Method for manufacturing a double-walled heat exchanger tube
The manufacturing process for double-walled heat exchanger tubes using a pure iron interphase addresses the challenges of cost and complexity in existing methods, achieving improved thermal conductivity and safety through a dense junction and resistance to fatigue defects.
Patent Information
- Application Number
- FR2023005571
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-02
AI Technical Summary
Existing manufacturing processes for double-walled heat exchanger tubes are expensive and complicated, and they do not effectively address the need for enhanced thermal conductivity, sealing, and resistance to pressure and fatigue defects.
A manufacturing process involving the co-axial assembly, brazing, co-deformation, and hot isostatic compression of metallic tubes with a pure iron interphase to create a dense junction between the tubes, eliminating mechanical clearance and ensuring uniform mechanical and thermal conductivity.
The process results in a double-walled heat exchanger tube with improved thermal conductivity, resistance to fatigue cracks, and enhanced safety against fluid contact, while reducing production costs and cycle times.
Abstract
Description
Title of the invention: Method for manufacturing a double-walled heat exchanger tube TECHNICAL FIELD OF THE INVENTION
[0001] The present invention relates to a method for manufacturing a double-walled heat exchanger tube, this double-walled tube being particularly intended to equip devices of the heat exchanger type.
[0002] Such heat exchangers find particular application in the chemical industry or in the energy sector. STATE OF THE ART
[0003] Heat exchangers are devices that allow the transfer of thermal energy from a first fluid to a second fluid, without mixing them.
[0004] Various types of two-fluid heat exchangers exist, among which are those equipped with a double-walled tube, also known as a "double-walled tube", which comprises two cylindrical (tubular) and coaxial tubes threaded one inside the other, the inner surface of the smaller diameter tube (inner tube) being intended to come into contact with one of the fluids and the outer surface of the larger diameter tube (outer tube) being intended to come into contact with the other fluid.
[0005] The particular structure of a double-walled heat exchanger tube has the advantage of providing enhanced safety to the heat exchanger equipped with it, insofar as each tube redundantly performs a dual function, namely a sealing function to prevent the two fluids from coming into contact and a function of resistance to the pressure exerted by the circulation of these two fluids.
[0006] This dual function is particularly important, for example, in cases where the heat exchanger is used in installations such as chemical reactors, where it is necessary to ensure safe and efficient heat exchange between a first fluid, such as reactive molten metals or metal salts, for example, sodium, lithium, or potassium-based, and a second fluid, such as water. Indeed, any failure occurring in a double-walled tube in such installations would have serious consequences for operation due to the chemical reactivity of the heat transfer fluid with the medium to be cooled. In this specific case, the stresses in service, in addition to the static pressure of the fluids and surface corrosion, result from thermal stresses and fatigue stresses imposed by operating cycles or vibrations induced by the thermohydraulics.
[0007] Most double-walled heat exchanger tubes plan to leave a mechanical gap, or space, between the inner and outer tubes.
[0008] By connecting this gap to a detection system, it is thus possible to detect the presence of fluid from the drilling of one of the two tubes before the integrity of the other tube is altered.
[0009] However, the presence of this gap is particularly detrimental with regard to the thermal conductivity properties of the double-walled heat exchanger tube and, moreover, does not allow for an effective response to a hypothetical simultaneous perforation of the two tubes constituting it.
[0010] To improve the thermal conductivity of double-walled heat exchanger tubes, it has been proposed to at least partially fill the gap existing between the two tubes.
[0011] Document CN 203928838, referenced [1] in this description, proposes a method for manufacturing a double-walled tube that includes a step of filling the gap between the inner and outer walls of such a tube with a metal powder. By ensuring a radial temperature distribution, this metal powder provides good thermal conductivity to the double-walled tube and also helps to mitigate the risks of degradation associated with abrupt thermal transitions.
