Method for improving strength, toughness, and uniformity of non-quenched and tempered steel with ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling

GB2626218BActive Publication Date: 2026-11-05JIANGSU YONGGANG GROUP CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
GB2023016838
Authority / Receiving Office
GB · GB
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-28
Filing Date
2022-12-16
Publication Date
2026-11-05
Estimated Expiration
2042-12-16

Smart Images

  • Figure 00000001_0000
    Figure 00000001_0000
  • Figure 00000001_0001
    Figure 00000001_0001
  • Figure 00000001_0002
    Figure 00000001_0002
Patent Text Reader

Abstract

Disclosed is a method for improving strength, toughness and uniformity of ultra-large-section non-quenched and tempered steel by cooperative regulation and control of multi-stage precipitation and con
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to a method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling, and belongs to the technical field of metal materials. BACKGROUND

[0002] Compared with quenched and tempered steels, non-quenched and tempered steels have advantages such as low cost, environmental friendliness, and operation friendliness, and are widely used in fields such as automobiles and engineering machinery. Compared with non-quenched and tempered steels for hot forging, non-quenched and tempered steels for direct cutting can achieve required mechanical properties when rolled into round bar steels, which can further shorten a production process. Generally, non-quenched and tempered steels for direct cutting can be used merely after procedures such as smelting and solidification, continuous rolling into round bar steels, and downstream cutting, which can further improve the cost and environmental protection advantages. Currently, the production of non-quenched and tempered steels for direct cutting that have high strength / toughness matching performance and a large cross-sectional area is an important development direction, and has promising application prospects. However, the increase of a cross-sectional area will significantly increase the difficulty in improving the strength and toughness of a non-quenched and tempered steel and ensuring the cross-sectional uniformity of a non-quenched and tempered steel.

[0003] Due to large core / surface temperature difference and poor deformation penetration during a rolling process of a non-quenched and tempered steel with an ultra-large cross section, there is a small reduction of area before and after rolling, and it easily causes a coarse structure and poor strength and toughness of a core of a rolled round bar steel, a significant difference between structures of the core and a surface, and poor cross-sectional uniformity, which makes performance of the core fail to meet standards while making it difficult to achieve machining of the surface of the round bar steel. Major reasons for a large core / surface difference of a round bar steel with an ultralarge cross section are as follows: (1) During high-temperature rolling, a core has poor deformation penetration, a small deformation amount, and coarse recrystallized grains; and a surface has a large deformation amount and fine recrystallized grains. (2) During medium- and low-temperature rolling, a core has a high temperature and is in a recrystallization zone, and in this zone, austenite grains still grow, and a new phase is nucleated only at an austenite grain boundary during cooling, resulting in a coarse structure; and a surface has a low temperature and is in a non-recrystallization zone, and in this zone, defects of deformed austenite grains increase significantly, and a new phase can be nucleated at an austenite grain boundary and an internal defect during cooling, resulting in a fine structure. (3) During cooling after rolling, a core has a small temperature drop and a high transition temperature, and there is a large interlamellar spacing among pearlite sheets; and a surface has a large temperature drop and a low transition temperature, and there is a small interlamellar spacing among pearlite sheets. The above three factors all make a non-quenched and tempered steel with an ultra-large cross section have a coarse core structure and a fine surface structure. After superposition of the above three factors, a core / surface difference increases significantly.

[0004] The structure and performance of a non-quenched and tempered steel are commonly regulated with microalloying elements such as Ti, Nb, V, N, and Al. However, the above means is mainly used in a controlled forging / controlled cooling process for producing a component from a non-quenched and tempered round bar steel for hot forging; and there are few studies on the use of the above means in rolling of a round bar steel for direct cutting and the influence of the above means on the structure and performance of the round bar steel. A rolling process is significantly different from a forging process.

[0005] Chinese Patent Publication No. CN113621882A discloses that the mechanical properties and surface quality of a round bar steel can be controlled by controlling contents of microalloying elements and a ratio of the microalloying elements, but does not involve the accurate control of a rolling process. Chinese Patent Publication No. CN104043660A and Chinese Patent Publication No. CN114472519A disclose that the cross-sectional uniformity of a non-quenched and tempered steel can be improved by controlling a through-water process after finish rolling of a round bar steel, but do not consider specific roles of different microalloying elements during a steel rolling process. Chinese Patent Publication No. CN113122776A, Chinese Patent Publication No. CN113122776A, and Chinese Patent Publication No. CN113134510B each disclose a composition range and a rolling process for non-quenched and tempered steels with medium and large cross sections for direct cutting, but do not consider a synergistic control role of a precipitated phase and a rolling process. Moreover, none of the above patents considers structural evolution characteristics of a nonquenched and tempered round bar steel with an ultra-large cross section (diameter: 160 mm or more) during a rolling process.

[0006] Therefore, it is necessary to develop a method for optimizing strength, toughness, and crosssectional uniformity of a ferritic-pearlitic non-quenched and tempered steel with an ultra-large cross section for direct cutting through synergistic regulation of microalloying element precipitation and a controlled rolling / controlled cooling process. SUMMARY

[0007] A technical problem to be solved by the present disclosure is to improve strength, toughness, and cross-sectional uniformity of a ferritic-pearlitic non-quenched and tempered steel with an ultra-large cross section of a diameter of 160 mm to 300 mm for direct cutting through a synergistic effect of a multi-stage precipitation process of microalloying elements and a controlled rolling / controlled cooling process.

