Method for activating a fuel cell by electrolysis
The activation method for PEMFCs using electrolysis with controlled voltage and humidity improves electrochemical performance by enhancing access to catalytic sites, addressing the limitations of existing processes and reducing cell count and cost.
Patent Information
- Application Number
- FR2022011720
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-11-10
AI Technical Summary
Existing fuel cell activation processes, particularly for proton exchange membrane fuel cells (PEMFC), do not adequately improve electrochemical performance, especially at high current densities, and can lead to irreversible degradation of the Pt/C catalyst.
An activation method involving an electrolysis phase with an applied voltage greater than 1 V and controlled humidity is used to facilitate access to catalytic sites by altering the porosity of the anode, followed by a conventional conditioning step, which enhances the accessibility of reactive gases to the catalytic sites without causing irreversible degradation.
The method improves the nominal operation of the fuel cell at high current densities, increasing current density and reducing the number of cells required, thus lowering the total cost while maintaining catalyst effectiveness.
Smart Images

Figure 00000022_0000 
Figure 00000023_0000 
Figure 00000024_0000
Abstract
Description
Title of the invention: Method for activating a fuel cell by electrolysis Technical field
[0001] The present invention relates to the field of fuel cells, in particular proton exchange membrane fuel cells (or PEMFC for Proton Exchange Membrane Fuel Cell). It can be implemented to condition or activate a PEFMC, and optimize its performance. STATE OF THE ART
[0002] A fuel cell is formed from a stack of “unitary” electrochemical cells, each comprising an anode and a cathode electrically separated from each other by an electrolyte. In the case of a hydrogen cell, the fuel (hydrogen) is brought into contact with the anode, and the oxidant (oxygen) is brought into contact with the cathode. When the cell operates as a current generator, the fuel and the oxidant are consumed by oxidation and reduction reactions which take place respectively at the anode and the cathode. These reactions produce electricity, water and heat. The nominal operating temperature of the cell is generally around 80°C.
[0003] The electrolyte can be in the form of a membrane allowing the protons resulting from the hydrogen oxidation reaction to pass through. This is the case for proton exchange membrane fuel cells (PEMFCs). Such a membrane is generally composed of a solid perfluorosulfonated polymer called an ionomer. The electrodes are typically porous, to promote the transport of fuel and oxidant gases, and to allow the evacuation of the water produced. Each electrode typically comprises two layers: a gas diffusion layer, typically carbon-based, and a catalytic layer, generally based on platinum nanoparticles deposited on porous carbon (Pt / C). The catalytic layers are arranged against the membrane, so that platinum nanoparticles are at the interface with the ionomer. The catalytic layers - also called active layers - are thus intercalated between the gas diffusion layers and the membrane.The membrane, diffusion layers and catalytic layers are commonly referred to by the acronym AME meaning “Assembly Membrane Electrodes”.
[0004] When implementing the PEMFC, an initial conditioning phase is generally carried out. This conditioning phase allows the PEMFC to reach its nominal performance.
[0005] This very first phase of operation of the PEMFC is carried out in a generally under favorable conditions in terms of humidity and temperature in order to properly hydrate the membrane and “activate” the catalytic layers to gradually increase the initial performance of the battery and reach its nominal performance.
[0006] The phenomena occurring during this conditioning phase, also called the “activation” or “running-in” phase, may include both the hydration of the ionomer in the membrane and in the active layers, and / or the decontamination of the catalytic layers and the diffusion layers as a whole.
[0007] In any event, the conditioning or activation phase produces an improvement in the performance of the PEMFC and is therefore a prerequisite for the nominal operation of the cell.
[0008] The document "Advances in rapid and effective break-in / conditioning / recovery of automotive PEMFC stocks, Shyam S. Kocha et al., Current Opinion in Electrochemistry, vol.31, 100843 (2022)" discloses different methods for activating a PEFMC. All these methods are based on operating the battery as a generator at low voltage, with a voltage per cell < 1 V. These numerous methods indicate that there is a need to improve current activation procedures. The electrochemical performance of the cells, particularly at high current density, can be further improved.
[0009] An object of the present invention is to provide a method of activating a fuel cell improving the electrochemical performance of the cells compared to known methods.
[0010] Other objects, features and advantages of the present invention will become apparent from the following description and accompanying drawings. It is understood that other advantages may be incorporated. SUMMARY
[0011] To achieve this objective, according to one embodiment, a method is provided for activating a fuel cell comprising a plurality of stacked electrochemical cells, each cell comprising a first electrode, a second electrode, and a proton exchange membrane interposed between said first and second electrodes, the first electrode comprising a first conductive gas diffusion layer and a first catalytic layer based on porous carbon and in contact with the membrane, the second electrode comprising a second conductive gas diffusion layer and a second catalytic layer based on porous carbon and in contact with the membrane.
[0012] The fuel cell is intended to operate, during at least one nominal operating phase, as an electric generator. During this nominal operating phase, the cell is conventionally supplied with reactive gases - the fuel and the oxidant, typically hydrogen at the anode (corresponding for example to the first electrode) and oxygen at the cathode (corresponding for example to the second electrode), and provides an electric current by consumption of the reactive gases.