[0012] Document CN 113458737, referenced [2], proposes a method for manufacturing a double-walled tube comprising an outer tube, an intermediate layer, and an inner tube, the outer and inner tubes as well as the intermediate layer being metallic, cylindrical, and coaxial. The method described in document [2] comprises the following successive steps:
[0013] (1) the placement of the inner tube coated with the intermediate layer in the tube external, the gap between the internal and external tubes being appropriate;
[0014] (2) the sealing and welding of the inner and outer tubes at each of their ex treacles; and
[0015] (3) the installation of the tubes thus welded for an isostatic compression step hot under conditions suitable for diffusion welding.
[0016] In this document [2], the intermediate layer, which is made of a material selected from copper, nickel, chromium, and vanadium, is produced by chemical or electrolytic deposition. In step (1), the appropriate gap between the inner and outer tubes is between 0.2 mm and 2 mm.
[0017] Although they improve the thermal conductivity properties of double-walled tubes, the manufacturing processes described in documents [1] and [2] are nevertheless relatively expensive and complicated to implement on an industrial level.
[0018] The object of the present invention is, therefore, to overcome the drawbacks of prior art methods and to propose a method for manufacturing a double-walled heat exchanger tube that has the dual function of sealing and resistance to pressure, in particular by resisting the propagation of fatigue defects, as well as good thermal conductivity properties, this process allows for advantageous productivity and industrial implementation costs compared to the processes described in documents [1] and [2]. Description of the invention
[0019] The objectives stated above and others are achieved by a method of manufacturing a double-walled heat exchanger tube of the aforementioned type, i.e. comprising an outer tube and an inner tube, the outer and inner tubes being metallic, cylindrical and coaxial.
[0020] According to the invention, the manufacturing process comprises the following successive steps (i) to (vii):
[0021] (i) the supply:
[0022] . of a first tube having an internal diameter dHnt and an external diameter diext, this The first tube is intended to form the outer tube.
[0023] . of a second tube having an internal diameter d2int and an external diameter d2ext, this the second tube being intended to form the inner tube, and
[0024] . of a cylindrical and coaxial tubular strip made of Fe° having an internal diameter internal diameter and an external diameter dexter,
[0025] such as
[0026] 0.15 mm < (dHnt - dext) < 0.25 mm,
[0027] 0.15 mm < (dint - d2ext) < 0.25 mm, and
[0028] 10 pm < (dext - dint) < 200 pm;
[0029] (ii) the coaxial assembly of the second tube and the strip inside the first tube, the strip being positioned between the first and second tubes;
[0030] (iii) brazing or gluing one end of the assembly obtained at the end of step (ii);
[0031] (iv) the co-deformation of the assembly obtained at the end of step (iii);
[0032] (v) the cutting of the ends of the co-deformed assembly at the end of the step (iv);
[0033] (vi) welding the cut ends of the assembly obtained at the end of step (v); and
[0034] (vii) the heat treatment of the assembly obtained at the end of step (vi), this heat treatment being carried out by hot isostatic compression, thereby obtaining the double-walled heat exchanger tube.
[0035] The process according to the invention makes it possible to form, between the outer and inner tubes, a dense metallic interphase of pure iron which fills the entire initial volume of the gap existing between the first and second tubes and thus ensures a junction Uniform mechanical resistance is achieved between the outer and inner tubes. The absence of mechanical play between the outer and inner tubes prevents movement of these two tubes relative to each other: as the two tubes essentially become a single tube, they deform in the same way as a monolithic tube under mechanical stress. Thanks to the manufacturing process according to the invention, a double-walled heat exchanger tube with particularly high geometric performance is obtained.
[0036] This pure iron metallic interphase also gives the double-walled heat exchanger tube excellent thermal conductivity properties by ensuring very good heat transfer between the outer and inner tubes, thereby increasing the efficiency of a heat exchanger equipped with such a double-walled heat exchanger. Unexpectedly and surprisingly, the Inventor found that this ductile and dense iron (Fe°) interphase provides excellent thermal conductivity, approaching a value close to that of an equivalent solid wall.
