Rubber composition

The rubber composition with silica, crosslinking system, and methacrylic acid ester copolymer addresses the balance of wet grip and rolling resistance in tires, improving both performance metrics.

FR3143617B1Active Publication Date: 2024-11-29MICHELIN & CO (CIE GEN DES ESTAB MICHELIN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022013425
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-11-29
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Tires face a challenge in achieving optimal grip on wet surfaces while minimizing rolling resistance, as existing rubber compositions struggle to balance these contradictory performance requirements.

Method used

A rubber composition incorporating a silica reinforcing filler, a crosslinking system, and a random copolymer with methacrylic acid ester monomer units, along with a specific coupling agent, enhances the compromise between wet grip and rolling resistance.

Benefits of technology

The composition achieves improved wet grip performance and reduced rolling resistance, as demonstrated by enhanced friction coefficients and lower loss factors, respectively.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a rubber composition comprising a reinforcing filler including silica; a crosslinking system; an elastomer A, a random copolymer comprising monomer units of a 1,3-diene and monomer units of a methacrylic acid ester, the monomer units of the methacrylic acid ester representing at least 30 mole percent of the monomer units of elastomer A; a coupling agent of the formula (R1)n(H)2-nN – R2 – Si(R4)m(OR3)3-m, where n is an integer from 0 to 2, m is an integer from 0 to 2, R1, R3, and R4 are alkyl groups, and R2 is a divalent hydrocarbon group. The rubber composition improves the balance between wet grip and rolling resistance of tires whose tread is made of the rubber composition.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Rubber composition

[0001] The field of the present invention is that of rubber compositions reinforced by a reinforcing filler which includes silica, in particular used in the manufacture of tires for vehicles.

[0002] One of the requirements for a tire is to ensure optimal road grip, particularly on wet surfaces. One way to give the tire high grip on wet surfaces is to use a rubber compound in its tread that exhibits a high hysteresis potential.

[0003] But at the same time, the tire tread must also minimize its contribution to the tire's rolling resistance, that is, be as hysteresis-free as possible. Thus, the rubber composition of the tread must satisfy two conflicting requirements: it must exhibit maximum hysteresis potential to meet the grip requirement and the lowest possible hysteresis to meet the rolling resistance requirement.

[0004] To improve wet grip performance while reducing rolling resistance of a tire tread, it has been proposed to introduce elastomers comprising monomer units of a methacrylic acid ester into the rubber compound of the tread. Reference may be made, for example, to the publication of patent application WO2016 / 001052. However, further improving the trade-off between these two performance characteristics (wet grip and rolling resistance) remains a constant concern for tire manufacturers.

[0005] The inventors discovered during their research that the introduction of a specific coupling agent into a rubber composition constituting a tire tread comprising elastomers including monomer units of a methacrylic acid ester makes it possible to significantly improve the trade-off between wet grip performance and tire rolling resistance.

[0006] Thus, the first object of the invention is a rubber composition comprising: - a reinforcing filler comprising silica - a crosslinking system - an elastomer A, a statistical copolymer comprising monomeric units of a 1,3-diene and monomeric units of a methacrylic acid ester, the monomeric units of the methacrylic acid ester representing at least 30% by mole of the monomeric units of elastomer A - a coupling agent corresponding to the following formula: (R*)n(H)2_nN - R2 - Si(R4)m(OR3)3m(I) where n is an integer ranging from 0 to 2; m is an integer ranging from 0 to 2; R1, R3 and R4 are alkyls; R2 is a divalent hydrocarbon group.

[0007] Another object of the invention is a semi-finished product, in particular a tread, comprising a rubber composition according to the invention.

[0008] The invention also relates to a tire comprising a rubber compound according to the invention or a semi-finished product, preferably a tread, which is according to the invention. Such a tire offers an improved compromise between wet grip performance and rolling resistance. Detailed description

[0009] Any interval of values ​​designated by the expression "between a and b" represents the domain of values ​​going from more than a to less than b (that is to say, bounds a and b excluded) while any interval of values ​​designated by the expression "from a to b" means the domain of values ​​going from a to b (that is to say, including the strict bounds a and b).

[0010] All percentages are mass percentages unless otherwise indicated.

[0011] The abbreviation "pc" means parts by weight per hundred parts of elastomers present in the elastomer matrix.

[0012] The term elastomer matrix refers to all the elastomers present in the rubber composition.

[0013] The compounds mentioned in the description (typically polymers, fillers, plasticizers, coupling agents, the vulcanization system, other additives, etc.) may be of fossil origin or bio-based. In the latter case, they may be partially or totally derived from biomass or obtained from renewable raw materials derived from biomass. Similarly, the compounds mentioned may also come from the recycling of materials already used, that is to say, they may be partially or totally derived from a recycling process, or obtained from raw materials themselves derived from a recycling process.

[0014] In the present application, a carbon chain is understood to mean a chain which contains one or more carbon atoms.

