Rheologically defined lignin compositions

JP2024099530A5Inactive Publication Date: 2024-10-31SUZANO CANADA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024057179
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-06-26
Filing Date
2024-03-29
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge in producing carbon fibers from isolated lignin lies in the trade-off between the ability to form fibers through spinning and maintaining fiber morphology during high-temperature carbonization, with existing lignins requiring slow heating rates for stabilization, making them economically unviable.

Method used

Development of lignin derivatives with specific viscoelastic metrics, including minimum storage modulus (G' min), onset of softening temperature (T 1), crossover temperature (T 2), and degree of crosslinking (ΔG' 2), allowing for improved processing and performance in industrial applications.

Benefits of technology

The lignin derivatives facilitate efficient processing into molded or extruded thermoplastic forms and fibrous materials like carbon fibers, with enhanced thermal stability and mechanical properties, overcoming the limitations of traditional lignins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000017_0000
    Figure 00000017_0000
  • Figure 00000018_0000
    Figure 00000018_0000
  • Figure 00000018_0001
    Figure 00000018_0001
Patent Text Reader

Abstract

To provide derivatives of native lignin having certain viscoelastic properties, as well as uses, processes, methods and compositions thereof.SOLUTION: Anthropogenic derivatives of native lignin are disclosed, having specific viscoelastic metrics which selectively facilitate the processing of these lignin derivatives into particular finished products. Such lignin derivatives are characterized by rheological metrics that include minimum storage modulus (G'min), onset of softening temperature (T1), and / or cross-over temperature (T2) from predominately viscous to predominately elastic behaviour.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to derivatives of natural lignin derived from lignocellulosic feedstocks and their industrial applications. More specifically, the present invention relates to derivatives of natural lignin having specific viscoelastic properties, and their uses, processes, methods and compositions. [Background technology]

[0002] Lignins are a heterogeneous class of complex cross-linked organic polymers. They form a relatively hydrophobic, aromatic phenylpropanoid complement to cellulose and hemicellulose in the structural components of vascular plants. Lignification is the final stage of plant cell wall development, with lignin acting as the "glue" that holds the cell wall together. Natural lignins as such do not have a universally defined structure. Natural lignins are complex macromolecules composed of 3-primary monolignols (e.g. phenylpropane units; p-coumaryl alcohol, coniferyl alcohol and sinapyl alcohol) connected through several different carbon-carbon and carbon-oxygen bonds. The type of monolignols and the linkages between the units vary depending on a variety of factors, including genetic and environmental factors, species, cell / growth type, and location within / between the cell walls.

[0003] Extracting lignin from lignocellulosic biomass generally results in the degradation / modification of lignin and the generation of numerous lignin fragments of various chemical and polymeric properties. Some processes used to remove lignin from biomass hydrolyze the lignin structures to low molecular weight fragments with a large amount of phenolic hydroxyl groups, thereby increasing their solubility in the treatment liquids (e.g., sulfuric acid lignin). Other processes not only degrade the lignin polymers but also introduce new functional groups into the lignin structures to improve their solubility and facilitate their removal (e.g., sulfite lignin). The lignin fragments generated are generally referred to as lignin derivatives and / or technical lignins. Since it is very difficult to elucidate and characterize such a complex mixture of molecules and polymers, lignin derivatives are usually described in terms of the lignocellulosic plant material used and the method by which they are produced and recovered. Namely, lignin isolated from the kraft pulping of softwood species is called softwood kraft lignin. Similarly, organosolv pulping of annual fibres produces annual fibre organosolv lignin and the like (see, e.g., U.S. Pat. Nos. 4,100,016; 7,465,791; and PCT Publication No. WO2012 / 000093; AL Macfarlane, M. Mai et al., 20 - Bio-based chemicals from biorefining: lignin conversion and utilisation, 2014).

[0004] Despite lignin being one of the most abundant natural polymers on earth (AL Macfarlane, M. Mai et al., 20 - Bio-based chemicals from biorefining: lignin conversion and utilisation, 2014), there has been limited large-scale commercial use of extracted lignin derivatives isolated from conventional pulping processes used to produce paper pulp. This is due to the inherent inconsistencies in their chemical and physical properties as well as the important role that lignin and lignin-containing processing liquors play in the chemical / energy recovery of the process. These inconsistencies can arise due to a number of factors such as variations in biomass supply (region / time / climate) and the specific extraction / generation / recovery conditions employed, which are further complicated by the inherent complexities in the chemical / molecular structure of the biomass itself.

[0005] Despite their complexity, lignins continue to be evaluated for a variety of thermoplastic, thermoset, elastomeric, and carbonaceous materials. For example, softwood kraft lignins have been shown to be effective alternative components in many adhesive systems (phenol-formaldehyde, polyurethane, epoxy resins), rubber materials, polyolefins, and carbon fibers (TQ Hu, Chemical Modification, Properties, and Usage of Lignin, 2002) (AL Macfarlane, M. Mai et al., 20 - Bio-based chemicals from biorefining: lignin conversion and utilisation, 2014).

