PROCEDURE OF PREPARATION OF A LOADING MATERIAL FROM A MIXTURE OF POLYCOTON AND POLYOLEFIN

A process for recycling mixed polycotton and polyolefin textiles through densification and mechanical treatment produces a recyclable, eco-friendly material with superior mechanical properties, addressing the inefficiencies of current recycling methods and providing a sustainable alternative to virgin plastics.

FR3147283A1Inactive Publication Date: 2024-10-04PLAXTIL
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
FR2023002920
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current textile recycling processes are inadequate for mixed natural and synthetic fibers, particularly polycotton and polyolefin materials, due to their heterogeneity, leading to complex and inefficient recycling methods that fail to handle all-purpose mixed textiles effectively.

Method used

A process involving densification and mechanical treatment of shredded polycotton and polyolefin textiles at specific temperatures to create a filled material suitable for large-scale recycling, which includes a mixture of polycotton fibers up to 75% and a polyolefin matrix, producing compound granules suitable for plastics processing.

Benefits of technology

The resulting material exhibits excellent mechanical properties, is recyclable for at least 10 cycles, and reduces environmental impact, offering a sustainable alternative to virgin plastics with comparable mechanical performance to virgin thermoplastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000011_0000
    Figure 00000011_0000
  • Figure 00000011_0001
    Figure 00000011_0001
  • Figure 00000011_0002
    Figure 00000011_0002
Patent Text Reader

Abstract

The invention relates to the field of recycled materials. More specifically, the invention concerns a process for preparing a polyolefin-based material loaded with polycotton-type textile fibers. The invention also relates to the resulting loaded material, which can be used in industry as a replacement for plastic. The resulting material is called "PLAXTIL material."
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: PROCESS FOR PREPARING A FILLED MATERIAL FROM A POLYCOTTON AND POLYOLEFIN MIXTURE

[0001] The invention relates to the field of recycled materials. More particularly, the invention relates to a process for preparing a polyolefin-based material filled with polycotton-type textile fibers. The invention also relates to the filled material obtained, a material which can be used in industry as a replacement for plastic. The material obtained is called "PLAXTIL material". Field of the invention

[0002] The fashion industry is considered the second most polluting industry in the world, after the oil industry. A very active sector whose CO2 emissions are higher than those of air and oil transport combined.

[0003] Faced with the environmental consequences of this sector, the textile recycling sector is growing rapidly and has been structuring itself for several years for the collection and sorting of textiles. However, to date, only a minimal proportion of textiles is actually recycled. This deficit is partly due to the heterogeneity of textile fibers, which makes large-scale recycling complex.

[0004] The processes of the prior art are generally adapted to particular types of textile fibers and the processes are quite complex. For example, patent FR2998572 may be cited which describes a process for recycling the constituents of a textile product, possibly comprising a pretreatment of the textile product to be recycled and at least the following steps: (i) hydrolysis of the animal fibers, (ii) hydrolysis of the cellulose fibers, (iii) glycolysis of the polyester fibers. The hydrolysis steps carried out in parallel each give rise to the production of a cake, the different cakes of residual textiles being mixed and the mixture extruded to produce a recycled plastic material.Another example is patent US2020 / 0262108, which describes a process for recycling a mixed cotton-polyester textile consisting of hydrolyzing the textile in an aqueous solution containing an organic acid catalyst heated to 110-180°C in a high-pressure reactor so as to separate the cotton fibers from the polyester and ultimately recover the cotton fibers using a vacuum filtration membrane.

[0005] None of these processes allows for the treatment of all-purpose mixed textiles. The choice of a “custom-made” treatment is explained in particular by the difficulty in mixing and homogenizing two materials whose densities differ significantly, in particular in the case of textiles comprising mixed natural synthetic fibers with a polymer.

[0006] Given the volumes of textile waste generated throughout the world, it is desirable to have suitable recycling means. Statement of the invention

[0007] The inventors propose a new filled material obtained from recycled cotton-polyester and polyolefin type textiles as well as a process for preparing such a material.

[0008] Thus the invention relates to a filled material comprising a mixture of textile fibers of the polycotton and polyolefin type, characterized in that the polycotton represents up to 75% of said material.

