Manufacturing process for photovoltaic subcells
The described process addresses the limitations of existing methods by using dielectric layers and chemical etching to produce photovoltaic sub-cells with passivated edges, enhancing efficiency and shape versatility.
Patent Information
- Application Number
- FR2022012693
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-12-02
AI Technical Summary
Existing methods for manufacturing photovoltaic sub-cells, such as laser cleavage and thermal separation, are inadequate for producing shapes other than rectangular or square and often result in silicon amorphization, making passivation difficult due to defects on the edges.
A process involving the formation of dielectric layers, laser ablation, and selective chemical etching to create photovoltaic sub-cells with varied shapes, reducing silicon amorphization and facilitating easy passivation.
Enables the production of photovoltaic sub-cells with easily passivated edges, improving efficiency by reducing defects and allowing for various shapes beyond rectilinear forms.
Smart Images

Figure 00000019_0000 
Figure 00000019_0001 
Figure 00000020_0000
Abstract
Description
Title of the invention: Method for manufacturing photovoltaic sub-cells Technical field
[0001] The invention relates to the technical field of photovoltaic cells. More specifically, the invention relates to the manufacture of photovoltaic sub-cells having a wide variety of shapes, for example square, rectangular, triangular, circular shapes, etc.
[0002] The invention finds its application in the manufacture of photovoltaic cells based on crystalline silicon, in particular in the manufacture of amorphous silicon / crystalline silicon heterojunction photovoltaic cells. However, other photovoltaic cell architectures are conceivable, for example a TOPCon (“Tunnel Oxide Passivated Contact”) type architecture where the passivated contact comprises a tunnel oxide film and a doped polycrystalline silicon layer, a monolithic multi-junction type architecture (e.g. silicon / perovskite tandem cell), a PERC type architecture (passivated emitter and rear cell), or a rear surface field type architecture made of Al-BSF aluminum (BSF for “Back Surface Field”). State of the art
[0003] A first method for manufacturing photovoltaic sub-cells, known from the state of the art, uses a laser cleavage technique (LDC for “Laser Direct Cleavage” in English). More specifically, a first variant of the first method comprises the steps: Aoi) use a photovoltaic cell, comprising: - a substrate, based on crystalline silicon, having first and second opposite surfaces; - first and second stacks of active layers, formed respectively on the first and second surfaces of the substrate; - first and second sets of metal pads, formed respectively on the first and second stacks of active layers; Boi) apply laser cleavage to the photovoltaic cell in order to: - locally obtaining, between metal pads of the first set, ablations of the first stack of active layers and of a first part of the substrate; - draw an outline delimiting photovoltaic sub-cells; - keep a second part of the substrate, extending in the extension of the ablations; Coi) separate the photovoltaic sub-cells delimited at the end of step BOi) by mechanical stress.
[0004] The first part of the substrate ablated during step BOi) makes it possible to weaken the photovoltaic sub-cells delimited at the end of step BOi), so that it is possible to separate them by mechanical stress during step COi).
[0005] Such a first variant of the first method, involving non-through grooves, is not very suitable for obtaining shapes other than square or rectangular for the photovoltaic sub-cells. In other words, such a first variant of the first method is only suitable when the contour delimits rectilinear portions. Indeed, during step COi) of separating the photovoltaic sub-cells by mechanical stress, a crack will be created and propagate along the preferential cleavage directions, which will induce breakage of the photovoltaic sub-cells.
[0006] A second variant of the first method comprises the steps: A'oi) use a photovoltaic cell, comprising: - a substrate, based on crystalline silicon, having first and second opposite surfaces; - first and second stacks of active layers, formed respectively on the first and second surfaces of the substrate; - first and second sets of metal pads, formed respectively on the first and second stacks of active layers; B'oi) apply laser cleavage to the photovoltaic cell so as to: - locally obtain, between metal pads of the first set, ablations of the first stack of active layers and of the entire substrate; - draw an outline delimiting photovoltaic sub-cells.
[0007] The photovoltaic sub-cells delimited at the end of step B'Oi) are spontaneously separated.
[0008] Such a second variant of the first method, involving through grooves, is suitable for obtaining various shapes for the photovoltaic sub-cells, unlike the first variant.