[0037] This ductility of the iron metallic interphase also makes it possible to deflect and / or stop the propagation of fatigue cracks, particularly high-cycle fatigue cracks, that would have formed and propagated within one of the two tubes, thus preserving the integrity of the other tube. In particular, when fatigue cracks are deflected, they propagate within the ductile metallic interphase, thus providing a 30% longer service life at room temperature.
[0038] This iron interphase is further characterized by a seal which allows it to prevent the capillary propagation of fluid from such a crack between the two tubes and, therefore, to drastically reduce the risks of contact between the first and second fluids of the heat exchanger, which is fundamental, in particular when the first and second fluids are reactive, when there is a risk of contamination or when the tubes are not controllable in service.
[0039] Furthermore, the process according to the invention does not implement any step exposing the constituent elements of the double-walled tube to hydrogen, unlike the electrolytic deposition which is implemented in the process of document [2] and which, when exposure to hydrogen is not controlled, can weaken the metallic material forming the constituent elements of the tube, in particular when this material is steel.
[0040] The process according to the invention makes it possible to manufacture a double-walled heat exchanger tube which has an internal diameter d1NT and an external diameter dEXT-
[0041] According to one embodiment, the internal diameter d1NT of the double-walled tube is between 6 mm and 30 mm and, advantageously, between 8 mm and 15 mm.
[0042] According to one embodiment, the external diameter d^y of the double-walled tube is between 6 mm and 30 mm and, advantageously, between 10 mm and 20 mm.
[0043] It is specified that the expression "between ... and..." which is used above but also in the rest of this description to define an interval, must be understood as defining not only the values of the interval, but also the values of the bounds of this interval.
[0044] The method according to the invention comprises the steps (i) to (vii) mentioned above and detailed below.
[0045] During step (i) of the manufacturing process according to the invention, two tubes are provided, a first tube which is intended to form the outer tube of the double-walled heat exchanger tube, and a second tube which is intended to form the inner tube of this double-walled heat exchanger tube.
[0046] The first tube has an internal diameter dHnt and an external diameter diext, and the second tube has an internal diameter d2int and an external diameter d2ext.
[0047] A cylindrical and coaxial tubular strip is also provided, which is made of iron in oxidation state 0, i.e. pure iron Fe°. This Fe° strip has an internal diameter dint and an external diameter dext.
[0048] The first and second tubes and the strip are such that:
[0049] 0.15 mm < (diint - dext) < 0.25 mm,
[0050] 0.15 mm < (dint - d2ext) < 0.25 mm, and
[0051] 10 pm < (deXt - dint) < 200 pm.
[0052] In other words, the strip has a thickness between 80 pm and 200 pm.
[0053] In an advantageous embodiment, the strip has a thickness between 80 µm and 150 µm.
[0054] In an advantageous embodiment of the method according to the invention, at least one of the elements chosen from the first tube, the second tube and the tubular strip is weld-free.
[0055] In a preferred embodiment of the method according to the invention, the first tube, the second tube, and the tubular strip are all weld-free. This maximizes reliability in terms of sealing and safety.
[0056] The first and second tubes, whether or not they are weld-free, can be produced by any conventional industrial process.
[0057] According to an advantageous embodiment, the first and second tubes are obtained by implementing, prior to step (i), the following successive steps (i0) and (ij):
[0058] (i0) hot spinning or hot rolling of a drilled rod (also called connecting rod), whereby a tubular rough shape is obtained, and
[0059] (ii) cold drawing or pilgrim step rolling of the tubular blank as obtained at the end of step (io).
[0060] The implementation of these steps (i0) and (ii) makes it possible to obtain seamless tubes which can reach lengths of up to 6 m.
