Pine-type perovskite-based photovoltaic cell
The use of an alumina buffer layer in a PIN-type perovskite photovoltaic cell addresses performance and stability issues by reducing charge recombination and ion diffusion, ensuring high efficiency and durability.
Patent Information
- Application Number
- FR2023004661
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional perovskite-based photovoltaic cells face performance degradation due to charge recombination at interfaces and ion diffusion, particularly when using metal oxide buffer layers, which require high deposition temperatures and are not suitable for industrial applications, while organic buffer layers lack stability at elevated temperatures and uniformity.
A PIN-type perovskite photovoltaic cell utilizing an alumina buffer layer of 1-5 nm thickness, deposited via ALD, which improves stability and performance by reducing charge recombination and ion diffusion, and is compatible with industrial production.
The alumina buffer layer enhances photovoltaic cell performance and stability, maintaining efficiency and reducing degradation, even under industrial conditions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Photovoltaic cell based on pin-type perovskite Technical field
[0001] The present invention relates to the general field of perovskite-based photovoltaic cells.
[0002] The invention relates to a photovoltaic cell based on PIN type perovskite.
[0003] The invention also relates to a method of manufacturing such a photocell. voltaic.
[0004] The invention is particularly interesting since it makes it possible to obtain photovoltaic cells having good performance while being stable over time. STATE OF THE PRIOR ART
[0005] Conventionally, a perovskite-based photovoltaic cell comprises, from the rear face to the front face:
[0006] - an upper electrode,
[0007] - a buffer layer,
[0008] - an n-type layer,
[0009] - an active perovskite layer,
[0010] - a p-type layer,
[0011] - a transparent conductive oxide,
[0012] - a substrate.
[0013] The incident light radiation arrives on the front face of the photovoltaic cell. This configuration corresponds to a PIN type solar cell (also called inverse type). The p-type layer is a hole transport layer (or HTL for "Hole transport Layer").
[0014] The part acting as the electron transport layer (or ETL for “Electron transport Layer”) is a bilayer formed from the n-type layer and the buffer layer.
[0015] Without the presence of the buffer layer, the performance of the cell is reduced. Charge recombinations at the interfaces between the perovskite layer and the upper electrode increase and the photovoltaic efficiency decreases. In addition, there is diffusion of ions (e.g. iodine ions) between the active perovskite layer and the upper electrode, which contributes to the degradation of stability of the photovoltaic cell.
[0016] The buffer layer serves to i) eliminate the accumulation of charges between the electrode upper and the n-type semiconductor, ii) facilitate the extraction of electrons and block the carrier holes and iii) thus reduce the recombination of charges at the n-layer / upper electrode interface.
[0017] It is possible to use several materials for the buffer layer of perovskite-based photovoltaic cells. Generally, these are materials chosen from LiF, SnS, metal oxides and BCP (bathocuproine).
[0018] Metal oxides have better temperature stability. However, they are formed by dry deposition methods requiring a high deposition temperature (typically above 100°C), which degrades the surface of the perovskite active layer.
[0019] As an example, the use of a 20 nm buffer layer of SnOx metal oxide above the n-layer (n / SnOx layer) has already been studied (H. Chen et al. “Regulating surface potential maximizes voltage in all-perovskite tandems”, Nature volume 613, pages 676-681 (2023)). The oxide layer is deposited by ALD. However, the deposition of a SnOx layer requires relatively long deposition times and may require temperatures above 90°C, leading to degradation of the lower layers (in particular to degradation of the active perovskite layer). Such a process is not suitable for industrial requirements.
[0020] The use of an organic layer in BCP makes it possible to obtain a good compromise between performance and stability. However, BCP does not have good stability at 85°C (temperature required to meet the standards of the International Electrotechnical Commission (or IEC for "International Electrotechnical Commission")). In addition, the BCP buffer layer must be thin enough for electrons to pass through it by tunneling. However, BCP is deposited by thermal evaporation, which does not lead to the formation of thin and uniform layers. In addition, for large surfaces (typically necessary for industrial applications), the BCP layers present constraints, which are detrimental to the proper functioning of the photovoltaic cell. Statement of the invention
[0021] An aim of the present invention is to propose a PIN type photovoltaic cell based on perovskite which overcomes the drawbacks of the prior art, and in particular which has good performance whilst being stable over time.