[0009] However, the first and second variants of such a first method of the state of the art are not entirely satisfactory insofar as the laser irradiation applied during step BOi) creates defects, in particular amorphization of the silicon on the edges of the photovoltaic sub-cells which makes the subsequent passivation of these edges difficult, or even impossible. Passivation of the surfaces of the substrate is a major challenge in the photovoltaic sector, making it possible to limit recombinations between carriers, which results in a significant improvement in efficiency. By "passivation" we mean the reduction of carrier recombinations at the substrate surfaces. Indeed, the surface of a crystalline silicon substrate has a density of defects (e.g. dangling bonds, impurities, crystal discontinuity, etc.) which can lead to significant losses linked to surface carrier recombination in the case of a photovoltaic application.
[0010] A second method of manufacturing photovoltaic sub-cells, known from the prior art, uses a thermal laser separation (TLS) technique. More specifically, the second method comprises the steps: A02) use a photovoltaic cell, comprising: - a substrate, based on crystalline silicon, having first and second opposite surfaces; - first and second stacks of active layers, formed respectively on the first and second surfaces of the substrate; - first and second sets of metal pads, formed respectively on the first and second stacks of active layers; B02) apply a laser thermal separation technique to the photovoltaic cell so as to: - locally obtaining, between metal pads of the first set, a propagation of a crack through the first stack of active layers and the entire substrate; - draw an outline delimiting photovoltaic sub-cells.
[0011] The photovoltaic sub-cells delimited at the end of step B02) are spontaneously separated.
[0012] Such a second method of the state of the art makes it possible, at the end of step B02), to obtain edges of photovoltaic sub-cells which can be passivated. However, such a second method of the state of the art is not entirely satisfactory insofar as it is poorly suited to obtaining various shapes for the photovoltaic sub-cells, in particular when the contour does not delimit rectilinear portions.
[0013] The person skilled in the art is therefore looking for a solution making it possible to obtain various shapes (i.e. not involving only rectilinear portions) for the photovoltaic sub-cells, with edges that can be easily passivated. Statement of the invention
[0014] The invention aims to remedy all or part of the aforementioned drawbacks. To this end, the invention relates to a method for manufacturing photovoltaic sub-cells, comprising the steps: a) use a photovoltaic cell, comprising: - a substrate, based on crystalline silicon, having first and second opposite surfaces; - first and second stacks of active layers, formed respectively on the first and second surfaces of the substrate; - first and second sets of metal pads, formed respectively on the first and second stacks of active layers; b) forming first and second dielectric layers, extending respectively over the first and second sets of metal pads, and extending respectively over the first and second stacks of active layers; c) applying laser radiation to the photovoltaic cell obtained at the end of step b) so as to: - locally obtaining, between metal pads of the first set, ablations of the first dielectric layer, of the first stack of active layers, and of a first part of the substrate; - draw an outline delimiting photovoltaic sub-cells; - retain a second part of the substrate, extending in line with the ablations, and adapted to maintain the mechanical strength of the photovoltaic sub-cells delimited by the traced outline; d) chemically etching, with an etching agent, at least partially the second part of the substrate extending in the extension of the ablations obtained at the end of step c), so as to weaken the photovoltaic sub-cells delimited at the end of step c); the etching agent being chosen so as to allow selective etching of the silicon relative to the first and second dielectric layers; e) separating the weakened photovoltaic sub-cells at the end of step d).
[0015] Thus, such a method according to the invention makes it possible to obtain photovoltaic sub-cells of various shapes (not necessarily involving only rectilinear portions) with edges that can be easily passivated, thanks to the combination of steps c) and d). Indeed, the laser ablation of step c) makes it possible to trace a contour of varied shape, which can be, for example, rectilinear or curvilinear. Step d), for its part, makes it possible to: (i) weaken the photovoltaic sub-cells delimited at the end of step c), and (ii) remove a large part of the defects linked to silicon amorphization (caused by laser irradiation) on the edges of the photovoltaic sub-cells, thanks to chemical etching.
[0016] Such a step d), considerably reducing the amorphization defects of the silicon, thus facilitates subsequent passivation of the edges of the photovoltaic sub-cells compared to the state of the art. The first and second layers di- electrical waves formed during step b) act as etching masks.
[0017] The method according to the invention may comprise one or more of the following characteristics.
[0018] According to a characteristic of the invention: - step d) is performed so that the second part of the substrate is completely chemically etched; - step e) consists of a spontaneous separation of the photovoltaic sub-cells weakened at the end of step d).
[0019] Thus, an advantage provided is to avoid operations dedicated to the separation of the photovoltaic sub-cells.