[0013] The activation method comprises, during an activation phase prior to at least one nominal operating phase: - An electrical power supply to the fuel cell by an external electrical generator, said electrical power supply being configured to apply an activation voltage per cell greater than or equal to 1 V, - A fluidic supply of wet gas at at least one of the first and second electrodes, said wet gas having a Relative Humidity (RH) such that 40% < RH < 100%.
[0014] The fuel cell thus operates in electrolysis during the activation phase. It receives an electric current and water vapor from the humid gas, and produces in particular hydrogen and oxygen. The first electrode becomes the cathode and the second electrode becomes the anode, the opposite of generator operation.
[0015] It has been noted that this method makes it possible to considerably improve the performance of the battery. The mechanisms at the origin of this unexpected performance, explored in the context of the development of the present invention, are explained in particular below.
[0016] The electrolytic operation of the battery, for an activation voltage per cell greater than or equal to 1 V, advantageously makes it possible to corrode part of the carbon of the anode, according to a reaction of the type C + 2H2O —> CO2 + 4H+ + 4e. This corrosion causes a modification of the porosity of the anode. This frees up access routes to catalytic sites of the catalytic layer. During the subsequent nominal operating phase, access to the catalytic sites is facilitated for the reactive gases.
[0017] The release of O2 at the anode, at the heart of the active layer, could also be a concomitant factor in the release of certain access routes for the reactants to the catalytic sites.
[0018] The transport of material, which is the predominant limitation when operating the battery as a high current density generator, is thus improved. This makes it possible to increase the current density supplied by the cell and by the battery during the nominal operating phase.
[0019] The activation method according to the invention thus improves the nominal operation of the battery in generator mode, in particular at high current density. The efficiency is improved for a given nominal power. As a corollary, for a given nominal power it is possible to reduce the number of cells in the stack, which reduces the total cost of the battery.
[0020] Preferably, the method further comprises a conditioning step in which the fuel cell operates as an electrical generator, said conditioning step being carried out before or after the electrolysis activation phase. This conditioning step is carried out in a conventional manner, for example according to a protocol recommended by the manufacturer of the cell or according to a conditioning method disclosed by the document “Advances in rapid and effective break-in / conditioning / recovery of automotive PEMFC stocks, Shyam S. Kocha et al., Current Opinion in Electrochemistry, vol. 31, 100843 (2022)”. The activation method according to the invention then typically complements the conventional conditioning method. The additional conditioning time linked to the activation method according to the invention is preferably less than or equal to 5 minutes, and preferably less than 3 minutes.This provides a performance gain for a limited additional packaging cost.
[0021] A non-intuitive principle of the invention thus consists of briefly operating the cells in “electrolysis” mode, that is to say that the battery becomes the receiver of the external electrical generator, at an imposed cell voltage typically greater than 1 V.
[0022] According to a technical prejudice, such operation in electrolysis is not recommended because it can cause irreversible degradation of the Pt / C catalyst of the cathode of the cell (during its operation as a generator), for example as mentioned in the document “Proton Exchange Membrane Fuel Cell Reversal: A Review, Congwei Qin et al., Catalysts, vol. 6, 197 (2016)”.
[0023] During the development of the present invention, it was found that the application of an electrolysis voltage typically between 1 V and 2 V per cell, under humid gas while controlling the Relative Humidity, does not alter the catalytic layers. These are typically oxidized and passivated by one or more PtOx oxides during the electrolysis activation phase, but this oxidation state is reversible. As soon as the cell operates again as a generator, the PtOx oxides are reduced and the catalytic properties are restored, while retaining the benefit of the prior electrolysis activation phase. In particular, the opening and / or creation of pores by corrosion of the porous carbon surrounding the Pt nanoparticles are retained.
[0024] The activation method according to the present invention thus makes it possible to improve the accessibility to the “metallic Pt” catalytic sites. The transport of the reactants to the catalytic sites is more efficient and the performance of the cell is improved.
[0025] According to another aspect, the invention relates to equipment comprising a fuel cell comprising a plurality of stacked electrochemical cells, each cell comprising a first electrode, a second electrode, and a proton exchange membrane interposed between said first and second electrodes, the first electrode comprising a first conductive gas diffusion layer and a first catalytic layer based on porous carbon and in contact with the membrane, the second electrode comprising a second conductive gas diffusion layer and a second catalytic layer based on porous carbon and in contact with the membrane, the equipment comprising an electrical generator and a control-command system configured to: - impose on the fuel cell an activation phase prior to a nominal operating phase of the cell, during which the control-command system controls and commands: • a fluid supply of wet gas at at least one of the first and second electrodes, said wet gas having a Relative Humidity (RH) such that 40% < RH < 100%, • An electrical power supply to the fuel cell by the electrical generator, said electrical power supply being configured to apply an activation voltage per cell greater than 1 V, - optionally, before or after the activation phase, carry out a conditioning step in which the fuel cell operates as an electric generator, during which the control-command system controls and commands: • a fluid supply of hydrogen at the first electrode and oxygen at the second electrode, • an electrical connection between the fuel cell and a load configured to deliver an electric current.
