POLYMER DECONTAMINATION PROCESS.

The single-step supercritical fluid extraction process for polyolefins, involving micronization and specific conditions, addresses the inefficiencies of current methods by achieving rapid and effective decontamination of polyolefins, exceeding 99% purity.

FR3147282A1Pending Publication Date: 2024-10-04PAPREC PLASTIQUES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
FR2023002907
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Current polymer purification processes, particularly for polyolefins, are complex and inefficient in achieving high decontamination efficiencies (>98.5%) for a wide variety of contaminants, especially when the incoming material is in the form of granules rather than films, leading to potential degradation and introduction of new contaminants.

Method used

A single-step supercritical fluid extraction process that micronizes contaminated polymer waste into particles with a diameter of 0.1 mm to 1 mm, followed by purification using a supercritical fluid at specific temperature and pressure conditions, effectively removing contaminants.

Benefits of technology

Achieves rapid and efficient decontamination of polyolefins exceeding 99% purity in a single step, simplifying the process and reducing the risk of material degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

POLYMER DECONTAMINATION PROCESS The invention relates to a process (100) for decontaminating a solid composition, referred to as contaminated (C0), from post-consumer waste, comprising the following successive steps: Reduction by micronization (S102) of the contaminated solid composition (C0) into particles (P) having a diameter between 0.1 and 1 mm, to obtain a powder (C1) comprising the polymer (PL) and the contaminants (CONT); Introduction, into an extractor (10) loaded with powder (C1), of a continuous flow of a supercritical fluid (F), the extractor (10) being simultaneously maintained at a temperature between 40°C and 130°C and a pressure between 80 and 450 bar for a period between 5 and 240 min, to physically extract (S104) the contaminants (CONT) by the supercritical fluid (F) and obtain a solid composition, referred to as decontaminated (C2), comprising the Polymer (PL), Figure to be published with the abbreviation: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR DECONTAMINATING POLYMER. TECHNICAL FIELD OF THE INVENTION

[0001] The technical field of the invention is that of technologies for recycling post-consumer and post-industrialization plastic waste, and in particular that of technologies for recycling polymers from post-consumer and post-industrialization, such as polyolefins.

[0002] The present invention relates to a process for decontaminating polymers such as polyolefins by extraction with a supercritical fluid to produce high purity recycled polyolefins. TECHNOLOGICAL BACKGROUND OF THE INVENTION

[0003] Polyolefins are polymers that are very present in plastic waste.

[0004] Polyolefins are particularly widely used in various consumer goods. and, more generally, in food packaging, for example as a type of shrink film.

[0005] Currently, some polyolefins, such as polypropylene (PP) or polyethylene (PE), are not used after recycling for food, medical and cosmetic uses, which constitutes a major obstacle to the implementation of a circular economy for plastics.

[0006] To overcome this obstacle, there is a need to better purify polyolefins, and more generally polymers, during recycling, so that they contain a quantity of pollutants, or contaminants, which does not pose a risk to human health.

[0007] More precisely, it is necessary to be able to purify them with an efficiency of between 98.5% and 100% (depending on the nature of the pollutants). The term "efficiency" designates the decontamination yield E, which is equal to the following ratio:

[0008] • Where Cinit is the initial contaminant concentration, • And Cres is the residual contaminant concentration, i.e., the contaminant concentration at the end of the purification step.

[0009] These strict performance criteria are imposed by the regulations of the American and European agencies FDA (acronym for Food and Drug Administration in English) and EFSA (acronym for European Food Security Authority in English).

[0010] A simple and economical way to purify a solid composition of contaminated polymers is to use an extractor into which an extraction fluid is introduced at the supercritical state.

[0011] Typically, the contaminated material is deposited in the extractor, then a flow of fluid in the supercritical state is introduced through it. As it passes through the material, it detaches the contaminants by dissolving them, and carries them out of the extractor and therefore out of the material. The supercritical state gives the fluid properties of high diffusivity, low viscosity and low surface tension, as well as a certain modularity of the strength of the solvent which particularly favor this extraction process. The extraction conditions are also relatively mild, due to low temperature and pressure, which allows the material not to be degraded.