[0006] Heat treatment is a common step in the preparation of a variety of different types of polymeric materials, including lignin-based materials. For example, the advantage of heat-softening plastics, or thermoplastics, as a general class of materials is that they can be heated to form a viscous, fluid-like state that can be repeatedly formed, molded, or extruded into a variety of shapes that are retained after the material has cooled. Examples of thermoplastics include polyesters, polycarbonates, polylactates, polyvinyls, polystyrenes, polyamides, polyacetates, polyacrylates, and classes of polyolefins such as polyethylene and polypropylene. Similarly, thermosetting plastic applications, particularly thermoset resin systems, utilize heat treatment to irreversibly harden an initially solid or viscous liquid polymer into an infusible, insoluble polymer network. Thermoset resins are typically malleable or liquid before hardening, and are often designed to be molded into a final shape, used as adhesives, or formed into fibrous materials such as carbon fiber. Examples of thermosetting resins include the classes of acrylic, polyester, unsaturated vinyl ester, epoxy, polyurethane, phenolic, amino, and furan resins.

[0007] When designing / developing new multiphase materials or considering replacing one constituent material with another, there are several key requirements: control of interfacial chemistry, microstructure, and reactivity (DR Paul and CB Bucknall, Polymer Blends: Formulation, 2000). In melt / heat processed systems, viscoelastic behavior can dictate the morphology, processability, and therefore performance of the multicomponent system. As with synthetic polymer systems, the thermal properties of lignin have a strong influence on the resulting performance of lignin-based materials. These thermal properties can vary significantly between different lignin types and may be characterized by a variety of techniques that quantify different physical phenomena. Typically, the glass transition temperature (T g ), softening temperature (Ts), and decomposition temperature (T d) measurements have been used to describe and predict the processability and performance of lignin-based materials.

[0008] Glass transition temperature (T g ) is the most frequently cited parameter that defines the temperature at which an amorphous polymer, such as lignin, changes from a hard, glassy solid to a soft, rubbery material. <T g At T>T, the movement of the lignin molecules is hindered by the rigidity of the polymer backbone and the intermolecular interactions between adjacent polymer chains, so that the individual lignin molecules remain fixed relative to each other. g In this case, the thermal energy present in the system is sufficient to increase the flexibility of the polymer and break down the network of hydrogen bonds and other interactions that hold the lignin molecules in place. This is called T g This means that at temperatures above T g The value of T is usually measured by differential scanning calorimetry (DSC), which measures the amount of heat energy required to raise the temperature of a sample contained in a crucible compared to an identical empty crucible. g is most commonly assigned to the midpoint of the step change in the sigmoidal shape of the differential heat flow signal. For isolated lignin, a wide range of T g The T values ​​reported are usually in the range of 80-200 °C. g The value of is known to vary greatly based on the particular biomass type, the delignification process used for separation, the moisture content, and the thermal history of the sample.

[0009] Due to their high carbon content, isolated lignins are candidate precursors for carbon materials such as activated carbon (AC) and carbon fibers (CF). The production of carbon materials requires heat treatment of the precursors at high temperatures (often above 1000 °C) under inert conditions to remove non-carbon elements from their chemical structure. This heat treatment is typically a series of steps designed to optimize processing costs and end product performance. The details of a particular heat treatment process are optimized for a particular type of carbon precursor. The large variability in thermal properties between isolated lignins makes it very difficult both to identify the type of lignin that is ideal for the production of carbon materials with specific properties and to optimize the heat treatment steps that will lead to the best possible carbon product at the lowest possible cost. The important thermal properties of lignin, mainly the T g Various thermal analysis techniques are used to define the thermal melting temperature, softening temperature Ts, and decomposition temperature Td. Accurate characterization of lignin's thermal properties allows for the conversion of lignin into high performance products, improving process efficiency and end product performance.

[0010] The challenge in producing CF from isolated lignin is that there is a trade-off between the ability to form fibers through the spinning process and the ability to maintain its fiber morphology during high-temperature carbonization (i.e., the fiber must not melt but must maintain its fiber shape and good mechanical properties). After fiber spinning and prior to carbonization, a stabilization step may be required to convert the fiber precursor to an infusible state that can maintain a solid form during carbonization. This is most commonly achieved by heating the fibers in air to induce chemical crosslinking, similar to a resin curing (thermosetting) process. Unfortunately, most commercial / semi-commercial industrially produced lignins with good melt spinning performance, e.g., Alcell lignin, cannot be economically converted to CF because they require very slow heating rates (and therefore long processing times) for successful stabilization.

