Active materials based on lithium manganese and iron phosphate and lithium-ion electrochemical element electrode comprising said active materials
By synthesizing LMFP particles with almost spherical shape and low internal porosity, the electrode porosity is reduced from 40 to 50% to 20 to 30%, thereby enhancing the volume capacity of lithium-ion electrodes.
Patent Information
- Application Number
- FR2023004797
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-15
AI Technical Summary
Existing lithium manganese iron phosphate (LMFP) electrodes have high porosity due to their flaky or granular shape, leading to insufficient volume capacity, with porosities ranging from 40 to 50%, which limits the effective utilization of the electrode material.
The development of LMFP particles with an almost spherical shape and internal porosity less than or equal to 5%, achieved through specific synthesis methods, ensures low electrode porosity ranging from 20 to 30% by using sphericity factors greater than 0.9, preferably 0.95 or higher, and controlled agglomeration of primary particles.
The low porosity LMFP particles significantly enhance the volume capacity of the electrode, allowing for a 40 to 50% increase in volume capacity compared to traditional LMFP electrodes.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Active materials based on lithium manganese and iron phosphate and lithium-ion electrochemical element electrode comprising said active materials Technical field of the invention
[0001] The technical field of the present invention is that of active materials based on lithium manganese and iron phosphate (LMFP) intended to be used in the cathode, that is to say the positive electrode, of an electrochemical element of the lithium-ion type, also called a lithium-ion element. Background to the invention
[0002] Lithium manganese and iron phosphates, abbreviated LMFP in the following, are known as active material in the positive electrode of lithium-ion electrochemical elements. These phosphates have satisfactory thermal stability but insufficient volume capacity. This is partly due to the difficulty of obtaining a low porosity electrode. The available LMFP particles have a flaky or granular shape with irregular contours. However, this particular shape makes it difficult to obtain a positive electrode with low porosity, and therefore with a high volume capacity. Typically, a positive electrode based on LMFP has a porosity ranging from 40 to 50%. Approximately half of the volume of the electrode is therefore made up of empty space. It has therefore been sought to increase the volume capacity of an electrode comprising an active material based on LMFP.
[0003] Document CN 113072049 (A) describes for example a method for preparing LMFP nanoparticles of spherical shape. The value of the internal porosity of the particles produced is not mentioned. No density value of the particles produced is indicated.
[0004] Document CN 1821065 (A) describes a process for preparing spherical lithium iron phosphate LiFePO4 (LFP) particles. The density values obtained range from 2.0 to 2.3 g / cm3. However, the theoretical density of LiFePO4 is 3.6 g / cm3. As a result, the porosity of the LiFePO4 powder produced under the process conditions described in this document is approximately 40%, which remains high.
[0005] Document CN 1632970 (A) describes a process for preparing spherical LFP or LMFP particles. Examples 4 to 7 of this document describe the preparation of a powder of LMFP particles with a size ranging from 8 to 10 pm and having a density of 2.08-2.20 g / cm3. However, the average theoretical density of LMFP is 3.3 g / cm3. As a result, the porosity of the LMFP powder produced under the conditions of this process is about 36%, which remains high.
[0006] The aim is to obtain a powder porosity of less than or equal to 30%, which guarantees obtaining an electrode porosity of 30% by applying reasonable pressure forces. Summary of the invention
[0007] The subject of the present invention is an electrode comprising one or more active materials, one of which is a lithium manganese and iron phosphate of formula LixMni y zFeyMzPO4 (LMFP) where 0.8 <x<l,2 ; 0,5<l-y-z<l ; 0<y<0,5 ; 0 <z<0,2 ; M being one or more elements selected from the group consisting of Al, B, Mg, Si, Ca, Ti, V, Cr, Co, Cu, Ni, Zn, Y, Zr, Nb, W and Mo, the electrode being characterized in that: - the lithium manganese and iron phosphate is in the form of particles, at least 90% by number of the particles have a sphericity factor greater than or equal to 0.90 and less than 1, the sphericity factor of a particle being defined as the ratio between the surface area of a sphere having the same volume as the particle and the surface area of this particle, and in that - the internal porosity of the lithium manganese and iron phosphate particles is less than or equal to 5%, the internal porosity being defined by the ratio Vvide / VLMFpOÙ Vvoid represents the void volume inside the lithium manganese and iron phosphate particles, VLMFP represents the geometric volume of lithium manganese iron phosphate particles.
[0008] The invention is based on the discovery that the use of LMFP particles having on the one hand a quasi-spherical shape and on the other hand an internal porosity of less than or equal to 5% makes it possible to reduce the porosity of the electrode. Low electrode porosity values ranging from 20 to 30% are achievable.
