Pigmented polymer particles and methods of production and uses thereof

JP2022084006A5Inactive Publication Date: 2024-11-28XEROX CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021189850
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-25
Filing Date
2021-11-24
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing thermoplastic polymers face challenges in homogeneous mixing of pigments, particularly in 3D printing applications, which is crucial for achieving structural and mechanical tolerances required in commercial and industrial objects.

Method used

Development of colored polymer particles with pigments having a melt-emulsified form, where the pigment is coated, embedded, or encapsulated by a thermoplastic polymer, enhancing their integration and stability during 3D printing processes.

Benefits of technology

The colored polymer particles improve the integrity of 3D printed objects by reducing void spaces and deformation, enabling effective identification, tracking, and authentication through color and phosphorescence properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide spherical pigmented polymer particles useful as starting material for additive manufacturing, and methods of production and uses thereof.SOLUTION: Pigmented polymer particles may comprise a thermoplastic polymer and a pigment, where at least some of the pigmented polymer particles have a morphology according to (a), (b), (c), or any combination thereof: (a) the pigment having a coating comprising the thermoplastic polymer and the coated pigment adhering to a thermoplastic polymer particle, (b) the pigment being embedded in an outer surface of the thermoplastic polymer particle, and (c) the pigment being encapsulated by the thermoplastic polymer particle. The pigmented polymer particles, especially highly spherical pigmented polymer particles, may be useful, among other things, as starting material for additive manufacturing.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to particles comprising a pigment and a thermoplastic polymer. These particles are referred to as colored polymer particles. This disclosure further relates to methods for preparing and using such colored polymer particles. [Background technology]

[0002] Thermoplastic polymers are often used to produce extruded objects such as films, bags, particles, and filaments. Many thermoplastic polymers are grayish-white polymers that have the ability to withstand rising and / or falling temperatures without losing their physical properties. Therefore, objects formed from thermoplastic polymers can be used in demanding applications such as power tools, automotive parts, gears, and electrical appliance components. In some cases, these applications may require that the parts made from thermoplastic polymers be colored or have other visible identifiers such as phosphorescence. For example, phosphorescence, color patterns, or color combinations can be used to identify parts as an anti-counterfeiting measure.

[0003] Because pigments are fine particles, homogeneous mixing in thermoplastic polymers can be difficult. One application where the homogeneous incorporation of pigments is particularly important is the rapidly growing field of three-dimensional (3D) printing, also known as additive manufacturing. While 3D printing has traditionally been used for rapid prototyping, this 3D printing technology is increasingly being adopted for the manufacture of commercial and industrial objects where structural and mechanical tolerances that are entirely different from those of rapid prototyping may be required.

[0004] 3D printing works by depositing either (a) small droplets or flows of a molten or solidifiable material, or (b) fine powder particles, into precise locations, and then solidifying them into a larger object (which may have any number of complex shapes). Such deposition and solidification processes are typically performed under computer control, stacking the larger object layer by layer. In certain examples, the solidification of fine powder particles may be performed in a 3D printing system that uses a laser to facilitate selective laser sintering (SLS). [Overview of the project] [Problems that the invention aims to solve]

[0005] This disclosure relates to colored polymer particles and methods for producing and using such particles. The colored polymer particles described herein, in particular highly spherical colored polymer particles, may be useful, among other things, as starting materials for additive manufacturing. Furthermore, visual properties (e.g., color, color combinations, phosphorescence, etc.) may be used for object identification, object tracking, object authentication, and / or determining the integrity of objects produced from colored polymer particles.

[0006] A composition comprising colored polymer particles containing a thermoplastic polymer and a pigment having a molten emulsion form is disclosed herein.

[0007] A composition comprising colored polymer particles comprising a thermoplastic polymer and a pigment is disclosed herein, wherein at least a portion of the colored polymer particles are in a form relating to (a), (b), (c), or any combination thereof: (a) the pigment has a coating comprising a thermoplastic polymer, and the coated pigment is attached to the thermoplastic polymer particle; (b) the pigment is embedded on the outer surface of the thermoplastic polymer particle; and (c) the pigment is encapsulated by the thermoplastic polymer particle.

[0008] A method is disclosed herein that includes depositing both or one of the aforementioned colored polymer particles on a surface in combination with other thermoplastic polymer particles in an optional manner, and after deposition, heating at least a portion of the particles to promote solidification of the particles and form a solidified body.

[0009] A method is disclosed herein that comprises mixing a mixture comprising a thermoplastic polymer, a dispersion medium that is miscible with the thermoplastic polymer, a pigment, and optionally an emulsifying stabilizer at a temperature higher than the melting or softening temperature of the thermoplastic polymer and at a shear rate high enough to disperse the thermoplastic polymer in the dispersion medium; cooling the mixture to below the melting or softening temperature of the thermoplastic polymer to form colored polymer particles comprising the thermoplastic polymer and a pigment having a molten emulsion form; and separating the colored polymer particles from the dispersion medium.

[0010] A method is disclosed herein that comprises mixing a mixture comprising a thermoplastic polymer, a dispersion medium immiscible with the thermoplastic polymer, a pigment, and optionally an emulsifying stabilizer at a temperature higher than the melting or softening temperature of the thermoplastic polymer and a shear rate high enough to disperse the thermoplastic polymer in the dispersion medium; and cooling the mixture to below the melting or softening temperature of the thermoplastic polymer to form colored polymer particles comprising the thermoplastic polymer and the pigment, wherein at least a portion of the colored polymer particles have a form conforming to (a), (b), (c), or any combination thereof: (a) the pigment has a coating comprising the thermoplastic polymer and the coated pigment is attached to the thermoplastic polymer particles; (b) the pigment is embedded on the outer surface of the thermoplastic polymer particles; and (c) the pigment is encapsulated by the thermoplastic polymer particles; and separating the colored polymer particles from the dispersion medium. [Brief explanation of the drawing]

[0011] The following figures are included to illustrate certain aspects of the embodiments and should not be regarded as exclusive embodiments. The disclosed subject matter is susceptible to considerable modifications, variations, combinations, and equivalents in form and function, as will occur to those skilled in the art having the benefit of this disclosure.

[0012] [Figure 1] FIG. 1 is a flowchart of a non-limiting exemplary method 100 of the present disclosure.

[0013] [Figure 2] FIG. 2 is a scanning electron micrograph of Samples 1-2 and 1-3, respectively, illustrating polymer-coated pigments adhering to the surface of polymer particles. [Figure 3] FIG. 3 is a scanning electron micrograph of Samples 1-2 and 1-3, respectively, illustrating polymer-coated pigments adhering to the surface of polymer particles.

[0014] [Figure 4] FIG. 4 is a cross-sectional scanning electron micrograph of Sample 1-2 (the sample was fixed in epoxy resin and cryomicrotomed prior to imaging), illustrating (a) pigments that are not attached, embedded, or encapsulated in polymer particles and (b) pigments embedded in the surface of polymer particles. [Figure 5] FIG. 5 is a cross-sectional scanning electron micrograph of Sample 1-2 (the sample was fixed in epoxy resin and cryomicrotomed prior to imaging), illustrating (a) pigments that are not attached, embedded, or encapsulated in polymer particles and (b) pigments embedded in the surface of polymer particles.

[0015] [Figure 6] FIG. 6 is a scanning electron micrograph of Sample 3-1 illustrating what is likely a polymer-coated pigment adhering to the surface of polymer particles. [Figure 7]Figure 7 is a scanning electron microscope image of sample 3-1, illustrating what are likely polymer-coated pigments adhering to the surface of polymer particles.

[0016] [Figure 8] Figure 8 shows cross-sectional scanning electron microscope images (the sample was fixed in epoxy resin and freeze-microtome-treated before imaging) illustrating (a) pigment embedded on the surface of polymer particles and (b) pigment encapsulated in polymer particles. [Figure 9] Figure 9 shows cross-sectional scanning electron microscope images (the sample was fixed in epoxy resin and freeze-microtome-treated before imaging) illustrating (a) pigment embedded on the surface of polymer particles and (b) pigment encapsulated in polymer particles. [Modes for carrying out the invention]

[0017] Three-dimensional (3D) printing, also known as additive manufacturing, is a rapidly growing field of technology. While 3D printing has traditionally been used for rapid prototyping, this technology is increasingly being adopted for the manufacture of commercial and industrial objects that require structural and mechanical tolerances entirely different from those of rapid prototypes.

[0018] This disclosure relates to polymer particles comprising a pigment and a thermoplastic polymer. The particles are referred to as colored polymer particles. The colored polymer particles may include particles having a form that conforms to (a), (b), (c), or any combination thereof: (a) the pigment has a coating comprising a thermoplastic polymer, and the coated pigment is attached to the thermoplastic polymer particle; (b) the pigment is embedded on the outer surface of the thermoplastic polymer particle; and (c) the pigment is encapsulated by the thermoplastic polymer particle.

[0019] The colored polymer particles described herein, particularly highly spherical colored polymer particles, may be useful, among other things, as starting materials for additive manufacturing. Furthermore, the color and / or phosphorescence imparted by the pigments may be used for object identification, object tracking, object authentication, and / or determining the integrity of objects made from colored polymer particles. Definitions and Test Methods

[0020] As used herein, the term “immiscible” refers to a mixture of two or more components that, when combined, form phases with a solubility of less than 5% by weight of each other at ambient pressure and room temperature, or, if solid at room temperature, at the melting point of the components. For example, polyethylene oxide with a molecular weight of 10,000 g / mol is solid at room temperature and has a melting point of 65°C. Therefore, if a material is liquid at room temperature and the polyethylene oxide has a solubility of less than 5% by weight at 65°C, the polyethylene oxide is immiscible with the material.

[0021] As used herein, the term "pigment" refers to particles that absorb and / or refract ultraviolet or visible light.

[0022] As used herein, the term "phosphorescence" and its grammatical variations refer to luminescence that persists for at least 10 nanoseconds after the excitation source (e.g., broad-spectrum light, ultraviolet wavelength light, specific wavelength light, etc.) has been removed.

[0023] As used herein, "phosphorescent pigment" refers to a pigment that emits phosphorescence when exposed to an excitation source.

[0024] As used herein, the term "thermoplastic polymer" refers to a plastic polymer material that reversibly softens and hardens upon heating and cooling. Thermoplastic polymers include thermoplastic elastomers.

[0025] As used herein, the term “elastomer” refers to a copolymer comprising a crystalline “rigid” portion and an amorphous “soft” portion. In the case of polyurethane, the crystalline portion may include a portion of polyurethane containing urethane functionality and optionally selected chain-extending groups, and the soft portion may include, for example, a polyol.

[0026] As used herein, the term "polyurethane" refers to the polymer reaction product between a diisocyanate, a polyol, and an optional chain extender.

[0027] As used herein, the term "oxide" refers to both metallic oxides and non-metallic oxides. For the purposes of this disclosure, silicon is considered a metal.

[0028] As used herein, the term “embedding” with respect to particles (e.g., nanoparticles and / or pigments) and the surface of polymer particles means that the particles extend at least partially onto the surface of the polymer particles such that the polymer is in contact with the nanoparticles to a greater extent than would be possible if the nanoparticles were simply placed on the surface of the polymer particles.

[0029] As used herein, the term “encapsulated” with respect to particles (e.g., nanoparticles and / or pigments) and polymer particles refers to particles that are enclosed by polymer particles. That is, portions of the particles (e.g., nanoparticles and / or pigments) do not extend beyond the surface of the polymer particles. The term “encapsulated” does not imply the extent to which the surface of the particle (e.g., nanoparticles and / or pigments) is in contact with the polymer. For example, the particles (e.g., nanoparticles and / or pigments) may be at least partially within the voids of the polymer particles, with only a portion of the particle's surface in contact with the polymer.

[0030] Hereinafter, D10, D50, D90, and diameter span are used primarily to describe particle size. As used herein, the term "D10" refers to a diameter in which 10% of the sample (on a volume basis, unless otherwise specified) consists of particles with a diameter less than that diameter value. As used herein, the term "D50" refers to a diameter in which 50% of the sample (on a volume basis, unless otherwise specified) consists of particles with a diameter less than that diameter value. As used herein, the term "D90" refers to a diameter in which 90% of the sample (on a volume basis, unless otherwise specified) consists of particles with a diameter less than that diameter value.

[0031] As used herein, the terms “diameter span,” “span,” and “span size” refer to diameter and provide an indicator of the extent of the particle size distribution, calculated as (D90-D10) / D50 (again, each D value is based on volume unless otherwise stated).

[0032] Particle size can be determined by light scattering techniques using a Malvern MASTERSIZER® 3000 or by analysis of optical digital microscope images. Unless otherwise stated, light scattering techniques are used to analyze particle size.

