Hydrogel Materials

JP2023543994A5Active Publication Date: 2024-10-04スタンダード ミロックス ファーマスーティカルス オサケユイチア
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023519017
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-01
Filing Date
2021-09-29
Publication Date
2024-10-04
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing hydrogels are inadequate for the controlled delivery and thermal stabilization of biologically active agents, particularly in injectable forms, and lack the ability to maintain biological activity under varying temperatures.

Method used

A hydrogel material comprising 0.15% to 21% functionalized triblock molecules, 0.85% to 4.0% silica, and 75% to 99% aqueous liquid, forming -Si-O-Si- bonds, which encapsulates biologically active agents, ensuring thermal stability and controlled release.

Benefits of technology

The hydrogel material provides thermal stability and controlled release of biologically active agents, maintaining biological activity over time and enhancing immune responses when administered.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a hydrogel material comprising a first hydrogel containing 0.15 to 21 wt % of a functionalized triblock molecule having the following formula (1): [Formula 1] TIFF2023543994000011.tif26161(1) Here, n is 4 to 680, and m is 1 to 10, based on the total weight of the first hydrogel. The first hydrogel contains 0.85 to 3.3 wt % silica based on the total weight of the first hydrogel and 75 to 99 wt % aqueous liquid based on the total weight of the first hydrogel, and the -Si-OH groups of the silica form -Si-O-Si- bonds with the -Si-(O)3- groups of the functionalized triblock molecule of formula (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to hydrogel materials. The hydrogel materials are particularly useful for the controlled delivery of bioactive agents.

Background Art

[0002] Hydrogels typically contain a network of polymer chains or aggregated colloids as a continuous solid phase and water as a dispersed liquid phase. The three-dimensional solid results from hydrophilic polymer chains being held together by cross-linking or is formed from colloids, such as colloidal particles by aggregation. Hydrogels are natural or synthetic polymer networks in which the liquid phase is water. They can be used as scaffolds for tissue engineering, as carriers for drugs or cells, or as drug delivery systems for sustained release drugs.

[0003] In this specification, the following terms are used in the following meanings.

[0004] A sol is a fluid and homogeneous mixture of at least one liquid phase and one solid phase, that is, a colloidal dispersion, where the liquid phase is, for example, water, ethanol, residues of precursors, etc. and is the continuous phase, and the solid phase is, for example, triblock molecules, functionalized triblocks, and silica here, etc., and is in the form of colloidal particles or polymers and is uniformly dispersed in the liquid phase.

[0005] A gel is a non-fluid homogeneous mixture of at least one solid phase and one liquid phase, that is, a colloidal dispersion, where the solid phase such as triblock molecules, functionalized triblocks, and silica forms a continuous solid phase, and the liquids such as water, ethanol, residues of the solid phase precursors, etc. are uniformly dispersed in the continuous solid phase. The solid phase is typically an aggregated or cross-linked molecular structure formed by a chemical reaction (e.g., by polymerization such as polycondensation) or by aggregation of colloids such as nanoscale particles. In the gel, aggregated and / or cross-linked solid phases form a continuous network throughout the defined space, and the liquid phase is uniformly dispersed within this continuous solid network.

[0006] A sol-gel transition is a term that refers to the process by which a sol changes into a gel. A sol-gel transition typically occurs when colloidal particles and / or polymers aggregate, the aggregates grow in size, and eventually the sol changes into a gel, where the aggregates form a continuous solid phase over the entire volume of the system without phase separation of the liquid phase, i.e., the liquid phase remains uniformly dispersed in the continuous solid phase.

[0007] A hydrogel is a gel in which the liquid phase is water or water-based, containing more than 50% by weight of water. A continuous hydrogel is a hydrogel in a single three-dimensional structure. A dispersed hydrogel is a set of hydrogel particles formed by breaking down a continuous three-dimensional hydrogel into smaller hydrogel particles, which are typically mixed with another continuous hydrogel.

[0008] In the context of the present invention, a fluid mixture refers to a sol having viscoelastic properties due to materials such as a solid phase and a liquid phase, but in which the fluid liquid phase is dominant over the solid phase. In the context of this invention, a non-flowing mixture refers to a viscoelastic material, such as a hydrogel, which does not have flow properties when at rest because the solid phase is more dominant than the liquid phase. In the case of fluid mixtures, the viscous properties (viscosity / loss modulus, denoted by G'' as determined by the rheological method) prevail over the elastic properties (modulus / storage modulus, denoted by G'). Similarly, in non-flowing mixtures, elastic properties (G') prevail over viscous properties (G''). G' and G'' can be measured in the linear viscoelastic region under small-angle vibrational shear, for example, by vibrational measurements using a rheometer with a cone-plate or plate-plate geometry.

[0009] In the context of the present invention, a hybrid material is a material comprising two or more components, such as triblock molecules and silica, with chemical bonds between the components. Furthermore, where the term "hybrid" is used herein, it refers to a solid phase comprising at least two components that together form a solid phase in the hydrogel.

[0010] Vol-% represents volume percentage, while wt-% represents weight percentage.

[0011] Nanoparticles (typically having a size of 1–100 nm) and colloids (typically having a size of 1–1000 nm) have overlapping size ranges within the 1–100 nm range. However, they have different chemical and physical properties. Nanoparticles usually have different material properties by a larger value compared to the same material (i.e., a material with exactly the same chemical composition). For example, they may have different surface properties, which can lead to different properties with respect to hydrophobicity and conductivity. Colloids of size 100–1000 nm begin to lose the special chemical properties of nanoparticles because gravity is still weaker than Brownian motion. Therefore, Brownian motion has a significant impact when producing various dispersions such as gels, suspensions, emulsions, and foams, and the goal is to obtain stable dispersions. The term "hydrophobic colloid" is used for colloidal dispersions where the colloid is not thermodynamically stable (although it may be stable for 15 or even 100 years). Although hydrophilic colloids are thermodynamically stable, they are rarely used.

[0012] Nanoparticles or liquid-poor colloids typically refer to a state in which certain molecular clusters have reached a size and chemical structure that prevents them from actually dissolving in the surrounding liquid. However, because nanoparticles or colloids are extremely small, they remain uniformly dispersed in the surrounding liquid even if their density is higher than that of the liquid. This is because Brownian motion is stronger than gravity. Therefore, when nanoparticles and colloids move through a liquid, they can collide with each other and form larger structures. For example, they can aggregate, and sometimes it can even be said that they polymerize. Therefore, colloidal particles are aggregates formed through chemical bonding and weaker interactions (such as van der Waals interactions), whereas the particles of this specification are formed when a three-dimensional gel is mechanically broken down to form particles, and thus include colloidal particles aggregated therein.

[0013] The paper “Radiopaque Organic-Inorganic Hybrids Based on Poly(D,L-lactide)”, Mazzocchetti et al., Biomacromolecules 2007, 8, 672-678” discloses hybrid organic-inorganic nanocomposites prepared from α,ω-triethoxysilane-terminated poly(D,L-lactide) that could be used as a potentially radiopaque biocompatible coating for medical devices. Not all components of the composite material, nor the composite material itself, are water-soluble. Furthermore, in this publication, tetraethyl orthosilicate (TEOS) is added directly to the system. [Prior art documents] [Non-patent literature]

[0014] [Non-Patent Document 1] Radiopaque Organic-Inorganic Hybrids Based on Poly(D,L-lactide)”, Mazzocchetti et al., Biomacromolecules 2007, 8, 672-678 [Overview of the Initiative] [Problems that the invention aims to solve]

[0015] (Purpose and Overview) It is suitable for the controlled delivery of biologically active agents, and particularly aims to provide a hydrogel useful for the protective encapsulation of various biologically active agents. One of the specific goals is encapsulation to ensure the thermal stability of biologically active agents. Another specific goal is to provide a hydrogel material that can encapsulate biologically active agents while being injectable.

Means for Solving the Problems

[0016] This specification relates to a hydrogel material as follows. A hydrogel material comprising a first hydrogel, wherein the first hydrogel - 0.15% to 21% by weight of a functionalized triblock molecule having the structure of the following formula (1),

Chemical Formula

[0017] This specification also relates to the use of a hydrogel material for the controlled delivery of biologically active agents and the protective encapsulation of biologically active agents.

