Lithium niobate solution and method for producing the same
Patent Information
- Application Number
- JP2023128828
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-04-28
- Filing Date
- 2023-08-07
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2042-03-10
AI Technical Summary
Existing lithium niobate precursor solutions face issues with stability due to hydrogen peroxide concentration, leading to decomposition and solubilized niobium acid formation, affecting dispersibility and solubility in water.
A lithium niobate solution with a lithium to niobium molar ratio of 0.8 to 2.0, containing ammonium ions and without hydrogen peroxide, with particle diameter less than 100 nm, ensuring high dispersibility and solubility in water, and improved storage stability.
The solution achieves stable lithium niobate dispersions with excellent long-term storage and film-forming capabilities, suitable for coating positive electrodes in lithium ion secondary batteries.
Abstract
Description
[Technical Field]
[0001] The present invention relates to a lithium niobate solution and a method for producing the same. [Background technology]
[0002] Lithium niobate is used as a nonlinear optical material in its single crystal form, and a technology for reducing the interfacial resistance occurring between the positive electrode and electrolyte of a lithium ion secondary battery by coating the surface of positive electrode active material particles of the lithium ion secondary battery with a solution of the lithium niobate is disclosed in Patent Document 1. Hydrogen peroxide water is added to the lithium niobate precursor aqueous solution disclosed in Patent Document 1 in order to improve storage stability. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 2020-66570 Summary of the Invention [Problem to be solved by the invention]
[0004] However, Patent Document 1 discloses the following points to be noted regarding lithium niobate precursor aqueous solutions to which hydrogen peroxide has been added: if the concentration of hydrogen peroxide is less than 0.1 mol per 1 mol of niobium, the generated niobium polyacid will react with hydroxide ions and decompose; if the amount of free hydrogen peroxide in the lithium niobate precursor aqueous solution is less than 0.01 mass %, it is difficult to maintain the stability of the precursor aqueous solution; and further, the presence of hydrogen peroxide in the lithium niobate precursor aqueous solution may cause a portion of the solubilized niobic acid to form an unstable peroxo complex.
[0005] In view of the above problems, the present invention provides a lithium niobate solution that has high dispersibility in water, good solubility in water, and excellent storage stability, and a method for producing the same. [Means for solving the problem]
[0006] The lithium niobate solution of the present invention, which has been made to solve the above-mentioned problems, is a lithium niobate solution containing lithium niobate having a lithium to niobium molar ratio Li / Nb of 0.8 or more and 2.0 or less, and ammonium ions, and is characterized in that the lithium niobate particle diameter (D50) in the lithium niobate solution, as measured by a dynamic light scattering method, is 100 nm or less. In the lithium niobate solution of the present invention, when the lithium niobate (LiNbO3) in the lithium niobate solution has a molar ratio of lithium to niobium (Li / Nb) of 0.8 or more and 2.0 or less, the formation of precipitates from the solution can be suppressed, and the stability of the solution can be improved. Furthermore, the molar ratio of lithium to niobium (Li / Nb) in the lithium niobate solution is more preferably 0.9 or more and 1.5 or less, and even more preferably 0.9 or more and 1.2 or less.
[0007] Here, it is assumed that the lithium niobate in the lithium niobate solution of the present invention exists in the solution as ions in a state in which niobic acid and lithium are ionic bonded. In the lithium niobate solution of the present invention, hydroxide ions exist as anions, while halide ions such as fluoride ions and chloride ions are hardly present, and lithium is thought to exist as a cation. Therefore, niobium is NbO3 - It is thought that these ions exist as anions such as these, or as polyoxometalate (polyacid) ions in which multiple niobium atoms are bonded to oxygen atoms.
[0008] Furthermore, the lithium niobate solution of the present invention contains ammonium ions in addition to lithium niobate. As will be described in detail in the method for producing a lithium niobate solution of the present invention below, in the production process, a hydrous ammonium niobate cake, which is a precipitate slurry containing niobium, is produced by a reverse neutralization method in which an acidic niobium solution is added to ammonia water, and then the lithium niobate solution of the present invention is produced. Therefore, it is believed that ammonium ions substituted for lithium ions are present as cations in the solution.
[0009] Methods for measuring the ammonium ion concentration in the solution include adding sodium hydroxide to the solution to separate the ammonia by distillation and quantifying the ammonium ion concentration using an ion meter, quantifying the N2 content in a gasified sample using a thermal conductivity meter, the Kjeldahl method, gas chromatography (GC), ion chromatography, and GC-MS (mass spectrometry).
[0010] The ammonium ion concentration of the ammonium ions contained in the lithium niobate solution of the present invention is preferably 0.001% by mass or more and 25% by mass or less, more preferably 0.5% by mass or more and 10% by mass or less, and even more preferably 1% by mass or more and 8% by mass or less.
[0011] Furthermore, a lithium niobate particle diameter (D50) of 100 nm or less in the lithium niobate solution measured by dynamic light scattering is preferred in terms of high dispersibility. Smaller lithium niobate particle diameters (D50) in the lithium niobate solution are more stable due to less change over time, and are also preferred in terms of forming a good coating film with no uncoated areas during film formation and ensuring a sufficient coating weight. The lithium niobate particle diameter (D50) in the lithium niobate solution is more preferably 80 nm or less, even more preferably 50 nm or less, particularly preferably 30 nm or less, even more particularly preferably 20 nm or less, even more particularly preferably 10 nm or less, still more particularly preferably 5 nm or less, and even more particularly preferably 3 nm or less. Thus, a solution in which the lithium niobate particle diameter (D50) in the lithium niobate solution of the present invention, as measured by dynamic light scattering, has a lithium niobate particle diameter (D50) of 100 nm or less is defined as the "lithium niobate solution" of the present invention.
