melt the mixture of raw materials) is also an essential element to take into account in the manufacturing process of E glass.
[0015] On this point, working with fine raw materials affects and significantly reduces the capacity of the mixture of raw materials, introduced into the furnace in lump form, to absorb the heat from the melting means, typically burners, arranged within the furnace, because the heat transferred from the flames to the mixture of raw materials depends greatly on the emissivity of said mixture. A lower emissivity of the raw materials therefore corresponds to a less efficient heat transfer.
[0016] More precisely, [Fig. 1] schematically illustrates a furnace 2 allowing the melting of raw materials. The raw materials are introduced as a mixture into the furnace 7 in the form of a compact lump 1. The lump 1 initially floats on the molten glass 6. The lower surface of the lump first melts thanks to the convection of the molten glass under the effect of electrical resistance 4 (electrical boosting) arranged in the lower part of the furnace. A bubbler 8 increases the convection of the glass and thus mechanically induces better homogeneity of the glass. The upper surface of the lump is also heated by radiation thanks to a series of burners 3 positioned at the side walls of the furnace as shown schematically by [Fig.l] below. After melting of the lump, a foaming phenomenon 5 is observed due to the refining of the glass.
[0017] It therefore follows from the above that if working with fine grained materials would theoretically improve the chemical homogeneity of the glass, it causes major drawbacks which are:
[0018] - the increase in the energy consumption of the oven, particularly on the first burner (energy transfer from burner to raw material less efficient).
[0019] - the generation of dust in the production plant, causing problems hygiene and safety of personnel,
[0020] - the generation of a phenomenon of dust entrainment in the furnace, which accelerates the corrosion of refractories.
[0021] The originality of the present invention lies in the choice of raw materials. Indeed, it has been discovered that it is possible to use certain silicates as raw materials in a process for manufacturing E-glass fibers to limit the energy consumption of its manufacturing process while maintaining good homogeneity of the final glass.
[0022] The object of the present invention is thus to propose a method for manufacturing E-glass fibers allowing a homogeneous distribution of Al2O3 in said final glass and thus limiting the number of breakages of the E-glass fiber, while reducing the energy consumption necessary for said manufacturing.
[0023] The object of the present invention is thus to propose a method for manufacturing E glass allowing a homogeneous distribution of the aluminum oxide in said final glass, while reducing the energy consumption necessary for said manufacturing.
[0024] More specifically, the present invention relates to a method for manufacturing E-glass fibers having a target composition, comprising the melting of a mixture of raw materials constituting a melt bath, said target composition meeting the following criteria, in weight percentages:
[0025] SiO2: between 45 and 60%, preferably between 50 and 60%
[0026] CaO: between 20 and 35%, preferably between 20 and 30%
[0027] A12O3: between 10 and 20%, preferably between 12 and 18%
[0028] B2O3: between 3 and 10%, preferably between 4 and 8%
[0029] MgO: less than 2%, preferably between 0 and 1%
[0030] K2O + Na2O: less than 2%, preferably between 0 and 1%
[0031] Iron oxide: less than 1%, preferably less than 0.5%
[0032] other oxide(s): between 0 and 3% cumulative,
[0033] the remainder being made up of unavoidable impurities,
[0034] said process being characterized in that the mixture of raw materials comprises a calcium and aluminum silicate comprising, in weight percentage, more than 35% of SiO2, more than 10% by weight of CaO and more than 20% of Al2O3, SiO2, CaO and Al2O3 together representing more than 70% and preferably more than 75% of said calcium silicate and in that said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose median grain diameter D50 is comprised
[0035]
[0036]
[0037]
[0038]
[0039]
[0040]
[0041]
[0042] between 10 and 300 micrometers. According to preferred embodiments of the present invention, which are not limiting but which can of course be combined with each other: - said calcium and aluminum silicate has the following composition, in weight percentages: - SiO2: between 40 and 60%, preferably between 45 and 55%, - CaO: between 10 and 30%, preferably between 12 and 20%, - A12O3: between 25 and 35%, - SiO2, CaO and A12O3 together representing more than 80%, preferably more than 85%, or even more than 90%, - Na2O: between 0 and 4%, - Fe2O3: between 0 and 4%, for example between 0.1 and 1% - less than 5% of other oxides, preferably less than 3% of other oxides. - Said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose median grain diameter is between 20 micrometers and 250 micrometers, preferably between 30 and 250 micrometers, and very preferably between 40 micrometers and 200 micrometers. - Said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose median grain diameter is between 50 and 150 micrometers. - Said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose maximum grain diameter is less than 1500 micrometers, more preferably less than 1250 micrometers. - The raw material mix includes: - said calcium and aluminum silicate, - at least one source of silicon chosen in particular from silica, E-glass cullet or recycled mineral fibers or their mixture, - a source of boron preferably chosen from borax or an oxide of boron and calcium, in particular colemanite, or an oxide of boron, sodium and calcium, in particular ulexite and / or tincalconite and / or kernite, - optionally a source of aluminum such as kaolin, possibly hydrated alumina or pyrophyllite, - optionally limestone CaCO3 or calcium hydroxide Ca (OH)2 or quicklime CaO, - optionally a milkman. - Said mixture comprises a boron and calcium oxide comprising, in weight percentage, more than 30% of B2O3 and more than 20% by weight of CaO. - Said mixture comprises a calcium silicate comprising, in weight percentage, more than 30% SiO2 and more than 20% CaO, preferably at least 25% CaO, CaO and SiO2 together representing more than 60%, or even more than 70% or even more than 80% of the total weight of said silicate.