[0020] According to a characteristic of the invention: - step d) is performed so that the second part of the substrate is partially chemically etched; - step e) is carried out by a separation technique chosen from thermal shock, mechanical stress, and ultrasonic treatment.
[0021] Thus, an advantage provided is to reduce the operating time linked to the chemical etching of the second part of the substrate.
[0022] According to a characteristic of the invention, step d) consists of immersing the photovoltaic cell obtained at the end of step c) in an etching bath.
[0023] Thus, an advantage provided is the simplicity of implementation of the method.
[0024] According to a characteristic of the invention: - the first and second dielectric layers formed during step b) are made of silicon oxide; - step d) is carried out so that the etching agent is chosen from a potassium hydroxide KOH solution, a tetramethylammonium hydroxide TMAH solution, a sodium hydroxide NaOH solution.
[0025] Thus, an advantage provided by such etching agents is to allow selective etching of silicon relative to a silicon oxide.
[0026] According to a characteristic of the invention, the laser radiation is applied during step c) in a direction parallel to the normal to the first and second surfaces of the substrate.
[0027] Thus, an advantage provided is to optimize the useful volume of the photovoltaic cell used during step a) to manufacture photovoltaic sub-cells.
[0028] According to a characteristic of the invention, the laser radiation applied during step c) is pulsed radiation having a fluence and a pulse duration adapted to obtain an ablation of the first dielectric layer, of the first stack of active layers, and of the first part of the substrate.
[0029] According to a characteristic of the invention, the separate photovoltaic sub-cells at the outcome of step e) have exposed side edges; the method comprising a step f) consisting of passivating the exposed side edges.
[0030] Thus, one advantage provided is to limit recombinations between the carriers, which results in a significant improvement in efficiency.
[0031] According to a characteristic of the invention, step f) comprises a step consisting of forming an aluminum oxide on the exposed lateral edges, by deposition of atomic layers.
[0032] Thus, an advantage provided is to be able to form a good quality passivation layer, after activation of the passivation (for example by annealing or by a treatment of the light exposure type “Light Soaking”), despite a potential high surface roughness of the exposed lateral edges.
[0033] According to a characteristic of the invention, the method comprises a step g) consisting of partially etching the first and second dielectric layers at the end of step e); step g) being carried out so that the partially etched first and second dielectric layers form anti-reflective layers.
[0034] Thus, an advantage provided is to avoid the formation of dedicated anti-reflective layers, requiring their deposition after the removal of the first and second dielectric layers, and thus significantly increasing the operating time of the process.
[0035] Definitions
[0036] - By “substrate” is meant a physical, self-supporting support intended for manufacturing of a photovoltaic cell. The substrate can be a wafer cut from a crystalline silicon ingot.
[0037] - By "crystalline silicon" is meant the multicrystalline form or the monocrystalline form crystalline silicon, therefore excluding amorphous silicon.
[0038] - By "based on" we mean that crystalline silicon is the main material and ma majority composing the substrate.
[0039] - By "active layer" we mean a layer having a role in the func operation of the photovoltaic cell, for example a charge separation role, a charge collection role, an electrical passivation role of the substrate surfaces, an optical anti-reflection role, a sub-cell role (other than crystalline silicon) in the case of a multi-junction, etc.
[0040] - By “plot” we mean an electrical contact pad.
[0041] - By "dielectric" is meant a layer made of a material having a electrical conductivity at 300 K less than or equal to 106 S / cm.
[0042] - By "ablation" is meant an ejection of material from a material passed through by laser radiation at a given fluence.
[0043] - By "contour" is meant all or part of the set of surfaces delimiting the exterior earlier the photovoltaic sub-cells. A partial outline is a part of the set of surfaces externally delimiting the photovoltaic sub-cells. A total contour is the set of surfaces externally delimiting the photovoltaic sub-cells.
[0044] - By "photovoltaic sub-cell" is meant a photovoltaic cell obtained from from a division of the initial photovoltaic cell, used in step a).
[0045] - By "mechanical strength", we mean that the photovoltaic sub-cells, limited at the end of step c), resist rupture in response to mechanical stress.
[0046] - By "at least partially" is meant that the second part of the substrate is by partially or completely chemically etched during step d).
[0047] - By "selective etching" is meant that the silicon of the substrate can be etched without significantly attack the material of the first dielectric layer (and the second dielectric layer). In practice, the etching agent is chosen so that the etching speed of the silicon is at least 3 times higher (preferably 5 times higher, more preferably 10 times higher) than that of the material of the first dielectric layer (and the second dielectric layer).