[0061] According to an advantageous embodiment, the seamless tubular strip is obtained by carrying out, prior to step (i), the following successive steps (i2) to (i4):
[0062] (i2) drilling an iron rod Fe°,
[0063] (i3) turning the drilled rod as obtained at the end of step (i2), by means of which gives us a tubular rough shape, and
[0064] (i4) the pilgrim step rolling of the tubular blank as obtained at the end of step (i3).
[0065] In one embodiment, which will be illustrated in the example described below, the pilgrim step (i4) of rolling can be repeated at least once. The process according to the invention may, furthermore, include a heat treatment step (i4') preferably conducted between each step (i4) and, for example, at 850 °C for 1 h.
[0066] According to an advantageous embodiment, the method according to the invention further comprises a cleaning step of at least the internal surface of the first tube, the internal and external surfaces of the tubular strip and the external surface of the second tube, this cleaning step being carried out prior to step (ii) of coaxial assembly.
[0067] This cleaning step optimizes the subsequent contact between the tubular strip and the surfaces of the external and internal tubes with which this strip will be in contact and, in so doing, improves the sealing and thermal conductivity of the double-walled heat exchanger tube.
[0068] The manufacturing process according to the invention comprises, after step (i), a step (ii) of coaxial assembly of the first and second tubes and the tubular iron strip Fe°. More particularly, in this step (ii), the second tube and the strip are introduced inside the first tube, the strip being arranged between the first and second tubes.
[0069] In other words, at the end of step (ii), an assembly is obtained in which the tubular iron strip Fe° is positioned between the first and second tubes.
[0070] The manufacturing process according to the invention comprises, after step (ii) of coaxial assembly, a step (iii) of brazing or gluing one end of the assembly obtained at the end of step (ii).
[0071] This brazing step (iii) makes it possible to maintain the assembly for the implementation of the following steps of the process according to the invention, in particular its co-deformation step (iv), but also to protect the tubular strip from any soiling, in particular from that generated by the lubricants which are used during this subsequent co-deformation step (iv).
[0072] The brazing alloy must advantageously have sufficient ductility to be able to co-deformed with the tubes and tubular strip during step (iv).
[0073] In a particular embodiment involving first and second stainless steel tubes, the brazing step (iii) is carried out with high silver brazing material.
[0074] The manufacturing process according to the invention comprises, after the brazing step (iii), a co-deformation step (iv) of the assembly obtained at the end of step (iii).
[0075] This co-deformation step (iv) reduces the volume of the mechanical play existing between the first tube and the strip, on the one hand, and between the second tube and the strip, on the other hand, which promotes the homogeneous elongation of the tubes and the strip, the preservation of the geometry of the assembly of these elements during subsequent operations, by guaranteeing the absence of wrinkling of the strip during the deformation.
[0076] This co-deformation step (iv) can, in particular, be implemented by co-stretching or co-rolling.
[0077] In an advantageous embodiment of the process according to the invention, this co-formation step (iv) is carried out by pilgrim-step co-rolling of the assembly obtained at the end of step (iii).
[0078] Choosing such a step (iv) of pilgrim-step co-rolling has the advantage of reducing the volume of mechanical clearance between the first and second tubes and the tubular strip. As a result, the amount of gas contained in the assembly becomes negligible, and no degassing step is necessary before carrying out the subsequent steps, in particular the welding step (vi).
[0079] In one embodiment, the manufacturing process according to the invention does not include a degassing step between the co-deformation step (iv) and the welding step (vi).
[0080] Eliminating such a degassing step, which is particularly complex to implement industrially in the context of manufacturing double-walled tubes, contributes to a significant reduction in cycle times, costs and production lead times.
[0081] The manufacturing process according to the invention comprises, at the end of the co-deformation step (iv), a cutting step (v) of the ends of the co-deformed assembly, so as to eliminate the ends of the assembly affected, for one, by the brazing and, for the other, by the percolation of lubricating fluids.
[0082] These ends cut in step (v) are then subjected to a welding step (vi).