[0009] The invention also relates to a method for preparing a charged material as defined above in the form of “compound” type granules from polycotton type textile and polyolefin comprising the following steps: - Arranging polycotton type textile in the form of ground materials - Densifying said ground textile materials by compressing the material - Mix said compressed ground material obtained in the previous step with said polyolefin - Mechanically treat the mixture obtained in the previous step at a temperature between 150 and 220°C, said treatment being carried out by extrusion. Advantages of the invention

[0010] The filled material obtained from polycotton and polyolefin is considered an ecological plastic.

[0011] This filled material has very good mechanical qualities, which make it suitable for use in plastics applications. It can replace plastic materials derived 100% from petroleum and constitutes a credible alternative to plastic for industry in general, and for the fashion industry in particular. The fibers improve the properties of the matrix by fulfilling the role of "reinforcement" in a similar way to a conventional composite material.

[0012] The process is characterized by its tolerance. It can be implemented from all-purpose cotton-polyester type textiles: textiles made of mixed natural and synthetic fibers, and remarkably, it is not required to know the relative percentage of these two components to implement the process. This makes it possible to process large volumes of used textiles, which removes a major obstacle compared to current recycling processes. In addition, the presence of other types of fibers in the textile, in a minority quantity compared to cotton-polyester, does not hinder the process.

[0013] The resulting charged material is recyclable over at least 10 reuse cycles and is part of the circular and sustainable economy. However, there is a gradual loss of mechanical performance inherent in the polymers themselves. In particular, the polymer chains break following successive melting cycles. The color of the compound darkens as it is recycled.

[0014] The life cycle of the materials according to the invention responds to a long-term recycling logic. Firstly because the materials are produced from recycled used textile materials (waste), but also because the loaded material can itself be recycled over a large number of cycles. Tests carried out over 10 cycles show a mechanical loss limited to 30% which is comparable to virgin plastic recycled 10 times. DETAILED DESCRIPTION OF THE INVENTION

[0015] A first subject of the invention relates to a filled material comprising a mixture of textile fibers of the polycotton and polyolefin type, characterized in that the polycotton represents up to 75% of said material.

[0016] Polycotton, also called "cotton-polyester" is a polymer made up of natural cotton fibers and synthetic polyester fibers. Textile fibers can be woven or non-woven. The relative percentage between these two types of fibers can vary, which constitutes an obstacle to recycling by currently available processes.

[0017] In the context of the present invention, the textiles from which the filled material is prepared are made of polyester and cotton fibers regardless of the ratio between these two materials. The cotton / polyester ratio may in particular be between 50 / 50 and 96 / 4; this ratio applies in both directions, namely that the cotton and the polyester may each represent between 4 and 96% of the polycotton material. For example, conventional polyester compositions may contain the following ratios: 80 / 20, 75 / 25, 50 / 50 and 60 / 40 (in both directions of the mixture: cotton / polyester or polyester / cotton).

[0018] Polycotton can represent up to 75% of the loaded material. In other words, the loading rate can reach 75%. Preferably, the loading rate is between 15% and 50% and usually this rate is between 20% and 45%.

[0019] Thus, the filled material comprises at least 25% polyolefin matrix and preferably, the polyolefin matrix represents between 50% and 85% of the material.

[0020] The polyolefin matrix may be virgin, recycled or derived from waste. The recycled matrix may also come from recycled synthetic fibers or any other waste source. In addition, it may contain up to 20% mineral filler; the presence of a mineral filler in these proportions does not disturb the general behavior of the filled material, nor its preparation process. The mineral filler may be made of material such as talc, mica, wollastonite, kaolin, CaCO3, BaSO4, Dolomite, Graphite MoS2.

[0021] By “polyolefin” or “polyolefin matrix” is meant thermoplastic polyolefins of the type: poly ethylene (PE), polypropylene (PP), polymethylpentene (PMP), polybutene-1 (PB-1) and polyisobutylene. Preferably, the polyolefin matrix comprises PE and / or PP.