[0012] Dynamic light scattering is a method for measuring the light scattering intensity from particles undergoing Brownian motion by irradiating a solution, such as a suspension, with light such as a laser beam. The particle size and distribution are then determined from the temporal fluctuations of this intensity. Specifically, particle size distribution is evaluated using a zeta potential, particle size, and molecular weight measurement system (Otsuka Electronics Co., Ltd.: ELSZ-2000) in accordance with JIS Z 8828:2019 "Particle Size Analysis - Dynamic Light Scattering." Just before measurement, the solution is filtered through a 2 μm pore size filter and ultrasonicated for 3 minutes at 28 kHz in an ultrasonic cleaner (AS ONE Corporation: VS-100III) to remove dust and other particles. The particle size (D50) refers to the median diameter (D50), which is the particle size at 50% of the cumulative distribution curve.
[0013] In the present invention, the term "solution" is not limited to a solute dispersed or mixed in a solvent in the form of a single molecule, but also includes aggregates in which multiple molecules are attracted to each other by intermolecular interactions, such as (1) polymeric molecules, (2) solvated molecules, (3) molecular clusters, and (4) colloidal particles dispersed in a solvent.
[0014] Furthermore, the lithium niobate solution of the present invention preferably does not contain hydrogen peroxide. Generally, when niobium oxide is present in a solution as a polyacid ion, hydrogen peroxide is added to prevent decomposition due to reaction with hydroxide ions, thereby improving stability. However, the lithium niobate solution of the present invention can ensure long-term stability even in the absence of hydrogen peroxide due to the presence of ammonium ions in the solution.
[0015] A method for detecting hydrogen peroxide in a solution can be, for example, using the standard addition method, by measuring the relative absorbance intensity with respect to a standard solution of hydrogen peroxide, thereby confirming the absence of hydrogen peroxide in the solution. Specifically, the wavelength region in which a change in absorbance associated with peroxo complex formation is observed is identified from the UV-visible absorption spectra of a standard solution containing a known concentration of hydrogen peroxide, e.g., 1% by mass, and a standard solution containing no added hydrogen peroxide. If the difference in absorbance between the standard solution containing no added hydrogen peroxide and a sample with an unknown hydrogen peroxide concentration in that wavelength region is less than 1%, it can be confirmed that the sample with an unknown hydrogen peroxide concentration is substantially free of hydrogen peroxide. If hydrogen peroxide is present in the solution, it reacts with niobium polyacid to form a peroxo complex. Therefore, the absence of hydrogen peroxide in the solution can be confirmed by checking the difference in absorbance with the standard solution containing no added hydrogen peroxide, as described above. In addition to the above-mentioned standard addition method, hydrogen peroxide in a solution may be qualitatively and quantitatively analyzed by, for example, using a commercially available hydrogen peroxide measurement kit, adding a reagent that undergoes a color reaction with hydrogen peroxide to the solution and measuring the color development, or by adding a reagent that undergoes a fluorescent reaction with hydrogen peroxide to the solution and measuring the light emission.
[0016] In addition, the lithium niobate solution of the present invention is preferably an aqueous solution. The lithium niobate in the lithium niobate solution of the present invention has high dispersibility in water and good solubility in water, so pure water can be used as the solvent.
[0017] The lithium niobate solution of the present invention is characterized in that the lithium niobate concentration in the lithium niobate solution is 0.1 to 30 mass %. Furthermore, the lithium niobate solution of the present invention is characterized in that the lithium niobate concentration in the lithium niobate solution is 5 to 20 mass %. The lithium niobate concentration in the lithium niobate solution is preferably 0.1 to 30 mass % in terms of achieving both practicality and stability of the lithium niobate solution, more preferably 1 to 25 mass %, even more preferably 3 to 21 mass %, and particularly preferably 5 to 20 mass %.
[0018] Here, the lithium niobate concentration in the lithium niobate solution is calculated by diluting the solution appropriately with dilute hydrochloric acid as needed, and measuring the Nb weight fraction and Li weight fraction in terms of niobium oxide (Nb2O5) using an ICP atomic emission spectrometry (AG-5110 manufactured by Agilent Technologies) in accordance with JIS K0116:2014. Note that the niobic acid in the lithium niobate solution of the present invention is not necessarily present in the form of Nb2O5. The content of niobic acid is expressed in terms of Nb2O5 because of the convention used when expressing niobium concentration.
[0019] The lithium niobate solution of the present invention can also be used for coating a positive electrode or positive electrode material for a lithium ion secondary battery, or for coating a positive electrode or positive electrode material for an all-solid-state lithium ion battery. The lithium niobate solution of the present invention is suitable for coating positive electrodes or positive electrode materials for lithium ion secondary batteries. These results show that the lithium niobate solution of the present invention is suitable for coating positive electrodes or positive electrode materials for lithium ion secondary batteries. These results include a stability test in which the state of the solution is visually observed after being left to stand for one month in an incubator set at room temperature (25°C), and a dynamic light scattering method in which the particle diameter (D50) of the lithium niobate particles in the solution over time is measured. In addition, a film-formability test in which the solution is applied to a glass substrate used as a substitute for a current collector plate for a positive electrode of a lithium ion secondary battery and the state of the coating film is observed under an optical microscope, and a safety test in which the solution is mixed with a positive electrode active material and the presence or absence of foaming is visually confirmed.