[0083] This step (vi) of welding the two ends of the assembly makes it possible to isolate the interfaces of the tubular strip with the first and second tubes from the environment.
[0084] In one embodiment, the welding step (vi) is carried out by an arc welding process with a non-consumable electrode, for example tungsten, and without filler metal of material. This welding can advantageously be carried out under inert gas.
[0085] The manufacturing process according to the invention comprises, after the welding step (vi), a heat treatment step (vii) of the assembly obtained at the end of the step (vi).
[0086] This step (vii) of heat treatment of the assembly obtained at the end of step (vi), is carried out by hot isostatic compression (HIC), thereby obtaining the double-walled heat exchanger tube.
[0087] This hot isostatic pressing step (vii) allows for the welding, by diffusion, of the inner surface of the first tube to the outer surface of the tubular strip and, conversely, of the outer surface of the second tube to the inner surface of the tubular strip. At the end of the hot isostatic pressing step (vii), a uniform mechanical joint is obtained between the first and second tubes, formed by a pure iron interphase originating from the tubular strip. The presence of a small amount of oxygen trapped in the surface roughness of the strip and the tubes (absence of outgassing) contributes to the formation of mixed iron and chromium oxides (in the case of steel tubes). These oxides play a beneficial role in surface delamination during the propagation of a fatigue crack.
[0088] This step (vii) of hot isostatic compression, which does not generate or causes little deformation of the first and second tubes and of the tubular strip, makes it possible to optimize the preservation of the geometry of the assembly formed by these tubes and strip and, consequently, to respect the geometric tolerances of the finished tubes, which makes it possible to ensure reproducibility, and therefore reliability, of the double-walled heat exchanger tubes manufactured by the process according to the invention.
[0089] In a particular embodiment, step (vii) is conducted at a temperature between 800 °C and 1200 °C, at a pressure between 50 MPa and 200 MPa and for a duration between 30 min and 4 h.
[0090] In an advantageous embodiment, step (vii) is conducted at a temperature between 1000 °C and 1200 °C, at a pressure between 100 MPa and 200 MPa and for a duration between 30 min and 2 h.
[0091] The process according to the invention makes it possible to manufacture double-walled heat exchanger tubes of variable lengths and geometries.
[0092] The materials of the first tube and the second tube may be identical or different, and may in particular include iron.
[0093] In an advantageous embodiment, the first and second tubes are made of a material comprising iron, in particular stainless steel. This stainless steel may advantageously be a martensitic steel, advantageously Eurofer-97 or T-91 steel.
[0094] In a preferred embodiment, the materials of the first and second tubes are identical.
[0095] In one embodiment, the manufacturing process according to the invention further comprises, after the heat treatment step (vii), one or more of the following steps (viii) to (xii):
[0096] (viii) the cooling of the double-walled heat exchanger tube, for example at a rate of 50 °C / h;
[0097] (ix) the bending of the double-walled heat exchanger tube obtained at the end of step (viii);
[0098] (x) the expansion of the double-walled heat exchanger tube obtained at the end of step (viii) or (ix);
[0099] (xi) the heat treatment of the double-walled heat exchanger tube obtained at the end of step (ix) or (x), such as quenching or normalized tempering; and
[0100] (xii) straightening the double-walled heat exchanger tube obtained at the end of step (ix), (x) or (xi).
[0101] In particular, and name when the first and second tubes are made of stainless steel and, more particularly, of Eurofer-97, a cooling step (viii) allows the double-walled tube to be kept in a state suitable for bending and / or flaring the tube.
[0102] The double-walled tubes manufactured by the process according to the invention can be bent and assembled like conventional tubes.
[0103] It should be noted that the choice of pure iron for the tubular strip and, consequently, for the interface of the double-walled tube does not alter the composition of the weld pool during the welding of such tubes. It is therefore possible to assemble the tubes in their full thickness without significantly altering the composition of the weld bead due to the presence of the iron interface.
