Low-reflection coatings, coating kits, cured products and laminates

JP2023068001A5Active Publication Date: 2024-11-13ARAKAWA CHEM IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023036511
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-20
Filing Date
2023-03-09
Publication Date
2024-11-13
Estimated Expiration
2041-11-16

AI Technical Summary

Technical Problem

Existing low-reflection coatings using hollow particles and solid alumina particles face issues of stability and reduced scratch resistance due to the coexistence of these particles in the same system.

Method used

A low-reflection coating agent containing acidic group-containing poly(meth)acrylate, hollow inorganic particles, and solid alumina particles, with a specific content of 2 to 15% by mass of solid alumina particles, is used to enhance stability and scratch resistance while maintaining low reflectivity.

Benefits of technology

The coating agent achieves good stability and scratch resistance, enabling the production of laminates with improved low reflectivity and durability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a low-reflection coating agent, a coating agent kit, a cured product, and a laminate. [Solution] The present disclosure provides a low-reflection coating agent comprising an acidic group-containing poly(meth)acrylate, hollow inorganic particles, and solid alumina particles, the solid alumina particles being present in an amount of 2 to 15 mass% of the solid content. The present disclosure also provides a coating agent kit comprising a low-reflection coating agent containing 2 to 15 mass% of solid alumina particles of the solid content, and an anchoring agent containing solid alumina particles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to low-reflection coating agents, coating agent kits, cured products, and laminates. [Background technology]

[0002] In recent years, liquid crystal displays have been used as display devices for televisions, personal computers, and other devices. In such liquid crystal displays, it has been proposed to use an anti-reflective coating that includes a low refractive index layer in order to prevent reflection of ambient light and improve image quality (Patent Document 1). [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2014-085383 [Overview of the Initiative] [Problems that the invention aims to solve]

[0004] Hollow particles are sometimes used in coatings to give them low reflectivity (low refractive index). However, because the particles are hollow, there is a problem in that their scratch resistance is reduced.

[0005] By further incorporating solid alumina particles into a coating agent containing hollow particles, the decrease in scratch resistance can be suppressed. However, it was found that stability becomes an issue when hollow particles and solid alumina particles coexist in the same system.

[0006] Therefore, one of the problems that the invention aims to solve is to provide a low-reflection coating agent with good stability.

[0007] One of the problems that this invention aims to solve is to provide a coating agent kit that can produce laminates with good scratch resistance while maintaining low reflectivity. [Means for solving the problem]

[0008] As a result of diligent research, the inventors of this invention have found that the above problem can be solved by using a specific component.

[0009] This disclosure provides the following items: (Item 1) Acid group-containing poly(meth)acrylate, Hollow inorganic particles and Contains solid alumina particles, The content of the solid alumina particles is 2 to 15% by mass of the solid content. Low-reflection coating agent. (Item 2) A low-reflection coating agent as described above, comprising a (meth)acryloyl group-containing perfluoropolyether. (Item 3) A low-reflection coating agent containing solid alumina particles at a concentration of 2-15% by mass in the solid content, and A coating kit containing an anchoring agent with solid alumina particles. (Item 4) A low-reflection coating agent and / or a cured product of a coating agent kit as described in any one of the above items. (Item 5) A laminate containing the cured material described in the above items.

[0010] In this disclosure, one or more of the features described above may be provided in combinations other than those explicitly stated. [Effects of the Invention]

[0011] The low-reflection coating agent according to this embodiment has good stability.

[0012] By using the coating agent kit according to this embodiment, laminates with good low reflectivity and scratch resistance can be manufactured. [Modes for carrying out the invention]

[0013] Throughout this disclosure, the ranges of numerical values ​​such as physical properties and content may be set as appropriate (for example, by selecting from the upper and lower limits described in each item below). Specifically, for numerical value α, if A3, A2, A1 (A3 > A2 > A1) are given as examples of the upper and lower limits of numerical value α, then the range of numerical value α may be A3 or less, A2 or less, less than A3, less than A2, A1 or more, A2 or more, greater than A1, greater than A2, A1 to A2 (A1 or more and A2 or less), A1 to A3, A2 to A3, A1 or more and less than A3, A1 or more and less than A2, A2 or more and less than A3, greater than A1 and less than A3, greater than A1 and A3 or less, greater than A1 and A2 or less, greater than A2 and A3 or less.

[0014] [Low-reflection coating agent: also called a coating agent] This disclosure relates to acidic group-containing poly(meth)acrylate, Hollow inorganic particles and Contains solid alumina particles, The content of the solid alumina particles is 2 to 15% by mass of the solid content. We provide a low-reflection coating agent.

[0015] <Poly(meth)acrylate containing acidic groups> Acidic group-containing poly(meth)acrylates can be used alone or in combination of two or more types.

[0016] In this disclosure, "acidic group-containing poly(meth)acrylate" means a compound having one or more acidic groups and two or more (meth)acryloyl groups.

[0017] In this disclosure, "acidic group" means a group in which one or more hydrogen atoms dissociate to form a base.

[0018] Examples of acidic groups include hydroxyl groups, carboxyl groups, sulfonic acid groups, and phosphate groups.

[0019] In this disclosure, "(meth)acrylic" means "at least one selected from the group consisting of acrylic and methacrylic." Similarly, "(meth)acrylate" means "at least one selected from the group consisting of acrylate and methacrylate." Also, "(meth)acryloyl" means "at least one selected from the group consisting of acryloyl and methacryloyl."

[0020] It is believed that the stability of low-reflectivity coating agents can be improved by using acidic group-containing poly(meth)acrylate. This is thought to be because the acidic group-containing poly(meth)acrylate acts as a dispersant for solid alumina particles, preventing aggregation and sedimentation of the solid alumina particles. However, the above is merely one theory, and the present invention is not intended to be bound by this theory.

[0021] Examples of acidic group-containing poly(meth)acrylates include hydroxyl group-containing poly(meth)acrylates and carboxyl group-containing poly(meth)acrylates.

[0022] (Hydroxyl group-containing poly(meth)acrylate) Examples of hydroxyl group-containing poly(meth)acrylates include hydroxyl group-containing (poly)pentaerythritol poly(alkylene oxide modified or epoxy modified) (meth)acrylate, hydroxyl group-containing (poly)trimethylolpropane poly(alkylene oxide modified or epoxy modified) (meth)acrylate, and hydroxyl group-containing (poly)glycerin poly(alkylene oxide modified or epoxy modified) (meth)acrylate.

[0023] • Hydroxyl group-containing (poly)pentaerythritol poly(alkylene oxide modified or epoxy modified) (meth)acrylate (Poly)pentaerythritol poly(alkylene oxide-modified or epoxy-modified)(meth)acrylate is a compound represented by formula (A'), etc. [ka] [wherein, n is an integer from 0 to 2, and R b5A ~R b6 ’ are each independently a hydrogen atom,

Chemical formula

Chemical formula

[0026] Examples of hydroxyl group-containing pentaerythritol poly(meth)acrylates include pentaerythritol di(meth)acrylate and pentaerythritol tri(meth)acrylate.

[0027] Examples of hydroxyl group-containing pentaerythritol polyalkylene oxide-modified (meth)acrylates include pentaerythritol di(ethylene oxide-modified (meth)acrylate), pentaerythritol tri(ethylene oxide-modified (meth)acrylate), pentaerythritol di(propylene oxide-modified (meth)acrylate), and pentaerythritol tri(propylene oxide-modified (meth)acrylate).

[0028] Examples of hydroxyl group-containing pentaerythritol polyepoxy-modified (meth)acrylates include pentaerythritol diepoxy (meth)acrylate and pentaerythritol triepoxy (meth)acrylate.

