Nickel-based lithium metal composite oxide, manufacturing method thereof, and lithium secondary battery having positive electrode containing the nickel-based lithium metal composite oxide

JP2023104990A5Active Publication Date: 2024-11-29SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023084797
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-06-30
Filing Date
2023-05-23
Publication Date
2024-11-29
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

The existing manufacturing process for nickel-based lithium metal composite oxides is complex and costly due to the need for repeated heat treatments of large and small secondary particles, leading to potential overbaking or incomplete sintering, which degrades performance and increases costs.

Method used

A method involving the simultaneous heat treatment of large and small secondary particles with controlled nickel content differences, resulting in a nickel-based lithium metal composite oxide with improved structural stability and simplified manufacturing.

Benefits of technology

The method produces a nickel-based lithium metal composite oxide with enhanced structural stability, leading to improved efficiency and lifespan of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a nickel-based lithium metal composite oxide and a manufacturing method thereof, and a lithium secondary battery having a positive electrode that contains the nickel-based lithium metal composite oxide.SOLUTION: A nickel-based lithium metal composite oxide, a manufacturing method thereof, and a lithium secondary battery having a positive electrode containing the nickel-based lithium metal composite oxide are disclosed. The nickel-based lithium metal composite oxide comprises primary particles, and secondary particles including aggregates of the primary particles. In the nickel-based lithium metal composite oxide, a nickel content is 50 mol% or more to a transition metal total content. The secondary particles include large secondary particles of 10 μm or more in particle size, and small secondary particles of 5 μm or less in particle size. The large secondary particles are larger than the small secondary particles in nickel content.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a nickel-based lithium metal composite oxide, a method for producing the same, and a lithium secondary battery including a positive electrode containing the same. [Background technology]

[0002] The development of portable electronic devices and communication devices has increased the need for the development of high-energy-density lithium secondary batteries.

[0003] When a lithium metal composite oxide is used as a positive electrode active material for a lithium secondary battery, mixing large secondary particles with small secondary particles can suppress the collapse of the active material even during pressing, thereby enabling the production of a lithium secondary battery with excellent performance and high energy density.

[0004] When manufacturing a lithium metal composite oxide containing a mixture of large and small secondary particles, the large and small secondary particles are heat-treated simultaneously. However, the large and small secondary particles have different properties, and if they are heat-treated simultaneously, the small or large secondary particles may be over- or incompletely sintered, resulting in reduced performance. Therefore, the large and small secondary particles are heat-treated separately, and then the heat-treated mixture is heat-treated again. However, because multiple heat treatments are required, the manufacturing process for the cathode active material becomes complicated and increases manufacturing costs, and improvements are needed. Summary of the Invention [Problem to be solved by the invention]

[0005] The problem to be solved by the present invention is to provide a nickel-based lithium metal composite oxide having improved structural stability.

[0006] Another problem to be solved by the present invention is to provide a method for producing the nickel-based lithium metal composite oxide, which can obtain the nickel-based lithium metal composite oxide at low production cost and through a simplified production process.

[0007] Another problem to be solved by the present invention is to provide a lithium secondary battery having a positive electrode containing the above-mentioned nickel-based lithium metal composite oxide, and having improved efficiency and lifespan. [Means for solving the problem]

[0008] In one aspect, there is provided a nickel-based lithium metal composite oxide comprising secondary particles including aggregates of primary particles, the nickel content being 50 mol% or more based on the total transition metal content in the nickel-based lithium metal composite oxide, the secondary particles including large secondary particles having a particle size of 10 μm or more and small secondary particles having a particle size of 5 μm or less, and the nickel content of the large secondary particles being higher than the nickel content of the small secondary particles.

[0009] The present invention provides a nickel-based lithium metal composite oxide having a positive electrode containing the nickel-based lithium metal composite oxide, in which the ratio (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) shown at a voltage of 4.1 V to 4.25 V at a current of 1 C in a dq / dv charge / discharge differential curve is 1.1 or more.

[0010] In another aspect, there is provided a method for producing a nickel-based lithium metal composite oxide, the method comprising the steps of mixing a large-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more, based on the total transition metal content in the large-particle nickel-based metal hydroxide, a small-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more, based on the total transition metal content in the small-particle nickel-based metal hydroxide, and a lithium precursor to obtain a precursor mixture, and then heat-treating the precursor mixture to obtain the nickel-based lithium metal composite oxide.

[0011] In yet another aspect, there is provided a lithium secondary battery including a positive electrode comprising the nickel-based lithium metal composite oxide described above. [Effects of the Invention]

[0012] The nickel-based lithium metal composite oxide according to an embodiment has excellent structural stability, and a lithium secondary battery having improved life and high-rate characteristics can be manufactured by using a positive electrode including such a nickel-based lithium metal composite oxide. [Brief explanation of the drawings]

[0013] [Figure 1] 1 is a graph showing dQ / dV charge / discharge differential curves after the first cycle in the lithium secondary batteries of Preparation Example 1 and Comparative Preparation Examples 1 and 2. [Figure 2] 1 is a graph showing dQ / dV charge / discharge differential curves after 30 cycles in the lithium secondary batteries of Preparation Example 1 and Comparative Preparation Example 2. [Figure 3] 1 is a graph showing dQ / dV charge / discharge differential curves after 50 cycles in the lithium secondary batteries of Preparation Example 1 and Comparative Preparation Example 2. [Figure 4] 1 is a graph showing dQ / dV charge / discharge differential curves for the lithium secondary battery of Preparation Example 1 at the first cycle, after 30 cycles, and after 50 cycles. [Figure 5] 1 is a graph showing dQ / dV charge / discharge differential curves for the lithium secondary battery of Comparative Preparation Example 2 at the first cycle, after 30 cycles, and after 50 cycles. [Figure 6] 1 is an X-ray diffraction analysis graph of the composite positive electrode active material obtained in Example 1. [Figure 7] 1 is a diagram illustrating a schematic structure of a lithium secondary battery according to an embodiment. [Figure 8] 1 is a graph showing the life characteristics of the lithium secondary batteries of Production Examples 1 and 2 and the lithium secondary battery of Comparative Production Example 1. [Figure 9]1 is a graph showing charge / discharge characteristics of coin cells fabricated according to Fabrication Example 1 and Comparative Fabrication Example 1. DETAILED DESCRIPTION OF THE INVENTION

[0014] Exemplary nickel-based lithium metal composite oxides, methods for producing the same, and lithium secondary batteries having positive electrodes containing the same are described in further detail below with reference to the accompanying drawings.

[0015] The nickel-based lithium metal composite oxide includes secondary particles comprising aggregates of primary particles, and has a nickel content of 50 mol% or more based on the total transition metal content in the nickel-based lithium metal composite oxide. The secondary particles include large secondary particles having a particle size of 10 μm or more and small secondary particles having a particle size of 5 μm or less, and the nickel content of the large secondary particles is higher than the nickel content of the small secondary particles. The particle size refers to the average particle size when the particles are spherical, and refers to the length of the major axis when the particles are non-spherical. The particle size can be measured using a particle size analyzer, a scanning electron microscope, and / or a transmission electron microscope. The particle size refers to, for example, the average particle size (D50).