[0008] To solve the above technical problem, the present disclosure adopts the following technical solutions. A method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section having a diameter of 160 mm to 300 m through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling is provided, specifically including the following steps: S1: continuously heating a continuous casting billet using a stepping heating furnace, the stepping heating furnace comprising a hot-rolling line, and included a preheating section, a first heating section, a second heating section, and a soaking section, where a temperature of the second heating section is 1,230°C to 1,250°C, a temperature of the soaking section is 1,210°C to 1,230°C, and a total time of maintaining the continuous casting billet in the second heating section and the soaking section is no less than 5 h, to ensure that all microalloying elements except for some TiN are dissolved in an austenite and undissolved TiN inhibits a growth of austenite grains; S2: after the continuous heating, descaling the continuous casting billet with water, and watercooling or naturally-cooling the continuous casting billet until a surface temperature of the continuous casting billet is lower than 1,100°C, to ensure that a surface hardness of the continuous casting billet is significantly higher than a hardness of a high-temperature metal of a core of the continuous casting billet; S3: subjecting the continuous casting billet to rough rolling with a reversible rough rolling machine to obtain an intermediate billet, having a square cross-section defining four adjacent vertical sides of the square cross-section (A, B, C, D) and a side length of 230 mm to 450 mm, wherein first two passes of rolling are conducted for two adjacent vertical sides (A, B; C,D) of the continuous casting billet, with a depression distance of 5 mm to 10 mm per pass; and subsequent 4 to 6 consecutive passes of rolling are conducted alternately for the two adjacent vertical sides (A, B; C, D) of the continuous casting billet, where alternate rolling means that two adjacent passes alternately roll the two adjacent vertical sides, with a deformation amount of higher than or equal to 20% per pass; and a finishing temperature of the rough rolling is higher than 1,050°C; S4: water-cooling or naturally-cooling the intermediate billet until a surface temperature of the intermediate billet is 900°C to 950°C, where TiN is completely precipitated and NbN and AlN are partially precipitated; S5: rolling the intermediate billet into a round bar steel through continuous finish rolling with a finishing temperature of 780°C to 820°C, where nitrides of Ti, Nb, and Al are completely precipitated; S6: immediately subjecting the round bar steel to 6 to 8 stages of forced through-water cooling until a surface temperature of the round bar steel is 550°C to 600°C, where air cooling is conducted for 5 s to 10 s between every two adjacent ones of the stages of the forced through-water cooling, a surface temperature drop of the round bar steel after each of the stages of the forced through-water cooling is not larger than 100°C, and then spraying the round bar steel with a water mist, to maintain the surface temperature of the round bar steel at 550°C to 600°C, where V is mainly precipitated in a form of VC; and S7: cooling the round bar steel by a stepping cooling bed with a straightening function until the surface temperature of the round bar steel is 300°C to 350°C, and incubating the round bar steel in a pit for at least 48 h to obtain a finished product.

[0009] In the method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling, the round bar steel includes the following chemical components in mass percentages: C: 0.35% to 0.45%, Si: 0.30% to 0.90%, Mn: 1.10% to 1.60%, V: 0.10% to 0.20%, Nb: 0.03% to 0.04%, Ti: 0.015% to 0.030%, Al: 0.10% to 0.30%, N: 0.008% to 0.020%, S: 0.01% to 0.04%, P: less than or equal to 0.02%, and Fe and unavoidable impurities: the balance.

[0010] Preferably, a mass percentage of Ti is 0.020% to 0.028%, a Ti / N mass percentage ratio is lower than 3.4, and a (Ti+Nb+Al) / N mass percentage ratio is higher than 12.5.

[0011] In the method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling, the continuous casting billet is a square or rectangular billet with a side length of 400 mm to 1,000 mm, and the intermediate billet is a square billet with a side length of 230 mm to 450 mm; and the round bar steel after the rolling has a diameter of 160 mm to 300 mm, a longitudinal tensile strength of 900 MPa to 1,050 MPa, a yield strength of 650 MPa to 800 MPa, an elongation at break of 15% to 19%, and an impact work KU2 of 40 J to 50 J at a 1 / 4 radius and a core.

[0012] The present disclosure has the following new features. (1) Through the synergistic regulation 4 of types and contents of alloying elements in a non-quenched and tempered steel and a controlled rolling / controlled cooling process, different types of precipitated phases can be precipitated in stages, which coordinates with the structural evolution during hot-rolling and subsequent cooling to improve the cross-sectional uniformity of a round bar steel while improving its strength and toughness. (2) High-temperature heating, low-temperature break-down rolling, and continuous single-pass large deformation are adopted for a rough rolling process to fully achieve deformation penetration and improve the cross-sectional uniformity during the rough rolling process. (3) Natural cooling before rolling and low-temperature break-down rolling are adopted for a finish rolling process, such that the whole cross section is rolled in a non-recrystallization zone. (4) After the finish rolling, a forced water cooling + alternate air cooling + water mist-controlled cooling mode is adopted to improve the uniformity of room-temperature structures and properties of the whole cross section.

[0013] Roles and proportion bases of the elements in the present disclosure are as follows. C is a basic element in a non-quenched and tempered steel. In addition to producing a sufficient proportion of a pearlite, a part of C enters carbonitrides of microalloying elements to play roles of fine crystal strengthening and precipitation strengthening. A too-low carbon content will lead to an insufficient strength of a steel, and a too-high carbon content will make an elongation at break and an impact work of a steel insufficient. Therefore, the C content of the present disclosure is 0.35% to 0.45%.

[0014] Si is a basic element for strengthening a ferrite. With the increase of a silicon content in a steel, a strength of the steel increases, and the plasticity of the steel decreases. The Si content of the present disclosure is 0.30% to 0.90%.

[0015] Mn can strengthen a matrix, increase a proportion of a pearlite, and reduce an interlamellar spacing among pearlite sheets, thereby improving the strength and toughness. MnS can be produced from Mn to improve the cutting performance. The Mn content of the present disclosure is 1.10% to 1.60%.

