Integrating carbon storage and metal value recovery through selective hydrometallurgy
Patent Information
- Application Number
- JP2023531576
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-26
- Filing Date
- 2021-11-26
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for carbon dioxide sequestration and metal value recovery from mineral feedstocks often release harmful mineral dissolution products and have unknown ecological impacts, lacking efficient integration of carbon capture with metal extraction processes.
A process integrating hydrometallurgical value extraction with electrochemical processes, using acid leachates and alkali hydroxides for selective precipitation of metals and carbonates, followed by electrolytic treatment to produce low-carbon-intensive products like nickel, iron, and magnesium hydroxides and carbonates, which can be used in construction materials and battery industries.
This method enables the co-production of low-carbon-intensive metal products and amorphous silicates, reducing the carbon footprint of industries like cement, tire, and battery manufacturing, while promoting low-carbon steelmaking and carbon dioxide capture.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical field
[0001] field The present invention is in the field of inorganic chemistry, integrating electrochemical processes with hydrometallurgical value extraction and carbon dioxide recovery steps. [Background technology]
[0002] background Technologies that efficiently sequester gaseous carbon dioxide could be an important tool in combating anthropogenic climate change. Various approaches have been proposed to sequester carbon as carbonates in minerals, including techniques that promote weathering reactions in minerals in ultramafic and mafic rocks. These approaches to promote weathering (on land) and improve ocean alkalinity (at sea) reduce CO 2 is consumed, but is always accompanied by the release of mineral dissolution products such as alkali species and metal compounds (e.g. Si, Ca, Mg, Fe, Ni, Co species). The ecological impact of these methods is unknown (Bach et al., CO 2 See Removal With Enhanced Weathering and Ocean Alkalinity Enhancement: Potential Risks and Co-benefits for Marine Pelagic Ecosystems, Frontiers in Climate, vol. 1, 2019, pg 7). Processes that integrate carbon capture and recovery of metal values from mineral feedstocks are needed. [Summary of the invention]
[0003] summary A process is provided in which successive steps of hydrometallurgical value extraction are carried out on mineral feedstocks such as olivine, mafic, saprolite or ultramafic feedstocks. In selected embodiments, the products of the carbon capture reaction and electrolytic reagent production process are utilized as inputs to a hydrometallurgical value recovery process. Electrolytic treatment uses acid leachate (HCl or H 2 S.O. 4 ) and alkali hydroxides (NaOH or KOH), which can be used directly as precipitants in hydrometallurgical processes or converted into alkali metal carbonates or bicarbonates that can be used as precipitants in hydrometallurgical processes. It can be used for conversion. In another embodiment, the alkali hydroxide from the chlor-alkali process can be used to precipitate the calcium hydroxide product, and the calcium hydroxide product can be used directly for use in carbon dioxide gas scrubbing, or C.O. 2 Can be used to accept carbonates provided by the scrubbing process.
[0004] Therefore, methods are provided for co-production from mineral feedstocks such as hydroxides and carbonate basalts of nickel, iron, calcium, and magnesium that are low in carbon intensity or low in carbon. Basaltic sand materials containing amorphous silicates can also be produced. These methods may include: (1) magnetic separation, (2) hydrochloric or sulfuric acid leaching, (3) selective precipitation of metal hydroxides or carbonates in successive steps with pH adjustment (optional). (4) electrolysis of the resulting effluent, e.g., NaCl (aq) Chlor-alkali process to treat Na 2 S.O. 4(aq) and (5) recycling of acid and alkaline reagents, e.g. in the case of chlor-alkali processes, the production of hydrochloric acid from the hydrogen and chlorine gas products of electrolysis.
[0005] The process of the invention allows the use of low carbon-intensive nickel, iron, calcium and magnesium hydroxides and carbonates, olivine and basaltic sands, amorphous silicates, etc. in marketable products. be able to. These can include, for example, feedstocks for the battery, steel, cement, tire, glass, aggregate, or concrete industries. The products of the process, such as solid silicate residues or iron precipitate products, may be subjected to, for example, washing and / or alkalization. Adjustment of pH by alkalization (alkali addition) improves the compatibility of the final product, making it suitable for use as a supplementary cementitious material (SCM) in cement, e.g. with improved cementitious properties. A residue can be generated.
[0006] The inventive method provides a path to co-produce less carbon-intensive nickel and iron hydroxides, and thus to decarbonize sectors relevant to the transition to a low-carbon economy, such as electric vehicles and batteries. there's a possibility that. The present invention also promotes low-carbon steelmaking by supplementing carbon-rich pyrometallurgy with carbon-reducing magnetic, hydrometallurgical, and electrochemical processes.
[0007] The method enables the co-production of low carbon-intensive amorphous silicates that can be sold as supplementary cement materials (SCM) for cement or in the tire manufacturing industry. Basaltic sand can be produced with an inert surface for use as aggregate in concrete mixtures. The invention facilitates the construction of concrete buildings with low carbon consumption.