[0043] - Said calcium silicate has the following composition, in weight percentages: - SiO2: between 30 and 60%, preferably between 40 and 55%, - CaO: between 25 and 55%, preferably between 35 and 50%, - Fe2O3: between 0 and 4%, for example between 0.1 and 0.5%, - A12O3: between 0 and 8%, for example between 0.5 and 2%, - CO2: between 0 and 20%, in particular between 0 and 15%, - less than 5% of other oxides, preferably less than 3% of other oxides.
[0044] - Kaolin or pyrophyllite is also used as a complementary source. of aluminum.
[0045] - The raw material mixture contains less than 12% by weight of CO2, preferably less than 10% CO2, more preferably less than 5% CO2.
[0046] - Glass cullet E or fibers are also introduced into the melting bath. recycled minerals, in particular recycled glass wool or recycled rock wool.
[0047] - Recycled E-glass cullet or recycled mineral fibers represents between 10 and 50% of the total weight of the weld pool.
[0048] - Recycled mineral fibers have the following composition:
[0049] SiO2: between 30 and 50%, preferably between 35 and 45%
[0050] Na2O: between 0 and 10%, preferably between 0.4 and 7%
[0051] CaO: between 10 and 35%, preferably between 12 and 25%
[0052] MgO: between 1 and 15%, preferably between 5 and 13%
[0053] CaO+MgO: between 11 and 40% cumulative,
[0054] A12O3: between 10 and 27%,
[0055] K2O: between 0 and 2%, preferably between 0 and 1%
[0056] Iron oxide: between 0.1 and 3%,
[0057] other oxide(s): between 0 and 5% cumulative, preferably less than 3%,
[0058] the remainder being made up of unavoidable impurities.
[0059] The invention also relates to the mixture of raw materials described above.
[0060] In particular, the invention also relates to the mixture of raw materials for the manufacture of E-glass fibers described above, and comprising a calcium and aluminum silicate comprising, in weight percentage, more than 35% of SiO2, more than 10% by weight of CaO and more than 20% of Al2O3, SiO2, CaO and Al2O3 together representing more than 70% and preferably more than 75% of said calcium silicate and in that said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose median grain diameter D50 is between 10 and 300 micrometers.
[0061] Such a mixture of raw materials preferably comprises:
[0062] - said calcium and aluminum silicate,
[0063] - a source of silicon notably chosen from silica, E-glass cullet or recycled mineral fibers or their mixture,
[0064] - a source of boron preferably chosen from borax or an oxide of boron and calcium, in particular colemanite, or an oxide of boron, sodium and calcium, in particular ulexite and / or tincalconite and / or kernite,
[0065] - optionally a source of aluminum such as kaolin, alumina even actually hydrated or pyrophyllite,
[0066] - optionally limestone CaCO3 or calcium hydroxide Ca(OH)2 or quicklime CaO.
[0067] - optionally a slag.
[0068] The mixture of raw materials according to the invention is intended to be heated to a temperature and under conditions allowing its melting to obtain a glass corresponding to said target composition.