[0016] Ti can be combined with N and then precipitated in a form of TiN to refine austenite grains. After the non-quenched and tempered steel is incubated at 1,250°C for a long time, a large amount of TiN is still not dissolved, which prevents the growth of austenite grains, thereby refining the roomtemperature structures and improving the strength and toughness. Generally, a content of Ti in a nonquenched and tempered steel is 0.01% to 0.02%. Because a non-quenched and tempered steel with an ultra-large cross section requires a high heating temperature and a long holding time before rolling, an increased amount of Ti is required to ensure that grains are still not coarse during high-temperature soaking. Therefore, the Ti content of the present disclosure is 0.015% to 0.030%. Preferably, a mass percentage of Ti is 0.020% to 0.028%.

[0017] Nb can increase a recrystallization temperature of an austenite and refine the room-5 temperature structures. Generally, about 0.02% to 0.03% of Nb is added in a non-quenched and tempered steel. Only a sufficient amount of solid-solution Nb atoms can increase a recrystallization temperature of an austenite to about 1,000°C, and in order to ensure that the whole cross section of an intermediate billet is in an austenite non-recrystallization zone during finish rolling, it is necessary to increase a content of solid-solution Nb in a steel. Therefore, the Nb content of the present disclosure is 0.030% to 0.040%.

[0018] In addition to playing a deoxidation role, Al can produce AlN to play roles of fine crystal strengthening and precipitation strengthening, and AlN usually begins to be precipitated in a large quantity when a temperature is lower than 1,100°C. In order to improve an effect of grain refinement during rough rolling, the Al content of the present disclosure is 0.10% to 0.30%.

[0019] V is a major element for precipitation strengthening. A temperature for precipitation of VN in a large quantity is about 900°C, and a temperature for precipitation of VC in a large quantity is 700°C to 800°C, where VC with a lower precipitation temperature is fine and diffuse. With the increase of a strength, a content of V in a ferritic-pearlitic non-quenched and tempered steel gradually increases, and is generally as high as about 0.1%. A cooling rate of a non-quenched and tempered steel with an ultra-large cross section after rolling is low, and thus a V content needs to be appropriately increased to produce sufficient carbonitrides to ensure a strength. Therefore, the V content of the present disclosure is 0.10% to 0.20%.

[0020] N can be used to produce carbonitrides of microalloying elements to refine austenite grains, and the carbonitrides can be precipitated to form a second phase for strengthening. An atomic weight ratio of Ti to N, an atomic weight ratio of Nb to N, and an atomic weight ratio of Al to N are 3.4, 6.6, and 1.9, respectively. A solid-solution temperature of a nitride of a microalloying element is significantly higher than a solid-solution temperature of a carbide of the same microalloying element. In order to ensure an effect of grain refinement during heating and rough rolling, Ti exists in a steel completely in a form of a nitride, and a Ti / N mass percentage ratio should be lower than 3.4. In addition, in order to obtain increased fine and diffuse VC, it is necessary to ensure that N is fixed by Ti, Nb, and Al as much as possible, and a (Ti+Nb+Al) / N mass percentage ratio is higher than 12.5. Therefore, the N content of the present disclosure is 0.008% to 0.020%.

[0021] S can be combined with Mn to produce MnS to improve the cutting performance of a nonquenched and tempered steel. Generally, a content of S in a non-quenched and tempered steel is 0.03% to 0.40%. A too-high S content will damage the transverse mechanical properties, and thus it is necessary to reduce an S content appropriately. Therefore, the S content of the present disclosure is 0.01% to 0.04%.

[0022] P is an impurity element in a steel and may promote the occurrence of cold shortness, and thus a total content of P in a non-quenched and tempered steel with an ultra-large cross section 6 needs to be strictly controlled. Therefore, the P content of the present disclosure is not higher than 0.02%.

[0023] The present disclosure mainly has the following beneficial effects. (1) For a non-quenched and tempered steel with an ultra-large cross section of a diameter of 160 mm to 300 mm for direct cutting after rolling, the present disclosure adopts the synergistic regulation of multi-stage precipitation of microalloying elements and a controlled rolling / controlled cooling process to give full play to grain refinement roles of TiN, NbN, and AlN during heating and rough rolling of a casting billet, a role of solid-solution Nb in increasing a temperature of a recrystallization zone during finish rolling, and a precipitation strengthening role of VC during controlled cooling after rolling, which can fully refine core structures and a VC size of a round bar steel, and significantly improve the uniformity of structures and performance of a core and a surface while improving the strength and toughness of the core.

[0024] (2) Through the synergistic regulation of multi-stage precipitation of microalloying elements and a controlled rolling / controlled cooling process, the present disclosure achieves the dynamic recrystallization rolling of a whole-cross-section austenite during rough rolling to distribute increased deformation to a core, thereby improving a refinement degree of a core and the core / surface uniformity. The non-dynamic recrystallization rolling of a whole-cross-section austenite is allowed during finish rolling to distribute increased deformation to a core, thereby improving a defect density of a core and the core / surface uniformity. The cooling after rolling can reduce a temperature of a core as soon as possible, such that the core and a surface are transformed under the same original structure and temperature, which improves the uniformity of roomtemperature structures and properties while improving the strength and toughness.