[0016] Unless otherwise defined, the term "average particle size (D50)" used herein refers to the average diameter of particles corresponding to 50% of the cumulative volume in a particle size distribution. This refers to the particle size value corresponding to 50% of the smallest particles when the total number of particles is 100% in a particle size distribution curve, where particle sizes are accumulated from the smallest to the largest. The average particle size (D50) can be measured using methods well known to those skilled in the art, such as a particle size analyzer (e.g., a HORIBA LA-950 Laser Particle Size Analyzer) or from TEM or SEM images. Alternatively, the average particle size (D50) can be easily calculated by measuring the number of particles in each particle size range using a dynamic light scattering (DLS) measurement device and analyzing the data.

[0017] In the nickel-based lithium metal composite oxide, the nickel content is 60 mol % or more, 75 mol % or more, or 75 mol % to 99 mol %.

[0018] The nickel-based lithium metal composite oxide has a differential capacity dQ / dV charge / discharge differential curve for a lithium secondary battery equipped with a positive electrode containing the nickel-based lithium metal composite oxide, and the ratio (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) shown at a current of 1 C and a voltage of 4.1 V to 4.25 V is 1.1 or more.

[0019] The dQ / dV charge / discharge differential curves were obtained in the voltage range of 3.0V to 4.3V, for example, 3.0V to 4.25V.

[0020] In the dQ / dV charge / discharge differential curve, V represents the voltage relative to the lithium metal anode, and Q represents the charge / discharge capacity of the lithium secondary battery. In the dQ / dV charge / discharge differential curve, the X axis represents voltage V, and the Y axis represents the value (dQ / dV) obtained by differentiating the charge / discharge capacity with respect to voltage.

[0021] In order to produce a lithium secondary battery having excellent capacity characteristics using this nickel-based lithium metal composite oxide, it is common to produce the battery by heat treating a large-particle nickel-based lithium metal composite oxide precursor, a small-particle nickel-based lithium metal composite oxide precursor, and a lithium precursor.

[0022] The large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal composite oxide precursor have different properties, and therefore, the desired nickel-based lithium metal composite oxide can only be obtained by separately calcining the precursors and then mixing them with a lithium precursor and carrying out a secondary calcination. As a result, three calcination steps are required to obtain the nickel-based lithium metal composite oxide, which increases production costs and complicates the production process, and improvements are needed.

[0023] To solve the above-mentioned problems, the present inventors have completed the present invention, which relates to a nickel-based lithium metal composite oxide having excellent structural stability and excellent capacity characteristics, which is produced by simultaneously heat-treating a large-particle nickel-based lithium metal composite oxide precursor, a small-particle nickel-based lithium metal composite oxide precursor, and a lithium precursor once while controlling the particle size and nickel content of the large-particle nickel-based lithium metal composite oxide precursor and a small-particle nickel-based lithium metal composite oxide precursor within a predetermined range.

[0024] The large-particle nickel-based lithium metal composite oxide precursor is, for example, a large-particle nickel-based metal hydroxide, and the small-particle nickel-based lithium metal composite oxide precursor is, for example, a small-particle nickel-based metal hydroxide.

[0025] In the large-particle nickel-based metal hydroxide and the small-particle nickel-based metal hydroxide, the nickel content is 50 mol % or more, 60 mol % or more, 75 mol % or more, or 75 mol % to 99 mol % based on the total transition metal content in the large-particle nickel-based metal hydroxide and the small-particle nickel-based metal hydroxide.

[0026] The difference in nickel content between the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal precursor is 10 mol% or more, 11 mol% or more, 11 mol% to 24 mol%, for example, 11 to 20 mol%, 11 to 18 mol%, or 12 to 16 mol%. When the difference in nickel content between the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal precursor is within the above-mentioned range, a nickel-based lithium metal composite oxide with excellent structural stability and energy density can be obtained.

[0027] The difference in nickel content between the large secondary particles and the small secondary particles contained in the nickel-based lithium metal composite oxide obtained from the precursor is maintained the same as the difference in nickel content between the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal precursor.

[0028] The difference in nickel content between the large and small secondary particles contained in the nickel-based lithium metal composite oxide is 10 mol % or more, 11 mol % or more, for example, 11 to 20 mol %, 11 to 18 mol %, or 12 to 16 mol %. When the difference in nickel content between the large and small secondary particles is within the above-mentioned range, the large and small nickel-based lithium metal precursors used to obtain them can be simultaneously heat-treated to produce a nickel-based lithium metal composite oxide with excellent structural stability and energy density.

[0029] In the large secondary particles, the nickel content is 85 to 99 mol%, for example, 85 to 95 mol%, for example, 88 to 95 mol%, based on the total content of transition metals, and in the small secondary particles, the nickel content is 75 to 89 mol%, for example, 80 to 85 mol%, for example, 75 to 85 mol%, based on the total content of transition metals.

[0030] The particle size of the large-particle nickel-based lithium metal composite oxide precursor is 10 μm to 17 μm, for example, 12 to 15 μm. The particle size of the small-particle nickel-based lithium metal composite oxide precursor is 2 μm to 5 μm, for example, 3 to 4 μm. The particle size of the large secondary particles contained in the nickel-based lithium metal (NCA) composite oxide obtained from such a precursor is 10 μm or more, 12 μm or more, 14 μm or more, or 15 μm or more, for example, 12 to 17 μm.

[0031] In one embodiment, the large secondary particles have a particle size of 10 to 15 μm, for example, 12 to 17 μm, and the small secondary particles have a particle size of 2 to 5 μm, for example, 3 to 4 μm.

[0032] When the particle sizes of the large and small secondary particles are within the aforementioned ranges, the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal composite oxide precursor used to obtain them can be simultaneously heat-treated to obtain a nickel-based lithium metal composite oxide with excellent structural stability and energy density. The content of the large-particle nickel-based lithium metal composite oxide precursor is 30 to 90 parts by weight, 50 to 90 parts by weight, 60 to 90 parts by weight, or 80 to 90 parts by weight, based on 100 parts by weight of the total content of the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal composite oxide precursor.

[0033] In the nickel-based lithium metal composite oxide of the present invention, the content of the large secondary particles is 30 to 90 parts by weight, 50 to 90 parts by weight, 60 to 90 parts by weight, or 80 to 90 parts by weight, based on 100 parts by weight of the total content of the large secondary particles and the small secondary particles.

[0034] When the mixing weight ratio of the large secondary particles to the small secondary particles is within the aforementioned range, the large-particle nickel-based lithium metal precursor and the small-particle nickel-based lithium metal precursor used to obtain them can be simultaneously heat-treated to obtain a nickel-based lithium metal composite oxide with excellent structural stability and energy density.

[0035] In a lithium secondary battery including a positive electrode containing the nickel-based lithium metal composite oxide according to an embodiment, the ratio (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) is 1.1 or more, for example, 1.1 to 1.5, in a dQ / dV charge / discharge differential curve at a current of 1 C and a voltage of 4.3 V to 3.0 V. The charge peak and discharge peak are observed at a current of 1 C and a voltage of 4.1 V to 4.25 V.

[0036] The charge and discharge conditions for the lithium secondary battery having the above-mentioned positive electrode are as follows.