[0015] In this application, Cx shall be a carbon chain (saturated or unsaturated) comprising x carbon atoms (x being an integer) and Cx-Cy shall be a carbon chain (saturated or unsaturated) comprising from x to y carbon atoms (y also being an integer). The designations alkanediyl Cx and alkyl Cx are used to refer respectively to an alkanediyl and an alkyl consisting of a a carbon chain having x carbon atoms. The designations alkanediyl Cx-Cy and alkyl Cx-Cy are used to refer respectively to an alkanediyl and an alkyl consisting of a carbon chain having x to y carbon atoms.

[0016] The invention described in more detail below relates to at least one of the objects defined according to any one of the following embodiments: 1. Rubber composition comprising: - a reinforcing filler comprising silica - a crosslinking system - an elastomer A, a statistical copolymer comprising monomeric units of a 1,3-diene and monomeric units of a methacrylic acid ester, the monomeric units of the methacrylic acid ester representing at least 30% by mole of the monomeric units of elastomer A - a coupling agent corresponding to the following formula: (R>)n(H)2_nN - R2 - Si(R4)m(OR3)3m (I) where n is an integer ranging from 0 to 2; m is an integer ranging from 0 to 2; R1, R3 and R4 are alkyls; R2 is a divalent hydrocarbon group. 2. Rubber composition according to embodiment 1 in which n is strictly less than 2, preferably n is equal to 0. 3. Rubber composition according to any one of embodiments 1 to 2 wherein R2 is a Ci-C5 alkanediyl, preferably a C3 alkanediyl. 4. Rubber composition according to any one of embodiments 1 to 3 in which m is equal to 0. 5. Rubber composition according to any one of embodiments 1 to 4 wherein R3 is an alkyl Ci-C5, preferably an alkyl CrC3, more preferably an alkyl Ci or C2. 6. Rubber composition according to any one of embodiments 1 to 5 in which silica represents more than 50% by mass of the reinforcing filler, preferably more than 80% by mass of the reinforcing filler. 7. Rubber composition according to any one of embodiments 1 to 6 wherein the monomer units of methacrylic acid ester represent at least 40% by mole of the monomer units of elastomer A. 8. Rubber composition according to any one of embodiments 1 to 7 wherein the monomer units of methacrylic acid ester represent at most 90% by mole, preferably at most 80% by mole, more preferably at most 60% by mole of the monomer units of elastomer A. 9. Rubber composition according to any one of the following embodiments 1 to 7 in which the monomer units of methacrylic acid ester represent at most 60% by mole of the monomer units of elastomer A. 10. Rubber composition according to any one of embodiments 1 to 9 in which the methacrylic acid ester conforms to the following formula: CH2=CMe-COOR5 (II) in which: - Me is a methyl group - R5 is an alkyl group, preferably a C2-Ci0 alkyl group, more preferably a C3-C8 alkyl group, even more preferably a C4 alkyl group, advantageously an n-butyl group. 11. Rubber composition according to any one of embodiments 1 to 10 wherein the 1,3-diene is 1,3-butadiene or isoprene or a mixture of 1,3-butadiene and isoprene, preferably 1,3-butadiene. 12. Rubber composition according to any one of embodiments 1 to 11 in which elastomer A is a random copolymer of 1,3-diene and methacrylic acid ester. 13. Rubber composition according to any one of embodiments 1 to 12 wherein the crosslinking system is a vulcanization system. 14. Semi-finished product comprising a composition according to any of the preceding embodiments. 15. Semi-finished product according to embodiment 14 characterized in that it is a tread for a tire. 16. Pneumatic comprising a semi-finished product according to any one of embodiments 14 to 15 or a rubber composition according to any one of embodiments 1 to 13.

[0017] An essential characteristic of the rubber composition according to the invention is that it comprises an elastomer, elastomer A, which includes monomer units of a 1,3-diene and monomer units of a methacrylic acid ester and which is a statistical copolymer.

[0018] The ester of methacrylic acid whose monomeric units constitute elastomer A corresponds in a known manner to the following formula: CH2 = CMe - COOR5 (II) in which: - Me is a methyl group - R5 is a carbon chain.

[0019] Preferably, R5 is a carbon chain comprising at least 2 carbon atoms, optionally substituted or interrupted by one or more heteroatoms. More preferably, R5 is a hydrocarbon chain, that is, one composed exclusively of carbon and hydrogen atoms. More preferably, R5 is an alkyl group.

[0020] Suitable alkyl groups include 2-ethylhexyl, n-octyl, isodecyl, n-tridecyl or n-butyl.

[0021] According to any one of the embodiments of the invention, R5 is preferably a C2-Ci0 alkyl group, more preferably a C3-C8 alkyl group, even more preferably a C4 alkyl group, advantageously an n-butyl group.

[0022] The monomer units of the methacrylic acid ester represent at least 30% by mole, preferably at least 40% by mole, of the monomer units of elastomer A.

[0023] According to a preferred embodiment of the invention, the monomer units of the methacrylic acid ester represent at most 90% by mole, preferably at most 80% by mole, even more preferably at most 60% by mole of the monomer units of elastomer A.

[0024] These preferred ranges for the molar percentages of the monomer units of methacrylic acid ester in elastomer A can be applied to any of the embodiments of the invention.

