Process for rectifying a polymer film

A method for covering low-wetting surfaces with thermoplastic polymers using a non-stick second substrate and finishing treatment addresses dewetting issues, ensuring complete coverage and facilitating electronic component manufacturing.

FR3147133A1Inactive Publication Date: 2024-10-04COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
FR2023003106
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing electronic component manufacturing processes face challenges in covering low-wetting surfaces with polymer films, leading to dewetting and uncovered areas that hinder subsequent processes.

Method used

A method involving a first substrate with a low surface energy, application of a thermoplastic polymer, bonding with a non-stick second substrate, and a finishing treatment to cover dewetted zones, followed by disassembly to achieve a continuous polymer film on the first substrate.

Benefits of technology

The method ensures complete coverage of low-wetting surfaces with a continuous polymer film, maintaining mechanical strength during bonding and allowing easy disassembly, facilitating subsequent manufacturing steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method for rectifying a polymer film (3) comprising the steps of: supplying a first substrate (1) comprising a front surface (2), the front surface (2) having a surface energy of less than about 22 mJ / m², spreading a thermoplastic polymer on the front surface (2) leading to the formation of a polymer film (3) and at least one dewetting zone (8) of the front surface (2), supplying a second substrate (4) comprising a non-stick surface (5), bonding the polymer film (3) and the non-stick surface (5) leading to the formation of a bonding interface (7) having an adhesion energy (Ea2) lower than the adhesion energy (Ea1) between the polymer film (3) and the front surface (2), applying a creep treatment such that at least one dewetting zone (8) of the front surface (2) is covered by creep of the polymer film (3),and disassembly at the bonding interface (7) so as to obtain the front surface (2) completely covered by the rectified polymer film (3). Figure for the abbreviation: figure 5,
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Method for rectifying a polymer film

[0001] The present invention relates to the field of semiconductor material structures for the manufacture of electronic components. In particular, the invention relates to a method for rectifying a polymer film on a poorly wetting surface. According to another aspect, the invention provides a multilayer structure obtainable by said method and an intermediate structure obtainable during said method.

[0002] Electronic component manufacturing processes often use organic polymers in the form of thin films. The polymer can be used for various applications:

[0003] • It can act as a permanent or temporary adhesive

[0004] • It can play a role as an electrical insulator

[0005] • It can protect components by encapsulating them

[0006] • It can be used as a masking resin during a photolithography step. photography, etc.

[0007] The polymer is generally provided in solution. It is spread as a thin film on a substrate such as a silicon wafer by spin coating. The spreading process results in a covering film of uniform thickness. However, if the surface on which it is spread is not sufficiently wetting, for example a surface with low surface energy, the polymer dewets and uncovered surface areas are observed. This structure makes it impossible to use the wafer, in particular for the aforementioned subsequent processes.

[0008] One of the aims of the present invention is to overcome at least the problem of covering a poorly wetting surface with a polymer film. To this end, the present invention provides a method for rectifying a polymer film comprising the steps of:

[0009] a) providing a first substrate comprising a front surface, the front surface having a surface energy of less than about 22mJ / m2,

[0010] b) spreading a thermoplastic polymer on the front surface leading to the formation of a polymer film and at least one dewetted area of ​​the front surface,

[0011] c) providing a second substrate comprising a non-stick surface,

[0012] d) bonding of the polymer film and the non-stick surface leading to the formation of a bonding interface having an adhesion energy Ea2 lower than the adhesion energy Eal between the polymer film and the front surface,

[0013] e) applying a finishing treatment to the polymer film so that the at least one dewetted area is covered by the finishing of the polymer film, and

[0014] f) disassembly of the second substrate and the first substrate at the bonding interface so as to obtain the front surface completely covered by the rectified polymer film.

[0015] Thus, the method of the invention advantageously uses the ability of thermoplastic polymers to flow to cover the dewetted areas of the low-wetting front surface by fining. The front surface is thus completely covered by the polymer film at the end of step e) or f). The polymer film obtained is continuous. Its exposed surface has a roughness identical to that of the surface of the second substrate. The fact of providing a non-stick surface on the second substrate allows low energy adhesion Ea2, in particular by the presence of Van der Waals type bonding, which allows the mechanical strength of the assembly bonded in step d) but which allows disassembly in step f).