[0026] According to another aspect, the invention relates to a use of this equipment for conditioning or activating a fuel cell, in initial conditioning or in addition to initial conditioning. BRIEF DESCRIPTION OF THE FIGURES
[0027] The aims, objects, as well as the characteristics and advantages of the invention will emerge more clearly from the detailed description of embodiments thereof which are illustrated by the following accompanying drawings in which:
[0028] [Fig.l] [Fig.l] shows a flowchart of the necessary (solid lines) and optional (dotted lines) steps of the activation method, according to an embodiment of the present invention.
[0029] [Fig.2] [Fig.2] schematically presents a cell and its AME in mode of “electrolysis” operation, according to an embodiment of the present invention.
[0030] [Fig.3] [Fig.3] schematically shows a cell and its AME in mode of “electric generator” operation, according to an embodiment of the present invention.
[0031] [Fig.4] [Fig.4] shows different polarization curves after applying the activation method at different activation times.
[0032] The drawings are given as examples and are not limiting of the invention. They constitute schematic representations of principle intended to facilitate the understanding of the invention and are not necessarily on the scale of practical applications. In particular, the bipolar electrical connection plates are not shown. DETAILED DESCRIPTION
[0033] Before beginning a detailed review of embodiments of the invention, optional features which may possibly be used in combination or alternatively are set out below:
[0034] According to one example, the fluid supply is configured to maintain a humidity level within the cells, in particular at the membrane of each cell, of between +20% and -20% of a nominal humidity level of the membrane. This nominal humidity level of the membrane may be provided by the manufacturer. It may be measured by high-frequency resistance measurements. Functionally, the humid gas is used in particular to provide the water necessary for the activation phase by electrolysis - which consumes water -, and to hydrate the membrane to promote proton conduction.
[0035] According to one example, the method further comprises a conditioning step in which the fuel cell operates as an electrical generator, said conditioning step being carried out before or after the electrolysis activation phase. The electrolysis activation phase and the conditioning step are typically complementary. The electrolysis activation phase makes it possible in particular to open the pores of the porous carbon-based electrode, by corrosion of the carbon, to improve the access of the reactants to the catalyst particles, in particular to the platinum nanoparticles. The conditioning step typically makes it possible to reduce the platinum oxides to make the catalyst active. The conditioning step also makes it possible to hydrate the ionomer in the membrane and the catalytic layers. Carrying out a conditioning step and an electrolysis activation phase makes it possible to significantly increase the performance of the cell.
[0036] According to one example, the conditioning step is carried out before the electrolysis activation phase, and the method further comprises, after the conditioning step and before the electrolysis activation phase, a step of heating the cell configured to reach a cell temperature of between 20°C and 60°C. Temperature control helps control reaction kinetics during electrolysis. The lower the temperature, the lower the carbon corrosion kinetics. This allows for better control of carbon corrosion kinetics during the activation phase.
[0037] According to one example, the fluidic supply comprises a first supply of a first wet gas at the first electrode and a second supply of a second wet gas at the second electrode, said first and second wet gases each having a Relative Humidity (RH) such that 40% < RH < 100%. This makes it possible to improve the water supply in the catalytic layers and / or the hydration of the ionomer necessary for the electrolysis reactions. The electrolysis is thus more efficient during the activation phase. The duration of the activation phase can for example be reduced.
[0038] According to one example, the first supply of a first wet gas is carried out by recirculation of hydrogen at controlled Relative Humidity. Hydrogen is already the gas used for the other conditioning or operating phases of the cell. The implementation of the activation method is therefore facilitated. According to one example, the second supply of a second wet gas is carried out by injection or recirculation of nitrogen at controlled Relative Humidity. Nitrogen is not reactive. This avoids unwanted reactions when the power supply is stopped by the external generator, at the end of the activation phase. This also makes it possible to eliminate the oxygen produced by the electrolysis reaction during the activation phase and at the end of the activation phase. The electrical potential of the electrode (anode in electrolysis, cathode in cell mode) decreases accordingly. This typically makes it possible to reduce the platinum oxides formed during the activation phase..
[0039] According to one example, the activation phase is carried out at a temperature less than or equal to 60°C, preferably less than or equal to 40°C. The lower the temperature, the lower the carbon corrosion kinetics. This makes it possible to better control the carbon corrosion kinetics during the activation phase.
[0040] According to one example, the activation voltage applied to each cell is between 1 V and 2 V, preferably between 1 V and 1.6 V. This makes it possible to obtain a significant carbon corrosion reaction, without being excessively rapid. The higher the activation voltage, the higher the carbon corrosion kinetics. A voltage between 1 V and 2 V, preferably between 1 V and 1.6 V, makes it possible to better control the carbon corrosion kinetics during the activation phase.