[0025] Suitable 1,3-dienes, whose monomeric units constitute elastomer A, include, in particular, 1,3-butadiene, 2-methyl-1,3-butadiene, and 2,3-di(Ci-C5 alkyl)-1,3-butadiene such as, for example, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-methyl-3-ethyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, an aryl-1,3-butadiene, and 1,3-pentadiene. The 1,3-diene is preferably 1,3-butadiene, isoprene, or a mixture of 1,3-butadiene and isoprene. More preferably, 1,3-diene is 1,3-butadiene.

[0026] The monomer units of 1,3-diene constituting elastomer A preferentially represent at least 10% by mole of the monomer units of elastomer A.

[0027] According to one embodiment of the invention, elastomer A is an elastomer obtained by radical polymerization, particularly in bulk, in solution, or in dispersed media, especially in emulsions, dispersions, or suspensions. Radical polymerization, particularly in bulk, in solution, or in dispersed media, is a process well known to those skilled in polymer synthesis. The choice of one or another of these three processes can be guided, for example, by the reactivity of the monomers to be polymerized, the polymerization kinetics, or the exothermicity of the polymerization reaction. For the choice of the polymerization process, reference may be made, for example, to the following publications: Macromolecules, 1998, 31, 2822-2827; Macromolecules, 2006, 39, 923-930; J. Am. Chem. Soc. 1951, 73, 5736. This method of rea- The application can be applied to any of the embodiments of the invention.

[0028] According to a preferred embodiment of the invention, elastomer A is a random copolymer of a 1,3-diene as defined above and a methacrylic acid ester of formula (II). Elastomer A can then be obtained by radical polymerization of the 1,3-diene and the methacrylic acid ester according to one of the processes mentioned above. According to this preferred embodiment, advantageously the monomer units of the methacrylic acid ester represent 40 to 60% by mole of the monomer units of elastomer A, and consequently the monomer units of the 1,3-diene represent 40 to 60% by mole of the monomer units of elastomer A.

[0029] The elastomer A itself can be made up of a single elastomer or of several elastomers which differ from each other in their composition or their macrostructure (in particular the distribution of molar masses of the polymer chains which compose them).

[0030] The rubber composition may include, in addition to elastomer A, other elastomers. Other suitable elastomers include those commonly used in rubber compositions for the manufacture of tires, such as polyisoprenes, polybutadienes, isoprene copolymers, and butadiene copolymers such as butadiene-styrene copolymers.

[0031] According to any one of the embodiments of the invention, the proportion of elastomer A in the rubber composition is preferably greater than 50 parts per annum, more preferably greater than 80 parts per annum, and even more preferably equal to 100 parts per annum. When elastomer A is used at a proportion of 100 parts per annum, it is then the only elastomer present in the rubber composition.

[0032] These preferred variants of the elastomer A content in the rubber composition can be applied to any of the embodiments of the invention.

[0033] The rubber composition according to the invention comprises a reinforcing filler comprising silica.

[0034] The silica (SiO2) used can be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenated silica. Examples of highly dispersible precipitated silicas (known as "HDS") include, for example, "Ultrasil" 7000 and "Ultrasil" 7005 silicas from Degussa, "Zeosil" 1165MP, 1135MP and 1115MP silicas from Rhodia, "Hi-Sil" EZ150G silica from PPG, "Zeopol" 8715, 8745 and 8755 silicas from Huber, and high specific surface area silicas as described in application WO 03 / 016387.

[0035] The physical state in which the silica is present is irrelevant, whether it is in the form powder, microbeads, granules, or even balls.

[0036] According to a preferred embodiment of the invention, silica represents more than 50% by mass of the reinforcing filler, preferably more than 80% by mass of the reinforcing filler. These preferred ranges of silica mass proportion in the reinforcing filler can be applied to any one of the embodiments of the invention.

[0037] It should be noted that the reinforcing filler may contain, in addition to silica, at least one other reinforcing filler which may be an inorganic reinforcing filler or an organic reinforcing filler.

[0038] In the present application, "reinforcing inorganic filler" is to be understood, by definition, as any inorganic or mineral filler (regardless of its color and origin (natural or synthetic)), also called "white" filler, "light" filler or even "non-black filler" ("non-black filler") as opposed to carbon black, capable of reinforcing on its own, without any other means than an intermediate coupling agent, a rubber composition intended for the manufacture of tires, in other words, capable of replacing, in its reinforcing function, a conventional carbon black of tire grade; such a filler is generally characterized, in a known way, by the presence of hydroxyl groups (-OH) on its surface.As examples of reinforcing inorganic fillers other than silica, mineral fillers of the aluminous type, in particular alumina (Al2O3) or aluminum (oxide)hydroxides, or reinforcing titanium oxides, for example described in US 6610261 and US 6747087, should also be mentioned.

[0039] If the reinforcing filler contains an organic reinforcing filler, the organic reinforcing filler is preferably carbon black. This organic reinforcing filler, preferably carbon black, is then preferably present in a weight percentage of less than 50%, more preferably less than 20%, relative to the total weight of the reinforcing filler.