[0033] For the light scattering technique, the control sample was glass beads with a diameter in the range of 15 μm to 150 μm, traded under the product name Quality Audit Standards QAS4002 (trademark), obtained from Malvern Analytical Ltd. Unless otherwise specified, the sample was analyzed as a dry powder. The analyzed particles were dispersed in air and analyzed using the AERO S dry powder dispersion module with MASTERSIZER (trademark) 3000. Particle size was derived using instrument software from a plot of volume density as a function of size.

[0034] Particle size and diameter span can also be determined by optical digital microscopy. Optical images are obtained using a Keyence VHX-2000 digital microscope with version 2.3.5.1 software (system version 1.93) for particle size analysis.

[0035] When used herein, if sieving is mentioned, the pore / screen size is as described by the USA Standard Sieve (ASTM E11-17).

[0036] As used herein, "roundness" and "sphericity" for a particle refer to how close the particle is to a perfect sphere. To determine roundness, an optical microscope image of the particle is taken. The perimeter (P) and area (A) of the particle in the plane of the microscope image are calculated (for example, using a SYSMEX FPIA 3000 particle shape and particle size analyzer available from Malvern Instruments). The roundness of the particle is C EA / P is and in the formula, C EA This is the circumference of a circle having an area equivalent to the area (A) of the actual particle.

[0037] As used herein, the term “shear force” refers to agitation or similar processes that induce mechanical agitation in a fluid.

[0038] As used herein, the term "aspect ratio" refers to the length divided by the width, where the length is greater than the width.

[0039] Unless otherwise specified, the melting point of the polymer shall be determined according to ASTM E794-06 (2018) with a heating rate and a cooling rate of 10°C / min.

[0040] Unless otherwise specified, the softening temperature or softening point of the polymer is determined according to ASTM D6090-17. The softening temperature can be measured using a 0.50 g sample at a heating rate of 1 °C / min with a cup-and-ball apparatus available from Mettler-Toledo.

[0041] The angle of repose is a measure of the fluidity of a powder. The angle of repose was determined using Hosokawa Micron's Powder Characteristics Tester PT-R, following ASTM D6393-14 "Standard Test Method for Bulk Solids Characterized by Carr Indices".

[0042] Hausner ratio (H r ) is a measure of the fluidity of powders, H r =ρ tap / ρ bulk It is calculated by, in the formula, ρ bulk This is the bulk density according to ASTM D6393-14, and ρ tap This is the tap density according to ASTM D6393-14.

[0043] When used herein, the viscosity of the dispersion medium is the kinematic viscosity at 25°C, measured according to ASTM D445-19, unless otherwise specified. For commercially sourced dispersion mediums (e.g., polydimethylsiloxane oil), the kinematic viscosity data referenced herein were provided by the manufacturer, whether or not they were measured according to the aforementioned ASTM or other standard measurement techniques. Colored polymer particles and method for producing them

[0044] The methods and compositions described herein relate to colored polymer particles. Pigments are included in the formation of a melt emulsion of colored polymer particles. Colored polymer particles may include polymer particles containing pigment and thermoplastic polymer. In particular, the form of the colored polymer particles may vary depending on the pigment composition, thermoplastic polymer composition, and melt emulsion process parameters. For example, the thermoplastic polymer may form a coating on the pigment, and the coated pigment may adhere to the surface of the thermoplastic polymer particles. In another example, the pigment may be embedded in the surface of the thermoplastic polymer particles. In such a case, the pigment embedded in the thermoplastic polymer particles may or may not have a coating containing thermoplastic polymer. In yet another exemplary form, the pigment may be encapsulated within the thermoplastic polymer particles. Any combination of those described herein may also exist, which may be referred to herein as the melt emulsion form. Furthermore, the compositions and methods described herein do not require that all thermoplastic polymer particles have pigments associated with them. In other words, the compositions and methods produced herein may include mixtures of particles comprising one or more of the following: (a) thermoplastic polymer particles that are not associated with any pigment (i.e., particles containing thermoplastic polymers) (e.g., thermoplastic polymer particles to which pigment is not attached, embedded, or encapsulated); (b) colored polymer particles comprising a thermoplastic polymer having a pigment in a molten emulsion form; and (c) thermoplastic polymer coated pigments that are not associated with thermoplastic polymer particles (e.g., thermoplastic polymer coated pigments to which thermoplastic polymer particles are not attached, embedded, or encapsulated).(b) Colored polymer particles comprising a pigment and a thermoplastic polymer having a melted emulsion form may include one or more of the following: (b1) thermoplastic polymer particles to which the pigment is attached via the polymer (e.g., pigments having a coating comprising a thermoplastic polymer, wherein the coated pigment is attached to the outer surface of the thermoplastic polymer particle), (b2) thermoplastic polymer particles to which the pigment is embedded on the surface of the polymer particle, and (b3) thermoplastic polymer particles in which the pigment is encapsulated within the polymer particle (where a single particle may have any combination of (b1), (b2), and (b3)).

[0045] While not limited to theory, it is believed that the melt emulsification process creates a closer bond between the thermoplastic polymer and the pigment, allowing the pigment to more readily associate with the polymer particles in one or more of various forms. Colored polymer particles in a melt emulsified form may improve the integrity of the resulting SLS additively manufactured articles (e.g., reduction of voids and / or deformation) while providing comparable color and / or phosphorescence compared to a mixture of pigment and polymer particles.

[0046] Figure 1 is a flowchart of a non-limiting exemplary method 100 of the present disclosure. A thermoplastic polymer 102, a dispersion medium 104, an optional emulsifying stabilizer 106, and a pigment 108 are combined 110 to produce a mixture 112. Components 102, 104, 106, and 108 can be added in any order and the process 110 of combining components 102, 104, 106, and 108 includes mixing and / or heating.

[0047] Next, the mixture 112 is treated by applying a sufficiently high shear force to the mixture 112 at a temperature higher than the melting or softening temperature of the thermoplastic polymer 102 to form a molten emulsion 116. Since the temperature is higher than the melting or softening temperature of the thermoplastic polymer 102, the thermoplastic polymer 102 becomes a polymer melt. The shear rate should be sufficient to disperse the polymer melt as droplets (i.e., polymer emulsion 116) in the dispersion medium 104. Although not bound by theory, it is assumed that, all other factors being equal, increasing the shear force should decrease the size of the polymer melt droplets in the dispersion medium 104. However, at some point, increasing the shear and decreasing the droplet size may result in reduced return, or the contents of the droplets may collapse, reducing the quality of the particles produced therefrom.

[0048] Next, the molten emulsion 116 in and / or outside the mixing container is cooled 118 to solidify the polymer droplets into colored polymer particles 124 (also referred to as solidified colored polymer particles). The thermoplastic polymer particles 124 contain a thermoplastic polymer. At least a portion of the colored polymer particles 124 / 130 contain a thermoplastic polymer (composed of thermoplastic polymer 102) and a pigment 108a having a molten emulsion form. The molten emulsion form may include at least one of the following: (a) the pigment has a coating containing a thermoplastic polymer, and the coated pigment is attached to the outer surface of the thermoplastic polymer particles; (b) the pigment is embedded in the outer surface of the thermoplastic polymer particles; and (c) the pigment is encapsulated by the thermoplastic polymer particles (wherein a single colored polymer particle may have any combination of (a), (b), and (c)). Preferably, the colored polymer particles 124 / 130 contain particles having the form of (b) and / or (c). Furthermore, as described above, other components of the product added to the colored polymer particles 124 may include pigments 108 coated with thermoplastic polymer 102 but not associated with the polymer particles, and / or polymer particles not associated with the pigments 108.

[0049] Next, the cooled mixture 120 can be processed 122 to isolate the colored polymer particles 124 from other components 126 (e.g., dispersion medium 104, excess emulsifying stabilizer 106, etc.), and the colored polymer particles 124 can be washed or otherwise purified. The colored polymer particles 124 comprise a thermoplastic polymer 102 and a pigment 108 containing particles having a molten emulsion form, and if present, at least a portion of the emulsifying stabilizer 106 coats the outer surface of the colored polymer particles 124. Furthermore, if a coated pigment is produced, the emulsifying stabilizer 106 may coat at least a portion of the polymer coating of the pigment 108. The emulsifying stabilizer 106 or a portion thereof may be deposited on the colored polymer particles 124 (and the coated pigment, if produced) as a coating, possibly as a uniform coating. In some cases, depending on non-limiting factors such as temperature (including cooling rate), the type of thermoplastic polymer 102, and the type and size of the emulsifying stabilizer 106, the nanoparticles of the emulsifying stabilizer 106 may be at least partially embedded within the outer surface of the colored polymer particles 124. Even without embedding, at least a portion of the nanoparticles in the emulsifying stabilizer 106 may remain firmly associated with the colored polymer particles 124, facilitating their further use. In contrast, dry mixing of already formed thermoplastic polymer microparticles (e.g., those formed by cryogenic grinding or precipitation processes) with a flow aid such as silica nanoparticles does not result in a robust and uniform coating of the flow aid on the thermoplastic polymer microparticles (and, if manufactured, coated pigments).

[0050] The colored polymer particles 124 may be optionally further purified to obtain 128 (described in more detail below) to obtain purified colored polymer particles 130.

[0051] The thermoplastic polymer 102 and the dispersion medium 104 should be selected such that they are immiscible at various processing temperatures (e.g., from room temperature to the process temperature). An additional factor to consider is the difference (e.g., difference or ratio) in process temperature between the molten thermoplastic polymer 102 and the dispersion medium 104. Differences in viscosity can affect droplet breakdown and particle size distribution. While not theoretically bound, if the viscosities of the molten thermoplastic polymer 102 and the dispersion medium 104 are too similar, the overall roundness of the product may decrease, and particles may become more oval and elongated.

[0052] Examples of thermoplastic polymers 102 include polyamides, polyurethanes, polyethylene, polypropylene, polyacetals, polycarbonates, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT), polyhexamethylene terephthalate, polystyrene, polyvinyl chloride, polytetrafluoroethylene, polyester (e.g., polylactic acid), polyethers, polyethersulfones, polyetheretherketones, polyacrylates, polymethacrylates, polyimides, and acrylonitrile butadiene styrene. Copolymers containing styrene (ABS), polyphenylene sulfide, vinyl polymer, polyarylene ether, polyarylene sulfide, polysulfone, polyether ketone, polyamide-imide, polyetherimide, polyether ester, polyether block and polyamide block (PEBA or polyether block amide), grafted or ungrafted thermoplastic polyolefin, functionalized or unfunctionalized ethylene / vinyl monomer polymer, functionalized or unfunctionalized ethylene / alkyl (meth)acrylate, functionalized or unfunctionalized (meth)acrylic acid polymer, functionalized or unfunctionalized ethylene / vinyl monomer / alkyl (meth)acrylate terpolymer, ethylene / vinyl monomer / carbonyl terpolymer, ethylene / alkyl (meth)acrylate / carbonyl terpolymer, methyl methacrylate-butadiene-styrene (MBS) type core-shell polymer, polystyrene-block-polybutadiene-block-poly(methyl methacrylate)Examples of such materials include, but are not limited to, methacrylate, SBM, block polymers, chlorinated or chlorosulfonated polyethylene, polyvinylidene fluoride (PVDF), phenolic resins, poly(ethylene / vinyl acetate), polybutadiene, polyisoprene, styrene-based block copolymers, polyacrylonitrile, silicones, and any combination thereof. Furthermore, copolymers comprising one or more of the aforementioned materials may be used in the methods and systems of this disclosure.

[0053] The thermoplastic polymer 102 in the compositions and methods of this disclosure may be an elastomer or not. Some of the aforementioned examples of thermoplastic polymer 102 may be an elastomer or not, depending on the exact composition of the polymer. For example, polyethylene, which is a copolymer of ethylene and propylene, may be an elastomer or not, depending on the amount of propylene in the polymer.

[0054] Thermoplastic elastomers generally fall within one of six classes: styrene-based block copolymers, thermoplastic polyolefin elastomers, thermoplastic vulcanized rubber (also called elastomer alloys), thermoplastic polyurethanes, thermoplastic copolyesters, and thermoplastic polyamides (typically block copolymers containing polyamides). Examples of thermoplastic elastomers can be found in Handbook of Thermoplastic Elastomers, 2nd ed., BMWalker and CPRader, eds., Van Nostrand Reinhold, New York, 1988. Examples of thermoplastic elastomers include, but are not limited to, elastomeric polyamides, polyurethanes, copolymers containing polyether blocks and polyamide blocks (PEBA or polyether block amides), methyl methacrylate-butadiene-styrene (MBS) type core-shell polymers, polystyrene-block-polybutadiene-block-poly(methyl methacrylate) (SBM) block copolymers, polybutadiene, polyisoprene, styrene-based block copolymers, as well as polyacrylonitrile and silicones. Elastic styrene-based block copolymers may include at least one block selected from the group consisting of isoprene, isobutylene, butylene, ethylene / butylene, ethylene-propylene, and ethylene-ethylene / propylene. More specific examples of elastic styrene-based block copolymers include, but are not limited to, poly(styrene-ethylene / butylene), poly(styrene-ethylene / butylene-styrene), poly(styrene-ethylene / propylene), poly(styrene-ethylene / propylene-styrene-ethylene-propylene), poly(styrene-butadiene-styrene), poly(styrene-butylene-butadiene-styrene), and any combination thereof.