[0012] Patent application WO2018121980A1 describes such a technique within a process for purifying a contaminated solid polyolefin composition. Specifically, supercritical fluid extraction is implemented in a first step of the process, with well-specified temperature and pressure conditions. To obtain high-purity polyolefin particles, this step is then followed by a step of heating the purified solid composition obtained at the end of the extraction step and then a step of producing particles using a gas-saturated solution or PGSS (acronym for "Particles from Gas Saturated Solutions"). This particle production step simultaneously makes it possible to further improve the purity of the polyolefins.

[0013] Although such a process makes it possible to obtain high-purity recycled polyolefin particles, it remains complex to implement, in particular because three stages (first purification by extraction, heating, particle production / second purification) are necessary.

[0014] The document “Supercritical CO2 extraction of contaminants from polypropylene intended for food contact: Effects of contaminant molecular structure and processing parameters” by Ben Said Anouar et al., Journal of supercritical Fluids 98 (2016) 22-31, describes a process for decontaminating polyolefins comprising a single purification step by extraction with a supercritical CO2 fluid.

[0015] However, satisfactory decontamination efficiencies (greater than 99% for all contaminants tested) are only obtained on condition that the contaminated solid composition is in the form of films 100 μm thick. When this contaminated composition is in the form of granules with an equivalent diameter of 2.5 mm, the efficiency varies between only 94.1% and 32.12% depending on the contaminants.

[0016] In practice, however, it is rather rare for the incoming material to be in the form of films. It is generally rather in the form of ground material (flakes) coming from the shredding of packaging such as bottles, etc. The proportion of films is quite low for polyethylene and even lower for polypropylene.

[0017] This means that, in order to achieve the desired decontamination efficiencies in a single extraction step, it would be necessary to consider producing films with these flakes. Such a step is technically complex and economically unattractive. In addition, there is a significant risk that during this step, new contaminants will be introduced and the polyolefins will be further degraded.

[0018] There therefore remains a need to improve polymer purification processes to obtain, in a simple manner, a decontamination efficiency greater than 98.5%, for a wide variety of contaminants. Summary of the invention

[0019] The invention offers a solution to the problems mentioned above, by making it possible to use only a single purification step by supercritical fluid extraction by reducing the incoming material by micronization into a powder of particles having an equivalent diameter of between 0.1 mm and 1 mm. This avoids a film production step.

[0020] One aspect of the invention relates to a method for decontaminating a so-called contaminated solid composition, derived from post-consumer and / or post-industrialization waste, comprising a polymer and contaminants, said method comprising the following successive steps: • Reduction by micronization of the contaminated solid composition into particles having a diameter between 0.1 mm and 1 mm, to obtain a powder comprising the polymer and the contaminants, • Loading the powder obtained into an extractor, • Introduction, into the powder-laden extractor, of a continuous flow of a supercritical fluid, the extractor being simultaneously maintained at a temperature of between 40°C and 130°C and a pressure of between 80 bars and 450 bars for a duration of between 5 min and 480 min, to physically extract the contaminants by the supercritical fluid and obtain a so-called decontaminated solid composition comprising the polymer, • Unloading of the decontaminated solid composition from the extractor, which has been brought back to temperature and pressure conditions allowing its opening.

[0021] Thus, the purification step by supercritical fluid extraction is carried out on a powder of contaminated polymer particles, the particles having a diameter of between 0.1 mm and 1 mm obtained by a first reduction step by micronization.

[0022] By diameter is meant a mesh diameter, measured by sieving.

[0023] The particles have a shape similar to a sphere, with contours rough, for example with contours that have facets.

[0024] These geometric properties differ from those of the granules. These firstly have an aspect ratio greater than 1. The granules are in fact either in the shape of a flattened sphere or in the shape of a cylinder. Furthermore, in this ratio, the smallest dimension varies between 2 mm and 3 mm (the largest dimension varying between 3 mm and 4 mm for the flattened sphere, and between 4 mm and 5 mm for the cylinder). The size of the granules is therefore greater than that of the particles, and far from the upper limit (1 mm) of the diameter range obtained at the end of the micronization step.

[0025] Experiments carried out within the scope of the invention have shown that, by carrying out micronization before extraction (and not after, as is often the case to obtain purified particles), by specifying it to obtain the specified diameter range for the particles, and by choosing the conditions of temperature, pressure and time in the extractor, a rapid decontamination, for example 140 minutes, and extremely effective, greater than 99%, of all the contaminants tested can be obtained in a simple manner.

[0026] As the particles have a diameter smaller than the diameter of the granules, the distance to penetrate to the core of the particle is reduced, which makes it possible to increase the diffusion speed of the supercritical fluid in the polymer, and therefore to obtain, in a single purification step, better decontamination efficiencies.