[0069] With such a mixture, it is possible to significantly reduce or even eliminate CO2 emissions from the raw materials, not only during the melting stage but also to significantly reduce them in the prior stages.
[0070] As demonstrated in the examples which follow, it was thus possible to obtain E glass fibers without defects, and whose homogeneity is improved, from the mixture according to the invention as will be shown in the examples which follow.
[0071] To produce the glass, the Si carrier (or source) is preferably introduced into the mixture of raw materials in the form of sand. The AI can advantageously be introduced into the mixture of raw materials in the form of a mixture of said calcium and aluminum silicate and kaolin. Each raw material is introduced into the mixture of raw materials in such a quantity that the molar percentage of its cation (such as Si, Ca, Al, B, etc.) relative to the sum of the moles of all the cations is the same as in the final glass. The raw materials of the mixture are chosen to lead to a glass whose target composition falls within the framework (the percentage ranges of the different oxides) described previously.
[0072] The mixture of raw materials is heated until a molten glass is obtained, generally in a furnace. The heating is more or less high in temperature and for a longer or shorter time depending on the quality of the glass that is sought, in particular according to the degree of tolerance in unmelted particles (called "unmelted") and bubbles. Generally, the maximum heating temperature of the molten glass is between 1400 and 1700°C. For the transformation of the raw material mixture into glass, glass melting techniques well known to those skilled in the art can be used. This transformation can be carried out in any type of furnace such as an electric electrode furnace, an overhead burner furnace such as a cross-burner furnace or a loop furnace, or a submerged burner furnace.
[0073] For heating and melting glass, the mixture of raw materials, if necessary moistened, can be introduced into a furnace in a powdered state, which implies that each raw material it contains is in a powdered state. For heating and melting glass, the mixture of raw materials, if necessary moistened, can be introduced into a furnace in a composition state comprising cullet and the mixture of raw materials, the latter being if necessary powdered.
[0074] In the context of the present invention, it is possible to dispense with the use of a system for shaping (i.e. forming) the mixture of raw materials by mechanical pressure, in particular using molds leading to calibrated agglomerates (briquettes, balls, granules, pellets, etc.), such as hoop compactors. Thus, before introduction into a furnace, the mixture of raw materials may not be shaped by mechanical pressure. It is also not necessary to use a technique for granulating the raw material according to which the material is rotated (in particular in a rotating drum type tank) generally in the presence of a binder so as to lead to granules (pellets in English).
[0075] Unless otherwise indicated, all particle size values (median diameter D50, maximum diameter Dmax) in the present description and the claims are given by mass and are obtained by conventional sieving techniques, in particular for the calcium and aluminum silicate according to the invention.
[0076] The invention will be better understood on reading the following examples intended to illustrate its advantages, without of course the invention being considered as limited to these, in any of the aspects described. Examples
[0077] According to these examples, different mixtures of raw materials are prepared in order to compare a mixture as currently used for the manufacture of E glass for the final production of the same composition, which has substantially the following formulation in percentage by weight of oxides:
[0078] [Tables2] Elements Percentage weight % SiO2 54 CaO 24 MgO <1 AI2O3 14 B2O3 6 Na2O <1 k2o <0.3 Na2O+ K2O <1 Fe2O3 <0.5
[0079] The compositions in percentages by weight of oxides of the different materials used are given in table 3 below.
[0080] [Tables3] SiO 2 A12O 3 CaO MgO B2O 3 Na2O K2O Fe2O 3 TiO 2 SO3 Loss on ignition Sand 99.2 0.37 0.04 0.02 0 0 0.01 0.06 0.08 0 0.21 Borax 0 0 0 0 48.5 21.9 0 0 0 0 29.6 Colemanite 4.7 0.1 28.1 1.93 39.9 0.07 0.03 0.03 0 0.27 23.9 Ca and Al silicate 50.5 30.5 14.6 0.15 0 2.5 0.28 0.59 0.05 0.01 0.8 Kaolin 45.4 38 0.18 0.17 0 0 0.17 0.55 1.48 0 14.05 Limestone 0.18 0.04 55.6 0.46 0 0.01 0 0.015 0.01 0.01 43.6 Sodium sulfate 0 0 0 0 0 43.4 0.015 0.000 2 0 56.1 0.46 Example 1 (prior art)
[0081] According to a first example, a mixture of raw materials is synthesized in a conventional manner, in proportions allowing the synthesis of E glass corresponding to the preceding formulation.