[0009] According to one embodiment, the sphericity factor is greater than or equal to 0.95.
[0010] According to one embodiment, the sphericity factor is greater than or equal to 0.98.
[0011] According to one embodiment, the internal porosity of the lithiated phosphate particles of manganese and iron range from 2 to 3%.
[0012] According to one embodiment, at least 95% by number of the particles of lithium manganese and iron phosphate have a sphericity factor greater than or equal to 0.9 and less than 1.
[0013] According to one embodiment, the particles of lithium manganese and iron phosphate are in the form of primary particles having a median diameter in volume Dv50 ranging from 500 nm to 20 pm or from 5 to 15 pm or from 1.5 to 4 pm.
[0014] According to one embodiment, the lithium manganese and iron phosphate particles are in the form of secondary particles having a volume median diameter Dv50 ranging from 1 μm to 50 μm, a secondary particle being made up of the agglomeration of primary particles having a volume median diameter Dv50 located in the range from 50 nm to 20 μm.
[0015] According to one embodiment, the lithium manganese and iron phosphate particles have a bimodal distribution, the first population being characterized by a first median diameter Dyso1, the second population being characterized by a second median diameter DV5o2, the ratio between Dyso1 and Dv5o2 ranging from 3 to 10.
[0016] According to one embodiment, in the lithium manganese and iron phosphate, 0.70 <l-y-z<l.
[0017] According to one embodiment, the electrode further comprises one or more active materials chosen from: - a lithium iron phosphate of formula iii) LixFei yMyPO4 (LFP) where 0.8 <x<l,2 ; 0<y<0,6 et M est choisi dans le groupe consistant en B, Mg, Al, Si, Ca, Ti, V, Cr, Co, Cu, Zn, Y, Zr, Nb et Mo ; - a lithium vanadium fluorophosphate of formula iv) Lii+XVPO4F (LVPF) where 0 <x<0,15, ou à un de ses dérivés de formule v) Lii+xVi yMyPO4Fz (LVMPF) où 0<x<0,15, 0<y<0,5, 0,8<z<l,2 et M est choisi dans le groupe consistant en Ti, Al, Y, Cr, Cu, Mg, Mn, Fe, Co, Ni, et Zr ; - a lithium oxide of nickel, manganese and cobalt of formula a) Liw(NixMnyCozMt)O2(NMC) where 0.9 <w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci, - a lithium oxide of nickel, cobalt and aluminum of formula b) Liw(NixCoyAlzMt)O2(NCA) where 0.9 <w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de B, Mg, Si, Ca, Ti, V, Cr, Mn, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, Sr, Ce, Ga, Ta, Nd, Pr, La et des mélanges de ceux-ci, - a lithium oxide of nickel and manganese of formula c) Liw(NixMnyCozMt)O2(NMX) where 0.9 <w<l,l ; 0,60<x<0,80 ; 0<y ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci, - un oxyde lithié de nickel et de manganèse de formule d) Liw(NixMnyCozMt)O2where 1.1 <w<1,6 ; 0<x ; 0,50<y<0,80 ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci.
[0018] According to one embodiment, said one or more active materials is an oxide lithium nickel chosen from: - a lithium oxide of nickel, manganese and cobalt of formula a) Liw(NixMnyCozMt)O2(NMC) where 0.9 <w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci, - un oxyde lithié de nickel, de cobalt et d’aluminium de formule b) Liw(NixCoyAlzMt)O2(NCA) où 0,9<w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de B, Mg, Si, Ca, Ti, V, Cr, Mn, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, Sr, Ce, Ga, Ta, Nd, Pr, La et des mélanges de ceux-ci, et - a lithium oxide of nickel and manganese of formula c) Liw(NixMnyCozMt)O2(NMX) where 0.9 <w<l,l ; 0,60<x<0,80 ; 0<y ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci, - un oxyde lithié de nickel et de manganèse de formule d) Liw(NixMnyCozMt)O2 where 1.1 <w<1,6 ; 0<x ; 0,50<y<0,80 ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci.
[0019] According to one embodiment, the lithium manganese and iron phosphate represents from 40 to 99% by mass of the total mass of lithium manganese and iron phosphate and lithium nickel oxide(s) and said one or more lithium nickel oxides represents from 1 to 60% by mass of the total mass of lithium manganese and iron phosphate and lithium nickel oxide(s).