[0008] Therefore, the following method is provided: Methods of processing crushed mineral feedstocks, including: optionally magnetically separating materials from the crushed mineral feedstock; a) leaching metal values from the ground mineral feedstock with an acid leachate to produce a solid siliceous residue and a loaded leachate; optionally subjecting the loaded leachate to a resin leaching process to selectively remove nickel and cobalt values from the loaded leachate to obtain a purified nickel and cobalt mixed product; optionally washing and / or alkalizing the solid siliceous residue to form a supplementary cementitious material (SCM), for example for use in cement; b) Precipitating iron and / or aluminum from a loaded leachate, the precipitation comprising: adding a first alkali metal carbonate or bicarbonate precipitating agent to produce a carbon dioxide offgas; or adding a first alkali hydroxide precipitant; producing a Fe / Al-depleted solution and a precipitate of iron and / or aluminum hydroxides or oxides (e.g. hematite); optionally carrying out cleaning and / or alkalization of iron and / or aluminum hydroxide precipitates; optionally adding a hematite seed material to the step of precipitating the iron and / or aluminum, further optionally the iron and / or aluminum hydroxide or oxide precipitate comprising a hematite seed material; recycling this to the precipitation process; c) Nickel and / or cobalt from a Fe / Al depleted solution or from a Ni / Co ion exchange eluate obtained from a Fe / Al depleted solution by selective extraction of nickel and / or cobalt on an ion exchange medium. precipitating, the precipitating being: a second alkali metal carbonate or bicarbonate precipitating agent, or a second alkaline hydroxide precipitant, to form a Ni / Co depleted solution and a nickel and / or cobalt carbonate or hydroxide precipitate; d) adding an oxidizing agent before or after step (c) to precipitate iron and / or aluminum and / or manganese from the Ni / Co-depleted solution, the precipitation comprising: a third alkali metal carbonate or bicarbonate precipitating agent, or third hydroxide alkali precipitant, to produce a Fe / Al / Mn depleted solution and iron and / or aluminum and / or manganese hydroxide precipitation products; optionally recycling the brine containing the Fe / Al / Mn depleted solution to the milling process to provide a milled mineral feedstock; e) Precipitating magnesium from a Fe / Al / Mn depleted solution, the precipitation comprising: a fourth alkaline hydroxide precipitant, or a fourth alkali metal carbonate or bicarbonate precipitating agent; to produce a Mg-depleted solution and a magnesium hydroxide or carbonate precipitation product; f) The Mg-depleted solution is subjected to electrolytic treatment to produce acid leachate and one or more alkaline hydroxide precipitants, or an alkali hydroxide product usable for conversion to one or more alkali metal carbonate or bicarbonate precipitates; generate; and g) Optionally CO 2 Separating carbon dioxide from contained gases. The method uses a scrubbing solution containing an alkaline hydroxide precipitant to remove CO2. 2 CO containing ambient air by treating the containing gas and producing one or more alkali metal carbonate or bicarbonate precipitants. 2 It may further include scrubbing carbon dioxide from the contained gas. Therefore, the following method is provided: Methods of processing crushed mineral feedstocks, including: a) leaching metal values from the ground mineral feedstock with an acid leachate to produce a solid siliceous residue and a loaded leachate; b) Precipitating iron and / or aluminum from a loaded leachate, the precipitation comprising: adding a first alkali metal carbonate precipitant to produce a carbon dioxide off-gas; or adding a first alkali hydroxide precipitant; producing a Fe / Al-depleted solution and a precipitate of iron and / or aluminum hydroxides or oxides (e.g. hematite); c) Nickel and / or cobalt from a Fe / Al depleted solution or from a Ni / Co ion exchange eluate obtained from a Fe / Al depleted solution by selective extraction of nickel and / or cobalt on an ion exchange medium. precipitating, the precipitating being: a second alkali metal carbonate or bicarbonate precipitating agent, or a second alkaline hydroxide precipitant, to form a Ni / Co depleted solution and a nickel and / or cobalt carbonate or hydroxide precipitate, such as a mixed Ni / Co hydroxide product; d) Before or after step (c), an oxidizing agent (chlorine gas (Cl 2(g) ) or sodium hypochlorite (NaOCl)) to precipitate iron and / or aluminum and / or manganese from the Ni / Co-depleted solution, the precipitation comprising: a third alkali metal carbonate or bicarbonate precipitating agent, or third hydroxide alkali precipitant, to produce a Fe / Al / Mn depleted solution and iron and / or aluminum and / or manganese hydroxide precipitation products; e) Precipitating magnesium from a Fe / Al / Mn depleted solution, the precipitation comprising: a fourth alkaline hydroxide precipitant, or a fourth alkali metal carbonate or bicarbonate precipitating agent; to produce a Mg-depleted solution and a magnesium hydroxide or carbonate precipitation product; f) The Mg-depleted solution is subjected to electrolytic treatment to produce acid leachate and one or more alkaline hydroxide precipitants, or alkali hydroxide products, to generate. The method may further include reacting the alkali hydroxide product of the electrolytic treatment, directly or indirectly, with a carbon source to produce one or more alkali metal carbonate or bicarbonate precipitants. The process of reacting the alkali hydroxide product with a carbon source involves CO2 in a scrubbing solution containing the alkali hydroxide product. 2 By processing the contained gas, CO 2 It can include scrubbing carbon dioxide from the contained gas and producing one or more alkali metal carbonate or bicarbonate precipitants. In selected embodiments, calcium is precipitated from the Mg-depleted solution with a fifth alkaline hydroxide precipitant to produce a calcium hydroxide product, and the calcium hydroxide product is converted to CO2. 2 May be treated with a containing gas or a carbon source such as a metal carbonate to produce one or more of an alkali metal carbonate or bicarbonate precipitant; 2 The contained gas may be air, for example. If the alkali hydroxide product contains NaOH, CO 2 Scrubbing carbon dioxide from the containing gas will correspondingly remove Na from the scrubbing solution. 2 C.O. 3 The hydrate is precipitated in the crystallization process and solid Na 2 C.O. 3 A crystalline product is produced, with one or more of the alkali metal carbonate or bicarbonate precipitates containing solid Na 2 C.O. 3 Contains crystalline products. In an alternative embodiment, the alkali metal carbonate or bicarbonate precipitant is NaHCO 3 , Na 2 C.O. 3 or K 2 C.O. 3 or a mixture thereof. The alkaline hydroxide precipitant may be one or both of NaOH, KOH, or a mixture thereof. Acid leaching solutions include, for example, HCl, H 2 S.O. 4 mineral acids such as, or mixtures thereof. Electrolytic treatment involves a chlor-alkali process and produces an alkali hydroxide precipitate and / or an alkali hydroxide product, Cl 2(g) product and H 2(g) products can be produced. Then Cl 2(g) product and H 2(g) The products can be reacted to produce HCl as an acid leachate. Mg-depleted solution is Na 2 S.O. 4 When containing H 2 S.O. 4 A salt decomposition step including: When precipitating magnesium from Fe / Al / Mn-depleted solutions using an alkaline hydroxide precipitant, CO 2(g) A precipitating agent can be added to produce a Mg-depleted solution and a magnesium carbonate precipitation product. C.O. 2(g) The precipitant may, for example, include or be made entirely of carbon dioxide offgas from a process that precipitates iron and / or aluminum from a loaded leachate. In alternative embodiments, an initial step of magnetically separating materials from the crushed mineral feedstock may be performed, for example, to enrich the feedstock with selective materials. In an alternative embodiment, the loaded leachate can be subjected to a resin leaching process to selectively remove nickel values from the loaded leachate to obtain a purified nickel product. The product of this step can be further processed, for example by washing and / or alkalizing solid siliceous residues, washing and / or alkalizing precipitates of iron and / or aluminum hydroxides or oxides. . A hematite seed material can be added to the step of precipitating the iron and / or aluminum to seed the precipitation of the hematite product. If the iron and / or aluminum hydroxide or oxide precipitate contains hematite seed material, the hematite seed material precipitates the iron and / or aluminum so as to seed the precipitation of the hematite product. may be recycled into the process. The brine containing some or all of the Fe / Al / Mn depleted solution can be recycled to the milling process to provide a milled mineral feedstock. The mineral feedstock may be, for example, nickel saprolite ore or slag, olivine ore or slag, asbestos ore or slag, mafic ore, saprolite material, ultramafic ore, olivine, wollastonite or combinations thereof. It may be one or more, or it may include one or more. [Brief explanation of drawings]
[0009] Brief description of the drawing
Figure 1
[0010]
Figure 2
[0011] [Figure 3] Figure 3 is a schematic diagram of an integrated process for extracting hydrometallurgical value from mineral feedstocks, where the reactants for the hydrometallurgical process are provided by carbon dioxide capture and a chlor-alkali electrochemical process.