[0048] - By "spontaneous separation" we mean a rupture of the photo sub-cells voltaic without external stress.
[0049] - By “silicon oxide” is meant an oxide of the empirical formula SixOy.
[0050] - By "passivate" we mean the reduction of carrier recombinations to substrate surfaces. Indeed, the edges of a crystalline silicon substrate have a density of defects (e.g. dangling bonds, impurities, crystal discontinuity, etc.) which can lead to significant losses linked to the surface recombination of carriers in the case of a photovoltaic application.
[0051] - By “aluminum oxide” is meant an oxide of the empirical formula AlxOy. Brief description of the drawings
[0052] Other characteristics and advantages will appear in the detailed description of different embodiments of the invention, the description being accompanied by examples and references to the attached drawings.
[0053] [Fig.l] is a schematic sectional view, illustrating a step a) of a method according to the invention.
[0054] [Fig.2] is a schematic sectional view, illustrating a step b) of a method according to the invention.
[0055] [Fig.3] is a schematic sectional view, virtually illustrating (in dotted lines) the first part of the substrate which will be ablated during step c), and the second part of the substrate, in the extension of the ablations, which will be preserved at the end of step c).
[0056] [Fig.4] is a schematic sectional view, illustrating a step c) of a method according to the invention.
[0057] [Fig.5] is a schematic sectional view, illustrating a step d) of a method according to the invention, the chemical etching of the second part of the substrate being partial.
[0058] [Fig.6] is a schematic sectional view, illustrating a step e) of a method according to the invention after partial chemical etching of the second part of the substrate.
[0059] [Fig.7] is a schematic sectional view illustrating a photovoltaic sub-cell obtained at the end of step e) in the case where the chemical etching of the second part of the substrate is partial during step d).
[0060] [Fig.8] is a schematic sectional view, similar to [Fig.7], illustrating a step f) of a method according to the invention, in which the exposed lateral edges of the photovoltaic sub-cell are passivated.
[0061] [Fig.9] is a schematic sectional view, similar to [Fig.7], illustrating a step g) a method according to the invention, in which the first and second dielectric layers are partially etched.
[0062] [Fig. 10] is a schematic sectional view, similar to [Fig. 5], illustrating a step d) of a method according to the invention, the chemical etching of the second part of the substrate being total. It should be noted that the photovoltaic cell illustrated in [Fig. 10] aims to improve understanding, but does not strictly represent reality since the second stack of active layers and the second dielectric layer remaining, on the rear face, at the end of the total chemical etching, do not allow mechanical strength of the photovoltaic cell to be ensured (spontaneous separation), their thickness being too small (a few tens to a few hundreds of nm).
[0063] [Fig. 11] is a schematic sectional view, similar to [Fig. 6], illustrating a step e) of a method according to the invention after total chemical etching of the second part of the substrate. It should be noted that the photovoltaic cell illustrated in [Fig. 11] aims to improve understanding, but does not strictly represent reality since the second stack of active layers and the second dielectric layer remaining, on the rear face, at the end of the total chemical etching, do not allow mechanical strength of the photovoltaic cell to be ensured (spontaneous separation), their thickness being too small (a few tens to a few hundreds of nm).
[0064] [Fig. 12] is a schematic sectional view, similar to [Fig. 7], illustrating a photovoltaic sub-cell obtained at the end of step e) in the case where the chemical etching of the second part of the substrate is complete during step d).
[0065] [Fig. 13] is a schematic top view of a photovoltaic cell used in step a), virtually illustrating (in dotted lines) a future outline that can be drawn in step c).
[0066] [Fig. 14] is a schematic top view of a photovoltaic sub-cell obtained by a method according to the invention, from the photovoltaic cell illustrated in [Fig. 13],
[0067] It should be noted that the drawings described above are schematic, and are not necessarily to scale for the sake of readability and to simplify their understanding. The sections are made along the normal to the first and second surfaces of the substrate. Detailed description of the implementation methods
[0068] Elements that are identical or provide the same function will bear the same references for the different embodiments, for the sake of simplification.
