Devices containing plant-active ingredients

Incorporating wood flour into poly(glycerol sebacate) formulations addresses fining and adhesion issues, maintaining effective release of active ingredients in plant treatment devices under high temperatures.

FR3147685A1Pending Publication Date: 2024-10-18MICHELIN & CO (CIE GEN DES ESTAB MICHELIN)

Patent Information

Application Number
FR2023003744
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing plant treatment devices using poly(glycerol sebacate) face challenges with fining and adhesion issues, particularly at high temperatures in tropical or subtropical zones, leading to the thinning of controlled release formulations containing phytosanitary and biostimulant active ingredients.

Method used

Incorporating a vegetable filler, such as wood flour, into the formulation enhances the resistance to fining and maintains adhesion properties of plant treatment devices at high temperatures by improving the stability of poly(glycerol sebacate) compositions.

Benefits of technology

The addition of wood flour significantly reduces fining while preserving adhesion, ensuring effective and sustained release of active ingredients on plant surfaces even in harsh environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000019_0000
    Figure 00000019_0000
  • Figure 00000020_0000
    Figure 00000020_0000
Patent Text Reader

Abstract

The invention relates to a composition comprising at least one biocompatible copolyester obtainable by the polycondensation of a diacid and a polyol with a molar mass greater than or equal to 1000 g / mol, a plant-based filler, and an aqueous solution of at least one active plant protection product and / or a biostimulant. This composition is particularly suitable for treating plants by application to the trunk of trees or shrubs, especially those selected from the group consisting of rubber trees, grapevines, olive trees, fruit trees, and ornamental plants, preferably rubber trees.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Devices containing plant-active ingredients Technical field

[0001] The field of the present invention is that of compositions for the treatment of plants applied to the aerial parts (leaf system or trunk) which may comprise an active ingredient such as, for example, a stimulant, a fertilizer, a pesticide, a fungicide or even a nutrient. STATE OF THE ART

[0002] The Applicant has developed, for the treatment of plants, a formulation comprising on the one hand a biosourced, biocompatible and biodegradable polymer, showing a certain antimicrobial activity and on the other hand a phytosanitary or biostimulant product, in particular a biostimulant product and in particular ethephon (application number FR2113693). The polymer material used is poly(glycerol sebacate) or PGS. This formulation contains a certain concentration of active product and makes it possible to apply a defined quantity of this product to a plant in a targeted manner, limiting losses in the environment generally due to conventional application techniques and climatic conditions. This formulation also allows a controlled release of the active product over time, guaranteeing continuous and regular treatment during the application time.The formulation can be applied as a paste to the aerial parts (leaf system or trunk) of trees and shrubs.

[0003] It is a constant concern to always improve existing plant treatment devices. More particularly, insofar as the plant treatment device developed by the Applicant is intended to release the active ingredient it contains in a controlled and continuous manner over time, it is appropriate to ensure the sustainability of the installation of the device on the aerial parts of the treated trees and shrubs.

[0004] However, it proves difficult to use formulation devices based on poly(glycerol sebacate) containing active substances with controlled release, applied to the aerial parts of the treated trees and shrubs, without being confronted with constraints of adhesion on the one hand, and of dimensional stability (thinning of the polymer or spreading) on ​​the other hand, especially when the device is exposed to certain high operating temperatures which can reach 40°C in tropical or subtropical zones. Indeed, under these conditions of use, a marked thinning of the controlled release device containing a formulation based on poly(glycerol sebacate) is observed. containing an aqueous solution of a phytosanitary and / or biostimulant active ingredient, particularly when the poly(glycerol sebacate) has a number-average molar mass greater than 1000 g / mol. TECHNICAL PROBLEM

[0005] The technical problem which arises is therefore to improve the resistance to fining of a plant treatment device containing a copolyester, in particular a poly(glycerol sebacate), whatever its number-average molar mass, as well as an aqueous solution of a phytosanitary and / or biostimulant active ingredient. Statement of the invention

[0006] The Applicant, continuing its research efforts, has surprisingly discovered that the use of a specific plant filler, in particular wood flour, in a device comprising a formulation based on poly(glycerol sebacate) containing an aqueous solution of a phytosanitary and / or biostimulant active ingredient, makes it possible to respond to the technical problem posed.

[0007] The composition according to the present invention makes it possible to significantly improve the resistance to tinting at a temperature which simulates natural exposure in a tropical or subtropical zone (around 40°C) of a plant treatment device, while retaining its adhesion properties on the wooden substrate on which it has been applied.