[0040] According to the particular embodiment in which silica represents more than 50% by mass of the reinforcing filler, carbon black is preferably used at a rate of less than 20%, more preferably less than 10% (for example, between 0.5 and 20%, in particular between 2 and 10%), and even more preferably less than 5%. Within the indicated ranges, the coloring (black pigmenting agent) and anti-UV properties of carbon black are benefited, without otherwise compromising the typical performance provided by the reinforcing inorganic filler.

[0041] All carbon blacks are suitable as carbon blacks, including those conventionally used in tires. Among the latter, special mention should be made of reinforcing carbon blacks of the 100, 200, and 300 series, or blacks of the 500, 600, or 700 series (ASTM grades), such as NI 15, N134, N234, N326, N330, N339, N347, N375, N550, N683, N772). These carbon blacks can be used in their isolated state, as commercially available, or in any other form, for example as a carrier for some of the rubberizing additives used.

[0042] Preferably, the reinforcing filler content in the rubber compound is between 40 and 200 parts per thousand (ppm). Below 40 ppm, the reinforcement of the rubber compound is insufficient to provide an adequate level of cohesion or wear resistance. Above 200 ppm, there is a risk of increased hysteresis and therefore increased rolling resistance of the tires. More preferably, the reinforcing filler content in the rubber compound is between 60 and 140 ppm. These preferred reinforcing filler content ranges can be applied to any one of the embodiments of the invention.

[0043] To couple the silica to at least one of the elastomers that constitute the elastomer matrix of the rubber composition, particularly in the case where the silica constitutes more than 50% by weight of the reinforcing filler of the rubber composition, a coupling agent (or bonding agent) corresponding to formula (I) is used (R')n(H)2_nN - R2 - Si(R4)m(OR3)3 m(I) in which: - n is an integer ranging from 0 to 2; - m is an integer ranging from 0 to 2; - R1, R3 and R4, whether identical or different, are alkyls; - R2 is a divalent hydrocarbon group.

[0044] As is well known, a coupling agent is an agent capable of establishing a sufficient chemical and / or physical bond between the filler in question and the elastomer, while facilitating the dispersion of this filler within the elastomer matrix. This at least bifunctional agent is intended to ensure a sufficient chemical and / or physical connection between the inorganic filler, in this case silica, and the elastomer.

[0045] The coupling agent of formula (I) can consist either of a single compound (all the molecules of the coupling agent of the composition then have the same chemical structure), or of a mixture of compounds corresponding to formula (I).

[0046] The choice of values ​​for n and m may be guided by the accessibility of the corresponding molecules, for example, according to their commercial availability. The preferred values ​​for n and m may apply to any one of the embodiments of the invention.

[0047] According to any one of the embodiments of the invention, m is preferred tially equal to 0, in which case the coupling agent of formula (I) is a trial-koxysilane.

[0048] Preferably, n is strictly less than 2. According to any one of the embodiments of the invention, more preferably n is equal to 0. The coupling agent is then a primary amine.

[0049] The length of the carbon chains constituting the alkyls represented by the symbols R1 and R4 in formula (I) can vary considerably: they may contain one or more carbon atoms. They may be linear or branched. The choice of alkyl is generally guided by the accessibility of the corresponding molecules, for example, according to their commercial availability. Among the alkyls represented by the symbols R1 and R4, the Ci-C5 alkyls are particularly suitable, and even more so the Ci-C2 alkyls. The alkyls represented by the symbols R1 and R4 may be identical or different.

[0050] According to any one of the embodiments of the invention, the divalent hydrocarbon group R2 of formula (I) is preferably an alkanediyl comprising from 1 to 5 carbon atoms (this type of divalent hydrocarbon group will then be denoted "alkanediyl Ci-C5"), more preferably comprising 3 carbon atoms.

[0051] According to any one of the embodiments of the invention, the carbon chain of the alkyl group R3 of formula (I) is preferably made up of 1 to 5 carbon atoms, more preferably of 1 to 3 carbon atoms, even more preferably of 1 or 2 carbon atoms, advantageously of 2 carbon atoms.

[0052] As a coupling agent, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminoethyltriethoxysilane are particularly suitable, available for example from suppliers Sigma-Aldrich, Gelest and Molport.

[0053] The content of the coupling agent of formula (I) in the rubber composition according to the invention, whether a single compound or a mixture of compounds, is advantageously less than 20 parts per million (ppm), it being understood that it is generally desirable to use as little as possible. Typically, the proportion of the coupling agent of formula (I) is from 0.5% to 15% by weight relative to the amount of silica. Its proportion is preferably between 0.5% and 12 ppm, more preferably in the range of 3% to 10 ppm. This proportion is easily adjusted by those skilled in the art according to the amount of silica used in the composition, and its preferred ranges are applicable to any of the embodiments of the invention.

[0054] Another essential characteristic of the composition according to the invention is that it comprises a crosslinking system.