[0011] In the field of lignin-based CF processing, gThe value of T has been used as a benchmark to predict whether a given lignin can be processed to produce fibers with desirable properties (DA Baker and TG Rials, Recent advances in low-cost carbon fiber manufacture from lignin, 2013). For example, T g It has been reported that isolated lignin at <130 °C can be melt spun to form filaments, but the time required for stabilization was on the order of several days, which was too long to be economical. Heat treatment of lignin prior to melt spinning has been shown to be effective in reducing the T g It is used to increase the T and modify the melt flow properties of the isolated lignin, with the added benefit of increasing the yield after carbonization (based on the weight of the stabilized precursor fiber). g Heat-treated lignin with 1,2-dichlorophenyl ether (DA Baker and TG Rials, Recent advances in low-cost carbon fiber manufacture from lignin, 2013) was shown to maintain spinnability and required a shorter stabilization time, but unfortunately, the T g Further increase in T decreased the melt processability of lignin and produced poor quality fibers with reduced strength. gWhen T was increased above about 160 °C, the lignin was not melt-spinnable, presumably due to the lack of thermal softening. This can be seen from published studies (DA Baker, FS Baker et al., Thermal Engineering of Lignin for Low-cost Production of Carbon Fiber, 2009; DA Baker and TG Rials, Recent advances in low-cost carbon fiber manufacture from lignin, 2013; I. Norberg, Y. Nordstrom et al., A new method for stabilizing softwood kraft lignin fibers for carbon fiber production, 2013; H. Mainka, O. Tager et al., Lignin - an alternative precursor for sustainable and cost-effective automotive carbon fiber, 2015), which show that if lignin has thermal softening properties, it is usually not reactive enough to form the necessary chemical crosslinks in an economical time frame. Researchers in this field include T g The value of T was used to determine where a particular lignin falls on the spectrum of softening and crosslinking. g is often considered to be a good indicator of the softening and crosslinking behavior expected for a particular type of isolated lignin.

[0012] Other researchers have studied the thermal properties of lignin using more advanced analytical techniques that capture more information about the thermal softening and reactivity of lignin. gA drawback of using rheological measurements is that they convey only limited information about the mechanical properties of lignin while it is subjected to heating. Rheological measurements can fill this information gap by allowing the stiffness of lignin to be measured as a function of temperature and deformation. For example, steady shear rheometry using parallel plates has been used to show that solvent-extracted kraft lignin has a much lower thermal reactivity than "crude", as-isolated kraft lignin. This assessment was based on measurements performed isothermally at selected temperatures under continuous shear deformation, showing that the apparent melt viscosity of "crude" kraft lignin increased as a function of time, while the solvent-extracted lignin maintained a constant apparent shear viscosity with time. Similar to the observations with Arcel lignin, this solvent-extracted kraft lignin was shown to have excellent melt spinnability, but due to its low thermal reactivity, stabilization requires very slow heating rates to avoid melting (DA Baker, NC Gallego et al., On the characterization and spinning of an organic-purified lignin toward the manufacture of low-cost carbon fiber, 2012).

[0013] Another variant of rheometry uses dynamic oscillations with small strain amplitudes to measure viscoelastic properties as a function of temperature and deformation. The advantage of dynamic oscillations is that the viscoelastic response of the material can be expressed in a resolved form. This provides information on the relative magnitudes of the elastic and viscous contributions to the overall stress response to deformation. For example, small amplitude oscillatory shear (SAOS) rheometry has been used to study the changes in viscoelastic properties during pyrolysis of biomass and its components, including lignin, and has also been used to study the carbonization of coal. This type of data has been used to identify the onset and extent of softening, the onset and extent of solidification, and the associated temperature ranges at heating rates ranging from 1 to 5 °C / min. Interestingly, the SAOS rheometry technique can distinguish between softening and non-softening lignin, but more powerfully, the technique can measure the magnitude of softening or crosslinking as a function of temperature and heating rate. This is in contrast to the T measured by differential scanning calorimetry. g The SAOS technique is also notable for clearly defining the temperature ranges associated with softening and crosslinking, which is not possible with the measurement of crosslinking alone. Summary of the Invention

[0014] Artificial derivatives of natural lignin are provided that have specific viscoelastic metrics that selectively facilitate the processing of these lignin derivatives into specific end products. Such lignin derivatives have, for example, a minimum storage modulus (G' min ), the onset of softening temperature (T1), and / or the crossover temperature from primarily viscous to primarily elastic behavior (T2).

[0015] Selected embodiments include lignin derivatives prepared for use in thermal treatment, e.g., having a G' of 10,000 Pa or less. min , T1 above 125°C, T2 above 175°C, and the degree of crosslinking (ΔG'2 = G' 250 / G' min ), and G' min Measured at 250°C (G' 250) is less than about 4 or greater than 7. This type of embodiment may be particularly suitable for use in methods of forming molded or extruded thermoplastic shapes, for example.