[0041] According to one example, the applied activation voltage is constant during the activation phase, without cycling below 1 V. Repeated voltage cycling below 1 V can cause atomic rearrangement of the platinum particles (by a reduction / dissolution mechanism) inducing a loss of active surface area.
[0042] According to one example, the method successively comprises: - a conditioning step in which the fuel cell operates as an electric generator, said conditioning step comprising: • a fluid supply of hydrogen at the first electrode and of oxygen at the second electrode, • an electrical connection between the fuel cell and a load configured so as to obtain a first circulation of electrons from the first electrode to the second electrode, - stopping the fluid supply of oxygen at the second electrode, - a disconnection of the load, - the electrolysis activation phase, comprising: • supplying or maintaining the fluid supply of hydrogen at the first electrode, • the fluid supply of wet gas at the second electrode, the wet gas being nitrogen, • the electrical power supply of the fuel cell by the external electrical generator, said electrical power supply being configured to apply an activation voltage per cell of between 1 V and 1.6 V, so as to obtain a second circulation of electrons from the second electrode to the first electrode - a shutdown of the power supply by the external electric generator, after an activation phase duration of less than or equal to 300 s, - a stoppage of the hydrogen fluid supply at the first electrode, - elimination of the oxygen produced during the activation phase at the second electrode, while maintaining the fluid supply of nitrogen, then - a stoppage of the nitrogen fluid supply at the second electrode.
[0043] According to one example, the method further comprises, after the conditioning step and before the activation phase, a step of cooling or heating the cell so that the temperature at the level of the cells is between 20°C and 60°C, preferably between 20°C and 40°C. The lower the temperature, the lower the corrosion kinetics of the carbon. This makes it possible to better control the corrosion kinetics of the carbon during the activation phase.
[0044] Unless incompatibility exists, technical features described in detail for a given embodiment may be combined with the technical features described in the context of other embodiments described by way of example and not limitation. In particular, elements described or illustrated in the figures for the cell or for the method may be combined so as to form another embodiment which is not necessarily illustrated or described. Such an embodiment is obviously not excluded from the invention. For reasons of clarity, a single cell is illustrated in Figures 2 and 3. A fuel cell according to the present invention typically comprises several electrochemical cells in a stack. Those skilled in the art will have no difficulty in implementing an embodiment of the method for one or more electrochemical cells.
[0045] In the context of the present invention, the term "fuel cell" means a system comprising one or more interconnected electrochemical cells. The cells are typically in the form of a Membrane-Electrode Assembly commonly referred to as MEA. The activation method here preferably applies to a cell sized for industrial applications. Thus, the cell preferably comprises a plurality of electrochemical cells, which typically form a power stack. The cell here preferably comprises at least five cells stacked within the MEA, and preferably at least ten.
[0046] The battery typically has different operating phases, in particular, one or more initial conditioning phases, one or more nominal production phases, possibly one or more regeneration phases, a shutdown phase.
[0047] During a nominal operating or production phase of the cell, the cells of the cell are typically supplied with fuel and oxidant at nominal concentrations and at nominal flow rates. The cell delivers a current and the power of the cell can be regulated either in voltage or in current. The cell thus operates as an electrical generator.
[0048] The activation method according to the present invention deals more particularly with the initial conditioning phases, also called activation or running-in, which occur before the nominal operating phase of the battery.
[0049] The initial conditioning phase(s) aim to bring the performance of the cell to a nominal performance level, or at least to 90% of the nominal performance level, according to the desired achievement level criterion. According to conventional conditioning or activation methods, the cell operates as an electrical generator according to fluid supply and / or regulation parameters which are not nominal. According to a known example, the cell is voltage regulated at low voltage, typically at a voltage < 0.5V. According to another known example, the cells can be supplied by a supply fluid having a reduced oxidant molar fraction.
[0050] The original idea implemented within the framework of the development of the present invention consists in particular of carrying out an activation phase in electrolysis, during which the battery consumes electric current and water, and produces in particular oxygen, hydrogen and carbon dioxide.
[0051] During a regeneration phase of the cell, the cell typically operates as an electrical generator, according to fluid supply and / or regulation parameters which are not nominal, as for conditioning. For example, the cells can be supplied by a supply fluid having a reduced oxidant molar fraction.
[0052] During a shutdown phase, the cell is no longer supplied with fuel and / or oxidant. The cell can continue to produce an electric current temporarily and in a decreasing manner.
[0053] “Relative Humidity (RH)” means the quantity of water vapor present in a gas, expressed as a percentage (% RH) of the quantity necessary to reach a saturation level, at a given temperature and a given pressure. Relative Humidity thus corresponds to the ratio of the partial pressure of the water vapor contained in the gas to the saturation vapor pressure, for the same temperature. It can typically be measured using a hygrometer. The reference temperature is typically the temperature of the battery, preferably the temperature of the cell.