[0055] Examples of polyamides include polycaproamide (nylon 6, polyamide 6, or PA6), poly(hexamethylene succinamide) (nylon 4,6, polyamide 4,6, or PA4,6), polyhexamethylene adipamide (nylon 6,6, polyamide 6,6, or PA6,6), polypentamethylene adipamide (nylon 5,6, polyamide 5,6, or PA5,6), polyhexamethylene sebacamide (nylon 6,10, polyamide 6,10, or PA6,10), polyundecamide (nylon 11, polyamide 11, or PA11), polydodecamide (nylon 12, polyamide 12, or PA12), and polyhexamethylene terephthalamide (nylon 6T, polyamide 6T, or PA6T), nylon 10,10 (polyamide 10,10 or PA10,10), nylon 10,12 (polyamide 10,12 or PA10,12), nylon 10,14 (polyamide 10,14 or PA10,14), nylon 10,18 (polyamide 10,18 or PA10,18), nylon 6,18 (polyamide 6,18 or PA6,18), nylon 6,12 (polyamide 6,12 or PA6,12), nylon 6,14 (polyamide 6,14 or PA6,14), nylon 12,12 (polyamide 12,12 or PA12,12), etc., and any combinations thereof, but are not limited thereto. Copolymers can also be used. Examples of copolymers include PA11 / 10,10, PA6 / 11, PA6,6 / 6, PA11 / 12, Pa 10,10 / 10,12, PA10,10 / 10,14, PA11 / 10,36, PA11 / 6,36, PA10,10 / 10,36, PA6T / 6,6, etc., and any combinations thereof, but are not limited thereto. In a polyamide where a first number followed by a comma and a second number, it is a polyamide having the first number of main-chain carbons between the nitrogens of the non-pendant part and the second number of main-chain carbons is between the two nitrogens of the part having a pendant. As a non-limiting example, nylon 6,10 is [NH-(CH2)6-NH-CO-(CH2)8-CO] nPolyamides followed by a number (multiple) and a backslash (multiple) are copolymers of polyamides, indicated by the numbers before and after the backslash.

[0056] Examples of polyurethanes include, but are not limited to, polyether polyurethanes, polyester polyurethanes, mixed polyethers and polyester polyurethanes, and any combination thereof. Examples of thermoplastic polyurethanes include, but are not limited to, poly[4,4'-methylenebis(phenylisocyanate)-alt-1,4-butanediol / di(propylene glycol) / polycaprolactone], ELASTOLLAN® 1190A (polyether polyurethane elastomer, available from BASF), ELASTOLLAN® 1190A10 (polyether polyurethane elastomer, available from BASF), and any combination thereof.

[0057] The phase solvent may optionally be used to improve the blending efficiency and effectiveness of the thermoplastic polyester with one or more thermoplastic polymers. Examples of polymer phase solvents include PROPOLDER® MPP2020 20 (polypropylene, available from Polygroup Inc.), PROPOLDER® MPP2040 40 (polypropylene, available from Polygroup Inc.), NOVACOM® HFS2100 (maleic anhydride-functionalized high-density polyethylene polymer, available from Polygroup Inc.), KEN-REACT® CAPS® L® 12 / L (organometallic binder, available from Kenrich Petrochemicals), KEN-REACT® CAPOW® L® 12 / H (organometallic binder, available from Kenrich Petrochemicals), KEN-REACT® LICA® 12 (organometallic binder, available from Kenrich Petrochemicals), and KEN-REACT® CAPS® KPR® 12 / LV (organometallic binder, available from Kenrich Petrochemicals). Available from Petrochemicals), KEN-REACT(trademark) CAPOW(trademark) KPR(trademark) 12 / H (organometallic binder, available from Kenrich Petrochemicals), KEN-REACT(trademark) titanate & zirconate (organometallic binder, KenrichAvailable from Petrochemicals), VISTAMAXX (Trademark) (Ethylene-propylene copolymer, available from ExxonMobil), SANTOPRENE (Trademark) (Thermoplastic vulcanized rubber of ethylene-propylene-diene rubber and polypropylene, available from ExxonMobil), VISTALON (Trademark) (Ethylene-propylene-diene rubber, available from ExxonMobil), EXACT (Trademark) (Plastomer, available from ExxonMobil), EXXEL OR (trademark) (polymer resin, available from ExxonMobil), FUSABOND (trademark) M603 (random ethylene copolymer, available from Dow), FUSABOND (trademark) E226 (anhydrous modified polyethylene, available from Dow), BYNEL (trademark) 41E710 (co-extrudeable adhesive resin, available from Dow), SURLYN (trademark) 1650 (ionomer resin, available from Dow), FUSABOND (trademark) P353 (chemically modified polypropylene copolymer) (Available from Dow), ELVALOY™ PTW (ethylene terpolymer, available from Dow), ELVALOY™ 3427AC (ethylene and butyl acrylate copolymer, available from Dow), LOTADER™ AX8840 (ethylene acrylate terpolymer, available from Arkema), LOTADER™ 3210 (ethylene acrylate terpolymer, available from Arkema), LOTADER™ 3410 (ethylene acrylate terpolymer) Polymers (available from Arkema), LOTADER® 3430 (ethylene acrylate terpolymer, available from Arkema), LOTADER® 4700 (ethylene acrylate terpolymer, available from Arkema), LOTADER® AX8900 (ethylene acrylate terpolymer, available from Arkema), LOTADER® 4720 (ethylene acrylate terpolymer, available from Arkema), BAXXODUR® EC 301 (amine for epoxy, available from BASF), BAXXODUR® EC 311 (amine for epoxy, available from BASF), BAXXODUR® ECExamples include, but are not limited to, 303 (epoxy amine, available from BASF), BAXXODUR® EC 280 (epoxy amine, available from BASF), BAXXODUR® EC 201 (epoxy amine, available from BASF), BAXXODUR® EC 130 (epoxy amine, available from BASF), BAXXODUR® EC 110 (epoxy amine, available from BASF), styrene, polypropylene, polyamide, polycarbonate, EASTMAN® G-3003 (maleic anhydride grafted polypropylene, available from Eastman), RETAIN® (polymer modifier, available from Dow), AMPLIFY TY® (maleic anhydride grafted polymer, available from Dow), INTUNE® (olefin block copolymer, available from Dow), and any combination thereof.

[0058] The thermoplastic polymer 102 may have a melting point or softening temperature of about 50°C to about 450°C (or about 50°C to about 125°C, or about 100°C to about 175°C, or about 150°C to about 280°C, or about 200°C to about 350°C, or about 300°C to about 450°C).

[0059] The thermoplastic polymer 102 may have a glass transition temperature (using a heating and cooling rate of 10°C / min as defined in ASTM E1356-08 (2014)) of approximately -50°C to approximately 400°C (or approximately -50°C to approximately 0°C, or approximately -25°C to approximately 50°C, or approximately 0°C to approximately 150°C, or approximately 100°C to approximately 250°C, or approximately 150°C to approximately 300°C, or approximately 200°C to approximately 400°C).

[0060] The thermoplastic polymer 102 may optionally contain additives. Typically, the additives are present before the thermoplastic polymer 102 is added to the mixture 110. Thus, in the thermoplastic polymer molten droplets and the resulting thermoplastic polymer particles, the additives are dispersed throughout the thermoplastic polymer. For this reason, for clarity, these additives are referred to herein as “internal additives.” The internal additives may be blended with the thermoplastic polymer immediately before the mixture 110 or wells are prepared.

[0061] When describing the amounts of components in the compositions described herein (e.g., mixture 112 and colored polymer particles 124), the weight percentages based on thermoplastic polymer 102 do not include internal additives. For example, a composition containing 1% by weight of emulsifying stabilizer per 100 g of thermoplastic polymer 102, which contains 10% by weight of internal additives and 90% by weight of thermoplastic polymer, is a composition containing 0.9 g of emulsifying stabilizer, 90 g of thermoplastic polymer, and 10 g of internal additives.

[0062] The internal additive may be present in the thermoplastic polymer 102 in an amount of about 0.1% to about 60% by weight (or about 0.1% to about 5% by weight, or about 1% to about 10% by weight, or about 5% to about 20% by weight, or about 10% to about 30% by weight, or about 25% to about 50% by weight, or about 40% to about 60% by weight) of the thermoplastic polymer 102. For example, the thermoplastic polymer 102 may consist of about 70% to about 85% by weight of the thermoplastic polymer and about 15% to about 30% by weight of the internal additive, such as glass fibers or carbon fibers.

[0063] Examples of internal additives include, but are not limited to, fillers, reinforcing agents, pigments, pH adjusters, and combinations thereof. Examples of fillers include, but are not limited to, glass fibers, glass particles, mineral fibers, carbon fibers, oxide particles (e.g., titanium dioxide and zirconium dioxide), metal particles (e.g., aluminum powder), and any combination thereof. Examples of pigments include, but are not limited to, organic pigments, inorganic pigments, carbon black, and any combination thereof.

[0064] The thermoplastic polymer 102 may be present in the mixture 112 in an amount of about 5% to about 60% by weight (or about 5% to about 25% by weight, or about 10% to about 30% by weight, or about 20% to about 45% by weight, or about 25% to about 50% by weight, or about 40% to about 60% by weight) of the combined thermoplastic polymer 102 and dispersion medium 104.

[0065] A suitable dispersion medium 104 has a viscosity at 25°C of approximately 1,000 cSt to approximately 150,000 cSt (or approximately 1,000 cSt to approximately 60,000 cSt, or approximately 40,000 cSt to approximately 100,000 cSt, or approximately 75,000 cSt to approximately 150,000 cSt).

[0066] Examples of dispersion medium 104 include, but are not limited to, silicone oil, fluorinated silicone oil, perfluorinated silicone oil, polyethylene glycol, alkyl-terminated polyethylene glycol (e.g., C1-C4 terminal alkyl groups such as tetraethylene glycol dimethyl ether (TDG)), paraffin, liquid petrolatum, mink oil, turtle oil, soybean oil, perhydrosqualene, sweet almond oil, calophyllum oil, palm oil, pearl reem oil, grapeseed oil, sesame oil, corn oil, rapeseed oil, sunflower oil, cottonseed oil, apricot oil, castor oil, avocado oil, jojoba oil, olive oil, cereal germ oil, lanolinic acid esters, oleic acid esters, lauric acid esters, stearic acid esters, aliphatic esters, higher fatty acids, aliphatic alcohols, fatty acid-modified polysiloxanes, aliphatic alcohol-modified polysiloxanes, polyoxyalkylene-modified polysiloxanes, and any combination thereof. Examples of silicone oils, but not limited to, include polydimethylsiloxane (PDMS), methylphenylpolysiloxane, alkyl-modified polydimethylsiloxane, alkyl-modified methylphenylpolysiloxane, amino-modified polydimethylsiloxane, amino-modified methylphenylpolysiloxane, fluorine-modified polydimethylsiloxane, fluorine-modified methylphenylpolysiloxane, polyether-modified polydimethylsiloxane, polyether-modified methylphenylpolysiloxane, and any combination thereof. If the dispersion medium 104 contains two or more of the above, the dispersion medium 104 may have one or more phases. For example, polysiloxanes modified with fatty acids and polysiloxanes modified with aliphatic alcohols (preferably having similar chain lengths to fatty acids and aliphatic alcohols) can form a single-phase dispersion medium 104. In another example, a dispersion medium 104 containing a silicone oil and alkyl-terminated polyethylene glycol can form a two-phase dispersion medium 104.

[0067] The dispersion medium 104 may be present in the mixture 112 in an amount of about 40% to about 95% by weight (or about 75% to about 95% by weight, or about 70% to about 90% by weight, or about 55% to about 80% by weight, or about 50% to about 75% by weight, or about 40% to about 60% by weight) of the combined thermoplastic polymer 102 and dispersion medium 104.

[0068] In some cases, the dispersion medium 104 has a density of approximately 0.6 g / cm³. 3 ~Approx. 1.5g / cm 3 It may also be the case that the thermoplastic polymer 102 has a density of approximately 0.7 g / cm³. 3 ~Approx. 1.7g / cm 3 The thermoplastic polymer may have a density that is similar to, lower than, or higher than the density of the dispersion medium.