[0022] In addition, the polycotton may comprise other components in addition to the polyester and cotton fibers. These other components are preferably thermoplastic textile materials such as polyamide, aramid fibers or modacrylic. These additional components, present in limited proportion, do not harm the process.

[0023] The polycotton may also include elastane (or other thermoset fibers) for which a proportion limit of up to 50% in the polycotton is acceptable. Beyond this, the polycotton material cannot be recycled by this process. In particular embodiments of the invention, the proportion of elastane in the polycotton is less than or equal to 40%, 30%, 20% or 10% depending on the nature of the textile and the polycotton / polyolefin ratio applied.

[0024] The filled material has good strength properties. It is suitable as a substitute for virgin PP type virgin plastic. It can be used in the industrial manufacture of common "plastic" objects, for example: measuring instruments (rulers, school protractors), hangers, supports or containers. The list is almost endless. By optimizing the choices and proportions of textiles / matrices / additives and by adapting the design of the part, any type of technical achievement in plastics is possible with this material.

[0025] A second subject of the invention relates to a process for preparing a charged material as defined above in the form of granules of thermoplastic material from polycotton and polyolefin type textiles comprising the steps of: - Arranging polycotton type textiles in the form of ground materials - Densifying said ground textiles by compressing the material - Mix said compressed ground material obtained in the previous step with said polyolefin - Mechanically treat the mixture obtained in the previous step at a temperature between 150 and 240°C, said treatment being carried out by extrusion.

[0026] The loaded material obtained is in the form of “compounds” or thermoplastic granules ready to be used in the plastics industry as a replacement for virgin plastics.

[0027] Obtaining a good quality loaded material depends on the “quality” of the materials entering into its composition. The inventors have highlighted the importance of the density parameter of the shredded textile fibers in this process and propose to densify the shredded textile fibers before mixing them with the polymer for melting. Densification allows the textile to be correctly dosed for mixing with the polymer and facilitates the textile-polymer blending. Typically, the shredded polycotton is compacted until it obtains a density at least 10 times higher than that of the starting shredded material. In a preferred embodiment, the densified shredded material is in the form of semi-solid and friable granules. This densification step is preferably carried out by compression. The granules obtained after densification are illustrated in Figure 1B, in comparison with the undensified shredded material shown in Figure 1A.

[0028] Preferably, the polycotton shreds before densification have a size of approximately 5 mm.

[0029] In a preferred embodiment of the invention, natural additives are added to the polycotton fibers before the densification step. The amount of these additives represents up to 10% of the amount of textile material, generally between 1 and 2% (by weight). These are process additives that provide fluidity to the textile material. This improves the cohesion of the fibers with each other and thus facilitates mixing with the polymer and their fusion so that the resulting filled material is homogeneous. These process additives ("process additives") are, for example, starch powder or conventional lubricants (for example, maleic anhydride introduced via a grafted PP); they do not change the material but stabilize the process.

[0030] Polyolefin is also supplied in the form of granules or ground. Recycled polyolefin can in particular come from textile fibers (woven or non-woven) previously ground and densified.

[0031] After densification, the cotton-polyester textile fibers are mixed with the polyolefin polymer grains in an extruder.

[0032] The treatment temperature of the mixture is between 150°C and 240°C. In a particular embodiment of the invention, it is between 160°C and 220°C, or even between 180°C and 210°C.

[0033] Preferably, the heat treatment for shaping the granules is carried out by extrusion. This extrusion makes it possible to carry out compounding.

[0034] Compounding is an extrusion-granulation process allowing the melt mixing of a polymer, here polyolefin (thermoplastic resin), with one or more reinforcing / filling additives, here cotton-polyester textile fibers, in order to obtain a plastic material in the form of “compounds” (a type of granule) with specific physical or thermal characteristics.

[0035] Other specific properties such as: antistatic, electrically conductive, anti- UV, antioxidant, etc. can be obtained by adding standard additives used to obtain said properties.

[0036] In the context of the invention, compounding consists of extruding granules of standard size similar to virgin granules of mixtures of thermoplastic materials. In compound form, the loaded material is compatible with all presses used for injectable products and can therefore be used by manufacturers like any plastic material.