[0037] The lithium secondary battery is charged at a constant current of 1 C until it reaches 4.3 V, and then charged at a constant voltage of 0.05 C until it reaches 0.05 C. After charging, the battery is rested for about 10 minutes, and then discharged at a constant current of 1 C until the voltage reaches 3 V. This cycle is repeated multiple times and evaluated.

[0038] The dQ / dV charge-discharge differential curves are those after the first 100 charge-discharge cycles, the first 80 charge-discharge cycles, or the first 50 charge-discharge cycles. The charge-discharge cycles can be repeated, for example, a total of 50 times.

[0039] The charging peak is indicated, for example, at 4.17V to 4.25V, for example, at 4.19V, and the discharging peak is indicated, for example, at 4.14V to 4.17V, for example, at 4.16V.

[0040] The dQ / dV charge / discharge differential curve represents the capacity characteristics of the working ions associated with the positive electrode active material at different voltages. The position, intensity difference, and area of ​​the main peak vary depending on the type and physical properties of the positive electrode active material.

[0041] dQ / dV is a graph showing the results of measuring the dq / dv distribution when a lithium battery including a positive electrode containing the nickel-based lithium metal composite oxide of the present invention and a lithium metal negative electrode is discharged at a rate of 1 C. The nickel-based lithium metal composite oxide is, for example, lithium nickel oxide (NCA).

[0042] The dQ / dV distribution has three to six, e.g., five, main peaks, of which the peak at approximately 3.65 V corresponds to the main peak of NCA, which is related to the phase transition from a hexagonal structure to a monoclinic structure, and the peaks in the voltage range of 4.1 V to 4.25 V indicate structural changes due to degradation of the NCA.

[0043] The ratio (A2 / A1) of the discharge peak intensity (A2) to the dQ / dV charge peak intensity (A1) is 1.1 to 1.5. The charge peak intensity indicates the amount of electrical energy stored in the lithium secondary battery, and the discharge peak intensity indicates the amount of structural change. When the ratio (A2 / A1) of the discharge peak intensity (A2) to the dQ / dV charge peak intensity (A1) is within the above range, it is related to the difference in Ni content and Co content between the large and small particles. When it is within this range, the NCA has low surface resistance, which can be used to manufacture lithium secondary batteries with excellent high-temperature life and storage characteristics.

[0044] The dQ / dV charge-discharge differential curves described above relate to the first charge-discharge cycle to the 50th charge-discharge cycle of the lithium secondary battery, for example, after the first charge-discharge cycle, after the 30th charge-discharge cycle, or after the 50th charge-discharge cycle. The conditions for evaluating the charge-discharge cycles are as described in Evaluation Example 1 below.

[0045] In the dQ / dV charge / discharge differential curve of the nickel-based lithium metal composite oxide according to an embodiment, the charge peak at a voltage of 3.5V to 3.8V has a gentle slope.

[0046] The nickel-based lithium metal composite oxide is also a compound represented by the following chemical formula 1:

[0047] [ka]

[0048] In the above formula 1, M is manganese (Mn), aluminum (Al), or a combination thereof; M' is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; and 0.95≦a≦1.3, 0 <x<0.5、0<y<0.5、0≦z<0.5、0<x+y+z≦0.5である。

[0049] The sum of x+y+z is, for example, 0.01 to 0.2, 0.01 to 0.12, 0.04 to 0.1, or 0.04 to 0.08.

[0050] In the compound of Chemical Formula 1, the nickel content is 50 mol % or more, which is higher than the content of each of the transition metals such as cobalt, M, and M'. By using a positive electrode containing such a nickel-based lithium metal composite oxide, it is possible to manufacture a lithium secondary battery having high lithium diffusivity, good conductivity, and a larger capacity at the same voltage.

[0051] In Chemical Formula 1, 0.95 ≦ a ≦ 1.3, 0 < x ≦ 0.3, 0 ≦ y ≦ 0.5, 0 ≦ z ≦ 0.05, and 0.5 ≦ 1 - x - y - z ≦ 0.95. In the aforementioned Chemical Formula 1, a is, for example, 1 to 1.1, x is 0.05 to 0.3, or 0.05 to 0.1, y is 0.05 to 0.3, z is 0, or z is 0.001 to 0.01.

[0052] According to one embodiment, in Chemical Formula 1, z is 0.

[0053] The compound of Chemical Formula 1 is, for example, Li 0.94 Ni 0.92 Co 0.05 Al 0.03 O 2、 LiNi 0.8 Co 0.1 MnAl 0.1 O2, LiNi 0.85 Co 0.1 Al 0.05 O2, Li 1.1 Ni 0.92 Co 0.05 Mn 0.03 O 2、 LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.85 Co 0.1 Mn 0.05 O2, Li 1.1 Ni 0.94 Co 0.03 Mn 0.03 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.94 Co 0.03 Al 0.03 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.96 Co 0.02 Al 0.02 such as O2.

[0054] According to one embodiment, the large secondary particles are a compound of Chemical Formula 1, where 0.88≦1−xyz≦0.95, 0.01≦x≦0.08, 0.001≦y≦0.05, and 0≦z≦0.01. And the small secondary particles are a compound of Chemical Formula 1, where 0.75≦1−xyz≦0.85, 0.01≦x≦0.15, 0.001≦y≦0.05, and 0≦z≦0.01.

[0055] According to an embodiment, the large secondary particles are a compound represented by the following Formula 1-1, and the small secondary particles are a compound represented by the following Formula 1-2.

[0056] [ka]

[0057] In the above formula 1-1, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof, and 0.95≦a≦1.3, 0 <x<0.5、0<y<0.5、0≦z<0.5である。

[0058] In chemical formula 1-1, 0.88≦1-xyz≦0.96, 0.01≦x≦0.08, 0.001≦y≦0.05, and 0≦z≦0.01;

[0059] [ka]

[0060] In the above formula 1-2, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof, and 0.95≦a≦1.3, 0 <x<0.5、0<y<0.5、0≦z<0.5である。

[0061] In chemical formula 1-2, 0.75≦1-xyz≦0.85, 0.01≦x≦0.05, 0.001≦y≦0.05, and 0≦z≦0.01.

[0062] The large secondary particles of formula 1-1 are, for example, Li 1.1 Ni 0.92 Co 0.05 Al 0.03 O 2、 LiNi 0.94 Co 0.03 Al 0.03 O2, LiNi 0.88 Co 0.08 Al 0.04 O2, LiNi 0.90 Co 0.05 Al 0.05 O2, LiNi 0.96 Co 0.02 Al 0.02 O2, LiNi 0.88 Co 0.06 Al 0.06 O2, etc., and the small secondary particles of chemical formula 1-2 are LiNi 0.8 Co 0.15 Al 0.05 O 2、 LiNi 0.75 Co 0.20 Al 0.05 O2, etc.

[0063] The specific surface area of ​​the large secondary particles is 0.1 to 1 m 2 / g, for example, 0.3 to 0.8 m 2 / g, and the specific surface area of ​​the small secondary particles is 2 to 15 m 2 / g, e.g., 2 to 10 m 2 / g. When the specific surface areas of the large secondary particles and the small secondary particles are within the above-mentioned ranges, a positive electrode and a lithium secondary battery having excellent capacity characteristics, life characteristics, and high-temperature storage characteristics can be produced. The specific surface area is the BET specific surface area measured by the Brunauer-Emmett-Teller method (BET method).