[0020] According to one embodiment, the lithium manganese and iron phosphate represents from 70 to 99% by mass of the total mass of lithium manganese and iron phosphate and lithium nickel oxide(s) and said one or more lithium nickel oxides represents from 1 to 30% by mass of the total mass of lithium manganese and iron phosphate and lithium nickel oxide(s).
[0021] The invention also relates to a lithium-ion electrochemical element comprising at least one positive electrode which is the electrode as described above and at least one negative electrode. Brief description of the figures
[0022] Embodiments of the invention are described below in more detail with reference to the following figures.
[0023] [Fig. 1] is a scanning electron microscopy photograph of a powder of the active material of Example A. This powder consists of non-porous, non-spherical primary LMFP nanoparticles with dimensions close to 100 nm. The contours of a primary nanoparticle have been drawn in order to individualize it and highlight it. the size.
[0024] [Fig.2] is a scanning electron microscopy photo of a powder of the active ingredient of example B. This powder is made up of porous spherical agglomerates resulting from the agglomeration of the primary nanoparticles of example A. The outline of an agglomerate has been drawn in order to individualize it and highlight its diameter.
[0025] [Fig.3] represents the variation of the porosity of powders of particles of the materials active A to D examples depending on the pressure applied to these powders. The porosity on the ordinate is the sum of the porosity between the particles and the internal porosity of the particles.
[0026] Description of the embodiments of the invention Active material(s) of the positive electrode
[0027] A positive electrode according to the invention comprises one or more active materials, one of which is made up of LMFP particles characterized on the one hand by a quasi-spherical shape and on the other hand by an internal porosity less than or equal to 5%. By quasi-spherical is meant a sphericity factor greater than or equal to 0.9, preferably greater than or equal to 0.95, more preferably greater than or equal to 0.97.
[0028] Preferably, at least 90% or at least 95% of the LMFP particles meet the sphericity criterion.
[0029] The evaluation of the degree of sphericity of LMFP particles can be carried out by scanning electron microscopy (SEM). On a SEM photo of particles, the smallest and largest dimensions of each particle are measured, and a statistical average of the ratio of the two is taken.
[0030] The fact that the LMFP particles only have a shape close to the sphere does not allow low electrode porosity values to be obtained. It is necessary that the LMFP particles also have an internal porosity of less than or equal to 5%.
[0031] LMFP particles having a quasi-spherical shape and an internal porosity of less than or equal to 5% can be obtained by preparing a non-lithiated spherical Fe and Mn phosphate precursor by sol-gel or hydrothermal method, preferably using an acid complexing agent rather than a basic complexing agent or no complexing agent. Sintering is then carried out by heat treatment, preferably less than 500°C on this spherical precursor. Other sintering steps are carried out during the heat treatments, preferably at a temperature greater than or equal to 600°C, applied after lithiation of the precursor and during the production of the optional carbon coating by pyrolysis of a carbon precursor.
[0032] Characterization of the porosity of LMFP particles: Mercury powder porosimetry allows visualization of the progressive absorption of mercury in the sample in two stages: - a first stage at low pressure (<150 bar) due to the absorption of mercury in the inter-particle spaces, - a second stage at high pressure (>150 bar) corresponding to the absorption of mercury in the open intra-particle porosity. The volume of mercury absorbed in this stage represents the internal open porosity of the LFMP. The closed internal porosity of the particles is inaccessible to mercury and is assessed by helium pycnometry. The difference in density between the theoretical density and the density measured by helium pycnometry is due to the closed internal porosity of the particles. The term internal porosity of LFMP particles here refers to the sum of the closed internal porosity and the open internal porosity of the LFMP particles.
[0033] Lithium manganese iron phosphate has the formula LixMni y zFeyMzPO4 (LMFP) where 0.8 <x<l,2 ; 0,5<l-y-z<l ; 0<y<0,5 ; 0<z<0,2 ; M étant un ou plusieurs éléments choisis dans le groupe consistant en Al, B, Mg, Si, Ca, Ti, V, Cr, Co, Cu, Ni, Zn, Y, Zr, Nb, W et Mo.
[0034] The stoichiometric index 1-yz of manganese may be at least 0.6 or at least 0.7 or at least 0.8. It may range from 0.7 to 0.9 or from 0.75 to 0.80. Preferably, 0.70 <l-y-z<l.
[0035] The stoichiometric index y of iron can be at most 0.4 or at most 0.3 or at most 0.2.
[0036] Examples of LMFP are LiMno>8Feoj2PC)4, LiMnojsFeo^PCL, LiMnoj7Feoj3P04, LiMn2 / 3Fei / 3PO4 and LiMnojFeojPCL.