[0027] The results obtained on polyolefin films, according to the state of the art or according to the experiments relating to the invention, show that beyond a thickness of 250 μm, some of the heaviest contaminants are not extracted effectively. These results thus suggested that the particle diameter range should also be restricted to 100 μm - 200 μm. However, it has surprisingly turned out that the particle diameter range can be extended well beyond 200 μm, precisely up to 1 mm.

[0028] The fact that the particle diameter range can be extended to 1 mm rather than limiting it to 200 pm is particularly interesting. Indeed, the micronization reduction step is made simpler, and therefore technically feasible.

[0029] In addition to the characteristics which have just been mentioned in the preceding paragraph, the method according to one aspect of the invention may have one or more complementary characteristics among the following, considered individually or according to all technically possible combinations: • the duration in the extractor under the flow of supercritical fluid is between 5 min and 240 min. • the supercritical fluid is based on supercritical CO2. • the flow rate of the supercritical fluid is between 0.1 kg / h and 100 Kg / h, preferably between 0.1 Kg / h and 50 Kg / h. • the contaminated solid composition is in the form of granules. • a load of 1 kg to 10,000 kg of powder comprising the polymer and the contaminants are loaded into the extractor. • the polymer of the contaminated solid composition is a polyolefin such as polypropylene (PP), or polyethylene (PE), or a mixture of polypropylene (PP) and polyethylene (PE) with or without a compatibilizing agent such as maleic anhydride. • the polyolefin of the contaminated composition has melt viscosity properties of between 0.01 g / 10 min and 200 g / 10 min. • the contaminated solid composition includes volatile organic contaminants in a content equal to a maximum of 5000 ppm, and / or non-volatile organic contaminants in a content equal to a maximum of 2000 ppm. • the contaminated solid composition includes pollutants other than the contaminants to be purified, such as: • ethylene vinyl alcohol copolymer or EVOH in a proportion of no more than 10% by mass, • polyamide or PA in a proportion of no more than 10% by mass, • polyethylene terephthalate or PET in a proportion of no more than 10% by mass, or • Aluminum, in a proportion of no more than 5% by mass. • a co-solvent, such as methanol, ethanol or water, is introduced into the extractor, simultaneously with the supercritical fluid during the extraction step. • the supercritical fluid is discharged from the extractor, then separated, in a separator, from the contaminants that were dissolved in the supercritical fluid during extraction, then reinjected into the extractor so that it is recycled. • at the end of the extraction stage, contaminants are extracted with an efficiency greater than 99%. • at the end of the step of unloading the decontaminated solid composition, the method comprises an additional extrusion step to form decontaminated polymer granules from the decontaminated solid composition.

[0030] The invention and its various applications will be better understood by reading the following description and examining the accompanying figures. BRIEF DESCRIPTION OF THE FIGURES

[0031] The figures are presented for information purposes only and in no way limit the invention. • [Fig.l] is a block diagram illustrating the sequence of steps of the decontamination process according to the invention, • [Fig.2] is a block diagram illustrating the sequence of sub-steps of the second step of the process of [Fig.l], • [Fig.3] is a schematic representation of a system for putting implement the method according to the invention. DETAILED DESCRIPTION

[0032] Unless otherwise specified, the same element appearing in different figures presents a unique reference.

[0033] [Fig.l] schematically represents the sequence of steps of a preferred mode of implementation of the method 100 for decontaminating polymers according to the invention.

[0034] This method 100 is particularly remarkable in that it makes it possible to obtain high-purity polymer particles while being quick and simple to implement.

[0035] With reference to [Fig.l], the method comprises the successive main steps S101, S102, S103, S104 and S105.

[0036] The method 100 begins with step S101 which is a step of providing a contaminated solid polymer composition, called contaminated composition C0, comprising a polymer PL and contaminants CONT.

[0037] The contaminated composition C0 comes from the shredding of post-consumer and post-industrialization waste. Post-consumer waste is, for example, packaging for consumer products, for example packaging such as bottles, milk bottles, food bags, food trays, etc., from a “post-consumer” sorting stream. Post-industrialization waste comes from another sorting stream, called post-industrial, and concerns scrap and production offcuts.

