Solder alloys, solder balls, and solder joints

JP2022130498A5Inactive Publication Date: 2024-11-22SENJU METAL IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022097573
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-19
Filing Date
2022-06-16
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lead-based and antimony-containing solder alloys used in semiconductor packaging, such as Sn-Ag-Cu-Ni-Ge, require further improvement in mechanical strength and compatibility with advanced electronic devices, particularly in applications beyond Ball Grid Array (BGA) like Quad Flat Package (QFP), while also addressing environmental and health concerns.

Method used

A lead-free and antimony-free solder alloy composition comprising specific balanced contents of Ag, Cu, Bi, Ni, and Ge, optimized to achieve a melting point of around 230°C and tensile strength of 50 MPa or more, with controlled intermetallic compound formation and improved wettability, suitable for both BGA and QFP applications.

Benefits of technology

The new solder alloy provides enhanced mechanical strength, improved wettability, and reduced intermetallic compound thickness, ensuring reliable solder joints with high tensile strength and environmental safety, suitable for advanced semiconductor packaging.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided are a lead-free and antimony-free solder alloy, solder ball, and solder joint, which have a melting point of approximately 230°C and a tensile strength of 50 MPa or more. [Solution] A lead-free and antimony-free solder alloy is used, having an alloy composition consisting of 1.0 to 4.0 mass% Ag, 0.1 to 1.0 mass% Cu, 0.1 to 9.0 mass% Bi, 0.005 to 0.3 mass% Ni, 0.001 to 0.015 mass% Ge, and the remainder being Sn.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a lead-free and antimony-free solder alloy, solder balls, and solder joints. This application claims priority based on US Patent Application No. 63 / 115,611, which was provisionally filed in the United States on November 19, 2020, and the content thereof is incorporated herein by reference.

Background Art

[0002] In recent years, there have been demands for high integration, large capacity, and high speed in electronic devices. For example, semiconductor packages such as QFP (Quad Flat Package) are used, and high integration and high functionality at the semiconductor chip level are achieved. In the manufacture of QFP, a packaging process is adopted in which a silicon chip cut out from a silicon wafer is die-bonded to a lead frame.

[0003] In a QFP obtained by bonding microelectrodes such as BGA (Ball Grid Array), a silicon chip and a lead frame are die-bonded with a solder alloy to form a solder joint. In microelectrodes such as BGA, solder bumps are formed using solder balls. When using solder balls, an adhesive flux is applied to the microelectrodes, and the solder balls are placed on the electrodes coated with the flux. Then, it is heated in a reflow furnace to melt the solder balls, and the molten solder wets the microelectrodes, thereby forming solder bumps on the microelectrodes.

[0004] By the way, conventionally, Sn-Ag-Cu solder alloy has been widely used and is used not only in the form of solder balls but also in die-bonding. When using this solder alloy, it may be necessary to improve heat cycle resistance, shock resistance, and discoloration resistance among various recent requirements. Therefore, various studies have been made to improve these characteristics regarding the conventionally widely used Sn-Ag-Cu solder alloy.

[0005] For example, Patent Document 1 discloses a solder alloy containing Ni and Ge as optional elements in a Sn-Ag-Cu solder alloy. This solder alloy is disclosed to exhibit heat cycle resistance when Ni is included, and impact resistance and discoloration resistance when Ge is included. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Patent No. 4144415 [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] As described above, the solder alloy disclosed in Patent Document 1 (Sn-Ag-Cu-Ni-Ge solder alloy) is an excellent alloy that can simultaneously exhibit three effects: impact resistance, discoloration resistance, and heat cycle resistance. However, there is still room for further improvement in alloy design.

[0008] Although each element in a solder alloy has its own specific purpose, it is a unified entity formed by the combination of all its constituent elements. Since each constituent element influences the others, it is necessary for the constituent elements to be present in a well-balanced manner as a whole. The solder alloy described in Patent Document 1 has the content of each constituent element individually optimized, and it is considered that the alloy composition was sufficient to obtain the effects described in Patent Document 1 at the time of filing. However, in solder alloys with similar constituent elements, if we want to improve other properties to meet recent demands, it is necessary to further optimize the content of each constituent element individually and then balance the constituent elements as a whole.

[0009] The invention described in Patent Document 1 is designed with the assumption that solder balls will be placed on a microelectrode such as a BGA. Therefore, when using Sn-Ag-Cu-Ni-Ge solder alloy for soldering, an improvement in mechanical strength is required. In this specification, mechanical strength may also be referred to as shear strength or tensile strength.

[0010] Thus, in recent years, with the increasing integration, capacity, and speed of electronic devices, there is a need for solder alloys that can be applied not only to BGA but also to die bonding, which is used in QFP.

[0011] Therefore, the present invention aims to provide a lead-free and antimony-free solder alloy, solder ball, and solder joint, which have a melting point of around 230°C and a tensile strength of 50 MPa or more. [Means for solving the problem]

[0012] Solder alloys are composed of two or more elements, and while the individual effects of each element can sometimes influence the overall properties of the solder alloy, as mentioned above, all constituent elements work together as a single unit, so each element is interconnected. The inventors focused on designing an alloy with improved shear strength so that it could be used not only for BGA but also for QFP, even if it had the same constituent elements as the solder alloy described in Patent Document 1.

[0013] Traditionally, when substrates containing lead (Pb) are discarded, acid rain can cause Pb to leach from the substrate and flow into groundwater. This can then accumulate in livestock and humans, potentially affecting their health. For this reason, Pb is designated as a regulated substance under the RoHS Directive. Furthermore, in recent years, there has been a growing demand to avoid the use of not only Pb but also Sb, which improves the heat cycle properties of Sn-based solder alloys, for environmental and health reasons. Therefore, we investigated how to obtain the desired properties while being lead-free and antimony-free.

[0014] In QFPs, which are obtained by joining microelectrodes such as BGAs (Ball Grid Arrays), the silicon chip and the lead frame are die-bonded with a solder alloy to form a solder joint. The silicon chip has a back metal formed on its outermost layer, for example, a nickel layer, to improve wettability with solder and enhance adhesion strength. When the outermost Ni layer comes into contact with molten solder, the Ni layer melts into the molten solder, causing Ni erosion. Normally, the back metal has a barrier layer of Ti or similar material to suppress the diffusion of Ni into the silicon chip. If Ni erosion progresses and the Ti layer is exposed, the solder alloy's wettability to Ti becomes very poor, causing the back metal to repel the molten solder. Furthermore, even if a small portion of the Ni layer remains, Ni atoms diffuse into the molten solder while Ti hardly diffuses into the Ni. As a result, voids increase at the atomic level at the interface between the Ti barrier layer and the Ni layer, drastically reducing the adhesion strength at the interface between the small remaining Ni and Ti layers. Consequently, the bonded joint after die bonding may have poor impact resistance and heat cycle resistance. Therefore, preserving the Ni layer of the back metal is extremely important in die bonding.

[0015] In this invention, the inventors re-examined the significance of adding each constituent element and then conducted a detailed compositional search, taking into account the balance of each constituent element. In this invention, the inventors have found that when the Ag, Cu, Bi, and Ni content is appropriate, the difference between the liquidus temperature and the solidus temperature of the solder alloy (hereinafter sometimes referred to as ΔT) falls within an appropriate range.

[0016] In this invention, the inventors also investigated the refinement of the intermetallic compound formed at the joint interface in order to improve the bonding strength of the solder joint. Since a Cu-Sn compound is formed at the bonding interface, the Cu-Sn content ratio must be within a predetermined range. Also, attention was paid to the fact that in the compound of Cu and Sn, refinement of the compound was achieved by substituting part of Cu with Ni. Furthermore, since the liquidus temperature of the solder alloy varies greatly depending on the contents of Cu and Ni, investigations were conducted to control the viscosity during melting so that ΔT does not become too large and to suppress the growth of Sn compounds. As a result, in the Sn-Ag-Cu-Bi-Ni-Ge solder alloy, it was also found that by containing Sn, Cu, and Ni in a well-balanced manner, ΔT is controlled, the intermetallic compound formed at the bonding interface becomes fine, and the shear strength and reliability are improved.

[0017] Furthermore, in the present invention, the inventors found that by adjusting the content of Ag within a predetermined range, precipitation of coarse Ag3Sn can be suppressed and precipitation of fine Ag3Sn can be caused at the grain boundaries, thereby improving the tensile strength and reliability.

[0018] Furthermore, in the present invention, the inventors found that by adjusting the content of Bi within a predetermined range, it is possible to give the solder ball an optimal mechanical strength. Also, the inventors found that when Bi is added in excess, the liquidus temperature decreases, ΔT increases, and the mechanical strength and the like decrease due to segregation.

