Polyethylene-based-resin composition and polyethylene-based-resin packaging material
The use of a specific copolymer A in the PE-based-resin composition addresses moldability and processability issues, enhancing film strength and productivity for PE-based-resin packaging materials, particularly when high inorganic compounds are involved, resulting in effective packaging solutions.
Patent Information
- Application Number
- GB2023003804
- Authority / Receiving Office
- GB · GB
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-16
- Filing Date
- 2020-09-16
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-09-16
AI Technical Summary
Existing PE-based-resin packaging materials face challenges in moldability and processability, especially when high amounts of inorganic compounds are present, leading to inferior film strength and bag-making performance.
A PE-based-resin composition containing a specific copolymer A is used, allowing for high inorganic compound incorporation while ensuring excellent moldability and film strength through appropriate molding and heat-sealing processes, such as inflation molding and T-die extrusion, with adjustable temperatures and film thickness.
The solution results in high productivity and robust packaging materials capable of handling heavy objects, with improved film moldability, bag-making processability, and film strength, even with high inorganic content.
Abstract
Description
Applications of the PE-based-resin packaging material are not particularly 5 limited, and a garbage bag, a shopping bag, a fashion bag, a storage bag, and a packing bag are exemplary examples.
[0031] As a method for producing the PE-based-resin packaging material according to the embodiment of the present invention, a known method can be adopted except that the 10 PE-based-resin composition according to the embodiment of the present invention is used. A method of molding the PE-based-resin composition according to the embodiment of the present invention into a film, and heat-sealing the film to make a bag is an exemplary example. As the method of molding into a film, inflation molding and T-die extrusion molding are exemplary examples. 15
[0032] The molding temperature (extrusion temperature) can be adjusted as appropriate, for example, 150°C or higher and 190°C or lower. The thickness of the film may be appropriately set according to the application, and can be, for example, 10 pm or more and 70 pm or less. 20
[0033] As described above, in the present invention, the PE-based-resin composition contains the specific copolymer A in a specific ratio. As a result, excellent moldability can be ensured even in a case where the amount of the inorganic compound is high, and a film excellent in bag-making processability and film strength is obtained. In addition, 25 the PE-based-resin packaging material obtained by using the PE-based-resin composition 15 05 24 according to the embodiment of the present invention can be produced with high productivity, and can withstand packaging and transportation of heavy objects.
[0034] Hereinafter, the present invention will be described in detail with reference to 5 Examples, but the present invention is not limited to the following description.
[0035] [Abbreviation] The following abbreviations have the following meanings. (Copolymer A) 10 A-l: C6-LLDPE, trade name “Novatec (RTM) SF720”, manufactured by Japan Polyethylene Corporation, MFR: 0.8 g / 10 min, melting point: 124°C A-2: C6-LLDPE, trade name “Harmolex NC564A”, manufactured by Japan Polyethylene Corporation, MFR: 3.5 g / 10 min, melting point: 124°C A-3: C6-LLDPE, trade name “D139FK”, manufactured by Chevron Phillips 15 (RTM) Chemical Company LLC., MFR: 1.0 g / 10 min, melting point: 90°C A-4: C6-LLDPE, trade name “Evolue (registered trademark) 2320”, manufactured by Prime Polymer Co., Ltd., MFR: 1.8 g / 10 min, melting point: 118°C A-5: C8-LLDPE, trade name “Moretec (registered trademark) 0168N”, manufactured by Prime Polymer Co., Ltd., MFR: 1.2 g / 10 min, melting point: 125°C 20 A-6: C8-LLDPE, trade name “O138NK”, manufactured by Prime Polymer Co., Ltd., MFR: 1.5 g / 10 min, melting point: 117°C
[0036] (Other polymer B) B-l: C4-LLDPE, trade name “FS153S”, manufactured by Sumitomo (RTM) 25 Chemical Asia Pte Ltd. 15 05 24 B-2: C6-LLDPE, trade name “TZ050”, manufactured by TOSOH (RTM) CORPORATION, MFR: 0.5 g / 10 min, melting point: 119°C B-3: C6-LLDPE, trade name “Harmolex NH645A”, manufactured by Japan Polyethylene Corporation, MFR: 8.0 g / 10 min, melting point: 121°C 5 B-4: HDPE, trade name “FJ00952”, manufactured by SABIC (RTM)
[0037] [Production Example 1] 80% by mass of calcium carbonate (Lighten BS-0, average particle size: 1.0 pm, manufactured by BIHOKU FUNKA KOGYO CO., LTD.) and 20% by mass of pellets of 10 the copolymer A-5 (C8-LLDPE) were mixed in a super mixer for 5 minutes, the mixture was extruded into strands with a twin-screw extruder, and the strands were cut into pellets to obtain a masterbatch (MB-1).