Brief Description of the Drawings

[0018] [Figure 1] Figure 1 schematically shows the structure of a functionalized triblock molecule. [Figure 2]Figure 2 schematically shows silica nanoparticle aggregates in silica sol. [Figure 3] Figure 3 schematically shows the structure of the reaction product between silica and a functionalized triblock molecule according to one embodiment. [Figure 4] Figure 4 shows the structure of a hydrogel material according to one embodiment. [Figure 5A] Figure 5A shows the structure of a hydrogel material according to another embodiment. [Figure 5B] Figure 5B shows the structure of a hydrogel material according to another embodiment. [Figure 6A] Figure 6A shows the cumulative release of antigen (norovirus P-particles) on day 4 and day 330 after storage at room temperature (25°C) for continuous hybrid / complex hydrogel R217-02 and two-phase hybrid / complex hydrogel #1 (R217-0.2 / R40-0.2A and R217-0.2 / R40-0.2B). [Figure 6B] Figure 6B shows the cumulative release of silica. [Figure 7] Figure 7 shows the cumulative release of the antigen (norovirus P-particles) and the dissolution of silica in the two-phase hybrid / complex hydrogel #2C. [Figure 8] Figure 8 shows the cumulative release of the antigen (norovirus P-particles) and the dissolution of silica in the two-phase hybrid / complex hydrogel #2D. [Figure 9] Figure 9 shows the cumulative release of eGFP and the dissolution of silica for continuous hybrid / complex R217-0.2 with 10 μg of eGFP in 100 μl of hydrogel. [Figure 10] Figure 10 shows the cumulative release of eGFP and the dissolution of silica for continuous hybrid / complex R217-0.2 with 20 μg of eGFP in 100 μl of hydrogel. [Figure 11] Figure 11 shows the cumulative diffusion of eGFP from a continuous hybrid / complex R217-0.2 with eGFP at a hydrogel concentration of 10 μg / 100 μl. [Figure 12]Figure 12 shows the cumulative diffusion of eGFP from a continuous hybrid / complex R217-0.2 with eGFP at a hydrogel concentration of 20 μg / 100 μl. [Figure 13] Figure 13 shows the decay coefficients (G'' / G') for continuous hybrid / complex hydrogel R217-0.2 and two-phase hybrid / complex hydrogel #1 (R217-0.2 / R40-0.2) after storage in syringes in aluminum foil bags at room temperature (25°C) on days 4 and 28. [Figure 14] Figure 14 shows the decay coefficient (G'' / G') after 360 days of storage at room temperature (25°C) for continuous hybrid / complex hydrogel R217-0.2 and two-phase hybrid / complex hydrogel #1 (R217-0.2 / R40-0.2). [Figure 15] Figure 15 shows the dynamic viscosity of continuous hybrid / composite hydrogel R217-0.2 and two-phase hybrid / composite hydrogel #1 (R217-0.2 / R40-0.2) after 4 days of storage at room temperature (25°C). [Figure 16] Figure 16 shows the dynamic viscosity of continuous hybrid / complex hydrogel R217-0.2 and two-phase hybrid / complex hydrogel #1 (R217-0.2 / R40-0.2) after one day of storage in an aluminum foil bag at room temperature. [Figure 17A] Figure 17A shows the thermal stability of norovirus P particles at different temperatures, measured by dynamic light scattering (DLS), for a proportion of 16 nm particles. [Figure 17B] Figure 17B shows the difference in distribution volume for P-particles measured at 50°C and 55°C. [Figure 18A] Figure 18A shows the total volume of 16 nm aggregates of norovirus P-particles released from a continuous hybrid / complex hydrogel R217-0.2 kept in solution at the indicated temperature determined by DLS. [Figure 18B]Figure 18B shows the total volume of 16 nm aggregates of norovirus P- particles released from controlled particles held in solution at the indicated temperature determined by DLS. [Figure 19] Figure 19 shows a TEM image of norovirus P-particles dissolved from the hydrogel. [Figure 20A] Figure 20A shows the dynamics of serum IgG antibodies in mice immunized with two doses of 10 μg of norovirus P-particles (pp) alone, or with a continuous hybrid / complex R217-0.2 hydrogel formulation. [Figure 20B] Figure 20B shows the dynamics of serum IgG antibodies in mice after immunization with a single dose of 20 μg of norovirus P-particles (pp) alone, or with a two-phase hybrid / complex #1 R217-0.2 hydrogel. [Figure 21A] Figure 21A shows the endpoint titration of serum IgG in mice immunized with two doses of 10 μg of norovirus P-particles (pp) alone, or with a serial hybrid / complex formulation in R217-0.2 hydrogel. [Figure 21B] Figure 21B shows the endpoint titration of serum IgG in mice immunized with a single dose of 20 μg of norovirus P-particles (pp) alone, or with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel. [Figure 22A] Figure 22A shows the endpoint titration of serum IgG1 in mice immunized with two doses of 10 μg of norovirus P-particles (pp) alone, or formulated with a continuous hybrid / complex R217-0.2 hydrogel. [Figure 22B] Figure 22B shows the endpoint titration of serum IgG1 in mice immunized with a single dose of 20 μg of norovirus P-particles (pp) alone, or with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel. [Figure 23A]Figure 23A shows the endpoint titration of serum IgG2a in mice immunized with two doses of 10 μg of norovirus P-particles (pp) alone, or with a continuous hybrid / complex R217-0.2 hydrogel formulation. [Figure 23B] Figure 23B shows the endpoint titration of serum IgG2 in mice immunized with a single dose of 20 μg of norovirus P-particles (pp) alone, or with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel. [Figure 24A] Figure 24A shows the avidity of serum IgG antibodies in mice immunized with two doses of 10 μg of norovirus P-particles (pp) alone, or with a continuous hybrid / complex R217-0.2 hydrogel formulation. [Figure 24B] Figure 24B shows the avidity of serum IgG antibodies in mice immunized with a single dose of 20 μg of norovirus P-particles (pp) alone, or with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel. [Figure 25A] Figure 25A shows the cross-reactive serum IgG response to heterologous NoV VLPs in mice immunized with two doses of 10 μg of norovirus P-particles (pp) alone, or with a continuous hybrid / complex R217-0.2 hydrogel formulation. [Figure 25B] Figure 25B shows the cross-reactive serum IgG response to heterologous NoV VLPs in mice immunized with a single dose of 20 μg of norovirus P-particles (pp) alone, or with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel. [Figure 26A] Figure 26A shows homologous blockade of GII.4 VLP binding to the HBGA receptor by serum antibodies in immunized mice, either after two administrations of 10 μg of norovirus P-particles (pp) alone or formulated with a continuous hybrid / complex R217-0.2 hydrogel. [Figure 26B]Figure 26B shows homologous blockade of GII.4 VLP binding to the HBGA receptor by serum antibodies in immunized mice, either with a single dose of 20 μg of norovirus P-particles (pp) alone or with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel. [Figure 27A] Figure 27A shows the endpoint titration of fecal IgG antibodies in mice immunized with two doses of 10 μg of norovirus P-particles (pp) alone, or formulated with a serial hybrid / complex R217-0.2 hydrogel. [Figure 27B] Figure 27B shows the endpoint titration of fecal IgG antibodies in mice immunized with a single dose of 20 μg of norovirus P-particles (pp) alone, or with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel. [Modes for carrying out the invention]

[0019] This specification relates to a hydrogel material comprising a first hydrogel as described below. The first hydrogel is - 0.15% to 21% by weight of a functionalized triblock molecule having the structure of formula (1) below, [ka] (1) Here, based on the total weight of the first hydrogel, n is between 4 and 680, and m is between 1 and 10. - Based on the total weight of the first hydrogel, 0.85 to 4.0% by weight of silica, and - Based on the total weight of the first hydrogel, it comprises 75-99% by weight of an aqueous liquid, The -Si-OH group of the silica forms an -Si-O-Si bond with the -Si-(O)3- group of the functionalized triblock molecule of formula (1).

[0020] This hydrogel material possesses several useful properties in various fields. It is known to be very suitable for the controlled delivery of biological agents. Some particularly suitable biological agents that can be used with this hydrogel material are vaccine antigens and pharmaceutical active ingredients. The hydrogel material can also be made into an injectable form to facilitate its administration. Therefore, the rheological properties of the hydrogel material can be adjusted over a wide range, and its injectability can be controlled. Injectable means that the product can be injected through a fine needle, such as a 25-27G needle or a 23-30G needle, most typically a 25-30G needle. This hydrogel is non-flowing when at rest, for example, during storage, regardless of the amount of aqueous liquid it contains. However, if the amount of aqueous liquid is sufficiently large, for example 96-99% by weight, and pressure is applied, for example by a syringe piston, the hydrogel will flow through the needle and become injectable. Therefore, such a hydrogel becomes shear-thinning.

[0021] This material and all its components are water-soluble. The liquid in this hydrogel is aqueous, which is particularly important for the administration of immunomodulators and therapeutic agents. In fact, in such use, it is necessary that the biological activity of the drug is maintained not only during the production of the end product but also in the final product. Furthermore, during drug delivery within the body, drug release is primarily controlled by the biological degradation of the hydrogel material. This biological degradation mainly occurs through dissolution into the aqueous phase of tissue fluid. All components of this hydrogel dissolve in the aqueous phase of tissue fluid. The polymer is also broken down by enzymatic reactions, and the enzymes are active in the aqueous phase as well. A particularly interesting advantage is that by encapsulating biological activators within this hydrogel material, their thermal stability is guaranteed, which means their biological activity can be maintained over a long period of time, in terms of storage time and temperature. Hydrogel materials also allow for a constant release rate of biologically active agents when administered.

[0022] Functionalized triblock molecules are sometimes called hybrids, oligomers, or polymers. They are end-capped with silica. The -Si-O-Si- bond between the -Si-OH group of silica and the -Si-(O)3- group of the functionalized triblock molecule of formula (1) is a chemical bond. In this specification, materials are generally referred to as hybrids / composites, as some materials are hybrids and others are composites.

[0023] The hydrogel material may consist of a single continuous hydrogel or dispersed hydrogel particles uniformly dispersed within a continuous hydrogel.

[0024] In equation (1) above, n is between 4 and 680, and m is between 1 and 10. The value of n is (depending on the value of m), for example, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 100, 120, 135, 150, 200, 225, 270, 300, 350, 400, 450, 500, 550 or The range is from 600 to 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 100, 120, 135, 150, 200, 225, 270, 300, 350, 400, 450, 500, 550, 600, or 680. The value of m (depending on the value of n) is, for example, from 1, 2, 3, 4, 5, 6, 7, or 8 to 2, 3, 4, 5, 6, 7, 8, 9, or 10.

[0025] Therefore, this hydrogel material has various forms, as summarized in Table 1 below. In this specification, the type names shown in Table 1 are used.

[0026] The following provides details about various types of hydrogel materials.

[0027] [Table 1]

[0028] According to one embodiment, the functionalized triblock molecule of formula (1) and silica form colloidal particles, the network of particles forming a continuous solid phase in which an aqueous liquid phase is uniformly distributed, and the solid phase and the aqueous liquid phase are in a single hydrogel entity. This is the continuous hybrid / composite shown in Table 1.

[0029] In this embodiment, the hydrogel is therefore a homogeneous mixture of solid particle aggregates (colloidal aggregates formed from colloidal particles) and an aqueous liquid. Silica is at least partially in the form of colloidal particles and colloidal aggregates, forming chemical bonds with triblock molecules to create a hybrid material. Colloidal silica particles are formed from spherical clusters of molecules, and the atoms on their surface can form chemical bonds with other compounds in the material, including not only triblock molecules but also other colloidal silica particles.

[0030] Both functionalized triblock molecules and silica have nanoscale structures. Functionalized triblock molecules are soluble or partially soluble in aqueous liquids, while silica takes the form of nanoparticles. Hybrids / complexes are formed when the Si-OH groups of silica form -Si-O-Si bonds with Si-O- groups at the ends of functionalized triblock molecules. One functionalized triblock molecule can also be linked to another functionalized triblock molecule using these bonds, thereby forming a network. Typically, each -Si-(O)3- group may be bonded to 0-3 functionalized triblock molecules or 0-3 silica molecules.

[0031] Furthermore, silica nanoparticles can also bond to one another (or aggregate or agglomerate through weak interactions). Silica nanoparticles may also form larger aggregates, but at least some of the nanoparticles are bound to at least one functionalized triblock molecule.