[0082] Table 4 below gives the proportions of the different raw materials (in weight percentage) of the mixture:
[0083] [Tables4] Example 1 kg / Tonne glass Sand 368 Pentaborax 18 Colemanite 148 Kaolin 363 Limestone 362 Sodium sulfate 3.8 Example 2:
[0084] In this example the mixture of raw materials is this time as described in table 5 below.
[0085] In this initial mixture, a mineral material consisting of a calcium and aluminium silicate according to the invention, the median diameter D50 of which is 78 micrometres, was introduced as a reagent to replace part of the kaolin, limestone and sand.
[0086] This material is introduced in a mixture with the other constituents in proportions adjusted accordingly to obtain a glass with a composition very close to that of reference example 1. In table 5 below, the proportions of the different raw materials used are shown:
[0087] [Tables5] kg / Tonne of glass Sand 342 Pentaborax 5.1 Colemanite 165 Kaolin 228 Limestone 305 Sodium sulfate 2.6 Silicate of Ca and Al 170 Example 3:
[0088] In this example, the same raw materials are used as in example 2, but a calcium and aluminum silicate with a larger particle size is used, i.e. D50 equal to 522 micrometers.
[0089] The particle sizes of the limestone and the calcium and aluminum silicate used in the previous examples are obtained by sieving, those of the kaolin and the sand are measured by laser.
[0090] The measurements are carried out on approximately 100g of representative sample (accuracy of 102g). The test sample is placed on the upper sieve of the column (Standard NF X 11501). The column is stirred for 5 minutes in a ROTAP sieve machine (Retsch AS200 TAP). The residue from the first sieve containing the grains is weighed (accuracy of 10 2g). The residue from each sieve is added, proceeding in the same way, to those from the previous sieves, and the cumulative mass is noted each time.
[0091] The results are expressed as a cumulative % relative to the final total mass MF.
[0092] X1% = M1 x 100 / MF
[0093] XI = % of cumulative rejection on sieve 1
[0094] Ml = mass of cumulative rejects on sieve 1
[0095] MF = final mass of product.
[0096] This calculation will be carried out for each nominal sieve opening.
[0097] The D50 is calculated from an interpolation of the upper and lower grain sizes closest to 50%.
[0098] In particular, the D50 is classically determined by the following equation:
[0099] D50 = [T<50%] + (50% - [X<50%]) x ([T<50%] - [T>50%]) / ([X<50%] - [X>50%])
[0100] With:
[0101] T<50% = Sieve opening less than 50% of rejection
[0102] T>50% = Sieve opening greater than 50% of rejection
[0103] X<50% =% of cumulative refusal on T<50%
[0104] X>50% =% of cumulative refusal on T>50%
[0105] The particle size of sand and kaolin is measured using a Malvern Instruments Mastersizer 300® laser particle sizer according to ISO 13320:2009, in isopropanol as dispersant.
[0106] All the granulometric data measured on the raw materials are reported in Table 6 below:
[0107] [Tableauxô] Sand* Limestone Kaolin* Al and Ca silicate (fine) Al and Ca silicate (coarse) D50 [pm] 14 114 10 78 522 Maximum grain size (pm) NM 250 NM 1000 NM Grain proportions <100 pm (%) NM 30.3 NM 69.5 NM
[0108] NM: not measured *: laser granulometer measurement
[0109] The following measurements are carried out:
[0110] 1°) The emissivity of the mixture of raw materials used is measured from the reflectance spectra using the law of conservation of energy for opaque materials: absorbance a(X, T) + reflectance p(X, T) = 1. Applying Kirchhoff's law, the spectral emittance can be expressed in terms of the total reflectance, [YES] e(X, T) = a(X, T)
[0112] with:
[0113] where Bt is the spectral irradiance of the black body at the temperature T of 2600°C, corresponding to the temperature of the oxygen-gas flame of the burner.
[0114] The measurements of the hemispherical reflectance at room temperature are carried out with a 150 mm integrating sphere mounted on a Lambda spectrophotometer are carried out between 300 and 2500 nm, using as a reflectance reference, a Spectralon plate.
[0115] For easy handling, the samples are pressed by applying a force of 0.4 tonnes / cm2 and wetted with 5% water prior to measurement.
[0116] 2°) The mixtures of the above examples are melted in a typical melting furnace based on flame technology shown schematically in [Fig.l] below.