[0037] LMFP may be coated with a layer of carbon. It may be coated in particular with graphite or amorphous carbon or carbon nanotubes.
[0038] Several LMFP type compounds of different formulas can be used in a mixture.
[0039] The invention can be implemented using: - either disjointed LMFP particles, also called primary particles, having a median diameter DV5o ranging from 500 nm to 20 pm or from 1 to 20 pm or from 5 to 15 pm or from 1.5 to 4 pm; - or agglomerates of primary LMFP particles, also called secondary particles, these agglomerates resulting from the agglomeration of primary particles characterized by a median diameter DVso ranging from 50 nm to 20 pm or from 5 pm to 15 pm or 1.5 pm to 4 pm. The median diameter Diodes secondary particles can range from 1 to 50 pm.
[0040] The expression "volume median diameter Dv50" means that, in a given population of particles, 50% of the volume of the particles consists of particles having a equivalent diameter less than the Dv50 value and 50% of the particle volume consists of particles having an equivalent diameter equal to or greater than the Dv50 value. The term "equivalent diameter" of a particle means the diameter of a sphere having the same volume as that particle. Dv50 can be measured by laser particle size analysis.
[0041] The size distribution of the LMFP particles can be monomodal or bimodal. A monomodal distribution makes it possible to achieve powder porosity values ranging from 25 to 30%. Preferably, the distribution is bimodal. The first population is characterized by a first median diameter Dyso1, the second population is characterized by a second median diameter DV5o2, the ratio between Dyso1 and D v5o2 preferably ranges from 3 to 10. Such a particle size distribution makes it possible to reduce the void volume between the LMFP particles and therefore to reduce the porosity of the electrode. A bimodal distribution makes it possible to achieve powder porosity values ranging from 20 to 30%. According to one embodiment, the mass percentage of particles characterized by a second median diameter Dv502 less than the first median diameter Dvso1 ranges from 10 to 20% relative to the mass of all the LMFP particles.
[0042] LMFP can be mixed with one or more lithiated phosphates containing cobalt or nickel or iron of respective formulas: i) LixCoi yMyPO4 (LCP) and 0.8 <x<l,2 ; 0<y<0,6 où M est choisi dans le groupe consistant en B, Mg, Al, Si, Ca, Ti, V, Cr, Mn, Ni, Cu, Zn, Y, Zr, Nb et Mo ; ii) LixNii yMyPO4 (LNP) and 0.8 <x<l,2 ; 0<y<0,6 où M est choisi dans le groupe consistant en B, Mg, Al, Si, Ca, Ti, V, Cr, Mn, Fe, Co, Cu, Zn, Y, Zr, Nb et Mo ; iii) LixFei yMyPO4 (LFP) and 0.8 <x<l,2 ; 0<y<0,6 où M est choisi dans le groupe consistant en B, Mg, Al, Si, Ca, Ti, V, Cr, Co, Cu, Zn, Y, Zr, Nb et Mo. Preferably, it is LFP.
[0043] LMFP can be mixed with a lithium vanadium fluorophosphate of formula iv) Lii+XVPO4F (LVPF) where 0 <x<0,15, ou à un de ses dérivés de formule v) Lii+xVi yMyPO4Fz (LVMPF) où0<x<0,15, 0<y<0,5, 0,8<z<l,2 et M est choisi dans le groupe consistant en Ti, Al, Y, Cr, Cu, Mg, Mn, Fe, Co, Ni et Zr.
[0044] LMFP can be mixed with one or more lamellar lithiated oxides of transition metals chosen from: a) Liw(NixMnyCozMt)O2(NMC) where 0.9 <w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci, b) Liw(NixCoyAlzMt)O2(NCA) where 0.9 <w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de B, Mg, Si, Ca, Ti, V, Cr, Mn, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, Sr, Ce, Ga, Ta, Nd, Pr, La et des mélanges de ceux-ci, et c) Liw(NixMnyCozMt)O2(NMX) where 0.9 <w<l,l ; 0,60<x<0,80 ; 0<y ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci. NMX peut être monocristallin ou polycristallin. d) Liw(NixMnyCozMt)O2 where 1.1 <w<1,6 ; 0<x ; 0,50<y<0,80; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci.
[0045] Preferably, LMFP is mixed with one or more NMC type compounds.