[0025] The present disclosure discloses a method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling. The multi-stage precipitation of precipitated phases is allowed through synergistic regulation of contents of Ti, Nb, Al, V, and N and a ratio of the elements and a controlled rolling / controlled cooling process, which coordinates with the structural evolution during rough rolling, finish rolling, and cooling after rolling to refine high-temperature and room-temperature structures of a core of a round bar steel. The method of the present disclosure can improve strength, toughness, and cross-sectional uniformity of a non-quenched and tempered steel with an ultra-large cross section of a diameter of 160 mm to 300 mm for direct cutting. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] FIG. 1 shows microstructure images of the rolled metal in Comparative Example 1, where (a) 7 shows a microstructure at a 1 / 4 radius from a surface and (b) shows a microstructure of a core. FIG. 2 shows microstructure images of the rolled metal in Example 1, where (a) shows a microstructure at a 1 / 4 radius from a surface and (b) shows a microstructure of a core. FIG. 3 shows microstructure images of the rolled metal in Example 2, where (a) shows a microstructure at a 1 / 4 radius from a surface and (b) shows a microstructure of a core. FIG. 4 shows test results of undissolved TiN in a continuous casting billet after heating, where (a) is a morphological image and (b) is an element analysis graph. FIG. 5 shows test results of TiN and NbN precipitated during rough rolling, where (a) is a morphological image and (b) is an element analysis graph. FIG. 6 shows test results of TiN, NbN, and AlN precipitated in an intermediate billet during watercooling or natural cooling, where (a) is a morphological image of TiN and NbN, (b) is an element analysis graph of TiN and NbN, (c) is a morphological image of AlN, and (d) is an element analysis graph of AlN. FIG. 7 shows test results of NbN and AlN precipitated during continuous finish rolling, where (a) is a morphological image, (b) is an element analysis graph of NbN, and (c) is an element analysis graph of AlN. FIG. 8 shows test results of VC precipitated during cooling after rolling, where (a) is a morphological image and (b) is an element analysis graph. FIG. 9 shows the morphology of an interlamellar spacing among pearlite sheets in a finished round bar steel product. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0027] The present disclosure is further described in detail below with reference to the accompanying drawings and specific examples. The following examples are only intended to illustrate the present disclosure, rather than to limit the scope of the present disclosure.

[0028] Reference Example 1 A method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling was provided. In this method, a continuous casting billet included the following chemical components in mass percentages: C: 0.38%, Si: 0.60%, Mn: 1.39%, P: 0.01%, S: 0.03%, Ti: 0.020%, Nb: 0.033%, Al: 0.12%, V: 0.15%, N: 0.012%, and Fe and unavoidable impurities: the balance, where Ti / N = 1.67 and (Ti+Nb+Al) / N = 14.42; and the continuous casting billet had a cross-sectional size of 430 mm x 480 mm.

[0029] The method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling included the following steps: The continuous casting billet was heated by a stepping heating furnace, where a temperature of a second heating section was 1,250°C, a temperature of a soaking section was 1,230°C, and a total time of maintaining the temperature of the second heating section and the temperature of the soaking section was 5.5 h. The continuous casting billet was descaled with water, then water-cooled or naturally cooled until a surface temperature of the continuous casting billet was 1,080°C, and rolled by a reversible rough rolling machine to obtain a square billet with a side length of 240 mm, where first two passes of rolling were conducted for two vertical sides of the continuous casting billet, with a depression distance of 10 mm per pass; subsequent 5 passes of rolling were conducted alternatively for two sides of the continuous casting billet, with a depression distance of 100 mm in total; and a finishing temperature was 1,080°C. The intermediate billet was water-cooled or naturally cooled until a surface temperature of the intermediate billet was 930°C, and then rolled by a continuous finish rolling machine to obtain a round bar steel with a diameter of 180 mm, where a finishing temperature was 800°C. The round bar steel was subjected to 6 alternate stages of forced through-water cooling, then sprayed with a water mist until a surface temperature of the round bar steel was 570°C, then aircooled on a cooling bed to 330°C, and incubated in a pit for 48 h to obtain a finished product.

[0030] The structure grades and mechanical properties of a core and a position at a 1 / 4 radius of the round bar steel in this example are shown in Table 1.

[0031] A principle of synergistic regulation of multi-stage precipitation of microalloying elements and controlled rolling / controlled cooling in this example is as follows. (1) In order to ensure fine core structures of a continuous casting billet with an ultra-large cross section during rough rolling and reduce the non-uniformity of a core and a surface, the following measures are taken: A. Heating and soaking temperatures for the continuous casting billet are increased, and the deformation resistance for the core of the continuous casting billet is reduced; and enough TiN is added to prevent the growth of austenite grains during heating.

[0032] B. After water-descaling, the continuous casting billet is water-cooled or naturally cooled until a surface temperature of the continuous casting billet was 1,080°C to increase a surface hardness, but a temperature of the core of the continuous casting billet is almost not reduced, and the core has a low hardness. During rough rolling, the surface deformation is small, and a large amount of deformation occurs in the core to fully refine austenite grains in the core. TiN and a small amount of NbN that are gradually precipitated can also prevent the growth of austenite grains during hot-rolling.

[0033] C. First two passes of small-deformation rough rolling are conducted to remove oxide scales and other defects on the surface, and subsequent passes of large-deformation rough rolling ensure 9 that the deformation fully penetrates into the core to refine austenite grains in the core.

[0034] D. A finishing temperature of the rough rolling is higher than 1,050°C, to ensure that both the core and the surface are rolled in an austenite recrystallization zone.

[0035] Measures at the heating and rough rolling stages of the continuous casting billet are taken mainly to refine austenite grains and improve toughness and cross-sectional uniformity of a round bar steel. As shown in FIG. 4, TiN of 3 pm to 5 pm is retained at the heating stage of the continuous casting billet, and can play roles of refining original structures and improving toughness. As shown in FIG. 5, TiN and NbN of 1 pm to 3 pm are precipitated during the rough rolling, and can play roles of recrystallized grain refinement, toughness improvement, and precipitation strengthening.