[0064] The compound of Chemical Formula 1 has a structure in which primary particles are aggregated to form spherical secondary particles, and the average particle size of the secondary particles is 1 to 25 μm, for example, 5 to 25 μm.

[0065] Hereinafter, a method for manufacturing a composite positive electrode active material according to an embodiment will be described.

[0066] A composite positive electrode active material can be obtained by mixing a nickel-based metal hydroxide, which is a large secondary particle, a nickel-based metal hydroxide, which is a small secondary particle, and a lithium precursor to obtain a precursor mixture, which is then heat-treated.

[0067] The nickel-based metal hydroxide is a precursor of a nickel-based lithium metal composite oxide.

[0068] The particle size of the nickel-based metal hydroxide that is the large secondary particles is 10 μm or more, for example, 12 to 17 μm, and the particle size of the nickel-based metal hydroxide that is the small secondary particles is 5 μm or less, for example, 2 to 5 μm.

[0069] The nickel-based metal hydroxide is also a compound represented by the following chemical formula 2.

[0070] [ka]

[0071] In the above formula 2, M is manganese (Mn), aluminum (Al), or a combination thereof; M' is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; <x<0.5、0<y<0.5、0≦z<0.5、0<x+y+z≦0.5である。

[0072] In Chemical Formula 2, 0 < x ≤ 0.3, 0 ≤ y ≤ 0.5, and 0 ≤ z ≤ 0.05. In Chemical Formula 2, x + y + z is from 0.01 to 0.25, for example, from 0.04 to 0.25.

[0073] The nickel-based metal hydroxide is also a compound represented by the following Chemical Formula 2-1.

[0074] [Chemical Formula]

[0075] In the aforementioned Chemical Formula 2-1, M is an element selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), and zirconium (Zr), where 0 < x < 0.5, 0 < y < 0.5, 0 ≤ z < 0.5, and 0 < x + y + z ≤ 0.50.

[0076] In Chemical Formula 2-1, for example, 0 < x ≤ 0.3, 0 ≤ y ≤ 0.5, and 0 ≤ z ≤ 0.05. In Chemical Formula 2-1, x + y + z is from 0.01 to 0.25, for example, from 0.04 to 0.25.

[0077] The nickel-based metal hydroxide according to an embodiment is, for example, Ni 0.92 Co 0.05 Al 0.03 (OH)2, Ni 0.94 Co 0.03 Al 0.03 (OH)2, Ni 0.88 Co 0.06 Al 0.06 (OH)2, Ni 0.96 Co 0.02 Al 0.02 (OH)2, Ni 0.93 Co 0.04 Al 0.03 (OH)2, Ni 0.8 Co 0.15 Al 0.05 O2(OH) 2、 Ni 0.75 Co 0.20 Al0.05 (OH) 2、 Ni 0.92 Co 0.05 Mn 0.03 (OH)2, Ni 0.94 Co 0.03 Mn 0.03 (OH)2, Ni 0.88 Co 0.06 Mn 0.06 (OH)2, Ni 0.96 Co 0.02 Mn 0.02 (OH)2, Ni 0.93 Co 0.04 Mn 0.03 (OH)2, Ni 0.8 Co 0.15 Mn 0.05 O2(OH) 2、 Ni 0.75 Co 0.20 Mn 0.05 (OH)2, or a combination thereof.

[0078] In this specification, the compositions of the large-particle and small-particle nickel-based metal hydroxide are controlled to correspond to the compositions of the large-particle and small-particle nickel-based metal composite oxide.

[0079] The lithium precursor may be, for example, lithium hydroxide, lithium fluoride, lithium carbonate, Li2COOH, or a mixture thereof, and the content of the lithium precursor is controlled so that the molar ratio of lithium in the lithium precursor to the transition metal in the nickel-based metal hydroxide (Li / M) is 0.95 or more, for example, more than 1.0, for example, 1.05 to 1.3, for example, 1.1 to 1.2.

[0080] The transition metal of the nickel-based metal hydroxide refers to the combined metals of Ni, Co, Mn, M, and M' in Chemical Formula 2. The contents of the lithium precursor and the nickel-based metal hydroxide are stoichiometrically adjusted so as to produce the nickel-based lithium metal composite oxide of Chemical Formula 1.

[0081] The above-mentioned mixing can be dry mixing or can be carried out using a mixer or the like.

[0082] The heat treatment is carried out in an oxidizing gas atmosphere.

[0083] The oxidizing gas atmosphere utilizes an oxidizing gas such as oxygen or air, for example, the oxidizing gas is composed of 10 to 20% by volume of oxygen or air and 80 to 90% by volume of an inert gas.

[0084] The heat treatment is preferably performed at a temperature within a range of 650°C to 800°C, 700°C to 750°C, e.g., 700°C to 720°C, at which the reaction between the lithium precursor and the nickel-based metal hydroxide proceeds and at a temperature not exceeding the densification temperature. Here, the densification temperature refers to a temperature at which sufficient crystallization occurs and the active material can exhibit charge capacity. The heat treatment is preferably performed at a temperature within a range of 650°C to 800°C, 700°C to 750°C, e.g., 700°C to 720°C.

[0085] The heat treatment time varies depending on the heat treatment temperature and the like.

[0086] The mixing weight ratio of the nickel-based metal hydroxide as the large secondary particles to the nickel-based metal hydroxide as the small secondary particles is 9:1 to 8:2.

[0087] The nickel-based metal hydroxides that are the large secondary particles and the nickel-based metal hydroxides that are the small secondary particles can be produced by a common method. For example, the nickel-based metal hydroxides that are the large secondary particles and the nickel-based metal hydroxides that are the small secondary particles differ only in the reaction time of the nickel-based metal hydroxide precursor (raw material) and the drying process of the product obtained after the reaction, and the remaining processes can be carried out in the same manner.

[0088] In the case of large-sized nickel-based metal hydroxides, the reaction time to obtain the nickel-based metal hydroxide is, for example, in the range of 90 to 130 hours, and drying is carried out at 180 to 200°C, 185 to 200°C, 190 to 200°C, for example, 200°C. In the case of small-sized nickel-based metal hydroxides, the reaction time of the precursor (raw material) of the nickel-based metal hydroxide is shorter than that of large-sized nickel-based metal hydroxides, for example, 20 to 30 hours, for example, 20 to 28 hours. The product after the reaction is dried at a temperature in the range of 200 to 220°C.

[0089] By using the method for preparing a nickel-based lithium metal composite oxide according to an embodiment, a positive electrode active material with high capacity, improved charge / discharge efficiency, and improved lifespan can be obtained.

[0090] Hereinafter, a method for manufacturing a lithium secondary battery having a positive electrode including a nickel-based lithium metal composite oxide according to an embodiment as a positive electrode active material, a negative electrode, a lithium salt-containing non-aqueous electrolyte, and a separator will be described.

