Repair method

JP2023093116A5Inactive Publication Date: 2024-11-01F CONSULTANT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021208542
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing decorative surfaces containing aggregates deteriorate over time, leading to uneven color tone and luster, and existing refurbishing methods fail to provide a new design property or adequately address uneven absorption issues.

Method used

A method involving the application of a coating material with a thixotropic index value of 1.5 or more, containing a synthetic resin and bright pigment, to form a design layer that suppresses unevenness and imparts a new glittering design.

Benefits of technology

The method effectively suppresses unevenness and enhances the aesthetic appeal of decorative surfaces by forming a uniform, glittering design while maintaining the original color and texture of the aggregates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023093116000001
    Figure 2023093116000001
Patent Text Reader

Abstract

To provide a repair method having beauty appearance on an aggregate-containing decorative surface.SOLUTION: A repair method of an aggregate-containing decorative surface includes a step of coating a covering material which contains a synthetic resin and a brilliant pigment and has a thixotropic index value (TI value) of 1.5 or more onto an aggregate-containing decorative surface, and forming a design layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for renovating an aggregate-containing decorative surface. [Background technology]

[0002] Traditionally, decorative layers with various patterns have been applied to the wall surfaces of buildings, civil engineering structures, and the like. Examples of such decorative layers include decorative surfaces such as coatings and sheets containing aggregate, with a wide variety of patterns (designs) including stone, earthen wall, and wood grain. These decorative surfaces contain synthetic resins and aggregates, and as they deteriorate over time, uneven color and gloss can occur, impairing their aesthetic appearance and necessitating repairs. Furthermore, in recent years, there has been an increase in requests for large-scale remodeling and renovation, which often requires new design finishes that change the appearance of the decorative surfaces.

[0003] As a method for repairing such decorative surfaces, for example, Patent Document 1 describes a repair method in which a matte water-based paint is applied to an uneven coating film base containing aggregate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 2019-104856 Summary of the Invention [Problem to be solved by the invention]

[0005] However, when a matte water-based paint is applied as in Patent Document 1, uneven absorption occurs on decorative surfaces containing aggregate, which may impair aesthetics. Furthermore, Patent Document 1 only provides a single-color finish and does not impart new design features. [Means for solving the problem]

[0006] The present invention has been made in consideration of the above problems, and has as its object to provide a repair method that provides a highly aesthetic appearance to aggregate-containing decorative surfaces.

[0007] That is, the present invention has the following features.

[0008] 1. A method for renovating an aggregate-containing decorative surface, comprising: a step of applying a coating material containing a synthetic resin and a photoluminescent pigment and having a thixotropic index (TI value) of 1.5 or more to form a design layer; A renovation method comprising: [Effects of the Invention]

[0009] According to the present invention, it is possible to suppress unevenness in an aggregate-containing decorative surface and form a decorative surface with excellent aesthetics. In particular, it is possible to impart a new design with brilliance, and it is possible to form a decorative surface with excellent aesthetics while suppressing unevenness in brilliance. DETAILED DESCRIPTION OF THE INVENTION

[0010] Hereinafter, an embodiment of the present invention will be described.

[0011] The present invention is a method for repairing an aggregate-containing decorative surface, which includes a step of forming a design layer having a lustrous appearance. The present invention is a repair method suitable for cases where the aggregate-containing decorative surface has deteriorated over time or has suffered some kind of damage.

[0012] <Aggregate-containing decorative surface> Examples of aggregate-containing decorative surfaces (hereinafter also referred to as "decorative surfaces" or "renovated surfaces") that are the target of the renovation method of the present invention include decorative surfaces obtained by applying a composition containing synthetic resin and aggregate (paint, coating material, finishing material), or decorative surfaces to which a building material formed from a composition containing synthetic resin and aggregate in the form of a sheet or plate has been attached. Furthermore, the surface may have some kind of protective layer.