[0055] The crosslinking system may be based on sulfur, peroxides or their mixtures. In other words, crosslinking can be based on reactions involving sulfur or peroxides, or both. The proportion of the compound(s) that constitute the crosslinking system introduced into the rubber compound is adjusted by a person skilled in the art according to the desired degree of crosslinking of the rubber compound and the chemical nature of the crosslinking system. This degree of crosslinking is determined by a person skilled in the art according to the desired stiffness of the crosslinked rubber compound, this stiffness varying according to the intended application of the rubber compound.

[0056] The crosslinking system according to the invention is preferably a vulcanization system, that is to say a system based on sulfur (or a sulfur-donating agent) and a primary vulcanization accelerator. To this basic vulcanization system, various known secondary accelerators or vulcanization activators such as zinc oxide, stearic acid or equivalent compounds, guanidine derivatives (in particular diphenylguanidine), or known vulcanization retarders may be added, incorporated during the first non-productive phase and / or during the productive phase as described later.A primary or secondary vulcanizing accelerator may be cited as any compound capable of acting as a vulcanizing accelerator for diene elastomers in the presence of sulfur, particularly thiazole-type accelerators and their derivatives, sulfenamide, thiuram, dithiocarbamate, dithiophosphate, thiourea, and xanthate-type accelerators. Sulfur is used at a preferential concentration between 0.5 and 12 parts per million (ppm), particularly between 1 and 10 ppm. The primary vulcanizing accelerator is used in the rubber compound at a preferential concentration between 0.5 and 10 ppm, more preferably between 0.5 and 5.0 ppm. These preferred ranges for sulfur and accelerator concentrations may be applied to any of the embodiments.

[0057] The rubber composition according to the invention may also contain coupling activators, silica coating agents or more generally processing aids capable, in a known manner, by improving the dispersion of the filler in the elastomer matrix and lowering the viscosity of the rubber composition, of improving its processing ability in the raw state, these agents being for example hydrolyzable silanes such as alkylalkoxysilanes, polyols, polyethers, hydroxylated or hydrolyzable polyorganosiloxanes.

[0058] The rubber composition according to the invention may also include all or some of the usual additives commonly used in rubber compositions intended for the manufacture of tires, such as plasticizers, pigments, and protective agents such as anti-stain waxes. ozone, chemical anti-ozonants, antioxidants, anti-fatigue agents and mixtures of such compounds.

[0059] The rubber composition according to the invention can be manufactured in suitable mixers, generally using two successive preparation phases well known to those skilled in the art: a first thermomechanical working or mixing phase (the so-called "non-productive" phase) at high temperature, up to a maximum temperature between 110°C and 190°C, preferably between 120°C and 180°C, followed by a second mechanical working phase (the so-called "productive" phase) down to a lower temperature, typically below 110°C, for example between 40°C and 100°C, a finishing phase during which the crosslinking system is incorporated.

[0060] The rubber composition according to the invention can be prepared according to a process which comprises the following steps: - thermomechanically knead the elastomer matrix, the reinforcing filler, the coupling agent, and the other additives of the rubber composition, with the exception of the crosslinking system, until a maximum temperature of between 110°C and 190°C is reached; - cool the assembly to a temperature below 100°C; - then incorporate the crosslinking system; - knead everything until a maximum temperature below 110°C to obtain a rubber composition.

[0061] After incorporating all the ingredients of the rubber composition, the resulting final composition is then calendered, for example in the form of a sheet or plate, particularly for laboratory characterization, or extruded, for example to form a rubber profile used as a rubber component or semi-finished product, particularly for the manufacture of a tire. The rubber composition according to the invention can be used as a calender in a tire. The calender or extrudate formed from the rubber composition constitutes, in whole or in part, a semi-finished product, in particular a tire.

[0062] Thus, according to a particular embodiment of the invention, the rubber composition according to the invention, which can be either in the raw state (before crosslinking or vulcanization) or in the cured state (after crosslinking or vulcanization), is in a tire, for example in a tire tread.

[0063] Crosslinking (or curing), where applicable vulcanization, is carried out in a known manner at a temperature generally between 130°C and 200°C, for a sufficient time which may vary, for example, between 5 and 120 minutes depending in particular on the curing temperature, the crosslinking system adopted and the re- kinetics ticulation of the composition under consideration.

[0064] The semi-finished product according to the invention has as its essential characteristic that it is made up, in whole or in part, of the rubber composition according to the invention. It can be manufactured according to the process described above.

[0065] The tire tread, another object of the invention, has as its essential characteristic that it is made entirely or partially of the rubber composition according to the invention and defined according to any one of the embodiments of the invention. The tread can be manufactured according to the process described above, which includes an additional step of calendering or extruding the rubber composition.

[0066] The invention also relates to the tread previously described both in the raw state (i.e., before baking) and in the baked state (i.e., after cross-linking or vulcanization).