[0012] [Figure 4] Figure 4 is a schematic diagram of an integrated process for extracting hydrometallurgical value from mineral feedstocks, where the reactants for the hydrometallurgical process are provided by carbon dioxide capture and a chlor-alkali electrochemical process.
[0013] [Figure 5] Figure 5 is a schematic diagram of an integrated process for extracting hydrometallurgical value from mineral feedstocks, where the reactants for the hydrometallurgical process are provided by carbon dioxide capture and chlor-alkali electrochemical process, Mg shows the use of Na2CO3 to precipitate.
[0014] [Figure 6]Figure 6 is a schematic diagram of an integrated process for extracting hydrometallurgical value from mineral feedstocks, where the reactants for the hydrometallurgical process are provided by carbon dioxide capture and chlor-alkali electrochemical process, Mg It shows the use of NaOH in combination with CO2(g) to precipitate .
[0015] [Figure 7] FIG. 7 is a schematic diagram of an integrated process for extracting hydrometallurgical value from mineral feedstocks, where the reactants of the hydrometallurgical process are provided by an electrolytic salt decomposition anion exchange process.
[0016] [Figure 8] Figure 8 is a schematic diagram of an integrated process for hydrometallurgically extracting value from mineral feedstocks, where the reactants of the hydrometallurgical process are provided by carbon dioxide capture (DAC) and electrolytic salt decomposition anion exchange processes. Ru.
[0017] [Figure 9] Figure 9 is a schematic diagram of an integrated process for hydrometallurgically extracting value from mineral feedstocks, where the reactants of the hydrometallurgical process are provided by carbon dioxide capture (DAC) and an electrolytic salt split anion exchange process. Ru.
[0018] [Figure 10] Figure 10 is a schematic diagram of an integrated process for extracting hydrometallurgical value from mineral feedstocks, where the reactants for the hydrometallurgical process are provided.
[0019] [Figure 11] FIG. 11 is a schematic diagram of an integrated process for hydrometallurgically extracting value from mineral feedstocks, including an initial stage of magnetic beneficiation to adjust the metal content of the processed material. [Details for carrying out the invention]
[0020] detailed description A method is provided for performing a continuous process of hydrometallurgical value extraction using carbon recovery (capture) and the products of an electrolytic reactant regeneration process, such as a chlor-alkali process or an electrolytic salt decomposition anion exchange process. The electrolytic reactant regeneration process provides an acid leachate and an alkali hydroxide, and the alkali hydroxide (such as NaOH) can be used directly as a precipitant in the hydrometallurgical process, or the alkali metal carbonate can be used as a precipitant in the hydrometallurgical process. Salt (Na 2 C.O. 3 etc.) and bicarbonate (NaHCO 3 etc.) can be used for conversion.
[0021] In an alternative embodiment, the alkali hydroxide from the chlor-alkali process can be used to precipitate the calcium hydroxide product, and the calcium hydroxide product can be used directly for carbon dioxide gas scrubbing or CO 2 It can be used to accept carbonate supplied from the scrubbing process.
[0022] In some embodiments, CO that has been treated with an alkali hydroxide (NaOH) product of a chlor-alkali process 2 Na from concentrated solution 2 C.O. 3 or Na 2 C.O. 3 A crystallizer step may be introduced to precipitate the hydrate. In such processes, a crystallizer can be used to reduce the water content in the hydrate by adjusting temperature, pressure, and NaOH concentration. Then solid Na 2 C.O. 3 The product can be used as a carbonate precipitant.
[0023] When carbonate precipitants are used to precipitate iron and aluminum from the leachate, at a suitably low pH, the carbonates decompose and release CO2. 2 discharges a concentrated stream of concentrated CO 2 The flow can in turn be isolated or fixed.
[0024] Figure 1 shows the leaching of metal values from a pulverized (“crushing and grinding”) mineral feedstock using an acid leaching solution (“HCl leaching”) to produce a solid siliceous residue (“amorphous silica residue for cement production”). ”) and shows the process of producing a loaded leach solution. As shown, the residue may be washed. Crushing and grinding in regenerated brine containing various chlorides or sulfates, such as magnesium and sodium salts, can be performed to avoid or minimize the need for non-brine additions. HCl acid leaching can be carried out at relatively high acid concentrations, such as 30-36% by weight HCl in water, which is a typical product from HCl production equipment attached to a chlor-alkali plant.
[0025] As shown in Figure 11, in one embodiment of the invention, the ferromagnetic content of the crushed ore is adjusted using, for example, a magnetic separator to increase or decrease the iron and nickel hydroxide products of the process. can do. For example, in inputs of (ultra)mafic sands containing olivine or wollastonite, MgSiO for nickel and iron 4 and CaSiO 4 The ratio of the contents of can be optimized through magnetic separation. As yet another method, a resin leaching process can be used to selectively remove the nickel content in the acidic leachate prior to the selective precipitation step to obtain a purified nickel product.
[0026] Leaching conditions can include leaching temperatures from 80°C to boiling point and above 115°C. Acid addition during HCl leaching may range, for example, from 500 to 1000 kg HCl per dry ton of solid feed, varying depending on the chemical composition of the feed. The leaching time may be, for example, an effective residence time of 1 hour to 8 hours. Leaching may be carried out, for example, in a single stage or in two or more countercurrent stages. In a single-stage process, the acid and ore are added together and allowed to react at the leaching temperature to completion. Multi-stage leaching involves contacting fresh ore with a partially reacted solution (low terminal acidity) to maximize acid usage, and in a second or subsequent stage, partial leaching (from the first stage). The ore is brought into contact with strong acids to maximize the extraction of Mg / Ni / Co / Fe, etc. Multi-stage processes may include additional solid-liquid separation steps to ensure countercurrent movement of solids and liquids.