[0038] [Production Example 2] 15 A masterbatch (MB-2) was obtained in the same manner as in Production Example 1, except that the copolymer A-4 (C6-LLDPE) was used instead of the copolymer A-5.
[0039] [Production Example 3] 20 A masterbatch (MB-3) was obtained in the same manner as in Production Example 1, except that the polymer B-l (C4-LLDPE) was used instead of the copolymer A-5.
[0040] [Example 1] 25 As an inflation molding machine, an extruder (manufactured by Placo Co., Ltd.) 15 05 24 having a cylinder inner diameter of 55 mm and a screw L / D of 32, and an annular die having a die diameter of 100 runup and a lip of 3 mm were used. Each of raw materials was weighed so that MB-1 was 65% by mass and the polymer B-l (C4-LLDPE) was 35% by mass and fed into the extruder to prepare a PE-5 based-resin composition, and a tubular film having a thickness of 30 pm and a folding width of 460 mm was molded by inflation molding. The extrusion temperature was 170°C, and the blow ratio was approximately 3.0. Next, the film was heat-sealed at intervals of 600 mm in a longitudinal direction by a bag-making machine (manufactured by Nozaki Kogyo Co., Ltd.), and was cut to produce a bag. The heat-sealing 10 temperature was 160°C or higher and 180°C or lower. The amount of calcium carbonate in the film (PE-based-resin composition) was 52% by mass, and the amount of the copolymer A was 13% by mass.
[0041] [Examples 2 to 6] 15 Bags were produced in the same manner as in Example 1, except that the composition of the PE-based-resin composition was changed as shown in Table 1.
[0042] [Examples 7 to 10] Bags were produced in the same manner as in Example 1, except that the 20 composition of the PE-based-resin composition was changed as shown in Table 1 and the thickness of the film was 20 pm.
[0043] [Comparative Examples 1 to 5] Bags were produced in the same manner as in Example 1, except that the 25 composition of the PE-based-resin composition was changed as shown in Table 2. 15 05 24 [Film moldability] The stability of the tube during film molding of each example was confirmed, and the moldability was evaluated according to the following standard. 5 “1”: more stable than normal resin (containing no inorganic compound) “2”: stable like normal resin “3”: slightly more unstable than normal resin, but capable of being continuously molded “4”: unstable and not capable of being molded 10
[0045] [Bag-making processability] The production speed during bag making and the finished shape of the sealed portion were confirmed, and the moldability was evaluated according to the following standard. 15 “1”: the production speed and the finish of the sealed portion were improved as compared with a case without the inorganic substance. “2”: the production speed and the finish of the sealed portion were equivalent to a case without the inorganic substance. “3”: the finish of the seal shape was poor as compared with a case without the 20 inorganic substance. “4”: the production speed was very inferior to a case without the inorganic substance.
[0046] [Film strength] 25 The film molded in each example was pierced with a thumb, and the spread of 15 05 24 the tear was observed in a case where force was applied to the pierced hole, and the film strength was evaluated according to the following standard. (Evaluation standard) “1”: the film could not be easily pierced. 5 “2”: the tear did not spread from the pierced hole. “3”: the tear spread from the pierced hole. “4”: a finger could be easily pierced.
