Improved method for manufacturing a metal annular part

By reversing material removal steps and optionally expanding the blank, the method addresses geometric defects in large diameter annular parts, improving circularity and reducing scrap rates, ensuring compliance with tight tolerances.

FR3148731A1Active Publication Date: 2024-11-22SAFRAN AIRCRAFT ENGINES SAS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
FR2023004865
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

Manufacturing large diameter annular metal parts, such as shrouds for turbomachine modules, often results in geometric defects due to residual stresses from heat treatments, leading to non-conformities and high scrap rates, particularly at shrink-fit interfaces where tight tolerances are required.

Method used

Reversing the material removal steps by initially forming orifices and grooves in the blank, followed by adjustment turning to achieve desired dimensions, and optionally incorporating an expansion step to redistribute stresses, thereby reducing residual stress release during machining.

Benefits of technology

Significantly reduces geometric defects and improves circularity, lowering scrap rates from 90% to 10% and ensuring compliance with tight tolerance intervals by enhancing the quality of the final parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Improved method for manufacturing a metal annular part. Method for manufacturing a metal annular part (10) comprising at least one diameter (De) having a predetermined value, the method comprising a forging step (S110) in which a rough blank of the annular part (10) is produced, at least one heat treatment step (S120, S130), a machining step (S200) comprising, on the one hand, the fit turning (S220') of the blank to adjust the diameter (De) of the blank to the predetermined value of the part to be manufactured, and on the other hand, the material removal (S210') of the blank in which at least 50% of the mass of the rough blank is removed and comprising at least the drilling of holes (14) and / or a groove (17, 19) in the rough blank, the material removal (S210') of the roughing being done before the adjustment turning (S220'). Figure for the abbreviation: Fig. 5.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Improved method of manufacturing a metallic annular part Technical field

[0001] The present disclosure relates to the field of industrial production, in particular the forging and machining of aeronautical parts. More specifically, the present disclosure relates to a method for manufacturing an annular part, for aeronautical engines but not only. Prior art

[0002] In the field of industrial production, the manufacture of metal parts comprises, in a known manner, a forging range and a machining range, these ranges generally coming from different and independent sources (blacksmith source and machinist source).

[0003] When forging the part, a metal block, or blank roughly having the shape of the final part to be produced, is manufactured using a high temperature furnace (between 900 and 1000°C), to shape the blank. The heated and shaped blank is then quenched in a cooling liquid in order to freeze the shape and obtain the desired metallurgy. One or more heat treatments may also be carried out.

[0004] The rough blank thus obtained is then machined in order to obtain the final part with the desired dimensions and dimensions. During machining, part of the material forming the rough blank is removed by turning the part in order to adjust the dimensions of the part (diameters, dimensions, etc.) to the desired values. The so-called three-dimensional (“3D”) parts of the part, in particular holes, grooves or scallops where applicable, are also produced, for example by milling.

[0005] However, during the manufacture of a large diameter annular part, for example greater than 50 cm, by means of the machining described above, geometric defects in the final part may appear. This is for example the case for the shells allowing the coupling of two turbomachine modules, for example the high pressure turbine and the low pressure turbine. Such shells involve tight tolerances, with a tolerance interval for example of 0.05 mm maximum, in particular at the level of the hooping interfaces between the shell and the turbomachine modules that it assembles. Failure to comply with this tolerance interval leads to defects in the final assembly, or even the scrapping of the manufactured shells.

[0006] However, these large diameter ferrules, for example approximately 1 m, have the characteristic of being flexible, given their dimensions and their material, gener- normally a refractory metal alloy such as a Waspaloy® type nickel alloy, for example. However, the processes described above (forging and machining) for manufacturing this ferrule frequently lead to geometric defects in the final part, making it impossible to respect the aforementioned tolerance intervals.

[0007] These defects may in particular be due to residual stresses remaining in the blank following heat treatments, in particular quenching, carried out after forging, and released during machining. These defects concern the circularity and the average diameter of the ferrule at the level of the shrink-fit interfaces. In other words, these parts are often produced with a defect in ovalization and sagging of the diameters, leading to possible non-conformities during assembly and a high reject rate.