[0016] Alternative embodiments include lignin derivatives prepared for use in forming fibers, films, sheets, coatings, particles, or nanoparticles, e.g., having a G' of 100,000 Pa or greater. min , T1 equal to or greater than 170° C., and T2 equal to or greater than 250° C. This type of embodiment may be particularly suitable for use in a method for producing a fibrous material, such as carbon fibre, for example.

[0017] Further embodiments include lignin derivatives prepared for use in forming fibers, films, sheets, coatings, particles, and nanoparticles, the lignin derivatives having a minimum storage modulus (G') of 100,000 Pa or greater. min ), and a tan(δ) of less than 1.

[0018] Also described herein is a method of forming a shaped molded or extruded thermoplastic form comprising heating a lignin derivative as described herein above T1 to form a heated thermoplastic material that is primarily in a viscous state and has a storage modulus of 10,000 Pa or less; forming the heated thermoplastic material into the shape of the thermoplastic form; and cooling the heated thermoplastic material below T1 to provide the thermoplastic form.

[0019] Also described herein is a method of thermoforming a composite material comprising bonding a plurality of parts comprised of solid materials into a solid composite form, the parts being joined by heating and compression in a mixture with an adhesive comprising a lignin derivative as described herein, where the heating and compression raises the temperature of the mixture above T1.

[0020] Provided herein is a method of forming a shaped molded or extruded thermoset form comprising heating a lignin derivative as described herein above T1 to form a heated material, where the heated material is in a predominantly viscous state and has a storage modulus of 10,000 Pa or less; forming the heated material into a shape of the thermoset form to form a molded thermoset form; heating the molded thermoset form above T2; holding the molded thermoset form at T2 for greater than 1 minute; and cooling the molded thermoset form below T1 to provide a molded or extruded thermoset form.

[0021] Also described herein is a method of solution forming a composite material comprising a plurality of portions comprised of solid materials into a solid composite form, wherein the portions are consolidated by heating and / or pressing as a mixture comprising a lignin derivative as described, and the heating and / or pressing brings the mixture to a temperature above T2, or G'. min The temperature is raised above the temperature at

[0022] Also described herein is a method of forming a composite material comprising a plurality of portions of solid materials into a mixture comprising a lignin derivative as described herein, by compacting the mixture, where the mixture is heated and / or compacted to a temperature above T1.

[0023] Also described herein is a method of forming a fibrous material comprising the steps of dissolving a lignin derivative described herein in a fiber spinning solvent to produce dissolved lignin; and spinning the dissolved lignin into fibers.

[0024] The lignin is separated from the cellulosic material and the lignin is tested to determine G' min Also described herein are methods of producing the lignin derivatives described herein, comprising measuring one or more rheological properties, including T1, T2, T3, T4, T5, T6, T7, T8, T9, T10, T11, T12, T13, T14, T15, T16, T17, T18, T19, T20, T21, T22, T23, T24, T25, T26, T27,

[0025] Also described herein is a method of solution forming a material that includes dissolving a lignin derivative as described herein in a solvent to produce dissolved lignin; and casting the dissolved lignin into a shape or form of a material. In various embodiments, the shape or form can be a fiber, film, sheet, coating, particle, nanoparticle, etc. [Brief description of the drawings]

[0026] [Figure 1] Temperature ramp of a derivative of native lignin showing the change in the viscoelastic moduli, G' and G", and their ratio (G" / G'=tan(δ)) as a function of temperature while applying a small amplitude sinusoidal strain to the sample. Points shown in the corresponding black box. <t1> 、 <t2>,<G’min> , and a close-up of <ΔG'2> is also included.

[0027] [Diagram 2] Weight loss as a function of temperature for derivatives of native lignin.

[0028] [Diagram 3] Storage modulus versus temperature for derivatives of natural lignin showing the influence of certain rheological metrics on their processability into carbon fiber.

[0029] [Figure 4] Effect of blending different lignins on the resulting blend viscoelastic metrics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Detailed Description of the Invention The present invention provides derivatives of natural lignin that have specific viscoelastic metrics: onset of softening (T1), minimum storage modulus (G' min Lignin derivatives with specific combinations of viscosity, crossover temperature (T2) from primarily viscous to primarily elastic behavior, and degree of crosslinking (ΔG'2) have been found to process more effectively in industrially relevant applications. Thus, selecting derivatives of native lignin with specific viscoelastic metrics results in products with higher and more predictable processing and material performance.

[0031] Minimum storage modulus (G') of 10,000 Pa or less min It has been found that derivatives of natural lignins having a softening temperature onset (T1) of 125°C or higher and a crossover temperature (T2) from primarily viscous to primarily elastic behavior of 175°C or higher are good heat-softening materials. min is about 8,000 Pa or less, about 5,000 Pa or less, or about 1,000 Pa or less, or about 100 Pa or less; T1 is about 130° C. or more, about 150° C. or more, or about 170° C. or more; and T2 is about 180° C. or more, about 200° C. or more, or about 220° C. or more.