[0013] The synthetic resin that constitutes the aggregate-containing decorative surface is not particularly limited, and any commonly available resin can be used. Examples of the resin form include solvent-soluble resins, non-aqueous dispersion resins, solventless resins, aqueous dispersion resins, and water-soluble resins. Examples of resin types include ethylene resins, vinyl acetate resins, polyester resins, alkyd resins, vinyl chloride resins, epoxy resins, acrylic resins, urethane resins, phenolic resins, melamine resins, amino resins, polycarbonate resins, acrylic silicone resins, acrylic vinyl acetate resins, acrylic urethane resins, silicone resins, and fluororesins. One or more of these resins can be used.

[0014] The aggregate is recognized as granular, and at least one selected from natural aggregates such as natural stone and crushed natural stone, and artificial aggregates such as colored aggregates can be suitably used. Specific examples include marble, granite, serpentine, granite, fluorite, kansui stone, feldspar, silica stone, silica sand, and crushed products thereof, crushed porcelain, crushed ceramic, crushed glass, glass beads, crushed resin, resin beads, metal particles, and those with colored coatings on their surfaces. These can be used alone or in combination of two or more.

[0015] The particle size of the aggregate is set depending on the pattern of the decorative surface, etc., and is preferably less than 5.6 mm (more preferably more than 20 μm and less than 4.75 mm, even more preferably more than 25 μm and less than 2 mm, and even more preferably more than 38 μm and less than 850 μm). The particle size of the aggregate is measured by sieving using a metal mesh sieve specified in JIS Z8801-1:2019.

[0016] The mixing ratio of the resin to the aggregate is preferably 1 to 50 parts by weight (more preferably 2 to 30 parts by weight, and even more preferably 3 to 25 parts by weight) of resin per 100 parts by weight of the total amount of aggregate, calculated as solid content. With such a ratio, an aggregated pattern (for example, a stone-like pattern) having fine irregularities derived from the aggregate can be obtained.

[0017] The aggregate-containing decorative surface may also contain other components (additives) as needed, as long as they do not significantly impair the effects of the present invention. Examples of such components include plasticizers, anti-algae agents, antibacterial agents, deodorizers, adsorbents, flame retardants, thickeners, antifoaming agents, crosslinking agents, coloring pigments, extender pigments, lustrous pigments, phosphorescent pigments, fluorescent pigments, fibers, ultraviolet absorbers, light stabilizers, antioxidants, and catalysts.

[0018] Furthermore, the aggregate-containing decorative surface of the present invention may have a textured pattern such as a stone-like pattern, a wood-grain pattern, or a joint pattern on its surface. The repair method of the present invention can repair these textured patterns while preserving them. When the height difference of the textured pattern is preferably within the range of 0.2 to 6 mm or less (more preferably 0.3 to 5.5 mm or less), the effects of the present invention can be fully exhibited. In the present invention, "a to b" is synonymous with "a or more and b or less."

[0019] <Design layer> The coating material forming the design layer of the present invention is characterized by containing a synthetic resin and a glittering pigment. By forming such a design layer, it is possible to impart a new design with glitter while making use of the color of the aggregate-containing decorative surface.

[0020] As the synthetic resin, a resin having a transparent coating can be used. Examples of the form of such a resin include solvent-soluble resins, non-aqueous dispersion resins, solventless resins, aqueous dispersion resins, and water-soluble resins, among which aqueous dispersion resins (resin emulsions) are preferred. Examples of the resin include acrylic resins, urethane resins, epoxy resins, vinyl chloride resins, vinyl acetate resins, acrylic silicone resins, fluororesins, silicone resins, and the like, as well as composites thereof. These resins can be used alone or in combination of two or more. Such resins may have the property of undergoing a crosslinking reaction.