[0016] The term 'dewetting' and its derivatives are understood in this document to mean the meaning used in physical chemistry which translates the fact that a film deposited on a surface spontaneously withdraws from an area of ​​said surface leading to a reduction in the contact area between the surface and the film.

[0017] The expression 'non-stick surface or film' means a surface or film which provides low adhesion with an object brought into contact with it, typically an adhesion energy less than or equal to approximately 1100 mJ / m2, in particular an adhesion energy less than or equal to approximately 1000 mJ / m2 and for example an adhesion energy less than or equal to approximately 900 mJ / m2.

[0018] According to one possibility, the adhesion energy Eal between the front surface and the polymer film and the adhesion energy Ea2 between the polymer film and the non-stick surface respects the following condition Eal > Ea2 + 100mJ / m2 so as to be able to easily dismantle the bonding interface in step f) while retaining the polymer film on the first substrate, covering the entire non-stick surface.

[0019] According to one arrangement, step b) is carried out by deposition by centrifugal coating (method also known as 'spin coating') of a liquid formulation comprising the thermoplastic polymer on the front surface.

[0020] According to one possibility, step b) comprises, after deposition by centrifugal coating, at least one step of applying a heat treatment for evaporation of one or more solvents of the liquid formulation.

[0021] According to another arrangement, step b) is carried out by deposition by nebulization (method also known as spray coating) of a liquid formulation comprising the thermoplastic polymer on the front surface.

[0022] According to a variant, step b) is carried out by dipping at least the front surface in a liquid formulation comprising the thermoplastic polymer.

[0023] According to one arrangement, the bonding step d) leads to the formation of an intermediate structure comprising the first substrate bonded to the second substrate with an energy Eal adhesion.

[0024] According to one arrangement, the finishing treatment according to step e) is obtained by applying a heat treatment to the polymer film, in particular to obtain a viscosity of the polymer film of less than 104 Pa.s. This viscosity allows the polymer to flow sufficiently to be able to spread and permanently cover the dewetted areas of the front surface of the first substrate. A multilayer structure comprising a rectified polymer film covering the entire front surface of the first substrate is then obtained.

[0025] According to one possibility, the heat treatment is carried out at a temperature T higher than the glass transition temperature Tg of the thermoplastic polymer, and in particular such that T > Tg +100°C. Compliance with this condition guarantees that the desired viscosity of the polymer is achieved. It can then spread to cover the dewetted area(s) of the front surface.

[0026] According to one arrangement, the creep treatment according to step e) is carried out under a pressure (or vacuum) of 0.01 Pa. This condition in particular avoids the presence of oxygen during step e) which could lead to degradation of the polymer film.

[0027] According to a particular embodiment of the invention, step e) of the creep treatment is completed by applying compression to the first substrate bonded to the second substrate. This compression is preferably applied in a direction substantially perpendicular to the plane of the bonding interface, in particular with an intensity of between 0.02 and 2 MPa, more specifically between 0.1 and IMPa for first and second substrates of 200 or 300 mm in diameter.

[0028] In practice, the compression can be applied directly in a thermocompression gluing machine.

[0029] Concretely, the dismantling step f) comprises the application of a mechanical stress to the bonding interface between the polymer film and the non-stick surface, such as the insertion of a wedge, a blade at the interface, or a jet of fluid, etc.

[0030] Alternatively, the mechanical stress is exerted by applying a tensile and / or shear force, or bending force to the structure obtained in step e).

[0031] According to one arrangement, the front surface of the first substrate has a high topography, for example linked to the presence of pillars of a few tenths of a micrometer in diameter over a height of a few micrometers or a few tens of micrometers.

[0032] According to one possibility, the second substrate comprises a rigid wafer and a release film forming the release surface.

[0033] By rigid wafer is meant a wafer which has the same rigidity properties as the first substrate.

[0034] Concretely, the material of the rigid wafer is chosen from silicon, germanium, glass, sapphire, SiC, GaAs, InP, LNO or LTO.

[0035] According to an exemplary embodiment, the non-stick film is formed by deposition on the rigid plate.

[0036] According to one possibility, the non-stick film is obtained from compounds chosen from organosilylates, such as OTS supplied by Sigma Aldrich, fluorinated polymers, such as the polymer 'Novec™ 1720 EGC' (for Electronic Grade Coating) from 3M™, Optool supplied by the company DAIKIN and the polymer 'Novec™ 2702 EGC' (for Electronic Grade Coating) from 3M™. One of the compounds is deposited by spin coating until a non-stick film having a thickness of approximately 5 nanometers is obtained on the rigid wafer.