[0019] Furthermore, the inventors found that by adjusting the content of Co within a predetermined range, ΔT is reduced, the tensile strength is 50 MPa or more, and the elongation, Poisson's ratio, and linear expansion coefficient can be improved.

[0020] To solve the above problems, the present invention adopted the following configuration. [1] A lead-free and antimony-free solder alloy having an alloy composition consisting of 1.0 to 4.0% by mass of Ag, from 0.1 to (此处原文有误,推测应为1.0)1.0% by mass of Cu, from 0.1 to 9.0% by mass of Bi, from 0.005 to 0.3% by mass of Ni, from 0.001 to 0.015% by mass of Ge, and the balance being Sn.

[0021] [2] The solder alloy according to [1], wherein the alloy composition is Ag: 1.0 to 3.5% by mass. [3] The solder alloy according to [1] or [2], wherein the alloy composition is Ag: 2.0 to 3.5% by mass. [4] The solder alloy according to any one of [1] to [3], wherein the alloy composition is Ag: 3.0 to 3.5% by mass. [5] The solder alloy according to any one of [1] to [4], wherein the alloy composition is Cu: 0.5 to 0.85% by mass. [6] The solder alloy according to any one of [1] to [5], wherein the alloy composition is Cu: 0.7 to 0.8% by mass. [7] The solder alloy according to any one of [1] to [6], wherein the alloy composition is Cu: 0.75 to 0.8% by mass. [8] The solder alloy according to any one of [1] to [7], wherein the alloy composition is Bi: 0.2 to 5.0% by mass. [9] The solder alloy according to any one of [1] to [8], wherein the alloy composition is Bi: 0.5 to 4.0% by mass.

[10] The solder alloy according to any one of [1] to [9], wherein the alloy composition is Bi: 1.0 to 3.0% by mass.

[0022]

[11] The solder alloy according to any one of [1] to

[10] , wherein the alloy composition is Ni: 0.02 to 0.09% by mass.

[12] The solder alloy according to any one of [1] to

[11] , wherein the alloy composition is Ni: 0.03 to 0.08% by mass.

[13] The solder alloy according to any one of [1] to

[12] , wherein the alloy composition is Ni: 0.04 to 0.06% by mass.

[14] The solder alloy according to any one of [1] to

[13] , wherein the alloy composition is Ge: 0.002 to 0.012% by mass.

[15] The solder alloy according to any one of [1] to

[14] , wherein the alloy composition is Ge: 0.003 to 0.010% by mass.

[16] The solder alloy according to any one of [1] to

[15] , wherein the alloy composition is Ge:​

[0023]

[17] Further, the alloy composition is the solder alloy according to any one of [1] to

[16] , satisfying 0.3 ≦ Ag / Bi ≦ 3.0. Ag and Bi each represent the content (% by mass) in the alloy composition.

[18] Further, the alloy composition is the solder alloy according to any one of [1] to

[16] , containing Co: 0.001 to 0.1% by mass.

[19] The alloy composition is the solder alloy according to

[18] , where Co: 0.002 to 0.015% by mass.

[20] The alloy composition is the solder alloy according to

[18] or

[19] , where Co: 0.004 to 0.012% by mass.

[21] The alloy composition is the solder alloy according to any one of

[18] to

[20] , where Co: 0.006 to 0.009% by mass.

[0024]

[22] Further, the alloy composition is the solder alloy according to any one of [1] to

[17] , satisfying 1 < Ag / Bi. Ag and Bi each represent the content (% by mass) in the alloy composition.

[23] A lead-free and antimony-free solder alloy having an alloy composition of Ag: 3.5% by mass, Cu: 0.8% by mass, Bi: 1.0 to 2.0% by mass, Ni: 0.05% by mass, Ge: 0.008% by mass, and the balance being Sn.

[24] A lead-free and antimony-free solder alloy having an alloy composition of Ag: 3.0 to 4.0% by mass, Cu: 0.7 to 0.9% by mass, Bi: 1.5% by mass, Ni: 0.03 to 0.08% by mass, Ge: 0.006 to 0.009% by mass, and the balance being Sn.

[25] A lead-free and antimony-free solder alloy having an alloy composition of Ag: 3.0 to 4.0% by mass, Cu: 0.7 to 0.9% by mass, Bi: 1.8% by mass, Ni: 0.03 to 0.08% by mass, Ge: 0.006 to 0.009% by mass, and the balance being Sn.

[26] Further, the alloy composition is the solder alloy according to any one of [1] to

[17] ,

[22] to

[25] , satisfying 1.2 ≦ Ag / Bi ≦ 3.0. Ag and Bi represent their respective content (mass%) in the alloy composition.

[0025]

[27] Furthermore, the alloy composition is a solder alloy according to any of [1] to

[17] , satisfying Ag / Bi ≤ 1. Ag and Bi represent their respective content (mass%) in the alloy composition.

[28] A lead-free and antimony-free solder alloy having an alloy composition consisting of Ag: 2.0 mass%, Cu: 0.8 mass%, Bi: 3.0-5.0 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn.

[29] A lead-free and antimony-free solder alloy having an alloy composition consisting of Ag: 1.0-3.0 mass%, Cu: 0.7-0.9 mass%, Bi: 4.0 mass%, Ni: 0.04-0.08 mass%, Ge: 0.006-0.009 mass%, and the remainder being Sn.

[30] Furthermore, the alloy composition is any of the solder alloys described in [1] to

[17] ,

[27] to

[29] , satisfying 0.3 ≤ Ag / Bi ≤ 0.7. Ag and Bi represent their respective content (mass%) in the alloy composition.

[0026]

[31] A lead-free and antimony-free solder alloy having an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 0.3-0.7 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, Co: 0.008 mass%, and the remainder being Sn.

[32] A lead-free and antimony-free solder alloy having an alloy composition consisting of Ag: 3.0-4.0 mass%, Cu: 0.7-0.9 mass%, Bi: 0.5 mass%, Ni: 0.03-0.08 mass%, Ge: 0.006-0.009 mass%, Co: 0.004-0.012 mass%, and the remainder being Sn.

[33] The alloy composition is Bi: 0.3 to 1.0 mass%, Furthermore, a solder alloy described in any of

[18] ~

[21] or

[31] ~

[32] that satisfies 5≦Ag / Bi≦15. Ag and Bi represent their respective content (mass%) in the alloy composition.

[0027]

[34] A lead-free and antimony-free solder alloy having an alloy composition consisting of Ag: 1.0 to 4.0% by mass, Cu: 0.7 to 1.0% by mass, Bi: 0.1 to 7.0% by mass, Ni: 0.040 to 0.095% by mass, Ge: 0.007 to 0.015% by mass, and the balance being Sn.

[35] Furthermore, the solder alloy according to

[34] , wherein the alloy composition contains Co: 0.001 to 0.1% by mass.

[36] Furthermore, the solder alloy according to

[34] or

[35] , which satisfies 0.007 < Ni / (Ag + Bi) < 0.017. Ni, Ag, and Bi each represent the content (% by mass) in the alloy composition.

[37] Furthermore, the solder alloy according to any one of

[34] to

[36] , which satisfies 46 < (Cu / Ni) × (Ag + Bi) < 120. Cu, Ni, Ag, and Bi each represent the content (% by mass) in the alloy composition.

[0028]

[38] A solder ball composed of the solder alloy according to any one of [1] to

[37] .

[39] The solder ball according to

[38] , having an average particle size of 1 to 1000 μm.

[40] The solder ball according to

[38] or

[39] , having a sphericity of 0.95 or more.

[41] The solder ball according to any one of

[38] to

[40] , having a sphericity of 0.99 or more.

[42] A Ball Grid Array formed using the solder ball according to any one of

[38] to

[41] .

[43] A solder joint made using the solder alloy according to any one of [1] to

[37] .

Advantages of the Invention

[0029] According to the present invention, it is possible to provide a lead-free and antimony-free solder alloy, a solder ball, and a solder joint having a melting point in the vicinity of 230°C and a tensile strength of 50 MPa or more.

Embodiments for Carrying Out the Invention

[0030] The solder alloy according to the embodiment of the present invention has a melting point of approximately 230°C. In the solder alloy according to the embodiment of the present invention, the main component is Sn, which has a melting point of 232°C. Even if the solder alloy according to the embodiment of the present invention contains elements other than Sn, its melting point remains around 230°C.

[0031] Here, the "melting point" of a solder alloy refers to the temperature of that solder alloy that is above the solidus temperature and below the liquidus temperature. "Near 230°C" means a temperature range of 170°C to 230°C. "The melting point of the solder alloy is around 230°C" means that "the solidus temperature of the solder alloy is between 170 and 225°C, and the liquidus temperature of the solder alloy is between 210 and 230°C."