[0021] Known luster pigments can be used. Examples include metal flakes such as aluminum flakes and stainless steel flakes, and pearl pigments in which a thin substrate is coated with a metal oxide or a mixture thereof. These can be used alone or in combination of two or more. The particle size (size) of the above-mentioned luster pigment may be appropriately selected depending on the desired color tone and luster (brightness), and is preferably 1 to 800 μm (more preferably 5 to 700 μm). The thickness of the luster pigment is not particularly limited, but is preferably in the range of 0.1 μm to 10 μm. In such a case, excellent luster can be exhibited. The particle size of the above-mentioned luster pigment can be measured using a laser diffraction particle size distribution analyzer.

[0022] Furthermore, in the present invention, it is preferable to use a combination of brilliant pigments with different particle sizes. In the present invention, "different particle sizes" refers to different upper and / or lower particle size limits. Examples of design layers using a combination of brilliant pigments with different particle sizes include a design layer formed by sequentially applying a coating material containing a brilliant pigment with particle size A and a coating material containing a brilliant pigment with particle size B, or a design layer formed by applying a coating material containing brilliant pigments with particle size A and particle size B. In the latter case, a design with even greater brightness can be obtained.

[0023] In the present invention, it is preferable to use a pearlescent pigment as the luster pigment. As the pearlescent pigment, for example, those having a color tone such as a silver-colored pearlescent pigment, a gold-colored pearlescent pigment, or an interference colored pearlescent pigment can be used, and among these, a silver-colored pearlescent pigment is preferred.

[0024] Examples of flaky substrates that serve as the substrate for pearl pigments include crushed naturally occurring mica, industrially synthesized mica, glass flakes, silica flakes, alumina flakes, and barium sulfate. These can be used alone or in combination of two or more. Examples of metal oxides that can be used to coat the flaky substrates include titanium dioxide, silicon dioxide, iron oxide, aluminum oxide, zirconium oxide, cobalt oxide, zinc oxide, tin oxide, chromium oxide, and nickel oxide. These can be used alone or in combination of two or more.

[0025] Furthermore, when pearlescent pigments with different particle sizes are used, it is preferable that they have the same color tone, thereby enabling the production of a highly aesthetic design with uniform brilliance. For example, in the case of a silver-colored pearlescent pigment, the particle size is preferably 5 to 600 μm (more preferably 10 to 500 μm). In this case, a strong silver-tone (metallic) brilliance can be obtained. Furthermore, it is preferable to use different particle sizes in combination within the above range. One embodiment of this is, for example, the combination of a pearlescent pigment with a particle size of 5 μm or more but less than 50 μm and 50 μm or more but not more than 400 μm with a pearlescent pigment with a particle size of 10 μm or more but not more than 100 μm and 100 μm or more but not more than 600 μm. This allows the production of a metallic design with uniform and strong brilliance.

[0026] The mixing ratio of the luster pigment is preferably 0.1 to 50 parts by weight (more preferably 0.3 to 45 parts by weight, and even more preferably 0.5 to 40 parts by weight) relative to 100 parts by weight of the synthetic resin. In this case, a highly aesthetic design with uniform luster can be obtained.

[0027] The coating material of the present invention is characterized by a thixotropic index (TI) value of 1.5 or more (preferably 1.8 to 8.0, more preferably 2.0 to 6.0). In the present invention, by setting the viscosity characteristics of the coating material to such conditions, uneven absorption into the aggregate-containing decorative surface can be suppressed, allowing for the formation of a uniform design layer that follows the irregularities. In addition, the stability of the luster pigment in the coating material is improved, allowing for the formation of a design layer in which the luster pigment is uniformly dispersed along the irregularities without the luster material being unevenly distributed in the depressions on the decorative surface. This allows for the creation of a design with luster (such as a metallic tone) that is uniform in gloss.