[0032] Furthermore, the derivatives of natural lignin also have a high degree of cross-linking (ΔG′2=G′ 250 / G' min ), i.e., G' min Measured at 250°C (G' 250 ) is greater than 600% (ΔG'2>7), resulting in a plastic material (e.g., melt / melt fiber spinning, thermosets, etc.) with a good combination of heat softening and heat setting properties. For example, ΔG'2 is about 7 or greater, about 8 or greater, about 9 or greater, about 10 or greater, or about 100 or greater. In other embodiments, ΔG'2 of about 4 or less, about 3 or less, about 2 or less, or about 1 or less also results in a plastic material with a good combination of heat softening and heat setting properties.

[0033] Similarly, a minimum storage modulus (G') of 100,000 Pa or greater is required, along with an onset of softening temperature (T1) of 170°C or greater and a crossover temperature (T2) from primarily viscous to primarily elastic of 250°C or greater. min Derivatives of natural lignin with G' yield good fiber-forming materials (e.g., carbon fibers) via solution spinning (e.g., wet, dry, gel, electrospinning, etc.). min is about 200,000 Pa or more, about 500,000 Pa or more, or about 1,000,000 Pa or more; T1 is about 175° C. or more, about 200° C. or more, about 225° C. or more, or about 245° C. or more; and T2 is about 260° C. or more, about 280° C. or more, or about 300° C. or more.

[0034] The present invention provides derivatives of native lignin recovered during or after pulping of a lignocellulosic feedstock. The pulp and / or lignin and / or derivatives thereof may be from any suitable lignocellulosic feedstock, including hardwood, softwood, annual fiber, and combinations thereof.

[0035] For example, derivatives of natural lignin from hardwood, softwood, or annual fiber sources, G' min It has been found that those with a T1 of 10,000 Pa or less, a T1 of 125° C. or more, and a ΔG'2 of 7 or more have excellent fiber melting / melt spinning and heat treatment (such as stabilization rate) for carbon materials. For example, G' min is about 5,000 Pa or less, 1,000 Pa or less, about 100 Pa or less, T1 is about 130° C. or more, about 150° C. or more, about 170° C. or more, and ΔG′2 is about 7 or more, about 8 or more, about 10 or more, or about 100 or more. In other embodiments, ΔG′2 of about 4 or less, about 3 or less, about 2 or less, or about 1 or less also results in lignin derivatization with good fiber melt / melt spinning and thermal processing into carbon materials.

[0036] Derivatives of natural lignin, such as from hardwood, softwood, or annual fiber sources, with a G' of 200,000 Pa or greater min It has been found that those having a T1 of 170° C. or more and a T2 of 250° C. or more can be easily spun into a fiber solution and heat-treated on a carbon material. For example, G' min is about 250,000 Pa or more, 500,000 Pa or more, or about 1,000,000 Pa or more; T1 is about 175°C or more, about 180°C or more, or about 200°C or more; T2 is about 260°C or more, about 280°C or more, or about 300°C or more.

[0037] In the present invention, the terms "onset of softening", "minimum storage modulus", "crossover temperature [from predominantly viscous to predominantly elastic behavior]" and "degree of crosslinking" refer to the viscoelastic behavior or "metrics" of the lignin derivatives. These viscoelastic metrics can be measured by small amplitude oscillatory shear (SAOS) rheometry (also called dynamic mechanical thermal analysis or DTMA), for example, using a TA Instruments DHR rheometer. A variety of sample forms can be utilized, including powders, pressed discs, sheets, fibers, and other woven / nonwoven fabrics, and analyzed under oxidizing and / or inert atmospheres. In a typical experiment, the lignin derivative is placed between two parallel circular plates, a sinusoidally varying strain, γ(t)=γ0sin(ωt), is applied, and the sample is heated over a specific temperature range while the mechanical response is measured.

[0038] In selected embodiments, signal quality and consistency of measurements may be better at low temperatures (before possible thermal softening) when compressed samples are used. Compressed samples are typically less susceptible to frictional dissipative losses, but are known to have dissipative losses as well, so coefficients reported therefrom are reported as nominal values.

[0039] In some embodiments, consistent low temperature modulus measurements may help facilitate proper execution of a temperature ramp program with the rheometer, where the sample is typically held under a small positive axial compression force to prevent slippage at low temperatures. The program can also be designed to reduce the axial compression at a set modulus value before significant thermal softening occurs, preventing a more fluid-like sample from being squeezed out between the plates.