[0036] (2) In order to ensure fine core structures of the intermediate billet during finish rolling and reduce the non-uniformity of a core and a surface, the following measures are taken: A. During the water-cooling or natural-cooling of the intermediate billet until a surface temperature of the intermediate billet is 930°C, TiN is completely precipitated and NbN and AlN are partially precipitated, which can increase a defect density during finish rolling and refine roomtemperature structures. Solid-solution Nb is retained in the core and can increase an austenite recrystallization temperature, such that both the core and the surface are in an austenite nonrecrystallization zone during finish rolling, which can reduce a difference between the structural evolution of the core and the structural evolution of the surface. In addition, the natural cooling makes the surface of the intermediate billet hard and the core of the intermediate billet soft, which is conducive to the penetration of deformation into the core and can refine core structures.

[0037] B. Continuous finish rolling is conducted with a finishing temperature of 800°C, and during the continuous finish rolling, nitrides of Ti, Nb, and Al are completely precipitated, which further strengthens an interaction between precipitated phases and deformation defects, improves a defect density, refines room-temperature structures, and improves strength and toughness of a round bar steel.

[0038] Measures at the natural cooling and finish rolling stages of the intermediate billet are taken mainly to refine room-temperature structures and improve toughness and cross-sectional uniformity of a round bar steel. As shown in FIG. 6, TiN, NbN, and AlN of 500 nm to 1 pm are precipitated at the natural cooling stage of the intermediate billet, and can play roles of refining austenite grains and improving toughness. In FIG. 6, (a) and (b) are for NbN, and (c) and (d) are for AlN. As shown in FIG. 7, NbN and AlN of 100 nm to 500 nm are precipitated during the finish rolling, and can improve a defect density of an austenite and refine room-temperature structures, thereby improving toughness; and in (a), a point indicated by the lower right arrow refers to NbN, and a point indicated by the upper left arrow refers to AlN. The above precipitated phases can also play a role of precipitation strengthening.

[0039] (3) In order to ensure fine core structures during cooling after rolling and reduce the non-10 uniformity of a core and a surface, the following measures are taken. A. The round bar steel obtained after final rolling is immediately subjected to 6 stages of forced through-water cooling until a surface temperature of the round bar steel is 570°C, where air cooling is conducted among the stages of forced through-water cooling, and a surface temperature drop of the round bar steel after each stage of forced through-water cooling is not larger than 100°C. The above operation can quickly reduce a temperature of a core of the round bar steel, inhibit the structural transformation of the core, and force fine and diffuse VC to be precipitated in the core at a low temperature, thereby improving strength and toughness of the core and reducing a core / surface difference. In addition, the above operation can avoid the appearance of non-equilibrium structures such as a bainite and a martensite due to a too-low temperature on the surface of the round bar steel.

[0040] B. The round bar steel is then subjected to 2 stages of water mist spraying to maintain a surface temperature of the round bar steel at 570°C. The water mist spraying can further remove heat of the core, such that both the surface and the core of the round bar steel are cooled to 570°C and then begin to undergo structural transformation. The core and the surface have similar ferrite amounts, similar interlamellar spacings among pearlite sheets, and improved strength and toughness, and the uniformity of the core and the surface is improved.

[0041] C. The round bar steel is cooled by a stepping cooling bed with a straightening function until a surface temperature of the round bar steel is 330°C, and then incubated in a pit for 48 h to obtain a finished product. This cooling operation completes a phase transition, reduces the deformation of the round bar steel, and releases an internal stress.

[0042] Measures at the cooling stage after rolling are taken mainly to reduce a VC size and an interlamellar spacing among pearlite sheets and improve the strength and cross-sectional uniformity of the round bar steel. As shown in FIG. 8, at this stage, VC of 5 nm to 20 nm is precipitated, and mainly plays a role of precipitation strengthening. FIG. 9 shows the morphology of an interlamellar spacing among pearlite sheets in a finished round bar steel product.

[0043] FIG. 2 shows microstructure images of a position at 1 / 4 radius from the surface and the core of the round bar steel finally obtained in this example, and it can be seen from this figure that austenite grains of the rolled metal are significantly refined, where the position at a 1 / 4 radius from the surface and the core have grain size grades of 8.0 and 7.0, respectively, and a core / surface grain size grade difference is merely 1 grade.

[0044] Example 2 A method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling was provided. In this method, a continuous casting billet included the following chemical components in mass percentages: C: 0.40%, Si: 0.46%, Mn: 1.22%, 11 P: 0.01%, S: 0.02%, Ti: 0.022%, Nb: 0.035%, Al: 0.15%, V: 0.18%, N: 0.016%, and Fe and unavoidable impurities: the balance, where Ti / N = 1.375 and (Ti+Nb+Al) / N = 12.94; and the continuous casting billet had a cross-sectional size of 800 mm x 800 mm.