[0054] Several embodiments of the invention implementing successive steps of the activation method are described below. Unless explicitly stated, the adjective “successive” does not necessarily imply, even if this is generally preferred, that the steps follow one another immediately, intermediate steps being able to separate them.
[0055] Furthermore, the term “step” means the carrying out of a part of the method, and can designate a set of sub-steps.
[0056] Furthermore, the term "step" does not necessarily mean that the actions carried out during a step are simultaneous or immediately successive. Certain actions of a first step may in particular be followed by actions linked to a different step, and other actions of the first step may be repeated subsequently. Thus, the term step does not necessarily mean unitary and inseparable actions in time and in the sequence of the phases of the process.
[0057] In the present application, an activation voltage Ue is applied by an external generator. The external generator is not part of the battery. The activation voltage Ue corresponds here to the potential difference between the anode and the cathode of the battery or cell in question. This activation voltage can therefore be directly measured on the battery. It is greater than or equal to 1 V. The activation voltage Ue is also called “electrolysis voltage” or “cell voltage” or simply “voltage” in the following, without ambiguity for those skilled in the art.
[0058] In the present application, in the illustrative figures the direction of the electric current represented by arrows corresponds to the actual direction of circulation of the electrons. The flow of electrons thus circulates from the anode to the cathode. This convention is true both in generator mode and in electrolysis mode.
[0059] [Fig.l] is a flowchart of the activation method according to an embodiment of the present invention.
[0060] The dotted lines indicate optional steps in the activation process. The solid lines indicate the main steps in the activation process.
[0061] According to one possibility, conditioning 100 or pre-conditioning of the battery is first carried out. Such conditioning 100 can be carried out in a standard manner, according to the operating conditions recommended by the manufacturer. During this conditioning 100, the battery is typically supplied 101 with reactive gases, for example air or oxygen at the cathode and hydrogen at the anode, and a load is connected 102 to the electrodes so that the battery delivers an electric current between the anode and the cathode, at a voltage U preferably less than or equal to 0.8 V.
[0062] According to one possibility, the cell is brought to temperature 110 so as to obtain a cell temperature between 20°C and 60°C. This may involve heating or preheating, typically if the cell has not been subjected to conditioning 100 immediately before the activation phase 200. This may involve cooling, typically if the cell has been subjected to conditioning 100 immediately before the activation phase 200.
[0063] The activation phase 200 in electrolysis of the battery can be carried out alone or preferably in addition to the conditioning 100. If the conditioning 100 has been carried out prior to the activation phase 200, the distribution of oxidant (air or oxygen) is preferably stopped. The load is preferably disconnected or stopped.
[0064] During the activation phase 200 by electrolysis, the cell is supplied 201 with humid gas, and connected to an external electric generator configured to circulate 202 an electric current through the cell at an activation voltage Ue greater than the open circuit cell voltage UOcv-
[0065] If the conditioning 100 has been carried out prior to the activation phase 200, the hydrogen distribution can be maintained, for example by recirculation, by controlling the Relative Humidity (RH) so that the hydrogen has a Relative Humidity greater than or equal to 40%. Alternatively, if the conditioning 100 has not been carried out before the activation phase 200, a humid gas of at least 40% RH and strictly less than 100% RH is injected at the electrode which becomes the cathode in the electrolysis configuration. This humid gas can be hydrogen, nitrogen or an inert gas for example.
[0066] This supply of wet gas, preferably by continuous sweeping, makes it possible to provide the water necessary for the electrolysis reaction and / or to hydrate the membrane of the cell.
[0067] If the conditioning 100 has been carried out prior to the activation phase 200, the distribution of oxygen at the other electrode, which becomes an anode in the electrolysis configuration, is preferably stopped and replaced by a distribution of humid gas having a Relative Humidity RH such that 40% < RH < 100%, for example nitrogen. The residual oxygen from the conditioning phase 100 is preferably eliminated so that the cell voltage U decreases, preferably to approximately 0.1 V. The elimination of the oxygen can be done by progressive replacement by nitrogen, or according to another possibility by consumption of the remaining oxygen by briefly activating the load.
[0068] Before connecting the external generator to the cell to start the electrolysis, the temperature of the cell is preferably set between 20°C and 60°C, preferably between 20°C and 40°C, for example of the order of 30°C. The kinetics of the reactions occurring during the electrolysis are thus reduced. This allows for better control of these reactions, in particular with regard to carbon corrosion, which is one of the reactions of interest occurring during the electrolysis.
[0069] The external generator is then connected, terminal “+” of the generator to the anode in electrolysis configuration, in order to apply 202 an activation voltage Ue to the cells, preferably constant and between 1 and 1.6 V. An activation voltage Ue < 1.6 V makes it possible to better control the reaction kinetics.
[0070] After an activation duration t to be chosen 210 by the user, according to an economic criterion for example, typically 10 s < t < 300 s, the electrical power supplied by the external generator is stopped 211. This makes it possible to stop the electrolysis. The activation phase 200 ends. The fluidic supply of wet gas can be stopped 212.