[0020] The positive electrode active material for a lithium ion secondary battery of the present invention is characterized in that its surface is coated with lithium niobate contained in the lithium niobate solution. By observing the coating state of the particle surface of the lithium niobate solution of the present invention using a scanning electron microscope, it is possible to confirm that the surface of the positive electrode active material for a lithium ion secondary battery is coated with lithium niobate. Furthermore, the amount of lithium niobate coating the surface of the positive electrode active material for a lithium ion secondary battery of the present invention can be calculated by dissolving the positive electrode active material for a lithium ion secondary battery in an appropriate amount of hydrofluoric acid and measuring the niobium weight fraction concentration of the lithium niobate coating the particle surface of the positive electrode active material using an ICP atomic emission spectrometry (Agilent Technologies: AG-5110) in accordance with JIS K0116:2014. The niobium weight fraction concentration is preferably 1 or greater, more preferably greater than 1, even more preferably 1.1 or greater, and particularly preferably 1.2 or greater.
[0021] Furthermore, the lithium niobate solution of the present invention may contain components other than those derived from lithium niobate and those derived from ammonia (referred to as "other components") to the extent that the effects of the solution are not impaired. Examples of other components include Na, Mg, Si, K, Ca, Ti, Mn, Ni, Zn, Sr, Zr, Ta, Mo, Ba, and W. However, the other components are not limited to these. The content of other components in the lithium niobate solution of the present invention is preferably less than 5% by mass, more preferably less than 4% by mass, and even more preferably less than 3% by mass. It is anticipated that the lithium niobate solution of the present invention may contain unintended, unavoidable impurities. The content of unavoidable impurities is preferably less than 0.01% by mass.
[0022] The lithium ion secondary battery of the present invention is characterized by having a positive electrode coated with the positive electrode active material. As described above, the positive electrode active material coated with the lithium niobate solution of the present invention is suitable for coating the surface of a positive electrode for a lithium ion secondary battery. Therefore, by coating the surface of a positive electrode with the positive electrode active material coated with the lithium niobate solution of the present invention, the performance of the lithium ion secondary battery can be improved.
[0023] The method for producing the lithium niobate solution of the present invention described above will be described below.
[0024] The method for producing a lithium niobate solution of the present invention includes the steps of: producing an acidic niobium solution containing niobium; obtaining a precipitate slurry containing niobium by a reverse neutralization method in which the acidic niobium solution is added to ammonia water; and mixing the obtained precipitate slurry containing niobium with lithium hydroxide and pure water, and maintaining the mixture at 20°C to 100°C while stirring, to obtain a lithium niobate solution.
[0025] First, in the step of producing an acidic niobium solution containing niobium, the acidic niobium solution refers to an acidic niobium solution containing fluoride ions obtained by solvent extraction of a solution in which niobium is dissolved in an acidic solution containing hydrofluoric acid. Note that, unless otherwise specified, niobium referred to in this specification includes niobate compounds.
[0026] Here, an acidic niobium solution containing fluoride ions, such as a niobium fluoride aqueous solution, is preferably adjusted to contain 1 to 100 g / L of niobium in terms of Nb2O5 by adding water (e.g., pure water). In this case, a niobium concentration of 1 g / L or more in terms of Nb2O5 is preferred because it results in a water-soluble niobic acid compound hydrate. From the viewpoint of productivity, 10 g / L or more is more preferred, and 20 g / L or more is even more preferred. On the other hand, a niobium concentration of 100 g / L or less in terms of Nb2O5 is preferred because it results in a water-soluble niobic acid compound hydrate. To more reliably synthesize a water-soluble niobic acid compound hydrate, a concentration of 90 g / L or less is more preferred, 80 g / L or less is even more preferred, and 70 g / L or less is particularly preferred. The pH of the niobium fluoride aqueous solution is preferably 2 or less, more preferably 1 or less, from the viewpoint of completely dissolving niobium or niobium oxide.
[0027] Next, in the step of obtaining a precipitation slurry containing niobium by a reverse neutralization method in which the acidic niobium solution is added to ammonia water (hereinafter referred to as a reverse neutralization step), it is preferable to add the acidic niobium solution containing fluoride ions to ammonia water of a predetermined concentration, i.e., to obtain a precipitation slurry containing niobium by the reverse neutralization method.
[0028] The ammonia concentration of the ammonia water used for reverse neutralization is preferably 10% by mass to 30% by mass. When the ammonia concentration is 10% by mass, niobium is less likely to remain undissolved, and niobium or niobic acid can be completely dissolved in water. On the other hand, when the ammonia concentration is 30% by mass or less, it is preferably close to a saturated aqueous solution of ammonia.
[0029] From this viewpoint, the ammonia concentration of the ammonia water is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass, while the ammonia concentration is preferably 30% by mass or less, more preferably 29% by mass or less, and even more preferably 28% by mass or less.