[0008] In view of these properties, the composition according to the invention predicts improved resistance to fining at temperatures in tropical or subtropical zones, without degradation of adhesion to the trunk of the treated trees and shrubs.

[0009] A first subject of the invention is a composition comprising at least one copolyester capable of being obtained by the polycondensation of a diacid and a polyol, a plant filler, and an aqueous solution of at least one active ingredient.

[0010] Another subject of the invention is a method for treating plants comprising the application to the aerial parts of trees or shrubs of a composition according to the invention. DESCRIPTION OF FIGURES

[0011] [Fig-1]: Table of results with photographs taken during the tests with the compositions appearing in table 2.

[0012] [Fig.2]: Table of results with photographs taken during the tests with the compositions shown in Table 3.

[0013] [Fig.3]: Table of results with photographs taken during the tests with the compositions DEFINITIONS

[0014] "Biocompatible" means: which is tolerated by an organism, here in particular which is tolerated by plants.

[0015] A phytosanitary product, plant protection product or phytopharmaceutical product is a substance or mixture of substances of a chemical or biological nature (of natural or synthetic origin) used in agriculture, horticulture or forestry to protect cultivated plants against bioaggressors (animal pests, phytopathogenic agents, parasitic plants, weeds), or to optimize crops by promoting the growth of cultivated plants and treating their environment (in particular the soil).

[0016] "Biostimulant" means a substance that stimulates the nutrition processes of plants, independently of the nutrients it contains, with the aim of improving one or more of the following characteristics of plants or their rhizosphere: nutrient use efficiency, tolerance to abiotic stress, quality characteristics, availability of nutrients confined in the soil or rhizosphere (in accordance with EU Regulation 2019 / 1009).

[0017] Biostimulants can be certain natural preparations of low concern (PNPP). PNPP are:

[0018] - Either natural substances for biostimulant use (SNUB).

[0019] - Either basic substances.

[0020] Basic substances are defined by Article 23 of Regulation (EC) No 1107 / 2009. These are substances of phytosanitary interest but whose main use is other than plant protection (e.g. foodstuffs). Summary of the invention

[0021] The invention, described in more detail below, has as its subject at least one of the embodiments listed in the following points:

[0022] 1. Composition comprising - at least one biocompatible copolyester capable of being obtained by the polycondensation of a diacid and a polyol with a number-average molar mass (Mn) greater than or equal to 1000g / mol, - a plant load, and - an aqueous solution of at least one phytosanitary active ingredient and / or a biostimulant.

[0023] 2. Composition according to the preceding embodiment in the form of a paste.

[0024] 3. Composition according to any one of the preceding embodiments in which the diacid is chosen from aliphatic dicarboxylic acids, preferably (C3-C2o)alkyl diacids, more preferably (C8-C15)alkyl diacids.

[0025] 4. Composition according to any one of the preceding embodiments in which the copolyester is poly(glycerol sebacate) (PGS).

[0026] 5. Composition according to any one of the preceding embodiments in which the copolyester has a number-average molar mass (Mn) ranging from 1000 g / mol to 10000 g / mol.

[0027] 6. Composition according to any one of the preceding embodiments in which the copolyester has a number-average molar mass (Mn) ranging from 1000 g / mol to 5000 g / mol.

[0028] 7. Composition according to any one of the preceding embodiments in which the copolyester content is at most 90% by weight relative to the total weight of the composition.

[0029] 8. Composition according to any one of the preceding embodiments in which the copolyester content varies in a range from 20% to 90% by weight relative to the total weight of the composition.

[0030] 9. Composition according to any one of the preceding embodiments in which the copolyester content varies in a range from 30% to 90% by weight, more preferably 40% to 90% by weight

[0031] 10. Composition according to any one of the preceding embodiments in which the plant load rate is at least 5% by weight relative to the total weight of the composition.

[0032] 11. Composition according to any one of the preceding embodiments in which the plant load rate varies in a range from 5% to 40% by weight, preferably from 8% to 30% by weight, relative to the total weight of the composition.

[0033] 12. Composition according to any one of the preceding embodiments in which the plant load rate varies in a range from 10% to 40% by weight, preferably from 15% to 30% by weight, relative to the total weight of the composition.

[0034] 13. Composition according to any one of the preceding embodiments in which the vegetable filler includes wood flour.

[0035] 14. Composition according to any one of the preceding embodiments in which the vegetable filler is wood flour.