[0032] 1. Composition of solder alloy The solder alloy of this embodiment has an alloy composition consisting of Ag: 1.0-4.0 mass%, Cu: 0.1-1.0 mass%, Bi: 0.1-9.0 mass%, Ni: 0.005-0.3 mass%, Ge: 0.001-0.015 mass%, and the remainder being Sn, and is lead-free and antimony-free.

[0033] (1)Ag: 1.0~4.0% by mass Ag is an element that improves the strength of solder alloys by precipitating fine Ag3Sn at the grain boundaries. The Ag content is more preferably 2.0% by mass or more, and even more preferably 3.0% by mass or more. The Ag content is preferably 3.5% by mass or less. The Ag content is 1.0 to 4.0% by mass, preferably 1.0 to 3.5% by mass, more preferably 2.0 to 3.5% by mass, and even more preferably 3.0 to 3.5% by mass. By ensuring that the Ag content is above the aforementioned lower limit, fine Ag3Sn can be sufficiently precipitated. By keeping the Ag content below the above upper limit, the amount of coarse Ag3Sn precipitated can be reduced. Alternatively, another aspect is that the strength of the joint after soldering can be increased by having an Ag content above the aforementioned lower limit. By keeping the Ag content below the aforementioned upper limit, the strength of the joint after soldering can be increased. Furthermore, by keeping the Ag content at 3.5% by mass or less, the effect of reducing the amount of coarse Ag3Sn precipitate can be further enhanced.

[0034] (2)Cu:0.1~1.0% by mass Cu is an element that can suppress Cu erosion and improve the amount of Cu6Sn5 precipitated. The Cu content is preferably 0.5% by mass or more, more preferably 0.7% by mass or more, and even more preferably 0.75% by mass or more. The Cu content is preferably 0.85% by mass or less, and more preferably 0.8% by mass or less. The Cu content is 0.1 to 1.0% by mass, preferably 0.5 to 0.85% by mass, more preferably 0.7 to 0.8% by mass, and even more preferably 0.75 to 0.8% by mass. By ensuring that the Cu content is above the aforementioned lower limit, Cu erosion can be suppressed, and Cu6Sn5 can be sufficiently precipitated, thereby reducing the amount of brittle SnNi compound precipitated. By keeping the Cu content below the aforementioned upper limit, an excessive rise in the liquidus temperature can be suppressed. Alternatively, another aspect is that by having a Cu content of 0.7% by mass or more, the thickness of the intermetallic compound layer at the bonding interface can be reduced. By keeping the Cu content below the aforementioned upper limit, the thickness of the intermetallic compound layer at the bonding interface can be reduced. A Cu content of 0.7% by mass or more can increase the strength of the joint after soldering. By keeping the Cu content below the aforementioned upper limit, the strength of the joint after soldering can be increased. By keeping the Cu content below the aforementioned upper limit, wettability can be improved. The Cu content is preferably 0.7 to 1.0% by mass, more preferably 0.7 to 0.85% by mass, and even more preferably 0.75 to 0.8% by mass.

[0035] (3) Bi:0.1~9.0% by mass The Bi content is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more. The Bi content is preferably 5.0% by mass or less, more preferably 4.0% by mass or less, and even more preferably 3.0% by mass or less. The Bi content is 0.1 to 9.0% by mass, preferably 0.2 to 5.0% by mass, more preferably 0.5 to 4.0% by mass, and even more preferably 1.0 to 3.0% by mass. By ensuring that the Bi content is above the aforementioned lower limit, optimal mechanical strength for the solder ball shape used as a BGA can be obtained, and creep resistance and wettability can also be improved. Furthermore, since Bi is solid-soluble in Sn, it distorts the crystal structure of (Cu,Ni)6Sn5, suppressing Cu erosion and allowing sufficient precipitation of Cu6Sn5, thereby reducing the amount of brittle SnNi compound precipitated. By keeping the Bi content below the aforementioned upper limit, an excessive decrease in the solidus temperature can be suppressed, thereby narrowing ΔT. This suppresses Bi segregation at the bonding interface, thereby preventing a decrease in mechanical strength and other properties. Alternatively, another aspect is that the strength of the joint after soldering can be increased by ensuring that the Bi content is above the aforementioned lower limit. Furthermore, by having a Bi content of 7.0% by mass or less, the strength of the joint after soldering can be increased. By ensuring that the Bi content is above the aforementioned lower limit, wettability can be improved. The Bi content is preferably 0.1 to 7.0% by mass, more preferably 0.2 to 5% by mass, and even more preferably 0.5 to 4% by mass.

[0036] (4)Ni:0.005~0.3% by mass The Ni content is preferably 0.02% by mass or more, more preferably 0.03% by mass or more, and even more preferably 0.04% by mass or more. The Ni content is preferably 0.09% by mass or less, more preferably 0.08% by mass or less, and even more preferably 0.06% by mass or less. The Ni content is 0.005 to 0.3 mass%, preferably 0.02 to 0.09 mass%, more preferably 0.03 to 0.08 mass%, and even more preferably 0.04 to 0.06 mass%. By ensuring that the Ni content is above the aforementioned lower limit, the liquidus temperature of the solder alloy can be controlled in the same way as Cu, and Ni corrosion can be suppressed. By keeping the Ni content below the aforementioned upper limit, an excessive rise in the liquidus temperature can be suppressed. Alternatively, another aspect is that, by having a Ni content of 0.04 mass% or more, the thickness of the intermetallic compound layer at the bonding interface can be reduced. Furthermore, the strength of the joint after soldering can be increased. Furthermore, by having a Ni content of 0.095% by mass or less, the thickness of the intermetallic compound layer at the bonding interface can be reduced. In addition, the strength of the joint after soldering can be increased. The Ni content is preferably 0.04 to 0.095% by mass, more preferably 0.04 to 0.08% by mass, and even more preferably 0.05 to 0.07% by mass.

[0037] (5)Ge:0.001~0.015% by mass The Ge content is preferably 0.002% by mass or more, and more preferably 0.003% by mass or more. The Ge content is preferably 0.012% by mass or less, more preferably 0.01% by mass or less, and even more preferably 0.009% by mass or less. The Ge content is 0.001 to 0.015% by mass, preferably 0.002 to 0.012% by mass, more preferably 0.003 to 0.01% by mass, and even more preferably 0.003 to 0.009% by mass. By having a Ge content above the aforementioned lower limit, the formation of oxidized Sn is suppressed, which distorts the crystal structure of the (Cu,Ni)6Sn5 compound, inhibiting the movement of Ni within the compound and thus inhibiting the movement of Ni to the solder alloy, thereby suppressing Ni corrosion. By keeping the Ge content below the aforementioned upper limit, an excessive rise in the liquidus temperature can be suppressed. Alternatively, another aspect is that the discoloration of the alloy can be suppressed by having a Ge content of 0.007 mass% or more. By keeping the Ge content below the above upper limit, wettability can be improved. Furthermore, the strength of the joint after soldering can be increased. The Ge content is preferably 0.007 to 0.015% by mass, more preferably 0.007 to 0.012% by mass, and even more preferably 0.007 to 0.009% by mass.

[0038] (6)Co:0.001~0.1% by mass The solder alloy of this embodiment may contain Co. The Co content is preferably 0.001% by mass or more, more preferably 0.002% by mass or more, even more preferably 0.004% by mass or more, and particularly preferably 0.006% by mass or more. The Co content is preferably 0.1% by mass or less, more preferably 0.015% by mass or less, even more preferably 0.012% by mass or less, and particularly preferably 0.009% by mass or less. The Co content is preferably 0.001 to 0.1% by mass, more preferably 0.002 to 0.015% by mass, still more preferably 0.004 to 0.012% by mass, and particularly preferably 0.006 to 0.009% by mass. When the Co content is within the above range, the tensile strength can be improved, and the elongation, Poisson's ratio, and linear expansion coefficient can be improved.

[0039] (7) The balance: Sn The balance of the solder alloy of the present embodiment is Sn. It may contain inevitable impurities in addition to the above-described elements. Even when it contains inevitable impurities, it does not affect the above-described effects. Specific examples of the inevitable impurities include As and Cd. Further, although the present invention is lead-free and antimony-free, it does not exclude the inclusion of Pb and Sb as inevitable impurities.

[0040] (8) Ag / Bi In the ratio represented by Ag / Bi, Ag and Bi each represent the content (% by mass) in the alloy composition. When the solder alloy of the present embodiment does not contain Co, the solder alloy of the present embodiment preferably satisfies 0.3 ≤ Ag / Bi ≤ 3.0. When Ag / Bi is within the above range, the tensile strength can be improved. When the solder alloy of the present embodiment does not contain Co, Ag / Bi ≤ 1 may be satisfied. In this case, when 0.3 ≤ Ag / Bi ≤ 0.7, the tensile strength can be further improved. When the solder alloy of the present embodiment does not contain Co, 1 < Ag / Bi may be satisfied. In this case, when 1.2 ≤ Ag / Bi ≤ 3.0, ΔT can be reduced and the tensile strength can be improved. When the solder alloy of the present embodiment contains Co, it preferably satisfies 5 ≤ Ag / Bi ≤ 15. When Ag / Bi is within the above range, ΔT is reduced, the tensile strength is 50 MPa or more, and the elongation, Poisson's ratio, and linear expansion coefficient can be improved.