[0037] According to a particular embodiment of the invention, the non-stick film is obtained by placing a sheet of non-stick material on said rigid wafer, such as a sheet of UPILEX-S polyimide or Teflon / PTFE. Said sheet preferably has a thickness sufficient to be self-supporting, in particular a few tens of micrometers. For example, the sheet of UPILEX-S polyimide or Teflon / PTFE has a thickness of approximately 50 micrometers.

[0038] According to this particular arrangement, step f) comprises the separation between the rigid wafer and the polymer film bonded to the first substrate, then the peeling of the sheet of non-stick material from the polymer film.

[0039] According to one possibility, the second substrate is a Teflon plate, in particular having a thickness of a few tens of mm, so as to guarantee the mechanical resistance necessary for carrying out the disassembly step f). Of course, the Teflon plate alone constitutes the second substrate and the non-stick surface.

[0040] Advantageously, the method comprises, before step b), a trimming step comprising the removal of material from the front surface of the first substrate so as to form a recess in an annular peripheral region of the first substrate. The recess makes it possible to receive any overflow of the thermoplastic polymer in the finishing step e).

[0041] According to one arrangement, the annular peripheral region extends along the peripheral periphery of the first substrate.

[0042] According to one possibility, the recess has a width L of between approximately 0.5 and 3 mm.

[0043] According to one arrangement, the recess has a height H of between 50 and 250 micrometers. The dimensions of the recess are variable depending on the risks of overflow of the thermoplastic material in the finished state, and therefore on the quantity of thermoplastic material deposited in step b). If the overflow is controlled, it is not necessary to carry out trimming, not to mention that depending on the case, the de- border can be managed by subsequent cleaning.

[0044] In concrete terms, the trimming step is simple to implement and can be carried out using a diamond trimming saw or a lapping machine. This method is inexpensive and allows for high homogeneity in the removal of peripheral material. The width L of the trimming is obtained with a variation of only 10 microns and the height H with a variation of only 1 to 2 microns.

[0045] According to another possibility, the trimming of step c) is carried out by a photolithography step followed by an ion etching or chemical etching step. This method allows a precision of homogeneity in dimensions of width L and height H of less than 1 micrometer.

[0046] According to an alternative embodiment, step e) of finishing treatment is concomitant with step d) of bonding between the polymer film and the non-stick surface.

[0047] According to another possibility, the method further comprises, after step f) - a step g) of bringing the polymer film, covering the front surface of the first substrate, into contact with a front face of a third substrate so as to obtain bonding with an adhesion energy Ea3, - a technological step h) carried out on a rear face of the third substrate, opposite the front face, in particular thinning by lapping followed by chemical-mechanical polishing, and - a step of dismantling i) the first substrate having an adhesion energy with the polymer film Eal < Ea3, so as to recover the third substrate.

[0048] The bonding of the polymer film with the third substrate is a strong bonding, having a high adhesion energy Ea3, and in all cases, greater than Eal.

[0049] This method is particularly advantageous in the case where it is not possible to spread the polymer film on the third substrate.

[0050] According to a second aspect, the invention provides a multilayer structure comprising a polymer film covering the entirety of a front surface of a first substrate, the front surface having a surface energy of less than approximately 22 mJ / m2. This multilayer structure allows the performance of numerous subsequent process steps, particularly in the field of manufacturing electronic components.

[0051] Preferably, the polymer film is made of thermoplastic polymer.