[0038] The contaminated composition C0 is of “food grade” level when the packaging is originally food (those which are in direct contact with food) or are generally used in cosmetics (shower gel, shampoos, etc.), and of “non-food grade” level otherwise. The “food-grade” and “non-food grade” levels are indicative of a level of contamination of the plastic material.

[0039] The contaminated composition C0 is solid, that is to say that it is in solid form (granules, flakes, films, etc.). The term "solid" excludes forms of liquid, fluid, or even gaseous contaminated composition. The solid composition contaminated is for example not a melted composition.

[0040] Preferably, the CO contaminated composition is in the form of granules. These granules can be supplied by factories, following sorting and extrusion steps.

[0041] The geometric properties (shape and size) of the granules are described below.

[0042] The shape of the pellets is mainly of two types. When the extrusion mode is in "head cutting", the shape is generally a flattened sphere. When the mode is in "rod cutting", the shape is generally a cylinder.

[0043] These shapes deviate from the shape of a sphere. Indeed, the size in at least one dimension differs significantly from that of the other dimensions. Thus, in the case of pellets in the shape of a flattened sphere, the thickness varies between 2 mm and 3 mm, and the width varies between 3 mm and 4 mm. In the case of pellets in the shape of a cylinder, the width varies between 2 mm and 3 mm and the length varies between 4 mm and 5 mm.

[0044] These shapes thus have an aspect ratio, defined as the ratio of the largest dimension (width of the flattened sphere, length of the cylinder) to the smallest dimension (thickness of the flattened sphere, width of the cylinder), which is greater than 1. In the case of particles, the aspect ratio is considered to be equal to 1.

[0045] In the remainder of the description, reference will be made to the smallest dimension to designate the size of a granule.

[0046] The contaminated composition C0 can also be presented ground, in the form of flakes. The flakes typically have dimensions of the order of 2 cm to 4 cm, for example 2 cm. The flakes generally have surfaces of between 0.5 cm2 and 4 cm2 with thicknesses of between 0.5 mm and 2 mm.

[0047] The contaminated composition C0 can also be in the form of fibers or films.

[0048] The PL polymer of the contaminated composition C0 is part of the family of thermoplastic compounds, that is to say compounds whose structure and viscosity can be modified by successive heating and cooling, in a reversible manner.

[0049] The PL polymer is more particularly part of the polyolefin family.

[0050] Polyolefins have structures based on the repetition of unitary units. These Unitary units generally originate from hydrocarbons. These structures have carbon chains and unitary unit repeats ranging from 1000 to 1,000,000,000 or more units. Below this number of repeating units, these structures are generally called oligomers.

[0051] The polymer is more particularly a polyolefin such as polyethylene or PE, or polypropylene (PP), or a copolymer (PE / PP) or a mixture of polypropylene and polyethylene (PP+PE) with or without a compatibilizing agent. An example of a compatibilizing agent is maleic anhydride.

[0052] Whatever the polyolefin, it has a viscosity in the molten state of between 0.01 g / 10 min and 200 g / 10 min. This viscosity is also referred to as the hot melt index or MFI (acronym for "Mass Flow Index" in English) according to the ISO 1133 standard.

[0053] Polyethylene is one of the most widely used thermoplastic resins in the world. It is used in particular to make bags, films, bottles, bottle crates, toys, buckets, bowls, flexible pipes or tanks.

[0054] Polyethylene is obtained by polymerization of ethylene and is in the form of a waxy solid, completely colorless and odorless. It is soluble from 60-80° in certain organic solvents and becomes brittle from -25°C. It is generally not plasticized.

[0055] The term polyethylene refers to several types of polyethylene, including: low density polyethylene LDPE, medium density polyethylene or MDPE, high density polyethylene or HDPE, ultra-high molecular weight polyethylene or UHMWPE (acronym for “Ultra-High molecular Weigh Polyethylene” in English), linear low density polyethylene or LPEBS, waxy polyethylene or WaxPE (acronym for “Wax Polyethylene” in English).

[0056] Low density polyethylene LDPE has a density between 0.91 g / cm3 and 0.925 g / cm3.

[0057] Linear low density polyethylene LPEBD has a density between 0.91 g / cm3-0.9 g / cm3.

[0058] Linear medium density polyethylene LPEMD has a density between 0.926 g / cm3 and 0.94 g / cm3.

[0059] High density polyethylene HDPE has a density between 0.941 g / cm3 and 9.965 gj cm3.