[0041] (9)Difference (ΔT) between liquidus temperature and solidus temperature The solder alloy of the present embodiment is preferable in that if ΔT is within a predetermined range, the solid-liquid coexistence region becomes narrow, an increase in the viscosity of the molten solder is suppressed, segregation of Bi at the bonding interface is suppressed, and a decrease in mechanical strength can be suppressed. The solidus temperature of the solder alloy of the present embodiment is 170 to 225°C, preferably 172 to 223°C, more preferably 174 to 221°C, and even more preferably 176 to 219°C. The liquidus temperature of the solder alloy of the present embodiment is 210 to 230°C, preferably 212 to 230°C, more preferably 212 to 228°C, and even more preferably 214 to 226°C. ΔT is preferably 50°C or less, more preferably 45°C or less, even more preferably 40°C or less, particularly preferably 30°C or less, and most preferably 15°C or less. The lower limit value of ΔT is not particularly limited, and for example, it may be 1°C.

[0042] (10) Ni / (Ag + Bi) In the ratio here, Ni, Ag, and Bi each represent the content (mass%) in the alloy composition. Ni / (Ag + Bi) is obtained by dividing Ni by the sum of Ag and Bi. The solder alloy of the present embodiment preferably has Ni / (Ag + Bi) greater than 0.007. By 0.007 < Ni / (Ag + Bi), coarsening of the intermetallic compound can be suppressed and an excessive decrease in the solidus temperature can be suppressed. The solder alloy of the present embodiment preferably has Ni / (Ag + Bi) less than 0.017. By Ni / (Ag + Bi) < 0.017, an excessive increase in the liquidus temperature can be suppressed. Thereby, the wettability can be made sufficient. The solder alloy of the present embodiment preferably satisfies 0.007 < Ni / (Ag + Bi) < 0.017.

[0043] (11) (Cu / Ni) × (Ag + Bi) In these ratios, Cu, Ni, Ag, and Bi each represent their content (mass %) in the alloy composition. (Cu / Ni) × (Ag + Bi) is obtained by multiplying the value obtained by dividing Cu by Ni by the sum of Ag and Bi. In this embodiment, the solder alloy preferably has a (Cu / Ni) × (Ag + Bi) ratio greater than 46. Having 46 < (Cu / Ni) × (Ag + Bi) suppresses an excessive rise in the liquidus temperature. This allows for sufficient wettability. In this embodiment, the solder alloy preferably has a (Cu / Ni) × (Ag + Bi) ratio of less than 120. Having (Cu / Ni) × (Ag + Bi) < 120 suppresses the coarsening of intermetallic compounds and prevents an excessive decrease in the solidus temperature. The solder alloy of this embodiment preferably satisfies the condition 46 < (Cu / Ni) × (Ag + Bi) < 120. The solder alloy of this embodiment may also have a composition that satisfies 46 < (Cu / Ni) × (Ag + Bi) < 110, or a composition that satisfies 46 < (Cu / Ni) × (Ag + Bi) < 100.

[0044] In the solder alloy of the embodiment described above, by having a specific alloy composition consisting of Ag, Cu, Bi, Ni, Ge, and Sn, it is possible to provide a lead-free and antimony-free solder alloy with a melting point of around 230°C and a tensile strength of 50 MPa or more. Furthermore, the solder alloy of the embodiment described above can reduce ΔT by keeping the Ag and Bi content within a predetermined range. In the embodiment of the solder alloy described above that contains Co, by adjusting the Co content to a predetermined range, ΔT can be reduced, and the elongation, Poisson's ratio, and coefficient of thermal expansion of the solder alloy can be improved.

[0045] Examples of the solder alloys used in this embodiment include those from the following first to fifth embodiments.

[0046] <First Embodiment> The solder alloy of the first embodiment has an alloy composition consisting of Ag: 1.0-4.0 mass%, Cu: 0.1-1.0 mass%, Bi: 0.1-9.0 mass%, Ni: 0.005-0.3 mass%, Ge: 0.001-0.015 mass%, and the remainder being Sn, and is a lead-free and antimony-free solder alloy, and 1 <Ag / Biである。 The content of Ag, Cu, Bi, Ni, and Ge may be as described above. In the ratios presented here, Ag and Bi represent their respective content (mass%) in the alloy composition.

[0047] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 1.0-2.0 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0048] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.0-4.0 mass%, Cu: 0.7-0.9 mass%, Bi: 1.5 mass%, Ni: 0.03-0.08 mass%, Ge: 0.006-0.009 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0049] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.0-4.0 mass%, Cu: 0.7-0.9 mass%, Bi: 1.8 mass%, Ni: 0.03-0.08 mass%, Ge: 0.006-0.009 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0050] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 1.5-3.0 mass%, Ni: 0.05 mass%, Ge: 0.003 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0051] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.0-4.0 mass%, Cu: 0.7-0.9 mass%, Bi: 2.0 mass%, Ni: 0.03-0.08 mass%, Ge: 0.002-0.004 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0052] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.0-4.0 mass%, Cu: 0.7-0.9 mass%, Bi: 2.5 mass%, Ni: 0.03-0.08 mass%, Ge: 0.002-0.004 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0053] The solder alloy of the first embodiment preferably satisfies 1.2 ≤ Ag / Bi ≤ 3.0, and more preferably satisfies 1.3 ≤ Ag / Bi ≤ 1.9. Ag and Bi represent their respective content (mass%) in the alloy composition. By keeping the Ag / Bi ratio within the above range, ΔT can be reduced while simultaneously improving tensile strength.

[0054] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 1.5 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0055] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 1.8 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0056] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 2.0 mass%, Ni: 0.05 mass%, Ge: 0.003 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0057] The solder alloy of the first embodiment may have an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 2.5 mass%, Ni: 0.05 mass%, Ge: 0.003 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0058] In the solder alloy of the first embodiment, by having a specific alloy composition consisting of Ag, Cu, Bi, Ni, Ge, and Sn, it is possible to provide a lead-free and antimony-free solder alloy with a melting point of around 230°C and a tensile strength of 50 MPa or more. The solder alloy of the first embodiment can be applied not only to BGA but also to die bonding. The solder alloy of the first embodiment is 1 <Ag / Biである。 In the solder alloy of the first embodiment, ΔT can be reduced by keeping the Ag and Bi content within a predetermined range.

[0059] The solder alloy of the first embodiment preferably has a solidus temperature of 208 to 223°C, more preferably 210 to 221°C, and even more preferably 212 to 219°C. The solder alloy of the first embodiment preferably has a liquidus temperature of 213 to 227°C, more preferably 215 to 225°C, and even more preferably 217 to 223°C. In the first embodiment, the solder alloy preferably has a ΔT of 10°C or less, more preferably 8°C or less, and even more preferably 7°C or less. The lower limit of ΔT is not particularly limited, but may be, for example, 1°C.

[0060] In the solder alloy of the first embodiment, the ratio of Ag / Bi is preferably 1.2 ≤ Ag / Bi ≤ 3.0, and more preferably 1.3 ≤ Ag / Bi ≤ 1.9. In the solder alloy of the first embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0061] Alternatively, in other respects, the solder alloy of the first embodiment is preferably 1.0 ≤ Ag / Bi ≤ 50.0, more preferably 1.0 ≤ Ag / Bi ≤ 3.0, and even more preferably 1.5 ≤ Ag / Bi ≤ 3.0. In the solder alloy of the first embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0062] Alternatively, from another perspective, the solder alloy of the first embodiment is preferably 10.0 ≤ Ag / Bi ≤ 50.0, and more preferably 20.0 ≤ Ag / Bi ≤ 40.0. In the solder alloy of the first embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0063] <Second Embodiment> The solder alloy of the second embodiment has an alloy composition consisting of Ag: 1.0-4.0 mass%, Cu: 0.1-1.0 mass%, Bi: 0.1-9.0 mass%, Ni: 0.005-0.3 mass%, Ge: 0.001-0.015 mass%, and the remainder being Sn. It is a lead-free and antimony-free solder alloy that satisfies Ag / Bi ≤ 1. The content of Ag, Cu, Bi, Ni, and Ge may be as described above. In the ratios presented here, Ag and Bi represent their respective content (mass%) in the alloy composition.