[0069] The pigment 108 should be sufficiently stable so as not to decompose at the temperature of the process 114. The pigment may yield colored, metallic, pearlescent, and / or phosphorescent particles. Examples of metallic and / or phosphorescent pigments include, but are not limited to, synthetic mica (e.g., fluorinated phlogopite), natural mica (e.g., muscovite), talc, sericite, kaolin, glass, SiO2 flakes, Al2O3 flakes, glass flakes, needle-shaped pigments (e.g., BiOCl, colored glass fibers, α-Fe2O3, and α-FeOOH), CaSO4, iron oxide, chromium oxide, carbon black, metallic effect pigments (e.g., Al flakes and bronze), optically variable pigments (OVP), liquid crystal polymer pigments (LCP), holographic pigments, titanium dioxide, titanium oxynitride, Al2O3, Fe2O3, Fe3O4, SnO2, Cr2O3, ZnO, CuO, NiO, zirconium oxide, iron oxide (iron titanate), other metal oxides, and any combination thereof. Examples of phosphorescent pigments include zinc sulfide pigments (e.g., zinc sulfide doped with copper and / or manganese); strontium aluminate pigments (e.g., SrAl2O4 doped with Eu and Dy, Sr4Al2O4 doped with Eu and Dy)14 O 25 Examples of pigments include, but are not limited to, strontium silicate pigments (e.g., Sr2MgSi2O7 doped with Dy and Eu, commercially available from USR Optonix Inc. as P170 SPS BLUE); cadmium sulfide pigments; phosphate silicate pigments; phosphate aluminate pigments; calcium silicate pigments; calcium aluminate pigments (e.g., CaAl2O4 doped with Eu and Nd); titanium aluminate pigments; titanium aluminosilicate pigments; magnesium aluminate pigments; barium aluminate pigments, and any combination thereof.

[0070] Examples of commercially available surface-treated metal and / or phosphorescent pigments include, but are not limited to, REFLEX® pigments (synthetic mica-based pearlescent pigments available from CQV), IRIODIN® (mica-based pearlescent pigments coated with metal oxides available from Merck) (e.g., IRIODIN® 300 "Gold Pearl" and IRIODIN® 100 "Silver Pearl"), SUNGEM® (glass plate-based pigments available from Sun Chemical), SUNMICA® (mica-based pigments available from Sun Chemical), SYNCRYSTAL® (synthetic fluorinated mica flakes coated with metal oxides available from Eckart), and any combination thereof. Other metallic pearlescent pigments from Merck include TIMIRON® Bronze MP60 with a D50 volume average particle size (where 50% of the pigment has a volume size less than the indicated size) of 22-37 micrometers, TIMIRON® Copper MP-65 with a D50 diameter of 22-37 micrometers, COLORONA® Oriental Beige with a D50 diameter of 3-10 micrometers, COLORONA® Aborigine Amber with a D50 diameter of 18-25 micrometers, COLORONA® Passion Orange with a D50 diameter of 18-25 micrometers, COLORONA® Bronze Fine with a D50 diameter of 7-14 micrometers, COLORONA® Bronze with a D50 diameter of 18-25 micrometers, and COLORONA® Bronze with a D50 diameter of 28-42 micrometers. COLORONA® Copper Fine (D50 diameter 7-14 micrometers), COLORONA® Copper (D50 diameter 18-25 micrometers), COLORONA® Copper Sparkle (D50 diameter 25-39 micrometers), and COLORONA® Red (D50 diameter 18-25 micrometers)This includes Brown, COLORONA® Russet with a D50 diameter of 18-25 micrometers, COLORONA® Tibetan Ochre with a D50 diameter of 18-25 micrometers, COLORONA® Sienna Fine with a D50 diameter of 7-14 micrometers, COLORONA® Sienna with a D50 diameter of 18-25 micrometers, COLORONA® Bordeaux with a D50 diameter of 18-25 micrometers, COLORONA® Glitter Bordeaux with a D50 diameter of 18-25 micrometers, and COLORONA® Chameleon with a D50 diameter of 18-25 micrometers. Furthermore, Merck mica-based pigments having a metal oxide particle coating, such as Merck silver-white pigment, are preferred. These include TIMIRON® Super Silk MP-1005 with a D50 size of 3-10 micrometers, TIMIRON® Super Sheen MP-1001 with a D50 size of 7-14 micrometers, TIMIRON® Super Silver Fine with a D50 size of 9-13 micrometers, TIMIRON® Pearl Sheen MP-30 with a D50 size of 15-21 micrometers, TIMIRON® Satin MP-11171 with a D50 size of 11-20 micrometers, TIMIRON® Ultra Luster MP-111 with a D50 size of 18-25 micrometers, TIMIRON® Star Luster MP-111 with a D50 size of 18-25 micrometers, and TIMIRON® Pearl Flake with a D50 size of 22-37 micrometers. MP-10, D50 size: TIMIRON® Super Silver (17-26 micrometers), D50 size: TIMIRON® Sparkle, MP-47, D50 size: 28-38 micrometers, D50 size: TIMIRON® ArcticExamples include Silver, XIRONA® Silver with a D50 size of 15-22 micrometers, RONASTAR® Silver with a D50 size of 25-45 micrometers, and any combination thereof. For very bright colors, Merck offers examples such as COLORONA® Carmine Red (D50 size 10-60 micrometers) which provides a red glossy effect, COLORONA® Magenta (D50 size 18-25 micrometers) which provides a pinkish-violet glossy effect, COLORONA® Light Blue (D50 size 18-25 micrometers) which provides a light blue glossy effect, COLORONA® Dark Blue (D50 size 18-25 micrometers) which provides a dark blue glossy effect, COLORONA® Majestic Green (D50 size 18-25 micrometers) which provides a green glossy effect, COLORONA® Brilliant Green (D5 size 19-26 micrometers) which provides a greenish-gold glossy effect, COLORONA® Egyptian Emerald (D50 size 18-25 micrometers) which provides a dark green glossy effect, and COLORONA® Patagonian (D50 size 18-25 micrometers) which provides a purple glossy effect. Examples include purple, and any combination thereof. Also, mica-based special effect pigments from Eckart with a D50 of approximately 18 micrometers to approximately 50 micrometers, such as DORADO® PX 4001, DORADO® PX 4261, DORADO® PX 4271, DORADO® PX 4310, DORADO® PX 4331, DORADO® PX 4542, PHOENIX® XT, PHOENIX® XT 2001, PHOENIX® XT 3001, PHOENIX® XT 4001, PHOENIX® XT 5001, PHOENIX® PX 1000, PHOENIX® PX 1001, PHOENIX® PX 1221, and PHOENIX® PX1231, PHOENIX(registered trademark) PX 1241, PHOENIX(registered trademark) PX 1251, PHOENIX(registered trademark) PX 1261, PHOENIX(registered trademark) PX 1271, PHOENIX(registered trademark) PX 1310, PHOENIX(registered trademark) PX 1320, PHOENIX(registered trademark) PX 1502, PHOENIX(registered trademark) PX 1522, PHOENIX(registered trademark) PX 1542, PHOENIX(registered trademark) PX 2000, PHOENIX(registered trademark) PX 2000 L, PHOENIX(registered trademark) PX 2001, PHOENIX(registered trademark) PX 2011, PHOENIX(registered trademark) PX 2021, PHOENIX(registered trademark) PX 2221, PHOENIX(registered trademark) PX 2231, PHOENIX(registered trademark) PX 2241, PHOENIX(registered trademark) PX 2251, PHOENIX(registered trademark) PX 2261, PHOENIX(registered trademark) PX 2271, PHOENIX(registered trademark) PX 3001, PHOENIX(registered trademark) PX 4000, PHOENIX(registered trademark) PX 4001, PHOENIX(registered trademark) PX 4221, PHOENIX(registered trademark) PX 4231, PHOENIX(registered trademark) PX 4241, PHOENIX(registered trademark) PX 4251, PHOENIX(registered trademark) PX 4261, PHOENIX(registered trademark) PX 4271, PHOENIX(registered trademark) PX 4310, PHOENIX(registered trademark) PX 4320, PHOENIX(registered trademark) PX 4502, PHOENIX(registered trademark) PX 4522, PHOENIX(registered trademark) PX 4542, PHOENIX® PX 5000, PHOENIX® PX 5001, PHOENIX® PX 5310, PHOENIX® PX5331, etc., and any combination thereof may be used. Special effect pigments such as Silverline aluminum flake pigments, e.g., DF-1667 of 16 micrometers, DF-2750 of 55 micrometers, DF-3500 of 27 micrometers, DF-3622 of 35 micrometers, DF-554 of 15 micrometers, DF-L-520AR of 20 micrometers, LED-1708AR of 20 micrometers, LED-2314AR of 13 micrometers, SILBERCOTE® PC 0452Z of 55 micrometers, SILBERCOTE® PC 1291X of 47 micrometers, SILBERCOTE® PC of 36 micrometers, SILBERCOTE® PC of 36 micrometers, SILBERCOTE® PC of 3331X of 31 micrometers, SILBERCOTE® PC of 4352Z of 33 micrometers, SILBERCOTE® PC of 33 micrometers You may use 4852X, SILBERCOTE® PC 6222X of 20 micrometers, SILBERCOTE® PC 6352Z of 27 micrometers, SILBERCOTE® PC 6802X of 25 micrometers, SILBERCOTE® PC 8152Z of 14 micrometers, SILBERCOTE® PC 8153X of 14 micrometers, SILBERCOTE® PC 8602X of 16 micrometers, SILVET® / SILVEX® 890 series of 20 micrometers, SILVET® / SILVEX® 950 series of 16 micrometers, and any combination thereof.

[0071] The pigment may have an average diameter (or D50) of approximately 1 micrometer to approximately 500 micrometers (or approximately 1 micrometer to approximately 25 micrometers, or approximately 5 micrometers to approximately 50 micrometers, or approximately 25 micrometers to approximately 200 micrometers, or approximately 100 micrometers to approximately 300 micrometers, or approximately 250 micrometers to approximately 500 micrometers).

[0072] The colored polymer particles of this disclosure may contain pigments (or cumulative pigments if more than one is used) in an amount of about 0.01% to about 30% by weight (or about 0.01% to about 1% by weight, or about 0.1% to about 5% by weight, or about 1% to about 10% by weight, or about 5% to about 20% by weight, or about 10% to about 30% by weight) of the thermoplastic polymer 102.

[0073] These colored polymer particles may contain one or more pigments. The composition and concentration of the pigments may be used to identify, track, authenticate, and / or determine the integrity of an object made from these colored polymer particles. In other words, the pigments may be used as fingerprints for identifying, tracking, and / or authenticating an object. Furthermore, the pigments may be used as indicators of parts of an object as a way to identify defects (e.g., cracks or wear) and / or the extent of such defects.

[0074] The emulsifying stabilizers used in the methods and compositions of this disclosure may include nanoparticles (e.g., oxide nanoparticles, carbon black, polymer nanoparticles, and combinations thereof), surfactants, and any combination thereof.

[0075] Oxide nanoparticles may be metal oxide nanoparticles, nonmetal oxide nanoparticles, or mixtures thereof. Examples of oxide nanoparticles include, but are not limited to, silica, titania, zirconia, alumina, iron oxide, copper oxide, tin oxide, boron oxide, cerium oxide, thallium oxide, and tungsten oxide, as well as any combination thereof. Mixed metal oxides and / or nonmetal oxides such as aluminosilicates, borosilicates, and aluminoborosilicates are also included in the term metal oxides. Oxide nanoparticles may be hydrophilic or hydrophobic, and may be natural particles or the result of surface treatment of particles. For example, silica nanoparticles having a hydrophobic surface treatment such as dimethylsilyl or trimethylsilyl may be used in the methods and compositions of this disclosure. In addition, silica with a functional surface treatment such as methacrylate functional groups may be used in the methods and compositions of this disclosure. Non-functionalized oxide nanoparticles may also be suitable for use.

[0076] Examples of commercially available silica nanoparticles include AEROSIL® (registered trademark) available from Evonik (e.g., AEROSIL® R812S (hydrophobic modified surface and 260±30m)). 2 Silica nanoparticles with an average diameter of approximately 7 nm and a BET surface area of ​​1 / g, AEROSIL® RX50 (hydrophobic modified surface and 35±10 m 2 Silica nanoparticles with an average diameter of approximately 40 nm and a BET surface area of ​​1 / g, AEROSIL® 380 (hydrophobic modified surface and 380±30m 2 Examples include, but are not limited to, silica nanoparticles having a surface area of ​​ / g, and any combination thereof.

[0077] Carbon black is another type of nanoparticle that may be present as an emulsifying stabilizer in the compositions and methods disclosed herein. Various grades of carbon black are familiar to those skilled in the art, and any of them may be used herein. Other nanoparticles capable of absorbing infrared radiation may be used similarly.