[0022] For this, the present invention proposes a photovoltaic cell based on pin-type perovskite comprising successively, from the rear face to the front face, at least:
[0023] - an alumina buffer layer, having a thickness between 1 nm and 5 nm,
[0024] - an n-type layer,
[0025] - an active perovskite layer of formula APbX3 with A representing cations methylammonium, dimethylammonium, formamidinium, guanidinium and / or cesium (i.e. the cations can be used alone or in mixture) and X representing halide anions.
[0026] The invention is fundamentally distinguished from the prior art by the use of an alumina buffer layer having a thickness of between 1 and 5 nm.
[0027] Alumina means aluminum oxide of formula A12O3. A slight tolerance on the stoichiometry may be allowed and the material may thus correspond to the formula A1OX with x between 0.8 and 1.5. By x between X and Y, it is meant here and hereinafter that the limits are included.
[0028] The alumina layer is a material stable at high temperature and humidity. The use of an alumina buffer layer instead of a BCP buffer layer improves not only the performance of the devices, but also the stability of the photovoltaic cell.
[0029] Advantageously, the alumina buffer layer has a thickness of between 3 and 4 nm.
[0030] Advantageously, the n-type layer is a C6o, PC6iBM, PC71BM, PCBM / C6o or PCBM / C layer.
[0031] Advantageously, an upper electrode made of silver, copper, aluminum or nickel covers the alumina buffer layer.
[0032] Advantageously, the cell comprises successively from the rear face to the front face:
[0033] - an upper electrode, for example made of silver,
[0034] - the alumina buffer layer,
[0035] - the n-type layer, for example in C60,
[0036] - the active layer based on APbX3 type perovskite, for example in CsAFPbIBr, and more particularly in (FAo.83Cso.i7)Pb(Io.6Bro.4)3,
[0037] - a p-type layer, for example a self-assembled layer, in particular a 2-PACz layer,
[0038] - a layer of transparent conductive oxide, for example indium-tin oxide,
[0039] - a substrate, for example made of glass.
[0040] The invention also relates to a method for manufacturing a photovoltaic cell as defined above. The method comprises a step during which the alumina buffer layer is formed by an atomic layer deposition (ALD) step on the n-type layer.
[0041] This deposition technique is not only suitable for the growth of thin and conformal layers, large surfaces but also for industrial requirements. In addition, compared to physical vapor deposition, ALD has a better lateral uniformity. It is adapted to the requirements of the photovoltaic market.
[0042] Advantageously, the temperature during the formation of the alumina buffer layer is between 25°C and 100°C, preferably between 40°C and 75°C.
[0043] Advantageously, the alumina buffer layer is formed, in a deposition chamber, by carrying out one or more times a cycle comprising the following sub-steps:
[0044] - injecting into the deposition chamber an aluminum precursor, preferably trimethylaluminum (formula A12(CH3)6, also noted TMA), then purge the deposition chamber,
[0045] - injecting into the deposition chamber an oxygen precursor, preferably water or ozone, then purge the deposition chamber.
[0046] Advantageously, the aluminum precursor is TMA and the oxygen precursor is water.
[0047] Advantageously, the cycle is carried out between 10 and 50 times, preferably between 30 and 40 times.
[0048] Advantageously, the temperature during the formation of the alumina buffer layer is between 45°C and 55°C and the cycle is carried out between 30 and 40 times.
[0049] The process has many advantages:
[0050] - production of continuous, uniform and homogeneous A12O3 / A1OX layer deposition on the n-layer of perovskite-based photovoltaic devices,
[0051] - deposition of a conforming layer and, consequently, adapted to industrial demands and / or textured substrates.