[0060] PP polypropylene is used in particular to produce rigid packaging (trays, pots, caps, etc.).

[0061] Polypropylene is obtained by polymerization of propylene. It offers significant heat resistance and melts at around 160°C or 170°C.

[0062] The term polypropylene refers to several types of polypropylene: homopolymer polypropylene and copolymer polypropylene and waxy polypropylene or Wax PP (acronym for “Wax Polypropylene” in English).

[0063] The contaminants of the contaminated composition C0 are typically volatile organic molecules, i.e. molecules with a molecular mass between 0 g / mol and 500 g / mol, and / or non-volatile organic molecules with a molecular mass greater than 500 g / mol.

[0064] These molecules are generally present in stabilizers, lubricants, plasticizers, fillers and pigments added during the manufacture of packaging, or more generally of plastic. They can also come from the migration of products in contact with the packaging (contents), for example fat from a food, molecules present in food such as limonene, etc.

[0065] The maximum contamination level depends on the organic molecule. It corresponds to the maximum contamination level for which the method 100 makes it possible to obtain effective decontamination of more than 99%, as will be described later in the description.

[0066] For volatile organic molecules, the maximum contamination level corresponds to a maximum content equal to 5000 ppm.

[0067] For non-volatile organic molecules, the maximum contamination level corresponds to a maximum content equal to 2000 ppm.

[0068] The contaminated solid composition may further comprise other pollutants than the contaminants to be purified, such as: • An ethylene vinyl alcohol copolymer or EVOH, in a proportion of no more than 10% by mass • A polyamide or PA (also known as nylon) in a proportion of no more than 10% by mass, • Polyethylene terephthalate or PET, in a proportion of no more than 10% by mass, or • Aluminum, in a proportion of no more than 5% by mass.

[0069] With reference to [Fig.l] and [Fig.2], the method 100 continues with step S102, which is a step of reduction by micronization of the contaminated composition provided in the previous step S101.

[0070] This step S102 aims to produce, by reduction by micronization of the contaminated composition, a powder Cl of particles P comprising the polymer and the contaminants.

[0071] Generally speaking, micronization is a technique which makes it possible to reduce the contaminated composition in P particles.

[0072] In the context of the method 100, the micronization is adapted so that the particles P obtained have a diameter of between 0.1 mm and 1 mm. In other words, the micronization is adapted so that the powder formed by the particles has a particle size distribution which extends between 0.1 mm and 1 mm, without constraint as to the position of the highest frequency within this range.

[0073] The particles P have a shape similar to a sphere with contours that may be rough (or have facets). The diameter is a mesh diameter (i.e. a diameter of an equivalent sphere), measured by sieving. The particle size distribution of the powder is a mass distribution.

[0074] With reference to [Fig.2], when the CO contaminated composition is supplied in the form of granules or flakes, the micronization is for example carried out by a spraying step S1021 then a sieving step S1022.

[0075] The spraying is carried out in devices called "micronizers". These machines with two plates (one fixed, and the other mobile) blow the granules or flakes onto the walls by the action of centrifugal force, before a rotor bursts the material peripherally.

[0076] Sieving is carried out on this pulverized material to obtain the desired particle size.

[0077] The powder Cl can be stored at the end of this step S120.

[0078] The CONT contaminants are not extracted during this step S120.

[0079] The contaminated composition C0 can be homogenized before spraying (not represented in [Fig.2]).

[0080] [Fig.3] represents a system for implementing the method 100 according to the invention comprising: • an extractor 10, • a separator 20, • a 30 compressor.

[0081] With reference to [Fig.l] and [Fig.3], the method 100 continues with step S103 which consists of loading the powder C1 with particles P comprising the polymer PL and the contaminants CONT into the extractor 10 of the system 3.

[0082] A load of 1 kg to 10,000 kg of the powder Cl of particles P can be loaded into this extractor 10.

[0083] Still with reference to [Fig.l] and [Fig.3], step S104 extends step S103.

[0084] Step S104 is a step of purifying contaminants by extraction of the contaminants by a supercritical fluid.

[0085] For this, a continuous flow of a supercritical fluid F is introduced into the extractor 10 loaded with powder Cl, the extractor 10 being simultaneously maintained at a temperature between 40°C and 130°C and a pressure between 80 bars and 450 bars for a duration between 5 min and 480 min.

[0086] This duration in the extractor 10 under flow of the supercritical fluid is preferably between 5 min and 240 min.