[0032] The silica in these hydrogel materials exists in the form of colloids, nanoparticles, or aggregated nanoparticles (which are also colloids). The four oxygen atoms of silica bond to another molecule, such as another silicon molecule. Silica tends to form cyclic structures, and these cyclic (i.e., spherical) silica molecules grow so rapidly that they become too large to dissolve in the surrounding liquid, and can therefore be called nanoparticles or colloids. While it is true that it forms its own solid phase in the surrounding liquid, it is too small to maintain a stable state in the liquid and to move around by Brownian motion like soluble molecules. The surface of the particles has numerous free Si-OH groups, which react with functionalized triblock molecules to form chemical bonds and create hybrids / complexes.

[0033] In this first type of material, nanostructures, namely functionalized triblock molecules and silica nanoparticles, aggregate (or polymerize), and when aggregation proceeds sufficiently, they form aqueous liquids and non-flowing hydrogels. When a hydrogel material is used to encapsulate another molecule, this molecule is added to the mixture before a non-flowing hydrogel is formed.

[0034] According to other embodiments, the hydrogel material further comprises a second hydrogel, which is as follows: - Based on the total weight of the second hydrogel, 0.15 to 0.8 wt% of the functionalized triblock molecule of formula (1) and - Based on the total weight of the second hydrogel, 0.85 to 3.3% by weight of silica and, - Based on the total weight of the second hydrogel, 75-99% by weight of aqueous liquid is added. Here, the -Si-OH group of silica forms an -Si-O-Si bond with the -Si-(O)3- group of the functionalized triblock molecule of formula (1) in the second hydrogel, and Here, the second hydrogel is in the form of uniformly dispersed particles dispersed within the first hydrogel, and the first hydrogel forms a continuous phase. However, the total amount of silica and functionalized triblock molecules having formula (1) in the second hydrogel is greater than the total amount of silica and functionalized triblock molecules having formula (1) in the first hydrogel.

[0035] This hydrogel material is the two-phase hybrid / composite #1 shown in Table 1. This hydrogel material therefore has two different hydrogels, which consist of the same components but in different amounts. The initial hydrogel forms a continuous phase of hybrid / complex #1. The second hydrogel first forms a non-flowing hydrogel, and then its physical structure is mechanically broken down to form particles. These particles are then mixed into the continuous phase of the first hydrogel while the first hydrogel is still flowable. Typically, the second hydrogel (i.e., the dispersed phase) contains less aqueous liquid than the first hydrogel.

[0036] According to one embodiment, the total amount of silica and functionalized triblock molecules having formula (1) is at least 20% greater in the second hydrogel than the total amount of silica and functionalized triblock molecules having formula (1) in the first hydrogel.

[0037] If a biological agent or analogue is encapsulated within this hybrid / complex #1, it is mixed with either a still-flowable second hydrogel or a still-flowable first hydrogel, or both. If slower delivery is desired, the drug is mixed with a second hydrogel, which is in the form of particles in the final product. Therefore, this hydrogel material is particularly suitable when two different release profiles are desired, as it may be possible to deliver drugs at two different rates depending on their position within the hydrogel material's components.

[0038] According to other embodiments, in a hydrogel, - The functionalized triblock molecule and the first part of the aqueous liquid of formula (1) are The form of particles obtained by decomposing the functionalized triblock molecule of formula (1) and the aqueous liquid hydrogel into particles, Dispersed in a silica sol obtained by mixing the second part of the aqueous liquid, - The -Si-OH group of silica forms an -Si-O-Si bond with the -Si-(O)3- group of the functionalized triblock molecule of formula (1), thus forming a hydrogel material.

[0039] This hydrogel material is a two-phase hybrid / composite #2 in Table 1. This hydrogel material has the same chemical composition as the hydrogel material described above, but has two different components. In this embodiment, the continuous phase is formed by silica and an aqueous liquid, and the dispersed phase is formed by first mixing functionalized triblock molecules with the aqueous liquid, which allows for the formation of a non-flowing hydrogel, and the resulting hydrogel is mechanically broken down into particles. These particles are mixed into a continuous phase, resulting in a hydrogel material. When adding a biological agent or analogue to a hydrogel, the addition is carried out by adding the agent while the mixture of the functionalized triblock molecule and the aqueous liquid is still flowable. Because silica gel forms a continuous phase, this type of hybrid / complex #2 can be formed for injection.

[0040] In this embodiment, the final hydrogel material is formed in the same manner as the first hydrogel; that is, the chemical reaction results in colloids, the colloids aggregate, and the chemical bonds are of the same type in the first hydrogel and the final hydrogel material.

[0041] In the first and second hydrogels, the components are the same, namely, the functionalized triblock molecule of formula (1), silica, and aqueous liquid. The amounts shown below are applied to the first and second hydrogels, with any necessary modifications.

[0042] The amount of the functionalized triblock molecule in formula (1) is 0.15 to 21.0% by weight, based on the total weight of the hydrogel. Therefore, the amounts of the functionalized triblock molecule in formula (1) are, for example, based on the total weight of the hydrogel, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 15.0, It can range from 18.5 or 19.5% by weight to 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 15.0, 18.0, 19.5, or 21.0% by weight.

[0043] The amount of silica is 0.85 to 4.0% by weight, based on the total weight of the hydrogel. Therefore, the amount of silica can range from, for example, 0.85, 1.0, 1.2, 1.5, 1.8, 2.0, 2.2, 2.5, 2.7, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6 or 3.7% by weight, based on the total weight of the hydrogel, to 1.0, 1.5, 1.8, 2.0, 2.2, 2.5, 2.7, 2.9, 3.0, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9 or 4.0% by weight.

[0044] The amount of aqueous liquid is 75-99% by weight, based on the total weight of the hydrogel. Therefore, the amount of aqueous liquid can range from 75, 78, 80, 82, 85, 88, 90, 92, or 95% by weight, for example, to 80, 82, 85, 88, 90, 92, 94, 94, 95, 96, 97, 98, or 99% by weight, based on the total weight of the hydrogel.

[0045] In this embodiment, one of the hydrogels takes the form of particles, and the particle size of the second hydrogel or the first hydrogel is less than 1 mm. In practice, the most typical particle size is several tens of micrometers, for example, to maintain the fluidity of the material so that it can pass through a 25-27 G needle. Preferably, the particle size is less than 0.3 mm. Particle sizes range from, for example, 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 120, 150, 200, 250, 300, 350, 300, 350, 500, 550, 600, 650, 700, 750, 800 or 850 μm to 10 The size can be up to 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 120, 150, 200, 250, 300, 350, 300, 350, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, or 1000 μm.

[0046] In this hydrogel material, the silica is preferably alkoxysilane-derived silica, and more preferably tetraethoxysilane-derived silica.

[0047] The aqueous liquids of the first hydrogel and the second hydrogel are preferably independently selected from water, a mixture of water and ethanol, and a biologically compatible buffer. Examples of such biologically compatible buffers include phosphate-buffered saline (PBS), citrates, succinates, acetates, benzoates, and mixtures thereof.

[0048] According to a preferred embodiment, the aqueous liquid is a mixture of water and ethanol, containing 50-95% by weight of water and the remainder being ethanol. Therefore, the mixture may contain, for example, 60% to 93% by weight of water, with the remainder being ethanol. Therefore, the amount of water can range from 50, 55, 60, 65, 70, 75, 80, or 85% by weight of the total weight of the aqueous liquid to 60, 65, 70, 75, 80, 85, 90, or 95% by weight. The aqueous liquid may consist of water alone.

[0049] This hydrogel material may further contain at least one encapsulated biologically active agent. Depending on its structure and the intended use of the hydrogel material, the biologically active agent can be encapsulated in different parts of the hydrogel. In fact, the biological activator may be encapsulated within the first hydrogel, within at least one of the first and second hydrogels, and / or within the gel of the functionalized triblock molecule of formula (1).

[0050] According to one embodiment, the biological activator is selected from the group consisting of immunomodulators and therapeutic activators.

[0051] Encapsulation of biological agents can be used for a variety of purposes, including delivery (e.g., oral or parenteral delivery), administration, desensitization, or protection of the biological agent (e.g., against heat).

[0052] Therefore, biological activators can be immunomodulators such as vaccines and desensitizers for allergies. Some examples include antigens, viruses, specific antigens, and virus-like particles (VLPs). Some examples of therapeutic agents, also called drugs, include drug molecules of various sizes, such as peptides, proteins, biological drugs, biopharmaceuticals, biosimilar drugs, biobetter drugs, nucleic acid-based drugs, and cell and viral vectors. In vaccines, in vivo studies have observed that when antigens are encapsulated in this hydrogel material, they can be administered without additional adjuvants (such as those typically used in vaccines).

[0053] This specification also relates to the use of the hydrogel materials described above for the controlled delivery of biological agents. This also relates to the use of such hydrogel materials for the protective encapsulation of biologically active agents. Protective encapsulation may be used, for example, to ensure the stability of biological activators and / or to protect them until controlled release.

[0054] In one particular embodiment, protective encapsulation is used to ensure the thermal stability of the biological activator. Thermal stability means that encapsulation ensures that the biological activator will not be destroyed, denatured, or altered in any way when the product containing the biological activator is exposed to temperatures above typical refrigeration storage temperatures (4-8°C). It can also protect biological activators during long-term or short-term storage at ambient temperatures (20-25°C) or high temperatures (>25°C, e.g., 35-50°C).

[0055] Furthermore, this hydrogel can be used to induce an adjuvant effect in immunization using biological activators, meaning that the hydrogel delivered together with the antigen elicits an enhanced immune response compared to the administration of the antigen alone.

[0056] This hydrogel material can be manufactured using various methods. One possible method for producing functionalized triblock molecules involves the following steps: - L-lactide and polyethylene glycol with a molecular weight of 200-30000 g / mol are reacted in the presence of a first catalyst in a molar ratio of polyethylene glycol to L-lactide of 2:1-20:1 to obtain a triblock molecule. - The obtained triblock molecule is reacted with isocyanate-topropyltriethoxysilane in the presence of a second catalyst in a molar ratio of 1:2 of the triblock molecule to the isocyanate-topropyltriethoxysilane to obtain a functionalized triblock molecule.

[0057] The second hydrogel is prepared in the same manner as the first hydrogel, except that the amount used is different, in order to obtain a second hydrogel having the same components but in different relative amounts. In both cases, the objective is to have an equal number of L-lactide groups at both terminal groups of the polyethylene glycol molecule, and therefore the molar ratio will be any even number within the above range.