[0029] Examples of hydroxyl group-containing polypentaerythritol poly(meth)acrylates include dipentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol di(meth)acrylate, tripentaerythritol tri(meth)acrylate, tripentaerythritol tetra(meth)acrylate, tripentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, and tripentaerythritol hepta(meth)acrylate.

[0030] Hydroxyl group-containing polypentaerythritol polyalkylene oxide-modified (meth)acrylates include dipentaerythritol di(ethylene oxide-modified (meth)acrylate), dipentaerythritol tri(ethylene oxide-modified (meth)acrylate), dipentaerythritol tetra(ethylene oxide-modified (meth)acrylate), dipentaerythritol penta(ethylene oxide-modified (meth)acrylate), and dipentaerythritol hexa(ethylene oxide-modified (meth)acrylate). Tripentaerythritol (ethylene oxide modified (meth)acrylate), dipentaerythritol di(propylene oxide modified (meth)acrylate), dipentaerythritol tri(propylene oxide modified (meth)acrylate), dipentaerythritol tetra(propylene oxide modified (meth)acrylate), dipentaerythritol penta(propylene oxide modified (meth)acrylate), tripentaerythritol di(ethylene oxide modified (meth)acrylate), tripentaerythritol tri(ethylene oxide modified (meth)acrylate) Tripentaerythritol tetra(ethylene oxide modified (meth)acrylate), tripentaerythritol penta(ethylene oxide modified (meth)acrylate), tripentaerythritol hexa(ethylene oxide modified (meth)acrylate), tripentaerythritol hepta(ethylene oxide modified (meth)acrylate), tripentaerythritol octa(ethylene oxide modified (meth)acrylate), tripentaerythritol di(propylene Examples include tripentaerythritol tri(propylene oxide modified (meth)acrylate), tripentaerythritol tetra(propylene oxide modified (meth)acrylate), tripentaerythritol penta(propylene oxide modified (meth)acrylate), tripentaerythritol hexa(propylene oxide modified (meth)acrylate), tripentaerythritol hepta(propylene oxide modified (meth)acrylate), etc.

[0031] Examples of hydroxyl group-containing polypentaerythritol polyepoxy-modified (meth)acrylates include dipentaerythritol diepoxy (meth)acrylate, dipentaerythritol triepoxy (meth)acrylate, dipentaerythritol tetraepoxy (meth)acrylate, dipentaerythritol pentaepoxy (meth)acrylate, tripentaerythritol diepoxy (meth)acrylate, tripentaerythritol triepoxy (meth)acrylate, tripentaerythritol tetraepoxy (meth)acrylate, tripentaerythritol pentaepoxy (meth)acrylate, tripentaerythritol hexapoxy (meth)acrylate, and tripentaerythritol heptapoxy (meth)acrylate.

[0032] • Hydroxyl group-containing (poly)trimethylolpropane poly(alkylene oxide modified or epoxy modified) (meth)acrylate Hydroxyl group-containing (poly)trimethylolpropane poly(alkylene oxide-modified or epoxy-modified) (meth)acrylate is a compound represented by formula (B'), etc. [ka] [In the formula, m is an integer from 0 to 2, R b7’ ~R b10 ’ Each of them is an independent hydrogen atom, [ka] {In the formula, each q is an independent integer from 0 to 16, R 1’ ~R 3’ Each is independently a hydrogen atom or an alkyl group, and R 1’ The base may differ for each unit. And, R b9’ The base may be different for each constituent unit. Formula (B ’ ) in R b7’ ~R b10 ’ Two or more of them [ka] {In the formula, q is an integer from 0 to 16, R 1’ ~R 3 ’ Each is independently a hydrogen atom or an alkyl group, and R 1’ The base may differ for each unit. And R b7’ ~R b10 ’ One or more of them are hydrogen atoms.

[0033] In this disclosure, "hydroxyl group-containing (poly)trimethylolpropane poly(alkylene oxide modified or epoxy modified) (meth)acrylate" means "at least one selected from the group consisting of hydroxyl group-containing trimethylolpropane poly(meth)acrylate, hydroxyl group-containing trimethylolpropane polyalkylene oxide modified (meth)acrylate, hydroxyl group-containing trimethylolpropane polyepoxy modified (meth)acrylate, hydroxyl group-containing polytrimethylolpropane poly(meth)acrylate, hydroxyl group-containing polytrimethylolpropane polyalkylene oxide modified (meth)acrylate, and hydroxyl group-containing polytrimethylolpropane polyepoxy modified (meth)acrylate."

[0034] Examples of hydroxyl group-containing trimethylolpropane poly(meth)acrylates include trimethylolpropane di(meth)acrylate.

[0035] Examples of hydroxyl group-containing trimethylolpropane polyalkylene oxide-modified (meth)acrylates include trimethylolpropane (ethylene oxide-modified (meth)acrylate) and trimethylolpropane (propylene oxide-modified (meth)acrylate).

[0036] Examples of hydroxyl group-containing trimethylolpropane polyepoxy-modified (meth)acrylates include trimethylolpropane diepoxy (meth)acrylate.

[0037] Examples of hydroxyl group-containing polytrimethylolpropane poly(meth)acrylates include ditrimethylolpropanedi(meth)acrylate and ditrimethylolpropanetri(meth)acrylate.

[0038] Examples of hydroxyl group-containing polytrimethylolpropane polyalkylene oxide-modified (meth)acrylates include ditrimethylolpropanedi (ethylene oxide-modified (meth)acrylate), ditrimethylolpropanetri (ethylene oxide-modified (meth)acrylate), ditrimethylolpropanedi (propylene oxide-modified (meth)acrylate), and ditrimethylolpropanetri (propylene oxide-modified (meth)acrylate).

[0039] Examples of hydroxyl group-containing polytrimethylolpropane polyepoxy-modified (meth)acrylates include ditrimethylolpropane diepoxy (meth)acrylate and ditrimethylolpropane triepoxy (meth)acrylate.

[0040] • Hydroxyl group-containing (poly)glycerin, poly(alkylene oxide modified or epoxy modified) (meth)acrylate Hydroxyl group-containing (poly)glycerin poly(alkylene oxide-modified or epoxy-modified) (meth)acrylate is a compound represented by formula (C'), etc. [ka] [In the formula, p is an integer from 0 to 7, R b11’ ~R b14 ’ Each of them is an independent hydrogen atom, [ka] {In the formula, q is an integer from 0 to 16, R 1’ ~R 3’ Each is independently a hydrogen atom or an alkyl group, and R 1’ The base may differ for each unit. And, R b13’The base may be different for each constituent unit. Formula (C ’ ) in R b11’ ~R b14 ’ Two or more of [ka] {In the formula, q is an integer from 0 to 16, R 1’ ~R 3 ’ Each is independently a hydrogen atom or an alkyl group, and R 1’ The base may differ for each unit. And R b11’ ~R b14 ’ One or more of them are hydrogen atoms.

[0041] In this disclosure, "hydroxyl group-containing (poly)glycerin poly(alkylene oxide-modified or epoxy-modified) (meth)acrylate" means "at least one selected from the group consisting of hydroxyl group-containing glycerin poly(meth)acrylate, hydroxyl group-containing glycerin polyalkylene oxide-modified (meth)acrylate, hydroxyl group-containing glycerin polyepoxy-modified (meth)acrylate, hydroxyl group-containing polyglycerin poly(meth)acrylate, hydroxyl group-containing polyglycerin polyalkylene oxide-modified (meth)acrylate, and hydroxyl group-containing polyglycerin polyepoxy-modified (meth)acrylate."

[0042] Examples of hydroxyl group-containing glycerin poly(meth)acrylates include glycerin di(meth)acrylate.

[0043] Examples of hydroxyl group-containing glycerol polyalkylene oxide-modified (meth)acrylates include glycerol (ethylene oxide-modified (meth)acrylate) and glycerol (propylene oxide-modified (meth)acrylate).