[0087] For example, the temperature, pressure and time in the extractor under supercritical fluid flow are respectively 80°C, 300 bars, and 240 min.

[0088] The flow rate of the supercritical fluid F is between 0.1 kg / h and 100 kg / h. Preferably it is between 0.1 kg / h and 50 kg / h, for example it is equal to 50 kg / h.

[0089] The supercritical fluid physically dissolves and extracts contaminants from the Cl powder.

[0090] Thus, at the end of this supercritical fluid extraction step S104, the composition C2 present in the extractor 10 is a powder of particles similar to the contaminated powder C1 from the point of view of its particle size distribution, but different from this powder C1 in that it no longer contains a portion of the contaminants. For this reason, the powder obtained at the end of the extraction step S104 is called decontaminated solid composition C2.

[0091] The supercritical fluid is preferably supercritical carbon dioxide (CO2). This is an economical, clean fluid with supercritical properties at temperatures and pressures low enough not to cause degradation of the polymer of the powder Cl.

[0092] The supercritical fluid can also be a fluid other than a CO2-based fluid, for example it can be a supercritical fluid based on water (H2O), ammonia (NH3), or nitrous oxide (N2O).

[0093] With reference to [Fig. 3], the supercritical fluid Fc containing the portion of the extracted contaminants is preferentially discharged from the extractor 10, then separated, in a separator 20, from these contaminants CONT. This separation step generally requires a decompression phase during which the supercritical fluid becomes a gas again, this gas being generally less dense than the contaminating molecules, the latter condensing. The gas can then be filtered to be purified and then be used again in the process 100. The supercritical fluid thus decontaminated Fdc is then reinjected, via a compressor 30, into the extractor 10 so that the supercritical fluid is a recycled fluid Frecyci.

[0094] The method 100 is thus economical.

[0095] A co-solvent (not shown in [Fig.l] or in [Fig.3]), such as methanol, ethanol or water, may further be introduced into the extractor 10, simultaneously with the supercritical fluid during this extraction step S104. This co-solvent makes it possible to rinse the contaminants located on the surface of the particles P, which increases the extraction efficiency of the contaminants.

[0096] Step S104 of supercritical fluid extraction is carried out in “batch” mode. (or in batches), which is an advantageous production method.

[0097] As illustrated in [Fig.l], the method 100 continues with step S105, which consists of discharging the decontaminated solid composition C2 from the extractor 10, which has been brought back to temperature and pressure conditions allowing its opening.

[0098] As will be described below with the results of experiments carried out within the framework of the invention, the method 100 makes it possible to carry out in a simple manner a rapid decontamination, for example in 140 minutes, and extremely effective, greater than 99%, of all the contaminants tested.

[0099] Thus, at the end of step S105 of method 100, a powder of high-purity polymer particles is obtained, allowing in particular use in the food sector.

[0100] The process 100 is discontinuous or “batch”: the contaminated composition C0 is in fact decontaminated in successive batches. This production method allows for simple and precise traceability, and provides production flexibility.

[0101] This step S105 may be followed by an additional step (not shown in [Fig.l]) of extrusion to form decontaminated polymer granules from the decontaminated solid composition.

[0102] This step S105 can be repeated several times so as to further increase the decontamination efficiency in the case where the initial contamination is abnormally high.

[0103] The experiments carried out within the framework of the invention are described below.

[0104] In these experiments, the contaminated composition C0 is specifically developed to comprise a polymer and a so-called “model” contaminant, i.e. one whose molecular weight and concentration in the contaminated composition are known.

[0105] The chosen PL polymer is polypropylene PP known as extrusion grade with the following characteristics MFR (@ 230°C / 2.16kg) / ISO 1133 / 0.85 g / 10min).

[0106] The model contaminant is a molecule whose molecular weight is close to the targeted contaminants. Its concentration is chosen to be close to the target concentrations prescribed by the European Safety Agency EFS A guidelines for recycling processes.

[0107] Specifically, four model contaminants CONTi, CONT2, CONT3 and CONT4 are chosen to develop, respectively, four contaminated compositions C0i, C02, C03, C04, each of these compositions having either the form of granules, in the dimensions and shapes described above, or the form of films. Two film thicknesses are obtained: 100 pm and 250 pm.

[0108] The characteristics of these contaminated compositions C0i, C02, C03, C04 are described in the following table.