[0064] The solder alloy of the second embodiment may have an alloy composition consisting of Ag: 2.0 mass%, Cu: 0.8 mass%, Bi: 3.0-5.0 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0065] The solder alloy of the second embodiment may have an alloy composition consisting of Ag: 1.0-3.0 mass%, Cu: 0.7-0.9 mass%, Bi: 4.0 mass%, Ni: 0.04-0.08 mass%, Ge: 0.006-0.009 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0066] In the second embodiment, the solder alloy preferably satisfies the condition 0.3 ≤ Ag / Bi ≤ 0.7. Ag and Bi represent their respective content (mass%) in the alloy composition. By keeping the Ag / Bi ratio within the above range, the tensile strength can be further improved.

[0067] The solder alloy of the second embodiment preferably has an alloy composition consisting of Ag: 2.0 mass%, Cu: 0.8 mass%, Bi: 4.0 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn, and is lead-free and antimony-free.

[0068] In the solder alloy of the second embodiment, by having a specific alloy composition consisting of Ag, Cu, Bi, Ni, Ge, and Sn, it is possible to provide a lead-free and antimony-free solder alloy with a melting point of around 230°C and a tensile strength of 50 MPa or more. The solder alloy of the second embodiment can be applied not only to BGA but also to die bonding. In the second embodiment, the solder alloy has an Ag / Bi ratio of ≤ 1. In the solder alloy of the second embodiment, ΔT can be reduced by keeping the Ag and Bi content within a predetermined range.

[0069] The solder alloy of the second embodiment preferably has a solidus temperature of 175 to 220°C, more preferably 175 to 218°C, and even more preferably 176 to 216°C. The solder alloy of the second embodiment has a liquidus temperature of 210 to 230°C, preferably 211 to 229°C, and more preferably 213 to 227°C. In the second embodiment, the solder alloy preferably has a ΔT of 50°C or less, more preferably 45°C or less, and even more preferably 40°C or less. The lower limit of ΔT is not particularly limited, but may be, for example, 1°C.

[0070] In the second embodiment, the solder alloy preferably has an Ag / Bi ratio of 0.3 ≤ 0.7. In the second embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0071] Alternatively, in other respects, the solder alloy of the second embodiment is preferably 0.1 ≤ Ag / Bi ≤ 0.8, more preferably 0.15 ≤ Ag / Bi ≤ 0.7, and even more preferably 0.2 ≤ Ag / Bi ≤ 0.6. In the solder alloy of the second embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0072] The solder alloy of the first embodiment can suppress the decrease in solidus temperature more effectively than the solder alloy of the second embodiment. The solder alloy of the first embodiment can reduce ΔT more effectively than the solder alloy of the second embodiment. The solder alloy of the second embodiment can have improved tensile strength compared to the solder alloy of the first embodiment.

[0073] <Third Embodiment> The solder alloy of the third embodiment has an alloy composition consisting of Ag: 1.0-4.0 mass%, Cu: 0.1-1.0 mass%, Bi: 0.1-9.0 mass%, Ni: 0.005-0.3 mass%, Ge: 0.001-0.015 mass%, Co: 0.001-0.1 mass%, and the remainder being Sn, and is a lead-free and antimony-free solder alloy. The content of Ag, Cu, Bi, Ni, Ge, and Co may be as described above.

[0074] The solder alloy of the third embodiment may have an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 0.3-0.7 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, Co: 0.008 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0075] The solder alloy of the third embodiment may have an alloy composition consisting of Ag: 3.0-4.0 mass%, Cu: 0.7-0.9 mass%, Bi: 0.5 mass%, Ni: 0.03-0.08 mass%, Ge: 0.006-0.009 mass%, Co: 0.004-0.012 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0076] In the third embodiment, the solder alloy has a Bi content of 0.3 to 1.0 mass%, and it is preferable that the ratio 5 ≤ Ag / Bi ≤ 15 is satisfied. Ag and Bi represent their respective content (mass%) in the alloy composition. By keeping the Ag / Bi ratio within the above range and adjusting the Co content to a predetermined range, ΔT can be reduced, improving tensile strength, elongation, Poisson's ratio, and coefficient of thermal expansion.

[0077] The solder alloy of the third embodiment preferably has an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 0.5 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, Co: 0.008 mass%, and the remainder being Sn, and is lead-free and antimony-free.

[0078] The solder alloy of the third embodiment has a Co content of 0.001 to 0.1% by mass. In the third embodiment, by having a specific alloy composition consisting of Ag, Cu, Bi, Ni, Ge, Co, and Sn, it is possible to provide a lead-free and antimony-free solder alloy with a melting point of around 230°C and a tensile strength of 50 MPa or more. The solder alloy of the third embodiment can be applied not only to BGA but also to die bonding.

[0079] The solder alloy of the third embodiment preferably has a solidus temperature of 212 to 222°C, more preferably 214 to 220°C, and even more preferably 216 to 218°C. The solder alloy of the third embodiment preferably has a liquidus temperature of 216 to 226°C, more preferably 218 to 224°C, and even more preferably 220 to 222°C. In the third embodiment, the solder alloy preferably has a ΔT of 10°C or less, more preferably 8°C or less, and even more preferably 7°C or less. The lower limit of ΔT is not particularly limited, but may be, for example, 1°C.

[0080] In the third embodiment, the solder alloy preferably has an Ag / Bi ratio of 5 ≤ 15. In the third embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength. Furthermore, in the third embodiment, having the Ag / Bi ratio within the above range makes it possible to improve elongation, Poisson's ratio, and coefficient of thermal expansion.

[0081] Alternatively, in other respects, the solder alloy of the third embodiment is preferably 0.2 ≤ Ag / Bi ≤ 15.0, more preferably 0.3 ≤ Ag / Bi ≤ 3.0, even more preferably 0.5 ≤ Ag / Bi ≤ 2.0, and particularly preferably 0.6 ≤ Ag / Bi ≤ 1.0. In the solder alloy of the third embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0082] The solder alloy of the third embodiment preferably has a solidus temperature of 200 to 223°C, more preferably 202 to 221°C, and even more preferably 204 to 219°C. The solder alloy of the third embodiment preferably has a liquidus temperature of 210 to 227°C, more preferably 211 to 225°C, and even more preferably 213 to 223°C. In the third embodiment, the solder alloy preferably has a ΔT of 30°C or less, more preferably 20°C or less, and even more preferably 15°C or less. The lower limit of ΔT is not particularly limited, but may be, for example, 1°C.

[0083] <Fourth Embodiment> The solder alloy of the fourth embodiment has an alloy composition consisting of Ag: 1.0-4.0 mass%, Cu: 0.7-1.0 mass%, Bi: 0.1-7.0 mass%, Ni: 0.040-0.095 mass%, Ge: 0.007-0.015 mass%, and the remainder being Sn, and is a lead-free and antimony-free solder alloy. The content of Ag, Cu, Bi, Ni, and Ge may be as described above.

[0084] The solder alloy of the fourth embodiment may have an alloy composition consisting of Ag: 3.0-3.5 mass%, Cu: 0.7-1.0 mass%, Bi: 1.0-2.0 mass%, Ni: 0.040-0.060 mass%, Ge: 0.007-0.010 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0085] Alternatively, the solder alloy of the fourth embodiment may have an alloy composition consisting of Ag: 1.5-2.5 mass%, Cu: 0.7-1.0 mass%, Bi: 3.0-5.0 mass%, Ni: 0.060-0.080 mass%, Ge: 0.007-0.010 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0086] In the fourth embodiment, by having a specific alloy composition consisting of Ag, Cu, Bi, Ni, Ge, and Sn, it is possible to provide a lead-free and antimony-free solder alloy with a melting point of around 230°C and a tensile strength of 50 MPa or more. The solder alloy of the fourth embodiment can be applied not only to BGA but also to die bonding.

[0087] The solder alloy of the fourth embodiment preferably satisfies 0.3 ≦ Ag / Bi ≦ 3.0, more preferably 1.2 ≦ Ag / Bi ≦ 3.0, and still more preferably 1.3 ≦ Ag / Bi ≦ 1.9. In the solder alloy of the fourth embodiment, when the ratio of Ag / Bi is within the above range, it becomes easier to reduce ΔT and easier to improve the tensile strength.

[0088] Alternatively, the solder alloy of the fourth embodiment preferably satisfies 0.3 ≦ Ag / Bi ≦ 3.0, and more preferably 0.3 ≦ Ag / Bi ≦ 0.7. In the solder alloy of the fourth embodiment, when the ratio of Ag / Bi is within the above range, it becomes easier to reduce ΔT and easier to improve the tensile strength.

[0089] The solder alloy of the fourth embodiment further has the following effects. The solder alloy of the fourth embodiment can reduce the thickness of the intermetallic compound layer at the bonding interface. Also, the solder alloy of the fourth embodiment can sufficiently precipitate fine Ag3Sn and reduce the precipitation amount of coarse Ag3Sn. Also, the solder alloy of the fourth embodiment can suppress discoloration of the alloy. Also, the solder alloy of the fourth embodiment can increase the strength of the joint after soldering.