[0046] Preferably, the mass percentage of LMFP represents at least 50% or at least less than 70% or at least 90% of the mass of all the active materials of the positive electrode. In this embodiment in which LMFP is the majority, the preferred lamellar lithium oxide is of the NMC type. Positive electrode
[0047] The positive electrode of the element comprises a current collector, at least one of the faces of which is coated with a layer of a composition of positive active materials. By "composition of active materials" is meant a composition comprising: - one or more active ingredients as described above, one of which is made up of LMFP particles of almost spherical shape and internal porosity less than or equal to 5%, and - possibly one or more binders and one or more electronically conductive materials.
[0048] The overall porosity of the electrode is the sum of the open internal porosity, the closed internal porosity of the active material particles (including the LMFP particles) and the porosity between the active material particles, the binder particles and the particles of possibly incorporated electronically conductive additive. The technique for measuring the open internal porosity and the closed internal porosity of the LMFP particles is described above.
[0049] The positive current collector is a solid or perforated metal strip which may be made of aluminum or an aluminum alloy or steel or stainless steel. Its thickness may be in the range of 6 to 30 μm or 5 to 20 μm or 10 to 15 μm, preferably 10 to 15 μm.
[0050] Before the current collector is coated with the active material composition layer, it may be coated, on one of its faces or on both of its faces, with a coating intended to improve the electronic conductivity between the active material composition layer and the foil and / or to improve the adhesion of the active material composition layer to the foil. The coating material may be selected from the group consisting of amorphous carbon, graphite, fibers of carbon, carbon nanotubes, and mixtures thereof. It is preferably made of amorphous carbon. The coating material may be obtained by coating the foil with a dispersion of the material and then evaporating the solvent from the dispersion, or it may be obtained by sputtering. Only certain portions of the foil may be coated with the coating material. The coated portions may be separated from each other by predetermined or periodic intervals ("intermittent coating"). The intermittent coating is preferably present on both sides of the foil. It facilitates electrode processing. Alternatively, one or both sides of the foil may have undergone a surface treatment intended to increase the adhesion of the active material composition layer to the foil. This may be a surface treatment creating asperities or microroughness, such as chemical etching or laser treatment.
[0051] The binder generally used in the active material composition strengthens the cohesion between the active material particles and improves the adhesion of the active material composition layer to the current collector. The binder may contain one or more of the following compounds: polyvinylidene fluoride (PVDF) and its copolymers, polytetrafluoroethylene (PTFE) and its copolymers, polyacrylonitrile (PAN), polymethyl or butyl methacrylate, polyvinyl chloride (PVC), polyvinyl formal, polyester, block polyetheramides, polymers of acrylic acid, methacrylic acid, acrylamide, itaconic acid, sulfonic acid, elastomers, and cellulose compounds such as carboxymethylcellulose (CMC). The elastomers that can be used as binders can be chosen from styrene-butadiene (SBR), butadiene-acrylonitrile (NBR), hydrogenated butadiene-acrylonitrile (HNBR).The binder can represent from 1% to 10% or from 1 to 5% or from 2 to 5% of the mass of the dry composition of active ingredients.
[0052] The electronically conductive material is generally chosen from graphite, carbon black, acetylene black, soot, graphene, carbon fibers, single-walled carbon nanotubes, multi-walled carbon nanotubes, and mixtures thereof. It may represent from 0.1 to 10% or from 0.1 to 5% of the mass of the dry composition of active materials. Preparation of the positive electrode:
[0053] An ink is prepared by dispersing the active material(s) in a solvent or a mixture of several solvents. Optionally, a binder and an electronically conductive material are added to the dispersion. By varying the amount of solvent incorporated in the mixture, the viscosity of the ink can be varied before it is deposited on one side of the current collector. The ink-coated current collector is dried and then rolled to adjust its thickness. After evaporation of the solvent(s), a layer of a composition of materials is obtained. active ingredients whose proportions of the various constituents are typically: - from 80 to 98% or from 90 to 95% by mass of positive active ingredients, - from 1 to 10% or from 2 to 5% by mass of binder(s), - from 0.1 to 10% or from 2 to 5% by mass of electronically conductive material. Negative electrode:
[0054] At least one negative electrode comprises a current collector, at least one of two faces of which is coated with a layer of a negative active material composition. The negative active material composition comprises at least one negative active material and optionally a binder and an electronically conductive material. The negative current collector is a solid or perforated metal strip which may be made of copper or a copper-based alloy. Its thickness may range from 3 to 10 μm, preferably from 5 to 8 μm.
[0055] Before the current collector is coated with the active material composition layer, it may be coated, on one or both sides, with a coating intended to improve the electronic conductivity between the active material composition layer and the foil and / or to improve the adhesion of the active material composition layer to the foil. The coating material and the method of depositing the coating may be the same as those described for the current collector of the positive electrode.