[0109] [Tableauxl] C0i C02 C03 C04 Polymer PL PP Contaminant CONT CONT1 CONT2 CONT3 CONT4 Molecular weight of contaminant (g / mol) 200 -300 400-500 750-800 750-800 Contaminant concentration (mg / kg) 855 721 458 857 Mass of contaminated composition (Kg) 300 300 300 300 Form of contaminated composition Granules Granules Granules Granules Film 250 pm Film 250 pm Film 250 pm Film 250 pm Film 100 pm Film 100 pm Film 100 pm Film 100 pm

[0110] The method 100 as described above is implemented using each of the contaminated compositions C01, C02, C03, C04 in the form of granules.

[0111] At the end of the micronization reduction step S102, four powders C11, C12, C13 and C14 are obtained, having particles with a diameter of between 0.1 mm and 1 mm, corresponding to the micronization of the contaminated compositions C01, C02, C03, C04 respectively. The following table illustrates the result of a measurement of the particle size distribution of one of these powders, this measurement being carried out by sieving.

[0112] [T ableaux2] Measured mesh diameter Percentage > 1.50 mm 8.9% > 1.00 mm 14.5% > 0.80 mm 13.1% >0.71 mm 13.0% > 0.63 mm 12.4% > 0.50 mm 17.6% < 0.50 mm 20.4%

[0113] During the extraction step S104, the extractor 10 of the extraction system 3 is used, supercritical CO2 as the Frecy supercritical fluid, and temperature, pressure and duration conditions are included in the ranges specified by the method 100. Specifically, the pressure is 300 bar, the temperature 80°C, the duration 140 min.

[0114] At the end of step S105 of unloading the decontaminated composition, four powders of decontaminated PP particles C2b C22, C23 and C24 are obtained.

[0115] To compare the performance of the method 100 with a method which would not include step S102 of reduction by micronization of the contaminated composition, only steps S103, S104 and S105 of the method 100 are also implemented, from each of the contaminated compositions in the form of granules and in the form of films.

[0116] The same system 3 is then used as for process 100, the same Frecy supercritical fluid, as well as temperature, pressure and duration conditions similar to those used in process 100 (300 bar, 80°C or 90°C, 140 min).

[0117] Decontaminated solid compositions are then obtained corresponding to the extraction by supercritical fluid of the granules and films.

[0118] The decontamination efficiency is then determined on each of these decontaminated solid compositions.

[0119] For this, each decontaminated solid composition is injected and quantitatively analyzed by gas chromatography coupled with a high-resolution mass spectrum or GCMS-HR (acronym for “Gas Chromatography Mass Spectroscopy High Resolution” in English).

[0120] The detection limit of contaminants corresponds to the detection limit of the chromatography apparatus: contaminants are considered as not detected when none of the model compounds are detected on the cor- chromatograms. respondent after supercritical CO2 extraction.

[0121] The decontamination efficiencies thus measured are given in the following table.

[0122] [Tables3] Incoming composition in the extractor Decontamination efficiency (%) CONT1 CONT2 CONT3 CONT4 Contaminated PP micro-particle powder (Process 100) 99.7 99.8 99.6 99.3 Contaminated PP granules 98.9 84.8 63.8 53.5 Contaminated PP 250 pm film 99.4 98.4 95.8 92.4 Contaminated PP 100 pm film 99.4 99.5 98.1 97.4

[0123] Thus, thanks to the micronization of the contaminated compositions, this before the extraction (and not after, as is often the case to obtain purified particles), and by specifying this micronization to obtain the diameter range 0.1 mm - 1 mm for the particles, a decontamination in 140 minutes, and extremely effective, greater than 99%, of all the contaminants tested is obtained. In other words, a rapid and effective decontamination is obtained in a simple manner, regardless of the contaminants tested.

[0124] Under these same conditions of temperature, pressure and time in the extractor, a lower efficiency, lower than the targeted efficiency, is obtained when micronization is not carried out and the material entering the extractor is in the form of granules or films.

[0125] Additional experiments have shown that by using films as input material, it is possible to carry out decontamination as effectively, although this is slower. It is necessary to increase the time in the extractor to 480 min to measure a decontamination efficiency equal to 99.8% for each of the contaminants CONT1, CONT2, CONT3 and CONT4.