[0036] 15. Composition according to any one of the preceding embodiments in which the plant filler has a median particle size between 20 and 700 microns.

[0037] 16. Composition according to any one of the preceding embodiments in which the at least one phytosanitary or biostimulant active ingredient is a precursor of ethylene, preferably ethephon.

[0038] 17. Composition according to any one of the preceding embodiments in which the rate of aqueous solution is at least 5% by weight relative to the total weight of the composition.

[0039] 18. Composition according to any one of the preceding embodiments in which the rate of copolyester varies in a range from 40% to 90% by weight relative to the total weight of the composition, the rate of aqueous solution is at least 5% by weight relative to the total weight of the composition, and the rate of vegetable filler varies from 5% to 40% by weight relative to the total weight of the composition.

[0040] 19. Composition according to any one of the preceding embodiments for the li controlled release of at least the active phytosanitary ingredient and / or the biostimulant.

[0041] 20. Composition according to any one of the preceding embodiments intended to be applied to the trunk of shrubs and trees.

[0042] 21. Method of treating plants comprising application to the trunk of trees or shrubs at least part of the plants of a composition according to any of the preceding embodiments.

[0043] 22. Method for treating plants according to the preceding embodiment, characterized in that that the trees and shrubs are chosen from the group consisting of rubber trees, vines, olive trees, fruit trees and ornamental plants, preferably rubber trees. DETAILED DESCRIPTION OF THE INVENTION

[0044] The invention relates to a controlled-release composition comprising a biocompatible copolyester obtainable by the polycondensation of a diacid and a polyol, an aqueous solution of at least one phytosanitary active ingredient and / or a biostimulant and a plant filler. Co-polyesters

[0045] The composition according to the invention comprises at least one biocompatible copolyester capable of being obtained by the polycondensation of a diacid and a polyol with a number-average molar mass (Mn) greater than or equal to 1000g / mol.

[0046] By the term "polyol", it is necessary to understand in the sense of the present invention an organic molecule comprising at least two alcohol functions.

[0047] The copolyesters according to the invention are polyesters composed of at least two different units, derived from at least one diacid and at least one polyol.

[0048] According to a preferred embodiment, the diacid is chosen from aliphatic carboxylic diacids, preferably (C3-C2o)alkyl diacids, more preferably (C8-C15)alkyl diacids.

[0049] The diacids are preferably chosen from diacids having two terminal carboxylic acid functions.

[0050] Preferably, the diacid is sebacic acid of general formula below.

[0051] [Chem.l] O

[0052] According to a preferred embodiment, the polyol is chosen from diols and triols, preferably from triols, preferentially the polyol is glycerol of general formula below.

[0053] [Chem.2] OH

[0054] The biocompatible and biodegradable copolyester is advantageously poly(glycerol sebacate) (PGS) and its derivatives, more preferably poly(glycerol sebacate) of general formula below.

[0055] [Chem.3]

[0056] The polyol monomer: diacid monomer ratio is advantageously between 0.3:1 and 1:0.3.

[0057] Poly(glycerol sebacate) can be obtained using a two-step synthesis: a first esterification step and a second polycondensation step, and optionally a third crosslinking step. The first step consists of an esterification reaction between an acid function of sebacic acid and an alcohol function of glycerol. The terminal alcohol functions react preferentially. The second step consists of growing the chains to obtain a PGS resin.

[0058] Then, different strategies can be used to adjust the properties of the polymer, such as long thermal crosslinking by esterification of the pendant secondary alcohol functions (often at high temperature and low pressure), or crosslinking via post-functionalization (such as for example functionalization of the polymer matrix, such as for example acrylate or methacrylate functions, then radical crosslinking or crosslinking with isocyanates, such as for example hexamethylenediamine diisocyanate). It is also possible to carry out a copolymerization of the PGS with blocks of other linear polymers, for example with polylactic acid (PLA), poly(lactic-co-glycolic acid) (PLGA), polycaprolactone (PCL) or poly(butyl succinate) (PBS).

[0059] For the purposes of the present invention, all of these compounds are grouped under the name poly(glycerol sebacate) and its derivatives.

[0060] For example, document WO2015 / 184313A1 describes the synthesis of PGS. Furthermore, PGS is commercially available, notably under the name Regenerez® Poly(glycerol sebacate) Resin.

[0061] Preferably, the biocompatible copolyester is biosourced.

[0062] According to certain embodiments of the invention, the copolyester preferably has a number-average molar mass (Mn) within a range from 1000 g / mol to 10000 g / mol.