[0027] The raw materials for this process can include various silicate minerals including magnesium, iron, nickel, cobalt and trace impurity elements. Therefore, the chemistry of acid leaching using HCl can be represented by the following reaction: Mg 2 SiO 4 + 4HCl = 2MgCl 2 +SiO 2 +2H 2 O Ni 2 SiO 4 + 4HCl = 2NiCl 2 +SiO 2 +2H 2 O Fe 2 SiO 4 + 4HCl = 2FeCl 2 +SiO 2 +2H 2 O
[0028] Other minerals present in the raw material, such as iron oxide and aluminum oxide, can also react with hydrochloric acid to form additional salts in solution: FeO(OH) + 3HCl = FeCl 3 +2H 2 O AlO(OH) + 3HCl = AlCl 3 +2H 2 O
[0029] Natural mineral raw materials are of course not pure compounds, so raw minerals contain various elements (e.g. Mg, Ni, Co, Fe in one silicate mineral) and may be hydrated or weathered. . Geologically, suitable feed materials include nickel saprolite ore, olivine ore, asbestos ore and slag.
[0030] The product of HCl leaching is a slightly acidic solution containing various chloride salts. The silica-rich residue is recovered as a solid product. This residue can be directed to cement production, e.g. by washing with fresh water to remove salts and excess acid and / or alkalizing (alkali-adjusting) to adjust the pH with a base. can be used as a replacement for other materials (thus lowering the carbon intensity of cement production), as a reinforcing agent to improve the yield strength of concrete, and as a supplementary cementitious material (SCM) in high-performance concrete.
[0031] Iron and / or aluminum can be mixed with alkali hydroxide (NaOH) or alkali metal carbonate or bicarbonate precipitants (NaOH as shown in Figure 1). 2 C.O. 3 ) from the loaded leachate (“Iron and Aluminum Precipitation”). Na 2 C.O. 3 is used as a precipitant, this is a carbon dioxide off-gas (“CO 2"off gas"), Fe / Al depleted solution, iron and / or aluminum hydroxide or oxide precipitate products ("Fe / Al hydroxide precipitate" as shown, consisting of magnetite in selective embodiments) generate. As shown, the residue is washed to provide a precipitate. When alkali hydroxide (e.g. KOH or NaOH) is used as a precipitant, the iron and aluminum content in the solution is generally reduced by increasing the pH with the alkali hydroxide (KOH or NaOH) solution. It is precipitated as a mixture of oxide solids. The NaOH solution can be added as a 50% solution, for example, and diluted with regenerated brine solution for process convenience and enhanced pH control (if adding a very strong base makes pH control difficult). ). Added NaOH neutralizes excess acid and precipitates Fe / Al and other trivalent cations if present: HCl + NaOH = NaCl + H 2 O FeCl 3 + 3NaOH = FeO(OH) + 3NaCl + H 2 O 2FeCl 3 + 6NaOH = Fe 2 O 3 (Hematite) + 6NaCl + 3H 2 O AlCl 3 + 3NaOH = AlO(OH) + 3NaCl + H 2 O 2AlCl 3 + 6NaOH = Al 2 O 3 + 6NaCl + 3H 2 O CrCl 3 + 3NaOH = CrO(OH) + 3NaCl + H 2 O 2CrCl 3 +6NaOH = Cr 2 O 3 + 6NaCl + 3H 2 O
[0032] pH adjustment can be carried out, for example, with stoichiometric amounts of alkali hydroxide. Base addition needs to be kept under control as excessive addition of NaOH can lead to Ni / Co precipitation (undesirable). The precipitation temperature of Fe / Al can be, for example, from 75° C. to the boiling point. Seeds (precipitates) can be recycled, for example in the form of hematite, to ensure growth of appropriately sized particles and materials to enhance solid-liquid separation. An initial mineral species, such as hematite, may be used to begin the process of precipitating a selected material, such as hematite. The Fe / Al precipitation time may be, for example, 1 to 8 hours. NaOH can be added stepwise through the settling tank (continuous), for example to promote settling of coarser / separable precipitates. The Fe / Al precipitation product may be subjected to S / L separation and washing.
[0033] The Fe / Al precipitation residue may be processed to form commercial products such as hematite, for example. For example, drying and partial reduction can be used to form magnetite and mixed Al / Cr oxides. Magnetite can be separated using magnetic separation and Al / Cr oxides can be sold as products for the refractory market.
[0034] Nickel and cobalt can be selectively recovered in a variety of ways. In HCl-based leaching process, Ni and Co are in solution with NiCl 2 and CoCl 2 Existing as salts, these salts can be recovered by ion exchange to extract Ni and Co in Na-foam resin using, for example, Dow M4195 resin. This resin can then be stripped with an HCl solution to form a highly purified solution of Ni / Co chloride salts. The resin can then be treated with NaOH solution after acid stripping and returned to the resin "loading" step.
[0035] In selected embodiments, Ni / Co recovery is by a mixed hydroxide precipitation (MHP) method. This can be done directly from the solution coming from the iron precipitation step or can be effective starting from an ion exchange eluent containing nickel chloride and cobalt chloride. In these methods, a solution of sodium hydroxide is added from the precipitate: NiCl 2 + 2NaOH = Ni(OH) 2 +2NaCl CoCl 2 + 2NaOH = Co(OH) 2 +2NaCl
[0036] Other metals may also precipitate together with Ni / Co, albeit in small amounts. For example, Mn, Fe (iron remaining in solution).
[0037] The selectivity of MHP precipitation for Ni / Co can be increased by using a two-stage MHP precipitation, in which the second stage precipitate is recovered and the effluent from the first stage or main leaching step is removed. (where acid is present to redissolve the Ni / Co and other metals from the second stage leaching).
[0038] The mixed hydroxide precipitate can be recovered by S / L separation and washing. To minimize entrained moisture in the cleaned Ni / Co MHP cake before shipping, a pressure filter can be used in a "squeeze" cycle.