[0008] There is therefore a need to at least partially overcome the aforementioned drawbacks. Statement of the invention

[0009] The present disclosure relates to a method of manufacturing a metallic annular part comprising at least one diameter having a predetermined value, the method comprising: - a forging step in which a rough blank of the annular part is manufactured, - at least one heat treatment step, - a machining step comprising on the one hand the adjustment turning of the blank to adjust the diameter of the blank to the predetermined value of the part to be manufactured, and on the other hand the removal of material from the blank in which at least 50% of the mass of the raw blank is removed and comprising at least the drilling of orifices and / or a groove in the raw blank, the removal of material from the blank being carried out before the adjustment turning.

[0010] It is understood that the part to be manufactured is annular, for example a ring, and therefore necessarily comprises at least one diameter, for example at least one internal diameter and one external diameter relative to the radial direction of the part, the part being able in particular to have a symmetry of revolution. However, the annular part may have a more complex shape than a ring, and comprise one or more flange(s), grooves or shoulders. Such a more complex geometry involves several internal and external diameters.

[0011] Furthermore, the term “predetermined diameter value” means the diameter value that the annular part must respect at the end of the manufacturing process to comply with the quality requirements, subject to a tolerance interval that is also predefined.

[0012] It is further understood that the rough blank is a rough annular metal block obtained at the end of the forging stage, for example a ring, roughly presenting the shape and dimensions of the final part, before the finishing stages by machining.

[0013] For this purpose, in a manner known per se, the rough blank is usually machined by turning in a first step. For this, the blank is rotated so as to machine its internal diameter and / or its external diameter, in order to adjust these diameters to the desired dimensions, that is to say to the predetermined dimensions. Once this step is completed, the blank is then usually machined, in particular by milling, so as to produce the so-called "3D" parts, in particular the orifices and / or the grooves.

[0014] This manufacturing method comprising these different stages carried out in this order constitutes the usual practices encountered in industrial production, and is based on the optimization of the implementation of manufacturing, to reduce the number of stages and costs.

[0015] However, the inventors have observed, through experiments and simulations carried out at each stage of the process, a significant release of the residual stresses present in the blank at the end of the heat treatment, at the time of removal of material from the blank, in particular drilling and milling of orifices, usually constituting the last stage of the machining operation and therefore the finishing of the part. The deformation of the part, resulting in an irregularity in its circularity, therefore takes place to a significant extent during milling.

[0016] Conversely, the inventors have found, surprisingly, that by removing a maximum amount of material, in particular at least 50% of the mass of the blank and by producing in particular the orifices and / or grooves in a first step, then by producing in a second step the geometries of revolution (diameters, faces) to adjust the part to the desired dimensions by the adjustment turning step usually carried out first, the defects observed in the resulting part decreased significantly.

[0017] Thus, reversing the material removal step, in which a significant amount of material is removed and at least holes and / or grooves are formed in the blank initially, and the adjustment turning step in which at least one diameter of the blank is adjusted to the predetermined value of the part to be manufactured, makes it possible to considerably improve the circularity of the annular part thus manufactured, consequently reducing the scrap rate. In particular, this solution, although contrary to the cutting strategies traditionally employed, makes it possible to go from a scrap rate of approximately 90% to 10%.

[0018] In certain embodiments, when removing material from the rough workpiece, at least 90% of an initial mass of the rough workpiece is removed. This makes it possible to remove a maximum amount of material at the start of machining, and thus to limit as much as possible the effects release of residual stresses during the adjustment turning step.

[0019] In some embodiments, the removal of material comprises forming scallops to be distributed circumferentially along an outer face of the annular part.

[0020] The festoons may be notches, or crenellations distributed circumferentially around the annular part, preferably pierced with an orifice allowing the part, for example a ferrule, to be fixed to another part, for example a turbine module. The inventors have found that the machining of festoons was responsible for a significant part of the stress releases, and therefore of deformations in the final part. Consequently, carrying out the removal of material, including the formation of festoons, before the adjustment and finishing turning of the part, makes it possible to further improve the quality of the part obtained.