[0063] According to certain embodiments, the copolyester preferably has a number-average molar mass (Mn) varying from 1000 g / mol to 5000 g / mol.

[0064] The Mn values ​​can be adjusted simply and in a known manner by modifying the stoichiometry of the monomers, in particular the glycerol / sebacic acid ratio.

[0065] Mn is measured by size exclusion chromatography (SEC) described below in the examples. Plant load

[0066] The composition according to the invention comprises a plant filler.

[0067] According to the invention, the term "plant filler" means a filler comprising lignocellulosic particles or a mixture composed essentially of lignocellulosic particles.

[0068] Lignocellulose is a combination of lignin, hemicellulose and cellulose present in the form of fibers in plant cell walls. Lignocellulosic fibers include wood fibers or fibers from cultivated plants. These include fibers extracted from the trunk or stems (coconut trunk, banana stems, bamboo), straw, fibers extracted from leaves, fibers extracted from seeds or fruits (cotton).

[0069] According to one embodiment of the invention, the plant filler consists of particles whose median size is less than one millimeter. Preferably, according to this embodiment of the invention, the plant filler consists of particles whose median size is within a range of 20 and 700 microns.

[0070] Thus, the lignocellulosic material used as plant filler is finely ground until it reaches this particle size using known grinding processes adapted to each material.

[0071] A major advantage of using this type of material is its reduced impact on the environment and its biodegradability under natural conditions.

[0072] According to a particular embodiment of the invention, the plant filler comprises wood flour, also called wood powder. Most preferably, the plant-based filler is essentially made up of wood flour.

[0073] Preferably, the composition according to the invention comprises at least 5% by weight relative to the total weight of the composition of a plant filler. Indeed, from 5% by weight of plant filler, a notable reduction in the fining of the composition according to the invention is observed, comprising a biocompatible copolyester capable of being obtained by the polycondensation of a diacid and a polyol, and an aqueous solution of at least one phytosanitary active ingredient and / or a biostimulant.

[0074] According to certain preferred embodiments, the composition comprises from 5% to 40% by weight, preferably 8% to 30% by weight, of a plant filler relative to the total weight of the composition.

[0075] According to certain embodiments, the rate of plant filler is advantageously from 10% to 40% by weight, or even from 15% to 30% by weight, relative to the total weight of the composition. Indeed, the fining of a composition comprising a copolyester according to the invention, in particular when the copolyester is a PGS, and an aqueous solution of at least one phytosanitary active ingredient and / or a biostimulant, is then low, "low" here means that a composition comprising a copolyester and an aqueous solution of at least one phytosanitary active ingredient and / or a biostimulant has a percentage weight loss of 5% or less under the conditions of the tests described below. Aqueous solution of at least one active ingredient

[0076] The composition according to the invention comprises an aqueous solution of at least one phytosanitary active ingredient and / or a biostimulant.

[0077] According to certain embodiments of the invention, the aqueous solution represents at least 5% by weight of the total weight of the composition.

[0078] According to other embodiments of the invention, the aqueous solution represents at least 10% by weight of the total weight of the composition.

[0079] Those skilled in the art will understand that the quantity of aqueous solution in the composition according to the invention depends in particular on the dilution rate of the active ingredient in the solution and the quantity of active ingredient desired in the composition.

[0080] Phytosanitary and / or biostimulant active ingredients

[0081] The composition according to the invention comprises at least one phytosanitary active ingredient and / or a biostimulant in solution in the aqueous solution. The active ingredient is preferably chosen from the group consisting of stimulants, fertilizers, pesticides, fungicides, nutrients, bactericides, insecticides, growth regulators.

[0082] Preferably, the composition according to the invention comprises a phytosanitary active ingredient and / or a biostimulant which is a precursor of ethylene, preferentially ethephon. Additives

[0083] The composition according to the invention may comprise one or more additives. Mention may in particular be made of stabilizers, compatibilizing agents, shaping agents, regulators of release of the active ingredient, antioxidants, etc. Shape

[0084] The composition according to the invention can advantageously be in the form of a paste. This paste can then be shaped in different ways depending on its application. Advantageously for application to a tree or shrub trunk, this paste can be shaped, for example, by molding or calendering, or it can be transferred by extrusion.

[0085] When the composition according to the present invention is in the form of a paste, the composition according to the invention advantageously comprises up to 90% by weight, preferably from 20% to 90% by weight, more preferably 30% to 90% by weight, more preferably 40% to 90% by weight of a biocompatible copolyester capable of being obtained by the polycondensation of a diacid and a polyol.