[0058] Silica sol can be prepared, for example, by hydrolyzing tetraethyl orthosilicate (TEOS) at pH 2 under stirring. The molar ratio (R) of water to TEOS can be, for example, 98 (R98). After hydrolysis, the silica sol is aged at room temperature for, for example, 115 minutes, and then the pH is adjusted to pH 7.2-7.4 using 0.1 M NaOH.

[0059] TEOS is partially converted to ethanol during the reaction. If the amount of water is in excess compared to TEOS (e.g., R200-R400), the resulting hydrogel material is more fluid and can usually be injected using a fine needle. Furthermore, the resulting silica sol does not contain TEOS.

[0060] A single-phase hydrogel material can be prepared by dissolving functionalized triblock molecules in an aqueous solution and adding this mixture to a silica sol. The mixture is then aged to form the hydrogel material.

[0061] Two-phase hybrid / composite hydrogel material #1 (described in Table 1 above) can be prepared by dispersing a second hydrogel material into gel particles by introducing shear force through injection via a fine needle.

[0062] To prepare two-phase hybrid / composite hydrogel material #2, a hydrogel material containing functionalized triblock molecules is formed into a non-flowing hydrogel, and then this hydrogel is broken down into particles. These particles are added to a freshly prepared silica sol while being mixed.

[0063] Other options for turning hydrogels into particles include: - Apply pressure to the gel, such as by pressing it; this will result in a paste-like product. - Apply a lateral shear force to the gel; this yields a paste-like or liquid product. - Mixing the gel is essentially similar to applying a lateral shear force; using a low rotation speed will result in a paste-like product, while a high rotation speed will yield a fluid gel. - Vibration is applied to the gel, such as by stirring with a vortex; the original homogeneous gel breaks down into small fragments, and the resulting fragments become paste-like. - Rapid decomposition is performed using Turrax mixing; the gel is broken down into small components, but when the components come into contact with the receptor wall, the gel returns to a paste-like state. - Cut the gel with a sharp tool; little paste-like gel is formed, the volume increases, and the material becomes electrostatically charged. - Shredding of the gel; no paste-like gel is formed, the volume increases, and the material becomes electrostatically charged. - The gel is crushed by pushing it through a sieve (the gel needs to be allowed to mature sufficiently, for example, for 3 days or more); this results in a porous, fluffy gel, which increases in volume fourfold and the material becomes electrostatically charged. - For example, the application of mechanical grinding to the gel using a mortar and pestle, or a ball mill or other type of mill.

[0064] [Detailed description of the drawing] Figures 1-5A schematically show the structures of various intermediate products and final hydrogel materials. Since the precise three-dimensional structures at the nanoscale are not precisely known, these should not be interpreted as scale-based or exact replicas of the structures.

[0065] Figure 1 schematically shows the structure of a functionalized triblock molecule. In this figure, LA1 represents lactide and PEG represents polyethylene glycol. In this figure, R represents propyl.

[0066] Figure 2 schematically shows silica nanoparticle aggregates in silica sol. Silica sol contains various structures1, i.e., aggregates made of silica particles, one of which is shown as an enlarged view 2.

[0067] Figure 3 schematically shows the structure of the reaction product between silica and a functionalized triblock molecule according to one embodiment. The silica particles in Figure 2 are shown to be bound to the ends of the functionalized triblock molecule. The schematic diagram indicated by reference numeral 3 shows the relative sizes of various parts of the product.

[0068] Figure 4 shows the structure of a hydrogel material according to one embodiment. It is shown that the hydrogel material forms a network structure.

[0069] Figure 5A shows the structure of a hydrogel material according to another embodiment, namely the two-phase hybrid / composite hydrogel #1 described above. Enlarged Figure 4 shows the substructure of hydrogel #1. Figure 5B shows the structure of a hydrogel material according to yet another embodiment, namely the two-phase hybrid / composite hydrogel #2 described above, and enlarged Figure 5 shows a partial structure of hydrogel #2.

[0070] Figures 6 to 27B show the experimental results, which will be discussed in more detail in the section on examples. [Examples]

[0071] Materials and methods Hydrogel preparation Three different types of hydrogel materials were prepared, as shown in Table 1 above.

[0072] The preparation of hydrogel materials consists of several steps. The first step is to prepare the linker molecule, followed by the preparation of the primary triblock, and then the preparation of the functionalized triblock molecule by functionalizing the triblock silica with isocyanate-propyltriethoxysilane. This functionalized triblock molecule is shown in formula (1) and Figure 1.

[0073] On the other hand, silica sol is a preparation agent for silica sol, as shown in Figure 2 (see Figure 4). Subsequently, a hybrid / complex is prepared from silica sol and functionalized triblock as shown in Figure 3, and a hybrid / complex hydrogel is formed (shown in Figure 4).

[0074] Two-phase hybrid / composite hydrogels #1 and #2 were prepared by dispersing one hydrogel into particles, as shown in Figures 5A and 5B, and then mixing the dispersed hydrogel particles into another hydrogel that functions as a continuous phase.

[0075] (Preparation of continuous hybrid / complex hydrogels and embedding of norovirus P-particles / proteins) The formation of the triblock was initiated by performing a ring-opening polymerization (ROP)-like reaction from L-lactide (Sigma Aldrich) to polyethylene glycol (PEG, Sigma Aldrich), catalyzed by tin(II) 2-ethylhexanoate (which also functions as an initiator), to prepare a linker molecule (PEG with both ends end-capped with L-lactide). The operation was carried out as solvent-free bulk polymerization in a Schlenk line system under an inert atmosphere of N2. The required amount of the intermediate block (polyethylene glycol, PEG, 200 g / mol) was calculated according to a molar ratio of 2:1 (PLA:PEG). PEG was added, and then the temperature was gently raised to 160°C while stirring. The mixture was heated until the contents dissolved. Tin(II) 2-ethylhexanoate (Sigma Aldrich) at a molar ratio of 0.05 (catalyst: PEG) was pipetteed into the molten material, and the container was sealed. The reaction was carried out at 160°C for 90 minutes. After the reaction, the product was cooled to ambient temperature. The product was purified using a two-solvent system of chloroform and hexane (Sigma Aldrich). The supernatant of hexane was decanted, and chloroform was evaporated in two steps. First, chloroform was evaporated using a rotary evaporator (IKA RV10) at a vacuum of 450 mbar and 40°C for 15 minutes. In the second step, the last trace amount of solvent was evaporated using a vacuum pump. The resulting triblock was heated to +60°C in a water bath, and the pressure was reduced to p<0.1mbar using a diffusion pump (Vacuubrand RZ 2.5). The evaporating substance was captured in a solvent trap immersed in liquid nitrogen (N2). This procedure was continued until no more bubbles formed on the molten material.

[0076] Next, the prepared Triblock was reacted with isocyanate-propyltriethoxysilane (IPTS, Sigma Aldrich) to produce functionalized Triblock molecules. This was done by dissolving Triblock, IPTS, and dibutyltin dilaurate (catalyst, Alfa Aesar) in tetrahydrofuran (THF, Sigma Aldrich) in a molar ratio of 1:2:0.05. As described in the Triblock preparation step above, the mixture was heated to 60°C under an inert atmosphere using a Schlenk line system. The reaction was allowed to proceed for 1 hour. Using a rotary evaporator (IKA RV10), THF was evaporated at 40°C for 10 minutes under a vacuum of 357 mbar. The resulting functionalized triblock molecules were then dissolved in a two-solvent system of hexane and chloroform. Further purification steps of the functionalized triblock molecules were carried out precisely as described above in the triblock preparation section.

[0077] Next, we will describe typical examples of other steps in the preparation process of hybrid / complex hydrogels. Several different formulations were prepared by varying the molecular weight of the polymer (i.e., the molecular weight of polyethylene glycol) and the amounts of P-particles, functionalized triblock molecules, water, and silica, while keeping the preparation process the same except for slight variations in mixing, aging, and gelling times.

[0078] The next step after the synthesis of the functionalized triblock molecule was the preparation of a silica sol. Tetraethyl orthosilicate (TEOS, Sigma Aldrich) was used as the silica precursor. TEOS was hydrolyzed with stirring at pH 2 (adjusted using 0.1 M HCl, Merck Titripur). The molar ratio (R) of water to TEOS was 98 (R98). After hydrolysis, the silica sol was aged at room temperature for 115 minutes, and then the pH was adjusted to pH 7.2–7.4 using 0.1 M NaOH (Merck Titripur). The resulting silica sol was filtered through a sterile 0.45 μm PES membrane syringe filter.

[0079] 200 mg of functionalized triblock molecules (containing PEG 200 g / mol) were dissolved in 50 ml of phosphate-buffered saline (PBS, Sigma Aldrich) containing norovirus P-particles at a concentration of 200 micrograms / ml (200 ppm). Next, this mixture was added to 50 ml of R98 silica sol (aged for approximately 3 minutes at pH 7.2-7.4) to obtain a P-particle concentration of 100 ppm in the resulting sol. Before the sol (total volume approximately 100 ml) changed into a non-flowing gel (gelation time varies depending on the details of the formulation), sol (1 ml) was transferred to a syringe within 2 to 5 minutes. Evaporation of the aqueous solution (water and ethanol) was minimized during the preparation and pH adjustment stages by covering the container with a plastic film. The obtained water-to-TEOS ratio (R) was 217 (R217), which corresponds to 1.5% by weight of silica in the final hydrogel material. The final concentration of the functionalized triblock molecule was 0.2% by weight, and the P-particle concentration was 100 ppm, i.e., 0.1 mg per 1 ml of the final hydrogel material. In the example above, the final code for the hydrogel material is R217-0.2, indicating the content of both silica and functionalized triblock molecules in the final material. The composition of the R217-0.2 hydrogel is shown in detail in Table 2.

[0080] [Table 2]

[0081] Actual hydrogels consist of functionalized triblock molecules, silica, water, and ethanol, with the antigen encapsulated within them. In addition, hydrogels may contain encapsulated residues within their structure, namely NaCl. Different hydrogel materials were prepared to correspond to different component concentrations (R217-0.15, R328-0.2, R328-0.4, R328-0.8, R40-0.2). Higher molar masses of PEG (2000 g / mol and 6000 g / mol) were also tested for the R217 continuous hybrid / complex, however, their injection characteristics were not optimal, so more extensive studies on the hybrid / complex were conducted with only 200 g / mol PEG in Triblock. However, such materials (i.e., PEG with a high molar mass) are useful for non-injectable delivery purposes because their properties are otherwise similar to those that have been modified and tested as follows.