[0039] Ni / Co MHP precipitation can be carried out at a temperature between 25 and 90°C with a terminal pH set in the range of 5 to 8. Base addition can also be controlled by stoichiometry, rather than or in addition to pH. The precipitation time of Ni / Co MHP may be, for example, 1 to 8 hours. Seed recycling can be used to maximize particle size and minimize contamination. The Ni / Co MHP process (in all steps) can be performed continuously.
[0040] As shown in Figure 1, in an alternative embodiment, the nickel and / or cobalt is combined with a second alkali metal carbonate or bicarbonate precipitant (Na 2 C.O. 3 ) can be used to precipitate from Fe / Al depleted solutions to produce Ni / CO depleted solutions and nickel and / or cobalt carbonate precipitates ("Ni / CO carbonates (for battery production)").
[0041] Most of the iron and aluminum are removed from the solution in the first iron removal step. Manganese is generally not removed from solution in either the initial iron control or Ni / Co MHP precipitation steps. Therefore, the second stage of iron precipitation is carried out to maximize iron removal with oxidants added to oxidize Mn and Fe to promote more complete removal and purification of all species. It can be carried out at elevated pH. Suitable oxidizing agents include gaseous chlorine or sodium hypochlorite (NaOCl). Examples of reactions include: 2FeCl 2 + NaOCl + 4NaOH = 2FeO(OH) + 5NaCl + H 2 O MnCl 2 + NaOCl + 2NaOH = MnO 2 + 3NaCl + H 2 O AlCl 3 + 3NaOH = AlO(OH) + 3NaCl + H 2 O
[0042] Conditions for iron and / or aluminum and / or manganese scrubbing can be designed to maximize precipitation of impurity elements while minimizing magnesium hydroxide formation. An oxidizing agent (eg, NaOCl) can be added to achieve suitably high oxidation / reduction potentials (ORP) to maximize oxidative removal of Fe / Mn. The scrubbing temperature can be, for example, 25° C. up to the boiling point. As with other precipitation processes, seed recycling can be used to improve performance. The scrubbing time can be, for example, 1 to 8 hours.
[0043] Alternatively, as illustrated in Figure 1, the iron and / or aluminum and / or manganese can be combined with a third alkali metal carbonate or bicarbonate precipitant (Na 2 C.O. 3 Scrub the Ni / CO depleted solution with an oxidizing agent, e.g. "Fe / Al / Mn hydroxide precipitate") may be generated. As illustrated, the brine containing the Fe / Al / Mn depleted solution can be recycled to the milling process to provide a milled mineral feedstock.
[0044] Magnesium remaining in solution is precipitated from the Fe / Al / Mn-depleted solution using an alkaline hydroxide precipitant (e.g. NaOH) and the Mg-depleted solution and magnesium hydroxide precipitate (“Mg hydroxide precipitate”). can be produced: MgCl 2 + 2NaOH = Mg(OH) 2 +2NaCl
[0045] This is, for example, MgCl 2can be carried out by adding NaOH to a solution of or by reversing the order of addition. In either case, the method can be carried out to almost completely remove Mg from solution as Mg(OH)2. In this case, approximately stoichiometric addition of NaOH is generally required.
[0046] The Mg-depleted solution is then subjected to further purification, e.g. in an ion-exchange resin separation step, or sent directly to electrolysis to produce an alkaline hydroxide precipitant and acid leachate (in Fig. Figure 7 shows a chlor-alkali plant producing HCl and NaOH for recycling. 2 S.O. 4 and a salt cracking plant that produces NaOH”). Standard chloralkali brine pretreatment may be performed on the Mg-depleted solution, e.g., to provide a purer Mg-depleted brine essentially free of undesirable solids and ions, e.g. Brine saturation / evaporation and softening, including first and abrasive filtration steps and high performance ion exchange softening. In the HCl-based extraction process, the final Mg-depleted solution is NaCl (aq) , some contaminants are present in the solution. This NaCl (aq) The solution is NaOH, Cl 2 and H 2 It is sent to a chlor-alkali plant for producing Cl 2 and H 2 is burned and washed with water to form a strong hydrochloric acid solution for reuse in leaching. Cl 2 and H 2 Excess heat from the combustion of can, for example, be recovered as steam and used to evaporate excess water from the solution.
[0047] As shown in Figure 1, CO 2 The containing gas is treated with a scrubbing solution containing an alkali hydroxide precipitant (NaOH as shown) to remove an alkali metal carbonate or bicarbonate precipitant (NaOH as shown). 2 C.O. 3 ) by producing one or more of the CO 2 Carbon dioxide may be scrubbed from the contained gas ("air" as shown).
[0048] In the method described above, CO 2 The process of scrubbing carbon dioxide from the containing gas removes Na from the scrubbing solution. 2 C.O. 3 A crystallization step may be included to precipitate the hydrate, and the alkaline hydroxide precipitant is NaOH. Solid Na 2 C.O. 3 The crystallizer can then be fed with one or more alkali metal carbonate or bicarbonate precipitating agents.
[0049] FIG. 2 shows a process similar to that shown in FIG. 1, using a potassium compound in place of the sodium compound in FIG.
[0050] Figures 3 and 4 illustrate an alternative implementation of precipitating calcium from a Mg-depleted solution using a fourth alkali metal hydroxide precipitant (NaOH as shown) to produce a Ca-depleted solution and a calcium hydroxide product. It shows the form. The calcium hydroxide product is then processed through an iron and / or aluminum precipitation step, for example by treating the calcium hydroxide product with a carbon source such as air (Figure 3) or carbon capture via KOH (Figure 4). can be used for carbon sequestration reactions by producing metal carbonate precipitates. In these methods, a Ca-depleted solution is subjected to electrolysis to produce one or more of a first, second, third or fourth alkali metal hydroxide precipitant and acid leaching agent.
[0051] The alkaline hydroxide precipitant may be NaOH (Figures 1, 3, 4) or KOH (Figure 2) accordingly. An exemplary process acid leachate is HCl. These products can be produced in a chlor-alkali process.
[0052] Figures 5 and 6 show that Mg(OH) 2 rather than MgCO 3 7 illustrates an alternative embodiment in which alternative paths are used to form a . These embodiments are based on Mg(OH) from the present process. 2 reflects indications for the use of: (1) CO 2 Direct air capture (DAC) of MgCO 3 or (2) by ocean alkalinity enhancement (OAE), Mg(OH) 2 directly added to the marine environment, Mg(HCO 3 ) 2 form. C.O. 2 MgCO by contact with air containing 3 Mg(OH) to form 2 The use of may suffer from unfavorable dynamics in some situations. The embodiments shown in Figures 5 and 6 show that MgCO 3 Provide an alternative route to form.