[0086] When the composition according to the present invention is in the form of a paste, it advantageously comprises from 1% to 50% by weight, preferably from 5% to 40% by weight, particularly preferably 5% to 30% by weight of aqueous solution of at least one active ingredient. Preparation process

[0087] Various methods for preparing the composition according to the invention comprising the copolyester, the plant filler and the phytosanitary active ingredient and / or the biostimulant may be used. Mention may be made, without limitation, of a mixture of molten copolyester with the plant filler and the aqueous solution.

[0088] This mixture can be produced in a conventional stirred reactor at relatively mild temperatures to limit the risks of degradation of the phytosanitary active ingredient and / or the biostimulant, preferably <100°C, using conventional mixers. The mixing process can be batch, semi-batch or continuous. Application process

[0089] According to the present invention, it is preferentially applied to at least part of the plants, preferably one or more aerial part(s).

[0090] According to one embodiment, the composition according to the invention is intended to be applied to the trunk of shrubs and trees. The composition is then presented in particular in the form of a paste as explained above.

[0091] According to one embodiment, the method for treating plants according to the invention relates to trees or shrubs and the composition is applied to the trunk.

[0092] The trees or shrubs are preferably chosen from the group consisting of rubber trees, vines, olive trees, fruit trees and ornamental plants.

[0093] When the composition according to the present invention is in the form of a paste, it is preferably sticky and can be spread with a spatula or with an application device of the mastic gun type, allowing application of a controlled mass to the plant.

[0094] A device composed of a “hard” layer in contact with a “sticky” layer of the patch type pre-cut to suitable dimensions can also be envisaged. It can be fixed to one or more aerial part(s) of the plant, for example on the trunk or for example on the leaves or fruits.

[0095] The following examples illustrate the invention without limiting its scope. Examples

[0096] Method of analysis by size exclusion chromatography (SEC)

[0097] The PGS samples were solubilized at a concentration of approximately 1.5 gL 1 in THF, then stirred for 2 hours before being injected.

[0098] The analytical conditions used are described in the table below:

[0099] [Tables 1] Eluent THF Injection volume 100 pL Concentration ~ 1.5 g / L Temperature 35 °C Detector RI Waters Mobile phase flow rate 1 mL / min Columns 2 Mixed D + 2 Mixed E calibration Polystyrene (PS)

[0100] The analyzable mass range is between 162 g / mol and 7,500,000 g / mol. The number-average molecular mass (Mn) is expressed in g / mol in PS equivalent, likewise the weight-average molecular mass (Mw) is expressed in g / mol in PS equivalent. The dispersity D is defined by the relation Mw / Mn. Copolyesters: Summary of PGS:

[0101] Three PGS samples were prepared by mixing glycerol with sebacic acid according to the following procedures: PGS1:

[0102] In a 500 mL double-jacketed reactor topped with a column of dis In a reactor configured for total reflux and a condenser connected to a distillate recovery vessel, glycerol (124 g, 1.5 molar equiv.) is mixed with water (24 g) at room temperature under nitrogen flow (0.1 L / min). Gentle stirring is implemented (50 rpm) for 5 min. After dissolving the glycerol, sebacic acid (182 g, 1 molar equiv.) is added to the aqueous mixture in the reactor. Finally, the remaining water is added to the medium (24 g). The reactor vessel is then heated to a jacket temperature of 140 °C. Stirring is gradually increased to 100 rpm and then 150 rpm with the melting and increasing solubilization of the acid. When the medium in the tank has become clear (around 95°C), the stirring is increased to a final value of 200 rpm and the medium left to reflux.When the vapor temperature at the top of the distillation column reaches 98°C, and after an equilibration time of 15 min, the column configuration is switched to total withdrawal. Esterification of the medium is carried out over a period of 26 hours. The water distilled during the test is recovered in a dedicated heat-insulated recovery pot.

[0103] Next, a vacuum installation is connected to the distillation condenser and a pressure below atmospheric pressure is applied to the reactor contents. The pressure is reduced slowly and stepwise (about 10 to 15% per step) over about 30 minutes to a target value of less than 10 mbar.

[0104] Once the pressure in the reaction vessel stabilizes at 5 mbar, the medium is left to react at 150 °C for a further 4 h. During this polycondensation step, the stirring speed is reduced to 115 rpm to account for the increased viscosity of the mixture.