[0028] The TI value in the present invention is a value determined by the following formula (1) using a BH type rotational viscometer. (Equation 1) TI value = η1 / η2 however, η1: Viscosity at 2 rpm (Pa·s: guideline value at second rotation, measurement temperature: 23°C) η2: Viscosity at 20 rpm (Pa·s: guideline value at 4th rotation, measurement temperature: 23°C)

[0029] The viscosity of the coating material of the present invention is preferably 0.3 to 10 Pa·s (more preferably 0.5 to 8 Pa·s). The viscosity in the present invention is a value determined by measuring the viscosity at 20 rpm (the indicator value at the fourth rotation) using a BH-type viscometer (measurement temperature: 23°C).

[0030] A preferred method for setting the TI value of the coating material within the above range is to add a thickener. Examples of thickeners include organic thickeners and inorganic thickeners. In the present invention, it is preferable to include an inorganic thickener.

[0031] Examples of organic thickeners include hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropylmethyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, polyvinylpyrrolidone, polyvinyl methyl ether, alkali swelling thickeners, hydrophobically modified alkali swelling thickeners, urethane associative thickeners, etc. These can be used alone or in combination of two or more.

[0032] Examples of inorganic thickeners that can be used include inorganic layered compounds, silica aerosil, and fumed silica. In the present invention, it is preferable to use an inorganic layered compound. Examples of inorganic layered compounds include natural or synthetic smectite clay minerals such as bentonite, montmorillonite, hectorite, saponite, sauconite, beidellite, and nontronite; magnesium aluminum silicate; and derivatives thereof modified with organic polymers such as carboxyvinyl polymers, xanthan gum, and guar gum. These compounds can be used alone or in combination of two or more.

[0033] The inorganic thickener of the present invention preferably has a transmittance of 90% or more in a 1% aqueous dispersion. Furthermore, the particle size of the inorganic layered compound contained in the inorganic thickener is preferably 5 to 50 nm, and the thickness thereof is preferably 0.5 to 2 nm. In this case, the transparency of the design layer formed by the coating material is not impaired, and the effects of the present invention can be fully exhibited.

[0034] Furthermore, the coating material may contain, as required, for example, coloring pigments (excluding the above-mentioned luster pigments), extender pigments, anti-algae agents, antibacterial agents, deodorizers, adsorbents, flame retardants, antifoaming agents, film-forming aids, antifreeze agents, ultraviolet absorbers, light stabilizers, antioxidants, catalysts, etc.

[0035] The design layer of the present invention is formed by applying a coating material containing the above-mentioned luster pigment. When the design layer is provided directly on the surface of the aggregate-containing decorative surface, a new design with luster can be imparted while taking advantage of the color of the aggregate-containing decorative surface. For example, when the decorative surface is monochromatic, a uniform luster can be imparted, and when the decorative surface is multicolored, a variety of luster can be imparted with different color tones and brilliance in different parts. The coating material may be applied to any location on the surface of the aggregate-containing decorative surface, but is preferably applied to the entire surface. The coating material can be applied using known tools, such as a spray or roller. The coating material can also be diluted with various solvents when applied. The solid content when applied is preferably 10 to 80% by weight (more preferably 15 to 60% by weight), and the amount applied per unit area is preferably 10 to 500 g / m. 2 (More preferably 20 to 300 g / m 2 ) The coating is preferably applied once or twice. In this case, the effects of the present invention can be fully achieved. The coating material may be cured by natural drying or may be forcibly cured by applying heat or the like.

[0036] In the repair method of the present invention, a colored layer can be applied to the surface of the aggregate-containing decorative surface before forming the design layer, allowing for the application of any desired color. Such a colored layer can be formed by applying and drying a colored coating material containing a resin component and a color pigment. By providing a colored layer, a metallic design with the desired color tone can be obtained.

[0037] Examples of the resin component include acrylic resin, urethane resin, vinyl acetate resin, urethane resin, silicone resin, fluororesin, acrylic vinyl acetate resin, acrylic urethane resin, acrylic silicone resin, etc., and one or more of these can be used. As such a resin component, a water-soluble resin and / or a water-dispersible resin is preferred.