[0052] Other characteristics and advantages of the invention will emerge from the additional description which follows.
[0053] It goes without saying that this additional description is given only as an illustration of the subject of the invention and must in no case be interpreted as a limitation of this subject. Brief description of the drawings
[0054] The present invention will be better understood on reading the description of exemplary embodiments given purely for informational purposes and in no way limiting, with reference to the appended drawings in which:
[0055] - [Fig.l] represents, schematically and in section, a photocell voltaic according to a particular embodiment of the invention; the incident light radiation arriving on the front face of the photovoltaic cell is represented by arrows,
[0056] - [Fig.2A]
[0057] - [Fig.2B]
[0058] - [Fig.2C]
[0059] - [Fig.2D] are graphs representing the filling factor (noted FF for "Fill Factor"), the short-circuit current density (denoted Jsc), the energy conversion efficiency (PCE) and the open-circuit voltage (Voc) for photovoltaic cells comprising alumina layers of different thicknesses, according to different particular embodiments of the invention, and for a photovoltaic cell comprising a BCP buffer layer according to an example given for comparison,
[0060] - [Fig.3A]
[0061] - [Fig.3B]
[0062] - [Fig.3C]
[0063] - [Fig.3D] are graphs representing the FF, the Jsc, the PCE and the Voc for photovoltaic cells comprising a 3.6nm thick alumina layer deposited at different temperatures, according to different particular embodiments of the invention, and for a photovoltaic cell comprising a BCP buffer layer according to an example given for comparison,
[0064] - [Fig.4] is a graph representing a JV curve of a photocell voltaic comprising an alumina buffer layer, according to a particular embodiment of the invention, and a photovoltaic cell comprising a BCP buffer layer given for comparison, under illumination (AM1.5G) at 25°C by applying upward or downward directions,
[0065] - [Fig.5] is a photographic image representing the front face of different photovoltaic cells: a photovoltaic cell comprising a BCP buffer layer used for comparison, one week (left) and 75 days (middle) after their preparation and a photovoltaic cell comprising an alumina buffer layer, according to a particular embodiment of the invention, 75 days after its preparation (right); the photovoltaic cells are stored under N2 during this period.
[0066] The different parts represented in [Fig.l] are not necessarily on a uniform scale, to make the figures more readable.
[0067] Furthermore, in the following description, terms that depend on the orientation, such as "above", "below", etc. of a structure apply with the assumption that the structure is oriented as illustrated in the figures.
[0068] DETAILED DESCRIPTION OF PARTICULAR EMBODIMENTS
[0069] We will now describe in more detail a perovskite-based photovoltaic cell with PIN-type architecture according to the invention.
[0070] More particularly, the photovoltaic cell, of the pin type, comprises from the rear face to the front face ([Fig.l]):
[0071] - an upper electrode 10,
[0072] - an alumina buffer layer 20,
[0073] - a layer of type n 30,
[0074] - an active layer of perovskite 40,
[0075] - a p 50 type layer,
[0076] - a layer of transparent conductive oxide 60,
[0077] - a substrate 70.
[0078] Preferably, the photovoltaic cell is made up of the different elements mentioned above.
[0079] The front face of the photovoltaic cell is intended to receive a luminous flux. The incident radiation is represented by arrows in [Fig.l].
[0080] The upper electrode 10 is, for example, made of Ag, Cu, Ni, Al. It has, for example, a thickness of between 50 and 300 nm.
[0081] The buffer layer 20 has a thickness of between 1 nm and 5 nm, preferably between 3 and 4 nm. It is advantageously continuous and conformal. It is in direct contact with the n-type layer.
[0082] This is a layer of alumina of formula A12O3 or formula A1OX with x between 0.8 and 1.5.
[0083] The n 30 type layer may be, for example, C6o, PC6iBM ([6,6]-phenyl-C6i-methyl butanoate or “[6,6]-phenyl-C6i-butyric acid methyl ester”), PC71BM ([6,6]-phenyl-C7i-methyl butanoate or “[6,6]-phenyl-C7i-butyric acid methyl ester”), PCBM / C60 or PCBM / C. Preferably, it is C60. The n 30 type layer has, for example, a thickness of between 5 and 50 nm.