[0056] The negative active material may be selected from carbon, graphite, coke, carbon black, glassy carbon, silicon, silicon oxide, a silicon-carbon composite, a silicon carbide, a titanium oxide, a lithiated titanium oxide, a titanium niobium oxide and a mixture thereof. The titanium oxide may be selected from H2Ti60i3, H2Tii2O25 and TiO2. The lithiated titanium oxide may be selected from Li4Ti50i2, Li2TiO3>Li2Ti3O7jLiTi2O4 and Li2Na2Ti60i4. The titanium niobium oxide may be selected from TiNb2O7, Ti2Nb2O9 and Ti2Nbi0O29. Preparation process of the negative electrode:
[0057] The negative electrode is prepared in a conventional manner. An ink is prepared by dispersing in a solvent or in a mixture of solvents one or more negative active materials, optionally with a binder. The binder may be such as those described in relation to the positive electrode.
[0058] The ink-coated current collector is dried and then rolled to adjust its thickness. This results in a negative electrode. Typical proportions of the components of the negative active ingredient composition layer, after evaporation of the solvent contained in the ink, are: - from 85 to 98% or from 90 to 98% by mass of negative active materials, - from 1 to 10% or from 1 to 5% by mass of binder(s), - from 0 to 5% by mass or from 1 to 5% of an electronically conductive material. Electrolyte:
[0059] The electrolyte may be liquid or solid. The liquid electrolyte is obtained by dissolving one or more lithium salts in one or more organic solvents. The solvent may be chosen from saturated cyclic carbonates, unsaturated cyclic carbonates, non-cyclic carbonates, alkyl esters, ethers, nitrile type solvents and tetrahydrothiophene dioxide (sulfolane).
[0060] Saturated cyclic carbonates include ethylene carbonate (EC), fluoroethylene carbonate (FEC), propylene carbonate (PC), butylene carbonate (BC), and mixtures thereof.
[0061] Unsaturated cyclic carbonates include vinylene carbonate (VC).
[0062] Non-cyclic carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), and mixtures thereof.
[0063] Alkyl esters include methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, and mixtures thereof.
[0064] Ethers include dimethyl ether (DME), diethyl ether (DEE) and mixtures thereof.
[0065] The lithium salt may be chosen from lithium perchlorate LiC104, lithium hexafluorophosphate LiPF6, lithium tetrafluoroborate LiBF4, lithium hexafluoroarsenate LiAsF6, lithium hexafluorantimonate LiSbF6, lithium trifluoromethanesulfonate LiCF3SO3, lithium bis(fluorosulfonyl)imide Li(FSO2)2N (LiFSI), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2 (LiTFSI), lithium tris(fluoromethanesulfonyl)methylide LiC(CF3 SO2)3 (LiTFSM), lithium bis(pentafluoroethylsulfonyl)imide LiN(C2F(SO2)2 (LiBeTI), lithium-4,5-dicyano-2-(trifluoromethyl)imidazolide (LiTDI), lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LIDFOB), lithium tris(pentafluoroethyl)trifluorophosphate LiPF3(CF2CF3)3 (LiFAP), lithium difluorophosphate LiPO2F2, and mixtures thereof.
[0066] The concentration of said at least one lithium salt may be in the range from 0.75 to 1.5 mol / L. It is preferably in the range from 1 to 1.5 mol / L. It is even better in the range from 1 to 1.2 mol / L. Separator:
[0067] A separator is interposed between a positive electrode and a negative electrode. The material of the separator can be chosen from the following materials: a polyolefin, for example polypropylene PP, polyethylene PE, a polyester, glass fibers bonded by a polymer, polyimide, polyamide, polyaramid, polyamide-imide and cellulose. The polyester may be chosen from polyethylene terephthalate (PET) and polybutylene terephthalate (PBT). Advantageously, the polyester or polypropylene or polyethylene contains or is coated with a ceramic material chosen from the group consisting of metal oxides, oxyhydroxides, carbides, nitrides, borides, silicides and sulfides. This ceramic material may be SiO2 or Al2O3. The separator may be a ceramic-coated polyolefin layer, preferably a polyethylene layer coated with ceramic on both sides. Preparation of the electrochemical beam:
[0068] An electrochemical bundle is formed by inserting a separator between at least one positive electrode and at least one negative electrode. The electrochemical bundle is inserted into the cell container. The cell container may be parallelepipedal or cylindrical in shape. In the latter case, the electrochemical bundle is spiraled to form a cylindrical assembly of electrodes.