[0078] Polymer nanoparticles are another type of nanoparticle that may be present as emulsifying stabilizers in this disclosure. Suitable polymer nanoparticles may comprise one or more polymers that are thermosetting and / or crosslinked so as not to melt when treated by melt emulsification according to this disclosure. High molecular weight thermoplastic polymers having high melting or decomposition points may also constitute suitable polymer nanoparticle emulsifying stabilizers.

[0079] The nanoparticles may have an average diameter (D50 based on volume) of approximately 1 nm to approximately 500 nm (or approximately 10 nm to approximately 150 nm, or approximately 25 nm to approximately 100 nm, or approximately 100 nm to approximately 250 nm, or approximately 250 nm to approximately 500 nm).

[0080] The nanoparticles have a BET surface area of ​​approximately 10 m². 2 / g~about 500m 2 / g (or approximately 10m 2 / g~about 150m 2 / g, or approximately 25m 2 / g~about 100m 2 / g, or approximately 100m 2 / g ~ approx. 250m 2 / g, or 250m 2 / g~about 500m 2 ( / g) is also acceptable.

[0081] Nanoparticles may be included in the mixture 112 at a concentration of about 0.01% to about 10% by weight (or about 0.01% to about 1% by weight, or about 0.1% to about 3% by weight, or about 1% to about 5% by weight, or about 5% to about 10% by weight) based on the weight of the thermoplastic polymer 102.

[0082] Surfactants may be anionic, cationic, nonionic, or dipolar ionic. Examples of surfactants include, but are not limited to, sodium dodecyl sulfate, sorbitan oleate, poly[dimethylsiloxane-co-[[3-(2-(2-hydroxyethoxy)ethoxy)propylmethylsiloxane], sodium docusate (sodium 1,4-bis(2-ethylhexoxy)-1,4-dioxobutane-2-sulfonate), and any combination thereof. Examples of commercially available surfactants include, but are not limited to, CALFAX® DB-45 (sodium dodecyldiphenyl oxide disulfonate, available from Pilot Chemicals), SPAN® 80 (sorbitan maleate nonionic surfactant), MERPOL® surfactant (available from Stepan Company), TERGITOL® TMN-6 (water-soluble nonionic surfactant, available from DOW), TRITON® X-100 (octylphenol ethoxylate, available from Sigma-Aldrich), IGEPAL® CA-520 (polyoxyethylene(5) isooctylphenyl ether, available from Sigma-Aldrich), BRIJ® S10 (polyethylene glycol octadecyl ether, available from Sigma-Aldrich), and any combination thereof.

[0083] The surfactant may be present in mixture 112 at a concentration of about 0.01% to about 10% by weight (or about 0.01% to about 1% by weight, or about 0.5% to about 2% by weight, or about 1% to about 3% by weight, or about 2% to about 5% by weight, or about 5% to about 10% by weight) based on the weight of polyamide 102. Alternatively, mixture 112 may not contain (or be free of) surfactants.

[0084] The weight ratio of nanoparticles to surfactant may be approximately 1:10 to 10:1 (or approximately 1:10 to 1:1, or approximately 1:5 to 5:1, or approximately 1:1 to 10:1).

[0085] As described above, components 102, 104, and 106 may be added in any order and may include mixing and / or heating in process 110 to combine components 102, 104, and 106. For example, the emulsifying stabilizer 106 may first be dispersed in the dispersion medium 104 before the thermoplastic polymer 102 is added, optionally accompanied by heating of the dispersion. In another non-limiting example, the thermoplastic polymer 102 may be heated to produce a polymer melt, to which the dispersion medium 104 and the emulsifying stabilizer 106 may be added together or in any order. In yet another non-limiting example, the thermoplastic polymer 102 and the dispersion medium 104 may be mixed at a temperature above the melting point or softening temperature of the thermoplastic polymer 102 and at a shear rate sufficient to disperse the thermoplastic polymer melt in the dispersion medium 104. The emulsifying stabilizer 106 can then be added to form a mixture 112, which can be maintained under suitable process conditions for a set period of time.

[0086] The combination of components 102, 104, and 106 in any combination 110 may be carried out in the mixing apparatus used for process 114 and / or another suitable container. In non-limiting examples, the thermoplastic polymer 102 may be heated in the mixing apparatus used for process 114 to a temperature above the melting point or softening temperature of the thermoplastic polymer 102, and the emulsifying stabilizer 106 may be dispersed in the dispersion medium 104 in a separate container. The dispersion may then be added to the molten thermoplastic polymer 102 in the mixing apparatus used for process 114.

[0087] The mixing apparatus used in process 114 to produce the molten emulsion 116 should be able to maintain the molten emulsion 116 at a temperature above the melting point or softening temperature of the thermoplastic polymer 102 and apply a shear rate sufficient to disperse the polymer molten material as droplets in the dispersion medium 104.

[0088] Examples of mixing equipment used in the process 114 for producing the molten emulsion 116 include, but are not limited to, extruders (e.g., continuous extruders, batch extruders, etc.), agitated reactors, blenders, reactors equipped with inline homogenizer systems, and equipment derived therefrom.

[0089] Processing 114 under suitable process conditions (e.g., temperature, shear rate, etc.) for a set period of time, and formation of a molten emulsion 116.

[0090] The temperature at which the treatment 114 and the molten emulsion 116 are formed should be above the melting or softening temperature of the thermoplastic polymer 102 and below the decomposition temperature of any of the components 102, 104, and 106 in the mixture 112. For example, the temperature at which the treatment 114 and the molten emulsion 116 are formed may be about 1°C to about 50°C (or about 1°C to about 25°C, or about 5°C to about 30°C, or about 20°C to about 50°C) above the melting or softening temperature of the thermoplastic polymer 102, provided that the temperature at which the treatment 114 and the molten emulsion 116 are formed is below the decomposition temperature of any of the components 102, 104, and 106 in the mixture 112.

[0091] The shear rate of the process 114 and the formation of the molten emulsion 116 should be high enough to disperse the polymer melt as droplets in the dispersion medium 104. These droplets should include droplets with a diameter of about 1000 μm or less (or about 1 μm to about 1000 μm, or about 1 μm to about 50 μm, or about 10 μm to about 100 μm, or about 10 μm to about 250 μm, or about 50 μm to about 500 μm, or about 250 μm to about 750 μm, or about 500 μm to about 1000 μm).

[0092] The time for maintaining the temperature and shear rate for the process 114 and the formation of the molten emulsion 116 may be 10 seconds to 18 hours or more (or 10 seconds to 30 minutes, or 5 minutes to 1 hour, or 15 minutes to 2 hours, or 1 hour to 6 hours, or 3 hours to 18 hours). Although not bound by theory, it is considered that the steady state of the droplet diameter will be reached at the point when the process 114 can be stopped. That time may depend, in particular, on the temperature, shear rate, the composition of the thermoplastic polymer 102, the composition of the dispersion medium 104, and the composition of the emulsifying stabilizer 106.

[0093] The molten emulsion 116 may then be cooled 118. The cooling 118 can be slow (e.g., allowing the molten emulsion to be cooled under ambient conditions) or fast (e.g., rapid cooling). For example, the cooling rate may range from about 10°C / hour to about 100°C / second, or even nearly instantaneous by rapid cooling (e.g., dry ice) (or about 10°C / hour to about 60°C / hour, or about 0.5°C / min to about 20°C / min, or about 1°C / min to about 5°C / min, or about 10°C / min to about 60°C / min, or about 0.5°C / second to about 10°C / second, or about 10°C / second to about 100°C / second).

[0094] During cooling, shear force may be applied little to no to the molten emulsion 116. In some cases, the shear force applied during heating may be applied during cooling.

[0095] The cooled mixture 120 obtained from the cooling 118 of the molten emulsion 116 contains solidified colored polymer particles 124 and other components 126 (e.g., dispersion medium 104, excess emulsifying stabilizer 106, etc.). The thermoplastic polymer particles may be dispersed in the dispersion medium or settled in the dispersion medium.

[0096] The cooled mixture 120 may then be processed 122 to separate the colored polymer particles 124 from the other components 126. Suitable processes include, but are not limited to, washing, filtering, centrifugation, and decanting, as well as any combination thereof.

[0097] The solvent used to wash the colored polymer particles 124 should generally be (a) miscible with the dispersion medium 104 and (b) nonreactive (e.g., non-swelling and non-soluble) with the thermoplastic polymer 102. The choice of solvent will depend, in particular, on the composition of the dispersion medium and the composition of the thermoplastic polymer 102.

[0098] Examples of solvents include, but are not limited to, hydrocarbon solvents (e.g., pentane, hexane, heptane, octane, cyclohexane, cyclopentane, decane, dodecane, tridecane, and tetradecane), aromatic hydrocarbon solvents (e.g., benzene, toluene, xylene, 2-methylnaphthalene, and cresol), ether solvents (e.g., diethyl ether, tetrahydrofuran, diisopropyl ether, and dioxane), ketone solvents (e.g., acetone and methyl ethyl ketone), alcohol solvents (e.g., methanol, ethanol, isopropanol, and n-propanol), ester solvents (e.g., ethyl acetate, methyl acetate, butyl acetate, butyl propionate, and butyl butyrate), halogenated solvents (e.g., chloroform, bromoform, 1,2-dichloromethane, 1,2-dichloroethane, carbon tetrachloride, chlorobenzene, and hexafluoroisopropanol), water, and any combination thereof.

[0099] The solvent may be removed from the colored polymer particles 124 by drying using a suitable method such as air drying, heat drying, vacuum drying, freeze-drying, or a hybrid thereof. Heating may preferably be carried out at a temperature lower than the glass transition temperature of the thermoplastic polymer (e.g., about 50°C to about 150°C).

[0100] Advantageously, the dispersion medium and washing solvent of the systems and methods described herein (e.g., Method 100) can be regenerated and reused. Those skilled in the art will recognize any necessary washing of the used dispersion medium and solvent required for the regeneration process.

[0101] The colored polymer particles 124, after being separated from the other components 126, may be optionally further purified 128. For example, to narrow the particle size distribution (or reduce the diameter span), the colored polymer particles 124 can be passed through a sieve with a pore size of approximately 10 μm to approximately 250 μm (or approximately 10 μm to approximately 100 μm, or approximately 50 μm to approximately 200 μm, or approximately 150 μm to approximately 250 μm).

[0102] In another exemplary purification technique, the colored polymer particles 124 may be washed with water to remove the surfactant while retaining substantially all of the nanoparticles associated with the surface of the colored polymer particles 124. In yet another exemplary purification technique, the colored polymer particles 124 may be blended with an additive to obtain the desired final product. For clarity, such an additive is referred to herein as an “external additive” because it is blended with the thermoplastic particles 124 or other particles obtained by the method described herein after the particles have solidified. Examples of external additives include flow aids, other polymer particles, fillers, and any combination thereof.

[0103] In some cases, the surfactants used to produce the colored polymer particles 124 may be undesirable in downstream applications. Therefore, yet another exemplary purification technique may include removing the surfactant from the colored polymer particles 124 (e.g., by washing and / or thermal decomposition).

[0104] The colored polymer particles 124 and / or purified colored polymer particles 130 (referred to as colored polymer particles 124 / 130) may be characterized by their composition, physical structure, etc.

[0105] As described above, the emulsifying stabilizer is located at the interface between the polymer melt and the dispersion medium. As a result, when the mixture cools, the emulsifying stabilizer remains at or near the interface. Therefore, the structure of the colored polymer particles 124 / 130 generally includes, when the emulsifying stabilizer is used, (a) the emulsifying stabilizer dispersed on the outer surface of the colored polymer particles 124 / 130 and / or (b) the emulsifying stabilizer embedded in the outer portion (e.g., outer 1 vol%) of the colored polymer particles 124 / 130.

[0106] Furthermore, if voids are formed inside the polymer molten droplets, the emulsifying stabilizer 106 should generally be located at (and / or embedded in) the interface between the void and the thermoplastic polymer. The voids generally do not contain the thermoplastic polymer. Rather, the voids may contain, for example, the dispersion medium, air, or be empty. The colored polymer particles 124 / 130 may contain the dispersion medium in an amount of about 5% by weight or less of the colored polymer particles 124 / 130 (or about 0.001% to about 5% by weight, or about 0.001% to about 0.1% by weight, or about 0.01% to about 0.5% by weight, or about 0.1% to about 2% by weight, or about 1% to about 5% by weight).

[0107] The thermoplastic polymer 102 may be present in the colored polymer particles 124 / 130 in an amount of about 90% to about 99.5% by weight (or about 90% to about 95% by weight, or about 92% to about 97% by weight, or about 95% to about 99.5% by weight) of the colored polymer particles 124 / 130.