[0126] Furthermore, these experiments showed that by using granules as input material, it was not possible to achieve the targeted efficiencies for all contaminants, even by increasing the time in the extractor. Thus, for a time in the extractor of 480 min, a decontamination efficiency of 99.8% was measured for the lightest contaminants CONT1 and CONT2, but a decontamination efficiency of 99.8% for the lightest contaminants CONT1 and CONT2, but a decontamination efficiency of 99.8% for the lightest contaminants CONT1 and CONT2. less than 99%, precisely equal to 93.8% and 89.8% for the heaviest CONT3 and CONT4 contaminants. Decontamination is therefore not effective or robust enough with respect to the different contaminants tested.

Claims

Claims

1. Method (100) for decontaminating a so-called contaminated solid composition (CO), derived from post-consumer and / or post-industrialization waste, comprising a polymer (PL) and contaminants (CONT), said method comprising the following successive steps: - Reduction by micronization (S 102) of the contaminated solid composition (CO) into particles (P) having a diameter of between 0.1 mm and 1 mm, to obtain a powder (Cl) comprising the polymer (PL) and the contaminants (CONT), - Loading (S103) of the powder (Cl) obtained into an extractor (10), - Introduction, into the extractor (10) loaded with powder (Cl), of a continuous flow of a supercritical fluid (F, Frecy), the extractor (10) being simultaneously maintained at a temperature of between 40°C and 130°C and a pressure of between 80 bars and 450 bars for a duration of between 5 min and 480 min,to physically extract (S 104) the contaminants (CONT) by the supercritical fluid (F, Frecy) and obtain a so-called decontaminated solid composition (C2) comprising the polymer (PL), - Unloading the decontaminated solid composition (C2) from the extractor (10), which has been brought back to temperature and pressure conditions allowing its opening.,

2. Decontamination method (100) according to claim 1, in which the supercritical fluid (F, Frecy) is based on supercritical CO2.

3. Decontamination method (100) according to one of claims 1 to 2, in which the flow rate of the supercritical fluid (F, Frecy) is between 0.1 Kg / h and 100 Kg / h, preferably between 0.1 Kg / h and 50 Kg / h.

4. Decontamination method (100) according to one of claims 1 to 3, in which the contaminated solid composition (C0) is in the form of granules.

5. Decontamination method (100) according to one of claims 1 to 4, in which a load of 1 kg to 10,000 kg of powder (Cl) comprising the polymer (PL) and the contaminants (CONT) is loaded into the extractor.

6. Decontamination method (100) according to one of claims 1 to 5, in which the polymer (PL) of the contaminated solid composition (CO) is a polyolefin such as polypropylene (PP), or polyethylene (PE), or a mixture of polypropylene (PP) and polyethylene (PE) with or without a compatibilizing agent such as maleic anhydride.

7. A decontamination method (100) according to claim 6, wherein the polyolefin of the contaminated composition (C0) has melt viscosity properties of between 0.01 g / 10 min and 200 g / 10 min.

8. Decontamination method (100) according to one of claims 1 to 7, in which the contaminated solid composition (C0) comprises volatile organic contaminants in a content equal to at most 5000 ppm, and / or non-volatile organic contaminants in a content equal to at most 2000 ppm.

9. Decontamination method (100) according to one of claims 1 to 8, in which the contaminated solid composition (C0) comprises pollutants other than the contaminants to be purified, such as: - ethylene vinyl alcohol copolymer or EVOH in a proportion at most equal to 10% by mass, - polyamide or PA in a proportion at most equal to 10% by mass, - polyethylene terephthalate or PET in a proportion at most equal to 10% by mass, or - Aluminum, in a proportion at most equal to 5% by mass.

10. A decontamination method (100) according to one of claims 1 to 9, wherein a co-solvent, such as methanol, ethanol or water, is introduced into the extractor, simultaneously with the supercritical fluid during the extraction step.

11. A decontamination method (100) according to one of claims 1 to 10, wherein the supercritical fluid (F, Frecy) is discharged from the extractor, then separated, in a separator, from the contaminants which have been dissolved in the supercritical fluid during extraction, then reinjected into the extractor so that it is recycled.

12. Method (100) of decontamination according to one of claims 1 to 11, wherein, at the end of the extraction step (S 104), the contaminants (CONT) are extracted with an efficiency greater than 99%.

Citation Information

Patent Citations

  • Process for recycling polyolefin

    WO2018121980A1

  • Supercritical carbon dioxide extraction recovery device for waste electric appliance combustion inhibitor and method thereof

    CN100536975C