[0067] The invention also relates to a tire comprising a rubber composition or a semi-finished product according to the invention, which tire is available in both its raw and cured states, the semi-finished product preferably being a tread. In the present invention, the term "tire" (in English, "tire") means a pneumatic or non-pneumatic tire. A pneumatic tire usually comprises two beads intended to contact a rim, a crown consisting of at least one crown reinforcement and a tread, and two sidewalls, the tire being reinforced by a carcass reinforcement anchored in the two beads. A non-pneumatic tire, on the other hand, usually comprises a base, designed, for example, for mounting on a rigid rim, a crown reinforcement ensuring the connection with a tread, and a deformable structure, such as spokes, ribs, or dimples, this structure being disposed between the base and the crown.Such non-pneumatic bandages do not necessarily include a sidewall. Non-pneumatic bandages are described, for example, in documents WO 03 / 018332 and FR2898077. According to any one of the embodiments of the invention, the pneumatic component according to the invention is preferably a pneumatic bandage.

[0068] The aforementioned features of the present invention, as well as others, will be better understood upon reading the following description of several examples of embodiments of the invention, given by way of illustration and not limitation. Examples

[0069] I. Measurements and tests used

[0070] 1.1 Determination of the glass transition temperature of elastomers The glass transition temperatures Tg and glass transition widths ATg of polymers are measured using a Differential Scanning Calorimeter ("Differential Scanning Calorimeter") according to ASTM D3418-08.

[0071] 1.2 Determination of the microstructure of elastomers by NMR (resonance) analysis (Nuclear magnetic field) The determination of the methacrylate unit content is carried out by 1H NMR analysis. Spectra are acquired on a BRUKER Avance 500 MHz spectrometer equipped with a 5 mm BBFO z-grad "broadband" cryosprobe for soluble samples and a 4 mm HRMAS 'H / 13C probe for insoluble crosslinked samples. The quantitative 1H NMR experiment uses a simple 30° pulse sequence and a 5-second repetition delay between each acquisition. The samples are solubilized in deuterated chloroform. Chemical shifts are calibrated with respect to the protonated impurity of chloroform relative to tetramethylsilane, TMS (µppm 'H and µppm 13C at 0 ppm).

[0072] Assignment of 1H NMR signals used for quantification in butadiene / n-butyl methacrylate copolymers: δ 1H (ppm) Number of protons Assignment 3.3-4.4 2 CH2-0 alpha to the ester group of n-butyl methacrylate motifs 4.4-5.0 2 CH2 ethylenic of the 1,2 (vinyl) motifs of the butadiene portion 5.0-5.9 1+2 CH ethylenic of the 1,2 motif of the butadiene portion and 2 CH ethylenic of the 1,4 motif of the butadiene portion

[0073] 1.3 Determination of the macrostructure of elastomers by SEC analysis The SEC (Size Exclusion Chromatography) technique is used, which separates macromolecules in solution according to their size using columns filled with a porous gel. The macromolecules are separated according to their hydrodynamic volume, with the largest being eluted first. SEC (PS calibration): The SEC is coupled to a refractometer, in which case it provides relative information. Using commercial standard products, the various number-average (M„) and weight-average (Mw) molar masses that characterize the polymer's molar mass distribution can be determined, and the polymolecularity index (Ip = MJMn) calculated via a Moore calibration. No special treatment of the polymer sample is required before analysis. It is simply solubilized in the elution solvent at a concentration of approximately 1 g / L. The solution is then filtered through a 0.45 µm porosity filter before injection. The equipment used is a "WATERS alliance" chromatographic system. The elution solvent is tetrahydrofuran, the flow rate is 1 mL / min, the system temperature is 35°C, and the analysis time is 45 min. A set of three AGILENT (Mixed BLS) columns is used. The injected volume of the polymer sample solution is 100 pL. The detector is a "WATERS 2414" differential refractometer, and the chromatographic data processing software is the "WATERS EMPOWER" system. The calculated average molar masses are relative to a calibration curve produced using commercially available "PSS READY CAL-KIT" standard polystyrenes.

[0074] 1.4 Determination of the coefficient of friction The coefficient of friction was measured on a test specimen and is listed in the table of examples under the name "p laboratory". Dynamic friction coefficient measurements were performed using a method identical to that described by L. Busse, A. Le Gai, and M. Küppel (Modelling of Dry and Wet Friction of Silica Filled Elastomers on Self-Affine Road Surfaces, Elastomer Friction, 2010, 51, p. 8). The test specimens were produced by molding and then curing a 6 mm thick square (50 mm x 50 mm) rubber support. After closing the mold, it was placed in a heated platen press at a pressure of 16 bar, at the temperature (typically 150°C) and for the time (typically several tens of minutes) required for the material to cure. The soil used for these measurements was a core sample taken from an actual road surface of BBTM-type bituminous concrete (NF P 98-137 standard).To prevent dewlipping and the development of unwanted adhesion forces between the soil and the material, the soil-specimen system is immersed in a 5% aqueous solution of a surfactant (Sinnozon - CAS number: 25155-30-0). The temperature of the aqueous solution is regulated using a thermostatic bath. The specimen is subjected to a sliding motion in translation parallel to the plane of the soil. The sliding velocity Vg is fixed at 1.2 m / s. The applied normal stress on is 300 kPa. These conditions are described below as "wet soil conditions." The shear stress ot, opposing the movement of the specimen on the soil, is continuously measured. The ratio between the shear stress ot and the normal stress on gives the coefficient of dynamic friction p.The values ​​of p are measured for an aqueous solution temperature of 5 to 45°C, and obtained in steady state after stabilization of the value of the shear stress ot. The maximum dynamic friction coefficient over the aqueous solution temperature range of 5 to 45 °C (denoted "p laboratory max" in the examples table) is a relevant descriptor of intrinsic wet surface adhesion performance of the tested rubber composition. The results being expressed on a base of 100, a value higher than that of the reference, arbitrarily set at 100, indicates an improved result.