[0044] Examples of hydroxyl group-containing glycerin polyepoxy-modified (meth)acrylates include glycerin diepoxy (meth)acrylate.

[0045] Examples of hydroxyl group-containing polyglycerin poly(meth)acrylates include diglycerin di(meth)acrylate, diglycerin tri(meth)acrylate, triglycerin di(meth)acrylate, triglycerin tri(meth)acrylate, and triglycerin tetra(meth)acrylate.

[0046] Examples of hydroxyl group-containing polyglycerin polyalkylene oxide-modified (meth)acrylates include diglycerin di(ethylene oxide-modified (meth)acrylate), diglycerin tri(ethylene oxide-modified (meth)acrylate), triglycerin di(ethylene oxide-modified (meth)acrylate), triglycerin tri(ethylene oxide-modified (meth)acrylate), triglycerin tetra(ethylene oxide-modified (meth)acrylate), diglycerin di(propylene oxide-modified (meth)acrylate), diglycerin tri(propylene oxide-modified (meth)acrylate), triglycerin di(propylene oxide-modified (meth)acrylate), triglycerin tri(propylene oxide-modified (meth)acrylate), triglycerin tetra(propylene oxide-modified (meth)acrylate), etc.

[0047] Examples of hydroxyl group-containing polyglycerin polyepoxy-modified (meth)acrylates include diglycerin diepoxy (meth)acrylate, diglycerin triepoxy (meth)acrylate, triglycerin diepoxy (meth)acrylate, triglycerin triepoxy (meth)acrylate, and triglycerin tetraepoxy (meth)acrylate.

[0048] (Carboxyl group-containing poly(meth)acrylate) Examples of carboxyl group-containing poly(meth)acrylates include reaction products of hydroxyl group-containing poly(meth)acrylates and carboxylic acid anhydrides.

[0049] Examples of carboxylic acid anhydrides include phthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, nadic anhydride, methylnadic anhydride, maleic anhydride, itaconic anhydride, and succinic anhydride.

[0050] Examples of carboxyl group-containing poly(meth)acrylate products include Arronix M510 (acid value: 80-120 mg KOH / g, manufactured by Toagosei Co., Ltd.) and Arronix M520 (acid value: 20-40 mg KOH / g, manufactured by Toagosei Co., Ltd.).

[0051] In one embodiment, the acidic group-containing poly(meth)acrylate is preferably a carboxyl group-containing poly(meth)acrylate from the viewpoint of good scratch resistance of the cured product, more preferably a reaction product of pentaerythritol tri(meth)acrylate or dipentaerythritol penta(meth)acrylate with a carboxylic acid anhydride, even more preferably a reaction product of pentaerythritol tri(meth)acrylate with a carboxylic acid anhydride, and particularly preferably a reaction product of pentaerythritol tri(meth)acrylate with succinic acid anhydride.

[0052] Examples of the upper and lower molecular weight limits for acidic group-containing poly(meth)acrylates include 50,000, 40,000, 30,000, 20,000, 10,000, 5,000, 4,000, 2,000, 1,000, 900, 800, 700, 600, 500, 450, 400, 300, 250, 100, and 50. In one embodiment, the above molecular weight is preferably 50 to 50,000.

[0053] In this disclosure, when the term "molecular weight" is used, it refers to either the formula weight or the number-average molecular weight. If the structure of a compound can be uniquely represented by a specific chemical formula (i.e., the molecular weight distribution is 1), the molecular weight refers to the formula weight. On the other hand, if the structure of a compound cannot be uniquely represented by a specific chemical formula (i.e., the molecular weight distribution is greater than 1), the molecular weight refers to the number-average molecular weight.

[0054] Examples of upper and lower limits for the acid value of acidic group-containing poly(meth)acrylate include 300, 290, 280, 270, 260, 250, 240, 230, 220, 210, 200, 190, 180, 170, 160, 150, 140, 130, 120, 110, 100, 90, 80, 70, 60, 50, 40, 30, 20, and 10 mgKOH / g. In one embodiment, the above acid value is preferably 10 to 300 mgKOH / g.

[0055] Examples of the upper and lower limits of the hydroxyl value of acidic group-containing poly(meth)acrylates include 280, 270, 260, 250, 240, 230, 220, 210, 200, 190, 180, 170, 160, 150, 140, 130, 120, 110, 100, 90, 80, 70, 60, 50, 40, 30, 20, 10, 5, and 0 mgKOH / g. In one embodiment, the above hydroxyl value is preferably 0 to 280 mgKOH / g, and more preferably 10 to 280 mgKOH / g.

[0056] Examples of upper and lower limits for the number of (meth)acryloyl groups in an acidic group-containing poly(meth)acrylate include 30, 28, 26, 24, 22, 20, 18, 16, 14, 12, 10, 9, 8, 7, 6, 5, 4, 3, and 2. In one embodiment, the above number is preferably around 2 to 30.

[0057] Examples of the upper and lower limits for the number of acidic groups in an acidic group-containing poly(meth)acrylate include 10, 9, 8, 7, 6, 5, 4, 3, 2, and 1. In one embodiment, the number is preferably 1 to 10.

[0058] Examples of upper and lower limits for the content of acidic group-containing poly(meth)acrylate in 100% by mass of the coating agent solid content include 70, 65, 60, 57, 55, 54, 53, 52, 51, 50, 49, 48, 47, 46, 45, 44, 43, 42, 41, 40, 35, 30, 25, and 20% by mass. In one embodiment, the above content is preferably 20 to 70% by mass.

[0059] <Hollow inorganic particles> Hollow inorganic particles can be used alone or in combination of two or more types.

[0060] Hollow particles can be used without particular limitations as long as they have voids inside. Hollow particles may be spherical, rod-shaped, plate-shaped, fibrous, or of any irregular shape.

[0061] Examples of hollow inorganic particles include hollow silica particles, hollow aluminosilicate particles, hollow alumina particles, hollow mullite particles, hollow titanium oxide particles, hollow magnesium fluoride particles, and fly ash balloons.

[0062] In one embodiment, the hollow inorganic particles are preferably modified hollow inorganic particles with a modified surface. Examples of modified hollow inorganic particles include (meth)acrylic modified hollow inorganic particles and silicone modified hollow inorganic particles.

[0063] Examples of upper and lower limits for the content of the modified portion relative to 100% by mass of modified hollow inorganic particles include 40, 35, 30, 25, 20, 15, 10, 5, 1, 0.1, and 0.01% by mass. In one embodiment, from the viewpoint of improving particle dispersibility and scratch resistance of the cured product, the above content is preferably about 0.01 to 40% by mass, more preferably 0.1 to 30% by mass, and even more preferably 1 to 20% by mass.

[0064] Examples of hollow inorganic particle products include Thru-Ria 5320, Thru-Ria 4320, Thru-Ria 4110, Thru-Ria 2320, Thru-Ria 1110, JX1008SIV, JX1009SIV (manufactured by JGC Catalysts & Chemicals Co., Ltd.), and Silinax (manufactured by Nippon Steel Mining Co., Ltd.).

[0065] Examples of upper and lower limits for the particle size of hollow inorganic particles include 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, and 40 nm. In one embodiment, the particle size is preferably 40 to 100 nm.

[0066] The particle size of hollow inorganic particles is measured using a scanning electron microscope (e.g., JSM-7800F Prime (manufactured by JEOL Ltd.)) and a STEM detector (manufactured by DEBEN UK Ltd.). Specifically, the measurement is performed according to the following procedure. First, the particle sample is diluted to a 0.2% concentration of the active ingredient with methyl isobutyl ketone and thoroughly mixed. Next, one drop of the above dispersion is placed on a microgrid with a support membrane for STEM (Hi-ResoCarbon HRC-C10 STEM Cu100P grid specification (manufactured by STEM Co., Ltd.)), and the resulting sample is dried to be used as the measurement sample. Next, using a scanning electron microscope, images are acquired at a magnification (e.g., 300kx) that allows for sufficient measurement of particles in the field of view, under an acceleration voltage of 30kV. The particle size of 50 randomly selected particles is then measured to determine the particle diameter based on the number of particles. Particle size can be measured manually or using a measuring tool.