[0084] According to other embodiments, the n-type layer 30 may be an oxide layer, for example SnOx (with x between 1 and 2), ZnO, Al:ZnO, ITO or IZO. Such layers have a thickness between 5 and 30 nm.
[0085] The active layer 40 is an active layer of perovskite of type APbX3 with A representing methylammonium, dimethylammonium, formamidinium, guanidinium or cesium cations (the aforementioned cations can be used alone or in a mixture) and X representing halide anions (preferably chlorine, bromine, iodine anions alone or in a mixture).
[0086] The active layer 40 has, for example, a thickness of between 200 nm and 1.5 pm.
[0087] According to a first variant, the p 50 type layer may be a layer of poly(3,4-ethylenedioxythiophene) (PEDOT) or poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine (PTAA). It may have a thickness between 5 and 50 nm.
[0088] According to a second variant, the p-type layer 50 is a self-assembled layer (or SAM for “Self-Assembled Monolayer”). The SAM layer can be a layer of 2PACz ([2-(9H-Carbazol-9-yl)ethyl]phosphonic acid), 3PACz (3-(9H-carbazol-9-yl)propyl)phosphonic acid), 4PACz (4-(9H-carbazol-9-yl)butyl)phosphonic acid), Me-4PACz (acid (4-(3,6-Dimethyl-9H-carbazol-9-yl)butyl)phosphonic acid), MeO-2PACz ((2-(3,6-Dimethoxy-9H-carbazol-9-yl)ethyl)phosphonic acid), 6dPA (1,6-hexylenediphosphonic acid) or a layer of MPA (methylphosphonic acid) or a layer obtained from a mixture of these molecules. It can also be one of their derivatives. Additives can also be added. The molecules of the SAM layer advantageously have a function allowing them to anchor themselves on the underlying oxide layer. Such a p 50 type layer can have a thickness between 1 and 5 nm.
[0089] According to a third variant, the p-type layer 50 is an oxide layer, for example a MoOx layer (having for example a thickness between 5 and 30 nm), a NiOx layer (having for example a thickness between 1 and 30 nm).
[0090] According to another variant, the p-type layer 50 may be an oxide / SAM bilayer, for example a NiOx / SAM bilayer.
[0091] The transparent conductive oxide layer 60 has, for example, a thickness of between 50 and 300 nm. Preferably, it is indium-tin oxide (or ITO).
[0092] These different elements are positioned on a substrate 70 arranged on the rear face. The substrate 70 is for example made of glass.
[0093] For example, the photovoltaic cell comprises from the rear face to the front face:
[0094] - an upper electrode 10 made of silver,
[0095] - an alumina buffer layer 20,
[0096] - a layer of type n 30 in C60,
[0097] - an active layer 40 in (FAo.83Cso.i7)Pb(Io.6Bro.4)3,
[0098] - a layer of type n 50 in 2PACz,
[0099] - a layer of transparent conductive oxide 60 in ITO,
[0100] - a substrate, preferably made of glass 70.
[0101] We will now describe in more detail the manufacturing process of such a photovoltaic cell.
[0102] The method comprises at least one step during which the alumina buffer layer 20 is deposited by ALD. This step is carried out at a temperature between 25°C and 100°C, preferably between 40 and 75°C, for example between 45 and 55°C.
[0103] The deposition of the alumina layer 20 is carried out from two precursors: an aluminum precursor and an oxygen precursor.
[0104] The precursor of aluminum is preferably trimethylaluminum A12(CH3)6 (TMA).
[0105] The oxygen precursor may be water or ozone. Preferably, it is water.
[0106] The ALD deposition step consists of carrying out the following cycle of sub-steps one or more times:
[0107] - injecting into a deposition chamber an aluminum precursor, preferably TMA, then purge the deposition chamber,
[0108] - injecting into the deposition chamber an oxygen precursor, preferably water, then purge the deposition chamber.