[0082] (Preparation of two-phase hybrid / complex hydrogels and embedding of norovirus P-particles / proteins) The above-mentioned functionalized triblock molecules are part of the two-phase hybrid / complex hydrogels #1 and #2 (listed in Table 1 above). In two-phase hybrid / complex hydrogel #1, the dispersed hydrogel fragments are composed of the same solid phase as the continuous phase, but with different amounts of water. In two-phase hybrid / complex hydrogel #2, the continuous hydrogel is inorganic silica gel, and the dispersed component is an organic hydrogel. The general structure of the two-phase hydrogel is shown in Figures 5A and 5B. Actual hydrogels consist of functionalized triblock molecules, silica, water, and ethanol, with the antigen encapsulated within them. In addition, hydrogels may contain encapsulated residues within their structure, namely NaCl.

[0083] In two-phase hybrid / complex hydrogel #1 (Table 3), both components are of the same type, containing alkoxysilane-functionalized triblock molecules-silica hybrid / complex (organic-inorganic hybrid / complex), the only difference being the amount of water used in the hydrogel. Different two-phase hydrogels were prepared with different water-to-TEOS molar ratios (R40, R217, and R328) and functionalized triblock molecule content (0.15 and 0.2 wt% for R217, 0.2, 0.4, and 0.8 wt% for R328, and 0.2 wt% for R40). However, R217-0.2 / R40-0.2 was selected for more rigorous characterization due to its superior rheological properties and injectability. The former component (here, R217-0.2) exhibits a continuous hydrogel phase, while the latter component (here, R40-0.2) is a hydrogel dispersed in the continuous hydrogel phase. Norovirus P-particles were embedded in dispersed hydrogels only, or in both dispersed hydrogels and continuous hydrogels, in the corresponding manner described above. In addition, monomeric green fluorescent protein (eGFP) was used as another encapsulating agent for R217-0.2. The dispersed hydrogel R40-0.2 was prepared by first allowing a non-flowing gel to form in this system (to ensure effective embedding of P-particles). Immediately after hydrogel formation, the non-flowing R40-02 was dispersed into the gel particles by introducing shear force through injection with a fine needle (18G). To prevent the aqueous liquid (water and ethanol) from evaporating from the system, this step was carried out rapidly (within 1-2 minutes). The primary function of continuous hydrogels is to function as an injection matrix, that is, to provide rheological properties suitable for injection into a fine needle in a two-phase system, but they can also be used as part of a controlled release system to achieve different release rates, such as two-phase release.

[0084] Table 3 shows the composition of the two-phase hybrid / complex hydrogel #1 (R217-0.2 / R40-0.2) containing encapsulated antigens and residues (A: Antigens in both R217 and R40 in a mass ratio of 25:75, and B: Antigens in R40 only).

[0085] [Table 3]

[0086] In the two-phase hybrid / complex hydrogel #2, the continuous component was a silica hydrogel, and the dispersed component was a hydrogel composed of alkoxylan-functionalized triblock molecules and water. Four different hydrogel formulations with varying weight ratios of silica, siloxane-functionalized triblock molecules, and water were prepared (Table 4). Tetraethyl orthosilicate (TEOS, Sigma Aldrich) was used as a silica precursor. TEOS was hydrolyzed under stirring at pH 2 (adjusted using 0.1 M HCl). The molar ratio (R) of water to TEOS was 220 (R220) for each formulation. Additional ethanol was used in the aqueous solution to establish a homogeneous system with silica, functionalized triblock molecules, and water (the formation of silica sol from TEOS results in the formation of ethanol as a byproduct). After adjusting the pH of the obtained silica to pH 5-6 (using 0.1 M NaOH), an organic hydrogel portion containing siloxane-functionalized triblock molecules and water was added. The preparation of the dispersed organic hydrogel was initiated by first allowing a non-flowing hydrogel to form in this system (to ensure effective embedding of P-particles). After hydrogel formation, the structure was dispersed into particles by grinding the hydrogel into hydrogel particles. To avoid water separation, dispersed organic hydrogel particles were rapidly added to a newly prepared silica sol within 1-2 minutes, and the entire system was homogenized using an Ultra-Turrax T25 (with stator S25N-18G). The method for dispersing the organic hydrogel differs from that of two-phase hybrid / complex hydrogel #1, because two-phase hybrid / complex hydrogel #2 has a greater amount of difference in solid content. The mixture of silica gel and organic hydrogel particles transforms into a non-flowing hydrogel in about 30 minutes. Mixing is performed prior to hydrogel formation to avoid sedimentation of the organic hydrogel portion.

[0087] Table 4 shows various compositions of two-phase hybrid / complex hydrogel #2 containing encapsulated antigens and residues.

[0088] [Table 4]

[0089] The norovirus P-particles were embedded in the two-phase hybrid / complex hydrogel #2 as described above (i.e., the P-particle solution was added to the system while it still had a fluid, liquid-like structure prior to hydrogel formation), but in this case, they were dispersed only within the organic hydrogel. If necessary, P-particles or other biological agents can also be embedded in both dispersed and continuous hydrogels.

[0090] (eGFP production and characteristics) Monomeric green fluorescent protein (eGFP) was produced using genetically modified Escherichia coli (E. coli transformed with the gene encoding monomeric green fluorescent protein) as the producing organism. The protein was purified using standard molecular biology methods.

[0091] The following procedure was used for embedding eGFP in the hydrogel. Protein stocks manufactured in 2017 and stored at -20°C were used in the experiment. Prior to the above experiment, the protein content was measured using μBCA (microBCA protein assay kit, microplate procedure, Thermo Scientific™). The concentration was 2.2 mg / ml. The molar mass of eGFP was determined to be approximately 40 kDa by SDS-PAGE (sodium dodecyl sulfate polyacrylamide gel electrophoresis).

[0092] Dissolution experiment (Release of P particles and eGFP and biodegradation of hybrid / complex hydrogels) Dissolution experiments, i.e., the release of P-particles and the dissolution of hybrid / complex hydrogels (R217-0.2 and R217-0.2-R40-0.2), were performed in either PBS or tris(hydroxymethyl)aminomethane (TRIS) buffered to approximately pH 7.4 in a shaking bath at 37°C. PBS was used for the release of P-particles, and TRIS was used for the dissolution of inorganic-organic hybrids / complexes. The dissolution experiments were actually conducted under sink conditions, which refer to the sink conditions for the inorganic portion (amorphous silica) of the hybrid / composite hydrogel (to ensure free dissolution without hindering the dissolution rate by the dissolution product). The dissolution medium was regularly refreshed at every sampling point to maintain the conditions in the sink (concentration of dissolved amorphous silica less than 30 ppm). Three replicas were collected at each time point.

[0093] P-particle and eGFP emission were analyzed by total protein analysis using a micro-BCA protein assay kit (Microplate Procedure, Thermo Scientific™) for colorimetric detection at 562 nm with a spectrophotometer (Hidex Sense Microplate Reader). The dissolution rates of hybrid / complex hydrogels (continuous hybrid / complex and two-phase hybrid / complex #1) were estimated by measuring the dissolution of silica by GF-AAS (Shimadzu 6650F, GFA-EX7) as a function of time, which corresponds to a total solids content of 3.5% (of two-phase hybrid / complex hydrogel #2-D) - 82.5% (of two-phase hybrid / complex hydrogel #1-B) for hybrid / complex hydrogels. Prior to analysis, the liquid sample containing P-particles was concentrated. Concentration was performed because dissolution measurements were carried out under sink conditions (for silica), resulting in a highly diluted sample (and sink conditions were used to find the actual mechanism of release, taking into account both biodegradation and diffusion-related components in the release, and to observe actual differences between different material versions). Since the settling limit of silica was approximately 30 ppm, the maximum concentration of the encapsulated material correlates to the same limit depending on the packing density. When the packing density of silica relative to the total mass is 1%, the maximum concentration of the encapsulated substance in the dissolved sample is only 0.3 ppm. The sample is concentrated by either centrifugal membrane filtration (Eppendorf Centrifuge 5810 R, 8000-10000G, 15-30 minutes, using Amicon® Ultra-15 centrifugal filter Ultracel®-3K) or lyophilization (Christ Epsilon 1-6D, loaded at -35°C and maximum freezing temperature, followed by a main drying with the temperature gradually increased to -15°C, and final drying at -10°C for 23 minutes and 20°C for 20 minutes), after which the lyophilized P- particles are redispersed in a smaller volume of liquid.

[0094] (Dissolution of P-particles from hydrogel R217 for the study of particle composition and consistency) To investigate whether the released antigen remained intact after being kept at various temperatures, a hydrogel containing 0.5 mg / ml of P-particles was dissolved in a 10 kDa cutoff dialysis cassette (Slide-A-Lyzer, ThermoFisher). First, the hydrogel was removed from the syringe, weighed, and transferred to a dialysis cassette. The cassette was then dialyzed in 0.8 L of PBS at room temperature, with the cassette being changed five times over a week. Next, after confirming that no gel residue was present in the cassette, the solution from the cassette was transferred to microcentrifuge tubes, dispensed, and stored at -20°C for analysis.

[0095] (Release mechanism experiment) The P-particle release mechanism was investigated in silica-saturated PBS or tris(hydroxymethyl)aminomethane (TRIS) buffered to approximately pH 7.4 in a shaking bath at 37°C. Silica-saturated media were prepared by dissolving amorphous sol-gel-inducing silica fragments in the medium until the silica saturation level (approximately 130 ppm) was reached. If the dissolution of the majority (silica) of the hybrid / complex hydrogel was prevented, P-particles were released primarily by diffusion. Next, the diffusion results were compared with release experiments conducted under sink conditions where both matrix biodegradation and diffusion could occur simultaneously. The release mechanism of eGFP from a continuous hybrid / complex containing R217-based encapsulated P-particles was investigated.

[0096] Rheological measurements and injection experiments Rheological measurements were performed using a modular rheometer (Anton Paar MCR 104). Samples were injected onto the geometry (20 mm plate-to-plate) using a 1 ml syringe (Becton Dickinson) and a 25 G needle (Becton Dickinson Microlance). Amplitude sweep measurements were performed at a constant angular frequency of 6.28 rad / s with strain values ​​from 0.01 to 10%. Frequency sweeps were performed at a constant strain defined by the amplitude sweep measurements with frequencies from 0.01 to 100 rad / s.