[0108] If present, the emulsifying stabilizer 106 may be present in the colored polymer particles 124 / 130 in amounts of about 10% by weight or less (or about 0.01% to about 10% by weight, or about 0.01% to about 1% by weight, or about 0.5% to about 5% by weight, or about 3% to about 7% by weight, or about 5% to about 10% by weight). After purification to remove at least substantially any surfactant or other emulsifying stabilizer, the emulsifying stabilizer 106 may be present in the particles 130 / 136 in amounts of less than 0.01% by weight (or 0% to about 0.01% by weight, or 0% to 0.001% by weight).

[0109] When using particulate emulsifying stabilizers to form thermoplastic microparticles according to the disclosure herein, at least a portion of the particulate emulsifying stabilizer, such as silica nanoparticles, may be arranged as a coating on the outer surface of the thermoplastic particles (and coated pigments, if manufactured). At least a portion of the surfactant, if used, may similarly associate on the outer surface. The coating may be distributed substantially uniformly on the outer surface. When used herein with respect to coatings, the term “substantially uniform” means a uniform coating thickness on the surface area covered by the coating composition (e.g., nanoparticles and / or surfactant), particularly over the entire outer surface. The emulsifying stabilizer 106 may form a coating covering at least 5% (or about 5% to about 100%, or about 5% to about 25%, or about 20% to about 50%, or about 40% to about 70%, or about 50% to about 80%, or about 60% to about 90%, or about 70% to about 100%) of the surface area of ​​the colored polymer particles 124 / 130. After purification to remove at least substantially any surfactant or other emulsifying stabilizer, the emulsifying stabilizer 106 may be present in particles 130 / 136 in an area of ​​less than 25% of the surface area of ​​particles 130 / 136 (or 0% to about 25%, or about 0.1% to about 5%, or about 0.1% to about 1%, or about 1% to about 5%, or about 1% to about 10%, or about 5% to about 15%, or about 10% to about 25%). The coverage of the emulsifying stabilizer 106 on the outer surface of the colored polymer particles 124 / 130 may be determined using analysis of scanning electron microscope images (SEM images). The emulsifying stabilizer 106 may form a coating covering at least 5% (or about 5% to about 100%, or about 5% to about 25%, or about 20% to about 50%, or about 40% to about 70%, or about 50% to about 80%, or about 60% to about 90%, or about 70% to about 100%) of the surface area of ​​the colored polymer particles 124 / 130 (and coated pigments, if manufactured). After purification to remove at least substantially any surfactant or other emulsifying stabilizer, the emulsifying stabilizer 106 may be present in particles 130 / 136 in amounts less than 25% (or 0% to about 25%, or about 0.1% to about 5%, or about 0.1% to about 1%, or about 1% to about 5%, or about 1% to about 10%, or about 5% to about 15%, or about 10% to about 25%) of the surface area of ​​particles 130 / 136.The coverage rate of the emulsifier stabilizer 106 on the outer surface of the colored polymer particles 124 / 130 may be determined using image analysis of SEM micrographs.

[0110] The colored polymer particles 124 / 130 may have a D10 of about 0.1 μm to about 125 μm (or about 0.1 μm to about 5 μm, about 1 μm to about 10 μm, about 5 μm to about 30 μm, or about 1 μm to about 25 μm, or about 25 μm to about 75 μm, or about 50 μm to about 85 μm, or about 75 μm to about 125 μm), a D50 of about 0.5 μm to about 200 μm (or about 0.5 μm to about 10 μm, or about 5 μm to about 50 μm, or about 30 μm to about 100 μm, or about 30 μm to about 70 μm, or about 25 μm to about 50 μm, or about 50 μm to about 100 μm, or about 75 μm to about 150 μm, or about 100 μm to about 200 μm), and a D90 of about 3 μm to about 300 μm (or about 3 μm to about 15 μm, or about 10 μm to about 50 μm, or about 25 μm to about 75 μm, or about 70 μm to about 200 μm, or about 60 μm to about 150 μm, or about 150 μm to about 300 μm), with D10 < D50 < D90. The colored polymer particles 124 / 130 may also have a diameter span of about 0.2 to about 10 (or about 0.2 to about 0.5, or about 0.4 to about 0.8, or about 0.5 to about 1.0, or about 1 to about 3, or about 2 to about 5, or about 5 to about 10). Without limitation, a diameter span value of 1.0 or greater is considered broad, and a diameter span value of 0.75 or less is considered narrow.

[0111] In a first non-limiting example, the colored polymer particles 124 / 130 may have a D10 of about 0.1 μm to about 10 μm, a D50 of about 0.5 μm to about 25 μm, a D90 of about 3 μm to about 50 μm, and D10 < D50 < D90. The colored polymer particles 124 / 130 may have a diameter span of about 0.2 to about 2.

[0112] In a second non-limiting example, the colored polymer particles 124 / 130 may have a D10 of about 5 μm to about 30 μm, a D50 of about 30 μm to about 70 μm, a D90 of about 70 μm to about 120 μm, and D10 < D50 < D90. The colored polymer particles 124 / 130 may have a diameter span of about 1.0 to about 2.5.

[0113] In a third non-limiting example, the colored polymer particles 124 / 130 may have a D10 of about 25 μm to about 60 μm, a D50 of about 60 μm to about 110 μm, a D90 of about 110 μm to about 175 μm, and D10 < D50 < D90. The colored polymer particles 124 / 130 may have a diameter span of about 0.6 to about 1.5.

[0114] In a fourth non-limiting example, the colored polymer particles 124 / 130 may have a D10 of about 75 μm to about 125 μm, a D50 of about 100 μm to about 200 μm, a D90 of about 125 μm to about 300 μm, and D10 < D50 < D90. The colored polymer particles 124 / 130 may have a diameter span of about 0.2 to about 1.2.

[0115] In a fifth non-limiting example, the colored polymer particles 124 / 130 may have a D10 of about 1 μm to about 50 μm (or about 5 μm to about 30 μm, or about 1 μm to about 25 μm, or about 25 μm to about 50 μm), a D50 of about 25 μm to about 100 μm (or about 30 μm to about 100 μm, or about 30 μm to about 70 μm, or about 25 μm to about 50 μm, or about 50 μm to about 100 μm), a D90 of about 60 μm to about 300 μm (or about 70 μm to about 200 μm, or about 60 μm to about 150 μm, or about 150 μm to about 300 μm), and D10 < D50 < D90. The colored polymer particles 124 / 130 may also have a diameter span of about 0.4 to about 3 (or about 0.6 to about 2, or about 0.4 to about 1.5, or about 1 to about 3).

[0116] The colored polymer particles 124 / 130 may have a roundness of approximately 0.9 or higher (or approximately 0.90 to approximately 1.0, or approximately 0.93 to approximately 0.99, or approximately 0.95 to approximately 0.99, or approximately 0.97 to approximately 0.99, or approximately 0.98 to approximately 1.0).

[0117] The colored polymer particles 124 / 130 may have an angle of repose of approximately 25° to approximately 45° (or approximately 25° to approximately 35°, or approximately 30° to approximately 40°, or approximately 35° to approximately 45°).

[0118] The colored polymer particles 124 / 130 may have a Hausner ratio of approximately 1.0 to approximately 1.5 (or approximately 1.0 to approximately 1.2, or approximately 1.1 to approximately 1.3, or approximately 1.2 to approximately 1.35, or approximately 1.3 to approximately 1.5).

[0119] The colored polymer particles 124 / 130 have a bulk density of approximately 0.3 g / cm³. 3 ~about 0.8g / cm 3 (or approximately 0.3 g / cm³) 3 ~about 0.6g / cm 3 , or approximately 0.4 g / cm³ 3 ~about 0.7g / cm 3 , or approximately 0.5 g / cm³ 3 ~about 0.6g / cm 3 , or approximately 0.5 g / cm³ 3 ~about 0.8g / cm 3 That's fine.

[0120] Depending on the temperature and shear rate of treatment 114, and the composition and relative concentration of components 102, 104, and 106, different structural shapes constituting the colored polymer particles 124 / 130 have been observed. Typically, the colored polymer particles 124 / 130 include substantially spherical particles (roundness of about 0.97 or greater). However, other structures, including disc-shaped and elongated structures, have been observed in the colored polymer particles 124 / 130. Therefore, the colored polymer particles 124 / 130 may include one or more of the following: (a) substantially spherical particles with roundness of 0.97 or greater, (b) disc-shaped structures with an aspect ratio of about 2 to about 10, and (c) elongated structures with an aspect ratio of 10 or greater. Each of the above structures (a), (b), and (c) has an emulsifying stabilizer dispersed on the outer surface of the structure (a), (b), and (c), and / or embedded in the outer portion of the structure (a), (b), and (c). At least some of the structures (a), (b), and (c) may aggregate. For example, the elongated structure of (c) may be located on the surface of the substantially spherical particles of (a).

[0121] The colored polymer particles 124 / 130 may have a sintering window within 10°C, preferably within 5°C, of ​​the sintering window of the thermoplastic polymer. Applications of colored polymer particles

[0122] The colored polymer particles described herein may be used to manufacture a variety of articles. In non-limiting examples, a 3D printing process of this disclosure may include depositing the colored polymer particles described herein onto a surface (e.g., in layers and / or in a particular shape), and, after deposit, heating at least a portion of the particles to promote solidification of the particles and form a solidified body (or object). The solidified body may have a porosity of about 5% or less after solidification (e.g., 0% to about 5%, or about 0.5% to about 2%, or about 1% to about 3%, or about 2% to about 5%). For example, heating and solidification of thermoplastic polymer particles may be carried out in a laser-based 3D printing apparatus such that heating and solidification are performed by selective laser sintering.

[0123] Examples of articles that can be formed in whole or in part using these colored polymer particles, and that can be manufactured by such method, include, but are not limited to, particles, films, packaging materials, toys, household goods, automotive parts, aerospace / aircraft parts, containers (e.g., for food, beverages, cosmetics, personal care compositions, pharmaceuticals, etc.), shoe soles, furniture parts, decorative household goods, plastic gears, screws, nuts, bolts, cable ties, jewelry, works of art, statues, medical items, prosthetic devices, orthopedic implants, the manufacture of artifacts to aid learning in education, 3D anatomical models to assist in surgery, robotics supplies, biomedical devices (orthotics), household appliances, dental supplies, electronic equipment, and sporting goods. Furthermore, the particles may be useful in applications such as, but are not limited to, paints, powder coatings, inkjet materials, electrophotographic toners, and 3D printing.

[0124] In addition to the colored polymer particles described herein, the object may have a specific fingerprint (e.g., a color spectrum, phosphorescence, etc., and any combination thereof) that is useful for identifying, tracking, authenticating, and / or determining the integrity of the object. Furthermore, the arrangement of the colored polymer particles or portions(s) of the object formed therefrom may be located within the object as another layer that identifies the object for identification, tracking, authenticating, and / or determining the integrity of the object.

[0125] A method for identifying, tracking, authenticating, and / or determining the integrity of an object may include (a) exposing an object containing or manufactured from the colored polymer particles to an excitation source (e.g., broad-spectrum light, ultraviolet light, specific wavelengths of light, etc.), (b) detecting one or more spectra related to color and / or phosphorescence, and (c) comparing the spectra to known spectra of pigments used in the object or a part thereof. Optionally, the location of the spectral region on the object may be compared to known locations where the spectral region should be. The comparison(s) can be used to identify and / or authenticate the object. For tracking purposes, the comparison(s) may be performed, and / or the detected spectra and / or spectral regions may be recorded in a database along with the physical location of the object. Furthermore, the integrity of objects that wear and / or crack can be verified. For example, the core portion of the article may contain or be formed from the colored polymer particles, while the outer portion may cover the core portion and may not contain or be formed from the colored polymer particles. Subsequently, the appearance of color and / or phosphorescence may indicate that the object is nearing the end of its lifespan. Exemplary Embodiments

[0126] The first non-limiting exemplary embodiment is a composition comprising colored polymer particles comprising a thermoplastic polymer and a pigment in a melt-emulsified form (e.g., a colored pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof). The first non-limiting exemplary embodiment may include one or more of the following: Element 1, wherein the melt-emulsified form has a coating comprising a thermoplastic polymer and a coated pigment attached to the thermoplastic polymer particles; Element 2, which is Element 1 and the coating has an emulsifier stabilizer coating (e.g., the emulsifier stabilizer may be embedded in the coating of the pigment); Element 3, wherein the pigment is embedded in the outer surface of the thermoplastic polymer particles; Element 4, wherein the pigment is encapsulated by the thermoplastic polymer particles; Element 5, wherein the composition has a coating and further comprises a pigment that is neither attached to, embedded in, nor encapsulated by the thermoplastic polymer particles; Element 6, which is Element 5 and the coating of the pigment has an emulsifier stabilizer coating (e.g., the emulsifier stabilizer may be embedded in the coating of the pigment); Element 7, wherein the colored polymer particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, a D90 of about 3 μm to about 300 μm, and D10 < D50 < D90; Element 8, wherein the colored polymer particles have a diameter span of about 0.2 to about 10; Element 9, wherein the colored polymer particles have a diameter span of about 1.0 to about 1.5; Element 10, wherein the colored polymer particles have an emulsifier stabilizer coating; Element 11, which is Element 10 and the emulsifier stabilizer comprises nanoparticles and includes the nanoparticles, and at least a portion of the emulsifier stabilizer is embedded in the outer surface of the colored polymer particles; Element 12, which is Element 10 and at least a portion of the colored polymer particles have voids containing an emulsifier stabilizer at the void / polymer interface; Element 13, which is Element 12 and the emulsifier stabilizer comprises nanoparticles and the nanoparticles are embedded at the void / polymer interface; and Element 14, which is Element 12 and the voids contain a dispersion medium.Examples of combinations include, but are not limited to, combinations of element 1 (arbitrarily combined with element 2) with one or more elements from 3 to 14; combinations of element 3 with one or more elements from 4 to 14; combinations of element 4 with one or more elements from 5 to 14; combinations of element 5 (arbitrarily combined with element 6) with one or more elements from 7 to 14; combinations of element 7 with one or more elements from 8 to 14; combinations of element 8 with one or more elements from 9 to 14; combinations of element 9 with one or more elements from 10 to 14; combinations of element 10 with element 11 and / or 12, and when combined with element 12, further combinations with element 13 and / or 14 (arbitrarily combined with element 6); and combinations of two or more elements from element 1 (arbitrarily combined with element 2), element 3, element 4, and element 5 (arbitrarily combined with element 6).