[0069] An object of the invention is a method for manufacturing photovoltaic sub-cells Cl, comprising the steps: a) use a photovoltaic C0 cell, comprising: - a substrate 1, based on crystalline silicon, having first and second opposite surfaces 10, 11; - first and second stacks 2a, 2b of active layers, formed respectively on the first and second surfaces 10, 11 of the substrate 1; - first and second sets PI, P2 of metal pads, formed respectively on the first and second stacks 2a, 2b of active layers; b) forming first and second dielectric layers 3a, 3b, extending respectively over the first and second sets PI, P2 of metal pads, and extending respectively over the first and second stacks 2a, 2b of active layers; c) applying laser radiation L to the photovoltaic cell C0 obtained at the end of step b) so as to: - locally obtaining, between metallic pads PI of the first set, ablations Al of the first dielectric layer 3a, of the first stack 2a of active layers, and of a first part SI of the substrate 1; - draw a contour C delimiting photovoltaic sub-cells Cl; - retain a second part S2 of the substrate 1, extending in the extension of the ablations Al, and adapted to retain mechanical strength of the photovoltaic sub-cells Cl delimited by the traced contour C; d) chemically etching, with an etching agent, at least partially the second part S2 of the substrate 1 extending in the extension of the ablations Al obtained at the end of step c), so as to weaken the photovoltaic sub-cells Cl delimited at the end of step c); the etching agent being chosen so as to allow selective etching of the silicon relative to the first and second dielectric layers 3a, 3b; e) separating the weakened photovoltaic Cl sub-cells at the end of step d).
[0070] Step a)
[0071] Step a) consists of using a photovoltaic C0 cell, comprising: - a substrate 1, based on crystalline silicon, having first and second opposite surfaces 10, 11; - first and second stacks 2a, 2b of active layers, formed respectively on the first and second surfaces 10, 11 of the substrate 1; - first and second sets PI, P2 of metal pads, formed respectively on the first and second stacks 2a, 2b of active layers.
[0072] The substrate 1 is based on crystalline silicon. The substrate 1 is advantageously made from monocrystalline silicon, preferably n-type doped. The first and second surfaces 10, 11 of the substrate 1 are intended to be exposed to light radiation (solar radiation). The first surface 10 of the substrate 1 may be intended to form the front face of the photovoltaic cell C0, while the second surface 11 of the substrate 1 may be intended to form the rear face of the photovoltaic cell C0.
[0073] Each of the first and second stacks 2a, 2b of active layers may comprise a passivation layer. By way of non-limiting example, the passivation layer may be made of a hydrogenated amorphous silicon, denoted a-Si:H. The hydrogenated amorphous silicon is intrinsic.
[0074] Each of the first and second stacks 2a, 2b of active layers may comprise a charge separation layer, formed on the passivation layer. The charge separation layer of the first stack 2a of active layers is doped with a first type. The charge separation layer of the second stack 2b of active layers is doped with a second type, opposite to the first type. By way of non-limiting example, the charge separation layer may be made of a-Si:H doped n by phosphorus on the front face, and a-Si:H doped p by boron on the back face.
[0075] Each of the first and second stacks 2a, 2b of active layers may comprise a transparent conductive oxide (e.g. indium-tin oxide ITO) formed on the charge separation layer. As a non-limiting example, the transparent conductive oxide of the first stack 2a of active layers (front face) may be made of ITO with a thickness of 10 nm. The transparent conductive oxide of the second stack 2b of active layers (rear face) may be made of ITO with a thickness of 80 nm.
[0076] The first and second surfaces 10, 11 of the substrate 1 may be flat. The first and second surfaces of the substrate 1 are advantageously textured in order to reduce the reflection coefficient and the optical losses in the photovoltaic cell C0. The first and second surfaces 10, 11 of the substrate 1 advantageously have a surface area greater than 120 cm2.
[0077] The first and second sets PI, P2 of metal pads are made of a metallic material, which may be for example silver Ag, copper Cu, or aluminum Al.
[0078] The photovoltaic CO cell used during step a) preferably has a square or rectangular shape.
[0079] The photovoltaic CO cell used in step a) may be of the heterojunction silicon type (i.e. amorphous silicon / crystalline silicon heterojunction). However, other photovoltaic cell architectures are conceivable, for example a TOPCon (“Tunnel Oxide Passivated Contact”) type architecture where the passivated contact comprises a tunnel oxide film and a doped polycrystalline silicon layer, a monolithic multijunction type architecture (e.g. silicon / perovskite tandem cell), a PERC type architecture (passivated emitter and rear cell), or a rear surface field type architecture made of aluminum Al-BSF (BSF for “Back Surface Field”).