[0045] The method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling included the following steps. The continuous casting billet was heated by a stepping heating furnace, where a temperature of a second heating section was 1,250°C, a temperature of a soaking section was 1,220°C, and a total time of maintaining the temperature of the second heating section and the temperature of the soaking section was 6 h. The stepping heating furnace was a heating furnace equipped with a hot-rolling line, and included a preheating section, a first heating section, a second heating section, and a soaking section. The continuous casting billet was descaled with water, then water-cooled or naturally cooled until a surface temperature of the continuous casting billet was 1,070°C, and rolled by a reversible rough rolling machine to obtain a square billet with a side length of 400 mm, where first two passes of rolling were conducted for two vertical sides of the continuous casting billet, with a depression distance of 10 mm per pass; subsequent 6 passes of rolling were conducted alternatively for two sides of the continuous casting billet, with a depression distance of 180 mm in total; and a finishing temperature was 1,090°C. Four consecutive sides of the continuous casting billet were named sides A, B, C, and D, respectively; the first two passes of rolling were conducted for adjacent sides A and B, and these two sides were vertical. The subsequent 6 passes of rolling were also conducted alternatively for sides A and B and could also be conducted alternately for sides C and D. This is because side C was actually rolled when side A was rolled. There were an upper roller and a lower roller, and side C was rolled when side A was rolled, that is, each pass of rolling was conducted for two sides. Sides A and C were a group of sides that were rolled simultaneously, and sides B and D were a group of sides that were rolled simultaneously. The intermediate billet was water-cooled or naturally cooled until a surface temperature of the intermediate billet was 940°C, and then rolled by a continuous finish rolling machine to obtain a round bar steel with a diameter of 280 mm, where a finishing temperature was 815°C. The round bar steel was subjected to 8 alternate stages of forced through-water cooling, then sprayed with a water mist until a surface temperature of the round bar steel was 560°C, then aircooled on a cooling bed to 330°C, and incubated in a pit for 48 h to obtain a finished product. Each stage of forced through-water cooling can be conducted for about 3 s to 5 s. In this example, each stage of forced through-water cooling was conducted for 5 s. A time of each stage of forced through-water cooling is specifically related to a water amount, and if the water amount is large, the time can be shortened as long as the surface temperature of the round bar steel can be reduced to 560°C. In this example, water for the water-cooling was at room temperature. The water mist spraying can be conducted continuously for about 2 min to 3 min in total. In this example, the water mist spraying was conducted for 3 min in total; and the water mist was at room temperature. A time interval between two stages of water mist spraying is not limited as long as a total time of the two stages of water mist spraying is 2 min to 3 min; and it is not necessary to set 2 stages of water mist spraying as long as the surface temperature of the round bar steel can be reduced to 560°C.

[0046] The structure grades and mechanical properties of the core and a position at a 1 / 4 radius of the round bar steel in this example are shown in Table 1.

[0047] FIG. 3 shows microstructure images of a position at 1 / 4 radius from the surface and the core of the round bar steel finally obtained in this example, and it can be seen from this figure that austenite grains of the rolled metal are significantly refined, where the position at a 1 / 4 radius from the surface and the core have grain size grades of 8.0 and 6.5, respectively, and a core / surface grain size grade difference is merely 1.5 grades.

[0048] Comparative Example 1 A non-quenched and tempered steel with an ultra-large cross section was provided. A continuous casting billet used included the following chemical components in mass percentages: C: 0.39%, Si: 0.58%, Mn: 1.52%, P: 0.01%, S: 0.03%, Ti: 0.040%, Nb: 0.030%, Al: 0.02%, V: 0.30%, N: 0.008%, and Fe and unavoidable impurities: the balance, where Ti / N = 5, which was higher than 3.4; and (Ti+Nb+Al) / N = 11.25, which was lower than 12.5; and the continuous casting billet had a crosssectional size of 430 mm x 480 mm.

[0049] A method for improving the non-quenched and tempered steel with an ultra-large cross section included the following steps: The continuous casting billet was heated by a stepping heating furnace, where a temperature of a second heating section was 1,250°C, a temperature of a soaking section was 1,230°C, and a total time of maintaining the temperature of the second heating section and the temperature of the soaking section was 2.0 h. The continuous casting billet was descaled with water, then water-cooled or naturally cooled until a surface temperature of the continuous casting billet was 1,150°C, and rolled by a reversible rough rolling machine to obtain a square billet with a side length of 240 mm, where first two passes of rolling were conducted for two vertical sides of the continuous casting billet, with a depression distance of 10 mm per pass; the subsequent 12 passes of rolling were conducted alternatively for two sides of the continuous casting billet, with a depression distance of 50 mm in total; and a finishing temperature was 1,080°C. The intermediate billet was cooled to 1,050°C, and then rolled by a continuous finish rolling machine to obtain a round bar steel with a diameter of 200 mm, where a finishing temperature was 880°C. The round bar steel was subjected to 2 stages of forced through-water cooling until a surface temperature of the round bar steel was 760°C, then air-cooled on a cooling bed to 430°C, and incubated in a pit.

[0050] The structure grades and mechanical properties of the core and a position at a 1 / 4 radius of 13 the round bar steel in Comparative Example 1 are shown in Table 1.

[0051] FIG. 1 shows microstructures of a position at a 1 / 4 radius from a surface and a core of the rolled metal in Comparative Example 1, and it can be seen from this figure that the position at a 1 / 4 radius from the surface and the core of the rolled metal have grain size grades of 6.5 and 4.0, respectively; core structures are coarse; and a core / surface grain size difference is extremely large, and core and surface grain sizes are non-uniform.

[0052] The structure grades and mechanical properties of a core and a position at a 1 / 4 radius of the round bar steel in each of Examples 1 and 2 and Comparative Example 1 are shown in Table 1.

[0053] Table 1 shows performance comparison results of Examples 1 and 2 and Comparative Example 1.

[0054] Table 1: Structure grades and mechanical properties of a core and a position at a 1 / 4 radius No. Diameter (mm) Original austenite grain size grade Ferrite proportion Tensile strength (MPa) Yield strength (MPa) Elongation at break (%) Impact work KU2 (J) Core of Comparative Example 1 200 4.0 2.5% 755 528 10.4 20 1 / 4 radius of Comparative Example 1 6.5 18% 821 604 11.3 28 Core of Example 1 180 7.0 22% 990 722 16.5 44 1 / 4 radius of Example 1 8.0 20% 1022 732 17.2 47 Core of Example 2 280 6.5 18% 1002 763 15.9 42 1 / 4 radius of Example 2 8.0 15% 1003 775 17.0 48 Example 3 A method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling was provided. In this method, a continuous casting billet 14 included the following chemical components in mass percentages: C: 0.35%, Si: 0.30%, Mn: 1.10%, P: 0.02%, S: 0.01%, Ti: 0.015%, Nb: 0.03%, Al: 0.10%, V: 0.10%, N: 0.008%, and Fe and unavoidable impurities: the balance, where Ti / N = 1.875 and (Ti+Nb+Al) / N = 18.125; and the continuous casting billet had a cross-sectional size of 400 mm x 400 mm.