[0021] In certain embodiments, the diameter of the annular part is greater than or equal to 50 cm. It is understood that the larger the diameter of the annular part, the more flexible and relatively thin it is, and consequently exposed to deformations. Consequently, this solution applied to parts with a large diameter, greater than or equal to 50 cm, makes it possible to significantly improve the circularity, and therefore the quality of the part obtained.

[0022] In some embodiments, the method comprises, after the step of forging the raw blank, then heat treating the raw blank by quenching in a cooling liquid, an expansion step, during which a diameter of the raw blank is increased relative to its initial diameter after quenching.

[0023] The inventors have found that, in particular on flexible annular parts of large diameter (> 50 cm) and in particular in nickel alloy which only allows rapid quenching freezing strong stress gradients, the detention heat treatments usually carried out do not allow a return to a situation without residual stresses.

[0024] Conversely, the inventors have found that stretching the raw blank by increasing its initial diameter, for example its initial internal diameter, during the expansion step after quenching, makes it possible to redistribute the stresses within the raw blank. Indeed, increasing the initial diameter of the blank causes plasticization to standardize the stresses within the blank, and therefore to reduce the significant local stress concentrations. This expansion step thus makes it possible, in addition to reversing the steps described above during machining, to further improve the circularity and quality of the annular parts obtained.

[0025] In some embodiments, during the expansion step, the diameter of the raw blank is increased by a value between 0.1% and 0.8% of its initial diameter.

[0026] These values ​​of expansion of the diameter, for example of the internal diameter of the raw blank, are sufficient to considerably reduce the residual stresses, and improve the quality of the parts obtained.

[0027] In some embodiments, the expanding step is performed by means of a jack pushing the rough blank radially outward so as to expand said rough blank.

[0028] It is for example possible to use a jack with pads arranged against the radially internal face of the annular part at several equidistant locations along this face, thus uniformly pushing the annular part outwards so as to stretch and widen it, and thus significantly increase the diameter of the annular part.

[0029] In certain embodiments, the annular part is a ferrule allowing the coupling of two aeronautical engine modules. The aeronautical engine modules can be the high and low pressure turbines of the engine for example. The tolerance intervals for such a ferrule being very tight, the implementation of a method according to the present disclosure is consequently particularly advantageous, in that it makes it possible more effectively to comply with these tolerance intervals by significantly improving the circularity and therefore the quality of the parts. Brief description of the drawings

[0030] The invention and its advantages will be better understood upon reading the detailed description given below of different embodiments of the invention given as non-limiting examples. This description refers to the appended pages of figures, in which:

[0031] [Fig-1] [Fig.l] represents a perspective view of an annular ferrule coupling manufactured by a method according to the present disclosure;

[0032] [Fig.2] [Fig.2] represents a section of the ferrule of [Fig.l] in a plane parallel to the central axis of the shell;

[0033] [Fig.3] [Fig.3] is a diagram schematically representing the different steps of a method of manufacturing an annular part according to the prior art;

[0034] [Fig.4] [Fig.4] is a graph showing the evolution of the number of pieces an nulars manufactured by the process of [Fig.3], depending on the deviations between a diameter measured on these samples and the theoretical predetermined value of this diameter;

[0035] [Fig.5] [Fig.5] is a diagram schematically representing the different steps of a method of manufacturing an annular part according to a first embodiment of the present disclosure;

[0036] [Fig.6] [Fig.6] is a graph (full on the left, and detailed on the right) representing the evolution of the number of annular parts manufactured by the process of [Fig.5], as a function of the deviations between a diameter measured on these samples and the theoretical predetermined value of this diameter;

[0037] [Fig.7] [Fig.7] is a diagram schematically representing the different steps of a method of manufacturing an annular part according to a second embodiment of the present disclosure;

[0038] [Fig.8] [Fig.8] is a graph (full on the left, and detailed on the right) representing the evolution of the number of annular parts manufactured by the process of [Fig.7], as a function of the deviations between a diameter measured on these samples and the theoretical predetermined value of this diameter. Description of the embodiments

[0039] In the remainder of the description, a method of manufacturing a coupling ferrule 10 for two aeronautical engine modules (not shown) will be described with reference to FIGS. 1 to 8. The invention is however not limited to the manufacture of such a ferrule, but can be applied to any flexible metal annular parts having a diameter greater than or equal to 50 cm.