[0053] Figure 5 MgCO 3 shows a process in which Na is formed by direct neutralization of Fe / Al / Mn-depleted solutions; 2 C.O. 3 , e.g. produced in a direct air capture (DAC) process and recovered from MgCl in Fe / Al / Mn-depleted solutions. 2(aq) Reacts with MgCO 3(s) Generate: MgCl 2 +Na 2 C.O. 3 = MgCO 3 +2NaCl
[0054] In selective embodiments, substantially all of the NaOH produced by the chlor-alkali process is CO captured directly from the atmosphere. 2 From Na 2 C.O. 3 into the DAC system to generate. In such a process, MgCO 3 sufficient Na to provide an alkali metal precipitant for all aspects of the process, including 2 C.O. 3 is generated. In this way, the adsorbent regeneration of DAC, i.e. NaOH, CO 2 combined with long-term mineralization of MgCO 3 Mineralization produces carbon negative products in the form of carbonates, which can be used as fillers and construction aggregates.
[0055] Figure 6 shows the Fe / Al / Mn-depleted solution with CO containing NaOH. 2 Add gas directly to MgCl in solution 2(aq) MgCO by reacting with 3(s) forming MgCO 3 shows an alternative process involving the formation of: MgCl 2 + 2NaOH + CO 2(g) = MgCO 3 + 2NaCl + H 2 O
[0056] As shown in Figure 6, some of the NaOH from the chlor-alkali process is CO 2(g) (For example, Na 2 C.O. 3 CO from precipitation of iron and aluminum using 2 MgCO 3 can be formed in situ. Alternatively, CO for Mg carbonate precipitation 2(g) can also be supplied from a source external to the process.
[0057] The reactions at each stage of this process can be expressed as follows: Neutralization Alkali hydroxide: 2HCl+2NaOH = 2NaCl+2H 2 O Alkali metal carbonate: 2HCl + Na 2 C.O. 3 = 2NaCl +H 2 O + CO 2(g) iron precipitation Alkali hydroxide: 2FeCl 3 + 6NaOH = 2FeO(OH) + 2H 2 O+6NaCl 2FeCl 3 + 6NaOH = Fe 2 O 3 (Hematite) + 6NaCl + 3H 2 O Alkali metal carbonate: 2FeCl 3 +3Na 2 C.O. 3 +H 2 O = 2FeO(OH) + 6NaCl + 3CO 2(g) nickel recovery Alkali hydroxide: NiCl 2 + 2NaOH = Ni(OH) 2 +2NaCl Alkali metal carbonate: NiCl 2 +Na 2 C.O. 3 = NiCO 3 +2NaCl Magnesium recovery Alkali hydroxide: MgCl 2+ 2NaOH = Mg(OH) 2 +2NaCl Alkali metal carbonate: MgCl 2 +Na 2 C.O. 3 = MgCO 3 +2NaCl Direct CO 2 :MgCl 2 + 2NaOH + CO 2(g) = MgCO 3 + 2NaCl + H 2 O
[0058] In an alternative embodiment, NaHCO is used in reactions at various stages of the process. 3 is Na 2 C.O. 3 can be substituted for.
[0059] Figures 7 to 10 illustrate the leaching of metal values (``H 2 S.O. 4 leaching"), a process for producing a solid siliceous residue ("amorphous silica residue for cement production") and a loaded leachate. As shown, the residue may be washed.
[0060] Alkaline hydroxide precipitant (Figure 7) or alkali metal carbonate or bicarbonate precipitant (Na 2 C.O. 3 Precipitate iron and / or aluminum from the loaded leachate ("Precipitation of iron and aluminum") using any of the methods in Figures 8-10). The use of alkali metal carbonate or bicarbonate precipitants eliminates carbon dioxide off-gas (“CO 2 an Fe / Al depleted solution, an iron and / or aluminum hydroxide or oxide precipitate product (an "Fe / Al hydroxide precipitate", which can be an oxide such as hematite), . concentrated CO 2 Off-gas can be isolated using a variety of approaches. As illustrated, the residue can be washed to provide a precipitate that can be used in magnetite production.
[0061] Nickel and / or cobalt can be added with an alkali hydroxide precipitant (e.g. NaOH, Figure 7) or an alkali metal carbonate or bicarbonate precipitant (e.g. NaOH). 2 C.O. 3 , Figures 8-10) from Fe / Al-depleted solutions, Ni / Co-depleted solutions and nickel and / or cobalt hydroxides (Figure 1, "MHP") or carbonate precipitates (Figure 1, "MHP"). 8-10, "Ni / Co carbonate (for battery manufacturing)") is produced.
[0062] Iron and / or aluminum and / or manganese can be removed using an alkali hydroxide precipitant (Figure 7) or an alkali metal carbonate or bicarbonate precipitant (Figures 8-10, Na 2 C.O. 3 ) and the exemplified sodium persulfate (Na 2 S 2 O 8 ) can be used to scrub from the Ni / Co-depleted solution and the Fe / Al / Mn-depleted solution and the iron and / or aluminum and / or manganese hydroxide precipitate products ('Fe / Al / Mn hydroxide precipitate) can be produced.
[0063] As shown, the brine containing the Fe / Al / Mn depleted solution can be recycled to the milling process to provide a milled mineral feedstock.
[0064] Magnesium can be extracted with an alkali hydroxide precipitant (NaOH shown in Figures 7 and 8), with an alkali metal carbonate or bicarbonate precipitant (Figure 9), or with a combined feed of an alkali hydroxide precipitant and CO2 (carbon dioxide). In the capture step, Fe / Al / Mn can be precipitated from the Fe / Al / Mn-depleted solution (Figure 10), producing Mg-depleted solution and magnesium hydroxide (Figures 7 and 8) or carbonate (Figures 9 and 10) precipitates. can. The Mg-depleted solution may then be electrolyzed to produce an alkali hydroxide precipitate and an acid leachate (“H 2 S.O. 4 and make NaOH”).
[0065] Carbon dioxide is CO 2 The containing gas is treated with a scrubbing solution containing an alkaline hydroxide precipitant (NaOH as shown) and first, second, third and fourth alkali metal carbonate or bicarbonate precipitants (NaOH as shown). 2 C.O. 3 ) by producing one or more of CO 2 can be scrubbed from the containing gas ("air" as shown) to produce i) iron and aluminum precipitation, ii) Ni / Co precipitation, iii) manganese-free iron and aluminum precipitation, and iv) Mg This is for use in the precipitation of .