[0091] The positive electrode and the negative electrode are fabricated by coating a positive electrode active material layer-forming composition and a negative electrode active material layer-forming composition, respectively, on a current collector and drying the coating. The positive electrode active material-forming composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent, and the positive electrode active material according to an embodiment is used as the positive electrode active material.

[0092] The binder is a component that aids in bonding the active material to the conductive agent and the current collector, and is added in an amount of 1 to 50 parts by weight based on 100 parts by weight of the total weight of the positive electrode active material. Non-limiting examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers. The binder content is 2 to 5 parts by weight based on 100 parts by weight of the total weight of the positive electrode active material. When the binder content is within the above range, the active material layer exhibits good adhesion to the current collector.

[0093] The conductive agent is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and examples thereof include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0094] The content of the conductive agent is 2 to 5 parts by weight based on 100 parts by weight of the total weight of the positive electrode active material. When the content of the conductive agent is within the above range, the final electrode has excellent conductivity.

[0095] Non-limiting examples of the solvent include N-methylpyrrolidone, and the amount of the solvent is 100 to 3,000 parts by weight based on 100 parts by weight of the positive electrode active material. When the amount of the solvent is within the above range, the process of forming the active material layer is easy.

[0096] The positive electrode current collector is not particularly limited as long as it has a thickness of 3 to 500 μm, does not induce chemical changes in the battery, and has high conductivity, and may be made of, for example, stainless steel, aluminum, nickel, titanium, heat-treated carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The current collector may have fine irregularities on its surface to enhance adhesion of the positive electrode active material, and may be in a variety of forms, such as a film, sheet, foil, net, porous material, foam, or nonwoven fabric.

[0097] Separately, a negative electrode active material, a binder, a conductive agent, and a solvent are mixed together to prepare a composition for forming a negative electrode active material layer.

[0098] The negative electrode active material is a material capable of absorbing and releasing lithium ions. Non-limiting examples of the negative electrode active material include carbon-based materials such as graphite and carbon; lithium metal and its alloys; and silicon oxide-based materials. According to one embodiment of the present invention, silicon oxide is used.

[0099] The binder may be any of a variety of binder polymers, including, but not limited to, polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers in which hydrogen is substituted with Li, Na, or Ca, or various copolymers. The binder may be added in an amount of 1 to 50 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material. Non-limiting examples of such binders include the same types as those used in the positive electrode.

[0100] The negative electrode active material layer-forming composition may further include a conductive agent. The conductive agent is not particularly limited as long as it is conductive and does not induce chemical changes in the battery. Examples of the conductive agent include graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. The conductive agent is preferably carbon black, more specifically, carbon black having an average particle size of several tens of nanometers.

[0101] The conductive agent may be present in an amount of 0.01 to 10 parts by weight, 0.01 to 5 parts by weight, or 0.1 to 2 parts by weight, based on 100 parts by weight of the total weight of the negative electrode active material layer.

[0102] The composition for forming a negative electrode active material layer may further include a thickener, which may be at least one of carboxymethyl cellulose (CMC), carboxyethyl cellulose, starch, regenerated cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and polyvinyl alcohol.

[0103] The amount of the solvent is 100 to 3,000 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material. When the amount of the solvent is within the above range, the process of forming the negative electrode active material layer is easy. The solvent may be the same as that used in manufacturing the positive electrode.

[0104] The negative electrode current collector is typically formed to a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it is conductive and does not induce chemical changes in the battery. Examples of such a negative electrode current collector include copper, stainless steel, aluminum, nickel, titanium, heat-treated carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, or silver, and aluminum-cadmium alloys. Similarly to the positive electrode current collector, the surface can be formed with fine irregularities to strengthen the binding strength of the negative electrode active material. The negative electrode current collector can be formed in a variety of forms, such as a film, sheet, foil, net, porous material, foam, or nonwoven fabric.

[0105] A separator is interposed between the positive electrode and negative electrode prepared by the above process.

[0106] The separator has a pore size of 0.01 to 10 μm and a thickness of 5 to 300 μm. Specific examples include sheets or nonwoven fabrics made of olefin polymers such as polypropylene and polyethylene, or glass fibers. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separator.

[0107] The lithium salt-containing non-aqueous electrolyte is composed of a non-aqueous electrolyte solution and a lithium salt. The non-aqueous electrolyte may be a non-aqueous electrolyte solution, an organic solid electrolyte, or an inorganic solid electrolyte.

[0108] Examples of the non-aqueous electrolyte include, but are not limited to, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, N,N-formamide, N,N-dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0109] Non-limiting examples of the organic solid electrolyte include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate ester polymers, polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride.

[0110] Non-limiting examples of the inorganic solid electrolyte that may be used include nitrides, halides, and sulfates of Li, such as LiN, LiI, LiNI, LiN-LiI-LiOH, LiSiO, LiSiS, LiSiO, LiSiO-LiI-LiOH, and LiPO-LiS-SiS.

[0111] The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, and non-limiting examples thereof include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (FSO2)2NLi, etc. may be used.

[0112] FIG. 7 is a cross-sectional view schematically illustrating a representative structure of a lithium secondary battery according to an embodiment.

[0113] Referring to FIG. 7 , a lithium secondary battery 21 includes a positive electrode 23, a negative electrode 22, and a separator 24. The positive electrode 23, the negative electrode 22, and the separator 24 are wound or folded and housed in a battery case 25. Next, an organic electrolyte solution is poured into the battery case 25 and sealed with a cap assembly 26 to complete the lithium secondary battery 20. The battery case 25 may be cylindrical, rectangular, thin-film, or the like. For example, the lithium secondary battery 20 may be a large-scale thin-film battery. The lithium secondary battery may also be a lithium-ion battery. A separator may be disposed between the positive electrode and the negative electrode to form a battery structure. The battery structures may be stacked in a bi-cell structure, impregnated with an organic electrolyte solution, and the resulting structure may be housed in a pouch and sealed to complete a lithium-ion polymer battery. Furthermore, a plurality of the battery structures may be stacked to form a battery pack, which may be used in any device requiring high capacity and high power output. For example, they are also used in laptop computers, smartphones, electric vehicles (EVs), and the like.

[0114] In addition, the lithium secondary battery has excellent storage stability, life characteristics, and high rate characteristics at high temperatures, and can therefore be used in electric vehicles, including hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs).

[0115] The present invention will be described in further detail through the following examples and comparative examples, which are provided for illustrative purposes only and are not intended to be limiting.

[0116] (Production of nickel-based metal hydroxides)

[0117] Production Example 1: Production of large nickel-based metal hydroxide particles The coprecipitation method described below was used to prepare large nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 (OH)2).

[0118] Ammonia water was added to the reactor, and the raw material for nickel-based metal hydroxide was added thereto in a stoichiometrically controlled manner to obtain the composition of the final product. The pH of the mixture in the reactor was adjusted using sodium hydroxide. The mixture was then allowed to react with stirring until the desired size was reached. The addition of the raw material solution was then stopped, and the product was obtained through a drying process. This manufacturing process is described in detail below.