[0090] For the solder alloy of the fourth embodiment, it is preferable that Ni / (Ag + Bi) is more than 0.007. When 0.007 < Ni / (Ag + Bi), coarsening of the intermetallic compound can be suppressed and an excessive decrease in the solidus temperature can be suppressed. For the solder alloy of the fourth embodiment, it is preferable that Ni / (Ag + Bi) is less than 0.017. When Ni / (Ag + Bi) < 0.017, an excessive increase in the liquidus temperature can be suppressed. Thereby, sufficient wettability can be achieved. The solder alloy of the fourth embodiment preferably satisfies 0.007 < Ni / (Ag + Bi) < 0.017. Ni, Ag, and Bi each represent the content (% by mass) in the alloy composition.

[0091] For the solder alloy of the fourth embodiment, it is preferable that (Cu / Ni) × (Ag + Bi) exceeds 46. By having 46 < (Cu / Ni) × (Ag + Bi), an excessive increase in the liquidus temperature can be suppressed. Thereby, the wettability can be made sufficient. For the solder alloy of the fourth embodiment, it is preferable that (Cu / Ni) × (Ag + Bi) is less than 120. By having (Cu / Ni) × (Ag + Bi) < 120, coarsening of the intermetallic compound can be suppressed, and an excessive decrease in the solidus temperature can be suppressed. The solder alloy of the fourth embodiment preferably satisfies 46 < (Cu / Ni) × (Ag + Bi) < 120. The solder alloy of the fourth embodiment may have a composition that satisfies 46 < (Cu / Ni) × (Ag + Bi) < 110, or may have a composition that satisfies 46 < (Cu / Ni) × (Ag + Bi) < 100.

[0092] For the solder alloy of the fourth embodiment, it is preferable that 1.0 ≤ Ag / Bi ≤ 50.0, more preferably 1.0 ≤ Ag / Bi ≤ 3.0, and even more preferably 1.5 ≤ Ag / Bi ≤ 3.0. In the solder alloy of the fourth embodiment, when the ratio of Ag / Bi is within the above range, it becomes easier to reduce ΔT and easier to improve the tensile strength.

[0093] Alternatively, as another aspect, for the solder alloy of the fourth embodiment, it is preferable that 10.0 ≤ Ag / Bi ≤ 50.0, and more preferably 20.0 ≤ Ag / Bi ≤ 40.0. In the solder alloy of the fourth embodiment, when the ratio of Ag / Bi is within the above range, it becomes easier to reduce ΔT and easier to improve the tensile strength.

[0094] Alternatively, the solder alloy of the fourth embodiment preferably has an Ag / Bi ratio of 0.1 ≤ Ag / Bi ≤ 0.8, more preferably 0.15 ≤ Ag / Bi ≤ 0.7, and even more preferably 0.2 ≤ Ag / Bi ≤ 0.6. In the solder alloy of the fourth embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0095] The solder alloy of the fourth embodiment has a solidus temperature of 170 to 225°C, preferably 172 to 223°C, more preferably 174 to 221°C, and even more preferably 176 to 219°C. The solder alloy of the fourth embodiment has a liquidus temperature of 210 to 230°C, preferably 212 to 230°C, more preferably 212 to 228°C, and even more preferably 214 to 226°C. ΔT is preferably 50°C or less, more preferably 45°C or less, and even more preferably 40°C or less. The lower limit of ΔT is not particularly limited, but may be, for example, 1°C.

[0096] <Fifth Embodiment> The solder alloy of the fifth embodiment has an alloy composition consisting of Ag: 1.0-4.0 mass%, Cu: 0.7-1.0 mass%, Bi: 0.1-7.0 mass%, Ni: 0.040-0.095 mass%, Ge: 0.007-0.015 mass%, Co: 0.001-0.1 mass%, and the remainder being Sn, and is a lead-free and antimony-free solder alloy. The content of Ag, Cu, Bi, Ni, Ge, and Co may be as described above.

[0097] The solder alloy of the fifth embodiment may have an alloy composition consisting of Ag: 3.0-3.5 mass%, Cu: 0.7-1.0 mass%, Bi: 0.3-0.7 mass%, Ni: 0.040-0.060 mass%, Ge: 0.007-0.010 mass%, Co: 0.005-0.010 mass%, and the remainder being Sn, and may be a lead-free and antimony-free solder alloy.

[0098] In the solder alloy of the fifth embodiment, by having a specific alloy composition consisting of Ag, Cu, Bi, Ni, Ge, Co, and Sn, a lead-free and antimony-free solder alloy with a melting point near 230 °C and a tensile strength of 50 MPa or more can be provided. The solder alloy of the fifth embodiment can be applied not only to BGAs but also to die bonding. The solder alloy of the fifth embodiment can improve elongation, Poisson's ratio, and the coefficient of linear expansion.

[0099] Preferably, in the solder alloy of the fifth embodiment, 5 ≤ Ag / Bi ≤ 15. In the solder alloy of the fifth embodiment, when the ratio of Ag / Bi is within the above range, it becomes easier to reduce ΔT and easier to improve the tensile strength. Also, it becomes easier to improve elongation, Poisson's ratio, and the coefficient of linear expansion.

[0100] The solder alloy of the fifth embodiment further has the following effects. The solder alloy of the fifth embodiment can reduce the thickness of the intermetallic compound layer at the bonding interface. Also, the solder alloy of the fifth embodiment can sufficiently precipitate fine Ag3Sn and reduce the precipitation amount of coarse Ag3Sn. Also, the solder alloy of the fifth embodiment can suppress discoloration of the alloy. Also, the solder alloy of the fifth embodiment can increase the strength of the joint after soldering.

[0101] Preferably, in the solder alloy of the fifth embodiment, Ni / (Ag + Bi) > 0.007. When 0.007 < Ni / (Ag + Bi), coarsening of the intermetallic compound can be suppressed, and an excessive decrease in the solidus temperature can be suppressed. The solder alloy of the fifth embodiment preferably has Ni / (Ag + Bi) less than 0.017. By having Ni / (Ag + Bi) < 0.017, an excessive increase in the liquidus temperature can be suppressed. Thereby, the wettability can be made sufficient. The solder alloy of the fifth embodiment preferably satisfies 0.007 < Ni / (Ag + Bi) < 0.017. Ni, Ag, and Bi each represent the content (% by mass) in the alloy composition.

[0102] The solder alloy of the fifth embodiment preferably has (Cu / Ni)×(Ag + Bi) greater than 46. By having 46 < (Cu / Ni)×(Ag + Bi), an excessive increase in the liquidus temperature can be suppressed. Thereby, the wettability can be made sufficient. The solder alloy of the fifth embodiment preferably has (Cu / Ni)×(Ag + Bi) less than 120. By having (Cu / Ni)×(Ag + Bi) < 120, coarsening of the intermetallic compound can be suppressed and an excessive decrease in the solidus temperature can be suppressed. The solder alloy of the fifth embodiment preferably satisfies 46 < (Cu / Ni)×(Ag + Bi) < 120. The solder alloy of the fifth embodiment may have a composition that satisfies 46 < (Cu / Ni)×(Ag + Bi) < 110, or may have a composition that satisfies 46 < (Cu / Ni)×(Ag + Bi) < 100.

[0103] The solder alloy of the fifth embodiment preferably has 0.2 ≦ Ag / Bi ≦ 15.0, and more preferably has 5 ≦ Ag / Bi ≦ 15. In the solder alloy of the fifth embodiment, when the ratio of Ag / Bi is within the above range, it becomes easier to reduce ΔT and easier to improve the tensile strength. Also, in the solder alloy of the fifth embodiment, when the ratio of Ag / Bi is within the above range, elongation, Poisson's ratio, and the linear expansion coefficient can be improved.

[0104] Alternatively, the solder alloy of the fifth embodiment is preferably 0.2 ≤ Ag / Bi ≤ 15.0, more preferably 0.3 ≤ Ag / Bi ≤ 3.0, even more preferably 0.5 ≤ Ag / Bi ≤ 2.0, and particularly preferably 0.6 ≤ Ag / Bi ≤ 1.0. In the solder alloy of the fifth embodiment, having the Ag / Bi ratio within the above range makes it easier to reduce ΔT and improve tensile strength.

[0105] The solder alloy of the fifth embodiment preferably has a solidus temperature of 200 to 223°C, more preferably 202 to 221°C, and even more preferably 204 to 219°C. The solder alloy of the fifth embodiment preferably has a liquidus temperature of 210 to 227°C, more preferably 211 to 225°C, and even more preferably 213 to 223°C. In the fifth embodiment, the solder alloy preferably has a ΔT of 30°C or less, more preferably 20°C or less, and even more preferably 15°C or less. The lower limit of ΔT is not particularly limited, but may be, for example, 1°C.