[0037] The method according to the invention aims to avoid degradation of the fibers, or at least to minimize it. Good fusion of the fibers with each other improves the dispersion of the fibers in the compound and can have an aesthetic effect with less visible fibers. The process parameters can be adjusted according to the desired visual rendering of the loaded material.

[0038] Thus, it has been established that the polycotton-polyolefin blend must be treated at a temperature between 150°C and 240°C (preferably between 160°C and 220°C) during the extrusion and injection phase so that the material obtained conforms in terms of expected properties. This temperature range allows good dispersion of the fibers in the polymer matrix in an industrial process.

[0039] All the composite materials according to the invention are recyclable. This interesting property is directly linked to the fact that the process does not induce any structural modification of the fibers or the polymer. In particular, no chemical agent capable of inducing such a modification of the material is used. However, it is possible to use small quantities of chemical agents to improve certain characteristics of the material, such as chain extenders to improve the mechanical performance in the context of a regeneration loop. In a particular embodiment of the invention, no chemical agent is used, even among the chemical agents not capable of inducing a structural modification of the fibers or the polymer, but which allow an improvement of certain characteristics of the loaded material.

[0040] Dyes and / or pigments can be added to modify the chromatic rendering. Other additives can also be used to functionalize the material (ESD-Biocide function, thermochromatic, photoluminescent, etc.), without affecting the structure of the fibers or the polymer. Similarly, the temperatures and forces applied during the process do not cause a change of state (no modification by reactive chemistry is sought). The filled material obtained typically has the behavior of a thermoplastic material.

[0041] The present invention will be better understood from reading the following examples, provided for illustration purposes and in no way to be considered as limiting the scope of the present invention. DESCRIPTION OF FIGURES

[0042] [Fig. 1] [Fig. 1]: Representation of the products obtained at the different stages of the process, here obtained from recycled surgical masks. A: starting textile shred, B: Densified textile shred in the form of semi-solid granules

[0043] [Fig.2] [Fig.2]: Graphical representation of the Young's modulus in bending in function of the number of recycling cycles

[0044] [Fig.3] [Fig.3]: Graphical representation of resilience with notches in function of the number of recycling cycles EXAMPLES

[0045] EXAMPLE 1: Preparation of the charged materials and appearance obtained

[0046] An exemplary method of preparing a filled material is described herein.

[0047] The polycotton-based textile is first uniformly ground to obtain ground particles with a size of approximately 5 mm. This ground material is then densified by compression until friable semi-solid granules are obtained, which are then dried, if necessary, in a steamer or desiccator to remove water. Water is responsible for the hydrolysis of plastics, one of the main reasons for the breakage of polymer chains and which therefore affects the mechanical properties of the materials. These textile granules are then mixed with polyolefin polymer grains in an extruder. The mixture is extruded at a temperature of 200°C in the form of standard-sized granules similar to virgin granules of thermoplastic material mixtures; this is the compounding step. The resulting filled material is generically called “PLAXTIL material”. EXAMPLE 2: Properties of charged materials

[0048] The tests were carried out according to ISO standards in order to be reproducible (NF EN ISO527-1 for traction for example).

[0049] The characteristics of the loaded materials obtained are presented below:

[0050] Charpy impact strength:

[0051] unnotched resilience: 20-40 KJ / m2

[0052] notched resilience: 15-22 KJ / m2

[0053] Bending test at 10 mm for 10 min

[0054] Maximum stress: 30-40 MPa

[0055] Flexural modulus: 1900-2300 MPa

[0056] Tensile test

[0057] Maximum stress: 10-17 MPa

[0058] Elongation at break at 10 mm for 10 min: <5%

[0059] Tensile modulus: 1200-1400 MPa

[0060] Melt flow index

[0061] MFR under 2.6 kg at 230°C: >5 g / 10 min (minimum value for compatibility with injection process)

[0062] These properties are comparable or mechanically superior to the virgin thermoplastic material. The material filled according to the invention is notably more rigid due to the presence of fibers.