[0071] The oxygen produced at the anode in the electrolysis configuration is preferably removed 213 to lower the electrode potential and thus reduce the platinum oxides formed during the electrolysis. The removal of oxygen can be done continuously by the wet nitrogen sweep used during the electrolysis, or alternatively by consuming the remaining oxygen by briefly connecting and activating the load until a cell voltage U < 0.8 V, and preferably U < 0.2 V, for example U < 0.1 V, is reached.
[0072] Alternatively, if conditioning 100 was not performed before activation phase 200, conditioning 100 may be performed after the activation phase. This also reduces platinum oxides and activates the catalyst.
[0073] The activation phase 200, with pre-conditioning or post-conditioning 100, advantageously makes it possible to prepare the cell for nominal operation 300. The nominal performance of the cell is improved thanks to the activation process.
[0074] [Fig.2] illustrates a cell 1 of a battery connected to an external electric generator 2 in electrolysis configuration, according to an embodiment of the activation phase according to the invention.
[0075] The cell typically comprises a membrane 10, a first catalytic layer 13a, a first gas diffusion layer 15a connected to a first fluid circuit 14a, and a second catalytic layer 13b, a second gas diffusion layer 15b connected to a second fluid circuit 14b. The membrane 10 is preferably based on a perfluorosulfonated ionomer, for example based on NAFION®. The first and second diffusion layers 11, 12 are preferably based on porous carbon. The first and second catalytic layers 13a, 13b are preferably based on platinum nanoparticles supported by porous carbon and ionomer. The first gas diffusion layer 15a and the first catalytic layer 13a form the first electrode 11. The second gas diffusion layer 15b and the second catalytic layer 13b form the second electrode 12.
[0076] The first and second electrodes 11, 12 are intended to be electrically connected either to a load (battery mode) or to a generator (electrolysis mode). This electrical connection is shown diagrammatically in Figures 2 and 3. In practice, this electrical connection is typically made via electrically conductive bipolar plates (not shown). In a known manner, the bipolar plates are generally in direct electrical contact with the gas diffusion layers 15a, 15b. They allow the electrical series connection of the different cells of the stack that forms the battery. Alternatively, the bipolar plates may in certain cases be in direct contact with the catalytic layers, which can then be considered as gas diffusion layers.
[0077] In electrolysis mode, the first electrode 11 corresponds to the cathode and the second electrode 12 corresponds to the anode. The external electrical generator 2 is connected by its “+” terminal to the anode and by its “-” terminal to the cathode. The external electrical generator 2 thus imposes a flow of electrons circulating from the anode to the cathode.
[0078] In this example, the cathode is supplied with a first wet gas 21 via the first fluid circuit 14a. This first wet gas 21 may be hydrogen or nitrogen for example. Other gases are also conceivable, for example inert gases. The water supplied by the first wet gas 21 will pass through the first gas diffusion layer 15a, the first catalytic layer 13a, and hydrate the membrane 10.
[0079] The anode is supplied with a second wet gas 22 via the second circuit fluidic layer 14b. This second humid gas 22 can be nitrogen or humid air for example. Other gases are also possible. The water supplied by the second humid gas 22 will pass through the second gas diffusion layer 15b, the second catalytic layer 13b, and hydrate the membrane 10.
[0080] The generator 2 is configured to deliver a current through the cell, with an activation voltage Ue that is substantially constant between the electrodes 11, 12. This activation voltage Ue is greater than or equal to 1 V. In particular, the activation voltage Ue is chosen such that 1 V < Ue < 2 V, preferably 1 V < Ue < 1.6 V.
[0081] The water will dissociate under the effect of the electric current and produce hydrogen at the level of the first catalytic layer 13a, oxygen at the level of the second catalytic layer 13b, carbon dioxide in contact with the carbon of the second catalytic layer 13b, and platinum oxides in contact with the platinum of the second catalytic layer 13b according to the following half-reactions:
[0082] At the anode:
[0083] H2O^ VzO2 + 2H+ + 2e
[0084] C + 2H2O -> CO2 + 4H+ + 4e
[0085] Pt + H2O -> Pt-0 + 2H+ + 2e
[0086] At the cathode:
[0087] 2H+ + 2e -> H2
[0088] The H+ protons pass through the proton exchange membrane 10, from the anode to the cathode. The hydrogen 23 can be recovered at the outlet of the first fluid circuit 14a. The oxygen and carbon dioxide 24 can be evacuated at the outlet of the second fluid circuit 14b.
[0089] These reactions occur for Ue > 1 V and preferably Ue > 1.2 V. Controlled corrosion of the carbon is one of the aspects of the activation process which contributes to increasing the performance of the battery during its nominal operation.
[0090] [Fig. 3] illustrates a cell 1 of a battery, connected to a load 3, in an electric generator configuration (battery mode). Such a configuration corresponds in particular to the nominal operation of the battery. Such a configuration also corresponds to standard conditioning of the battery before its nominal operation.
[0091] In battery mode, the first electrode 11 corresponds to the anode and the second electrode 12 corresponds to the cathode. The two electrodes 11, 12 are connected to a load 3.