[0030] In the reverse neutralization step, the amount of niobium fluoride aqueous solution added to ammonia water is preferably such that the NH3 / Nb2O5 molar ratio is 95 or more and 500 or less, more preferably 100 or more and 450 or less, and even more preferably 110 or more and 400 or less. Furthermore, from the viewpoint of producing amines or niobic acid compounds that are soluble in diluted ammonia water, the amount of niobium fluoride aqueous solution added to ammonia water is preferably such that the NH3 / HF molar ratio is 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. On the other hand, from the viewpoint of cost reduction, the NH3 / HF molar ratio is preferably 100 or less, more preferably 50 or more, and even more preferably 40 or more.
[0031] In the reverse neutralization step, the time required for adding the niobium fluoride aqueous solution to the ammonia water is preferably within 1 minute, more preferably within 30 seconds, and even more preferably within 10 seconds. That is, rather than gradually adding the niobium fluoride aqueous solution over time, it is preferable to add it to the ammonia water in as short a time as possible, for example, by adding it all at once, to allow the neutralization reaction to occur. In addition, in the reverse neutralization step, the acidic niobium fluoride aqueous solution is added to the alkaline ammonia water, so the neutralization reaction can be carried out while maintaining a high pH. The niobium fluoride aqueous solution and the ammonia water can be used at room temperature.
[0032] The method for producing a lithium niobate solution of the present invention also includes a step of removing fluoride ions from a niobium-containing precipitate slurry obtained by the reverse neutralization method to obtain a niobium-containing precipitate from which fluoride ions have been removed. Since the niobium-containing precipitate slurry obtained by the reverse neutralization method contains fluorine compounds such as ammonium fluoride as impurities, it is preferable to remove these.
[0033] Any method for removing fluorine compounds can be used, and examples of such methods include reverse osmosis filtration using aqueous ammonia or pure water, filtration using a membrane such as ultrafiltration or microfiltration, centrifugation, and other known methods. When removing fluoride ions from a niobium-containing precipitate slurry, temperature control is not particularly required, and the removal may be carried out at room temperature.
[0034] Specifically, the niobium-containing precipitate slurry obtained by the reverse neutralization method is decanted using a centrifuge and washed repeatedly until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby obtaining a niobium-containing precipitate from which fluoride ions have been removed.
[0035] The cleaning solution used to remove fluoride ions is preferably ammonia water. Specifically, ammonia water of 5.0 mass % or less is preferred, ammonia water of 4.0 mass % or less is more preferred, ammonia water of 3.0 mass % or less is even more preferred, and ammonia water of 2.5 mass % is particularly preferred. When ammonia water of 5.0 mass % or less is used, ammonia and ammonium ions are suitable for fluorine, and unnecessary increases in costs can be avoided.
[0036] The niobium-containing precipitate thus obtained, from which fluoride ions have been removed, is diluted with pure water or the like to obtain a precipitate slurry containing niobium from which fluoride ions have been removed. The niobium concentration of the niobium-containing precipitate slurry is determined by taking a portion of the slurry, drying it at 110°C for 24 hours, and then calcining it at 1,000°C for 4 hours to produce NbO. The weight of the NbO thus produced can be measured, and the niobium concentration of the slurry can be calculated from the weight.
[0037] The niobium-containing precipitate slurry from which the fluoride ions have been removed is mixed with lithium hydroxide monohydrate, and the resulting mixture is stirred and maintained at 20°C to 100°C, thereby obtaining the lithium niobate solution of the present invention.
[0038] Specifically, the resulting niobium-containing precipitate slurry is mixed with lithium hydroxide monohydrate so that the final mixture has a lithium niobate concentration of 0.1 to 30 mass% in terms of NbO and a lithium to niobium molar ratio (Li / Nb) of 0.8 to 2.0, resulting in a translucent white slurry. The colorless and transparent lithium niobate solution of the present invention is obtained by stirring the translucent white slurry and maintaining the liquid temperature at 50 to 100°C (e.g., 70°C) for 1 to 24 hours. Alternatively, pure water or an alkaline aqueous solution, such as aqueous ammonia, may be added to the mixture of the niobium-containing precipitate slurry and lithium hydroxide monohydrate. The aqueous ammonia added to the mixture may have any ammonia concentration. For example, the ammonia concentration may be 0.1 to 30 mass%, or 10 to 25 mass%.
[0039] The resulting lithium niobate solution is then allowed to cool to room temperature. By drying the lithium niobate solution of the present invention, lithium niobate powder can be obtained.
[0040] The lithium niobate solution of the present invention obtained by the above-mentioned production method preferably has a pH of 9 or higher, since the lithium niobate solution is stable. Furthermore, the lithium niobate solution of the present invention more preferably has a pH of 10 or higher, even more preferably 10.5 or higher, and particularly preferably 11 or higher.
[0041] Furthermore, a method for producing the positive electrode active material for a lithium ion secondary battery coated with the lithium niobate solution of the present invention will be described below.
[0042] The method for producing a positive electrode active material for a lithium-ion secondary battery coated with a lithium niobate solution is characterized by comprising the steps of: mixing a lithium niobate solution, a positive electrode active material, and an aqueous lithium hydroxide solution to produce a slurry of the positive electrode active material for a battery containing lithium niobate; and drying the slurry of the positive electrode active material for a battery containing lithium niobate.
[0043] First, a battery positive electrode active material, for example, LiMn2O4 (manufactured by Merck: spinel type, particle size <0.5 μm) is added to an aqueous lithium niobate solution prepared by diluting the lithium niobate solution of the present invention with pure water, to obtain a slurry containing lithium niobate. Then, while stirring the slurry containing lithium niobate, an aqueous lithium hydroxide solution is added dropwise, and the mixture is maintained at 90°C for 10 minutes, to produce a battery positive electrode active material slurry containing lithium niobate.