[0119] A mixed solution was prepared by dissolving nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and aluminum sulfate (Al2(SO4)3·H2O) in distilled water as the solvent in a molar ratio of 94:3:3 to prepare the raw materials for nickel-based metal hydroxide. A diluted solution of ammonia water (NH4OH) and sodium hydroxide (NaOH) were also prepared as a precipitant to form the complex compound. The mixed metal source solution, ammonia water, and sodium hydroxide were then each added to the reactor. Sodium hydroxide was added to maintain the pH inside the reactor. The reaction was then carried out for approximately 95 hours with stirring, after which the addition of the raw solution was discontinued.

[0120] The slurry solution in the reactor was filtered, washed with high-purity distilled water, and then dried in a hot air oven at 200°C for 24 hours to obtain large-sized nickel-based metal hydroxide (Ni) with a particle size (D50) of approximately 12 μm. 0.94 Co 0.03 Al 0.03 (OH)2) powder was obtained.

[0121] Production Example 2: Production of small nickel-based metal hydroxide Small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05The same process as in Preparation Example 1 was carried out, except that the contents of nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and aluminum sulfate (Al2(SO4)3·H2O) were stoichiometrically controlled to obtain small nickel-based metal hydroxide (Ni(OH)2) of about 3 μm in size, the precursor drying process was changed from 24 hours in a hot air oven at 200°C to 24 hours in a hot air oven at 210°C, and the reaction time was changed to 25 hours. 0.8 Co 0.15 Al 0.05 (OH)2) powder was obtained.

[0122] Production Example 3: Production of large nickel-based metal hydroxide particles As large-grain nickel-based metal hydroxide, Ni 0.96 Co 0.02 Al 0.02 The same process as in Preparation Example 1 was carried out to obtain large particles of nickel-based metal hydroxide (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and aluminum sulfate (Al2(SO4)3·H2O), with the exception that the contents were stoichiometrically controlled to obtain nickel (OH)2. 0.96 Co 0.02 Al 0.02 (OH)2) powder was obtained.

[0123] Production Example 4: Production of large nickel-based metal hydroxide particles Large nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 Instead of (OH)2, large particles of nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 The same procedure as in Preparation Example 1 was followed, except that sodium hydroxide was added to maintain the pH inside the reactor so as to obtain (OH)2), and the reaction time was changed to about 90 hours while stirring.

[0124] Production Example 5: Production of large nickel-based metal hydroxide particles Large nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 Instead of (OH)2, large particles of nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 The same procedure as in Preparation Example 1 was followed, except that sodium hydroxide was added to maintain the pH inside the reactor so as to obtain (OH)2), and the reaction time was changed to about 130 hours while stirring.

[0125] Production Example 6: Production of small nickel-based metal hydroxide Small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 Instead of (OH)2, small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 The same procedure as in Preparation Example 2 was followed, except that sodium hydroxide was added to maintain the pH inside the reactor so as to obtain (OH)2), and the reaction time was changed to about 22 hours while stirring.

[0126] Production Example 7: Production of small nickel-based metal hydroxide Small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 Instead of (OH)2, small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 The same procedure as in Preparation Example 2 was followed, except that sodium hydroxide was added to maintain the pH inside the reactor so as to obtain (OH)2), and the reaction time was changed to about 28 hours while stirring.

[0127] (Production of nickel-based lithium metal composite oxide)

[0128] Example 1 The large nickel-based metal hydroxide particles having a size of 12 μm obtained in Production Example 1 and the small nickel-based metal hydroxide particles having a size of 3 μm obtained in Production Example 2 were mixed in a mixing weight ratio of 80:20.

[0129] The large-particle nickel-based metal hydroxide, the small-particle nickel-based metal hydroxide mixture, and lithium hydroxide (LiOH) were mixed in a dry state at a ratio of 1:1.05 using a Henschel mixer, and then heat-treated in an oxygen atmosphere at approximately 720°C for 10 hours to produce a nickel-based lithium metal composite oxide Li containing large secondary particles and small secondary particles. 1.05 Ni 0.92 Co 0.05 Al 0.03 The average particle size (D50) of the large secondary particles was 12 μm, the average particle size (D50) of the small secondary particles was 3 μm, the mixing weight ratio of the large secondary particles to the small secondary particles was 80:20, and the difference in nickel content between the large and small secondary particles was 14 mol%.

[0130] Example 2 The same procedure as in Example 1 was carried out, except that the mixing weight ratio of the large nickel-based metal hydroxide particles measuring 12 μm obtained in Preparation Example 1 to the small nickel-based metal hydroxide particles measuring 3 μm obtained in Preparation Example 2 was changed to a 90:10 weight ratio, and heat treatment was carried out in an oxygen atmosphere at about 720°C for 10 hours, to obtain a nickel-based lithium metal composite oxide containing large and small secondary particles as shown in Table 1 below. The large secondary particles had an average particle size (D50) of 12 μm, the small secondary particles had an average particle size (D50) of 3 μm, the mixing weight ratio of the large secondary particles to the small secondary particles was 90:10, and the difference in nickel content between the large and small secondary particles was 14 mol%.

[0131] [Table 1]

[0132] Examples 3 to 6 As shown in Table 2 below, the nickel-based lithium metal composite oxide was obtained in the same manner as in Example 1, except that the heat treatment temperature of the nickel-based metal hydroxide was changed.

[0133] [Table 2]

[0134] Example 7 Instead of the large nickel-based metal hydroxide particles having a size of 12 μm obtained in Production Example 1, the nickel-based metal hydroxide particles (Ni 0.96 Co 0.02 Al 0.02 The same procedure as in Example 1 was carried out except that (OH)2) was used, and a nickel-based lithium metal composite oxide satisfying the conditions in Table 3 below was obtained.

[0135] [Table 3]

[0136] Example 8 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Preparation Example 4 and the small-particle nickel-based metal hydroxide of Preparation Example 2 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0137] Example 9 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Preparation Example 5 and the small-particle nickel-based metal hydroxide of Preparation Example 2 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0138] Example 10 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Preparation Example 1 and the small-particle nickel-based metal hydroxide of Preparation Example 6 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0139] Example 11 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Production Example 1 and the small-particle nickel-based metal hydroxide of Production Example 7 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0140] [Table 4]

[0141] Comparative Example 1 The large-particle nickel-based metal hydroxide obtained in Production Example 1 was Ni 0.94 Co 0.03 Al 0.03 (OH)2 was used to prepare small nickel-based metal hydroxide particles, such as Ni 0.96 Co 0.02 Al 0.02 The same procedure as in Example 1 was carried out except that (OH)2 was used to obtain a nickel-based lithium metal composite oxide.

[0142] Comparative Example 2 The large-particle nickel-based metal hydroxide obtained in Production Example 1 and lithium hydroxide (LiOH) were dry mixed in a molar ratio of 1:1.05 using a Henschel mixer, and the mixture was subjected to a primary heat treatment in an oxygen atmosphere at approximately 740°C for 10 hours to obtain large secondary particles of a nickel-based lithium metal composite oxide. The average particle size (D50) of the large secondary particles was 12 μm.

[0143] Separately, the 3 μm small-particle nickel-based metal hydroxide obtained in Preparation Example 2 and lithium hydroxide (LiOH) were dry mixed in a 1:1.01 molar ratio using a Henschel mixer, and subjected to a secondary heat treatment in an oxygen atmosphere at approximately 680°C for 10 hours to obtain small secondary particles of a nickel-based lithium metal composite oxide. The small secondary particles had an average particle size (D50) of 3 μm.