[0104] It would be quite different with an interphase made of copper, chromium, nickel or vanadium as described in document [2] which imposes a significant change in the composition of the weld bead, with the possible risk of modifying the mechanical properties of the weld bead of such a tube.
[0105] The process according to the invention therefore greatly facilitates the industrial manufacture of double-walled heat exchanger tubes, by avoiding the creation of interphase-free zones, also called reserves, located at the future welds.
[0106] In general, the heat treatment step (xi) is intended to confer the expected mechanical properties for the double-walled tube manufactured by the process according to the invention.
[0107] This heat treatment (xi) can, for example, be chosen from quenching, normal tempering and annealing, or even be a combination of these (quenching followed by normal tempering), this treatment being adapted to the specifications of the material(s) forming the first and second tube(s).
[0108] Furthermore, due to the phase change(s) that may occur during the heat treatment step (xi), geometric distortion of the double-walled heat exchanger tube is possible. A straightening step (xii) can then be considered to ensure the geometric conformity of this double-walled heat exchanger tube.
[0109] Other features and advantages of the invention will become apparent from the following example, which relates to the manufacture of a double-walled heat exchanger tube.
[0110] It is specified that this example is given only as an illustration of the object of the invention and does not in any way constitute a limitation of this object. [YES] DETAILED DESCRIPTION OF A PARTICULAR METHOD OF IMPLEMENTATION
[0112] A double-walled heat exchanger tube was manufactured by the process according to the invention.
[0113] Fabrication of tubes and strip
[0114] The first and second tubes intended to form respectively the outer tube and the inner tube of the double-walled heat exchanger tube were made of Eurofer-97 stainless steel, the composition of which (in mass percentage) is specified in Table 1 below. [Tables 1] V Cr Mn Ta W c N Fe 0.2 9 0.4 0.075 1.1 0.11 0.03 the remainder
[0115] These first and second tubes are seamless cylindrical tubes which were produced by a conventional industrial process from a blank made of Eurofer-97 steel which was drawn to obtain tubes with a length of 2.5 m and:
[0116] - for the first tube, a thickness of 1.45 mm and external and internal diameters respective 14.00 mm (diext) and 11.12 mm (dHnt), and
[0117] - for the second tube, a thickness of 1.20 mm and external and internal diameters respective of 10.62 mm (d2ext) and 8.2 mm (d2int).
[0118] The cylindrical tubular strip made of pure iron was prepared from pure iron marketed by the Liffs company under the name ARMCO® Pure Iron grade 4.
[0119] Tubular blanks of 500 mm in length and of respective outside and inside diameters of 16.22 mm and 12.57 mm were first machined by drilling and then by turning before being rolled.
[0120] The tubular blanks were then subjected to a first roller milling, followed by a first heat treatment at 850 °C for 1 h, then to a second roller milling followed by a second heat treatment at 850 °C for 1 h, then to a third roller milling followed by a third heat treatment at 850 °C for 1 hour and, finally, a fourth and final rolling with a pilgrim's step.
[0121] Following these rolling steps interspersed with heat treatment steps, the seamless tubular strip was obtained having a thickness of 100 pm and respective external and internal diameters of 10.97 mm (dext) and 10.77 mm (dint).
[0122] Surface preparation
[0123] The internal surface of the first tube intended to form the external tube was cleaned by means of Corundum sandblasting so as not to affect the internal diameter dHnt by more than 50 pm.
[0124] The external surface of the second tube intended to form the inner tube was brushed using a Scotch-Brite™ type abrasive brush so as not to affect the external diameter d2ext by more than 50 pm.
[0125] The internal and external surfaces of the first and second tubes, as well as the internal and external surfaces of the pure iron tubular strip, were carefully cleaned with a cloth and then with acetone.
[0126] Assembly of tubes and strip
[0127] The second tube and the tubular strip were then coaxially assembled inside the first tube, with the tubular strip being positioned between the first and second tubes.