[0092] In this example, the anode is supplied with a combustible gas 31, typically hydrogen, via the first fluid circuit 14a. The cathode is supplied with an oxidizing gas 32, typically oxygen or air, via the second fluid circuit 14b. In a known manner, the hydrogen and oxygen pass through the first and second gas diffusion layers 15a, 15b respectively and react within the first catalytic layer 13a and the second catalytic layer 13b respectively.
[0093] The hydrogen and oxygen react to produce water, heat and electric current. The unconsumed hydrogen 33 can be recovered at the outlet of the first fluid circuit 14a. The gas 34 depleted in oxidant and the water can be evacuated and / or recovered at the outlet of the second fluid circuit 14b.
[0094] The load 3 is configured to absorb the flow of electrons generated by the battery. This flow of electrons flows from the anode to the cathode. The voltage U between the electrodes 11, 12, for an initial conditioning phase, is typically lower than the open circuit battery voltage UOcv-
[0095] Such an initial conditioning phase, carried out in combination with the activation phase, before or after said activation phase, makes it possible to obtain significant gains in performance during the nominal operation of the battery.
[0096] According to one example, after initial conditioning, an activation phase at low temperature, of the order of 30°C, maintaining a humidity of the order of 80% RH, and at an activation voltage Ue of between 1.4 V and 1.6 V, is carried out. This makes it possible to corrode the carbon sufficiently and without excess, while easily controlling the reaction kinetics. The reproducibility of the activation process is thus improved.
[0097] The performances of the battery were evaluated by performance measurements using polarization curves. [Fig.4] shows polarization curves obtained after implementation of the activation process, for different durations t of the electrolysis activation phase: t = 30 s (Ci), t = 90 s (C2), t = 150 s (C3), t = 210 s (C4), t = 270 s (C5). The activation phase was carried out with hydrogen circulating at the cathode and nitrogen circulating at the anode, at 80% RH at 30°C, and for an activation voltage Ue = 1.6 V. The polarization curves C1...C5 are compared to the polarization curve Co carried out for a battery having been conditioned only by the initial conditioning phase, without an electrolysis activation phase. At 1.5 A / cm2, the maximum gain (curve C5) is about 50 mV (or about 9% in voltage). At 0.55 V, the maximum gain (curve C5) is 0.3 A / cm2 (or about 20% in power).The battery's performance is therefore significantly improved, particularly at low voltage U < 0.7 V and for high current densities.
[0098] Additional cyclic voltammetry measurements of the catalytic layer 13b under inert gas (not shown) also show that the cell does not suffer from any significant alteration of the platinum electroactive surface after the electrolysis activation phase according to the activation method. The performance of the cell for a voltage greater than 0.8 V is not degraded by this electrolysis activation phase.
[0099] It thus appears clearly that the activation method according to the invention is very effective and allows a significant gain in performance compared to the conditioning methods according to the state of the art. It can advantageously be implemented in as part of initial conditioning of the battery, before any use in the nominal operating phase.
[0100] The parameters of the activation phase described above can be adjusted and optimized depending on the design of the AME or a performance level to be achieved for the stack.
[0101] The choice of the activation phase parameters can be validated by performance measurements, for example by carrying out a comparison of polarization curves before and after implementation of the activation method.
[0102] These measurements can be supplemented by an evaluation of the evolution of the diffusion or polarization resistance, by impedance spectroscopy (resistance to be minimized).
[0103] These measurements may be supplemented by performance measurements at one or more specific operating points, for example at nominal and maximum power or current density.
[0104] These measurements can be supplemented by an evaluation of the evolution of the electroactive surface of platinum by cyclic voltammetry (losses to be minimized).
[0105] The invention is not limited to the embodiments previously described. All activation possibilities, with or without initial conditioning, for a battery comprising one or more cells, with recirculation or injection of wet gas, can be envisaged.
Claims
Claims
1. Method for activating a fuel cell comprising a plurality of stacked electrochemical cells (1), each cell (1) comprising a first electrode (11), a second electrode (12), and a proton exchange membrane (10) interposed between said first and second electrodes (11, 12), the first electrode (11) comprising a first conductive layer (15a) for gas diffusion and a first catalytic layer (13a) based on porous carbon and in contact with the membrane (10), the second electrode (12) comprising a second conductive layer (15b) for gas diffusion and a second catalytic layer (13b) based on porous carbon and in contact with the membrane (10), the fuel cell being intended to operate, during at least one nominal operating phase (300), as an electric generator, the method comprising, during an activation phase (200) prior to the at least one phase nominal operating temperature (300): - An electrical power supply (202) of the fuel cell by an external electrical generator (2), said electrical power supply being configured to apply an activation voltage per cell (1) greater than or equal to IV, - A fluidic supply (201) of wet gas at at least one of the first and second electrodes (11, 12), said wet gas having a Relative Humidity (RH) such that 40% < RH < 100%, so that the fuel cell operates in electrolysis during the activation phase (200) called by electrolysis, the method being characterized in that the fluid supply (201) comprises a first supply of a first humid gas (21) at the first electrode (11) and a second supply of a second humid gas (22) at the second electrode (12), said first and second humid gases each having a Relative Humidity (RH) such that 40% < RH < 100%, and in that the first supply of a first humid gas (21) is carried out by recirculation of hydrogen at controlled Relative Humidity and the second supply of a second humid gas (22) is carried out by injection or recirculation of nitrogen at controlled Relative Humidity.