[0052] According to other characteristics, the invention comprises one or more of the following optional characteristics considered alone or in combination: - The adhesion energy Eal between the polymer film and the front surface is less than 0.9 J / m2 and in particular less than 0.5 J / m2 and for example approximately 0.2 J / m2. - The front surface of the first substrate has a surface energy in less than about 20mJ / m2, in particular less than about 18mJ / m2 and for example less than about 16mJ / m2. - The adhesion energy Ea2 between the polymer film and the non-stick surface is between approximately 0.05 J / m2 and 0.1 J / m2. - The polymer film has a thickness between 15 and 120 micrometers. - The front surface comprises a high topography, such as a structured surface, and / or having a low surface energy. - The first substrate is made of semiconductor material such as silicon, germanium, glass, sapphire, SiC, GaAs, InP, LNO or LTO. - The thermoplastic polymer is chosen from BrewerBOND® 305 available from the supplier Brewer Science, TWM12000 available from the supplier TOK and a polymer whose viscosity is less than 10 4Pa.s from a given temperature. - The front surface of the first substrate has a structure consisting of pillars with a height of between 3 and 10 micrometers. - The trimming step is performed before or after the front surface structuring step. - The pillars have a generally square cross-section. - The cross-sectional dimensions are between 3 and 8 micrometers. - The front surface has a structure comprising pillars of 5 micrometers on each side and a height of 5 micrometers with an inter-pillar spacing of 10 micrometers. - At the end of step f) the polymer film extends at least over the entire upper surface of all the pillars of the front surface. - At the end of step f), the lateral sides and the bottom surface of the trenches delimited by the pillars are partially covered with polymer. - The front surface of the first substrate having a surface energy of less than 22 mJ / m2 is constituted by a layer deposited on a substrate. - The release film forming the release surface of the second substrate has a thickness of between 1 and 10 nanometers.

[0053] According to yet another aspect, the present invention provides an intermediate structure comprising the multilayer structure as previously described and a second substrate, the polymer film being bonded to a non-stick surface of the second substrate with an adhesion energy Ea2 lower than the adhesion energy Eal between the polymer film and the front surface of the first substrate, and in particular Eal > Ea2 +100 mJ / m2.

[0054] Other aspects, aims and advantages of the present invention will appear better on reading the following description of the different variant embodiments thereof, given by way of non-limiting example and with reference to the appended drawings. The figures do not necessarily respect the scale of all the elements represented so as to improve their readability. In the remainder of the description, for the sake of simplification, identical, similar or equivalent elements of the different embodiments bear the same numerical references.

[0055] Furthermore, all the adhesion energies described in this document are determined by the double lever technique with imposed displacement (wedge insertion method or Maszara method, well known to those skilled in the art). The attached figures are:

[0056] [Fig.l] illustrates steps a) and b) of the method according to one embodiment of the invention.

[0057] [Fig.2] illustrates steps c) to e) of the method according to the embodiment of [Fig.l].

[0058] [Fig.3] illustrates step f) of the method according to the embodiment of [Fig.2].

[0059] [Fig.4] illustrates step a) and the cutting step of the process according to a second mode of carrying out the invention.

[0060] [Fig.5] illustrates steps b) to e) of the method according to a second embodiment of the invention.

[0061] [Fig.6] illustrates step f) of the method according to the second embodiment of the invention.

[0062] [Fig.7] illustrates a multi-layer structure in which the front surface is structured according to another embodiment of the invention.

[0063] Figures 1 to 3 illustrate the principle of the rectification method according to the invention which makes it possible to cover the entirety of a non-stick or low-wetting surface of a first substrate (surface energy less than approximately 22 mJ / m2) with a polymer film from a liquid formulation of a thermoplastic polymer.

[0064] With reference to [Fig.l], a first substrate 1 whose front surface 2 is poorly wetting is provided (step a), its surface energy is less than 20 mJ / m2. A liquid formulation of a polymer film 3 consisting of a thermoplastic polymer is deposited by spin coating on the front surface 2 (step b - adhesion energy Eal). If necessary, heat treatments are carried out so as to remove the solvents from the liquid formulation after deposition. Dewetting of the polymer film 3 is observed, it leads to the formation of one or more dewet zones 8 of the front surface 2.

[0065] [Fig.2] illustrates the provision according to step c) of a second substrate 4 having a non-stick surface 5. As can be seen in this particular embodiment, the second substrate 4 is formed of a rigid wafer 4' and a non-stick film 5' arranged on the surface, the latter forming the non-stick surface 5. Then according to step d), the polymer film 3 is bonded to the non-stick film 5' to form an intermediate structure 10, the non-stick film 5' being chosen so that the adhesion energy Eal between the polymer film 3 and the first substrate 1 is greater than the adhesion energy Ea2 between the polymer film 3 and the non-stick film 5'. Typically, the adhesion energy Eal is at least greater than Ea2 + 0.1 J / m2.