[0105] The produced PGS is transferred from the reactor vessel to a container after the installation has been depressurized and allowed to cool to room temperature. The product is then transferred to a freezer for storage, where it is frozen for at least about 24 hours before analysis.

[0106] The polymer obtained has the following characteristics: Number average molecular mass (Mn, g / mol) 1316 Weight average molecular mass (Mw, g / mol) 2297 Polydispersity index D 1.7 PGS 2

[0107] In a 500 mL double jacketed reactor topped with a distillation column configured in total reflux and a condenser connected to a distillate recovery pot, glycerol (112 g, 1.3 molar equiv.) is mixed with water (25 g) at room temperature under nitrogen flow (0.1 L / min). Gentle stirring is implemented (50 rpm) for 5 min. After dissolution of the glycerol, acid Sebacic acid (189 g, 1 molar equiv.) is added to the aqueous mixture in the reactor. Finally, the remaining water is added to the medium (25 g). The reactor vessel is then heated to a jacket temperature of 140 °C. Stirring is gradually increased to 100 rpm and then 150 rpm with the melting and increasing solubilization of the acid. When the medium in the vessel has become clear (around 95 °C), stirring is increased to a final value of 200 rpm and the medium is left to reflux. When the vapor temperature at the top of the distillation column reaches 98 °C, and after an equilibration time of 15 min, the column configuration is switched to total withdrawal. Esterification of the medium is carried out over a period of 26 h. The water distilled during the test is collected in a dedicated heat-insulated recovery pot.

[0108] Next, a vacuum installation is connected to the distillation condenser and a pressure below atmospheric pressure is applied to the reactor contents. The pressure is reduced slowly and stepwise (about 10 to 15% per step) over about 30 minutes to a target value of less than 10 mbar.

[0109] Once the pressure in the reaction vessel stabilizes at 5 mbar, the medium is left to react at 150 °C for a further 5 h. During this polycondensation step, the stirring speed is reduced to 115 rpm to account for the increased viscosity of the mixture.

[0110] The produced PGS is transferred from the reactor vessel to a container after the installation has been brought back to atmospheric pressure and allowed to cool to room temperature. The product is then transferred to a freezer for storage, where it is frozen for at least about 24 hours before analysis.

[0111] The polymer obtained has the following characteristics: Number average molecular mass (Mn, g / mol) 1659 Weight average molecular mass (Mw, g / mol) 3455 Polydispersity index D 2.1 PGS 3

[0112] In a 10L double-jacketed stainless steel reactor topped with an instrumented distillation column configured for total reflux and a condenser connected to a distillate recovery pot, glycerol (1.94 kg, 1 molar equiv.) is mixed with water (0.56 kg) at 40 °C under nitrogen flow (0.5L / min). Gentle stirring is implemented (20 rpm) for 5 min. After dissolving the glycerol, sebacic acid (4.25 kg, 1 molar equiv.) is added to the aqueous mixture in the reactor. Finally, the remaining water is added to the medium (0.56 kg). The reactor vessel is then gradually heated, respecting a gradual temperature increase ramp with intermediate stages, until a jacket temperature of 172 °C is reached. after 5 hours, corresponding to a medium temperature of 170°C, measured using a immersion probe. Stirring is increased to 80 rpm when the medium temperature exceeds 90°C. The medium is left at reflux at the start of the test. When the vapor temperature at the top of the distillation column reaches 98°C, and after an equilibration time of 15 min, the column configuration is switched to total withdrawal in order to selectively recover the water produced during the reaction.

[0113] The esterification of the medium is carried out over a total duration of 8h30, considering as the starting point the moment when the distillation begins, i.e. approximately 30 min after the introduction of the reagents. The water distilled during the test is recovered in a dedicated heat-insulated recovery pot.

[0114] Next, a vacuum installation is connected to the distillation condenser and a pressure below atmospheric pressure is applied to the reactor contents. The pressure is reduced slowly and stepwise (about 10 to 15% per step) over about 30 minutes to a target value of less than 30 mbar.

[0115] Once the pressure in the reaction vessel stabilizes at 28 mbar, the medium is left to react at 170 °C for a further 4 hours. During this polycondensation step, the stirring speed is maintained at 80 rpm.

[0116] The produced PGS is transferred from the reactor vessel to a container and allowed to cool to room temperature. The product is then transferred to a freezer for storage, where it is frozen for at least about 24 hours before analysis.