2. Method according to the preceding claim further comprising a conditioning step in which the fuel cell operates as an electrical generator, said conditioning step (100) being carried out before or after the activation phase (200) by electrolysis.
3. Method according to the preceding claim in which the conditioning step (100) is carried out before the activation phase (200) by electrolysis, said method further comprising, after the conditioning step (100) and before the activation phase (200) by electrolysis, a step of heating (110) the battery configured to reach a battery temperature of between 20°C and 60°C.
4. Method according to any one of the preceding claims in which the activation phase (200) is carried out at a temperature less than or equal to 60°C, preferably less than or equal to 40°C.
5. Method according to any one of the preceding claims in which the activation voltage applied to each cell (1) is between 1 V and 2 V, and preferably between 1 V and 1.6 V.
6. A method according to any preceding claim wherein the applied activation voltage is constant during the activation phase (200), without cycling below 1 V.
7. Method according to any one of the preceding claims comprising successively: • a conditioning step (100) in which the fuel cell operates as an electrical generator, said conditioning step comprising: - a fluidic supply (101) of hydrogen (31) at the first electrode (11) and of oxygen (32) at the second electrode (12), - an electrical connection (102) between the fuel cell and a load (3), so as to obtain a first circulation of electrons from the first electrode (11) to the second electrode (12), • a stopping of the fluidic supply of oxygen at the second electrode (12), • a disconnection of the load (3), • the activation phase (200) by electrolysis comprising: - the supply (201) or a maintenance of the supply - the fluidic supply (201) of hydrogen at the first electrode (11), - the fluidic supply (201) of wet gas (22) at the second electrode (12), the wet gas being nitrogen, - the electrical supply (202) of the fuel cell by the external electrical generator (2), said electrical supply being configured to apply an activation voltage of between IV and 1.6V, so as to obtain a second circulation of electrons from the second electrode (12) to the first electrode (11), • a stoppage (211) of the electrical supply by the external electrical generator (2), after an activation phase duration t (210) of less than or equal to 300 s, • a stoppage (212) of the fluidic supply of hydrogen at the first electrode (11), • an elimination (213) of the oxygen produced during the activation phase at the second electrode (12), while maintaining the fluid supply of nitrogen,then • a stop (212) of the fluid supply of nitrogen at the level of the second electrode (12).,
8. Method according to the preceding claim further comprising, after the conditioning step (100) and before the activation phase (200), a temperature-setting step (110), for example cooling or heating the battery, so that the temperature at the level of the cells (1) is between 20°C and 60°C, preferably between 20°C and 40°C.
9. Equipment comprising a fuel cell comprising a plurality of stacked electrochemical cells, each cell (1) comprising a first electrode (11), a second electrode (12), and a proton exchange membrane (10) interposed between said first and second electrodes (11, 12), the first electrode (11) comprising a first conductive layer (15a) for gas diffusion and a first catalytic layer (13a) based on porous carbon and in contact with the membrane (10), the second electrode (12) comprising a second conductive layer (15b) for diffusion of gases and a second catalytic layer (13b) based on porous carbon and in contact with the membrane (10), the equipment comprising an electric generator (2) and a control-command system configured to: • impose on the fuel cell an activation phase (200) prior to a nominal operating phase of the cell, during which the control-command system controls and commands: - a fluidic supply (201) of hydrogen at the first electrode (11) and of nitrogen at the second electrode (12), the hydrogen and the nitrogen having a Relative Humidity (RH) such that 40% < RH < 100%, - An electrical power supply (202) of the fuel cell by the electrical generator (2), said electrical power supply being configured to apply an activation voltage per cell (1) greater than or equal to IV.
10. Equipment according to the preceding claim in which the control-command system is configured to: • before or after the activation phase (200), carry out a conditioning step (100) in which the fuel cell operates as an electric generator, during which the control-command system controls and commands: - a fluidic supply (101) of hydrogen at the level of the first electrode (11) and of oxygen at the level of the second electrode (12), - an electrical connection (102) of the first and second electrodes (11, 12) with a load (3) configured to deliver an electric current between the first and second electrodes (11, 12).
11. Equipment according to the preceding claim in which the conditioning step (100) is carried out before the activation phase (200) by electrolysis, and in which the control-command system is configured to carry out, after the conditioning step (100) and before the activation phase (200) by electrolysis, a step of heating (110) the battery to reach a battery temperature of between 20°C and 60°C.
12. Use of the equipment according to any one of the three preceding claims for conditioning or activating a fuel cell.