[0040] The elastic modulus corresponding to the stress component in phase with the strain wave is commonly called the storage modulus, equal to τ0' / γ0, and usually denoted as G'. The elastic modulus corresponding to the stress component that is 90° out of phase with the strain wave (in phase with the strain wave velocity) is commonly called the loss modulus, equal to τ0" / γ0, and usually denoted as G". In this example, the frequency is kept constant at 1 Hz (6.2 rad / s) and γ0 is kept within limits to ensure that the measurements are made within the linear viscoelastic region of the material. As shown here (Figure 1), the small strain viscoelastic moduli G' and G" provide valuable information on the viscoelastic behavior of lignin as a function of temperature and time. Additionally, in some embodiments, it is useful to define the ratio G" / G' = tan(δ) to describe the relative magnitudes of the viscous and elastic contributions to the measured shear stress. While a sinusoidal strain is applied to the lignin sample, it can be heated at a controlled rate up to 5 °C / min (a practical upper limit to avoid lag between the sample's actual temperature and the set temperature), and values ​​of G' and G" can be measured as a function of temperature at various heating rates. Current viscoelastic metrics relate to samples heated at a rate of 3 °C / min, but slower or faster heating rates can be used to reveal the relative thermoplastic and reactive, i.e., softening and crosslinking behavior, of lignin and its derivatives.

[0041] Artificial derivatives of native lignin can be obtained, for example, by (1) solvent extraction of finely ground wood (ground wood lignin, MWL) or (2) acidic dioxane extraction of wood (acidolysis). Derivatives of native lignin can also be isolated from pretreated biomass using (3) steam explosion, (4) dilute acid hydrolysis, (5) ammonia fiber swelling, and (6) autohydrolysis methods. Derivatives of native lignin can be recovered after pulping of lignocellulose, including industrially engineered (3) Kraft and (4) soda pulping (and their modifications) and (5) sulfite pulping. In addition, many different pulping methods have been developed but not commercially adopted, including: (1) ethanol / solvent pulping (aka the Alcell® process); (2) alkaline sulfite anthraquinone methanol pulping (aka the "ASAM" process); (3) methanol pulping followed by methanol, NaOH, and anthraquinone pulping (aka the "Organocel" process); (4) acetic acid / hydrochloric or formic acid pulping (aka the "Acetosorb" process); and (5) high boiling solvent pulping (aka "HBS" pulping).

[0042] Before or after extraction, isolation and / or pulping, the artificial derivatives of native lignin can be separated into separate fractions by one or more purification techniques. These purification techniques include, for example, filtration (e.g., nano-, micro-, or ultrafiltration), extraction (e.g., liquid-liquid or liquid-solid extraction), heat treatment (e.g., at atmospheric or reduced pressure), and the like. In various embodiments, before or after extraction, isolation and / or pulping, the artificial derivatives of native lignin are separated into separate fractions by extraction and / or heat treatment. In other embodiments, the artificial derivatives of native lignin are not separated into separate fractions by purification techniques before or after extraction, isolation, or pulping.

[0043] The derivatives of natural lignin herein can be utilized alone or can be incorporated into a polymer composition. The compositions disclosed herein can include a derivative of natural lignin according to the present invention and a polymer-forming component. As used herein, the term "polymer-forming component" refers to a component that can be polymerized into a polymer as well as an already formed polymer. For example, in certain embodiments, a polymer-forming component can include monomeric units that can be polymerized. In certain embodiments, a polymer component can include oligomeric units that can be polymerized. In certain embodiments, a polymer component can include a polymer that is already substantially polymerized.

[0044] Polymer-forming components for use herein may result in thermoplastic or thermosetting polymers and copolymers such as epoxy resins, urea-formaldehyde resins, phenol-formaldehyde resins, polyimides, polyacrylates, polynitriles, isocyanate resins, etc. For example, polyolefins such as polyethylene and polypropylene, and polynitriles such as polyacrylonitrile copolymers.

[0045] Typically, the derivatives of native lignin will comprise about 0.1% or more, about 0.5% or more, about 1% or more by weight of the composition.Typically, the lignin derivatives will comprise about 99.9% or less, about 80% or less, about 60% or less, about 40% or less, about 20% or less, about 10% or less by weight of the composition.

[0046] The compositions include derivatives of natural lignin and polymer forming components, but may also include a variety of other optional ingredients, such as adhesion promoters; biocides (antimicrobials, bactericides, fungicides), antifog agents; antistatic agents; adhesives, blowing agents, foaming agents; dispersants; fillers and extenders; fire and flame retardants and smoke suppressants; impact modifiers; initiators; lubricants; mica; pigments, colorants, dyes; plasticizers; processing aids; mold release agents; silanes, titanates and zirconates; slip and antiblocking agents; stabilizers; stearates; ultraviolet light absorbers; blowing agents; defoamers; curing agents; odorants; deodorizers; stain repellents; viscosity modifiers; waxes; and combinations thereof.