[0117] The polymer obtained has the following characteristics: Number average molecular mass (Mn, g / mol) 2656 Weight average molecular mass (Mw, g / mol) 16520 Polydispersity index D 6.2

[0118] The PGS obtained have the characteristics summarized in Table 1.

[0119] [Tables 1] PGS 1 PGS 2 PGS 3 Mn 1316 1659 2656 IP 1.7 2.1 6.2

[0120] Tests with different compositions in accordance with the invention Formulation of the compositions:

[0121] A sample of PGS is introduced into a pot of suitable size and heated in a water bath at 50°C until a viscous texture is obtained. After homogenizing the PGS using a spatula, a 50% by mass aqueous solution of ethephon is added to the PGS outside the water bath and incorporated by mixing at the spatula. If necessary, wood flour is also added to the mixture, dividing the additions as needed. The composition is mixed with a spatula until a homogeneous paste is obtained. The mixture is then cooled to room temperature and then packed in the freezer.

[0122] The proportions of the different constituents, expressed as a percentage by weight relative to the total weight of the composition, are reported in Tables 2 and 3, respectively concerning the compositions based on PGS of Mn 1300 g / mol and the compositions based on PGS of Mn 1660 g / mol.

[0123] [Tables2] Compositions Constituents MP5 (control n) MP5+1 0 MP15 (control n) MP 15+ 5 MP15+1 0 MP15+1 5 MP15+2 0 PGS 1 (1316g / mol) 95 85 85 80 75 70 65 Soil aq 50% ethephon 5 5 15 15 15 15 15 Wood flour (*) 0 10 0 5 10 15 20 Total by weight 100 100 100 100 100 100 100

[0124] * Wood flour from the company Sylvadec with an average size of 200 microns

[0125] [Tables3] Compositions Constituents HP15 (control) HP 15+5 HP15+10 HP15+15 HP 15+20 PGS 2 (1659g / mol) 85 80 75 70 65 Sol aq 50% ethephon 15 15 15 15 15 Wood flour (*) 0 5 10 15 20 Total by weight 100 100 100 100 100

[0126] * Wood flour from the company Sylvadec with an average size of 200 microns

[0127] In the notation MPY+X and HPY+X, it is necessary to understand Y as the rate of aqueous solution and X as the rate of wood flour. Production of the pellets of composition:

[0128] The preparation is taken out of the freezer. 10g of the desired formulation is placed between two silicone sheets. The mixture is calendered with a cylinder tool between the two silicone sheets at 3mm and then pellets are cut with a die cutter: thickness = 3mm, diameter = 40mm, mass approximately 4g.

[0129] Peeled poplar boards measuring 8cm x 5cm with a 1cm x 1xm grid are prepared and dried in an oven at 40°C for 72 hours. A pellet is pressed onto each piece of wood, then the grid is completed on the pellet and weighed.

[0130] The poplar plate / patch assemblies for each composition are placed in a vertical position in an oven at 40°C (without humidity control). The evolution of the patches is monitored daily by taking photos and weighing them.

[0131] The purpose of these tests is to show the effect of the plant load on the finishing of a composition comprising PGS and an aqueous solution of a biostimulant active ingredient such as ethephon. Results.

[0132] The results visible in [Fig.l] and in [Fig.2] come from measurements and observations involving the loss of mass and the dimensional change (via photos) on each wooden test piece after 96 hours of steaming at 40°C.

[0133] It is thus noted that compared to the control compositions, respectively MP5, MP15 and HP15, the addition of wood flour in these compositions (respectively MP5+X, MP15+X and HP15+X, X being the wood flour content) makes it possible to reduce the fining at 40°C, or even to very significantly reduce the fining at 40°C when X is at least 10 (i.e. 10% by weight of wood flour) without impacting the adhesion to the wood substrate after 96 hours.

[0134] It can thus be seen, according to the examples of the invention described here, that by introducing a proportion of a vegetable filler of the wood flour type, it is possible to avoid fining while retaining good adhesion properties of a composition based on poly (glycerol sebacate) and an aqueous solution of ethephon on a wood surface. Tests on the nature of the filler Formulation of the compositions:

[0135] The following tests aim to show the effect of the plant filler on the finishing of a composition comprising PGS and an aqueous solution in comparison with other fillers.

[0136] In these tests, a sample of PGS of Mn 2656 g / mol is introduced into a pot of suitable size and heated in a water bath at 50°C until a viscous texture is obtained. After homogenizing the PGS using a spatula, water is added to the PGS outside the water bath and incorporated by mixing with the spatula. A filler is then added to the mixture, dividing the additions as needed. The composition is mixed with the spatula until a homogeneous paste is obtained. The mixture is then cooled to room temperature and then packaged in the freezer.