[0075] 1.5 Determination of the loss factor The dynamic properties tan θ max are measured on a viscoelastic analyzer (Metravib VA4000), according to ASTM D 5992-96. The response of a vulcanized composite sample (cylindrical specimen 4 mm thick and 400 mm² cross-section) is recorded under sinusoidal loading in alternating simple shear at a frequency of 10 Hz, under standard temperature conditions (23°C) according to ASTM D 1349-99. A strain amplitude sweep is performed from 0.1% to 100% (forward cycle), then from 100% to 0.1% (return cycle). The result used is the loss factor tan θ between the values ​​at 0.1% and 100% strain (Payne effect). For the return cycle, the maximum observed tan θ value is recorded, denoted tan θ max return. The maximum return tan θ is a relevant descriptor of the intrinsic rolling resistance performance of the tested rubber compound. Since the results are expressed as a base of 100, a value lower than the reference value, arbitrarily set at 100, indicates an improved result (lower rolling resistance).

[0076] II Preparation of the elastomer The elastomer used for the examples is prepared as follows:

[0077] The reaction takes place in a 10-liter reactor. 67 g (5 wt.) of sodium stearate are dissolved in 2.56 liters of demineralized water. 1 g of tert-dodecyl mercaptan (0.05 transfer agent equivalent to potassium persulfate), 369 g of 1,3-butadiene, and 990.5 g of n-butyl methacrylate are added to the reaction mixture. The reactor is heated to 50°C and the stirring is started. 25.6 g (1.2 wt.) of potassium persulfate in solution in 789 mL of water are then added. After 80 minutes of polymerization reaction, 60% conversion of monomers to copolymer is achieved. The reaction is then stopped by adding 27.5 g of resorcinol (2.6 equivalents of resorcinol relative to potassium persulfate) in solution in 789 mL of water. The latex is then coagulated in two volumes of an acetone / ethanol mixture. The copolymer is then dried in an oven at 45°C.0.74 kg of 1,3-butadiene and n-butyl methacrylate copolymer are recovered with a volatile matter content of less than 1%.

[0078] The resulting copolymer has the following characteristics: Tg = -46°C and ATg = 7°C Mn = 356,000 g / mol (PS calibration) and Ip = 3.4 molar % (n-butyl methacrylate monomer unit) = 44.4 molar % (butadiene monomer unit) = 55.6

[0079] III. Preparation of rubber compositions Two Cl and C2 rubber compositions are prepared. The formulations (in pieces) of the Cl and C2 compositions are described in Table 1.

[0080] Composition C2 conforms to the invention; composition Cl does not conform to the invention. Compositions Cl and C2 both contain an elastomer, a statistical copolymer comprising monomer units of a 1,3-diene (in this case, monomer units of 1,3-butadiene) and monomer units of a methacrylic acid ester (in this case, monomer units of n-butyl methacrylate), the methacrylic acid ester monomer units representing at least 30% by mole (in this case, 44% by mole) of the elastomer monomer units. Compositions Cl and C2 both also contain a reinforcing filler, in this case, silica. Compositions Cl and C2 both also contain a coupling agent. In composition Cl, the coupling agent is bis(triethoxysilylpropyl)tetrasulfide, commonly known as TESPT and marketed as "Si69" by Evonik. One molecule of this coupling agent contains six ethoxysilyl groups. In formula C2, the coupling agent is (3-aminopropyl)triethoxysilane of formula (III), also known as "Gamma-APS Silane" (GAPS). One molecule of this coupling agent contains three ethoxysilyl Si-O-Et groups. Formula (III) !— bb^. / \

[0081] The formulas of the Cl and C2 compositions are such that they contain the same number of moles of ethoxysilyl functions from the coupling agent per unit mass of silica. The crosslinking systems of Cl and C2 compositions are vulcanization systems.

[0082] The manufacturing process for these compositions is carried out as follows: the elastomer, silica, coupling agent, plasticizer, and various other ingredients, with the exception of the crosslinking system, are successively introduced into an internal mixer (final filling rate: approximately 70% by volume), the initial tank temperature of which is approximately 60°C. A thermomechanical process (non-productive phase) is then carried out in a single step, lasting a total of 5 minutes, until a maximum "drop" temperature of 165°C is reached. The mixture thus obtained is collected, cooled, and then the crosslinking system is incorporated on a mixer (homo-finisher) at 23°C, mixing everything (productive phase) for an appropriate time (for example between 5 and 12 min). The compositions thus obtained are then calendered into plates (with a thickness ranging from 2 to 3 mm) or thin sheets of rubber, for the measurement of their physical properties after vulcanization for 30 min at 170°C.