[0066] In the method described above, CO 2 The process of scrubbing carbon dioxide from the containing gas removes Na from the scrubbing solution. 2 C.O. 3 A crystallization step may be included to precipitate the hydrate, and the alkaline hydroxide precipitant is NaOH. Then solid Na 2 C.O. 3 The crystalline product may be directed to provide one or more alkali metal carbonate or bicarbonate precipitates.
[0067] The process acid leachate illustrated is H 2 S.O. 4 It is. Thus, a process is provided that uses a sulfate-based system for the treatment of magnesium silicate. In selective embodiments, (Figure 7) H 2 S.O. 4 / NaOH / Na 2 S.O. 4 Salt decomposition is used to produce amorphous silica for cement, iron residue, nickel and cobalt hydroxide mixtures, and magnesium hydroxide, which can be used for carbon sequestration. In alternative embodiments, various direct air carbon capture (DAC) steps are integrated into the sulfate system (Figures 8-10). In particular, Figure 8 shows how CO in air can be extracted using some of the alkaline hydroxide precipitant NaOH. 2 It shows the process of removing . The resulting sodium carbonate is then used in the iron removal and nickel / cobalt precipitation steps. Figure 9 shows the complete use of NaOH in the DAC and the NaOH 2 C.O. 3 It shows the process of generating . Na 2 C.O. 3 By adding MgCO to the Mg precipitation step, MgCO 3 is directly precipitated and carbon sequestration takes place. Figure 10 shows that the alkali hydroxide precipitant NaOH is added directly to the Mg precipitation stage with CO 2 In combination with MgCO 3 3 illustrates an alternative embodiment for forming a .
[0068] The steps of the sulfuric acid process can be characterized by the reactions involved: Acid leaching (simplified); Mg 2 SiO 4 +2H 2 S.O. 4 = 2MgSO 4 +SiO 2 +2H 2 O Ni 2 SiO 4 +2H 2 S.O. 4 = 2NiSO 4 +SiO 2 +2H 2 O Co 2 SiO 4 +2H 2 S.O. 4 = 2CoSO 4 +SiO 2 +2H 2 O Fe 2 SiO 4 +2H 2 S.O. 4 = 2FeSO 4 +SiO 2 +2H 2 O MnO 2 +2FeSO 4 +2H 2 S.O. 4 = MnSO 4 +Fe 2 (S.O. 4 ) 3 +2H 2 O 2FeO(OH) + 3H 2 S.O. 4 =Fe 2 (S.O. 4 ) 3 +4H 2 O 2AlO(OH) + 3H 2 S.O. 4 =Al 2 (S.O. 4 ) 3 +4H 2 O Removal of iron and aluminum (with products); H 2 S.O. 4 + 2NaOH = Na 2 S.O. 4 +2H 2 O Al 2 (S.O. 4 ) 3 + 6NaOH = 2Al(OH) 3 +3Na 2 S.O. 4(aluminum hydroxide) Fe 2 (S.O. 4 ) 3 + 6NaOH = 2Fe(OH) 3 +3Na 2 S.O. 4 (iron hydroxide) Al 2 (S.O. 4 ) 3 + 6NaOH = 2AlO(OH) + 3Na 2 S.O. 4 +2H 2 O (aluminum oxyhydroxide) Fe 2 (S.O. 4 ) 3 + 6NaOH = 2FeO(OH) + 3Na 2 S.O. 4 +2H 2 O (iron oxyhydroxide) Fe 2 (S.O. 4 ) 3 + 6NaOH = Fe 2 O 3 +3Na 2 S.O. 4 +3H 2 O (hematite) 3Al 2 (S.O. 4 ) 3 + 12NaOH = 2NaAl 3 (S.O. 4 ) 2 (OH) 6 +5Na 2 S.O. 4 (Alunite) 3Fe 2 (S.O. 4 ) 3 + 12NaOH = 2NaFe 4 (OH) 6 +5Na 2 S.O. 4 (Jarosite) nickel cobalt precipitation NiSO 4 + 2NaOH = Ni(OH) 2 +Na 2 S.O. 4 CoSO 4 + 2NaOH = Co(OH) 2 +Na 2 S.O. 4 Iron, aluminum and manganese removal stage 2 Al 2 (S.O. 4 ) 3 + 6NaOH = 2Al(OH) 3 +3Na 2 S.O. 4 (aluminum hydroxide) Fe 2 (S.O. 4 ) 3 + 6NaOH = 2Fe(OH) 3 +3Na 2 S.O. 4 (iron hydroxide) Al 2 (S.O. 4 ) 3 + 6NaOH = 2AlO(OH) + 3Na 2 S.O. 4 +2H 2 O (aluminum oxyhydroxide) Fe 2 (S.O. 4 ) 3 + 6NaOH = 2FeO(OH) + 3Na 2 S.O. 4 +2H 2 O (iron oxyhydroxide) 3Al 2 (S.O. 4 ) 3 + 12NaOH = 2NaAl 4 (OH) 6 +5Na2SO 4 (Alunite) 3Fe 2 (S.O. 4 ) 3 + 12NaOH = 2NaFe 4 (OH) 6 +5Na 2 S.O. 4 (Jarosite) MnSO 4 + Na S O 228 + 4NaOH = MnO 2 +3Na 2 S.O. 4 +2H 2 O Precipitation of magnesium hydroxide MgSO 4 + 2NaOH = Mg(OH) 2 +Na 2 S.O. 4 Salt decomposition (anion exchange membrane) 2Na 2 S.O. 4 +4H 2 O = 4NaOH + 2H 2 S.O. 4 +2H 2 + O 2
[0069] In alternative embodiments, the process involves NaOH, NaHCO 2 or Na 2 C.O. 3 Use a precipitant. Below are some alternative chemicals: Neutralization Alkali hydroxide:H 2 S.O. 4 + 2NaOH = Na 2 S.O. 4 +2H 2 O Alkali metal carbonate:H 2 S.O. 4 +Na 2 C.O. 3 = Na 2 S.O. 4 +H 2 O + CO 2 (g) iron precipitation Alkali hydroxide: Fe 2 (S.O. 4 ) 3 + 6NaOH = 2Fe(OH) 3 +3Na 2 S.O. 4 or Fe 2 (S.O. 4 ) 3 + 6NaOH = Fe 2 O 3 +3Na 2 S.O. 4 +3H 2 O Alkali metal carbonate: Fe 2 (S.O. 4 ) 3 +3Na 2 C.O. 3 + H2O = 2FeO(OH) + 3Na 2 S.O. 4 +3CO 2 (g) nickel recovery Alkali hydroxide: NiSO 4 + 2NaOH = Ni(OH) 2 +Na 2 S.O. 4 Alkali metal carbonate: NiSO 4 +Na 2 C.O. 3 = NiCO 3 +Na 2 S.O. 4 Magnesium recovery Alkali hydroxide: MgSO 4 + 2NaOH = Mg(OH) 2 +Na 2 S.O. 4 Alkali metal carbonate (Na 2 C.O. 3 ):MgSO 4 +Na 2 C.O. 3 = MgCO 3 +Na 2 S.O. 4 Alkali metal carbonate with NaOH / CO 2 (g) added: MgSO 4 + 2NaOH + CO 2 = MgCO 3 +Na 2 S.O. 4 +H 2 O
[0070] This process can be integrated with other carbon sequestration processes such as ocean alkalinization. This process for producing synthetic brookite and calcium hydroxide addresses the environmental risks of direct marine alkalinity enrichment using untreated mafic rocks. The process also creates a less carbon-intensive source of magnesium and calcium hydroxide for use as feedstock in carbon capture and storage, including direct air capture technologies. The use of the brookite or calcium hydroxide products of the present process in direct air capture (DAC) processes can be implemented to eliminate the calcination and slack steps otherwise required in these processes. This process consists of nickel and iron hydroxides and amorphous silicates (SiO 2 ), enabling the use of basaltic sand for less carbon-intensive industrial purposes.