[0109] The precursors are introduced into the deposition chamber sequentially, one after the other, after purging the deposition chamber with an inert gas (N2). Thus, the precursors react only with the surface of the material and not with each other.
[0110] The pressure in the deposition chamber is, for example, between 0.6 and 10 mbar (i.e. between 60 Pa and 1000 Pa).
[0111] The thickness of AlOx deposited per cycle is equal to 1 Å. For example, in order to have a 3-4 nm A1OX layer, the cycle will be repeated between 30 and 40 times.
[0112] By way of illustration and not limitation, the deposition of the alumina layer is obtained by carrying out several cycles comprising the following sub-steps:
[0113] - insertion of the TMA gas into the deposition chamber; the duration of the pulse and the flow of TMA are 500 ms and 300 sccm respectively,
[0114] - insertion of N2 into the chamber to perform a purge; the duration of the pulse and the flow of N2 are 5 s and 300 sccm respectively,
[0115] - insertion of H2O gas into the deposition chamber: the duration of the pulse and the flow of H2O are 500 ms and 300 sccm respectively,
[0116] - insertion of N2 into the chamber to perform a purge; the duration of the pulse and the flow of N2 are 6 s and 300 sccm respectively.
[0117] The upper electrode 10 can be deposited by thermal evaporation or by physical vapor deposition (EBPVD or “Electron Beam Physical Vapor Deposition”).
[0118] When the n 30 type layer is made of C60, PC6iBM, PC7iBM, PCBM / C60 or PCBM / C, it can be deposited by thermal evaporation or by liquid deposition technique.
[0119] By way of illustration and non-limiting example, here and hereinafter, the liquid deposition technique may be, for example, spin coating, a slot die coating technique or a doctor blade coating technique.
[0120] When the n-type layer 30 is an oxide layer, it can be deposited by ALD or sputtering for example. A SnOx layer could also be deposited by a liquid deposition technique.
[0121] The active layer 40 can be deposited by thermal evaporation or co-evaporation (for example, physical vapor deposition, also known as PVD), short-distance sublimation (or CSS for “Close space sublimation”), pulsed laser ablation deposition (PLD for “Pulsed Laser deposition”). Hybrid deposition methods can also be envisaged. This could involve one of the aforementioned deposition methods combined with a liquid deposition technique.
[0122] When the p-type layer 50 is a PEDOT or PTAA layer, it can be deposited by a liquid deposition technique.
[0123] When the p-type layer 50 is a self-assembled layer, it can be deposited by a liquid deposition technique or by thermal evaporation.
[0124] When the p-type layer 50 is an oxide layer, it can be deposited, for example, by thermal evaporation, ALD or sputtering.
[0125] The conductive transparent oxide layer 60 can be deposited by cathode sputtering.
[0126] Illustrative and non-limiting examples of an embodiment
[0127] In the illustrative and comparative examples which follow, the different elements of the photovoltaic cells (apart from the buffer layer) were all manufactured according to the same protocol. Manufacturing of the photovoltaic cell
[0128] The photovoltaic cells were manufactured according to the following steps:
[0129] - providing a glass substrate 70 covered by a transparent oxide layer conductor 60, preferably ITO,
[0130] - depositing by spin coating a p 50 type layer of 2PACz; the deposit is carried out in a glove box under N2; then carry out a heat treatment for 10 min at 100°C,
[0131] - deposit by spin coating a layer of perovskite 40, the deposition is carried out in a glove box under N2; then carry out a heat treatment for 1 hour at 100°C,
[0132] - deposit a layer of type n 30 in C60 by thermal evaporation under vacuum (1.10 6 mbar, or 1.10 4 Pa) with a deposition rate of 0.1 to 0.3 Å / s; during deposition the stack of glass / ITO / 2PACz / perovskite layers is not heated,
[0133] - deposit a buffer layer 20,
[0134] - forming an upper electrode 10 in silver by thermal evaporation under vacuum (1.10-6 mbar) with a deposition rate of 0.2 to 2 Å / s; during deposition the stack of glass / ITO / 2PACz / perovskite / C60 / buffer layers is not heated.