[0067] Examples of upper and lower refractive indices for hollow inorganic particles include 1.5, 1.4, 1.3, 1.2, and 1.1. In one embodiment, the refractive index of the hollow inorganic particles is preferably between 1.1 and 1.5.

[0068] The refractive index of hollow inorganic particles is calculated by forming a film of a composition containing the substance to be measured in solid matter ratios of 1%, 10%, and 20% in an active energy ray curable resin (for example, dipentaerythritol polyacrylate manufactured by Shin Nakamura Chemical Industry Co., Ltd.: product name NK Ester A-9550W), and measuring the refractive index for the D-line wavelength of sodium in accordance with JIS K7142:2014 using an Abbe refractometer (product name "NAR-1T SOLID", manufactured by Atago Co., Ltd.), and extrapolating this to a solid matter ratio of 100% by mass.

[0069] Examples of upper and lower limits for the content of hollow inorganic particles in 100% by mass of the coating agent solid content include 65, 60, 55, 50, 45, 44, 43, 42, 41, 40, 39, 38, 37, 35, 30, 25, and 20% by mass. In one embodiment, the above content is preferably 20 to 65% by mass.

[0070] <Solid alumina particles> Solid alumina particles can be used alone or in combination of two or more types.

[0071] A solid particle is a particle that does not have voids inside.

[0072] Alumina refers to aluminum oxide represented by Al2O3, and is known to exist in various forms such as α-type, γ-type, σ-type, and mixtures thereof.

[0073] The solid alumina particles may be spherical, rod-shaped, plate-shaped, fibrous, or of any other shape.

[0074] In one embodiment, the solid alumina particles are preferably modified solid alumina particles with a modified surface. Examples of modified solid alumina particles include (meth)acrylic modified solid alumina particles and silicone modified solid alumina particles.

[0075] Examples of solid alumina particle products include Aluminol F-3000 (manufactured by Kawaken Fine Chemicals Co., Ltd.), Bailar AL-7 (manufactured by Taki Chemical Co., Ltd.), NANOBYK-3610 (manufactured by BYK Chemie), and Optisol LAA530U (manufactured by RANCO).

[0076] Examples of upper and lower limits for the primary particle diameter of solid alumina particles include 110, 100, 90, 80, 70, 60, 50, 40, 30, 20, 15, 10, 7, and 3 nm. In one embodiment, the primary particle diameter is preferably 3 to 110 nm.

[0077] The primary particle size of solid alumina particles can be measured using the same method as the method for measuring the particle size of hollow inorganic particles described above.

[0078] Examples of upper and lower limits for the secondary particle diameter of solid alumina particles include 110, 100, 90, 80, 70, 60, 55, 50, 45, 40, 35, 30, and 25 nm. In one embodiment, the secondary particle diameter is preferably 25 to 110 nm.

[0079] The secondary particle size of solid alumina particles is measured by the following procedure. First, the particle sample is diluted with methyl isobutyl ketone to a 1% concentration of the active ingredient to prepare a sample solution. Next, the prepared sample solution is measured using a nanoparticle diameter analyzer (product name "NanoTrack UPA-EX150" manufactured by MicroTrack-Bell Co., Ltd.) using the dynamic light scattering method. The particle diameter obtained by this measurement method is the volume-average particle diameter, and the median diameter value is defined as the particle diameter.

[0080] Examples of upper and lower limits for the content of solid alumina particles in 100% by mass of the coating agent solid content include 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, and 2% by mass. In one embodiment, the above content is preferably 2 to 15% by mass, and more preferably 6 to 15% by mass.

[0081] <(meth)acryloyl group-containing perfluoropolyether> In one embodiment, the coating agent may include a (meth)acryloyl group-containing perfluoropolyether. The (meth)acryloyl group-containing perfluoropolyether may be used alone or in combination of two or more types.

[0082] In this disclosure, (meth)acryloyl group-containing perfluoropolyether means a compound in which one or more (meth)acryloyl groups are bonded to a perfluoropolyether. Perfluoropolyether means a compound in which perfluoroalkylene ether is a repeating unit.

[0083] Examples of (meth)acryloyl group-containing perfluoropolyethers include perfluoropolyethers containing (meth)acryloyl groups at both ends and perfluoropolyethers containing a (meth)acryloyl group at one end.

[0084] Examples of perfluoropolyether products containing (meth)acryloyl groups include KY-1203 and KY-1207 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0085] In one embodiment, from the viewpoint of imparting water-repellent, oil-repellent, slippery, and fingerprint-resistant properties to the cured surface, a perfluoropolyether containing silicon atoms and (meth)acryloyl groups is preferred. Examples of commercially available perfluoropolyethers containing silicon atoms and (meth)acryloyl groups include KY-1203.

[0086] Examples of upper and lower limits for the content of (meth)acryloyl group-containing perfluoropolyether in 100% by mass of the coating agent solids include 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, and 0% by mass. In one embodiment, the above content is preferably 0 to 10% by mass.

[0087] <Photopolymerization initiator> In one embodiment, the coating agent may include a photopolymerization initiator. The photopolymerization initiator may be used alone or in combination of two or more.

[0088] Examples of photopolymerization initiators include radical-based photopolymerization initiators, cationic-based photopolymerization initiators, and anionic-based photopolymerization initiators.

[0089] Examples of radical-type photopolymerization initiators include alkylphenone-type photopolymerization initiators, acylphosphine oxide-type photopolymerization initiators, hydrogen abstraction-type photopolymerization initiators, and oxime ester-type photopolymerization initiators.

[0090] Examples of alkylphenone-type photopolymerization initiators include benzyldimethyl ketals such as 2,2-dimethoxy-1,2-diphenylethane-1-one, α-hydroxyalkylphenones such as 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, and α-aminoalkylphenones such as 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one.

[0091] Examples of acylphosphine oxide type photopolymerization initiators include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.

[0092] Examples of hydrogen abstraction type photopolymerization initiators include phenylglyoxylic acid methyl esters.

[0093] Examples of oxime ester type photopolymerization initiators include 1,2-octanedione, 1-[4-(phenylthio)-,2-(O-benzoyl oxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-,1-(O-acetyl oxime), etc.

[0094] Examples of cationic photopolymerization initiators include a mixture of iodonium,(4-methylphenyl)]4-(2-methylpropyl)phenyl]-hexafluorophosphate (1-) and propylene carbonate, triarylsulfonium hexafluorophosphate, and triarylsulfonium tetrakis-(pentafluorophenyl)borate.

[0095] Examples of anionic photopolymerization initiators include cobaltamine complexes, o-nitrobenzyl alcohol carbamate esters, and oxime esters.

[0096] Examples of upper and lower limits for the content of the photopolymerization initiator in 100% by mass of the coating agent solids include 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, and 0% by mass. In one embodiment, the above content is preferably 0 to 10% by mass.

[0097] <organic solvents> In one embodiment, the coating agent may include an organic solvent. The organic solvent may be used alone or in combination of two or more.

[0098] Examples of organic solvents include ketone solvents, aromatic solvents, alcohol solvents, glycol solvents, glycol ether solvents, ester solvents, petroleum-based solvents, haloalkane solvents, and amide solvents.

[0099] Examples of ketone solvents include methyl ethyl ketone, acetylacetone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone.

[0100] Examples of aromatic solvents include toluene and xylene.