[0071] Although various embodiments of the invention are disclosed herein, many adaptations and modifications can be made within the scope of the invention in accordance with the common general knowledge of those skilled in the art. Such modifications include the substitution of known equivalents for any aspect of the invention to achieve the same result in substantially the same way. Terms such as "exemplary" or "illustrative" are used herein to mean "serving as an example, illustration, or illustration." Any implementation described herein as "exemplary" or "exemplary" is not necessarily to be construed as preferred or advantageous over other implementations, and such implementations are not necessarily to be construed as preferred or advantageous over other implementations. are all independent embodiments. Unless otherwise stated, numerical ranges are inclusive of the numbers defining the range, and the numbers are not necessarily approximations of the given decimal numbers. As used herein, the word "comprising" is used as an open-ended term and is substantially equivalent to the expression "including, but not limited to," and the word "comprises" has the corresponding meaning. have As used herein, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "a thing" includes a plurality of such things. Citation of a reference herein is not an admission that such reference is prior art to the present invention. Any priority documents and all publications, including but not limited to patents and patent applications, cited herein, and all documents cited in such documents and publications, are referred to herein if each individual publication is is herein incorporated by reference as if specifically and individually indicated to be incorporated by reference herein and as if fully set forth herein. The invention includes substantially all embodiments and variations as herein described with reference to the examples and drawings.
Claims
1. 1. A method for processing a crushed nickel saprolite mineral feedstock, comprising: a) leaching iron, aluminum, nickel, cobalt, manganese, and magnesium metallic values from a crushed mineral feedstock with an HCl acid leachate to produce a solid siliceous residue and a loaded leachate; b) precipitating iron and aluminum from the loaded leachate, said precipitation comprising: Add a first NaOH alkaline hydroxide precipitant; Producing an Fe / Al depleted solution and a precipitate of iron and / or aluminum hydroxides or oxides; c) precipitating nickel and cobalt from the Fe / Al-depleted solution, said precipitation comprising: A second alkaline hydroxide precipitant, NaOH; to produce a Ni / Co depleted solution and a mixed hydroxide precipitate of nickel and cobalt; d) adding an oxidizing agent to precipitate manganese from the Ni / Co-depleted solution, said precipitation comprising: a third NaOH alkaline hydroxide precipitant; to produce a depleted solution of Fe / Al / Mn and a manganese hydroxide precipitation product; e) precipitating magnesium from the Fe / Al / Mn depleted solution, said precipitation comprising: A fourth alkaline hydroxide precipitant, NaOH; to produce a Mg-depleted solution and a precipitate product of magnesium hydroxide; f) subjecting the Mg-depleted solution to a chloralkali process to produce a NaOH alkaline hydroxide precipitant, a Cl2(g) product and a H2(g) product, and further reacting the Cl2(g) product with the H2(g) product to produce HCl as an HCl acid eluant.
2. The method further comprises reacting the NaOH alkali hydroxide product of the electrolysis process with a CO2-containing gas, thereby producing CO 2 10. The method of claim 1, comprising scrubbing carbon dioxide from a containing gas to produce an alkali metal carbonate or bicarbonate precipitate comprising NaHCO3 or Na2CO3.
3. CO 2 Scrubbing carbon dioxide from the contained gas removes Na from the scrubbing solution in the crystallization process. 2 CO 3 The hydrate is precipitated to give solid Na 2 CO 3 The method of claim 2 comprising producing a crystalline product.
4. The oxidizing agent is chlorine gas (Cl 2(g) 4. The method according to claim 1, further comprising the step of:
5. The method of any one of claims 1 to 4, further comprising magnetically separating material from the comminuted mineral feedstock.
6. 6. The method of any one of claims 1 to 5, further comprising subjecting the loaded leachate to a resin leaching process so as to selectively remove nickel values from the loaded leachate to obtain a refined nickel product.
7. The method of any one of claims 1 to 6, further comprising washing and / or alkalizing the solid siliceous residue.
8. A method according to any one of claims 1 to 7, further comprising washing and / or alkalizing the iron and / or aluminium hydroxide or oxide precipitation product.
9. 9. The method of any one of claims 1 to 8, further comprising adding hematite seed material to the step of precipitating iron and aluminum to seed the precipitation of the hematite product.
10. 10. A method according to any one of the preceding claims, wherein the iron and / or aluminium hydroxide or oxide precipitation product comprises hematite seed material, and the hematite seed material is recycled to the iron and / or aluminium precipitating step so as to seed the precipitation of the hematite product.
11. A method according to any one of claims 1 to 10, further comprising recycling the brine containing the Fe / Al / Mn depleted solution to the grinding process to provide ground mineral feedstock.