[0047] The present invention provides the use of the derivatives of natural lignin as functional components in thermoplastics, thermosets, and fiber-forming polymers, alone or in combination with conventional or evolving polymers. For example, the application can be to improve the thermal stability and mechanical performance of thermoplastic polymers such as polyethylene, polypropylene, polyamide, polynitrile, styrene-butadiene, and combinations thereof. Other examples include increasing the cure of butyl rubber, improving the wear index of synthetic rubbers (polybutadiene, nitrile, neoprene, styrene-butadiene) and natural rubber; improving the yield and heat processing of polyacrylonitrile copolymers to carbon fiber; improving the mechanical properties, adhesion, and reducing emissions (formaldehyde, etc.) of adhesive sealants, epoxy resins, and phenol-formaldehyde resins. EXAMPLES

[0048] Example 1: Temperature ramp curve for a lignin sample (Typical curves for lignin samples heated at 3 °C / min under nitrogen gas flow in the absence of oxygen are shown in Figure 1. The general shape of the curves in Figure 1 indicates that a significant degree of softening occurs at approximately 125-225 °C. At low temperatures, the storage modulus (G') is about an order of magnitude larger than the loss modulus (G"), indicating that the lignin pellets exhibit predominantly elastic or solid-like mechanical behavior (the analysis temperature is T g , as expected). Just prior to softening, both moduli increase to a peak value. This can be attributed to the compression / densification of the sample as it is heated above its glass transition temperature, increasing its overall resistance to deformation. After reaching their peak values, both G' and G" decrease by approximately four orders of magnitude as the temperature is increased from 125 to 225 °C. This decrease in modulus corresponds to thermal softening.

[0049] One aspect of this example involves the definition and determination of select points along a temperature ramp curve in the rheological characterization of lignin. In one aspect of the invention, there are three alternative points of rheological properties that can be used to classify lignin, which are indicated by the black boxes in FIG. 1 and further illustrated in the associated enlarged image.

[0050] point <t1>represents the temperature (T = T1) at the first point of crossover where G’ = G”, and beyond which G’ < G”. In this example, the apparent viscoelastic coefficients G’ and G” are about 10 6 Pa. Beyond this point, the material still shows a large resistance to deformation, but as the temperature rises and the viscous contribution to the shear stress becomes greater than the elastic contribution, this resistance rapidly decreases. The temperature value at point T1 is called the softening onset temperature. Similarly, the second crossover is represented by T2, which represents the temperature at which G’ = G” again, and beyond which G” < G’ once more. This point indicates the transition from mainly viscous liquid behavior back to mainly elastic behavior, and is represented by the crossover temperature T2. Beyond this point, as the temperature further increases, both coefficients continue to decrease until they reach a minimum value at point G’ min . At this point, the lignin sample reaches its softest state, defining the minimum storage modulus G’ min . It should be noted that not all lignin samples show a minimum value of the storage modulus lower than the onset of thermal decomposition. Therefore, in these cases, the degree of softening is determined based on the change in the storage modulus between the onset of softening at T1 and the modulus at the thermal decomposition onset temperature. This is about 250 °C for most lignins. For this typical kraft lignin, a graph of the weight loss % as a function of temperature at a heating rate of 10 °C / min is shown in Figure 2.

[0051] For the lignin sample shown in Figure 1, it is seen that G’ begins to increase between G’ min and 250 °C, indicating the onset of thermally induced crosslinking; another phenomenon of interest in the production of lignin-based materials by heat treatment routes. Since 250 °C is a common temperature for the oxidative thermal stabilization of lignin fibers in preparation for the production of carbon fibers, this temperature is also a convenient endpoint for the evaluation of thermal softening and low-temperature crosslinking, and can be considered a practical upper limit for the processing of some commercially available thermoplastics. Therefore, the degree of crosslinking (ΔG’2) is defined as the change in the modulus between G’ min and 250 °C (ΔG’2 = G’ 250 / G’ min ).

[0052] Example 2: Rheological comparison of different lignins and corresponding thermal processability Figure 3 shows the rheological fingerprints of the three lignins measured in air using 25 mm lignin pellets. Lignin 1 (lower curve) has a G' min Lignin 2 (upper curve) exhibits a high degree of thermal softening (G' min >10,000 Pa) and moderate cross-linking (ΔG'2 = 6.3). Lignin 3 (middle curve) shows moderate thermal softening (G' min >1,000 Pa) and a high degree of cross-linking (ΔG'2=19.4). Lignins 1 and 3 are readily thermally processed, e.g., thermoformed or melt spun into a variety of forms, including fibers, whereas lignin 2 does not soften sufficiently to be hot spun into fiber form. Similarly, lignin 1 cannot be converted to carbon fibers at commercially relevant processing rates, requiring very slow heat stabilization rates of less than 1 °C / min. On the other hand, lignin 3 can be readily spun into fibers and is heat stabilized at heating rates well above 5-10 °C / min.