[0117] Measurement of the energy consumed in the furnace for melting the mixtures:
[0118] During the various melting tests corresponding to the examples above, the gas consumption is adjusted in order to maintain a similar profile temperature inside the furnace and at all points of it. From this, a gas consumption and therefore energy consumption necessary to reach the same heating point is deduced.
[0119] 3°) Homogeneity in A12O3 in the final glass:
[0120] A sample is melted in a cylindrical platinum crucible from the same mixture of raw materials as described previously. The sample is heated in air at 1410°C for 4 hours. The cooled glass is then cored and cut to obtain a blade comprising the cross-section of the cylinder. This blade was polished, carbon-metallized and analyzed using an electron microprobe at 15kV. The analysis consisted of determining the mass percentage of A12O3 over the entire height of the blade (or of the melted sample) at 50 measurement points, the measurement step was 200 microns.
[0121] It is thus possible on this basis to calculate the average of the A12O 3 concentration and the standard deviation. A criterion of homogeneity of A12O3 in the glass is provided by the ratio standard deviation divided by the average concentration (oakcb / [A12O3]). The smaller this value, the better the homogeneity of the A12O3 concentration in the final glass.
[0122] The results obtained are reported in Table 7 below:
[0123] [Tables7] Example 1 2 3 Aluminum source Kaolin Al and Ca silicate (fine) Al and Ca silicate (coarse) Emissivity of the mixture 0.31 0.32 NM Homogeneity in glass (OA12O3 / [ A12O3]) (%) >5 (ref) 1.4 > ref Energy consumed by the first burner in the furnace Reference -5.1% / ref NM
[0124] NM: not measured
[0125] Example 2 according to the invention, in which a calcium and aluminum silicate of suitable particle size according to the invention is used as raw material for the molten bath as an aluminum carrier, replacing part of the kaolin, allows an energy adjustment on the first burner (closest to the charging, i.e. the entry of the raw materials into the furnace) in the direction of a reduction in energy expenditure. Also, in the sense previously described, the homogeneity in Al2O3 appears very improved for example 2 according to the invention, compared to the reference example 1.
[0126] As described above, the homogeneity of A12O3 in the E-glass finally obtained is essential for the strength of the glass fibers, in particular during the fiberizing stage, where the fibers are mechanically stressed.
[0127] The breakage rate of the glass fiber is evaluated, i.e. the number of breaks per 100 kg of glass fiber produced.
[0128] The breakage rate obtained for 100 kg of glass fiber produced is 1.2 for the reference example and 0.9 for example 2 according to the invention, i.e. a 25% reduction in fiber breakages.
Claims
Claims
1. A method of manufacturing E-glass fibers having a target composition, comprising melting a mixture of raw materials constituting a melt bath, said target composition meeting the following criteria, in weight percentages: SiO2: between 45 and 60%, preferably between 50 and 60% CaO: between 20 and 35%, preferably between 20 and 30% A12O3: between 10 and 20%, preferably between 12 and 18% B2O3: between 3 and 10%, preferably between 4 and 8% MgO: less than 2%, preferably between 0 and 1% K2O + Na2O: less than 2%, preferably between 0 and 1% Iron oxide: less than 1%, preferably less than 0.5% other oxide(s): between 0 and 3% cumulatively, the remainder being unavoidable impurities, said process being characterized in that the mixture of raw materials comprises a calcium and aluminum silicate comprising, in percentage by weight, more than 35% of SiO2, more than 10% by weight of CaO and more than 20% of Al2O3, SiO2, CaO and Al2O3 together representing more than 70% and preferably more than 75% of said calcium silicate and in that said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose median grain diameter D 50 is between 10 and 300 micrometers,wherein the mixture of raw materials comprises:, - said calcium and aluminum silicate, - at least one source of silicon chosen in particular from silica, E-glass cullet or recycled mineral fibers or their mixture, - a source of boron preferably chosen from borax or an oxide of boron and calcium, in particular colemanite, or an oxide of boron, sodium and calcium, in particular ulexite and / or tincalconite and / or kemite, - optionally a source of aluminum such as kaolin, possibly hydrated alumina or pyrophyllite, - optionally limestone CaCO3 or calcium hydroxide Ca (OH)2 or quicklime CaO, - optionally a milkman.