[0127] A second non-limiting exemplary embodiment is a composition comprising colored polymer particles comprising a thermoplastic polymer and a pigment (e.g., a colored pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof), wherein at least a portion of the colored polymer particles have a form that conforms to (a), (b), (c), or any combination thereof: (a) the pigment has a coating comprising a thermoplastic polymer, and the coated pigment is attached to the thermoplastic polymer particle; (b) the pigment is embedded in the outer surface of the thermoplastic polymer particle; and (c) the pigment is encapsulated by the thermoplastic polymer particle. The second non-limiting exemplary embodiment may also include one or more of elements 2; 5; 6; 7; 8; 9; 10; 11; 12; 13; and 14, including any combination of the first non-limiting exemplary embodiment.

[0128] A third non-limiting exemplary embodiment is a method comprising depositing colored polymer particles of the first or second non-limiting exemplary embodiment (optionally combined with one or more of elements 1 to 14) on a surface in combination with other thermoplastic polymer particles, and after deposition, heating at least a portion of the particles to promote solidification of the particles and form a solidified body.

[0129] A fourth non-limiting exemplary embodiment is a method comprising: mixing a mixture of a thermoplastic polymer, a dispersion medium that is miscible with the thermoplastic polymer, a pigment (e.g., a color pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof), and optionally an emulsifying stabilizer, at a temperature higher than the melting or softening temperature of the thermoplastic polymer and at a shear rate high enough to disperse the thermoplastic polymer in the dispersion medium; cooling the mixture to below the melting or softening temperature of the thermoplastic polymer to form colored polymer particles containing the thermoplastic polymer and a pigment having a molten emulsion form; and separating the colored polymer particles from the dispersion medium.

[0130] A fifth non-limiting exemplary embodiment is a method comprising: mixing a mixture of a thermoplastic polymer, a dispersion medium immiscible with the thermoplastic polymer, a pigment (e.g., a color pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof), and optionally an emulsifying stabilizer, at a temperature higher than the melting or softening temperature of the thermoplastic polymer and at a shear rate high enough to disperse the thermoplastic polymer in the dispersion medium; and cooling the mixture to below the melting or softening temperature of the thermoplastic polymer to form colored polymer particles comprising the thermoplastic polymer and the pigment, wherein at least a portion of the colored polymer particles are in a form conforming to (a), (b), (c), or any combination thereof: (a) the pigment has a coating comprising the thermoplastic polymer and the coated pigment is attached to the thermoplastic polymer particles; (b) the pigment is embedded on the outer surface of the thermoplastic polymer particles; and (c) the pigment is encapsulated by the thermoplastic polymer particles; and separating the colored polymer particles from the dispersion medium.

[0131] A fourth or fifth non-limiting exemplary embodiment may include one or more of the following: Element 1; Element 2; Element 3; Element 4; Element 5; Element 6; Element 7; Element 8; Element 9; Element 15, wherein the pigment is a first pigment and the mixture further comprises a second pigment different from the first pigment; Element 16, wherein the colored polymer particles contain 0.01% to 30% by weight of the pigment based on the weight of the thermoplastic polymer in the colored polymer particles; Element 17, wherein the mixture contains an emulsifying stabilizer that coats at least a portion of the outer surface of the colored polymer particles; and Element 18, which is Element 17, wherein the emulsifying stabilizer is embedded in the outer surface. Examples of combinations include, but are not limited to, combinations of two or more elements from element 1 (arbitrarily combined with element 2), element 3, element 4, and element 5; combinations of one or more elements from elements 1 to 6 with one or more elements from elements 7 to 9 and 15 to 18; combinations of element 7 with one or more elements from elements 8 to 9 and 15 to 18; combinations of element 8 with element 9 and one or more elements from 15 to 18; combinations of element 9 with one or more elements from elements 15 to 18; combinations of element 15 with one or more elements from elements 16 to 18; and combinations of two or more elements from elements 16 to 18. Clause

[0132] Clause 1. A composition comprising a thermoplastic polymer and colored polymer particles containing a pigment having a molten emulsion form (e.g., a colored pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof).

[0133] Clause 2. The composition according to Clause 1, wherein the molten emulsion form comprises a pigment having a coating containing a thermoplastic polymer, the coated pigment adhering to the outer surface of thermoplastic polymer particles.

[0134] Clause 3. The composition according to Clause 2, wherein the coating has an emulsifying stabilizer coating.

[0135] Clause 4. The composition according to Clause 1, wherein the molten emulsion form comprises a pigment embedded on the outer surface of thermoplastic polymer particles.

[0136] Clause 5. The composition according to Clause 1, wherein the molten emulsion form comprises a pigment encapsulated by thermoplastic polymer particles.

[0137] Clause 6. The composition according to Clause 1, further comprising a pigment having a coating and not being attached to, embedded in, or encapsulated on thermoplastic polymer particles.

[0138] Clause 7. The composition according to Clause 6, wherein the pigment coating has an emulsifying stabilizer coating.

[0139] Clause 8. The composition according to Clause 1, wherein the colored polymer particles have a roundness of about 0.90 to about 1.0.

[0140] Clause 9. The composition according to Clause 1, wherein the colored polymer particles have an emulsifying stabilizer that coats at least a portion of the outer surface of the colored polymer particles.

[0141] Clause 10. The composition according to Clause 9, wherein the emulsifying stabilizer comprises nanoparticles and said nanoparticles, and at least a portion of the emulsifying stabilizer is embedded on the outer surface of the colored polymer particles.

[0142] Clause 11. The composition according to Clause 9, wherein at least a portion of the colored polymer particles have voids containing an emulsifying stabilizer at the void / polymer interface.

[0143] Clause 12. The composition according to Clause 11, wherein the emulsifying stabilizer comprises nanoparticles, the nanoparticles being embedded in the void / polymer interface.

[0144] Clause 13. The composition according to Clause 11, wherein the voids contain a dispersion medium.

[0145] Clause 14. A method comprising: depositing colored polymer particles as described in Clause 1 on a surface in an optional combination with other thermoplastic polymer particles; and, after deposition, heating at least a portion of the particles to promote solidification of the particles and form a solidified body.

[0146] Clause 15. A composition comprising colored polymer particles comprising a thermoplastic polymer and a pigment (e.g., a colored pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof), wherein at least a portion of the colored polymer particles are in a form conforming to (a), (b), (c), or any combination thereof: (a) the pigment has a coating comprising a thermoplastic polymer, and the coated pigment is attached to the thermoplastic polymer particles; (b) the pigment is embedded on the outer surface of the thermoplastic polymer particles; and (c) the pigment is encapsulated by the thermoplastic polymer particles.

[0147] The composition according to Clause 15, wherein a form exists in which the pigment coating has an emulsifying stabilizer coating.

[0148] Clause 17. The composition according to Clause 15, further comprising a pigment having a coating and not being attached to, embedded in, or encapsulated on thermoplastic polymer particles.

[0149] Clause 18. The composition according to Clause 17, wherein the pigment coating has an emulsifying stabilizer coating.

[0150] Clause 19. The composition according to Clause 15, wherein the colored polymer particles have a roundness of about 0.90 to about 1.0.

[0151] Clause 20. The composition according to Clause 15, wherein the colored polymer particles have an emulsifying stabilizer that coats at least a portion of the outer surface of the colored polymer particles.

[0152] Clause 21. The composition according to Clause 20, wherein the emulsifying stabilizer comprises nanoparticles and said nanoparticles, and at least a portion of the emulsifying stabilizer is embedded on the outer surface of colored polymer particles.

[0153] Clause 22. The composition according to Clause 20, wherein at least a portion of the colored polymer particles have voids containing an emulsifying stabilizer at the void / polymer interface.

[0154] Clause 23. The composition according to Clause 22, wherein the emulsifying stabilizer comprises nanoparticles, the nanoparticles being embedded in the void / polymer interface.

[0155] Clause 24. The composition according to Clause 22, wherein the voids contain a dispersion medium.

[0156] Clause 25. A method comprising depositing colored polymer particles as described in Clause 1 on a surface in combination with other thermoplastic polymer particles as optional, and after deposition, heating at least a portion of the particles to promote solidification of the particles and form a solidified body.

[0157] Clause 26. A method comprising: mixing a mixture comprising a thermoplastic polymer, a dispersion medium that is miscible with the thermoplastic polymer, a pigment (e.g., a color pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof), and optionally an emulsifying stabilizer, at a temperature higher than the melting or softening temperature of the thermoplastic polymer and at a shear rate high enough to disperse the thermoplastic polymer in the dispersion medium; cooling the mixture to below the melting or softening temperature of the thermoplastic polymer to form colored polymer particles comprising the thermoplastic polymer and a pigment having a molten emulsion form; and separating the colored polymer particles from the dispersion medium.

[0158] Clause 27. A method comprising: mixing a mixture comprising a thermoplastic polymer, a dispersion medium that is miscible with the thermoplastic polymer, a pigment (e.g., a color pigment, a metallic pigment, a pearlescent pigment, a phosphorescent pigment, or any combination thereof), and optionally an emulsifying stabilizer, at a temperature higher than the melting or softening temperature of the thermoplastic polymer and at a shear rate high enough to disperse the thermoplastic polymer in the dispersion medium; and cooling the mixture to below the melting or softening temperature of the thermoplastic polymer to form colored polymer particles comprising the thermoplastic polymer and the pigment, wherein at least a portion of the colored polymer particles are in a form conforming to (a), (b), (c), or any combination thereof: (a) the pigment has a coating comprising the thermoplastic polymer and the coated pigment is attached to the thermoplastic polymer particles; (b) the pigment is embedded on the outer surface of the thermoplastic polymer particles; and (c) the pigment is encapsulated by the thermoplastic polymer particles; and separating the colored polymer particles from the dispersion medium.

[0159] Clause 28. The method according to Clause 26 or 27, wherein the pigment is a first pigment, and the mixture further comprises a second pigment different from the first pigment.

[0160] Clause 29. The method according to Clause 26 or 27, wherein the colored polymer particles contain 0.01% to 30% by weight of pigment, based on the weight of the thermoplastic polymer in the colored polymer particles.

[0161] Clause 30. The method according to Clause 26 or 27, wherein an emulsifying stabilizer is included in the mixture, and the emulsifying stabilizer coats at least a portion of the outer surface of the colored polymer particles.

[0162] Clause 31. The method according to Clause 30, wherein an emulsifying stabilizer is embedded on the outer surface.

[0163] Clause 32. The method according to clause 26 or 27, wherein the colored polymer particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, a D90 of about 3 μm to about 300 μm, and D10 < D50 < D90.

[0164] Clause 33. The method according to clause 26 or 27, wherein the colored polymer particles have a diameter span of about 0.2 to about 10.

[0165] Clause 34. The method according to clause 26 or 27, wherein the colored polymer particles have a circularity of about 0.90 to about 1.0.

[0166] Clause 35. The method according to clause 26 or 27, wherein the colored polymer particles have a Hausner ratio of about 1.0 to about 1.5.

[0167] Clause 36. The method according to clause 26 or 27, wherein the melt-emulsion form contains a pigment having a coating containing a thermoplastic polymer, and the coated pigment is attached to the outer surface of the thermoplastic polymer particles.