[0135] When the buffer layer is made of PCB, the deposition of the buffer layer is carried out by thermal evaporation under vacuum (for example at 1.106 mbar). The deposition speed is between 0.1 and 0.4 Å / s. During the deposition the stack of glass / ITO / 2PACz / perovskite / C6o was not heated.
[0136] When the buffer layer 20 is made of alumina, the buffer layer is deposited by ALD from the following two precursors: trimethylaluminium A12(CH3)6 (TMA) and water (H2O).
[0137] The precursors are introduced into the deposition chamber sequentially (i.e. one after the other). An inert gas (N2) purge is carried out after the injection of each precursor so that the precursors react only with the surface of the material and not with each other.
[0138] By way of illustration, to deposit a 3.6 nm alumina layer 20 at a temperature of 50°C on the n-type layer, the method may comprise the following steps: a. preheating the deposition chamber to 50°C b. introduction of the samples into the deposition chamber c. adjustment and maintenance of the temperature and pressure (for example 0.7 mbar, or 70 Pa), d. deposition by ALD by carrying out the cycle comprising the following sub-steps:
[0139] - Insertion of the TMA gas into the deposition chamber; the duration of the pulse and the flow of TMA are 500 ms and 300 sccm respectively,
[0140] - insertion of N2 into the chamber to purge the chamber; the duration of the pulse and the flow of N2 are 5 s and 300 sccm respectively,
[0141] - inertion of the H2O gas in the deposition chamber; the duration of the pulse and the flow of H2O are 500 ms and 300 sccm respectively,
[0142] - insertion of N2 into the chamber; the duration of the pulse and the flow of N2 is 6 s and 300 sccm respectively.
[0143] The cycle is repeated until the desired thickness is achieved.
[0144] Then, an N2 purge is carried out before venting the chamber and removing the samples. The chamber temperature returns to room temperature (between 20 and 25°C).
[0145] The total duration of the procedure is 30 minutes.
[0146] Optimization of the thickness of the alumina buffer layer 20 and the temperature used during the deposition of the alumina buffer layer 20
[0147] Different thicknesses of AIOx buffer layer (from 0.6 nm to 5 nm) were tested. Figures 2A, 2B, 2C and 2D are graphs illustrating the photovoltaic parameters for each thickness and compare the results obtained with a reference cell comprising a BCP buffer layer.
[0148] The best photovoltaic cells were obtained for an AIOx buffer layer with a thickness of 3.6 nm.
[0149] Figures 3A, 3B, 3C and 3D are graphs showing the photovoltaic properties of photovoltaic cells with AlOx buffer layers deposited at different temperatures (50°C, 75°C, 100°C). The optimal temperature is 50°C. The results obtained are compared with a photovoltaic cell having a BCP buffer layer.
[0150] In addition, JV (current-voltage density) measurements as a function of the applied voltage sweep direction (upward and downward) are illustrated in [Fig.4]. The AIOx buffer layer does not lead to hysteresis problems.
[0151] These figures clearly show that it is possible to replace the BCP buffer layer with an alumina buffer layer. The photovoltaic efficiency of the cells with the alumina buffer layer is good.
[0152] A very low dispersion of the values (Voc, FF, Jsc, PCE) is observed.
[0153] The optimal conditions for the deposition of the AIOx buffer layer are: a tem temperature of 50°C during the deposition of the alumina layer and a deposited thickness between 3 and 3.6 nm (inclusive). Such thicknesses are obtained by repeating the ALD deposition cycle between 30 and 36 times.
[0154] Study on the stability of the photovoltaic cell using an alumina buffer layer 20
[0155] [Fig.5] shows the surface of a photovoltaic cell having a BCP buffer layer one week after device preparation and 2.5 months (75 days) after storage of the cell under N2, as well as the surface of a photovoltaic cell having an alumina buffer layer 2.5 months (75 days) after storage of the cell under N2. The use of AIOx as a buffer layer protects the Ag electrode by blocking the diffusion of iodine from the perovskite to the electrode. The AIOx buffer layer forms a better diffusion barrier to iodine than the BCP buffer layer.