[0040] Such a ferrule 10, shown in perspective in [Fig.l], measures for example 1 m in internal diameter, and comprises a refractory nickel alloy, for example Waspaloy®. The ferrule 10 extends around an axial direction X, corresponding to the center of the ferrule 10, a radial direction R of the ferrule 10 being perpendicular to the axial direction X. The terms “internal”, “external” and their derivatives are therefore considered according to this radial direction R, “internal” being understood as closer to the axis X, and “external” being understood as further from the axis X.

[0041] The ferrule 10 comprises a plurality of festoons 12, that is to say notches distributed circumferentially around the ferrule 10, along its radially external face. These festoons 12 are each crossed by an orifice 14. The ferrule 10 also has a complex shape, clearly visible in the section shown in [Fig.2].

[0042] The ferrule 10 comprises in particular, on a first axial face, a first annular flange 15, and a first annular groove 17. On a second axial face, the ferrule 10 comprises in particular a shoulder 18 and a second annular groove 19. A second annular flange 16 is further formed at the radially internal end of the ferrule.

[0043] Each of these geometric structures that the ferrule 10 comprises involves dimensions that must respect predetermined values. In particular, the internal and external diameters of these different portions, in particular of the first annular flange 15 constituting a hooping interface with an aeronautical module, must have predetermined values, which must respect a restricted tolerance interval.

[0044] The following example concerns the external diameter De of the first annular flange 15 (hereinafter referred to more simply as “flange 15”). However, the description could also apply to other portions of the part. It is understood that the external diameter De is the distance between the axis X and the external surface of the first annular flange 15, identified by the dotted line in [Fig.2].

[0045] [Fig. 3] is a diagram representing the different steps of a method for manufacturing such a ferrule 10 according to the prior art. Such a method comprises, firstly, a manufacturing step (step S100) in which a rough blank of the part is manufactured by forging, and secondly, a machining step (step S200), in which the rough blank obtained in step S100 is machined so as to obtain the desired shape and dimensions of the ferrule 10.

[0046] Manufacturing step S100 comprises forging comprising firstly the shaping of a raw metal block in which, in a manner known per se, the block is placed in a furnace at 900-1000°C, then a significant force is applied to the hot block to give it the desired shape (step S110). The block thus shaped is again placed in the furnace at approximately 1000°C and is then quenched in a cooling liquid (step S120), which may be water, oil, or a polymer liquid. During this step, due to the high cooling speed, quenching sets significant stress gradients within the part. In particular, the edges of the metal block cool faster than the core, resulting in strong stress gradients. An additional de-stressing heat treatment is then carried out to attempt to reduce these residual stresses (step S130).

[0047] Such a detention heat treatment may comprise, in a manner known per se, tempering treatments, in particular by subjecting the part for 4 hours to a temperature of 850°C±10 and for 16 hours to 760°C±10, allowing the part to cool in the open air.

[0048] At the end of the manufacturing step S100 including forging and heat treatments, a rough blank of the ferrule is obtained. This rough blank has, for example, the shape of a metal ring of rectangular section. During the machining step S200, this metal blank is initially placed on a tool allowing it to be rotated, so as to adjust the diameters, in particular the external diameter De, to the predetermined values ​​(adjustment turning step S210).

[0049] Once the diameters have been adjusted to the desired dimensions, the blank is then machined so as to form the highly 3D parts of the ferrule 10, in particular the grooves 17, 19, the orifices 14 and the festoons 12 (material removal step S220), by through a strawberry for example.