[0097] The injection performance of the prepared hybrid / complex hydrogel materials was investigated. The tests were performed on continuous hybrid / complex and two-phase hybrid / complex #1 hydrogels. The material was injected with normal force from a 1 ml syringe (Becton Dickinson) through a 25 G needle (Becton Dickinson Microlance). The hydrogel lines were injected into a plastic tray and the results were visually examined. The smoothness of injection, signs of phase separation, apparent homogeneity, and compatibility with the lysis buffer were recorded and evaluated.

[0098] 2.4 Manufacturing and purification of norovirus P-particles His-tagged norovirus P-particles were generated in E. coli BL21 star cells, as described by Koho et al. (Journal of Virological Methods 179(2012)1-7). Pelleted bacterial cells were dissolved in lysis buffer (50 mM NaH2PO4, 600 mM NaCl, 10 mM imidazole, pH 8.0) using an EmulsiFlex®-C3 homogenizer (Avestin Inc.). The cell lysates were clarified at 10000Xg at 4°C for 30 minutes, and the clarified lysate was used for affinity purification using nickel-charged Sepharose (Merck, HisTrap FF Crude). The purified P-particles were dialyzed against PBS and then aseptically filtered for analysis and further use. The concentration of P-particles was measured by BCA assay (Pierce).

[0099] Dynamic light scattering analysis Dynamic light scattering (DLS) analysis of P-particles was performed using a Zetasizer Nano ZS instrument (Malvern Instruments Ltd., Worcestershire, UK). The hydrodynamic diameter was determined using three 10 × 10 sec datasets in PBS at 25°C. Samples were also subjected to stepwise heating, as described by Koho et al. (Antiviral Research 104 (2014) 93-101). That is, starting at 25°C, each sample was increased by 5°C, and equilibrated at each temperature for 5 minutes before analysis. Samples were heated to a final temperature of 90°C and then cooled to 25°C. To investigate the integrity and composition of P-particles dissolved in PBS from the continuous hybrid / complex hydrogel R217-0.2, analysis was performed using DLS at 25°C.

[0100] Endotoxin measurement To confirm that endotoxins had been removed from the purified antigen, the endotoxin levels of P-particles were measured using the ToxinSensor™ Gel Clot Endotoxin Assay Kit (GenScript) according to the manufacturer's instructions.

[0101] Norovirus VLP manufacturing and purification Norovirus (NoV) GII capsid virus-like particles (VLPs) derived from GII.4 (1999, acc. no. AF080551), GII.4 New Orleans (NO; 2010, acc. no. GU445325), GII.4 Sydney (Syd; 2012, acc. no. AFV08795.1), GII.12 (1998, acc. no. AJ277618), and GII.17 (2015, acc. no. BAR42289) are referenced in other literature (Huhti et al. Arch Virol 2010 155; Blazevic et al. Vaccine 2011 29; Malm et al. Clinical and vaccine immunology 2015). As described in detail in 22), it was produced in Sf9 insect cells using a Bac-to-Bac baculovirus expression system (Invitrogen, Carlsbad, CA) and purified by sucrose gradient ultracentrifugation. These VLPs were used as antigens in in vitro immunogenicity assays.

[0102] Animal immunization Sterile female 6-week-old BALB / c OlaHsd mice (Envigo, Horst, Netherlands) were randomly divided into eight groups (Groups I-VIII, 3 or 5 mice per experimental group) and acclimatized under specific control conditions for one week before the start of the experiment. Animals were immunized with NoV P- particles diluted in sterile PBS (Lonza, Verviers, Belgium) in two doses of 10 μg or one dose of 20 μg, or with continuous hybrid / complex R217-0.2 or biphase hybrid / complex #1R217-0.2 / R40-0.2 (A and B, Table 3) hydrogels. The test substance was administered by subcutaneous (sc) injection (100 μl volume) into the right flank during weeks 0 and 3 of the study. Table 5 shows the vaccine formulation, injection dose, and immunization method used. The control group received only P-particles containing R217-0.2 or R217-0.2 / R40-0.2 hydrogel, or Al(OH)3 (Alhydrogel; InvivoGen, San Diego, California). Immunization was performed under general anesthesia by inhalation of isoflurane (Attane vet, Vet Medic Animal Health Oy).

[0103] To examine the dynamics of the serum antibody response, blood samples were collected from the tail during study week 0 (before blood collection, non-immune serum) and study week 3. Whole blood and feces were collected at the time of slaughter (5 or 6 weeks) and processed according to known procedures ("Norovirus VLPs and rotavirus VP6 protein as combined vaccine for childhood gastroenteritis" Blazevic et al, Vaccine Oct 19;29(45):8126-33.; "A comparison of immunogenicity of norovirus GII-4 virus-like particles and P-particles", Tamminen et al., Immunology 2012 Jan;135(1):89-99). The experimental procedures were carried out in accordance with the rules and guidelines of the Finnish National Experimental Committee (permit number ESAVI / 10800 / 04.10.07 / 2016). Every effort was made to minimize animal suffering. Animal welfare was monitored throughout the study period.

[0104] Table 5 shows the antigen composition, injection volume, and immunization method.

[0105] [Table 5]

[0106] Antigen-specific antibody reaction The antibody reaction against P-particles was determined by measuring IgG and IgG subtype levels in individual mouse serum samples using ELISA. The ELISA procedure used was similar to one previously published by our laboratory (Blazevic et al. Vaccine 2011 29; Tamminen et al. Immunology. 2012 135(1):89-99), and therefore only a brief outline is provided below. Half-area polystyrene plates (Corning Inc., Corning, NY) were coated with 50 ng of NoV P- particles per well. Antigen-specific antibodies in serum at a 1:200 dilution or 2-fold serial dilution were detected using combinations of HRP-conjugated anti-mouse IgG (Sigma-Aldrich), IgG1 (Invitrogen), or IgG2a (Invitrogen) with a SIGMA FAST OPD substrate (Sigma-Aldrich). The endpoint titer was defined as the reciprocal of the highest sample dilution at OD490 (>0.1 OD490 units) exceeding the cutoff value.

[0107] Antibody avidity The avidity of NoV GII.4-specific IgG antibodies was evaluated in 1:200 diluted serum according to the ELISA method described in 1.5 above (Tamminen et al. Immunology. 2012 135(1):89-99), but additional urea treatment was performed to remove antibodies with low avidity. The plates were coated with 50 ng of NoV GII.4 VLP. The results were expressed as the avidity index: (OD490 with urea / OD490 without urea) × 100%.

[0108] Cross-reactive antibodies Cross-reactive NoV-specific IgG antibodies were detected by ELISA as described above. However, the plates were coated with 50 ng of heterologous NoV VLPs containing GII.4 NO, GII.4 Sydney, GII.12, and GII.17 VLPs per well. A 1:200 serum dilution was used for the assay.

[0109] Blocking antibody The ability of the inducing antibody to prevent the binding of NoV VLP to the HBGA receptor was evaluated in a blocking assay using PGM type III (Sigma Chemicals) as the HBGA source (Lindesmith et al. J Virol 2012; 86:873-83) according to a previously known procedure (Malm et al. Clin Exp Immunol 2017;189(3):331-41). Specifically, a mixture of pre-incubated GII.4 VLP and serially diluted serum was added to a microwell plate coated with PGM. The bound VLPs were detected using a combination of human NoV GII.4 antiserum and HRP-bound anti-human IgG according to the receptor binding assay described in 1.2. The results were expressed as a blocking index: 100% - [(OD490 sample / OD490 maximum binding) × 100%].

[0110] Mucosal IgG reaction To detect mucosal IgG antibodies, serially diluted 10% fecal suspensions were tested using the ELISA method described in 1.5 above. Plates were coated with 50 ng of NoV GII.4 VLP.

[0111] Results and Discussion In vitro dissolution and antigen release Figures 6-8 show the in vitro dissolution results for antigen (P-particle) release rate and silica dissolution rate of different hybrid / complex hydrogels. Figure 6A shows the antigen (P-particle) release rates for two variations of continuous hybrid / complex R217-0.2 and two-phase hybrid / complex hydrogel #1; R217-0.2 / R40-0.2A (antigen (AG) present in both R217-0.2 and R40-0.2 hydrogels) and R217-0.2 / R40-0.2B (antigen (AG) present only in R40-0.2 hydrogel) after being placed in syringes in aluminum foil bags and stored at room temperature (25°C) for 4 days and 330 days, respectively. Figure 6B shows the cumulative release of silica under the same conditions.

[0112] Figure 7 shows the cumulative release of antigen (P-particles) and silica dissolution for two-phase hybrid / complex hydrogel #2C. The weight ratios of silica and P-particle emissions at different time points are shown on the second Y-axis on the right.

[0113] Figure 8 shows the cumulative release of antigen (P-particles) and dissolution of silica in two-phase hybrid / composite hydrogel #2D. The weight ratio of silica and P-particle release at different time points is shown on the second Y-axis on the right.

[0114] The release results of R217-0.2 containing encapsulated eGFP indicate that silica dissolution and eGFP release occur simultaneously, although there are slight differences in the amount of encapsulated eGFP. In the case of 20 μg of eGFP in 100 μl of R217-0.2, both the release rate of eGFP and the dissolution rate of silica are initially slightly slow, but reach approximately 100% almost simultaneously.

[0115] Figure 9 shows the cumulative release of eGFP and the dissolution of silica in R217-0.2 after adding 10 μg of eGFP to 100 μl of hydrogel. The weight ratios of silica and eGFP release at different time points are shown on the second Y-axis on the right.

[0116] Figure 10 shows the cumulative release of eGFP and the dissolution of silica in R217-0.2 when 20 μg of eGFP is added to 100 μl of hydrogel. The weight ratio of silica to eGFP release at different time points is shown on the second Y-axis on the right.

[0117] To investigate the encapsulation efficiency of the material, the cumulative release of eGFP from a silica-saturated dissolution medium containing 10 μg and 20 μg of eGFP per 100 μl of hydrogel from R217-0.2 was measured. As shown in Figures 9 and 10, the rate at which eGFP diffused from the hydrogel during the first 5 hours was approximately 50% slower than under sink conditions. The release rate slowed slightly after 24 hours, leveling off at 25% for the 10 μg / 100 μl material and 35% for the 20 μg / 100 μl version.

[0118] Figure 11 shows the cumulative diffusion of eGFP from R217-0.2 at an eGFP concentration of 10 μg / 100 μl of hydrogel.

[0119] Figure 12 shows the cumulative diffusion of eGFP from R217-0.2 at an eGFP concentration of 20 μg / 100 μl of hydrogel.