[0044] In addition to the above-mentioned LiMn2O4, other positive electrode active materials for batteries include LiCoO2, LiNiO2, LiFeO2, Li2MnO3, LiFePO4, LiCoPO4, LiNiPO4, LiMnPO4, LiNi 0.5 Mn 1.5 O4, LiMn 1 / 3 Co 1 / 3 Ni 1 / 3 O2, LiCo 0.2 Ni 0.4 Mn 0.4 O2, lithium molybdate, LiMnO4, LiNi 0.8 Co 0.15 Al0.05 O2, LiMnO2 can be used.
[0045] Next, the battery positive electrode active material slurry containing lithium niobate is dried in an atmospheric drying furnace for 15 hours while the furnace temperature is maintained at 110°C, thereby producing a positive electrode active material for a lithium ion secondary battery coated with lithium niobate.
[0046] In the method for producing a positive electrode active material for a lithium ion secondary battery described above, the positive electrode active material for a battery is added, but this may be changed as appropriate depending on the application. For example, a dispersant, a pH adjuster, a colorant, a thickener, a wetting agent, a binder resin, etc. may be added. [Effects of the Invention]
[0047] The lithium niobate solution of the present invention has high dispersibility in water, good solubility in water, and excellent storage stability. BEST MODE FOR CARRYING OUT THE INVENTION
[0048] The lithium niobate solution according to the embodiment of the present invention will be further described below with reference to the following examples, although the present invention is not limited to these examples.
[0049] Example 1 100 g of niobium pentoxide was dissolved in 200 g of 55% aqueous hydrofluoric acid, and 830 mL of ion-exchanged water was added to obtain a niobium fluoride aqueous solution containing 100 g / L of niobium in terms of NbO (NbO = 8.84 mass%). 200 mL of this niobium fluoride aqueous solution was added to 1 L of ammonia water (NH concentration 25 mass%) over a period of less than 1 minute (NH / NbO molar ratio = 177.9, NH / HF molar ratio = 12.2) to obtain a reaction solution (pH 11). This reaction solution was a slurry of niobium acid compound hydrate, in other words, a slurry of niobium-containing precipitates.
[0050] The reaction solution was then decanted using a centrifuge and washed until the amount of liberated fluoride ions was 100 mg / L or less, to obtain a niobium-containing precipitate from which the fluoride ions had been removed. At this time, aqueous ammonia was used as the washing liquid.
[0051] The niobium-containing precipitate from which the fluoride ions had been removed was then diluted with pure water to obtain a slurry. A portion of this slurry was dried at 110°C for 24 hours and then calcined at 1,000°C for 4 hours to produce Nb2O5, and the Nb2O5 concentration in the slurry was calculated from its weight.
[0052] Then, the slurry of the niobium-containing precipitate diluted with pure water was mixed with lithium hydroxide monohydrate and pure water so that the niobium concentration in the final mixture was 1 mass % in terms of Nb2O5 and the Li / Nb molar ratio was 1, thereby obtaining a translucent slurry mixture. This mixture was stirred and held at a liquid temperature of 50°C to 100°C, for example 70°C, for 1 hour, and then a colorless and transparent lithium niobate aqueous solution according to Example 1 was obtained. The pH of the obtained lithium niobate aqueous solution according to Example 1 was 11.
[0053] Example 2 In Example 2, the same production method as in Example 1 was carried out, except that the niobium concentration of the translucent slurry mixture was 5 mass % in terms of NbO, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 2. The pH of the obtained lithium niobate aqueous solution according to Example 2 was 11.
[0054] Example 3 In Example 3, a similar production method to that of Example 1 was carried out, except that the niobium concentration of the translucent slurry mixture was 10 mass % in terms of NbO, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 3. The pH of the obtained lithium niobate aqueous solution according to Example 3 was 11.
[0055] Example 4 In Example 4, the same production method as in Example 1 was carried out, except that the niobium concentration of the translucent slurry mixture was 20 mass % in terms of NbO, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 4. The pH of the obtained lithium niobate aqueous solution according to Example 4 was 11.
[0056] Example 5 In Example 5, a colorless and transparent lithium niobate aqueous solution according to Example 5 was obtained by the same production method as in Example 1, except that the niobium concentration of the translucent slurry mixture was 10 mass % in terms of NbO and the molar ratio of Li / Nb was 2. The pH of the obtained lithium niobate aqueous solution according to Example 5 was 11.
[0057] Example 6 In Example 6, a colorless and transparent lithium niobate aqueous solution according to Example 6 was obtained by the same production method as in Example 1, except that the niobium concentration of the translucent slurry mixture was 10 mass% in terms of NbO and the Li / Nb molar ratio was 0.9. The pH of the obtained lithium niobate aqueous solution according to Example 6 was 11.
[0058] Example 7 In Example 7, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 2 hours with stirring, and then cooled to room temperature. Pure water was added to replenish the water evaporated by this heating, and the concentration was adjusted so that the niobium concentration of the colorless and transparent slurry mixture was 5 mass% in terms of NbO, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 7. The pH of the obtained lithium niobate aqueous solution according to Example 7 was 11.