[0101] Examples of alcoholic solvents include methanol, ethanol, n-propanol, isopropanol, and butanol.

[0102] Examples of glycol solvents include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, polyethylene glycol, and polypropylene glycol.

[0103] Examples of glycol ether solvents include ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol monoisobutyl ether, and ethylene glycol mono-t-butyl ether.

[0104] Examples of ester solvents include ethyl acetate, butyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, and propylene glycol monomethyl ether acetate.

[0105] Examples of petroleum-based solvents include Solvesso #100 (manufactured by Exxon Technologies) and Solvesso #150 (manufactured by Exxon Technologies).

[0106] Examples of haloalkane solvents include chloroform.

[0107] Examples of amide solvents include dimethylformamide.

[0108] Examples of upper and lower limits for the organic solvent content in 100% by mass of the coating agent include 99, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 2, 1, and 0% by mass. In one embodiment, the above content is preferably 0 to 99% by mass.

[0109] Examples of upper and lower limits for the mass ratio (mass of acidic group-containing poly(meth)acrylate / mass of hollow inorganic particles) in the coating agent include 3.5, 3.3, 3, 2.7, 2.5, 2.3, 2, 1.7, 1.5, 1.3, 1, 0.7, 0.5, 0.3, etc. In one embodiment, the above mass ratio is preferably between 0.3 and 3.5.

[0110] Examples of upper and lower limits for the mass ratio (mass of acidic group-containing poly(meth)acrylate / mass of solid alumina particles) in the coating agent include 11.7, 11.5, 11.3, 11, 10.7, 10.5, 10.3, 10, 9.7, 9.5, 9.3, 9, 8.7, 8.5, 8.3, 8, 7.7, 7.5, 7.3, 7, 6.7, 6.5, 6.3, 6, 5.7, 5.5, 5.3, 5, 4.7, 4.5, 4, 3.7, 3.5, 3.3, 3, 2.7, 2.5, 2.3, 2, 1.7, 1.5, 1.3, etc. In one embodiment, the above mass ratio is preferably between 1.3 and 11.7.

[0111] Examples of upper and lower limits for the mass ratio (mass of hollow inorganic particles / mass of solid alumina particles) of hollow inorganic particles to solid alumina particles in the coating agent include 10.8, 10.5, 10.3, 10, 9.7, 9.5, 9.3, 9, 8.7, 8.5, 8.3, 8, 7.7, 7.5, 7.3, 7, 6.7, 6.5, 6.3, 6, 5.7, 5.5, 5.3, 5, 4.7, 4.5, 4, 3.7, 3.5, 3.3, 3, 2.7, 2.5, 2.3, 2, 1.7, 1.5, 1.3, etc. In one embodiment, the above mass ratio is preferably between 1.3 and 10.8.

[0112] <Additives> The above coating agent may contain as an additive any agent that does not fall under any of the following categories: acidic group-containing poly(meth)acrylate, hollow inorganic particles, solid alumina particles, (meth)acryloyl group-containing perfluoropolyether, photopolymerization initiator, or organic solvent.

[0113] Examples of additives include binder resins (acrylic resins, urethane resins, polyester resins, epoxy resins, alkyd resins, etc.), anti-slip agents, slip agents, preservatives, rust inhibitors, pH adjusters, pigments, dyes, lubricants, leveling agents, catalysts, defoamers, and photosensitizers (amines, quinones, etc.).

[0114] In one embodiment, examples of additive content include less than 1 part by mass, less than 0.1 parts by mass, less than 0.01 parts by mass, and 0 parts by mass, per 100 parts by mass of coating agent. Also, examples of additive content include less than 1 part by mass, less than 0.1 parts by mass, less than 0.01 parts by mass, and 0 parts by mass, per 100 parts by mass of any of the following: acidic group-containing poly(meth)acrylate, hollow inorganic particles, solid alumina particles, (meth)acryloyl group-containing perfluoropolyether, photopolymerization initiator, and organic solvent.

[0115] The above coating agent can be produced by dispersing and mixing acidic group-containing poly(meth)acrylate, hollow inorganic particles, and solid alumina particles, as well as (meth)acryloyl group-containing perfluoropolyether, a photopolymerization initiator, an organic solvent, and additives, using various known methods. The order of addition of each component is not particularly limited. Various known devices (emulsifiers, ultrasonic dispersers, etc.) can be used for dispersion and mixing.

[0116] [Coating Kit] This disclosure provides a low-reflection coating agent containing 2 to 15% by mass of solid alumina particles in its solid content, and a coating agent kit containing an anchoring agent containing solid alumina particles.

[0117] Examples of the components and quantities included in the low-reflection coating agent in the coating agent kit are those mentioned above.

[0118] Furthermore, after manufacturing the coating agent kit, the laminate can be produced using the kit within a time frame that does not pose a stability issue. In this case, the desired laminate can be obtained even if the coating agent kit does not contain acidic group-containing poly(meth)acrylate. In addition, low reflectivity can be achieved by using fluororesins or the like, even without using hollow inorganic particles.

[0119] <Anchoring agent> Examples of solid alumina particles included in the anchoring agent include those mentioned above. Solid alumina particles can be used alone or in combination of two or more types.

[0120] Examples of upper and lower limits for the content of solid alumina particles in 100% by mass of anchoring agent solids include 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, and 2% by mass. In one embodiment, the above content is preferably 2 to 18% by mass.

[0121] • Poly(meth)acrylate In one embodiment, the anchoring agent may include poly(meth)acrylate. Poly(meth)acrylate may be used alone or in combination of two or more types.

[0122] Examples of poly(meth)acrylates include acidic group-containing poly(meth)acrylates and urethane poly(meth)acrylates.

[0123] Examples of acidic group-containing poly(meth)acrylates include those mentioned above.

[0124] Examples of urethane poly(meth)acrylates include reaction products of compounds containing hydroxyl group-containing poly(meth)acrylates and polyisocyanates.

[0125] Examples of hydroxyl group-containing poly(meth)acrylates used as raw materials for urethane poly(meth)acrylate include those mentioned above.

[0126] In this disclosure, "polyisocyanate" means a compound having two or more isocyanate groups (-N=C=O).

[0127] Examples of polyisocyanates include linear aliphatic polyisocyanates, branched aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, and their biuret, isocyanurate (nurate), allophanate, and adduct derivatives.

[0128] Examples of linear aliphatic polyisocyanates include methylene diisocyanate, dimethyl diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, heptamethylene diisocyanate, octamethylene diisocyanate, nonamethylene diisocyanate, and decamethylene diisocyanate.

[0129] Examples of branched aliphatic polyisocyanates include diethylpentylene diisocyanate, trimethylbutylene diisocyanate, trimethylpentylene diisocyanate, and trimethylhexamethylene diisocyanate.

[0130] Examples of alicyclic polyisocyanates include monocyclic alicyclic polyisocyanates, crosslinked cyclic alicyclic polyisocyanates, and condensed cyclic alicyclic polyisocyanates.

[0131] Examples of monocyclic alicyclic polyisocyanates include hydrogenated xylene diisocyanate, isophorone diisocyanate, cyclopentylene diisocyanate, cyclohexylene diisocyanate, cycloheptylene diisocyanate, cyclodecylene diisocyanate, 3,5,5-trimethylcyclohexylene diisocyanate, and dicyclohexylmethane diisocyanate.

[0132] Examples of cross-linked alicyclic polyisocyanates include tricyclodecile diisocyanate, adamantane diisocyanate, and norbornene diisocyanate.

[0133] Examples of condensed alicyclic polyisocyanates include bicyclodecile diisocyanate.

[0134] Examples of aromatic groups include monocyclic aromatic groups and fused ring aromatic groups. Furthermore, one or more hydrogen atoms in an aromatic group may be substituted by a linear or branched alkyl group.