[0144] The large secondary particles and the small secondary particles were mixed in a weight ratio of 80:20, and then subjected to a tertiary heat treatment at approximately 700°C to obtain a nickel-based lithium metal composite oxide containing large secondary particles and small secondary particles.

[0145] According to Comparative Example 2, three heat treatment steps must be performed to obtain NCA, which increases the manufacturing cost and time, making it difficult to practically apply this method.

[0146] (Lithium secondary battery manufacturing)

[0147] Example 1 The nickel-based lithium metal composite oxide secondary particles obtained in Example 1 were used as the positive electrode active material, and a lithium secondary battery was produced as follows.

[0148] A mixture of 96 g of the nickel-based lithium metal composite oxide secondary particles obtained in Example 1, 2 g of polyvinylidene fluoride, 47 g of N-methylpyrrolidone as a solvent, and 2 g of carbon black as a conductive agent was mixed in a mixer to remove air bubbles, thereby producing a uniformly dispersed slurry for forming a positive electrode active material layer.

[0149] The slurry prepared by the above process was coated on an aluminum foil using a doctor blade to form a thin electrode plate, which was then dried at 135°C for 3 hours or more, rolled, and vacuum dried to prepare a cathode.

[0150] A 2032-type coin cell was fabricated using the above-mentioned positive electrode and a lithium metal counter electrode as the opposite electrode. A separator (thickness: approximately 16 μm) made of a porous polyethylene (PE) film was placed between the above-mentioned positive electrode and the above-mentioned lithium metal counter electrode, and an electrolyte was injected to fabricate a 2032-type coin cell. The electrolyte used was a solution containing 1.1 M LiPF6 dissolved in a solvent made by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:5.

[0151] The formation process for the coin cell fabricated by the above process was carried out as follows.

[0152] The first charge / discharge cycle consisted of a 10-hour rest period followed by a constant current charge at 0.2C until the voltage reached 4.25V, followed by a constant voltage charge at 0.05C until the voltage reached 3V. After a 10-minute rest period, the coin cell was discharged at a constant current of 0.2C until the voltage reached 3V (first cycle). After a further 10-minute rest period, the second charge / discharge cycle consisted of a constant current charge at 0.2C until the voltage reached 4.25V, followed by a constant voltage charge at 0.05C until the voltage reached 3V. After a 10-minute rest period, the coin cell was discharged at a constant current of 0.2C until the voltage reached 3V (second cycle).

[0153] Examples 2 to 11 A lithium secondary battery was fabricated in the same manner as in Preparation Example 1, except that the nickel-based lithium metal composite oxides prepared in Examples 2 to 11 were used instead of the nickel-based lithium metal composite oxide prepared in Example 1.

[0154] Comparative production examples 1 and 2 Lithium secondary batteries were fabricated in the same manner as in Preparation Example 1, except that the nickel-based lithium metal composite oxides prepared in Comparative Preparation Examples 1 and 2 were used instead of the nickel-based lithium metal composite oxide prepared in Example 1.

[0155] Evaluation example 1: dQ / dV analysis The coin cells produced in Production Example 1 and Comparative Production Examples 1 and 2 were evaluated for charge / discharge characteristics using a charger / discharger (manufacturer: TOYO, model: TOYO-3100).

[0156] The charge / discharge characteristic evaluation process will be described in more detail below.

[0157] The cells were charged at a constant current of 1 C until the voltage reached 4.3 V, and then charged at a constant voltage of 0.05 C until the voltage reached 3 V. After the charging was complete, the cells were allowed to rest for approximately 10 minutes, and then discharged at a constant current of 1 C until the voltage reached 3 V (first cycle). This charge-discharge cycle was repeated 50 times in total.

[0158] After the first cycle, 30 cycles, and 50 cycles, the ratios (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) were measured for the dQ / dV charge / discharge differential curve distributions shown in the voltage range of 4.1 V to 4.25 V. The results are shown in Table 5 below and Figures 1 to 5.

[0159] The charging peak is the peak shown between 4.17V and 4.25V, and the discharging peak is the peak shown between 4.14V and 4.17V.

[0160] FIG. 1 shows the dQ / dV charge-discharge differential curves after the first cycle for the lithium batteries of Preparation Example 1 and Comparative Preparation Examples 1 and 2, and FIG. 2 shows the dQ / dV charge-discharge differential curves after 30 cycles for the lithium batteries of Preparation Example 1 and Comparative Preparation Example 2.

[0161] Figure 3 shows the dQ / dV charge / discharge differential curves after 50 cycles for the lithium batteries of Preparation Example 1 and Comparative Preparation Example 2, Figure 4 shows the dQ / dV charge / discharge differential curves after the first cycle, after 30 cycles, and after 50 cycles for the lithium battery of Preparation Example 1, and Figure 5 shows the dQ / dV charge / discharge differential curves after the first cycle, after 30 cycles, and after 50 cycles for the lithium battery of Comparative Preparation Example 2.

[0162] [Table 5]

[0163] 1 to 5 and Table 5, the lithium secondary battery of Preparation Example 1 exhibited an A2 / A1 ratio of 1.1 or greater after the first cycle, 30 cycles, and 50 cycles, while the lithium batteries of Comparative Preparation Examples 1 and 2 exhibited an A2 / A1 ratio of less than 1.0 after the first cycle, 30 cycles, and 50 cycles. Furthermore, the lithium battery of Preparation Example 1 exhibited a reduced A2 / A1 change rate compared to Comparative Preparation Examples 1 and 2. The A2 / A1 change rate represents the ratio of A2 / A1 after 50 cycles to A2 / A1 after one cycle. The reduced A2 / A1 change rate indicates that the lithium battery of Preparation Example 1 experienced less structural change due to degradation after charge / discharge cycling.

[0164] Evaluation example 2: X-ray diffraction analysis X-ray diffraction analysis was performed on the nickel-based lithium metal composite oxide of Example 1 using X'pert pro (PANalytical) utilizing Cu Kα radiation (1.54056 Å). The results of the X-ray diffraction analysis are shown in FIG.

[0165] Referring to FIG. 6, it was found that the nickel-based lithium metal composite oxide of Example 1 was free of impurities and formed an ordered layer structure.

[0166] Evaluation example 3: Charge / discharge efficiency and capacity retention rate The charge / discharge efficiency and capacity retention rate of the coin cells fabricated in Preparation Examples 1 to 6 and Comparative Preparation Example 1 were evaluated using a charger / discharger (manufacturer: TOYO, model: TOYO-3100) as follows.

[0167] (1) Charging and discharging efficiency Each coin cell was charged at a constant current of 0.2 C at 25°C until it reached 4.25 V, and then charged at a constant voltage of 0.05 C. After charging, the cells were rested for approximately 10 minutes, and then discharged at a constant current of 0.2 C until the voltage reached 3 V. This cycle was repeated 50 times for evaluation.

[0168] (2) Capacity retention rate (CRR) Each coin cell was charged at a constant current of 1 C at 45°C until it reached 4.3 V, and then charged at a constant voltage of 0.05 C. After the charging was completed, the cell was rested for about 10 minutes, and then discharged at a constant current of 1 C until the voltage reached 3 V. This cycle was repeated 50 times and evaluated.