[0059] Example 8 In Example 8, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 6 hours with stirring, and then cooled to room temperature. Pure water was added to replenish the water evaporated by this heating, and the concentration was adjusted so that the niobium concentration of the colorless and transparent slurry mixture was 5 mass% in terms of NbO, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 8. The pH of the obtained lithium niobate aqueous solution according to Example 8 was 11.
[0060] Example 9 In Example 9, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 25 hours with stirring, and then cooled to room temperature. Pure water was added to replenish the water evaporated by this heating, and the concentration was adjusted so that the niobium concentration of the colorless and transparent slurry mixture was 5 mass% in terms of NbO, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 9. The pH of the obtained lithium niobate aqueous solution according to Example 9 was 11.
[0061] Example 10 In Example 10, the same production method as in Example 1 was carried out, except that when the slurry of the niobium-containing precipitate according to Example 1 was mixed with lithium hydroxide monohydrate and pure water so that the translucent slurry mixture had a niobium concentration of 5% by mass in terms of Nb2O5 and an NH3 concentration of 5.5% by mass, part of the pure water was replaced with ammonia water (NH3 concentration 25% by mass), thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 10. The pH of the obtained lithium niobate aqueous solution according to Example 10 was 11.
[0062] Example 11 In Example 11, the same production method as in Example 1 was carried out, except that when the slurry of the niobium-containing precipitate according to Example 1 was mixed with lithium hydroxide monohydrate and pure water so that the niobium concentration of the translucent slurry mixture was 5% by mass in terms of Nb2O5 and the NH3 concentration was 10% by mass, part of the pure water was replaced with ammonia water (NH3 concentration 25% by mass), thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 11. The pH of the obtained lithium niobate aqueous solution according to Example 11 was 11.
[0063] Example 12 In Example 12, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 6 hours with stirring, and then cooled to room temperature. Pure water was added to replenish the water evaporated by this heating, and the concentration was adjusted so that the niobium concentration of the colorless and transparent slurry mixture was 10 mass% in terms of NbO, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 12. The pH of the obtained lithium niobate aqueous solution according to Example 12 was 11.
[0064] Example 13 In Example 13, the same production method as in Example 1 was carried out, except that when the slurry of the niobium-containing precipitate according to Example 1 was mixed with lithium hydroxide monohydrate and pure water so that the niobium concentration of the translucent slurry mixture was 10 mass % in terms of Nb2O5 and the NH3 concentration was 8.2 mass %, part of the pure water was replaced with ammonia water (NH3 concentration 25 mass %), thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 13. The pH of the obtained lithium niobate aqueous solution according to Example 13 was 11.
[0065] (Comparative Example 1) In Comparative Example 1, 35% hydrogen peroxide water was added to the colorless and transparent lithium niobate aqueous solution according to Example 1 so that the molar ratio of H2O2 / Nb became 0.3, thereby obtaining a lithium niobate aqueous solution according to Comparative Example 1. The pH of the obtained lithium niobate aqueous solution according to Comparative Example 1 was 11.
[0066] (Comparative Example 2) In Comparative Example 2, a 35% aqueous solution of hydrogen peroxide was added to the colorless and transparent aqueous solution of lithium niobate according to Example 1 so that the molar ratio of H2O2 / Nb became 1, thereby obtaining an aqueous solution of lithium niobate according to Comparative Example 2. The pH of the obtained aqueous solution of lithium niobate according to Comparative Example 2 was 8.
[0067] (Comparative Example 3) In Comparative Example 3, the above-mentioned niobium fluoride aqueous solution was slowly added to 500 mL of a 1% lithium hydroxide aqueous solution to obtain a microparticle dispersion having an Nb2O5 content of 5 mass% and a Li / Nb molar ratio of 1. Then, this microparticle dispersion was filtered and washed using an ultrafiltration device until the amount of liberated fluoride ions reached 100 mg / L, thereby obtaining a lithium niobate sol according to Comparative Example 3. The pH of the obtained lithium niobate sol according to Comparative Example 3 was 8.6.
[0068] Comparative Example 4 In Comparative Example 4, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 73 hours with stirring, and then cooled to room temperature. It was confirmed that a precipitate was formed after heating for 73 hours. Pure water was added to replenish the water evaporated by heating, and the concentration was adjusted so that the niobium concentration of the slurry mixture was 5 mass% in terms of Nb2O5, thereby obtaining a lithium niobate aqueous solution according to Comparative Example 4. The pH of the obtained lithium niobate aqueous solution according to Comparative Example 4 was 11.
[0069] The following physical properties were measured for the lithium niobate aqueous solutions obtained in Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3. The measured physical properties and the methods for measuring the physical properties are shown below, and the measurement results are shown in Table 1.
[0070] <Elemental analysis> If necessary, the sample was diluted appropriately with dilute hydrochloric acid, and the Nb weight fraction and Li weight fraction in terms of Nb2O5 were measured using an ICP optical emission spectrometry (Agilent Technologies: AG-5110) in accordance with JIS K0116:2014.
[0071] <Quantitative analysis of ammonia> 25 ml of sodium hydroxide solution (30 g / 100 ml) was added to 1–5 ml of the sample solution, and the mixture was boiled and distilled. The distillate (approximately 200 ml) was poured into a container containing 20 ml of pure water and 0.5 ml of sulfuric acid to separate the ammonia. The separated ammonia was then transferred to a 250 ml volumetric flask and the volume was adjusted to 250 ml with pure water. 10 ml of the solution was then transferred to a 100 ml volumetric flask. 1 ml of sodium hydroxide solution (30 g / 100 ml) was added to the solution and the volume was adjusted to 100 ml with pure water. The resulting solution was quantitatively analyzed using an ion meter (main unit: HORITA F-53, electrode: HORIBA 500 2A) to measure the ammonium ion concentration (mass%) in the solution.