[0128] Taking into account the respective external and internal diameters of the first and second tubes and of the tubular strip as obtained after the preparation of the different surfaces, a technical clearance of at least 150 °pm exists between the strip and the first tube, on the one hand, and between the strip and the second tube on the other hand, which obviously facilitates the assembly of these three elements.
[0129] Brazing of the assembly
[0130] The second inner tube was positioned so as to extend several centimeters beyond the first tube. The first and second tubes were then heated with an oxyacetylene torch before silver brazing was applied between them. It is specified that the silver brazing alloy has a content compatible with the steel of the first and second tubes, which contains 9% chromium by mass. The brazing alloy percolates through the gap between the tubes over the area heated by the torch. It should be noted that this brazing alloy is characterized by sufficient ductility to be co-formed with the tubes and the strip during the subsequent co-forming step.
[0131] Step-by-step cooling was then carried out in order to avoid generating a brittle martensitic structure.
[0132] Co-deformation of the assembly
[0133] The assembly was then subjected to a pilgrim step rolling.
[0134] Table 2 below shows the external and internal diameters (denoted external, internal and expressed in mm) of the first and second tubes and of the tubular strip before and after this step of co-deformation by pilgrim step rolling of the assembly.
[0135] [Tables2] Before co-deformation After co-deformation ^external ^internal ^external ^internal First tube 14.00 11.12 13.50 10.60 Strip 10.97 10.77 10.60 10.40 Second tube 10.62 8.20 10.40 8.00
[0136] Cutting and welding
[0137] The ends of the assembly as obtained at the end of the co-deformation step were cut to eliminate the end thermally affected by the brazing as well as the opposite end possibly affected by the percolation of the lubricating fluid.
[0138] The assembly was then cut into sections with a length compatible with the enclosure in which the hot isostatic compression (HIC) step was subsequently carried out.
[0139] The sections were then welded by a tungsten electrode welding process without filler material and under inert gas. This welding step is carried out without prior degassing, as the technical clearance between the tubes and the strip is very small after the co-deformation step.
[0140] Heat treatment by hot isostatic compression (HIC)
[0141] The sections were then placed in an enclosure to undergo a hot isostatic compression cycle conducted at a temperature of 1100 °C, at a pressure of 1200 bar (120 MPa), for 1 h.
[0142] Additional treatments
[0143] After the CIC step, the double-walled tube sections as obtained were cooled at a rate of 50 °C / h, giving them a ferritic metallurgical state (no martensite) allowing them to be bent like conventional tubes.
[0144] These tubes, thus shaped and welded, were then heat-treated by quenching and tempering.
[0145] The double-walled tube sections thus manufactured by the process according to the invention had an outside diameter of 13.50 mm (± 0.25 mm) and a thickness of 2.75 mm (± 0.35 mm).
[0146] The double-walled tube thus manufactured makes it possible to contain pressurized water at an average temperature of 325 °C, it being specified that each of the first and second tubes can, on its own, withstand the stresses related to water pressure. BIBLIOGRAPHY
[0147] [1] CN 203928838
[0148] [2] CN 113458737
Claims
Claims
1. A method of manufacturing a double-walled heat exchanger tube comprising an outer tube and an inner tube, the outer and inner tubes being metallic, cylindrical and coaxial, said manufacturing method being characterized in that it comprises the following successive steps (i) to (vii): (i) providing: . a first tube having an internal diameter diint and an external diameter diext, this first tube being intended to form the outer tube, . a second tube having an internal diameter d2int and an external diameter d2ext, this second tube being intended to form the inner tube, and .of a cylindrical and coaxial tubular strip made of Fe° having an internal diameter dint and an external diameter dext, such that 0.15 mm < (diint - dext) < 0.25 mm, 0.15 mm < (dint - d2ext) < 0.25 mm, and 10 pm < (dext - dint) < 200 pm; (ii) the coaxial assembly of the second tube and the strip inside the first tube, the strip being positioned between the first and second tubes; (iii) the brazing or bonding of one end of the assembly obtained at the end of step (ii); (iv) the co-deformation of the assembly obtained at the end of step (iii); (v) the cutting of the ends of the co-deformed assembly at the end of step (iv); (vi) welding the cut ends of the assembly obtained at the end of step (v); and (vii) heat treatment of the assembly obtained at the end of step (vi), this heat treatment being carried out by hot isostatic pressing, whereby the double-walled heat exchanger tube is obtained.