[0050] [Fig. 4] is a graph showing the distribution of the measurement results of the diameter De, at a given location, on 67 samples, and in particular the deviation E in mm (millimeters) between the measured diameter De and the predetermined value that this diameter De must respect, for example 958.1 mm. The interval I between the two dotted lines represents the tolerance interval that the diameter De must respect at the end of the manufacturing process described above, this interval I being 0.05 mm. The solid line curve represents the average variations in the number of samples as a function of the deviation E.

[0051] The graph in [Fig.4] shows a significant number of samples with different deviations E, indicating a significant dispersion of the measured diameter values ​​De, and therefore a non-repeatability of the results obtained by this method, and further shows that the vast majority of the measured deviations E are beyond the tolerance interval I.

[0052] [Fig. 5] is a diagram representing the different steps of a method for manufacturing a ferrule 10 according to a first embodiment of the present disclosure. The manufacturing step S100 in this first embodiment is identical to the step S100 of the method according to the prior art. On the other hand, the machining step S200 differs from the step S200 of the method according to the prior art in that the steps S210 and S220 are reversed.

[0053] More precisely, during the machining step S200, the metal blank is firstly machined so as to form the highly 3D parts of the ferrule 10, in particular the grooves 17, 19, the orifices 14 and the festoons 12 (material removal step S210'), and so as to remove a large part of the mass of the blank, in particular at least 50% of its mass, preferably at least 90%.

[0054] Then, the metal blank is placed on a tool allowing it to be rotated, so as to adjust the diameters, in particular the external diameter De, to the predetermined values ​​(adjustment turning step S220'). Thus, step S210' constitutes a roughing of the part in which the majority of the mass of the blank is removed and making it possible to obtain a ferrule 10 having overall the desired final shape, including in particular the orifices 14, festoons 12 and grooves 17, 19, and step S220' constitutes a finishing step in which the diameters are adjusted by a suitable tool.

[0055] It will be noted that the step S210' of removing material may also comprise turning of the blank, the latter however constituting a roughing turning (in addition to the milling of orifices and / or grooves) making it possible to remove material to approach the final shape and dimensions of the ferrule 10, but which is different from the adjustment turning (step S220'), making it possible to adjust the diameters with the precise desired and predetermined dimensions.

[0056] [Fig.6] is a graph showing the distribution of the measurement results of the diameter De, at a given location, on 18 samples, in particular of the deviation E in mm (millimeters) between the measured diameter De and the predetermined value of this diameter. In particular, the graph on the right represents that on the left in more detail, the abscissa scale being enlarged.

[0057] The graph in [Fig. 6] shows a lower dispersion of the measured diameter values ​​De compared to the result of the method according to the prior art ([Fig. 4]) showing better repeatability of the results, and shows a larger proportion of the measured deviations E below the tolerance interval I of 0.05 mm. It will also be noted that the inversion of steps S210 and S220 makes it possible to obtain a rate of ferrules having, after the machining step S200, a circularity conforming to the quality requirements, of 64.5%, compared to 1% in the absence of such an inversion with the method according to the prior art. Thus, the fact of releasing a large proportion of the residual stresses by carrying out the step S210' of material removal and roughing in a first step, before the finishing step of adjusting the diameters, makes it possible to improve the circularity of the ferrules 10.

[0058] [Fig. 7] is a diagram representing the different steps of a method for manufacturing a ferrule 10 according to a second embodiment of the present disclosure. The machining step S200 in this second embodiment is identical to the step S200 of the method according to the first embodiment. On the other hand, the manufacturing step S100 differs from the step S100 of the method according to the prior art and according to the first embodiment in that it comprises, after the step S120 of quenching the raw blank in a cooling liquid, an expansion step S140, during which an initial diameter of the raw blank after the quenching step S120 is increased.

[0059] Thus, according to this second embodiment, the method comprises on the one hand the expansion step S140 during the manufacture of the blank, and on the other hand the fact of carrying out the step of removing material S210' from the blank before the adjustment turning step S220'.