[0072] <Qualitative analysis of hydrogen peroxide> The UV-visible absorbance spectra of a standard solution containing no added hydrogen peroxide and a standard solution containing 1% hydrogen peroxide by mass (calculated as HO) were measured, and the wavelength at which the rate of change in absorbance was greatest was designated "λ." Next, the absorbance at wavelength λ was measured in the same manner for a sample with an unknown hydrogen peroxide concentration. If the ratio of the absorbance at wavelength λ of the sample with an unknown hydrogen peroxide concentration to the absorbance at wavelength λ of the standard solution containing no added hydrogen peroxide was 1% or less, it was determined that no hydrogen peroxide had been added to the sample.
[0073] The conditions for measuring the ultraviolet-visible absorption spectrum may be as follows. Equipment: UH4150 spectrophotometer (Hitachi High-Tech Science Corporation) Measurement mode: Wavelength scan Data mode: %T (transparent) Measurement wavelength range: 200 to 2,600 nm Scan speed: 600nm / min Sampling interval: 2nm
[0074] Dynamic Light Scattering Particle size distribution was evaluated using a zeta potential, particle size, and molecular weight measurement system (Otsuka Electronics Co., Ltd.: ELSZ-2000) in accordance with JIS Z 8828:2019 "Particle size analysis - dynamic light scattering." To remove dust and other particles from the solution immediately before measurement, the solution was filtered through a 2 μm pore size filter and ultrasonicated for 3 minutes at 28 kHz using an ultrasonic cleaner (AS ONE Corporation: VS-100III). The particle size (D50) refers to the median diameter (D50), which is the particle size at 50% of the cumulative distribution curve. In Table 1, "Initial particle size D50 (nm)" refers to the lithium niobate particle size (D50) in the lithium niobate aqueous solution immediately after production. In addition, "particle diameter D50 (nm) over time" in Table 1 refers to the particle diameter (D50) of lithium niobate in the lithium niobate aqueous solution after being left to stand for one month in an incubator set at room temperature of 25°C.
[0075] <Stability test over time> The lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3 were left to stand for one month in an incubator set at room temperature (25°C), and then visually observed for the presence or absence of white precipitation or gelation. Those in which no white precipitation or gelation was observed were evaluated as having temporal stability and marked with a "Good." Those in which even one white precipitation or gelation was observed were evaluated as not having temporal stability and marked with a "Poor." Gelling was determined by placing each tantalate compound dispersion in a plastic container, and turning the container upside down. The particle diameter (D50) of lithium niobate over time in the lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3 after one month of standing was measured using the dynamic light scattering method described above.
[0076] <Film-forming test> The appearance of the coating film formed on the surface of a glass substrate, which served as a substitute for a current collector plate, was evaluated by observation with an optical microscope. The lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3, were filtered through a 2-μm pore filter and dropped onto a 50 mm × 50 mm glass substrate that had been degreased and washed with acetone and then dried using a syringe. The solution was then applied by spin coating (1,500 rpm, 15 seconds). The applied area was then allowed to dry naturally, forming a coating film on the glass substrate. A central 15 mm × 15 mm area of the formed coating film was observed with an optical microscope (magnification: 40x). A glass substrate with no bubbles, coating irregularities, or cracks was evaluated as having excellent film-forming properties and rated as "Good." A glass substrate with even one or more bubbles, coating irregularities, or cracks was evaluated as having poor film-forming properties and rated as "Poor."
[0077] <Safety Test> The lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3 were added to a positive electrode active material, and the presence or absence of bubbles was visually observed and evaluated. 50 mL of the lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3 were all mixed together with 5 g of lithium manganate, which was the positive electrode active material, in a test container, and the presence or absence of bubbles was visually observed. Those in which no bubbles were observed were deemed safe and were evaluated as "○", and those in which even one bubble was observed were deemed unsafe and were evaluated as "×".
[0078] <Method for producing positive electrode active material> The coating observation was carried out and the coating amount was measured for the positive electrode active materials coated with the lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3. The positive electrode active materials for which the coating observation and coating amount measurement were carried out were produced by the following production procedure.
[0079] After standing for one month at room temperature (25°C), the lithium niobate aqueous solution was diluted with pure water to a niobium concentration of 2.3% by mass, calculated as NbO. Furthermore, if the niobium concentration in the lithium niobate aqueous solution after standing for one month was less than 2.3% by mass, calculated as NbO, dilution was not performed. A positive electrode active material (lithium manganate) was added to the diluted lithium niobate aqueous solution so that the niobium / lithium manganate weight ratio was 2 / 100, thereby obtaining a positive electrode active material slurry containing lithium niobate. Next, while stirring the resulting positive electrode active material slurry containing lithium niobate, 0.4 mol / L of lithium hydroxide aqueous solution was added dropwise to the slurry so that the final Li / Nb molar ratio was 2. The solution was stirred for 10 minutes while maintaining the liquid temperature at 90°C. The resulting positive electrode active material slurry containing lithium niobate was then dried in an atmospheric drying oven at 110° C. for 15 hours to obtain a positive electrode active material coated with lithium niobate.