[0080] Step a) may include the steps: ai) use a photovoltaic C0 cell, comprising: - a substrate 1, based on crystalline silicon, having first and second opposite surfaces 10, 11; - first and second stacks 2a, 2b of active layers, formed respectively on the first and second surfaces 10, 11 of the substrate 1; a2) forming first and second sets PI, P2 of metal pads, respectively on the first and second stacks 2a, 2b of active layers.
[0081] Step a2) can be carried out by depositing a screen printing paste through a screen printing screen delimiting the patterns of the metal pads P1, P2. The screen printing paste can be spread on the screen printing screen using a doctor blade. The screen printing paste can comprise a metallic mineral matrix in powder form, for example in silver, copper or aluminum (or in a mixture of these elements). The screen printing paste can then be deposited on the screen printing screen using a temporary vehicle conventionally comprising a solvent, a binder, a plasticizer and a dispersant. As a variant, the screen printing paste can comprise an organic matrix, made from a thermosetting polymer, and a metallic filler (silver, copper or aluminum).Step a2) of printing the first and second sets PI, P2 of metal pads (electrodes) is generally followed by annealing steps (evaporation of the solvents, increase in the conductivity of the electrodes). Other metallization techniques are possible for carrying out step a2). Examples include physical vapor deposition, inkjet deposition, vacuum evaporation deposition, and electrodeposition.
[0082] Step a) may include a step a3) consisting of forming alignment marks, for example by printing, in order to subsequently facilitate the alignment of the laser radiation L during step c) relative to the metal pads PI of the first set, and possibly relative to the metal pads P2 of the second set.
[0083] Step b)
[0084] Step b) consists of forming first and second dielectric layers 3a, 3b, extending respectively over the first and second sets PI, P2 of metal pads, and extending respectively over the first and second stacks 2a, 2b of active layers.
[0085] The first and second dielectric layers 3a, 3b completely cover, respectively, the first and second sets PI, P2 of metal pads.
[0086] The first and second dielectric layers 3a, 3b formed during step b) may be made of a silicon oxide. However, other dielectric materials are conceivable. Examples include a silicon oxynitride Six OyNz, a silicon nitride SixNy, an aluminum oxide AlxOy.
[0087] The first and second dielectric layers 3a, 3b may be formed during step b) by a deposition technique known to those skilled in the art. Examples include physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), plasma-enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (LPCVD), etc.
[0088] More precisely, the deposition technique is advantageously chosen to have a compliance rate (ratio between the width of the sides of the deposited dielectric layer 3a, 3b and the surface thickness of the deposited dielectric layer 3a, 3b) sufficient to allow the surface topology of the first and second sets PI, P2 of metal pads to be followed. In this respect, preference will be given to deposition by ALD or deposition by LPCVD which have compliance rates close to 1. In other words, the deposition technique is advantageously chosen to have a dielectric layer 3a, 3b with the greatest possible coverage.
[0089] It is possible to combine several deposition techniques to form a dielectric layer 3a, 3b. For example, the formation of a dielectric layer 3a, 3b can start with an ALD deposition, for excellent conformity, and continue with a PECVD deposition, for high deposition speed.
[0090] The first and second dielectric layers 3a, 3b formed during step b) may have a thickness of between 10 nm and 1 μm, preferably of between 10 nm and 200 nm.
[0091] The first and second dielectric layers 3a, 3b formed during step b) may respectively be made of first and second dielectric materials. The first and second dielectric materials may be identical. However, the first and second dielectric materials may be different. Furthermore, it is also possible to combine several dielectric materials to form a dielectric layer 3a, 3b.
[0092] The main role of the first and second dielectric layers 3a, 3b is to form a protective barrier layer against the chemical attack of step d). In other words, the first and second dielectric layers 3a, 3b act as an etching mask. However, the first and second dielectric layers 3a, 3b may have additional functions. Examples include a function of protection against UV radiation, a buffer layer function to protect the surface active layers, etc.
[0093] Step c)
[0094] Step c) consists of applying laser radiation L to the photovoltaic cell C0 obtained at the end of step b) so as to: - locally obtaining, between metallic pads PI of the first set, ablations Al of the first dielectric layer 3a, of the first stack 2a of active layers, and of a first part SI of the substrate 1; - draw a contour C delimiting photovoltaic sub-cells Cl; - retain a second part S2 of the substrate 1, extending in the extension of the ablations Al, and adapted to maintain mechanical strength of the photovoltaic sub-cells Cl delimited by the traced contour C.