[0120] Since the eGFP concentration after 24 or 25 hours is less than 0.5% of the protein stock concentration, it is unlikely that eGFP will prevent its own release in terms of saturation. Furthermore, during diffusion measurements, when the sample volume was 10 μg / 100 μl, the release rate of eGFP reached a plateau after 24 hours and remained somewhat stable, a similar observation was made with the 20 μg / 100 μl version, which also appeared to be stable. Compared to dissolution in the sink, this suggests that while some diffusion occurs, the entire eGFP payload is not effectively released unless the material decomposes.

[0121] Rheology Figure 13 shows the decay coefficients (G'' / G') for continuous hybrid / composite hydrogel R217-0.2 and two-phase hybrid / composite hydrogel #1 (R217-0.2 / R40-0.2) on day 4 and day 28 after storage in syringes surrounded by aluminum foil bags at room temperature (25°C).

[0122] Figure 14 shows the decay coefficient (G'' / G') for continuous hybrid / composite hydrogel R217-0.2 and two-phase hybrid / composite hydrogel #1 (R217-0.2 / R40-0.2) after 360 days of storage at room temperature (25°C). The syringes were isolated in an aluminum foil bag. The sample underwent a three-part measurement process: the first step was a frequency sweep, followed by a rotational measurement (shear rate ramp 1-100 1 / s), and then another frequency sweep measurement.

[0123] Figure 15 shows the dynamic viscosity of continuous hybrid / complex hydrogel R217-0.2 and two-phase hybrid / complex hydrogel #1 (R217-0.2 / R40-0.2) after 4 days of storage at room temperature (25°C).

[0124] Figure 16 shows the dynamic viscosity of continuous hybrid / complex hydrogel R217-0.2 and two-phase hybrid / complex #1 (R217-0.2 / R40-0.2) after 360 days of storage in a sealed aluminum foil bag at room temperature.

[0125] Rheological measurements show that the investigated hybrid / composite hydrogels retained their rheological properties very well even after being stored for 28 days in syringes placed in aluminum foil bags at 25°C. The damping coefficient (also called the loss tangent or loss coefficient) is the ratio of the loss modulus to the storage modulus (G'' / G') and indicates the viscoelastic properties of a hybrid / composite hydrogel at rest (e.g., in a syringe). The results of the decay coefficient indicate that the hydrogel retains its structure during storage and that its properties do not change significantly even after being stored at 25°C for 28 days (Figure 13). Dynamic viscosity (Figure 16) simulates injection from a syringe, and both hydrogels examined clearly showed shear thinning after being stored at 25°C for 4 days. The properties remained relatively unchanged over one year (Figures 14 and 17). The difference primarily occurs in dynamic viscosity. Overall, the minimum viscosity at low shear rates is significantly reduced, and the rate at which the material shears is slower compared to the D4 and D28 cases. The overall behavior remains unchanged, and the material was able to retain its rheological properties during storage.

[0126] Injectability In addition to rheological measurements, the injectability and stability of the hybrid / composite hydrogels were evaluated by injecting the material through a 25G needle from a 1ml syringe. The potential for injectability or phase separation was evaluated on a scale from 0 to 5 for continuous hybrid / composite hydrogels embedded with P-particle R217-0.2(AG), and two variations of two-phase hybrid / composite hydrogel #1 embedded with P-particle R217-0.2(AG) and P-particles (R217-0.2-R40-0.2(AG) and R217-0.2(AG)-R40-0.2(AG)), after storage in syringes in aluminum foil bags at room temperature (25°C) for 4, 28, 180, and 330 days (Table 6). The criteria for injectability smoothness were defined as follows: 5 = Very smooth, 4 = Mostly smooth, 3 = Fairly smooth, 2 = Partially smooth, 1 = Uneven, not smooth at all, 0 = Cannot be injected. The criteria for phase separation are defined as follows: 5 = No phase separation, 4 = Minimal phase separation, 3 = Phase separation present but reversible after injection, 2 = Phase separation present but irreversible after injection, 1 = Clear phase separation, 0 = Not gel at all.

[0127] Table 6 shows injection experiments regarding injection smoothness and phase separation at various time points after storage at 25°C. The scores are the average of three repeated injections.

[0128] [Table 6]

[0129] The injection experiment showed that the smoothness observed on day 4 did not change during storage, and the small changes observed between the continuous hybrid / complex hydrogel and the two-phase hybrid / complex hydrogel #1 stemmed from structural differences, namely the distinct gel particles present in both versions of the two-phase hybrid / complex hydrogel #1. While all of them are injectable, the results suggest that R217-0.2(AG)-R40-0.2(AG), which contains P-particles encapsulated in both the continuous and dispersed phases, is somewhat heterogeneous in nature, but is still injectable. Because the amount of encapsulated antigen is very small, it is unlikely to have such an effect; rather, it is a slight difference in the preparation process (the addition of P-particles in R217-0.2), which highlights the need for strict control of the preparation process. The minimal or fair phase separation observed is related to the initial release of small amounts of water or clumps of hydrogel associated with the injection. However, these gel clumps reintegrate after the injection, forming a molded hydrogel body.

[0130] Aggregation of P-particles in high-temperature solutions As previously shown (Journal of Virological Methods 179 (2012) 1-7), norovirus P-particles, when analyzed by DLS, have a diameter of approximately 15-17 nm in solution (not shown). To investigate the thermal stability of P- particles, we first determined the temperature at which they aggregate in solution. This analysis revealed that rapid temperature-induced aggregation occurs at temperatures above 50°C, and all P- particles form aggregates in the range of 300–830 nm at 55°C (Figure 17). Based on these results, long-term storage and dissolution experiments were conducted using the following temperatures: RT, 37°C, and 50°C.

[0131] Figure 17 shows the thermal stability of P-particles measured by DLS. Figure 17A shows the proportion of 16 nm particles at different temperatures, and Figure 17B shows the difference in volume distribution of P-particles measured at 50°C and 55°C. Both Figures 17A and 17B show the average of three individual measurements.

[0132] Particle consistency after dissolution The consistency of particles dissolved from the hydrogel was examined using DLS. During a 28-week follow-up, virtually all particles released from hydrogels kept at room temperature remained at their expected size, and particles released from hydrogels kept at 37°C were within the expected radius range of 15–17 nm up to 19 weeks (Figure 18). Control samples in solution stored at RT remained intact, while those stored at 37°C began to deteriorate after 6 weeks and were completely destroyed within 16 weeks. Furthermore, both hydrogel and solution samples kept at 50°C deteriorated within 4 weeks and 2 weeks, respectively.

[0133] Figure 18 shows the total volume of 16 nm aggregates of P-particles released from a continuous hybrid / composite hydrogel R217-0.2 (Figure 18A) or from control particles kept in a solution at a temperature determined by DLS (Figure 18B).

[0134] TEM image Transmission electron microscope images show that the hydrogel protects P-particles longer at 37°C than control particles kept at the same temperature in solution.

[0135] TEM shows that the control P-particle has a typical shape and is of the expected size of approximately 17–20 nm (Figure 19, top panel). P-particles remain stable in solution at RT for 20 weeks (Figure 19, lower left panel), but appear to disappear when kept in solution at 37°C for 12 weeks (Figure 19, center panel). P-particles dissolved from the hydrogel after storage at RT and 37°C appear intact even after 19 weeks (Figure 19, lower center panel).

[0136] Endotoxin level The endotoxin level was determined to confirm the removal of endotoxins from the antigen. Since the antigen did not contain bacterial endotoxins (<0.012 EU / 10 μg protein), no residual impurities were detected in the purified P-particles.

[0137] Generation of serum IgG antibodies To investigate the potential of this hydrogel to function as an adjuvant / delivery system, mice were immunized with two 10 μg doses of P-particles alone, or embedded in a continuous hybrid / complex R217-0.2 hydrogel, or with a single 20 μg dose of P-particles alone, or embedded in a two-phase hybrid / complex #1R217-0.2 / R40-0.2 hydrogel. For comparison, one of the experimental groups was administered P-particles containing Al(OH)3. Figure 20 shows the development of serum IgG antibodies against P-particles at study weeks 0, 3, and 5 or 6. The results showed that a single dose of P-particles induced only a very strong immune response when co-administered with the antigen in R217-0.2 hydrogel or R217-0.2 / R40-0.2A hydrogel (25 wt-%, antigen in R217-0.2). This indicates that the increase in antibody response at 3 weeks after monoimmunization originated from the R217-0.2 component rather than the R40-0.2 component. A second dose of P-particles containing the R217-0.2 hydrogel significantly increased the already induced response.

[0138] Figure 20 shows the dynamics of serum IgG antibodies in mice after immunization with two 10 μg doses of P-particles (pp) alone or in combination with R217-0.2 hydrogel (Figure 20A), or with a single 20 μg dose of P-particles alone or in combination with R217-0.2 / R40-0.2 hydrogel (Figure 20B). Control mice were administered either P-particles containing Al(OH)3 or a hydrogel that did not contain the antigen. The group-mean OD values ​​for tail blood samples and final serum during the indicated study week are shown. Immune points are indicated by arrows.

[0139] Furthermore, the geometric mean titer was considerably higher in the group of mice administered P-particles containing R217-0.2 or R217-0.2 / R40-0.2A hydrogel (25% by weight of antigen in R217-0.2) (reciprocal titer > 4.2 log). 10 ), simultaneous administration yielded levels 18 times or 10 times higher than those observed with P-particles alone (Figure 21). This indicates that R217-0.2 increases the magnitude of the antigen-specific IgG response. However, the observed effect of R217-0.2 on P-particles is similar to that of Al(OH)3 hydrogel (Figures 21 and 22). Negative control mice showed no response to P-particles.

[0140] Figures 21A and 21B show the endpoint titration of serum IgG in mice immunized with two 10 μg doses of P particles (pp) alone or with R217-0.2 hydrogel (Figure 21A), or with a single 20 μg dose of P- particles alone or with R217-0.2 / R40-0.2 hydrogel (Figure 21B). Control mice were administered P- particles containing Al(OH)3 or a hydrogel without the antigen. The mean OD of the group is shown.