[0135] Examples of monocyclic aromatic groups include phenyl groups (phenylene groups), tolyl groups (trylene groups), and mesityl groups (mesitylene groups). Examples of fused ring aromatic groups include naphthyl groups (naphthylene groups).

[0136] Examples of aromatic polyisocyanates include monocyclic aromatic polyisocyanates and fused-ring aromatic polyisocyanates.

[0137] Examples of monocyclic aromatic polyisocyanates include dialkyldiphenylmethane diisocyanates such as 4,4'-diphenyldimethylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanates such as 4,4'-diphenyltetramethylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-dibenzyli isocyanate, 1,3-phenylenedi isocyanate, 1,4-phenylenedi isocyanate, tolylene diisocyanate, xylylene diisocyanate, and m-tetramethylxylylene diisocyanate.

[0138] Examples of condensed ring aromatic polyisocyanates include 1,5-naphthylene diisocyanate.

[0139] The biuret form of polyisocyanates is The following structural formula: [ka] [where n b is an integer greater than or equal to 1, and R bA ~R bE Each of these is independently an alkylene group or an arylene group, and R bα ~R bβ Each of these independently comprises an isocyanate group or [ka] (n b1 is a non-negative integer, and R b1 ~R b5 Each of these is independently an alkylene group or an arylene group, and R b '~R b Each of the '' represents an isocyanate group or R bα ~R bβ It is the foundation of itself. R b4 ~R b5 , R b '' may have different bases for each constituent unit. ) bD ~R bE , R bβThe group may differ for each constituent unit. Examples include compounds represented by [ ].

[0140] Examples of polyisocyanate biuret compounds include Duranate 24A-100, Duranate 22A-75P, Duranate 21S-75E (all manufactured by Asahi Kasei Corporation), and Desmodule N3200A (hexamethylene diisocyanate biuret compound) (both manufactured by Sumika Covestro Urethane Co., Ltd.).

[0141] The isocyanurate derivatives of polyisocyanates are The following structural formula: [ka] [where n i is a non-negative integer, and R iA ~R iE Each of these is independently an alkylene group or an arylene group, and R iα ~R iβ Each of these independently comprises an isocyanate group or [ka] (n i1 is a non-negative integer, and R i1 ~R i5 Each of these is independently an alkylene group or an arylene group, and R i '~R i Each of the '' independently represents an isocyanate group or R iα ~R iβ It is the foundation of itself. R i5 , R i '' may have different bases for each constituent unit. ) iD ~R iE , R iβ The group may differ for each constituent unit. Examples include compounds represented by [ ].

[0142] Commercially available isocyanurate forms of polyisocyanates include Duranate TPA-100, Duranate TKA-100, Duranate MFA-75B, Duranate MHG-80B (manufactured by Asahi Kasei Corporation), Coronate HXR, Coronate HX, Coronate HK (isocyanurate form of hexamethylene diisocyanate), Coronate 2037 (manufactured by Tosoh Corporation), Takenate D-127N (isocyanurate form of hydrogenated xylylene diisocyanate), Takenate D-131N (isocyanurate form of xylylene diisocyanate), Takenate D-204EA-1 (isocyanurate form of tolylene diisocyanate) (manufactured by Mitsui Chemicals, Inc.), VESTANAT T1890 / 100 (isocyanurate form of isophorone diisocyanate) (manufactured by Evonik Japan Co., Ltd.), etc.

[0143] The allophanate form of polyisocyanate is represented by the following structural formula:

Chemical formula

Chemical formula

[0144] Examples of commercially available polyisocyanate allophanates include Coronate 2793 (manufactured by Tosoh Corporation) and Takenate D-178N (manufactured by Mitsui Chemicals, Inc.).

[0145] Polyisocyanate adducts are The following structural formula: [ka] [where n ad is a non-negative integer, and R adA ~R adE Each is independently an alkylene group or an arylene group, and R ad1 ~R ad2 Each is independent [ka] (In the formula, n ad’ is a non-negative integer, R ad’ ~R ad’’ These are, independently, either an alkylene group or an arylene group. R ad’’’ R ad1 ~R ad2 It is the foundation of himself, R ad’ ~R ad’’’ (The base may differ for each constituent unit.) And R adD ~R adE , R ad2 The base may differ for each constituent unit. The adduct compounds of trimethylolpropane and polyisocyanate shown, The following structural formula [ka] [where n ad1 is a non-negative integer, R adα ~R adεThese are, independently, either an alkylene group or an arylene group. R adA ~R adB Each is independent [ka] (In the formula, n ad1’ is a non-negative integer, R adδ’ ~R adε’ These are, independently, either an alkylene group or an arylene group. R adB’ R adA ~R adB It is the foundation of himself, R adδ’ ~R adε’ , R adB’ The base may differ for each constituent unit. R adδ ~R adε The base may differ for each constituent unit. Examples include glycerin and polyisocyanate adducts shown.

[0146] Examples of polyisocyanate adducts include Duranate P301-75E (manufactured by Asahi Kasei Corporation), Takenate D110N, Takenate D160N (manufactured by Mitsui Chemicals, Inc.), Coronate L, Coronate HL (manufactured by Tosoh Corporation), and others.

[0147] Examples of upper and lower limits for the NCO content (NCO%) of polyisocyanate include 30%, 25%, 20%, 15%, and 10%. In one embodiment, the above NCO content (NCO%) is preferably 10 to 30%.

[0148] Examples of upper and lower limits for the isocyanate group equivalents of polyisocyanates include 10, 9, 8, 7, 6, 5, 4, 3, 2, and 1 meq / g. In one embodiment, the above isocyanate group equivalent is preferably 1 to 10 meq / g.

[0149] In this disclosure, isocyanate group equivalent refers to the amount of substance of isocyanate groups present in 1 g of solid.

[0150] The group of compounds used as raw materials for urethane poly(meth)acrylate may include alkylene polyols, polyether polyols, polyester polyols, polycarbonate polyols, acrylic polyols, polyolefin polyols, and the like.

[0151] Alkylene polyol Examples of alkylene polyols include linear alkylene polyols and branched alkylene polyols.

[0152] Examples of linear alkylene polyols include ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, and decanediol.

[0153] Examples of branched alkylene polyols include neopentyl glycol, 2,4-diethyl-1,5-pentanediol, 2,4-dibutyl-1,5-pentanediol, 1-methylethylene glycol, 1-ethylethylene glycol, trimethylolpropane, and pentaerythritol.

[0154] Examples of cycloalkylene polyols include monocyclic cycloalkylene polyols and crosslinked ring cycloalkylene polyols.

[0155] Examples of monocyclic cycloalkylene polyols include 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and 2,2'-bis(4-hydroxycyclohexyl)propane.

[0156] Examples of crosslinked ring cycloalkylene polyols include tricyclodecanedimethanol.

[0157] Polyether polyol In this disclosure, "polyether polyol" means a compound having two or more hydroxyl groups and two or more repeating units containing ether bonds. Two or more polyether polyols may be used in combination. In one embodiment, the polyether polyol has the following structural formula HO-(R 3’ -O-) n H (In the formula, R 3’ ) is an alkylene group or a cycloalkylene group, and n is an integer greater than or equal to 2.

[0158] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0159] Polyester polyol In this disclosure, "polyester polyol" means a compound having two or more hydroxyl groups and two or more repeating units containing ester bonds within the molecule. Two or more types of polyester polyols may be used in combination. In one embodiment, the polyester polyol has the following structural formula HO-{R 4a’ -OC(O)-R 4b’ -C(O)O} m -R 4a’ -OH (In the formula, R 4a’ and R 4b’ Each of these is independently an alkylene group or a cycloalkylene group, and m is an integer greater than or equal to 2. ) This is represented as .