[0080] <Coating observation> The coating state of the particle surface of the positive electrode active material coated with lithium niobate was evaluated by observation with a scanning electron microscope (SEM). Using a scanning electron microscope (SEM), five SEM images (20 μm × 20 μm) were observed at a magnification of 50,000 times under conditions of an acceleration voltage of 1 kV to observe the coating state of the particle surface of the positive electrode active material. Under the above observation conditions, if not even one uncoated area was observed within a 1 μm square on the particle surface, it was evaluated as "○", and if even one uncoated area was observed, it was evaluated as "×".
[0081] <Measurement of coating amount> An appropriate amount of hydrofluoric acid was added to the positive electrode active material coated with lithium niobate to obtain a solution in which the lithium niobate coating the surface of the positive electrode active material was dissolved.The solution was then subjected to ICP optical emission spectrometry (AG-5110, manufactured by Agilent Technologies) in accordance with JIS K0116:2014 to measure and calculate the niobium weight fraction concentration in the solution in which the lithium niobate coating the surface of the positive electrode active material was dissolved.
[0082] [Table 1]
[0083] As shown in Table 1, the lithium niobate aqueous solutions according to Examples 1 to 13, when the molar ratio of lithium to niobium (Li / Nb) was 0.8 or more and 2.0 or less, and the lithium niobate particle size (D50) in the aqueous solution measured by dynamic light scattering method was 100 nm or less, gave good results in all of the results of the stability test, film-forming test, and safety test.
[0084] The lithium niobate aqueous solutions according to Examples 1 to 13 did not contain hydrogen peroxide, but even after one month had passed, the particle diameter (D50) of lithium niobate over time did not differ significantly from the initial particle diameter (D50), demonstrating excellent stability over time. It was impossible to measure the initial particle diameter (D50) and the particle diameter (D50) over time of lithium niobate in the lithium niobate aqueous solution according to Comparative Example 2 due to gelation. Furthermore, it was confirmed that a precipitate was formed in the lithium niobate aqueous solution according to Comparative Example 4, so the initial particle diameter (D50) and the particle diameter (D50) over time of lithium niobate were not measured.
[0085] The lithium niobate aqueous solutions according to Examples 1 to 13 had improved stability during long-term storage when the lithium niobate concentration in the aqueous solutions was 0.1 to 30 mass %.
[0086] The positive electrode active materials coated with the lithium niobate aqueous solution according to Examples 1 to 13 were observed with an SEM to confirm that the particle surfaces were completely coated with the lithium niobate. Furthermore, the niobium weight fraction concentration of the lithium niobate coating the surfaces of these positive electrode active materials was 1.0 mass% or more. On the other hand, the positive electrode active material coated with the lithium niobate aqueous solution according to Comparative Example 1 had a niobium weight fraction concentration of 1.0 mass% in the lithium niobate coating the surfaces of the positive electrode active material, but uncoated areas were observed with an SEM to confirm the particle surfaces were completely coated with the lithium niobate.
[0087] The inventions disclosed in this specification include, in addition to the configurations of each invention and embodiment, those specified by changing these partial configurations to other configurations disclosed in this specification, to the extent applicable, or those specified by adding other configurations disclosed in this specification to these configurations, or those specified as higher-level concepts specified by deleting these partial configurations to the extent that partial effects can be obtained. [Industrial Applicability]
[0088] The lithium niobate aqueous solution according to the present invention has high dispersibility in water, good solubility in water, and excellent storage stability, and is therefore suitable for coating the positive electrode active material of a lithium ion secondary battery.
Claims
1. A lithium niobate solution containing lithium niobate having a lithium to niobium molar ratio Li / Nb of 0.8 to 2.0, and ammonium ions, The lithium niobate solution is characterized in that the lithium niobate particle diameter (D50) in the lithium niobate solution is 100 nm or less as measured by a dynamic light scattering method.
2. The lithium niobate solution described in claim 1, characterized in that the lithium niobate solution is filtered through a filter having a pore size of 2 μm, dropped onto a glass substrate (50 mm x 50 mm), and applied onto the glass substrate using spin coating (1,500 pm, 15 seconds), and when observed with an optical microscope (magnification: 40x), no air bubbles, uneven coating, or cracks are observed within the center (15 mm x 15 mm) of the coating film formed on the glass substrate.
3. The lithium niobate solution according to claim 1 or 2, further characterized in that it contains at least one selected from Na, Mg, Si, K, Ca, Ti, Mn, Ni, Zn, Sr, Zr, Ta, Mo, Ba and W.
4. A lithium niobate solution as described in claim 2 or 3, characterized in that the pH of the lithium niobate solution is 9 or higher.
5. 5. The lithium niobate solution according to claim 1, wherein the lithium niobate solution does not contain hydrogen peroxide.
6. The lithium niobate solution according to any one of claims 1 to 5, characterized in that the lithium niobate solution is an aqueous solution.
7. 7. The lithium niobate solution according to claim 1, wherein the lithium niobate solution has a concentration of 0.1 to 30 mass %.
8. A positive electrode active material for a lithium ion secondary battery, the surface of which is coated with the lithium niobate contained in the lithium niobate solution according to any one of claims 1 to 7.
9. A lithium ion secondary battery comprising a positive electrode coated with the positive electrode active material for lithium ion secondary batteries according to claim 8.