[0055] The method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling included the following steps: The continuous casting billet was heated by a stepping heating furnace, where a temperature of a second heating section was 1,230°C, a temperature of a soaking section was 1,210°C, and a total time of maintaining the temperature of the second heating section and the temperature of the soaking section was 5 h. The continuous casting billet was descaled with water, then water-cooled or naturally cooled until a surface temperature of the continuous casting billet was 1100°C, and rolled by a reversible rough rolling machine to obtain a square billet with a side length of 230mm, where first two passes of rolling were conducted for two vertical sides of the continuous casting billet, with a depression distance of 5mm per pass; the subsequent 4 passes of rolling were conducted alternatively for two sides of the continuous casting billet, with a depression distance of 80mm in total; and a finishing temperature was 1,050°C. The intermediate billet was water-cooled or naturally cooled until a surface temperature of the intermediate billet was 900°C, and then rolled by a continuous finish rolling machine to obtain a round bar steel with a diameter of 160 mm, where a finishing temperature was 780°C. The round bar steel was subjected to 7 alternate stages of forced through-water cooling, then sprayed with a water mist until a surface temperature of the round bar steel was 550°C, then aircooled on a cooling bed to 300°C, and incubated in a pit for 50 h to obtain a finished product. In this example, each stage of forced through-water cooling was conducted for 3 s, and a total time of the water mist spraying was 2 min.

[0056] For the finished product obtained in this example, a position at a 1 / 4 radius has a longitudinal tensile strength of 900 MPa, a yield strength of 650 MPa, an elongation at break of 15%, and an impact work KU2 of 40 J; and a core has a longitudinal tensile strength of 920 MPa, a yield strength of 669 MPa, an elongation at break of 15.5%, and an impact work KU2 of 42 J.

[0057] Example 4 A method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling was provided. In this method, a continuous casting billet included the following chemical components in mass percentages: C: 0.45%, Si: 0.90%, Mn: 1.60%, P: 0.015%, S: 0.04%, Ti: 0.030%, Nb: 0.04%, Al: 0.30%, V: 0.20%, N: 0.020%, and Fe and unavoidable impurities: the balance, where Ti / N = 1.5 and (Ti+Nb+Al) / N = 18.5; and the continuous casting billet had a cross-sectional size of 1,000 mm x 1,000 mm.

[0058] The method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling included the following steps: The continuous casting billet was heated by a stepping heating furnace, where a temperature of a second heating section was 1,240°C, a temperature of a soaking section was 1,220°C, and a total time of maintaining the temperature of the second heating section and the temperature of the soaking section was 7 h. The continuous casting billet was descaled with water, then water-cooled or naturally cooled until a surface temperature of the continuous casting billet was 1,090°C, and rolled by a reversible rough rolling machine to obtain a square billet with a side length of 450 mm, where first two passes of rolling were conducted for two vertical sides of the continuous casting billet, with a depression distance of 7 mm per pass; the subsequent 6 passes of rolling were conducted alternatively for two sides of the continuous casting billet, with a depression distance of 250 mm in total; and a finishing temperature was 1,090°C. The intermediate billet was water-cooled or naturally cooled until a surface temperature of the intermediate billet was 950°C, and then rolled by a continuous finish rolling machine to obtain a round bar steel with a diameter of 300 mm, where a finishing temperature was 820°C. The round bar steel was subjected to 8 alternate stages of forced through-water cooling, then sprayed with a water mist until a surface temperature of the round bar steel was 600°C, then aircooled on a cooling bed to 350°C, and incubated in a pit for 48 h to obtain a finished product.

[0059] For the finished product obtained in this example, a position at a 1 / 4 radius has a longitudinal tensile strength of 1,027 MPa, a yield strength of 779 MPa, an elongation at break of 17%, and an impact work KU2 of 46 J; and a core has a longitudinal tensile strength of 1,050 MPa, a yield strength of 800 MPa, an elongation at break of 19%, and an impact work KU2 of 50 J.

[0060] Example 5 This example was different from Example 4 only in that, in the method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling, a continuous casting billet included the following chemical components in mass percentages: C: 0.40%, Si: 0.75%, Mn: 1.35%, P: 0.015%, S: 0.02%, Ti: 0.028%, Nb: 0.04%, Al: 0.30%, V: 0.20%, N: 0.0082%, and Fe and unavoidable impurities: the balance, where Ti / N = 3.37 and (Ti+Nb+Al) / N = 44.88.

[0061] For the finished product obtained in this example, a position at a 1 / 4 radius has a longitudinal tensile strength of 1,005 MPa, a yield strength of 766 MPa, an elongation at break of 16.1%, and an impact work KU2 of 40 J; and a core has a longitudinal tensile strength of 1,022 MPa, a yield strength of 778 MPa, an elongation at break of 17%, and an impact work KU2 of 45 J.

[0062] It should be understood that, in order to simplify the present disclosure and help understand one or more aspects of the present disclosure, in the above description of exemplary embodiments of the present disclosure, various features of the present disclosure are sometimes grouped together into a single embodiment, figure, or description thereof. However, the method of the present disclosure should not be interpreted as reflecting the intention that the claimed present disclosure has features more than the features expressly stated in each claim. More precisely, as reflected in the claims, each aspect of the present disclosure has features less than all features of the embodiments disclosed above. Therefore, the claims following specific embodiments are hereby expressly incorporated into the specific embodiments, where each claim itself serves as a separate embodiment of the present disclosure.