[0063] EXAMPLE 3: Study of the environmental impact of the process according to the invention

[0064] The textile materials recycling process according to the invention differs from incineration treatment processes by its reduced environmental impact: the recycling and injection process leads to CO2 emissions of 1.71 kg / T of recycled material while incineration produces between 1,000 and 1,700 kg of CO2 / T. The environmental impact is therefore divided by 1000 thanks to the process according to the invention and the latter makes it possible to produce composite materials of interest as a replacement for plastic, where incineration only destroys.

[0065] Furthermore, the comparative analysis of the life cycle between the same object in virgin PP (origin Asia or Europe) and in PLAXTIL material (1st use or recycled) demonstrates the interest of using PLAXTIL material in terms of resources consumed. Indeed, on average, the impact on resources is divided by 3. EXAMPLE 4: Recyclability of loaded materials

[0066] The mechanical performance of the recycled materials was evaluated using Young's flexural modulus and resilience measurement.

[0067] [Fig.2] shows that the Young's modulus is impacted by approximately 30% over the first cycles and then remains stable. This result shows good maintenance of mechanical properties for 10 recycling cycles.

[0068] [Fig.3] shows the impact of the number of recycling cycles on resilience. It should be noted that the material's ability to resist crack propagation decreases over the cycles, but this decrease remains moderate up to 7 cycles, which is already significant. The use of recycled material can, moreover, be adapted to the material's life cycle by taking this parameter into account.

[0069] These results can be compared with data relating to the recycling of polyethylene terephthalate (PET). PET is the most widely used plastic in packaging (bottles) and the most recycled in the world, via primary or secondary recycling. PET recycling has reached one of the most advanced levels of maturity among consumer plastics. However, the loss of mechanical properties of PET after each recycling cycle remains problematic. It appears that the breaking stress of "virgin" PET is 42% but that this value drops to 0.7% after the fifth recycling cycle. This substantial loss of mechanical properties thus limits the ultimate number of cycles that can be carried out.

[0070] The material loaded according to the invention can be recycled more than 4 times, without sub- standard of mechanical properties and by an environmentally friendly process.

Claims

Claims

1. Filled material comprising a mixture of polycotton and polyolefin textile fibers, characterized in that said polycotton represents up to 75% by weight of said material.

2. Filled material according to claim 1 wherein the polyester / cotton or polyester / cotton ratio of the polycotton is between 50 / 50 and 4 / 96 by total weight of the textiles.

3. Filled material according to one of the preceding claims in which the filler rate is between 15% and 50% by weight.

4. Filled material according to one of the preceding claims wherein said polyolefin may be virgin, recycled, derived from waste and may contain up to 20% by weight of mineral filler.

5. Filled material according to one of the preceding claims further comprising other thermoplastic textile materials from said polycotton type textile such as polyamide, aramid fibers and modacrylic.

6. Filled material according to one of the preceding claims further comprising elastane from said polycotton type textile in a proportion of up to 50% by weight of said textile.

7. Process for preparing a filled material as defined in one of claims 1 to 6 in the form of thermoplastic granules from polycotton type textile and polyolefin comprising the steps of: • Arranging polycotton type textiles in the form of ground materials • Densifying said ground textile materials by compressing the material • Mixing said compressed ground materials obtained in the previous step with said polyolefin • Mechanically treating the mixture obtained in the previous step at a temperature between 150 and 240°C, said treatment being carried out by extrusion.

8. A method according to claim 7 wherein a process additive is added to said textile fibers prior to the densification step.

Citation Information

Patent Citations

  • Recycling components of textile product, involves pretreating textile product to be recycled, performing hydrolysis of animal and cellulosic fibers, performing glycolysis of polyester fibers, and performing extrusion of residual textile

    FR2998572A1

  • Method for separating and recycling a waste polyester-cotton textile by means of a hydrothermal reaction catalyzed by an organic acid

    US20200262108A1

  • Waste textile / thermoplastic resin composite material and preparation method thereof

    CN109401062A

  • Preparation method of hydrogenated C9 petroleum resin coated polyester / chinlon / spandex modified HDPE

    CN113416390A

  • Fiber-plastic composite material prepared from mixed waste textiles, preparation method and application thereof