[0095] The laser radiation L is advantageously applied during step c) in a direction d parallel to the normal to the first and second surfaces 10, 11 of the substrate 1.
[0096] The laser radiation L applied during step c) is advantageously a pulsed radiation having a fluence and a pulse duration adapted to obtain an ablation Al of the first dielectric layer 3a, of the first stack 2a of active layers, and of the first part SI of the substrate 1. In other words, the laser radiation L applied during step c) must reach the substrate 1 in order to expose the crystalline silicon. The pulse duration may be of the order of a nanosecond or a picosecond. The scanning speed of the laser radiation L applied during step c) is also adjusted to obtain the desired ablation depth, which may be for example of the order of 25 microns. The width of the amorphized zone of the silicon by the laser irradiation may be of the order of 5 microns.
[0097] The laser radiation L applied during step c) may have a wavelength belonging to the infrared, or to the visible spectrum (e.g. green, blue). As by way of non-limiting example, the wavelength may be 1024 nm.
[0098] The laser radiation L applied during step c) can form an irradiated zone having a diameter of the order of 30 microns.
[0099] It is possible to apply the laser radiation L to the photovoltaic cell C0 obtained at the end of step b) so as to: - locally obtaining, between metal pads P2 of the second set, additional ablations of the second dielectric layer 3b, of the second stack 2b of active layers, and of a first additional part of the substrate 1; - draw a contour C delimiting photovoltaic sub-cells Cl; - retain a second additional part of the substrate 1, extending in the extension of the additional ablations, and adapted to maintain mechanical strength of the photovoltaic sub-cells Cl delimited by the traced contour C.
[0100] Step d)
[0101] Step d) consists of chemically etching, with an etching agent, at least partially the second part S2 of the substrate 1 extending in the extension of the ablations Al obtained at the end of step c), so as to weaken the photovoltaic sub-cells Cl delimited at the end of step c).
[0102] The etching agent is chosen so as to allow selective etching of the silicon relative to the first and second dielectric layers 3a, 3b.
[0103] According to a first embodiment, step d) is executed so that the second part S2 of the substrate 1 is completely chemically etched.
[0104] According to a second embodiment, step d) is executed so that the second part S2 of the substrate 1 is partially chemically etched.
[0105] Step d) advantageously consists of immersing the photovoltaic C0 cell obtained at the end of step c) in an etching bath.
[0106] When the first and second dielectric layers 3a, 3b formed during step b) are made of a silicon oxide, step d) is advantageously carried out so that the etching agent is chosen from a potassium hydroxide KOH solution, a tetramethylammonium hydroxide TMAH solution, a sodium hydroxide NaOH solution. By way of non-limiting example, step d) can be carried out at a temperature of 80°C with a potassium hydroxide KOH solution as etching agent, having a mass percentage of 2.5%.
[0107] Step e)
[0108] Step e) consists of separating the photovoltaic sub-cells C1 weakened at the end of step d).
[0109] When step d) is carried out so that the second part S2 of the substrate 1 is completely chemically etched, step e) consists of a spontaneous separation of the photovoltaic sub-cells Cl weakened at the end of step d).
[0110] When step d) is performed so that the second part S2 of the substrate 1 is partially chemically etched, step e) is advantageously performed by a separation technique chosen from thermal shock, mechanical stress, and ultrasonic treatment. Those skilled in the art know how to adjust the parameters of the thermal shock, the mechanical stress, and the ultrasonic treatment in order to obtain physical separation.
[0111] The photovoltaic sub-cells Cl separated at the end of step e) have exposed lateral edges BL. The photovoltaic sub-cells Cl advantageously have a P / S ratio greater than or equal to 8.9 102 mm1, where “P” is the perimeter of the photovoltaic sub-cell Cl, and “S” is the surface area of the photovoltaic sub-cell Cl.
[0112] Step f)
[0113] The method advantageously comprises a step f) consisting of passivating the exposed BL side edges. In other words, step f) consists of forming a passivation layer 4 on each of the exposed BL side edges.
[0114] Step f) advantageously comprises a step consisting of forming an aluminum oxide 4 on the exposed lateral edges BL, by deposition of atomic layers, prior to a step of activating the passivation by annealing or by a treatment of the light exposure type “Light Soaking”. However, other passivation layers 4 (different passivation materials) can be formed on the exposed lateral edges BL, including by other deposition techniques.