[0038] The color pigment may be commercially available or a known material, but examples thereof include inorganic color pigments such as titanium oxide, zinc oxide, alumina, magnesium oxide, zirconium oxide, yttrium oxide, indium oxide, carbon black, ferric oxide (red iron oxide), yellow iron oxide, iron oxide, ultramarine, and cobalt green; composite oxide pigments such as iron-chromium composite oxide, manganese-bismuth composite oxide, manganese-yttrium composite oxide, and manganese-iron-cobalt composite oxide; and organic color pigments such as azo, naphthol, pyrazolone, anthraquinone, perylene, quinacridone, disazo, isoindolinone, benzimidazole, phthalocyanine, and quinophthalone; and the like. One or more of these may be used. In addition to these color pigments, extender pigments such as barium sulfate, calcium carbonate, silicon oxide, and magnesium oxide may also be used.

[0039] The colored coating material may contain various other components in addition to those described above, provided that the effects of the present invention are not significantly impaired. Examples of such components include thickeners, film-forming aids, leveling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, antifoaming agents, crosslinking agents, ultraviolet absorbers, and antioxidants.

[0040] Furthermore, the colored coating material preferably has a thixotropic index (TI) value of 1.5 or more (preferably 1.8 to 8.0, more preferably 2.0 to 6.0), which prevents uneven absorption into the aggregate-containing decorative surface and allows the formation of a uniform colored layer.

[0041] This colored coating material may be applied to any desired location on the aggregate-containing decorative surface, but is preferably applied to the entire surface. Known application tools such as brushes, rollers, and sprayers can be used. The amount of colored coating material applied when forming a colored layer is preferably 10 to 500 g / m2 in terms of solid content. 2 (More preferably 20 to 300 g / m 2 )

[0042] Furthermore, in the repair method of the present invention, after forming the design layer, a clear coat material can be applied to the outermost surface to form a colorless, transparent clear layer, for example, for purposes of surface protection, improved weather resistance, and stain resistance, as long as the effects of the present invention are not impaired. This can further enhance the brilliance (sensation of brightness). While known clear paints can be used for such a clear layer, it is preferable to use the same type of synthetic resin emulsion as the design layer. This makes it less likely that transparency will be reduced, and the lens effect of the clear layer can further enhance the brilliance (sensation of brightness).

[0043] This clear coating is preferably applied to the entire surface. As the application tool, for example, a brush, roller, spray, or other known application tool can be used. The amount of coating material applied when forming a colored layer is preferably 10 to 500 g / m2 in terms of solid content. 2 (More preferably 20 to 300 g / m 2 ) [Example]

[0044] The following examples will clarify the features of the present invention.