[0160] In this disclosure, "polyester polyol" is a reaction product of a polycarboxylic acid or its anhydride with a polyol.

[0161] Examples of polycarboxylic acids include dicarboxylic acids.

[0162] Examples of dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanediic acid, 2-methylsuccinic acid, 2-methyladipic acid, 3-methyladipic acid, 3-methylpentanedioic acid, 2-methyloctanedioic acid, 3,8-dimethyldecanediic acid, 3,7-dimethyldecanediic acid, phthalic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, trimellitic acid, trimesic acid, cyclohexanedicarboxylic acid, and other dicarboxylic acids.

[0163] Examples of polycarboxylic acid anhydrides include acetic anhydride, propionic anhydride, succinic anhydride, maleic anhydride, phthalic anhydride, and trimellitic anhydride.

[0164] Examples of polyols include the alkylene polyols and cycloalkylene polyols mentioned above.

[0165] Polycarbonate polyol In this disclosure, "polycarbonate polyol" means, for example, a compound having two or more hydroxyl groups and two or more repeating units containing carbonate bonds. Polycarbonate polyols may be used alone or in combination of two or more types.

[0166] In one embodiment, the polycarbonate polyol has the following structural formula HO-{R aCarbo -OC(=O)O} p -R bCarbo -OH (In the formula, R aCarbo , and R bCarbo Each of these is independently an alkylene group or a cycloalkylene group, and p is an integer greater than or equal to 2. ) This is represented as .

[0167] Examples of polycarbonate polyols include reaction products of polyols and phosgene, and ring-opening polymers of cyclic carbonate esters (such as alkylene carbonates).

[0168] Examples of polyols include the alkylene polyols mentioned above.

[0169] Examples of alkylene carbonates include ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, and hexamethylene carbonate.

[0170] Acrylic polyol Acrylic polyols are polymers of monomers containing hydroxyl group monomers. The above monomer group may also contain hydroxyl group-free monomers.

[0171] Polyolefin polyol Polyolefin polyols are polyolefins having two or more hydroxyl groups. Examples of polyolefin polyols include polybutadiene polyols, hydrogenated polybutadiene polyols, polyisoprene polyols, hydrogenated polyisoprene polyols, and their chlorinated derivatives.

[0172] Examples of the upper and lower limits of the number of (meth)acryloyl groups in the poly(meth)acrylate contained in the anchoring agent include 15, 14, 12, 13, 11, 10, 9, 8, 7, 6, 5, 4, 3, and 2. In one embodiment, the above number is preferably 2 to 15, and more preferably 3 to 15.

[0173] Examples of the upper and lower limits for the poly(meth)acrylate content in 100% by mass of the anchoring agent solids include 94, 90, 88, 85, 80, 75, 70, 66, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 1, and 0% by mass. In one embodiment, the above content is preferably 0 to 94% by mass.

[0174] • Photopolymerization initiator In one embodiment, the anchoring agent may include a photopolymerization initiator. The photopolymerization initiator may be used alone or in combination of two or more.

[0175] Examples of photopolymerization initiators include those mentioned above.

[0176] Examples of upper and lower limits for the content of the photopolymerization initiator in 100% by mass of the anchoring agent solids include 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, and 0% by mass. In one embodiment, the above content is preferably 0 to 10% by mass.

[0177] Examples of upper and lower limits for the mass ratio (mass of poly(meth)acrylate / mass of solid alumina particles) in the anchoring agent include 47, 45, 43, 41, 40, 39, 37, 35, 33, 31, 30, 29, 27, 25, 23, 21, 20, 19, 17, 15, 13, 11, 10, 9, 8, 7, 5, 4, 3, 2, 1, 0.5, 0.2, 0.1, 0, etc. In one embodiment, the above mass ratio is preferably between 0 and 47.

[0178] Examples of upper and lower limits for the mass ratio (mass of photopolymerization initiator / mass of solid alumina particles) of the anchoring agent include 5, 4.5, 4, 3.5, 3, 2.5, 2, 1.5, 1, 0.9, 0.7, 0.5, 0.4, 0.3, 0.2, 0.1, and 0. In one embodiment, the above mass ratio is preferably between 0 and 5.

[0179] • Organic solvents In one embodiment, the anchoring agent may include an organic solvent. The organic solvent may be used alone or in combination of two or more.

[0180] Examples of organic solvents include those mentioned above.

[0181] Examples of upper and lower limits for the content of organic solvents in 100% by mass of anchoring agent solids include 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 2, 1, and 0% by mass. In one embodiment, the above content is preferably 0 to 80% by mass.

[0182] • Additives for anchoring agents The above-mentioned anchor agent may contain, as an additive for the anchor agent, an agent that does not fall under any of solid alumina particles, poly(meth)acrylate, a photopolymerization initiator, and an organic solvent.

[0183] Examples of the additive for the anchor agent include those described above.

[0184] In one embodiment, examples of the content of the additive for the anchor agent include less than 1 part by mass, less than 0.1 part by mass, less than 0.01 part by mass, 0 part by mass, etc., based on 100 parts by mass of the anchor agent. Also, examples of the content of the additive for the anchor agent include less than 1 part by mass, less than 0.1 part by mass, less than 0.01 part by mass, 0 part by mass, etc., based on 100 parts by mass of any one of the solid alumina particles, poly(meth)acrylate, photopolymerization initiator, and organic solvent in the anchor agent.

[0185] The above-mentioned anchor agent can be produced by dispersing and mixing solid alumina particles and, if necessary, poly(meth)acrylate, a photopolymerization initiator, an organic solvent, and an anchor agent additive by various known means. The order of addition of each component is not particularly limited. Also, various known apparatuses (such as an emulsifying disperser, an ultrasonic dispersing apparatus, etc.) can be used as the dispersing and mixing means.

[0186] [Cured product] The present disclosure provides a cured product of the above-mentioned low-reflection coating agent and / or the above-mentioned coating agent kit.

[0187] Examples of the curing conditions include those described later.

[0188] [Laminate] The present disclosure provides a laminate including the above-mentioned cured product.

[0189] In one embodiment, a cured layer made of the low-reflection coating agent or the cured product of the coating agent kit is laminated on at least one side of the substrate. In another embodiment, an anchor agent cured product layer made of the cured product of the anchor agent is laminated on at least one side of the substrate, and a low-reflection coating agent cured product layer made of the cured product of the low-reflection coating agent is laminated on the anchor agent cured product layer.

[0190] Examples of upper and lower limits for the substrate thickness include 125, 120, 110, 100, 90, 75, 50, 25, 10, 9, 5, and 1 μm. In one embodiment, the substrate thickness is preferably 1 to 125 μm.

[0191] Examples of upper and lower limits for the thickness of the cured low-reflection coating layer include 200, 175, 150, 125, 100, 90, 75, 60, and 55 nm. In one embodiment, the thickness of the cured low-reflection coating layer is preferably 55 to 200 nm.

[0192] Examples of upper and lower limits for the thickness of the cured anchoring agent layer include 6, 5, 4, 3, 2, and 1 μm. In one embodiment, the thickness of the cured anchoring agent layer is preferably 1 to 6 μm.

[0193] The above-mentioned laminates are manufactured by various known methods. In one embodiment, the method for manufacturing the laminate includes the steps of: coating an anchoring agent on at least one side of a substrate (anchoring agent coating step); coating a low-reflection coating agent on top of the anchoring agent coating layer (low-reflection coating agent coating step); and forming a cured layer by irradiating with active energy rays (active energy ray curing step).

[0194] The anchoring agent coating process and the low-reflection coating agent coating process are collectively referred to as the coating process.

[0195] (Coating process) Coating methods include bar coating, wire bar coating, Meyer bar coating, air knife coating, gravure coating, reverse gravure coating, flow coating, offset printing, flexographic printing, and screen printing.