[0069] The electrochemical element can also be in pouch format. Filling and closing the container:
[0070] In the case of a container of parallelepiped or cylindrical format, a cover is assembled on the container of the element, for example by laser welding. The container of the element is filled with electrolyte. For this purpose, the cover may comprise a filling hole through which the electrolyte is introduced. Once the electrolyte has been introduced, this filling hole is closed by a stainless steel ball via electrical welding of the ball to the hole. EXAMPLES
[0071] The porosities of powders of different active ingredients were compared. Table 1 below shows the active ingredients used. [Tables 1] Active ingredient A* Primary non-porous, non-spherical LMFP particles of approximately 100 nm B* Secondary porous spherical LMFP particles with a diameter of approximately 10 pm. C Non-porous spherical LMFP particles with a monomodal size distribution D Non-porous spherical LMFP particles with a bimodal size distribution characterized by a Dvso' / Dvso2 ratio equal to 7 * Electrode outside the invention
[0072] Figures 1 and 2 are SEM photographs of the powders of active ingredients A and B. A primary particle is highlighted in [Fig.l]. An agglomerate is highlighted in [Fig.2].
[0073] The powders of active materials A and B were subjected to an increasing compression force. [Fig. 3] represents the variation in the porosity of a powder of active material A and that of a powder of active material B, as a function of the pressure applied. It can be seen that even for a high pressure of 1000 bar, the porosity of a powder of active material A or B outside the invention remains greater than 40%. Concerning the powder of active material A, its high porosity is due to the non-spherical nature of the particles. Concerning the powder of active material B, its high porosity is due to the porous nature of the particles. The theoretical porosity of a powder of active material C according to the invention comprising particles with a monomodal size distribution is 26%. That of a powder of active material D according to the invention comprising particles with a bimodal size distribution is 20%.The lower porosity value of active material powder D than that of active material powder C is explained by the bimodal distribution of the particles. Active materials C and D therefore make it possible to increase the volume capacity of the positive electrode by approximately 40 to 50% compared to active materials A and B.
Claims
Claims
1. An electrode comprising one or more active materials, one of the active materials being a lithium manganese iron phosphate of formula LixMni y zFeyMzPO4 (LMFP) where 0.8 <x<l,2 ; 0,5<l-y-z<l ; 0<y<0,5 ; 0<z<0,2 ;M being one or more elements selected from the group consisting of Al, B, Mg, Si, Ca, Ti, V, Cr, Co, Cu, Ni, Zn, Y, Zr, Nb, W and Mo, the electrode being characterized in that: - the lithium manganese and iron phosphate is in the form of particles, at least 90% by number of the particles have a sphericity factor greater than or equal to 0.90 and less than 1, the sphericity factor of a particle being defined as the ratio between the surface area of a sphere having the same volume as the particle and the surface area of this particle, and in that - the internal porosity of the lithium manganese and iron phosphate particles is less than or equal to 5%, the internal porosity being defined by the ratio Vvoid / VLMFPwhere Vvoid represents the void volume inside the lithium manganese and iron phosphate particles, VLMFP represents the geometric volume of the phosphate particles lithium manganese and iron.;
2. The electrode of claim 1, wherein the sphericity factor is greater than or equal to 0.
95.
3. The electrode of claim 2, wherein the sphericity factor is greater than or equal to 0.
98.
4. Electrode according to one of claims 1 to 3, in which the internal porosity of the particles of lithium manganese and iron phosphate ranges from 2 to 3%.
5. Electrode according to one of the preceding claims, in which at least 95% by number of the particles of lithium manganese and iron phosphate have a sphericity factor greater than or equal to 0.9 and less than 1.
6. Electrode according to one of the preceding claims, in which the particles of lithium manganese and iron phosphate are in the form of primary particles having a volume median diameter Dv50 ranging from 500 nm to 20 pm or from 5 to 15 pm or from 1.5 to 4 pm.
7. Electrode according to one of claims 1 to 5, in which the particles of lithium manganese and iron phosphate are in the form of secondary particles having a volume median diameter Dv50 ranging from 1 pm to 50 pm, a secondary particle consisting of the agglomeration of primary particles having a volume median diameter Dv50 located in the range from 50 nm to 20 pm.
8. Electrode according to one of the preceding claims, in which the particles of lithium manganese and iron phosphate have a bimodal distribution, the first population being characterized by a first median diameter Dyso1, the second population being characterized by a second median diameter DV5o2, the ratio between Dyso1 and Dv5o2 ranging from 3 to 10.
9. Electrode according to one of the preceding claims, in which in the lithium manganese and iron phosphate, 0.70 <l-y-z<l.