[0168] Clause 37. The method according to clause 26 or 27, wherein the melt-emulsion form contains a pigment embedded in the outer surface of the thermoplastic polymer particles.

[0169] Clause 38. The method according to clause 26 or 27, wherein the melt-emulsion form contains a pigment encapsulated by the thermoplastic polymer particles.

[0170] Unless otherwise stated, all figures used in this specification and related claims, such as quantities of components, molecular weights and other properties, process conditions, etc., should be understood in all cases to be modified by the term "approximately." Therefore, unless otherwise indicated, the numerical parameters described in the following specification and appended claims are approximations that may vary depending on the desired properties to be obtained by embodiments of the present invention. At the very least, without attempting to limit the application of the doctrine of equivalents to the claims, each numerical parameter should be interpreted by applying the usual rounding method in light of the number of significant figures reported.

[0171] One or more exemplary embodiments incorporating embodiments of the present invention disclosed herein are presented herein. For clarity, not all features of physical implementations are described or represented in this application. It is understood that in developing physical implementations incorporating embodiments of the present invention, numerous implementation-specific decisions must be made to achieve the developer's objectives, such as compliance with system-related, business-related, government-related, and other constraints, which vary by implementation and time. While the developer's efforts may be time-consuming, such efforts are routine for those skilled in the art and will benefit from this disclosure.

[0172] Although compositions and methods are described herein using the term “containing” various components or processes, compositions and methods may also “essentially consist of” or “consist of” various components and processes.

[0173] To facilitate a better understanding of the embodiments of the present invention, the following examples of preferred or representative embodiments are provided. The following examples should not be interpreted in any way as limiting or defining the scope of the present invention. [Examples]

[0174] 117 g of PDMS (PSF® 30,000 cSt, available from Clearco) was added to a 1-1,500 mL glass reactor containing a control sample. A slurry was prepared by mixing approximately 20 g of the measured PDMS with 0.75 g of AEROSIL® RX50 fumed silica. This slurry was added to the glass reactor, followed by 50 g of polypropylene homopolymer resin (ULTRA HOPP® 20, manufactured by ResMart). The reactor was heated to 250°C with one P4 shaft set to 150 revolutions per minute (rpm). Once this temperature was reached, the rpm was increased to 500. After 30 minutes, the molten material was discharged into a metal container containing dry ice. After the dry ice sublimated, the molten material was washed three times with heptane and isolated by vacuum filtration. The particles were dried overnight in a vacuum oven at room temperature and then sieved through a 250 μm screen.

[0175] The procedure for control sample 1-1 was repeated for control sample 1-2. The resulting particles were cyclically mixed with 15% by weight of pigment powder using a high-intensity powder mixer operated at approximately 13,500 rpm for approximately 30 seconds. The pigment was GloTech International GT8400 natural pigment with a D50 of less than 25 μm.

[0176] The procedure for control sample 1-1 was repeated, except that 5% by weight of pigment was added after adding RX50 fumed silica to sample 1-1, and the mixture was stirred until the reactor reached its temperature.

[0177] The procedure for sample 1-1 was repeated, except that 10% by weight of pigment was added to sample 1-2.

[0178] The procedure for sample 1-1 was repeated, except that 3.15% by weight of pigment was added to sample 1-1.

[0179] Table 1 provides the characteristics of the generated samples. [Table 1]

[0180] Figures 2 and 3 are scanning electron microscope images of samples 1-2 and 1-3, respectively, illustrating polymer-coated pigments attached to the surface of polymer particles. Figures 4 and 5 are cross-sectional scanning electron microscope images of sample 1-2 (the sample was fixed in epoxy resin and subjected to freeze microtome treatment before imaging), illustrating (a) pigments that are neither attached to, embedded in, nor encapsulated on polymer particles, and (b) pigments embedded on the surface of polymer particles.

[0181] The sample was 3D printed on a SNOWWHITE SLS printer (available from Sharebot). A 30mm x 30mm x 0.1mm square was printed as a preliminary screening object. In short, sieved particles were coated onto an aluminum plate using a bar coater (powder thickness 40 mil / gap of 40 mil per approximately 1 mm of powder layer thickness). The sample was placed in a SNOWWHITE chamber. The motor was disabled as no multilayer objects were printed. The chamber temperature was set to 115°C. The optimal printing conditions were determined by varying the laser speed and laser power. After the chamber and powder bed cooled to room temperature, the parts were removed. Table 2 provides the printing parameters and characteristics of the obtained printed square. [Table 2]

[0182] Control sample 2 - 117 g of PDMS (PSF® 30,000 cSt, available from Clearco) was added to a 1,500 mL glass reactor. Using approximately 20 g of the measured PDMS, a slurry was prepared by mixing the PDMS with 0.75 g of AEROSIL® RX50 fumed silica. This slurry was added to the glass reactor, followed by 50 g of polypropylene homopolymer resin (ULTRA HOPP® 20, ResMart). The reactor was heated to 250°C with one P4 shaft set to 150 revolutions per minute (rpm). Once this temperature was reached, the rpm was increased to 500. After 30 minutes, the molten material was discharged into a metal container containing dry ice. After the dry ice sublimated, the molten material was washed three times with heptane and isolated by vacuum filtration. The particles were dried overnight in a vacuum oven at room temperature and then sieved through a 250 μm screen.

[0183] The resulting particles were cyclically mixed with 15% by weight of pigment powder using a high-intensity powder mixer operated at approximately 13,500 rpm for approximately 30 seconds. The pigment was ULTRAGLOW® pigment (a europium-based phosphorescent powder available from Aqua Glow) with a D50 of approximately 28 μm.

[0184] The procedure for control sample 2-1 was repeated, except that 15% by weight of pigment was added after adding RX50 fumed silica to sample 2-1, and the mixture was mixed until the reactor reached its temperature.

[0185] Table 3 provides the characteristics of the generated samples. [Table 3]

[0186] Using a SNOWWHITE SLS printer, a 30mm × 30mm × 0.1mm square was printed for sample 2-1 as described above. The control sample 2-1 was not sufficiently printed. Table 4 provides the characteristics of the obtained printed squares. [Table 4]

[0187] Sample 3: 117 g of PDMS (PSF® 10,000 cSt, available from Clearco) was added to a 1,500 mL glass reactor. Using approximately 20 g of the measured PDMS, a slurry was prepared by mixing it with 0.5 g of AEROSIL® RX50 fumed silica. This slurry was added to the glass reactor, followed by 15 wt% pigment (GT8400 natural pigment, available from GloTech International) and 50 g of polyamide-12 homopolymer resin (RTP 200F, available from RTP). The reactor was set to 250 rpm and heated to 220°C. Once this temperature was reached, the rpm was increased to 1000. After 30 minutes, the molten material was cooled on a bench. After cooling, the molten material was washed three times with heptane and isolated by vacuum filtration. The particles were dried overnight in a vacuum oven at room temperature, and then sieved through a 250 μm screen.

[0188] Table 5 provides the characteristics of the generated samples. [Table 5]

[0189] Figures 6 and 7 are scanning electron microscope images of sample 3-1, illustrating what are likely polymer-coated pigments adhering to the surface of polymer particles. Figures 8 and 9 are cross-sectional scanning electron microscope images (the sample was fixed in epoxy resin and freeze-microtome-treated before imaging) illustrating (a) pigment embedded on the surface of polymer particles and (b) pigment encapsulated within polymer particles. Energy-dispersive X-ray spectroscopy in Figure 9 shows that the encapsulated particles contain strontium and are therefore pigments.

[0190] Accordingly, the present invention is well-adapted to achieve the objectives and advantages described above, as well as the inherent advantages therein. The specific embodiments disclosed above are illustrative only, and the present invention can be modified and implemented in different but equivalent ways, which will be obvious to those skilled in the art who are interested in the teachings herein. Furthermore, it is not intended to limit the present invention to any structural or design details other than those described in the following claims. Accordingly, the specific exemplary embodiments disclosed above may be changed, combined, or modified, and it is clear that all such variations will be considered within the scope and spirit of the present invention. The present invention as illustrated herein may be implemented in the absence of any elements not specifically disclosed herein and / or any optional elements disclosed herein. Compositions and methods are described using the terms “comprising,” “containing,” or “including” various components or processes, but compositions and methods may also “essentially consist of” or “consist of” various components and processes. All numbers and scopes disclosed above may vary somewhat. Whenever a numerical range with lower and upper limits is disclosed, any number and any range included within that range are specifically disclosed. In particular, all ranges of values ​​disclosed herein (in the form of "about a to about b," or equivalently "approximately a to b," or equivalently "about a to b") should be understood to describe all numbers and ranges encompassed within a broad range of values. Furthermore, terms in the claims have plain, ordinary meanings unless explicitly and clearly defined by the patent holder. In addition, when used in claims, the indefinite article "a" or "an" is defined herein to mean one or more of the elements it introduces.

Claims

1. providing a mixture comprising a thermoplastic polymer, a carrier medium immiscible with said thermoplastic polymer, a pigment, and an emulsion stabilizer, said emulsion stabilizer comprising nanoparticles selected from the group consisting of oxide nanoparticles, polymeric nanoparticles, and combinations thereof; applying a shear force to the mixture at a temperature above the melting point or softening temperature of the thermoplastic polymer and at a shear rate high enough to disperse the thermoplastic polymer as droplets in the dispersion medium; cooling the mixture below the melting point or softening temperature of the thermoplastic polymer to form colored polymer particles comprising the thermoplastic polymer, the pigment, and the nanoparticles, wherein the nanoparticles are coated on an outer surface of the colored polymer particles, and at least a portion of the colored polymer particles are: (a) the pigment is coated with the thermoplastic polymer to define a coated pigment, the coated pigment being adhered to the exterior surface; (b) the pigment is embedded in the outer surface; and (c) the pigment is encapsulated by the thermoplastic polymer below the outer surface; and separating the pigmented polymer particles from the dispersion medium, the pigmented polymer particles having a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, and a D90 of about 3 μm to about 300 μm, where D10<D50D<90; A method comprising:

2. The method of claim 1 , wherein the pigment comprises a first pigment and a second pigment different from the first pigment.

3. The method of claim 1, wherein the pigmented polymeric particles comprise from 0.01% to 30% by weight of pigment, based on the weight of the thermoplastic polymer in the pigmented polymeric particles.

4. The method of claim 1 , wherein the nanoparticles are embedded in the exterior surface.

5. The method of claim 1 , wherein the pigmented polymer particles have a diameter span of about 0.2 to about 10.

6. The method of claim 1 , wherein the pigmented polymer particles have a circularity of from about 0.90 to about 1.

0.

7. The method of claim 1 , wherein the pigmented polymer particles have a Hausner ratio of from about 1.0 to about 1.

5.

8. The method of claim 1, wherein the nanoparticles comprise silica nanoparticles.

9. A process for providing a mixture comprising a thermoplastic polymer, a dispersing medium immiscible with the thermoplastic polymer, a pigment, and an emulsion stabilizer, wherein the emulsion stabilizer comprises nanoparticles selected from the group consisting of oxide nanoparticles, polymeric nanoparticles, and combinations thereof, and the dispersing medium is selected from the group consisting of silicone oil, fluorinated silicone oil, perfluorinated silicone oil, polyethylene glycol, alkyl terminated polyethylene glycol, tetraethylene glycol dimethyl ether, paraffin, liquid petrolatum, mink oil, turtle oil, soybean oil, perhydrosqualene, sweet almond oil, carophyllum oil, palm oil, pearl oil, grapeseed oil, sesame oil, corn oil, rapeseed oil, sunflower oil, cottonseed oil, apricot oil, castor oil, avocado oil, jojoba oil, olive oil, cereal germ oil, esters of lanolin acid, esters of oleic acid, esters of lauric acid, esters of stearic acid, fatty esters, fatty acids, fatty alcohols, fatty acid modified polysiloxanes, fatty alcohol modified polysiloxanes, polyoxyalkylene modified polysiloxanes, and any combination thereof; applying a shear force to the mixture at a temperature above the melting point or softening temperature of the thermoplastic polymer and at a shear rate high enough to disperse the thermoplastic polymer as droplets in the dispersion medium; cooling the mixture below the melting point or softening temperature of the thermoplastic polymer to form colored polymer particles comprising the thermoplastic polymer, the pigment, and the nanoparticles, wherein the nanoparticles are coated on an outer surface of the colored polymer particles, and at least a portion of the colored polymer particles are: (a) the pigment is coated with the thermoplastic polymer to define a coated pigment, the coated pigment being adhered to the exterior surface; (b) the pigment is embedded in the outer surface; and (c) the pigment is encapsulated by the thermoplastic polymer below the outer surface; and separating the pigmented polymer particles from the dispersion medium; A method comprising:

10. The method of claim 1, wherein the colored polymer particles have a diameter span of about 0.2 to about 1.2.