2. A method according to claim 1, wherein the first and second tubes provided in step (i) are weld-free, each of these first and second tubes having been advantageously obtained by carrying out, prior to step (i), the following successive steps (i0) and (ij): (i0) hot extrusion or hot rolling of a pierced rod, whereby a tubular blank is obtained, and (ii) cold drawing or pilgrim rolling of the tubular blank as obtained at the end of step (i0).
3. Method according to claim 1 or 2, in which the tubular strip provided in step (i) is weld-free and is advantageously obtained by carrying out, prior to step (i), the following successive steps (i2) to (i4): (i2) drilling an Fe° iron rod, (i3) turning the drilled rod as obtained at the end of step (i2), whereby a tubular blank is obtained, and (i4) pilgrim rolling the tubular blank as obtained at the end of step (i3).
4. The method of claim 3, wherein the pilgrim rolling step (i4) is repeated at least once, the method being further capable of comprising a heat treatment step (i4') preferably conducted between each step (i4) and, for example, at 850°C for 1 h.
5. Method according to any one of claims 1 to 4, further comprising a step of cleaning at least the internal surface of the first tube, the internal and external surfaces of the tubular strip and the external surface of the second tube, this cleaning step being carried out prior to step (ii) of coaxial assembly.
6. Method according to any one of claims 1 to 5, in which the co-deformation step (iv) is carried out by co-stretching or by co-rolling and, preferably, by pilgrim step co-rolling, of the assembly obtained at the end of step (iii).
7. A method according to any one of claims 1 to 6, which does not comprise a degassing step between the co-deformation step (iv) and the welding step (vi).
8. Method according to any one of claims 1 to 7, in which the welding step (vi) is carried out by an arc welding process with a non-consumable electrode, for example made of tungsten, and without adding material.
9. A method according to any one of claims 1 to 8, wherein step (vii) is carried out at a temperature of between 800°C and 1200°C, at a pressure of between 50 MPa and 200 MPa and for a time of between 30 min and 4 h.
10. A method according to any one of claims 1 to 9, further comprising, after step (vii), one or more of the following steps (viii) to (xii): (viii) cooling the double-walled heat exchanger tube, for example at a rate of 50°C / h; (ix) bending the double-walled heat exchanger tube obtained at the end of step (viii); (x) expanding the double-walled heat exchanger tube obtained at the end of step (viii) or (ix); (xi) heat treating the double-walled heat exchanger tube obtained at the end of step (ix) or (x), such as quenching or normalized tempering; and (xii) straightening the double-walled heat exchanger tube obtained at the end of step (ix), (x) or (xi).
11. A method according to any one of claims 1 to 10, wherein the first and second tubes are made of martensitic stainless steel, advantageously Eurofer-97 or T-91 steel.
12. A method according to any one of claims 1 to 11, wherein the materials of the first and second tubes are the same.
Citation Information
Patent Citations
Hot isostatic pressing preparation process of double-wall cooling pipe suitable for fusion reactor cladding
CN113458737A
Double-wall heat exchange tube comprising metal powder interlayer in molten salt heat exchanger
CN203928838U
Method for producing irregular-section composite pipe
CN101745793A
An aluminum-stainless steel composite tube for thermal control of space vehicles
CN104235515B
A hot isostatic pressing process for manufacturing double-walled cooling tubes suitable for fusion reactor blankets
CN113458737B