[0106] 2. Solder ball The lead-free and antimony-free solder alloys of the embodiments described above are ideal for the form of solder balls used in BGAs. The sphericity of the solder ball in this embodiment is preferably 0.90 or higher, more preferably 0.95 or higher, and most preferably 0.99 or higher. Sphericity can be determined by various methods, such as the least squares center method (LSC method), the smallest area center method (MZC method), the largest inscribed center method (MIC method), and the smallest circumscribed center method (MCC method). In this invention, the sphericity of the solder ball is measured using a CNC image measurement system (ULTRA QV350-PRO measuring device manufactured by Mitutoyo Corporation) employing the minimum zone center method (MZC method). In this invention, sphericity represents the deviation from a perfect sphere, and is the arithmetic mean calculated by dividing the diameter of each of the 500 balls by its major axis. The closer the value is to the upper limit of 1.00, the closer it is to a perfect sphere.

[0107] The solder balls of this embodiment are used for forming electrodes and bumps on substrates of semiconductor packages such as BGAs (Ball Grid Arrays). The diameter of the solder ball in this embodiment is preferably in the range of 1 to 1000 μm, and more preferably 50 μm to 300 μm. Solder balls can be manufactured using general solder ball manufacturing methods. In this embodiment, the diameter refers to the diameter measured by the Mitutoyo UltraQuickVision, ULTRA QV350-PRO measuring device.

[0108] 3. Solder joints The solder joint of this embodiment is suitable for use in connecting an IC chip and its substrate (interposer) in a semiconductor package, or in connecting a semiconductor package and a printed circuit board. Here, the "solder joint" according to the present invention refers to a connection between an IC chip and a substrate, which is connected using the solder alloy according to the present invention described above, and includes electrode connection parts and connection parts between a die and a substrate.

[0109] 4. Others The joining method using the solder alloy of the embodiment described above can be carried out according to a standard procedure, for example, using the reflow method. The heating temperature may be adjusted as appropriate depending on the heat resistance of the chip and the liquidus temperature of the solder alloy. From the viewpoint of minimizing thermal damage to the chip, a temperature of around 240°C is preferable. When performing flow soldering, the melting temperature of the solder alloy may be approximately 20°C higher than the liquidus temperature. Furthermore, when joining using the solder alloy according to this embodiment, considering the cooling rate during solidification can further refine the microstructure. For example, the solder joint should be cooled at a cooling rate of 2-3°C / s or higher. Other joining conditions can be appropriately adjusted depending on the alloy composition of the solder alloy.

[0110] The solder alloy according to the present invention can be manufactured by using a low-alpha-dose material as its raw material. When such a low-alpha-dose alloy is used to form solder bumps around memory, it is possible to suppress soft errors. [Examples]

[0111] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.

[0112] The solder alloys of Examples 1 to 4 were synthesized with the compositions shown below. Measurements were performed on each solder alloy using the method described below.

[0113] (1) Measurement of solidus temperature and liquidus temperature The solidus and liquidus temperatures were measured using differential scanning calorimetry (DSC) with a thermomechanical analyzer (EXSTAR 6000, Seiko Instruments). The solidus temperature was measured according to the method specified in JIS Z3198-1. The liquidus temperature was measured using a DSC method, similar to the solidus temperature measurement method specified in JIS Z3198-1.

[0114] (2) Measurement of tensile strength and elongation Tensile tests were performed on specimens with a parallel section of 30 mm and a diameter of 8 mm using a universal material testing machine (Instron: 5966) to determine tensile strength and elongation.

[0115] (3) Poisson's ratio The Poisson's ratio was measured for a cubic test specimen with sides of 15 mm using a sing-around type sound velocity measuring device (Ultrasonic Industry Co., Ltd.: UVM-2).

[0116] (4) Coefficient of linear expansion The coefficient of linear thermal expansion was measured for a test specimen with a diameter of 8 mm and a length of 15 mm using a thermomechanical analyzer (EXSTAR 6000, Seiko Instruments).

[0117] (Example 1) A solder alloy was manufactured having an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 1.5 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn. The solder alloy in Example 1 had a solidus temperature of 214°C, a liquidus temperature of 219°C, and a ΔT of 5°C. The solder alloy of Example 1 had a tensile strength of 66.2 MPa.

[0118] (Example 2) A solder alloy was manufactured having an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 1.8 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, and the remainder being Sn. The solder alloy in Example 2 had a solidus temperature of 213°C, a liquidus temperature of 218°C, and a ΔT of 5°C. The solder alloy in Example 2 had a tensile strength of 69.9 MPa.

[0119] (Example 3) A solder alloy was manufactured having an alloy composition consisting of Ag: 2.0 mass%, Cu: 0.75 mass%, Bi: 4.0 mass%, Ni: 0.07 mass%, Ge: 0.008 mass%, and the remainder being Sn. The solder alloy in Example 3 had a solidus temperature of 206°C, a liquidus temperature of 219°C, and a ΔT of 13°C. The solder alloy of Example 3 had a tensile strength of 83.8 MPa.

[0120] (Example 4) A solder alloy was manufactured having an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 0.5 mass%, Ni: 0.05 mass%, Ge: 0.008 mass%, Co: 0.008 mass%, and the remainder being Sn. The solder alloy in Example 4 had a solidus temperature of 217°C, a liquidus temperature of 221°C, and a ΔT of 4°C. The solder alloy of Example 4 had a tensile strength of 55.5 MPa. The solder alloy in Example 4 had an elongation of 33%. The solder alloy in Example 4 had a Poisson's ratio of 0.35. The solder alloy of Example 4 had a coefficient of thermal expansion of 21.5 ppm / K.

[0121] (Example 5) A solder alloy was manufactured having an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 2.0 mass%, Ni: 0.05 mass%, Ge: 0.003 mass%, and the remainder being Sn. The solder alloy in Example 5 had a solidus temperature of 212°C, a liquidus temperature of 218°C, and a ΔT of 6°C. The solder alloy of Example 5 had a tensile strength of 72.3 MPa.

[0122] (Example 6) A solder alloy was manufactured having an alloy composition consisting of Ag: 3.5 mass%, Cu: 0.8 mass%, Bi: 2.5 mass%, Ni: 0.05 mass%, Ge: 0.003 mass%, and the remainder being Sn. The solder alloy of Example 6 had a solidus temperature of 211°C, a liquidus temperature of 216°C, and a ΔT of 5°C. The solder alloy of Example 6 had a tensile strength of 78.0 MPa.

[0123] <Preparation of solder alloy powder> (Test examples A1-A15, Test examples B1-B16) The solder alloy powders used in the test examples were prepared with the compositions shown in Tables 1-5 below. The solder alloy powder has a size (particle size distribution) that satisfies symbol 6 in the powder size classification (Table 2) of JIS Z 3284-1:2014. In this solder alloy powder, the mass fraction of powder with a particle size of 5 to 15 μm is 80% or more of the total mass (100%) of the solder alloy powder.

[0124] Test examples A1 to A12 and test example A14 correspond to the fourth embodiment. Test examples A13 and A15 correspond to the fifth embodiment.

[0125] Test examples B1 to B16 do not correspond to either the fourth or fifth embodiment. Test examples B3, B5-B6, B8-B9, and B11-B16 are within the scope of the present invention. Test examples B1-B2, B4, B7, and B10 are outside the scope of the present invention.

[0126] Using the solder alloy powder prepared above, the following evaluations were performed according to the evaluation methods described in <Evaluation> below: <Evaluation of intermetallic compound (IMC) layer thickness>, <Evaluation of Ag3Sn size>, <Evaluation of discoloration resistance>, <Evaluation of wettability>, and <Evaluation of solder joint strength>. The results are shown in Tables 1 and 2.

[0127] <Rating> Evaluation of the thickness of the intermetallic compound (IMC) layer Solder balls with a diameter of 0.3 mm were fabricated using the solder alloy powders from each example. For the CSP module board (S / F: electrolytic Ni / Au, size 12 x 12 mm), flux (manufactured by Senju Metal Industry Co., Ltd., WF-6400) was applied, and then solder balls were mounted. Next, reflow soldering was performed (220°C or higher, 40 seconds, peak temperature 245°C). This resulted in obtaining a CSP with solder ball electrodes. Furthermore, electrode patterns (S / F: Cu-OSP) were printed onto a glass epoxy substrate (FR-4, size 30 × 120 mm, thickness 0.8 mm) using solder paste. The solder alloy powder contained in the solder paste was a solder alloy consisting of 3 mass% Ag, 0.5 mass% Cu, and the remainder being Sn. Next, evaluation boards were fabricated by reflow soldering (220°C or higher, 40 seconds, peak temperature 245°C) using the above-mentioned CSP with solder ball electrodes and the printed glass epoxy substrate. Cross-sectional observation of the evaluation substrate after soldering was performed using a field emission scanning electron microscope (JEOL Ltd.: JSM-7000F). The observation area was the IMC at the bonding interface on the CSP side. The IMC thickness was measured using image processing software (Olympus: Scandium). The evaluation results for test examples A1-A15 and B1-B16 are shown in Tables 1 and 2.