[0169] The capacity retention ratio (CRR) was calculated using the following Equation 1, and the initial charge-discharge efficiency was calculated using the following Equation 2. Some of the capacity retention ratio and initial charge-discharge efficiency characteristics were investigated and are shown in Table 6 and Figure 8. Figure 8 shows the capacity retention ratio characteristics of Preparation Examples 1 and 2 and Comparative Preparation Example 1.

[0170]

number

[0171]

number

[0172] [Table 6]

[0173] 8, it can be seen that the coin cells manufactured according to Manufacturing Examples 1 to 6 have improved capacity retention characteristics compared to Comparative Manufacturing Example 1. In addition, the coin cells of Manufacturing Examples 1 to 6 exhibit improved initial charge-discharge efficiency characteristics compared to Comparative Manufacturing Example 1.

[0174] The coin cell of Comparative Example 2 exhibited excellent capacity retention characteristics. However, the positive electrode of the coin cell of Comparative Example 2 used the nickel-based lithium metal composite oxide of Comparative Example 2, which was obtained by firing large particles and small particles separately and then firing three times. The nickel-based lithium metal composite oxide of Comparative Example 2 must undergo three heat treatment processes, which increases manufacturing costs and time, making this method difficult to apply in practice.

[0175] The charge-discharge characteristics of the coin cells of Production Examples 7 to 11 were evaluated in the same manner as in the coin cell of Production Example 1 described above.

[0176] As a result of the evaluation, the charge-discharge characteristics of the coin cells of Preparation Examples 7 to 11 were at a similar level to the charge-discharge characteristics of the coin cell of Preparation Example 1 described above.

[0177] Evaluation example 4: Charge / discharge characteristics The coin cells manufactured in Preparation Example 1 and Comparative Preparation Example 1 were evaluated for charge / discharge characteristics under the following conditions.

[0178] To measure the charge-discharge characteristics, each coin cell was charged at a constant current of 0.2 C at 25°C until the voltage reached 4.25 V, and then charged at a constant voltage of 0.05 C. After charging, the cells were allowed to rest for approximately 10 minutes, and then cycled to discharge at a constant current of 0.2 C until the voltage reached 3 V.

[0179] The results of the above evaluation are shown in FIG.

[0180] As shown in FIG. 9, the coin cell of Preparation Example 1 had improved charge-discharge characteristics compared to the coin cell of Comparative Example 1.

[0181] Although one embodiment has been described above with reference to the drawings and examples, it is understood that the same is for illustrative purposes only, and that various modifications and equivalent embodiments are possible. Therefore, the scope of protection of the present invention is defined by the following claims. [Explanation of symbols]

[0182] 21 Lithium secondary battery 22 Negative electrode 23 Positive electrode 24 Separator 25 Battery case 26 Cap Assembly

Claims

1. A nickel-based lithium metal composite oxide comprising secondary particles including aggregates of primary particles, the nickel content being 50 mol % or more based on the total transition metal content in the nickel-based lithium metal composite oxide, The secondary particles include large secondary particles having an average particle size (D50) of 10 μm or more and small secondary particles having an average particle size (D50) of 5 μm or less, A nickel-based lithium metal composite oxide, wherein the large secondary particles have a higher nickel content than the small secondary particles, The large secondary particles are a compound represented by the following chemical formula 1-1, and the small secondary particles are a compound represented by the following chemical formula 1-2, A nickel-based lithium metal composite oxide, in which the BET specific surface area of ​​the small secondary particles measured by a BET method is at least twice as large as the BET specific surface area of ​​the large secondary particles: 【Chemistry 1-1】 In the formula 1-1, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; 0.95≦a≦1.3, 0.88≦1−x−y−z≦0.96, 0.01≦x≦0.08, 0.001≦y≦0.05, and 0≦z≦0.01, 【Chemistry 1-2】 In the formula 1-2, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; 0.95≦a≦1.3, 0.75≦1-x-y-z≦0.85, 0.01≦x≦0.05, 0.001≦y≦0.05, and 0≦z≦0.

01.

2. The nickel-based lithium metal composite oxide described in claim 1, wherein the charge peak is a peak indicated at 4.17 V to 4.25 V, and the discharge peak is a peak indicated at 4.14 V to 4.17 V.

3. The nickel-based lithium metal composite oxide of claim 1, wherein the ratio (A2 / A1) of the discharge peak intensity (A2) to the dQ / dV charge peak intensity (A1) is 1.1 to 1.

5.

4. A nickel-based lithium metal composite oxide as described in claim 1, wherein the difference in nickel content between the large secondary particles and the small secondary particles is 10 mol % or more.

5. The nickel-based lithium metal composite oxide of claim 1, wherein the nickel content in the large secondary particles is 85 to 99 mol % based on the total content of transition metals.

6. A nickel-based lithium metal composite oxide as described in claim 1, wherein the nickel content in the small secondary particles is 75 to 89 mol % based on the total transition metal content of the small secondary particles.

7. The nickel-based lithium metal composite oxide as described in claim 1, wherein the average particle size (D50) of the large secondary particles is 10 μm to 17 μm.

8. The nickel-based lithium metal composite oxide described in claim 1, wherein the small secondary particles have an average particle size (D50) of 2 μm to 5 μm.

9. A nickel-based lithium metal composite oxide as described in claim 1, wherein the content of the large secondary particles is 30 to 90 parts by weight based on 100 parts by weight of the total content of the large secondary particles and the small secondary particles.

10. A method for producing a lithium precursor comprising the steps of: mixing a large-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more based on the total transition metal content in a large-particle nickel-based metal hydroxide; mixing a small-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more based on the total transition metal content in a small-particle nickel-based metal hydroxide; and obtaining a precursor mixture and carrying out a heat treatment; A method for producing a nickel-based lithium metal composite oxide, comprising the step of obtaining the nickel-based lithium metal composite oxide according to any one of claims 1 to 9.

11. The method for producing a nickel-based lithium metal composite oxide as described in claim 10, wherein the heat treatment is at 650°C to 800°C.

12. A method for producing a nickel-based lithium metal composite oxide as described in claim 10, wherein the large-particle nickel-based metal hydroxide has a higher nickel content than the small-particle nickel-based metal hydroxide, and the difference in nickel content is 10 mol % or more.

13. The large-grain nickel-based metal hydroxide has a nickel content of 85 to 99 mol % based on the total transition metal content of the large-grain nickel-based metal hydroxide; 11. The method for producing a nickel-based lithium metal composite oxide according to claim 10, wherein the nickel content of the small nickel-based metal hydroxide is 75 to 89 mol% based on the total transition metal content of the small nickel-based metal hydroxide.

14. The method for producing a nickel-based lithium metal composite oxide as described in claim 10, wherein the lithium precursor is lithium hydroxide, lithium fluoride, lithium carbonate, or a mixture thereof.

15. A lithium secondary battery comprising a positive electrode, a negative electrode, and an electrolyte interposed between the positive electrode and the negative electrode, the positive electrode containing the nickel-based lithium metal composite oxide according to any one of claims 1 to 9.