[0115] Step g)
[0116] The method advantageously comprises a step g) consisting of partially etching the first and second dielectric layers 3a, 3b at the end of step e). Step g) is carried out so that the partially etched first and second dielectric layers 3a, 3b form anti-reflective layers. The desired final thickness of the first and second dielectric layers 3a, 3b [at the end of step g)] can be previously verified using reflectivity measurements of the surfaces of the photovoltaic sub-cells C1. By way of non-limiting example, the desired final thickness of the first and second dielectric layers 3a, 3b can be of the order of 100 nm.
[0117] When the first and second dielectric layers 3a, 3b formed during step b) are made of silicon oxide, step g) can be carried out with an acid etching solution, for example based on hydrofluoric acid.
[0118] It should be noted that steps f) and g) can be reversed.
[0119] The invention is not limited to the embodiments disclosed. Those skilled in the art are able to consider their technically effective combinations and to substitute equivalents for them.
Claims
Claims
1. Method for manufacturing photovoltaic sub-cells (Cl), comprising the steps: a) use a photovoltaic cell (CO), comprising: - a substrate (1), based on crystalline silicon, having first and second opposite surfaces (10, 11); - first and second stacks (2a, 2b) of active layers, formed respectively on the first and second surfaces (10, 11) of the substrate (1); - first and second sets (PI, P2) of metal pads, formed respectively on the first and second stacks (2a, 2b) of active layers; b) forming first and second dielectric layers (3a, 3b), extending respectively over the first and second sets (PI, P2) of metal pads, and extending respectively over the first and second stacks (2a, 2b) of active layers; c) applying laser radiation (L) to the photovoltaic cell (CO) obtained at the end of step b) so as to: - locally obtaining, between metal pads (PI) of the first set, ablations (Al) of the first dielectric layer (3a), of the first stack (2a) of active layers, and of a first part (SI) of the substrate (1); - draw an outline (C) delimiting photovoltaic sub-cells (Cl); - retain a second part (S2) of the substrate (1), extending in the extension of the ablations (Al), and adapted to retain mechanical strength of the photovoltaic sub-cells (Cl) delimited by the traced contour (C); d) chemically etching, with an etching agent, at least partially the second part (S2) of the substrate (1) extending in the extension of the ablations (Al) obtained at the end of step c), so as to weaken the photovoltaic sub-cells (Cl) delimited at the end of step c); the etching agent being chosen so as to allow selective etching of the silicon relative to the first and second dielectric layers (3a, 3b); e) separating the weakened photovoltaic sub-cells (Cl) at the end of step d).
2. Method according to claim 1, in which: - step d) is carried out so that the second part (S2) of the substrate (1) is completely chemically etched; - step e) consists of a spontaneous separation of the photovoltaic sub-cells (Cl) weakened at the end of step d).
3. Method according to claim 1, wherein: - step d) is carried out so that the second part (S2) of the substrate (1) is partially chemically etched; - step e) is carried out by a separation technique chosen from thermal shock, mechanical stress, and ultrasonic treatment.
4. Method according to one of claims 1 to 3, in which step d) consists of immersing the photovoltaic cell (CO) obtained at the end of step c) in an etching bath.
5. Method according to one of claims 1 to 4, in which: - the first and second dielectric layers (3a, 3b) formed during step b) are made of a silicon oxide; - step d) is carried out so that the etching agent is chosen from a potassium hydroxide KOH solution, a tetramethylammonium hydroxide TMAH solution, a sodium hydroxide NaOH solution.
6. Method according to one of claims 1 to 5, in which the laser radiation (L) is applied during step c) in a direction (d) parallel to the normal to the first and second surfaces (10, 11) of the substrate (1).
7. Method according to one of claims 1 to 6, in which the laser radiation (L) applied during step c) is a pulsed radiation having a fluence and a pulse duration adapted to obtain an ablation (Al) of the first dielectric layer (3a), of the first stack (2a) of active layers, and of the first part (SI) of the substrate (1).
8. Method according to one of claims 1 to 7, in which the photovoltaic sub-cells (Cl) separated at the end of step e) have exposed lateral edges (BL); the method comprising a step f) consisting of passivating the exposed lateral edges (BL).
9. A method according to claim 8, wherein step f) comprises a step of forming an aluminum oxide (4) on the exposed side edges (BL), by atomic layer deposition.
10. Method according to one of claims 1 to 9, comprising a step g) consisting of partially etching the first and second dielectric layers (3a, 3b) at the end of step e); step g) being carried out so that the partially etched first and second dielectric layers (3a, 3b) form anti-reflective layers.