[0141] Serum antigen-specific IgG1 and IgG2a subtypes Analysis showed that only P-particles formulated with the antigen-specific IgG subtypes IgG1 (characteristic of Th2 reaction) and IgG2a (characteristic of Th1 reaction) in a continuous hybrid / complex hydrogel R217-0.2 or Al(OH)3 induce mixed immunoassays, i.e., Th2 and Th1 types (Figures 22 and 23). Although each P-particle formulation induced a Th2 immune response, co-administration of P-particles with R217-0.2, or two-phase hybrid / complex #1R217-0.2 / R40-0.2A hydrogel (25% by mass of antigen in R217-0.2), or Al(OH)3 generated higher levels of IgG1 compared to administration of P-particles alone (Figure 22). Rather, a moderate Th1 immune response was induced only by P- particles administered simultaneously with R217-0.2 hydrogel or Al(OH)3 (Figure 23). These results suggest that R217-0.2 improves the quality of the immune response and preferably functions as a Th2 adjuvant similar to Al(OH)3.

[0142] Figure 22 shows the endpoint titration of serum IgG1 in mice immunized with two 10 μg doses of P-particles (pp) alone or in combination with R217-0.2 hydrogel (Figure 22A), or with a single 20 μg dose of P-particles alone or in combination with R217-0.2 / R40-0.2 hydrogel (Figure 22B). Control mice were administered either P-particles containing Al(OH)3 or a hydrogel without the antigen. The mean OD of the group is shown.

[0143] Figure 23 shows the endpoint titration of serum IgG2a in immunized mice using two 10 μg doses of P-particles (pp) alone or in combination with R217-0.2 hydrogel (Figure 23A), or a single 20 μg dose of P-particles alone or in combination with R217-0.2 / R40-0.2 hydrogel (Figure 23B). Control mice were administered either P-particles containing Al(OH)3 or a hydrogel without the antigen. The mean OD of the group is shown.

[0144] Antibody avidity Individual immunoserological evaluations regarding the avidity of anti-GII.4 IgG antibodies (Figure 24) showed that immunization with P-particles alone induced antibodies with significantly lower avidity (avidity index <10%) compared to antibodies induced with a combination of P-particles and continuous hybrid / complex hydrogel R217-0.2 or two-phase hybrid / complex hydrogel #1R217-0.2 / R40-0.2A hydrogel (25 wt% antigen in R217-0.2) (avidity index >60%). Nearly the same level was induced by P-particles containing Al(OH)3. This analysis indicates that R217-0.2 enhances antibody affinity.

[0145] Figure 24 shows the avidity of serum IgG antibodies in mice immunized with two 10 μg doses of P-particles (pp) alone or in combination with R217-0.2 hydrogel (Figure 24A), or with a single 20 μg dose of P-particles alone or in combination with R217-0.2 / R40-20 hydrogel (Figure 24B). Control mice were administered either P-particles containing Al(OH)3 or a hydrogel without the antigen. The mean avidity index (%) for each group is shown.

[0146] Cross-reactive serum IgG reaction Serum antibody cross-reactivity was measured against four heterologous NoV VLPs derived from gene group II (GII.4 NO, GII.4 Sydney, GII.12, and GII.17). No cross-reactive IgG antibodies were detected after immunization with P-particles alone, but antibodies with fairly broad cross-reactivity were obtained with R217-0.2 hydrogel or formulations containing Al(OH)3 (Figure 25). The results suggest that the increase in cross-reactive antibody reactions originates from R217-0.2 but not from R40-0.2.

[0147] Figure 25 shows cross-reactive serum IgG responses to heterologous NoV VLPs in mice immunized with two 10 μg doses of P-particles (pp) alone or in combination with a continuous hybrid / complex R217-0.2 hydrogel (Figure 25A), or with a single 20 μg dose of P-particles alone or in combination with a two-phase hybrid / complex #1 R217-0.2 / R40-0.2 hydrogel (Figure 25B). Control mice were administered P-particles containing Al(OH)3 or a hydrogel without the antigen. The mean OD of the group is shown.

[0148] neutralizing antibody The neutralizing ability of the induced antibodies was investigated by measuring their blocking activity against homologous GII.4 VLPs using a PGM-based blocking assay. Experimental groups receiving either a 10 μg dose of P particle formulation or a 20 μg dose of a two-phase hybrid / complex #1 R217-0.2 / R40-0.2A (containing 25 wt% antigen in R217-0.2) produced antibodies with detectable blocking ability, and their activity was significantly increased by co-administration of a continuous hybrid / complex R217-0.2 hydrogel or Al(OH)3 with the antigen (Figure 26). Only P-particles containing R217-0.2 hydrogel or Al(OH)3 induced antibodies capable of blocking VLP binding by more than 50%. Based on the analysis, the significant increase in blocking antibodies is attributable to formulations containing R217-0.2 and Al(OH)3.

[0149] Figure 26 shows homologous blockade of GII.4 VLP binding to the HBGA receptor by serum antibodies in mice immunized with two 10 μg doses of P-particles (pp) alone or with R217-0.2 hydrogel (Figure 26A), or with a single 20 μg dose of P-particles alone or with R217-0.2 / R40-0.2 hydrogel (Figure 26B). Control mice were administered either P-particles containing Al(OH)3 or a hydrogel without the antigen. The figures shown represent the mean blocking index (%) for each group.

[0150] mucosal antibodies Mucosal antibody analysis showed that immunization with P-particles alone resulted in very low (or negative) levels of fecal antibodies, while antigen formulation with serial hybrid / complex R217-0.2 hydrogel or Al(OH)3 increased the scale of mucosal antibodies (Figure 27).

[0151] Figure 27 shows the endpoint titration of fecal IgG antibodies in mice immunized with two 10 μg doses of P-particles (pp) alone or with R217-0.2 hydrogel (Figure 27A), or with a single 20 μg dose of P-particles alone or with a two-phase hybrid / complex R217-0.2 / R40-0.2 hydrogel (Figure 27B). Control mice were administered either P-particles containing Al(OH)3 or a hydrogel that did not contain the antigen. The displayed value is the group's average blocking index (%). The displayed value is the group's average OD (Optical Disorder).

[0152] conclusion The continuous hybrid / complex R217-0.2 hydrogel functions as an adjuvant to increase the magnitude of serum and mucosal immune responses, and to improve the quality and function of immune responses in terms of antibody avidity, cross-reactivity, and neutralizing antibodies.

[0153] The observed adjuvant effect of R217-0.2 is comparable to that of Al(OH)3 hydrogels. According to DLS, the proteins released from the hydrogel resemble the original P-particles. Furthermore, DLS indicates that the P-particles aggregate at temperatures above 55°C.

[0154] Furthermore, it was shown that 16nm particles may be released from the hydrogel after storage at room temperature and 37°C, but not after storage at 50°C, and that the concentration of released particles appears to decrease over time. Compared to storage in solution, this hydrogel appears to show an increased proportion of 15 nm particles at 37°C after a storage period of more than 5 weeks, suggesting stabilization of P- particles in the hydrogel.

Claims

1. A hydrogel material comprising a first hydrogel, the first hydrogel comprising: - 0.15% to 21% by weight of a functionalized triblock molecule having the structure of formula (1): 【Chemistry 1】 (1) Wherein, n is 4 to 680 and m is 1 to 10, based on the total weight of the first hydrogel; - 0.85 to 4.0% by weight of silica, based on the total weight of said first hydrogel; and - 75-99% by weight of an aqueous liquid based on the total weight of said first hydrogel, The -Si-OH groups of the silica are -Si-(O) groups of the functionalized triblock molecule of formula (1). 3 - groups and form -Si-O-Si- bonds.

2. The functionalized triblock molecule of formula (1) and silica form colloidal particles, 2. The hydrogel material of claim 1, wherein the network of particles forms a continuous solid phase within which an aqueous liquid phase is uniformly distributed, and wherein the solid phase and the aqueous liquid phase are within a single hydrogel entity.

3. The method further comprises the steps of: - 0.15 to 21% by weight of said functionalized triblock molecule of formula (1), based on the total weight of said second hydrogel; - 0.85 to 4.0% by weight of silica, based on the total weight of said second hydrogel; - 75-99% by weight of an aqueous liquid based on the total weight of the second hydrogel, Here, the -Si-OH groups of the silica are substituted with -Si-(O) groups of the functionalized triblock molecule of formula (1) of the second hydrogel. 3 - groups to form -Si-O-Si- bonds, and wherein the second hydrogel is in the form of uniformly distributed particles dispersed within the first hydrogel, the first hydrogel forming a continuous phase; 3. The hydrogel material of claim 1, wherein the total amount of silica and the functionalized triblock molecule having formula (1) in the second hydrogel is greater than the total amount of silica and the functionalized triblock molecule having formula (1) in the first hydrogel.

4. said functionalized triblock molecule of formula (1) and a first portion of an aqueous liquid are in the form of particles obtained by decomposing a hydrogel of said functionalized triblock molecule of formula (1) and an aqueous liquid into particles dispersed in a silica sol obtained by mixing with a second portion of an aqueous liquid; and The -Si-OH groups of the silica are linked to the -Si-(O) groups of the functionalized triblock molecule of formula (1) 3 2. The hydrogel material of claim 1, wherein the -Si-O-Si- group forms a -Si-O-Si- bond with the -Si-O-Si- group, thus forming a hydrogel material.

5. The hydrogel material according to claim 1 , wherein the silica is an alkoxysilane-derived silica.

6. The hydrogel material described in claim 5, wherein the silica is silica derived from tetraethoxysilane.

7. The aqueous liquid of the first hydrogel and the second hydrogel is 4. The hydrogel material of claim 3, wherein the hydrogel is independently selected from water, a mixture of water and ethanol, and a biologically compatible buffer.

8. 8. The hydrogel material of claim 7, wherein the aqueous liquid is a mixture of water and ethanol, containing 50-95% by weight water, the remainder being ethanol.

9. 9. The hydrogel material of claim 2, 5, 6, 7 or 8, further comprising at least one encapsulated biologically active agent in the first hydrogel.

10. 9. The hydrogel material of claim 3, 7 or 8, further comprising at least one encapsulated biologically active agent in at least one of the first hydrogel and the second hydrogel.

11. 9. The hydrogel material of claim 4, further comprising at least one encapsulated biologically active agent in the hydrogel of the functionalized triblock molecule of formula (1).

12. 12. The hydrogel material of claim 9, wherein the biologically active agent is selected from the group consisting of immunomodulatory agents and therapeutically active agents.

13. 13. Use of the hydrogel material according to any one of claims 1 to 12 for the protective encapsulation of a biologically active agent.

14. The use of claim 13, wherein the biologically active agent is encapsulated to ensure thermal stability.