[0047] Tables 1 and 2 show the composition of the PE-based-resin composition, the 10 thickness of the film, and the evaluation results of each example. In Tables 1 and 2, “LLDPE (C6 to C8)” indicates LLDPE in which the number of carbon atoms in a-olefin was 6 to 8. “CaCoa content” indicates the amount of calcium carbonate in the PE-based-resin composition (film). “LLDPE (C6 to C8) content” indicates the total amount of LLDPE in which the number of carbon atoms in a- 15 olefin in the PE-based-resin composition (film) was 6 to 8. “Copolymer A content” indicates the amount of the copolymer A in the PE-based-resin composition (film). “1.0, 1.2” in the column of MFR indicates that LLDPE having an MFR of 1.0 g / 10 min and LLDPE having an MFR of 1.2 g / 10 min were used in combination, and the same applies to other columns. “90, 118” in the column of melting point indicates that 20 LLDPE having a melting point of 90°C and LLDPE having a melting point of 118 °C were used in combination, and the same applies to other columns. [Table 1] 15 05 24 Example 1 2 3 4 5 6 7 8 9 10 Copolymer A A-l (C6-LLDPE) 35 A-2 (C6-LLDPE) 20 A-3 (C6-LLDPE) 25 10 10 25 30 A-6 (C8-LLDPE) 15 Other polymer B-l (C4-LLDPE) 35 10 20 25 20 B-2 (C6-LLDPE) B-3 (C6-LLDPE) B-4 (HDPE) 20 15 5 10 5 Masterbatch MB-1 (A-5 (C8-LLDPE): 20 wt%) 65 65 65 65 65 65 65 MB-2 (A-4 (C6-LLDPE): 20 wt%) 65 65 80 MB-3 (B-l (C4-LLDPE): 20 wt%) MFR of LLDPE (C6 to C8) [10 g / min] 1.2 1.0, 1.8 1.8, 1.5 1.2, 3.5 0.8, 1.2 1.8 1.0, 1.2 1.0, 1.2 1.0, 1.2 1.0, 1.2 Melting point of LLDPE (C6 to C8) [°C] 125 90, 118 117, 118 124, 125 124, 125 127 90, 125 90, 125 90, 125 90, 125 CaCOs content [% by mass] 52 52 52 52 52 64 52 52 52 52 LLDPE (C6 to C8) content [% by mass] 13 38 28 38 48 16 25 25 38 43 Copolymer A content [% by mass] 13 38 28 38 48 16 25 25 38 43 Film thickness [pm] 30 30 30 30 30 30 20 20 20 20 Film moldability 2 2 2 2 2 2 2 1 1 1 Bag-making processability 2 2 2 2 2 2 2 1 1 1 Film strength 2 2 2 2 2 2 1 2 2 2 [Table 2] 15 05 24 Comparative Example 1 2 3 4 5 Copolymer A A-l (C6-LLDPE) A-2 (C6-LLDPE) A-3 (C6-LLDPE) A-6 (C8-LLDPE) Other polymer B-l (C4-LLDPE) 35 35 B-2 (C6-LLDPE) 35 B-3 (C6-LLDPE) 35 B-4 (HDPE) 20 Masterbatch MB-1 (A-5 (C8-LLDPE): 20 wt%) MB-2 (A-4 (C6-LLDPE): 20 wt%) 30 MB-3 (B-l (C4-LLDPE): 20 wt%) 65 80 65 65 35 MFR of LLDPE (C6 to C8) [10 g / min] - - 8.0 0.5 1.8 Melting point of LLDPE (C6 to C8) [°C] - - 121 119 127 CaCOs content [% by mass] 52 64 52 52 52 LLDPE (C6 to C8) content [% by mass] 0 0 35 35 6 Copolymer A content [% by mass] 0 0 0 0 6 Film thickness [pm] 30 30 30 30 30 Film moldability 2 2 4 3 2 Bag-making processability 2 2 4 3 2 Film strength 4 4 4 4 3
[0050] As shown in Tables 1 and 2, in Examples 1 to 10 in which the PE-based-resin 5 composition contained the copolymer A in a specific ratio, the film moldability, the bagmaking processability, and the film strength were all excellent. On the other hand, in Comparative Examples 1 to 4 in which the PE-based-resin composition did not contain the copolymer A, and in Comparative Example 5 in which the amount of the copolymer A in the PE-based-resin composition was small, one or 10 more of the film moldability, the bag-making processability, and the film strength was inferior.
Claims
1. A polyethylene-based-resin composition comprising:5 an inorganic compound;an ethylene-a-olefin copolymer, anda high-density polyethylene,wherein:10 the inorganic compound is calcium carbonate;at least a part of the ethylene-a-olefin copolymer is an ethylene-a-olefin copolymer A in which a-olefin has 6 to 8 carbon atoms and a melt flow rate is 1.0 g / 10 min or more and 2.0 g / 10 min or less,an amount of the inorganic compound is 50% by mass or more and 80% by mass15 or less with respect to a total mass of the resin composition,an amount of the ethylene-a-olefin copolymer A is 10% by mass or more and 45% by mass or less with respect to the total mass of the resin composition; andan amount of the high-density polyethylene is 5% by mass or more and 15% by mass or less with respect to the total mass of the resin composition.20
2. The polyethylene-based-resin composition according to Claim 1,wherein the ethylene-a-olefin copolymer A has a melting point of 90°C or higher and 130°C or lower.25
3. A polyethylene-based-resin packaging material formed from the polyethylene-CXIo LObased-resin composition according to Claim 1 or 2.
4. The polyethylene-based-resin packaging material according to Claim 3, wherein the polyethylene-based-resin packaging material is for a garbage bag, a5 shopping bag, a fashion bag, a storage bag, or a packing bag.
Citation Information
Patent Citations
Resin composition comprising recovered polyethylene terephthalate resin and film produced from the same resin composition
JP2000256517A
Composition for inorganic-filled polyethylene film
JP1993017636A
Garbage bag
JP1995206005A