[0063] Although the present disclosure is described according to the limited number of examples, those skilled in the art appreciate that other examples may be conceived from the above description within the defined scope of the present disclosure. In addition, it should be noted that the language used in this specification is selected primarily for readability and teaching, but not for explaining or defining the subject of the present disclosure. Thus, without departing from the scope and spirit of the appended claims, many modifications and changes are apparent to those of ordinary skill in the art. Within the scope of the present disclosure, the disclosure of the present disclosure is illustrative rather than restrictive. The scope of the present disclosure is defined by the appended claims.

[0064] The above are merely preferred implementations of the present disclosure. It should be noted that a person of ordinary skill in the art may further make several improvements and modifications without departing from the principle of the present disclosure, but such improvements and modifications should be deemed as falling within the protection scope of the present disclosure.

Claims

What is claimed is:

1. A method for improving strength, toughness, and uniformity of a non-quenched and tempered steel with an ultra-large cross section having a diameter of 160 mm to 300 mm through synergistic regulation of multi-stage precipitation and controlled rolling / controlled cooling, characterized in that the non-quenched and tempered steel with the ultra-large cross section comprises the following chemical components in mass percentages: C: 0.35% to 0.45%, Si: 0.30% to 0.90%, Mn: 1.10% to 1.60%, V: 0.10% to 0.20%, Nb: 0.03% to 0.04%, Ti: 0.015% to 0.030%, Al: 0.10% to 0.30%, N: 0.008% to 0.020%, S: 0.01% to 0.04%, P: less than or equal to 0.02%, and Fe and unavoidable impurities: the balance, wherein a Ti / N mass percentage ratio is lower than 3.4 and a (Ti+Nb+Al) / N mass percentage ratio is higher than 12.5; andthe method comprises the following steps:S1: continuously heating a continuous casting billet using a stepping heating furnace, the stepping heating furnace comprising a hot-rolling line, and included a preheating section, a first heating section, a second heating section, and a soaking section, wherein a temperature of the second heating section is 1,230°C to 1,250°C, a temperature of the soaking section is 1,210°C to 1,230°C, and a total time of maintaining the continuous casting billet in the second heating section and the soaking section is no less than 5 h;S2: after the continuous heating, descaling the continuous casting billet with water, and watercooling or naturally-cooling the continuous casting billet until a surface temperature of the continuous casting billet is lower than 1,100°C;S3: subjecting the continuous casting billet to rough rolling with a reversible rough rolling machine to obtain an intermediate billet, having a square cross-section defining four adjacent vertical sides of the square cross-section and a side length of 230 mm to 450 mm; wherein first two passes of rolling are conducted for two adjacent vertical sides of the continuous casting billet, with a depression distance of 5 mm to 10 mm per pass; subsequent 4 to 6 consecutive passes of rolling are conducted alternately for the two adjacent vertical sides of the continuous casting billet, where alternate rolling means that two adjacent passes alternately roll the two adjacent vertical sides, with a deformation amount of higher than or equal to 20% per pass; and a finishing temperature of the rough rolling is higher than 1,050°C;S4: water-cooling or naturally-cooling the intermediate billet until a surface temperature of the intermediate billet is 900°C to 950°C;S5: rolling the intermediate billet into a round bar steel through continuous finish rolling with a finishing temperature of 780°C to 820°C;S6: subjecting the round bar steel to 6 to 8 stages of forced through-water cooling until a surface temperature of the round bar steel is 550°C to 600°C, wherein air cooling is conducted for 5 s to 10 s between every two adjacent ones of the stages of the forced through-water cooling, a surface temperature drop of the round bar steel after each of the stages of the forced through-water cooling is not larger than 100°C, and then spraying the round bar steel with a water mist, to maintain the surface temperature of the round bar steel at 550°C to 600°C; andS7: cooling the round bar steel by a stepping cooling bed with a straightening function until the surface temperature of the round bar steel is 300°C to 350°C, and incubating the round bar steel in a pit for at least 48 h to obtain a finished product.

2. The method according to claim 1, characterized in that a mass percentage of Ti is 0.020% to 0.028%.

3. The method according to claim 1, characterized in that the continuous casting billet is a square or rectangular billet with a side length of 400 mm to 1,000 mm.

4. The method according to claim 1, characterized in that the finished product has, at a 1 / 4 radius and a core, a longitudinal tensile strength of 900 MPa to 1,050 MPa, a yield strength of 650 MPa to 800 MPa, an elongation at break of 15% to 19%, and an impact work KU2 of 40 J to 50 J.

5. The method according to claim 1, characterized in that in S1, TiN of 3 pm to 5 pm is retained during the continuous heating of the continuous casting billet.

6. The method according to claim 1, characterized in that in S3, TiN and NbN of 1 pm to 3 pm are precipitated during the rough rolling.

7. The method according to claim 1, characterized in that in S4, TiN, NbN, and AlN of 500 nm to 1 pm are precipitated during the water-cooling or natural-cooling of the intermediate billet.

8. The method according to claim 1, characterized in that in S5, NbN and AlN of 100 nm to 500 nm are precipitated during the finish rolling; and in S6, VC of 5 nm to 20 nm is precipitated during the cooling after the finish rolling.

Citation Information

Patent Citations

  • ViewWO2022/227891A1onEspacenetopensinnewtab

  • ViewCN111549282AonEspacenetopensinnewtab

  • ViewCN109554618AonEspacenetopensinnewtab

  • ViewCN111647799AonEspacenetopensinnewtab