[0083] IV. Properties of rubber compositions The properties of the Cl and C2 compositions are given as a base of 100 relative to Cl in Table 2.

[0084] Composition C2, according to the invention, has a tan θ max significantly lower than that of composition Cl (index 49 on a base of 100), which means that it has a significantly improved rolling resistance performance compared to that of composition CL Furthermore, composition C2, according to the invention, exhibits a laboratory p-value significantly higher than that of composition Cl (index 116 on a base of 100), meaning that it has a significantly superior wet surface adhesion performance compared to composition CL. The results obtained therefore show that the composition according to the invention makes it possible here to solve the technical problem in that it leads to a better compromise between adhesion on wet ground and rolling resistance.

[0085] [Tables 1] Cl C2 Elastomer (1) 100 100 Silica (2) 91.5 91.5 Silane Si69 (3) 9.1 - Silane GAPS (4) - 7.5 Plasticizer (5) 33.5 33.5 DPG (6) 1.5 1.5 Antioxidant (7) 1.9 1.9 Stearic acid 2 2 ZnO (8) 3 3 Sulfur 1.5 1.5 Sulfenamide (9) 1.5 1.5

[0086] (1) Copolymer of 1,3-butadiene and n-butyl methacrylate (see paragraph II.) (2) "Zeosil 1165 MP" silica from the company Solvay-Rhodia in the form of microbeads (3) Liquid silane triethoxysilylpropyltetrasulfide (TESPT) “Si69” from the Evonik company (4) Silane 3-aminopropyltriethoxysilane “SIA0610.0” from the company Gelest (5) Trioctyl phosphate (tri-2-ethylhexyl phosphate) “Disflamoll TOF” from the Lanxess company (6) Diphenylguanidine (“Perkacit” DPG from Flexsys) (7) N-(l,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (“6PPD” from Flexsys) (8) ZnO, industrial grade zinc oxide from Umicore (9) N-cyclohexyl-2-benzothiazol-sulfenamide (“Santocure CBS” from Flexsys)

[0087] [Tables2] Cl C2 tan θ max return 23 °C 10 Hz 100 49 p laboratory max 3 bars 1.2 m / s 100 116

Claims

Claims

1. Rubber composition comprising: - a reinforcing filler comprising a silica - a crosslinking system - an elastomer A, a random copolymer comprising monomer units of a 1,3-diene and monomer units of a methacrylic acid ester, the monomer units of the methacrylic acid ester representing at least 30 mol% of the monomer units of the elastomer A - a coupling agent corresponding to the following formula: (R*)n(H)2_nN - R2 - Si(R4)m(OR3)3m (I) where n is an integer ranging from 0 to 2; m is an integer ranging from 0 to 2; R1, R3 and R4 are alkyls; R2 is a divalent hydrocarbon group.

2. Rubber composition according to claim 1 in which n is strictly less than 2, preferably n is equal to 0.

3. Rubber composition according to any one of claims 1 to 2 in which R2 is a C1-C5 alkanediyl, preferably a C3 alkanediyl.

4. A rubber composition according to any one of claims 1 to 3 wherein m is 0.

5. Rubber composition according to any one of claims 1 to 4 in which R3 is a C1-C5 alkyl, preferably a C1-C3 alkyl, more preferably a C1 or C2 alkyl.

6. Rubber composition according to any one of claims 1 to 5 in which the silica represents more than 50% by mass of the reinforcing filler, preferably more than 80% by mass of the reinforcing filler.

7. A rubber composition according to any one of claims 1 to 6 wherein the monomer units of the methacrylic acid ester represent at least 40 mol% of the monomer units of elastomer A.

8. Rubber composition according to any one of claims 1 to 7 in which the monomer units of the methacrylic acid ester represent at most 90 mol%, preferably at most 80 mol%, more preferably at most 60 mol% of the monomer units of elastomer A.

9. A rubber composition according to any one of claims 1 to 8 in which the methacrylic acid ester corresponds to the following formula: CH2=CMe-COOR5 (II) in which: - Me is a methyl group - R5 is an alkyl group, preferably a C2-Ci0 alkyl group, more preferably a C3-C8 alkyl group, even more preferably a C4 alkyl group, advantageously an n-butyl group.

10. A rubber composition according to any one of claims 1 to 9 wherein the 1,3-diene is 1,3-butadiene or isoprene or a mixture of 1,3-butadiene and isoprene, preferably 1,3-butadiene.

11. A rubber composition according to any one of claims 1 to 10 wherein elastomer A is a random copolymer of 1,3-diene and methacrylic acid ester.

12. A rubber composition according to any one of claims 1 to 11 wherein the crosslinking system is a vulcanization system.

13. A semi-finished product comprising a composition according to any one of the preceding claims.

14. Semi-finished product according to claim 13 characterized in that it is a tire tread.

15. A tire comprising a semi-finished product according to any one of claims 13 to 14 or a rubber composition according to any one of claims 1 to 12.