[0045] <Aggregate-containing decorative surface> The following decorative surfaces were used, which had been deteriorated by outdoor exposure. Cosmetic surface 1 A decorative surface (sandstone-like pattern, uneven height difference (maximum): 3.0 mm, color: white) formed on a base material (slate board) using an aggregate-containing finishing material containing 100 parts by weight of aggregate (grain size: 200 μm to 400 μm) and 20 parts by weight of acrylic resin. <Coating material> ·Covering material 1 Coating material 1 (TI value: 0.9) containing 200 parts by weight of acrylic resin emulsion (solid content: 50% by weight), 15 parts by weight of lustrous pigment 1 (silver pearl pigment, rutile-type titanium dioxide-coated mica, particle size 20 to 200 μm), 150 parts by weight of water, and additives (film-forming aids, etc.). ·Covering material 2 Coating material 2 (TI value: 1.9) containing 200 parts by weight of acrylic resin emulsion (solid content: 50% by weight), 15 parts by weight of lustrous pigment 1 (silver pearl pigment, rutile-type titanium dioxide-coated mica, particle size 20-200 μm), 1 part by weight of synthetic smectite clay mineral, 150 parts by weight of water, and additives (film-forming aids, etc.). ·Covering material 3 Coating material 3 (TI value: 2.5) containing 200 parts by weight of acrylic resin emulsion (solid content: 50% by weight), 15 parts by weight of lustrous pigment 1 (silver pearl pigment, rutile-type titanium dioxide-coated mica, particle size 20-200 μm), 2 parts by weight of synthetic smectite clay mineral, 150 parts by weight of water, and additives (film-forming aids, etc.). ·Covering material 4 Coating material 4 (TI value: 5.5) containing 200 parts by weight of acrylic resin emulsion (solid content: 50% by weight), 15 parts by weight of lustrous pigment 1 (silver pearl pigment, rutile-type titanium dioxide-coated mica, particle size 20 to 200 μm), 2.5 parts by weight of synthetic smectite clay mineral, 150 parts by weight of water, and additives (film-forming aids, etc.). ·Covering material 5 Coating material 5 (TI value: 2.5) containing 200 parts by weight of acrylic resin emulsion (solid content: 50% by weight), 15 parts by weight of lustrous pigment 2 (silver pearl pigment, rutile-type titanium dioxide-coated mica, particle size 45 to 500 μm), 2 parts by weight of synthetic smectite clay mineral, 150 parts by weight of water, and additives (film-forming aids, etc.). ·Covering material 6 Coating material 6 (TI value: 2.5) containing 200 parts by weight of acrylic resin emulsion (solid content: 50% by weight), lustrous pigment 1 (silver pearl pigment, rutile-type titanium dioxide coated mica, particle size 20-200 μm) 7.5 parts by weight, lustrous pigment 2 (silver pearl pigment, rutile-type titanium dioxide coated mica, particle size 45-500 μm) 7.5 parts by weight, synthetic smectite clay mineral 2 parts by weight, water 150 parts by weight, and additives (film-forming aids, etc.).

[0046] (Examples 1 to 6, Comparative Example 1) The coating material was applied to the decorative surface in the combination shown in Table 1 (weight per unit area: 100 g / m 2) and hardened (at 23°C for 3 hours) to form a decorative layer, thereby improving the decorative surface. In Example 5, the coating material 3 was applied in the first time at a weight per unit area of ​​50 g / m 2 and hardened (at 23°C for 3 hours). The second time, coating material 5 was applied at a weight per unit area of ​​50 g / m. 2 The decorative surface was then visually inspected and evaluated as follows:

[0047] (Evaluation method) Aesthetics The evaluation was conducted on a four-point scale (excellent: A>B>C>D: poor), with "A" being given to products with no uneven color or brilliance (sensation of brightness) and excellent aesthetics, and "D" being given to products with uneven color or brilliance (sensation of brightness) that were observed. Brightness There are four levels, with "A" representing excellent brightness and "D" representing poor brightness (excellent: A>B>C>D: poor).

[0048] [Table 1]

[0049] In Examples 1 to 6, a silver metallic design without uneven color or brilliance was obtained. In particular, in Examples 2 to 6, a highly aesthetic design with uniform brilliance was obtained.

[0050] Example 7 A blue colored coating material (200 parts by weight of acrylic resin emulsion (solid content 50% by weight), 20 parts by weight of phthalocyanine blue, and additives (film-forming aids, etc.) - TI value: 2.2) was applied to the decorative surface at an amount of 150 g / m 2 (solid content) to form a colored coating layer, and after curing for one day, coating material 6 was applied (weight per unit area 100 g / m 2) and hardened (at 23°C for 3 hours) to form a design layer, restoring the decorative surface. An excellent design with a uniform brilliance of blue metallic tone was obtained, making the most of the blue color of the base. When evaluated in the same way as above, it received an aesthetic rating of "A" and a brightness rating of "A".

Claims

[Claim 1] A method for repairing decorative surfaces containing aggregate, A step of forming a design layer by applying a coating material containing a synthetic resin and a glossy pigment, having a thixotropic index (TI value) of 1.5 or higher. A modification method characterized by including the following.