10. Electrode according to one of the preceding claims, further comprising one or more active materials chosen from: - a lithium iron phosphate of formula iii) LixFei yMyP04 (LFP) where 0.8 <x<l,2 ; 0<y<0,6 et M est choisi dans le groupe consistant en B, Mg, Al, Si, Ca, Ti, V, Cr, Co, Cu, Zn, Y, Zr, Nb et Mo ; - un fluorophosphate lithié de vanadium de formule iv) Lii+XVPO4F (LVPF) où 0<x<0,15, ou à un de ses dérivés de formule v) Lii+xVi yMy PO4Fz (LVMPF) où0<x<0,15, 0<y<0,5, 0,8<z<l,2 et M est choisi dans le groupe consistant en Ti, Al, Y, Cr, Cu, Mg, Mn, Fe, Co, Ni, et Zr ; - un oxyde lithié de nickel, de manganèse et de cobalt de formule a) Liw (NixMnyCozMt)O2(NMC) où 0,9<w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ;M being selected from the group consisting of Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La and mixtures thereof, - a lithium oxide of nickel, cobalt and aluminium of formula b) Liw (NixCoyAlzMt)O2(NCA) where 0.9 <w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de B, Mg, Si, Ca, Ti, V, Cr, Mn, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, Sr, Ce, Ga, Ta, Nd, Pr, La et des mélanges de ceux-ci, - un oxyde lithié de nickel et de manganèse de formule c) Liw(NixMnyCozMt)O2(NMX) où 0,9<w<l,l ; 0,60<x<0,80 ; 0<y ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci,; - a lithium oxide of nickel and manganese of formula d) Liw(NixMnyCo zMt)O2 where 1.1 <w<1,6 ; 0<x ; 0,50<y<0,80 ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci.
11. Electrode according to claim 10, wherein said one or more active materials is one or more lithium nickel oxides chosen from: - a lithium nickel, manganese and cobalt oxide of formula a) Liw (NixMnyCozMt)O2(NMC) where 0.9 <w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci, - un oxyde lithié de nickel, de cobalt et d’aluminium de formule b) Liw(NixCoyAlzMt)O2(NCA) où 0,9<w<l,l ; 0<x ; 0<y ; 0<z ; 0<t ; M étant choisi dans le groupe constitué de B, Mg, Si, Ca, Ti, V, Cr, Mn, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, Sr, Ce, Ga, Ta, Nd, Pr, La et des mélanges de ceux-ci, et - un oxyde lithié de nickel et de manganèse de formule c) Liw(NixMnyCozMt)O2(NMX) où 0,9<w<l,l ; 0,60<x<0,80 ; 0<y ; 0<z<0,02 ; 0<t ;M being selected from the group consisting of Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La and mixtures thereof, and - a lithium oxide of nickel and manganese of formula d) Liw(NixMnyCo zMt)O2 where 1.1 <w<1,6 ; 0<x ; 0,50<y<0,80 ; 0<z<0,02 ; 0<t ; M étant choisi dans le groupe constitué de Al, B, Mg, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, W, Mo, S, Sr, Ce, Ta, Ga, Nd, Pr, La et des mélanges de ceux-ci.;
12. Electrode according to claim 11, in which: - the lithium manganese and iron phosphate represents from 40 to 99% by mass of the total mass of lithium manganese and iron phosphate and lithium nickel oxide(s); - said one or more lithium nickel oxides represents from 1 to 60% by mass of the total mass of lithium manganese and iron phosphate and lithium nickel oxide(s).
13. Electrode according to claim 12, in which: - the lithium manganese and iron phosphate represents from 70 to 99% by mass of the total mass of lithium manganese and iron phosphate and of lithium nickel oxide(s); - said one or more lithium nickel oxides represent from 1 to 30% by mass of the total mass of lithium manganese and iron phosphate and lithium nickel oxide(s).
14. Lithium-ion electrochemical element comprising: - at least one positive electrode which is the electrode according to one of claims 1 to 13, - at least one negative electrode.
Citation Information
Patent Citations
Preparation method of high-compaction-density lithium manganese iron phosphate / carbon composite positive electrode material
CN113072049A
Method for preparing high-density spherical lithium iron phosphate and lithium iron manganese phosphate
CN1632970A
Process for preparing high density spherical lithium ferric phosphate
CN1821065A
Electrode, secondary battery, battery pack, electric vehicle, electric power storage system, electric power tool, and electronic apparatus
US20130149604A1
Electrode material for lithium-ion secondary battery and lithium-ion secondary battery
US20180277887A1