[0128] Judgment criteria: A: The thickness of the IMC layer is less than 1.4 μm. B: The thickness of the IMC layer is 1.4 μm or more.

[0129] 《Evaluation of Ag3Sn size》 Solder balls with a diameter of 0.3 mm were fabricated using the solder alloy powders from each test example. After applying flux (manufactured by Senju Metal Industry Co., Ltd.: WF-6317) to the electrode (S / F: Cu-OSP), the resulting solder ball was mounted. Reflow soldering was performed using a reflow soldering machine (SNR-615, manufactured by Senju Metal Industries Co., Ltd.) with a peak temperature of 245°C and a cooling rate of 2°C / s. Cross-sectional observations were performed on the soldered samples using a field emission scanning electron microscope (JEOL Ltd.: JSM-7000F). The evaluation results for test examples A1-A15 and B1-B16 are shown in Tables 1 and 2.

[0130] Judgment criteria: A: The maximum length of Ag3Sn is less than 5 μm. B: The maximum length of Ag3Sn is between 5 μm and 90 μm. The maximum length of C:Ag3Sn is 90 μm or more.

[0131] 《Evaluation of colorfastness》 Solder balls with a diameter of 0.3 mm were fabricated using the solder alloy powders from each example. The solder balls were placed in a highly accelerated life testing chamber (HAST chamber, ESPEC Corporation: EHS-211M). The temperature was set to 125°C / 100%RH, and after 4 hours, the presence or absence of discoloration of the solder balls was visually checked. The evaluation results for test examples A1-A15 and B1-B16 are shown in Tables 1 and 2.

[0132] Judgment criteria: A: The solder ball has not changed color. B: The solder ball is discolored.

[0133] Evaluation of wettability Solder balls with a diameter of 0.3 mm were fabricated using the solder alloy powders from each example. After applying flux (manufactured by Senju Metal Industry Co., Ltd.: WF-6317) to the substrate (S / F: Cu-OSP), the resulting solder balls were mounted. Next, reflow soldering was performed (220°C or higher, 40 seconds, peak temperature 245°C). After reflow soldering, the length of the wetted area was measured using a digital microscope (Keyence Corporation: VHX-6000). The evaluation results for test examples A1-A15 and B1-B16 are shown in Tables 1 and 2.

[0134] Judgment criteria: A: The wetting spread length is 1000 μm or more. B: The wetting spread length is less than 1000 μm.

[0135] Evaluation of the strength of solder joints Solder balls with a diameter of 0.76 mm were fabricated using the solder alloy powders from each example. After applying flux (WF-6400, manufactured by Senju Metal Industry Co., Ltd.) to an electrolytically treated Ni / Au substrate, solder balls were placed on top of it. Next, reflow soldering was performed (220°C or higher, 40 seconds, peak temperature 245°C). The test was performed on soldered samples using a pull tester (Nordson Advanced Technologies, Inc.: Dage4000HS) at a test speed of 1000 μm / s. The number of tests was N=20. The evaluation results for test examples A1-A15 and B1-B16 are shown in Tables 1 and 2.

[0136] Judgment criteria: A: The percentage of tests in which the IMC layer was destroyed was 50% or less of the total number of tests. B: The proportion of tests in which the IMC layer was destroyed exceeded 50% of the total number of tests.

[0137] [Table 1]

[0138] [Table 2]

[0139] As shown in Table 1, test examples A1 to A15, which correspond to the fourth or fifth embodiment, received an evaluation of A for the thickness of the IMC layer. Furthermore, in test examples B1-B2 and B7-B16, where the Cu content was 0.7-1.0 mass% and the Ni content was 0.040-0.095 mass% or less, the IMC layer thickness was evaluated as A. In contrast, test examples B3 to B6, in which the Cu or Ni content was outside the above range, received a rating of B for the thickness of the IMC layer.

[0140] As shown in Table 1, test examples A1 to A15, which correspond to the fourth or fifth embodiment, received an evaluation of A or B for the size of Ag3Sn. In Test Examples A1, A3-A14, B1, and B3-B15, where the Ag content was 3.5% by mass or less, the size evaluation of Ag3Sn was A. Furthermore, in Test Examples A2 and B16, which had an Ag content of 4.0% by mass, the size evaluation of Ag3Sn was B. In contrast, in test example B2, which had an Ag content of over 4.0% by mass, the size evaluation of Ag3Sn was C.

[0141] As shown in Table 1, test examples A1 to A15, which correspond to the fourth or fifth embodiment, received a discoloration resistance rating of A. Furthermore, test examples B1-B8 and B10-B12, which had a Ge content of 0.007% by mass or more, received a discoloration resistance rating of A. In contrast, test examples B9, B13-B16, which had a Ge content of less than 0.007% by mass, received a B rating for discoloration resistance.

[0142] As shown in Table 1, Test Examples A1 to A15, which correspond to the fourth or fifth embodiment, received a wettability evaluation of A. Furthermore, test examples B2-B3, B5, and B8-B9 received an A rating for wettability. In contrast, test examples B1, B6, and B11-B13, where 0.017 ≤ Ni / (Ag+Bi) and (Cu / Ni) × (Ag+Bi) ≤ 46, received a wettability evaluation of B. Furthermore, test example B4, which had a Cu content of more than 1.0% by mass, received a wettability rating of B. Furthermore, test example B7, which had a Bi content of less than 0.1% by mass, received a wettability rating of B. Furthermore, test example B10, which had a Ge content of more than 0.015% by mass, received a wettability rating of B. Furthermore, test example B14, which did not contain sufficient Ag or Bi, received a wettability rating of B.

[0143] As shown in Table 1, test examples A1 to A15, which correspond to the fourth or fifth embodiment, received an A rating for the strength of the solder joints. Furthermore, in test examples B1-B8, B9, and B11-B16, where the composition was Ag: 1.0-4.0 mass%, Cu: 0.7-1.0 mass%, Bi: 0.1-7.0 mass%, Ni: 0.040-0.095 mass%, and Ge: 0.015 mass% or less, the strength of the solder joints was evaluated as A. In contrast, test examples B1 and B2, in which the Ag content was outside the above range, received a rating of B for the strength of the solder joints. Furthermore, in test examples B3 and B4, where the Cu content was outside the above range, the strength evaluation of the solder joint was rated as B. Furthermore, in test examples B5 and B6, where the Ni content was outside the above range, the strength evaluation of the solder joint was rated as B. Furthermore, in test examples B7 and B8, where the Bi content was outside the specified range, the strength evaluation of the solder joints was rated as B. Furthermore, in test example B10, which had a Ge content of more than 0.015 mass%, the strength of the solder joint was evaluated as B.

[0144] As described above, the solder alloys of the fourth and fifth embodiments provide the following effects. The aforementioned solder alloy can reduce the thickness of the intermetallic compound layer at the bonding interface. Furthermore, the aforementioned solder alloy can sufficiently precipitate fine Ag3Sn particles while reducing the amount of coarse Ag3Sn precipitated. Furthermore, the solder alloy of the fifth embodiment can suppress discoloration of the alloy. Furthermore, the solder alloy of the fifth embodiment can increase the strength of the joint after soldering. The aforementioned solder alloy can improve wettability.

[0145] Furthermore, the solidus and liquidus temperatures were measured using the solder alloy powder prepared above, following the procedure described in "(1) Measurement of Solidus Temperature and Liquidus Temperature". Additionally, the tensile strength was measured using the solder alloy powder prepared above, following the procedure described in "(2) Measurement of Tensile Strength and Elongation". The measurement results are shown in Tables 3-4. Test examples A1 to A15 had a melting point of around 230°C and a tensile strength of 50 MPa or more.

[0146] [Table 3]

[0147] [Table 4] [Industrial applicability]

[0148] According to the present invention, lead-free and antimony-free solder alloys, solder balls, and solder joints can be provided, having a melting point of around 230°C and a tensile strength of 50 MPa or more. These solder alloys, solder balls, and solder joints can be suitably used in QFPs.

Claims

1. A lead-free and antimony-free solder alloy having an alloy composition consisting of 1.0 to 4.0 mass% Ag, 0.1 to 1.0 mass% Cu, 0.1 to 9.0 mass% Bi, 0.005 to 0.3 mass% Ni, 0.001 to 0.015 mass% Ge, and the balance being Sn.

2. A solder ball made of the solder alloy according to claim 1.

3. A ball grid array formed using the solder balls according to claim 2.