[0156] To study the stability of photovoltaic cells under illumination, the photovoltaic cells were placed under N2 and in a transparent sealed bag to avoid humidity and O2 penetration. Then they were illuminated for 72 hours continuously.
[0157] The following table shows the photovoltaic parameters of the photovoltaic cell with the AIOx buffer layer and with the BCP buffer layer before and after 72 hours of exposure to light. These results were obtained after storing the cells under N2 for 2.5 months. The decrease in PCE is very low using the AIOx buffer layer: the efficiency (PCE) corresponds to 92.4% of the initial value, i.e. before aging under illumination. It is better than that of a cell with a BCP buffer layer.
[0158] [Tables 1] Condition Time of measurement Voc (mV) Jsc (mA / cm2) FF (%) PCE (%) With BCP before storage 1086 18.9 57.4 11.8 With AIOx before storage 1149 19.5 71.4 16.0 With BCP After 2.5 months of storage 976 18.4 57.4 10.3 With BCP After 2.5 months of storage 1136 14.8 47.4 7.9 With AIOx After 2.5 months of storage and 72 hours of illumination 1155 19.5 75.8 17.0 With AIOx After 2.5 months of storage and 72 hours of illumination 1098 18.9 75.9 15.7
[0159] Cells with alumina buffer layer 20 show good stability to illumination.
Claims
Claims
1. Photovoltaic cell based on pin-type perovskite comprising successively, from the rear face to the front face, at least: - an alumina buffer layer (20), having a thickness between 1 nm and 5 nm, - an n-type layer (30), - an active layer (40) made of perovskite of formula APbX3 with A representing methylammonium, dimethylammonium, formamidinium, guanidinium and / or cesium cations and X representing halide anions.
2. Photovoltaic cell according to claim 1, characterized in that the alumina buffer layer (20) has a thickness of between 3 and 4
3. llili. Photovoltaic cell according to one of the preceding claims, characterized in that the n-type layer (30) is a C60, PC6i BM, PC71BM, PCBM / C60 or PCBM / C layer.
4. Photovoltaic cell according to one of the preceding claims, characterized in that the cell comprises successively from the rear face to the front face: - an upper electrode (10), for example made of silver, - the alumina buffer layer (20), - the n-type layer (30), for example made of C60, - the active layer (40) made of perovskite of formula APbX3, for example made of (FAo.83Cso.i7)Pb(Io.6Bro.4)3, - a p-type layer (50), for example made of PACz, - a transparent conductive oxide layer (60), for example made of indium-tin oxide, - a substrate (70), for example made of glass.
5. A method of manufacturing a photovoltaic cell as defined in any one of the preceding claims, characterized in that the method comprises a step during which the alumina buffer layer (20) is formed by a step of depositing atomic layers on the n-type layer (30).
6. Method according to the preceding claim, characterized in that the temperature during the formation of the alumina buffer layer (20) is between 25°C and 100°C, preferably between 40°C and 75°C.
7. Method according to one of claims 6 and 7, characterized in that the alumina buffer layer (20) is formed, in a deposition chamber, by carrying out one or more times a cycle comprising the following sub-steps: - injecting an aluminum precursor into the deposition chamber, then purging the deposition chamber, - injecting an oxygen precursor into the deposition chamber, then purging the deposition chamber.
8. Method according to claim 7, characterized in that the precursor of aluminum is TMA and the precursor of oxygen is water.
9. Method according to one of claims 7 and 8, characterized in that the cycle is carried out between 10 and 50 times, preferably between 30 and 40 times.
10. Method according to one of claims 7 to 9, characterized in that the temperature during the formation of the alumina buffer layer (20) is between 45°C and 55°C and in that the cycle is carried out between 30 and 40 times.