[0060] The expansion step S140 is carried out by means of a jack (not shown), for example a jack with pads arranged against the radially internal face of the annular blank at several equidistant locations along this face, thus uniformly pushing the blank outwards so as to stretch and widen it, and thus substantially increase the diameter of the annular part. The internal diameter of the raw blank can be increased by a value between 0.1% and 0.8% of its initial diameter, for example by 0.71%.

[0061] [Fig.8] is a graph showing the distribution of measurement results of the diameter De, at a given location, on 18 samples, in particular the deviation E in mm (millimeter) between the measured diameter De and the predetermined value of this diameter. In particular, the graph on the right represents that on the left in more detail, the abscissa scale being enlarged.

[0062] The graph in [Fig. 8] indicates a lower dispersion of the measured diameter values ​​De compared to the result of the method according to the prior art ([Fig. 4]) and according to the first embodiment ([Fig. 6]) and shows an even greater proportion of the measured deviations E below the tolerance interval I of 0.05 mm, all of the samples tested respecting this interval in this example. It will also be noted that the addition of step S140, in addition to the inversion of steps S210 and S220, makes it possible to obtain a rate of ferrules having, after the machining step S200, a circularity conforming to the quality requirements of 96%.

[0063] Furthermore, a detention heat treatment step S150 can be carried out after the expansion step S140, the step S150 being identical to the step S130 described previously with reference to the method according to the prior art.

[0064] Although the present invention has been described with reference to specific exemplary embodiments, it is obvious that modifications and changes may be made to these examples without departing from the general scope of the invention as defined by the claims. In particular, individual features of the various illustrated / mentioned embodiments may be combined in additional embodiments. Therefore, the description and drawings should be considered in an illustrative rather than restrictive sense.

Claims

Claims

1. A method of manufacturing a metal annular part (10) comprising at least one diameter (De) having a predetermined value, the method comprising: - a forging step (S1 10) in which a rough blank of the annular part (10) is manufactured, - at least one heat treatment step (S120, S130), - a machining step (S200) comprising on the one hand the adjustment turning (S220') of the blank to adjust the diameter (De) of the blank to the predetermined value of the part to be manufactured, and on the other hand the removal of material (S210') of the blank in which at least 50% of the mass of the rough blank is removed and comprising at least the drilling of orifices (14) and / or a groove (17, 19) in the rough blank, the removal of material (S210') of the roughing being carried out before the adjustment turning (S220').

2. The method of claim 1, wherein, when removing material (S210') from the blank, at least 90% of an initial mass of the raw blank is removed.

3. A method according to claim 1 or 2, wherein the removal of material (S210') comprises the formation of festoons (12) intended to be distributed circumferentially along an external face of the annular part (10).

4. A method according to any one of claims 1 to 3, wherein the diameter of the annular part (10) is greater than or equal to 50 cm.

5. A method according to any one of claims 1 to 4, comprising, after the step of forging (S110) the rough blank and then heat treating (S120) the rough blank by quenching in a cooling liquid, an expansion step (S140), during which a diameter of the rough blank is increased relative to its initial diameter after quenching.

6. The method of claim 5, wherein, in the expansion step (S140), the diameter of the raw blank is increased by a value between 0.1% and 0.8% of its initial diameter.

7. A method according to claim 5 or 6, wherein the expanding step (S140) is performed by means of a jack pushing the rough blank radially outward so as to expand said rough blank.

8. Method according to any one of claims 1 to 7, in which the annular part (10) is a ferrule allowing the coupling of two aeronautical engine modules.

Citation Information

Patent Citations

  • A thin-walled inner ring component of a stator and its processing method

    CN107931997B

  • Preparation method of thin-wall part

    CN113059318A

  • Method for reinforcing mechanical characteristics of wall delimiting bore of disk of turbojet engine by plasticization, involves retracting rod from outlet position toward inserted position in actuator such that tool traverses disk bore

    FR2956601A1