[0066] A step e) of applying a finishing treatment is then carried out by thermocompression. To do this, a sufficiently high compression and temperature are applied to the intermediate structure 10. The temperature T of the thermocompression step is notably well above the glass transition temperature Tg of the thermoplastic polymer (T> Tg + 100°C). Under these conditions, the polymer film 3 becomes fluid, it thins and fills the dewetted areas 8 of the front surface 2, the finishing and filling of the dewetted areas being guaranteed when the viscosity of the polymer 3 is less than 104 Pa.s.

[0067] As illustrated in [Fig. 3], the application of a mechanical stress, such as the insertion of a wedge into the bonded intermediate structure 10, makes it possible to dismantle the bonding interface 7 which has the lowest adhesion energy Ea2, namely the interface between the polymer film 3 and the non-stick surface 5 of the second substrate 4. Thus, the method of the invention makes it possible to rectify the polymer film 3 on a front surface 2 which is not very wet and to obtain a multilayer structure 20 which can be used in subsequent stages of manufacturing electronic components.

[0068] According to a possibility not illustrated, in replacement of the non-stick film 5' arranged on the rigid plate 4', a non-stick sheet (e.g.: a UPILEX-S polyimide sheet) is inserted between the surface of the polymer film 3 and the rigid plate 4'.

[0069] According to yet another variant not illustrated, the second substrate 4 is a Teflon plate which intrinsically has a non-stick surface 5. Detailed examples of achievement

[0070] The following examples are made using 1,4 silicon substrates with a diameter of 300 mm. Example 1:

[0071] According to a possibility illustrated in [Fig.4], the first substrate 1 is trimmed using a diamond saw so as to form a recess 6 in the annular peripheral region of the front surface 2 over a width L of 1.5 mm and a depth (or height H) of 200 pm. Then a fluorinated layer 2' of Novec™ 1720 is deposited on a first silicon substrate 1 so as to form the poorly wetting front surface 2 ([Fig.4]).

[0072] A thermoplastic polymer of BrewerBOND® 305 is then spread with a thickness of 40 μm on the front surface 2 so as to form the polymer film 3. A dewetting of the polymer 3 is observed. The adhesion energy Eal between the polymer film 3 in BrewerBOND® 305 and the front surface 2 in Novec™ 1720 is 0.2 J / m2.

[0073] On a rigid silicon wafer 4' is deposited a non-stick film 5' of octadecyltrichlorosilane (OTS) from a solution of OTS in isooctane leading to obtaining the second substrate 4 and its non-stick surface 5 ([Fig.5]). Once brought into contact according to step d), the adhesion energy Ea2 between the polymer film 3 in BrewerBOND® 305 and the non-stick surface 5 in OTS is 0.07 J / m2. The first and second substrates 1,4 are then placed at a temperature of 250°C, under a compression of 0.28 MPa, a pressure (or a vacuum) of 0.01 Pa for a duration of 20 min (steps d) and e). These conditions cause the polymer film 3 to thin out of BrewerBOND® 305, which fills the dewetted areas 8 of the front surface 2 (step e). The intermediate structure 10 thus obtained is then dismantled at the bonding interface 7 between the polymer film 3 of BrewerBOND® 305 and the fluorinated non-stick surface 5 by inserting a wedge ([Fig.6]).The final multilayer structure 20 is obtained: the polymer film 3 in BrewerBOND® 305 is rectified, it covers the entire front surface 2 of the first substrate 1. Example 2:

[0074] According to an alternative embodiment not illustrated, a fluorinated layer 2' of Novec™ 1720 is deposited on a first silicon substrate 1 so as to form a low-wetting front surface 2. The first substrate 1 is then cut with a diamond saw to form a recess 6 with a width of 2 mm and a depth of 100 μm.

[0075] A thermoplastic polymer of BrewerBOND® 305 is then deposited to form a polymer film 3 with a thickness of 20 μm on the poorly wetting front surface 2 (step b). Dewetting of the polymer film 3 is observed. The adhesion energy Eal between the polymer film 3 made of BrewerBOND® 305 and the front surface 2 made of Novec™ 1720 is 0.2 J / m2.