2. Method according to the preceding claim in which said calcium and aluminum silicate corresponds to the following composition, in weight percentages: - SiO2: between 40 and 60%, preferably between 45 and 55%, - CaO: between 10 and 30%, preferably between 12 and 20%, - A12O3: between 25 and 35%, - SiO2, CaO and A12O3 together representing more than 80%, more preferably more than 85%, or even more than 90%, - Na2O: between 0 and 4%, - Fe2O3: between 0 and 4%, for example between 0.1 and 1% - less than 5% of other oxides, preferably less than 3% of other oxides.
3. Method according to one of the preceding claims, in which said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose median grain diameter is between 20 micrometers and 250 micrometers, preferably between 30 and 250 micrometers, and very preferably between 40 micrometers and 200 micrometers.
4. A method according to any preceding claim, wherein said calcium aluminum silicate is introduced into the mixture in the form of a powder with a median grain diameter of between 50 and 150 micrometers.
5. A method according to any preceding claim, wherein said calcium aluminum silicate is introduced into the mixture in the form of a powder having a maximum grain diameter of less than 1500 micrometers, more preferably less than 1250 micrometers.
6. A method according to any preceding claim, wherein said mixture comprises a boron and calcium oxide comprising, in weight percentage, more than 30% B2O3 and more than 20% CaO.
7. A method according to one of the preceding claims, wherein said mixture comprises a calcium silicate comprising, in weight percentage, more than 30% SiO2 and more than 20% CaO, preferably at least 25% CaO, CaO and SiO2 together representing more than 60%, or even more than 70% or even more than 80% of the total weight of said silicate.
8. The method of the preceding claim, wherein said silicate of calcium has the following composition, in weight percentages: - SiO2: between 30 and 60%, preferably between 40 and 55%, - CaO: between 25 and 55%, preferably between 35 and 50%, - Fe2O3: between 0 and 4%, for example between 0.1 and 0.5%, - A12O3: between 0 and 8%, for example between 0.5 and 2%, - CO2: between 0 and 20%, in particular between 0 and 15%, - less than 5% of other oxides, preferably less than 3% of other oxides.
9. A method according to any preceding claim, wherein kaolin or pyrophyllite is additionally used as a supplementary source of aluminum.
10. Method according to one of the preceding claims, in which the mixture of raw materials contains less than 12% by weight of CO2, preferably less than 10% of CO2, more preferably less than 5% of CO2.
11. Method according to one of the preceding claims, in which E-glass cullet or recycled mineral fibres, in particular recycled glass wool or recycled rock wool, are additionally introduced into the melt.
12. Method according to the preceding claim, in which the recycled E-glass or recycled mineral fiber cullet represents between 10 and 50% of the total weight of the molten bath.
13. Method according to one of the preceding claims in which the recycled mineral fibers have the following composition: SiO2: between 30 and 50%, preferably between 35 and 45% Na2O: between 0 and 10%, preferably between 0.4 and 7% CaO: between 10 and 35%, preferably between 12 and 25% MgO: between 1 and 15%, preferably between 5 and 13% CaO+MgO: between 11 and 40% cumulatively, A12O3: between 10 and 27%, K2O: between 0 and 2%, preferably between 0 and 1% Iron oxide: between 0.1 and 3%, other oxide(s): between 0 and 5% cumulatively, preferably less than 3%, the remainder consisting of unavoidable impurities.
14. Mixture of raw materials for the manufacture of E-glass fibers comprising a calcium and aluminum silicate comprising, in weight percentage, more than 35% of SiO2, more than 10% by weight of CaO and more than 20% of Al2O3, SiO2, CaO and Al2O3 together representing more than 70% and preferably more than 75% of said calcium silicate and in that said calcium and aluminum silicate is introduced into the mixture in the form of a powder whose median grain diameter D50 is between 10 and 300 micrometers,
15. said mixture comprising: - said calcium and aluminum silicate, - a source of silicon chosen in particular from silica, E-glass cullet or recycled mineral fibers or their mixture, - a source of boron preferably chosen from borax or an oxide of boron and calcium, in particular colemanite, or an oxide of boron, sodium and calcium, in particular ulexite and / or tincalconite and / or kernite, - optionally a source of aluminum such as kaolin, possibly hydrated alumina or pyrophyllite, - optionally limestone CaCO3 or calcium hydroxide Ca(OH)2 or quicklime CaO. - optionally a milkman