[0137] These tests show that only a plant-based charge makes it possible to reduce the fining of a composition based on PGS and water.

[0138] The proportions of the different constituents, expressed as a percentage by weight relative to the total weight of the composition, are shown in Table 4.

[0139] [Tables4] Compositions Constituents HP0 HP1 HP2 HP3 HP4 PGS 3 (2656 g / mol) 100 80 80 80 80 Wood flour (1) 20 CO filler (2) 20 CaCO3 filler (3) 20 Kaolin filler (4) 20 Total by weight 100 100 100 100 100

[0140] (1) Wood flour from the company Sylvadec, average size 200 microns (2) Eggshell powder from Lunderland Company, median size 17 microns (3) Calcium carbonate powder of average size 6 microns (4) Natural kaolin grade Argirec B24 from the company IMERYS with an average size of 200 microns. Preparation of the composition tablets:

[0141] The sample pellets are made in accordance with the operating protocol described above. Results.

[0142] The results visible in [Fig.3] come from measurements and observations involving mass loss and dimensional change (via photos) on each wooden test piece after 96 hours of steaming at 40°C.

[0143] It is thus noted that unlike compositions HP2, HP3 and HP4 containing respectively an eggshell filler, calcium carbonate and kaolin, the composition of the invention HP1 containing wood flour, has a reduced fining at 40°C without impacting the adhesion to the wood substrate after 96 hours.

[0144] It can thus be seen that by introducing a proportion of vegetable filler of the wood flour type, it is possible to significantly reduce the fining at 40°C while retaining good adhesion properties of a composition based on poly (glycerol sebacate) and water on a wood surface.

Claims

Claims

1. Composition comprising - at least one biocompatible copolyester capable of being obtained by the polycondensation of a diacid and a polyol with a molar mass greater than or equal to 1000g / mol, - a plant filler, and - an aqueous solution of at least one phytosanitary active ingredient and / or a biostimulant.

2. Composition according to the preceding claim in which the diacid is chosen from aliphatic carboxylic diacids, preferably (C3-C2o)alkyl diacids, more preferably (C8-C15)alkyl diacids.

3. A composition according to any preceding claim wherein the copolyester is poly(glycerol sebacate) (PGS).

4. Composition according to any one of the preceding claims in which the copolyester has a number-average molar mass (Mn) in a range from 1000 g / mol to 10000 g / mol.

5. Composition according to any one of the preceding claims in which the copolyester content varies within a range from 20% to 90% by weight relative to the total weight of the composition.

6. Composition according to any one of the preceding claims in which the rate of plant filler is at least 5% by weight relative to the total weight of the composition.

7. Composition according to any one of the preceding claims in which the rate of plant filler varies in a range from 5% to 40% by weight, preferably from 8% to 30% by weight, relative to the total weight of the composition.

8. Composition according to any one of the preceding claims in which the vegetable filler is a wood flour.

9. A composition according to any preceding claim wherein the plant filler has a median particle size of between 20 and 700 microns.

10. Composition according to any one of the preceding claims in which the at least one phytosanitary or biostimulant active ingredient is a precursor of ethylene, preferably ethephon.

11. A composition according to any preceding claim. in which the rate of aqueous solution is at least 5% by weight relative to the total weight of the composition.

12. Composition according to any one of the preceding claims for the controlled release of at least the phytosanitary active ingredient and / or the biostimulant.

13. Composition according to any one of the preceding claims intended to be applied to the trunk of shrubs and trees.

14. A method of treating plants comprising applying to the trunk of trees or shrubs at least a portion of the plants a composition according to any one of the preceding claims.

15. Method of treating plants according to the preceding claim, characterized in that the trees and shrubs are chosen from the group consisting of rubber trees, vines, olive trees, fruit trees and ornamental plants, preferably rubber trees.

Citation Information

Patent Citations

  • FR2113693A5

  • Composite containing poly(glycerol sebacate) filler

    US20170246316A1

  • Composition, articles and methods for wound care

    US20180050128A1

  • Methods of electrospinning and compositions made therefrom

    US20180251596A1

  • Water-mediated preparations of polymeric materials

    WO2015184313A1

Cited By

  • Use of poly(2-oxazoline) for improving the extensibility of crosslinked glycerol polyesters

    WO2026087530A1