[0076] The first substrate 1 is bonded with a rigid silicon wafer 4' on which is placed a 5' sheet of UPILEX-S polyimide of 50 μm, which acts as a non-stick surface 5 between the two substrates 1, 4 (step d). The finishing treatment (step e) is carried out by applying a temperature of 250°C, with a compression of 0.28 MPa, a vacuum of 0.01 Pa over a period of 20 min. These conditions cause the finishing of the polymer film 3 which fills the dewetted areas 8 of the front surface 2 (step e). The adhesion energy Ea2 between the polymer film 3 and the 5' sheet of UPILEX-S is very low, for example < 0.05 J / m2. A wedge is inserted into the intermediate structure 10 to disassemble the rigid wafer 4' then the UPILEX-S sheet is peeled from the surface of the polymer film 3. The multilayer structure 20 obtained comprises the rectified polymer film 3, covering the entire front surface 2 (in Novec™ 1720) of the first substrate 1.

[0077] According to another variant not illustrated, a Teflon / PTFE sheet of a few tens of micrometers is used instead of the UPILEX-S sheet.

[0078] According to an alternative, a single Teflon plate a few tens of millimeters thick is used to replace the second substrate 4 or the rigid plate 4' and the non-stick sheet 5'.

[0079] According to yet another alternative, a press with a Teflon-coated head is used instead of the second substrate having a non-stick surface (not shown). This Teflon-coated press is also used to apply the compression treatment. In this exemplary embodiment, the first substrate will advantageously be held in place, in particular by a suction table, during the raising of the head. This variant advantageously makes it possible to carry out the grinding on several substrates simultaneously. Example 3:

[0080] According to another embodiment variant not illustrated, a first silicon substrate 1 is cut with a diamond saw to form a recess 6 with a width of 3 mm and a depth of 250 μm.

[0081] A layer 2' of perfluorodecyltrichlorosilane (FDTS: C13Si(CH2)2(CF2)7CF3) is deposited on the first substrate 1 cut out, in order to create the poorly wetting front surface 2. A polymer film 3 in TWM12000 of 100 pm is then deposited on the front surface 2 (step b). Dewetting of the thermoplastic polymer film 3 is observed. The adhesion energy Eal between the polymer film 3 in TWM12000 and the front surface 2 in FDTS is 0.9 J / m2.

[0082] A silicon wafer 4' is in parallel covered with an anti-adhesive film 5' of Optool so as to provide the second substrate 4. Contact with the polymer film 3 leads to obtaining the intermediate structure 10 and an adhesion energy Ea2 of less than 0.1 J / m2.

[0083] The finishing treatment is then carried out by applying a heat treatment at a temperature of 240°C with a compression of 0.23 MPa, under a vacuum of 0.01 Pa for a duration of 20 min. These conditions cause the finishing of the thermoplastic polymer film 3 which fills the dewetted areas 8 of the front surface 2 (step e). A wedge is inserted into the structure 10 and the second substrate 4 is dismantled, the final multilayer structure 20 comprising the rectified polymer 3, covering the entire front surface 2 is obtained (step f). Example 4:

[0084] According to an alternative embodiment illustrated in [Fig.7], the method comprises, before step a), a step of photolithography / etching of the front surface 2 of the first silicon substrate 1 so as to structure the surface 2 by creating pillars 9 with lateral dimensions of 5 micrometers by 5 micrometers and also with a height of 5 micrometers, leading de facto to a front surface 2 with low wetting. Step b) consists of depositing a thermoplastic polymer of BrewerBOND® 305 to form a polymer film 3 20 micrometers thick, which leads to a dewetted zone 8 on the front surface.

[0085] A second substrate 4 is provided. It comprises a rigid silicon wafer 4' covered by a non-stick fluorinated film 5' of Novec™ 1720 which forms the non-stick surface 5 (step c). The polymer film 3 is brought into contact with the non-stick surface 5 and then the finishing treatment is applied by carrying out a heat treatment at 250°C accompanied by a compression of 0.28 MPa under a vacuum of 0.01 Pa for a period of 20 minutes (step d) and e)). The finishing of the thermoplastic polymer film 3 makes it possible to fill the dewetted areas 8 of the front surface 2 (step e). The insertion of a wedge at the interface 7 between the polymer film 3 and the non-stick surface 5 allows the disassembly of the second substrate 4 and the obtaining of the multilayer structure 20 in which the polymer film 3 rectified in BrewerBOND® 305 covers the entire structured front surface 2 of the first substrate 1, as illustrated in [Fig.7].