[0196] The amount of coating is not particularly limited. The amount of coating is such that the mass after drying is 0.1 to 30 g / m². 2 It is preferable.

[0197] (Activated energy ray curing process) Examples of active energy rays used in active energy ray curing reactions include ultraviolet rays and electron beams. Examples of ultraviolet light sources include xenon lamps, high-pressure mercury lamps, and ultraviolet irradiation devices with metal halide lamps. The light intensity, light source arrangement, and transport speed can be adjusted as needed. When using a high-pressure mercury lamp, it is preferable to cure with a transport speed of about 2 to 50 m / min using one lamp with a light intensity of about 80 to 160 W / cm. On the other hand, in the case of electron beams, it is preferable to cure with a transport speed of about 5 to 50 m / min using an electron beam accelerator with an acceleration voltage of about 10 to 300 kV. [Examples]

[0198] The present invention will be specifically described below through examples and comparative examples. However, the description of preferred embodiments above and the following examples are provided for illustrative purposes only and are not intended to limit the present invention. Accordingly, the scope of the present invention is not limited to the embodiments or examples specifically described herein, but is limited only by the claims. In addition, in each example and comparative example, unless otherwise specified, numerical values ​​such as parts and percentages are on a mass basis.

[0199] (Example 1-1: Manufacturing of a low-reflection coating agent) As an acidic group-containing poly(meth)acrylate, 40 parts by mass of carboxyl group-containing poly(meth)acrylate (product name: "Aronix M-510", manufactured by Toagosei Co., Ltd.), as hollow inorganic particles, 42 parts by mass of hollow silica particles (product name: "Thruia 4320", 20 mass% methyl isobutyl ketone sol, manufactured by JGC Catalysts and Chemicals Ltd.), 10 parts by mass of solid alumina particles (product name: "NANOBYK-3610", 30 mass% methoxypropyl acetate, manufactured by BYK Chemie), 4 parts by mass of (meth)acryloyl group-containing perfluoropolyether (product name: "KY-1203", manufactured by Shin-Etsu Chemical Co., Ltd., 20 mass%), and 4 parts by mass of 2-hydroxy-1-{4-[{4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one (product name: "Omnirad 127D", manufactured by IGM Resins) as a photoinitiator were mixed, and then diluted with methyl isobutyl ketone to produce a low-reflection coating agent with a solid content of 2 mass%.

[0200] Unless otherwise specified, Example 1 and Comparative Example 1 other than Example 1-1 were carried out in the same manner as Example 1-1, except that they were changed as shown in the following table.

[0201] (Stability Test of Low-Reflection Coating Agent) The above low-reflection coating agent was placed in a 20 mL screw tube and stored for 1 month at room temperature of 50 °C in a light-shielded environment, and then the state of the contents of the screw tube was evaluated. The evaluation criteria are as follows. 〇: All are liquid, and there is no gel-like part. ×: Part or all has changed to a gel state. As described above, when hollow particles and solid alumina particles are present in one system, stability becomes a problem. This can be understood from the fact that the stability of the comparative example in which hollow particles and solid alumina particles are not present in one system is not poor.

[0202]

Table 1

[0203] <Explanation of abbreviations> Aronix M-306: Pentaerythritol triacrylate, manufactured by Toagosei Co., Ltd. NK Ester A-TMMT: Pentaerythritol tetraacrylate, manufactured by Shin-Nakamura Chemical Industry Co., Ltd. NK Ester A-DPH: Dipentaerythritol hexaacrylate, manufactured by Shin-Nakamura Chemical Industry Co., Ltd. ELCOM V8802: Solid silica particles, 40% by mass methyl isobutyl ketone sol, manufactured by JGC Catalysts & Chemicals Co., Ltd.

[0204] (Manufacturing Example 1: Manufacturing of anchoring agents) A 40% solids anchor was prepared by mixing 66 parts by mass of aliphatic urethane acrylate (product name "Beamset 577", manufactured by Arakawa Chemical Industries, Ltd.), 22 parts by mass of dipentaerythritol polyacrylate (product name "NK Ester A-9550W", manufactured by Shin Nakamura Chemical Industry Co., Ltd.), 9 parts by mass of (product name "NANOBYK-3610", 30% by mass methoxypropyl acetate, manufactured by BYK Chemie), and 3 parts by mass of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxymethylpropanone (product name "Omnirad 2959", manufactured by IGM Resins), and diluting with methyl isobutyl ketone.

[0205] Unless otherwise specified, the manufacturing examples other than Manufacturing Example 1 and the comparative manufacturing examples were carried out in the same manner as Manufacturing Example 1, except for the modifications shown in the table below.

[0206] [Table 2]

[0207] (Example 2-1: Manufacturing of Laminates) The anchoring agent manufactured as described above was applied to a polyester (PET) film (product name "Lumirror 50U483", manufactured by Toray Industries, Inc.) using a bar coater to achieve a film thickness of 4 μm after drying. After drying at 80°C for 1 minute, it was subjected to high-pressure mercury lamp (200 mJ / cm²). 2The anchor film was cured using a bar coater. The low-reflection coating agent prepared above was applied to the anchor agent coated surface of this anchor film using a bar coater so that the film thickness after drying was 100 nm, dried at 80°C for 1 minute, and then cured under nitrogen flow with a high-pressure mercury lamp (600 mJ / cm²). 2 The laminate was obtained by curing it using ).

[0208] Unless otherwise specified, Examples 2-1, Example 2, and Comparative Example 2 were carried out in the same manner as Example 2-1, except that the composition of the coating agent kit was changed as shown in the table below.

[0209] The properties of the obtained laminate were evaluated for the following items. The results are shown in the table below.

[0210] (Total light transmittance and haze) In accordance with the JIS K 7361-1 (1997) standard, the total light transmittance and haze of the laminate were measured using a haze meter (product name "HZ-V3", manufactured by Suga Test Instruments Co., Ltd.).

[0211] (Initial water contact angle) The laminates were fixed to a glass plate with the low-reflection coating surface facing upwards. After static electricity was removed, a 2 μL droplet of deionized water was gently applied using a DropMaster DM500 contact angle meter manufactured by Kyowa Interface Science Co., Ltd., and the contact angle after 1 second was measured (analysis method: θ / 2 method).

[0212] (Water contact angle after steel wool test) The laminate was placed in a steel wool testing machine with the low-reflection coating surface facing upwards, and 1 kg / 4 cm of #0000 steel wool was used. 2 A steel wool test was conducted by rubbing the test area 500 times back and forth over a sliding distance of 4 cm under a load. After the steel wool test, the water contact angle was measured at the test site using the same method as for the initial water contact angle.

[0213] (Steel wool resistant) The laminate was placed in a steel wool testing machine with the low-reflection coating surface facing upwards, and 1 kg / 4 cm of #0000 steel wool was used. 2 A steel wool test was conducted by rubbing the material with a load over a sliding distance of 4 cm for the following number of reciprocating motions. After the test, the number of scratches that occurred on the laminate was visually inspected and evaluated according to the following criteria. ○: Fewer than 5 injuries after 1000 round trips. ×: More than 6 scratches after 1000 round trips

[0214] [Table 3]

Claims

1. A coating agent kit comprising a low-reflection coating agent containing 2 to 15 mass % of solid alumina particles in the solid content, and an anchor agent containing solid alumina particles.

2. The low-reflection coating agent comprises one or more selected from the group consisting of hydroxyl group-containing poly(meth)acrylates and carboxyl group-containing poly(meth)acrylates; 2. The low-reflection coating kit according to claim 1, wherein the hydroxyl value of the hydroxyl-containing poly(meth)acrylate is 100 to 280 mgKOH / g.

3. A cured product of the low-reflective coating agent kit according to claim 1 or 2.

4. A laminate comprising the cured product according to claim 3.