[0086] Also illustrated, the recess obtained by trimming the first substrate 1 acts as a reservoir for the thermoplastic polymer which thins. This makes it possible to prevent it from overflowing from the multilayer structure 20. As seen previously, this trimming step can be omitted if there is no risk of overflow (for example in the case of a very thin layer of polymer film 3) or if the overflow can be managed by subsequent cleaning.

[0087] According to another aspect not illustrated in the figures, the polymer film 3 covering the front surface 2 of the first substrate 1 obtained in step f) is brought into contact according to a step g) with a front face of a third substrate for strong bonding, having an adhesion energy Ea3 > Eal. Steps for producing electronic circuits h) can thus be applied to the third substrate, such as thinning by CMP, deposition, photolithography, etc., thanks to the presence of the first substrate 1 which serves as a handle. Then the first substrate 1 having weak adhesion with the polymer film 3 is disassembled (step i) so as to recover the third substrate. This is particularly advantageous in the case where it is not possible to spread the polymer film 3 on the third substrate.

[0088] Thus, the present invention provides a method which is simple to implement and allowing a polymer film 3 to be rectified on a poorly wetting surface 2 of a substrate 1 which can be used in a large number of subsequent steps for the manufacture of electronic compounds.

Claims

Claims

1. A method of rectifying a polymer film (3) comprising the steps of: a) providing a first substrate (1) comprising a front surface (2), the front surface (2) having a surface energy of less than about 22 mJ / m2, b) spreading a thermoplastic polymer over the front surface (2) resulting in the formation of a polymer film (3) and at least one dewetted area (8) of the front surface (2), c) providing a second substrate (4) comprising a release surface (5), d) bonding the polymer film (3) and the release surface (5) resulting in the formation of a bonding interface (7) having an adhesion energy (Ea2) lower than the adhesion energy (Eal) between the polymer film (3) and the front surface (2), e) applying a finishing treatment to the polymer film (3) such that the at least one dewetted area (8) of the front surface (2) is covered by the finishing of the polymer film (3),and f) disassembling the second substrate (4) and the first substrate (1) at the bonding interface (7) so as to obtain the front surface (2) completely covered by the rectified polymer film (3).,

2. A method of rectifying a polymer film (3) according to claim 1, wherein the finishing treatment according to step e) is obtained by applying a heat treatment to the polymer film (3) so that the polymer film (3) reaches a viscosity of less than 104Pa.s.

3. Method for rectifying a polymer film (3) according to one of claims 1 to 2, in which step e) of the finishing treatment is completed by applying compression to the first substrate (1) bonded to the second substrate (4).

4. Method for rectifying a polymer film (3) according to one of claims 1 to 3, in which the dismantling step f) comprises the application of a mechanical stress to the bonding interface (7) between the polymer film (3) and the non-stick surface (5).

5. A method of rectifying a polymer film (3) according to one of claims 1 to 4, wherein the second substrate (4) comprises a rigid wafer (4') and a release film (5'), the release film (5') forming the release surface (5).

6. A method of rectifying a polymer film (3) according to claim 5, wherein the release film (5') is obtained by placing a sheet of release material on said rigid wafer (4'), such as a sheet of UPILEX-S polyimide or Teflon / PTFE.

7. A method of rectifying a polymer film 3 according to one of claims 1 to 4, wherein the second substrate (4) is a Teflon plate.

8. A method of rectifying a polymer film (3) according to one of claims 1 to 7, which comprises before step b) a trimming step comprising removing material from the front surface (2) of the first substrate (1) so as to form a recess (6) in an annular peripheral region of the first substrate (1).

9. A multilayer structure (20) comprising a ground polymer film (3) covering an entire front surface (2) of a first substrate (1), the front surface (2) having a surface energy of less than about 22 mJ / m2.

10. Intermediate structure (10) comprising the multilayer structure (20) according to claim 9 and a second substrate (4), the polymer film (3) being bonded to a non-stick surface (5) of the second substrate (4) with an adhesion energy (Ea2) lower than the adhesion energy (Eal) between the polymer film (3) and the front surface (2) of the first (1).

Citation Information

Patent Citations

  • Method and apparatus for planarizing a polymer layer

    US20090309253A1

  • Programmable deposition of thin films of a user-defined profile with nanometer scale accuracy

    US20150048050A1

  • A method for manufacturing a handle substrate for the temporary bonding of a substrate

    US20170025301A1

  • Method for manufacturing a nanoimprint lithography mold

    WO2020120627A1