[0053] Table 1 shows the effect of lignin viscoelastic metrics on solution formation and subsequent heat treatment. Lignin 4 has a G' min It exhibits low thermal softening at <100,000 Pa and is a moderately viscous material with tan(δ)>1. Lignin 5 has a G' min It shows little softening at pressures >100,000 Pa and tan(δ)<1 indicating predominantly elastic behavior. Lignin 4 requires significantly lower heat treatment rates than lignin 5, which can be heat treated at heating rates in excess of 20°C / min. [Table 1]

[0054] Example 3: Effect of lignin mixing to manipulate viscoelastic metrics. Figure 4 shows the effect of blending Lignins 1 and 2 from Example 3 on the resulting blend viscoelastic metrics measured in air using 25mm lignin pellets. It can be seen that increasing the amount of Lignin 1 and diluting Lignin 2 has the effect of decreasing all of the viscoelastic metrics. The softening temperature (T1) decreases with a corresponding decrease in the degree of crosslinking, ΔG'2.

[0055] Example 4: Effect of lignin viscoelastic metrics on the shear strength of phenol-formaldehyde resins. Table 2 shows the effect of lignin viscoelastic metrics on the performance of the resulting thermoset resin in a typical engineered wood product application. Lignin 1 and Lignin 3 from Example 2 were used to replace 25% of a standard phenol-formaldehyde (PF) resin and the effect on shear strength was determined using an Automated Bond Evaluation System (ABES). Approximately 1.8 g of resin was applied to a conditioned (25°C / 50% RH) set hardwood veneer and adhesive strength was measured after curing at 190°C for 15 seconds. It can be seen that Lignin 3, which has a higher crosslinking potential (larger ΔG'2), exhibited better bond strength than Lignin 1. [Table 2]

[0056] References Baker, DA and TG Rials (2013). "Recent advances in low-cost carbon fiber manufacture from lignin." Journal of Applied Polymer Science 130(2): 713-728.

[0057] Baker, DA, FS Baker and NC Gallego (2009). Thermal Engineering of Lignin for Low-cost Production of Carbon Fiber. The Fiber Society 2009 Fall Conference. Athens Georgia.

[0058] Baker, DA, NC Gallego and FS Baker (2012). "On the characterization and spinning of an organic-purified lignin toward the manufacture of low-cost carbon fiber." Journal of Applied Polymer Science 124(1): 227-234.

[0059] Hu, TQ (2002). Chemical Modification, Properties, and Usage of Lignin. Springer US.

[0060] Macfarlane, AL, M. Mai and JF Kadla (2014). 20 - Bio-based chemicals from biorefining: lignin conversion and utilisation. Advances in Biorefineries. K. Waldron, Woodhead Publishing: 659-692.

[0061] Mainka, H., O. Tager, E. Korner, L. Hilfert, S. Busse, FT Edelmann and AS Herrmann (2015). "Lignin - an alternative precursor for sustainable and cost-effective automotive carbon fiber." Journal of Materials Research and Technology 4(3): 283-296.

[0062] Norberg, I., Y. Nordstrom, R. Drougge, G. Gellerstedt and E. Sjoholm (2013). "A new method for stabilizing softwood kraft lignin fibers for carbon fiber production." Journal of Applied Polymer Science 128(6): 3824-3830.

[0063] Paul, DR and CB Bucknall (2000). Polymer Blends: Formulation, Wiley. < / t1>

Claims

1. An artificial lignin derivative prepared for use in forming fibers, films, sheets, coatings, particles, and nanoparticles, said lignin derivative having a minimum storage modulus (G') of 100,000 Pa or greater. min ), an artificial lignin derivative characterized by having a tan(δ) of less than 1.

2. The artificial lignin derivative according to claim 1, characterized in that it has a G' min of 200,000 Pa or more.

3. 3. The artificial lignin derivative of claim 1 or 2, wherein the lignin is derived in whole or in part from coniferous biomass.

4. An artificial lignin derivative as described in claim 1 or 2, wherein the lignin is derived from coniferous biomass.

5. 5. The artificial lignin derivative of claim 1 , wherein the lignin derivative is produced by a process comprising pulping of lignocellulose by kraft pulping.

6. Dissolving the lignin derivative of any one of claims 1 to 5 in a fiber spinning solvent to produce dissolved lignin; and Spinning the dissolved lignin into fibers 2. A method for producing a fibrous material comprising:

7. The method of claim 6, wherein the fiber spinning solvent comprises one or more co-solvents, fiber-forming polymers, fiber-forming additives, fiber-forming fillers, fiber-forming catalysts or thermal stability modifiers.

8. The method of claim 6 or 7, wherein the fiber spinning process is electrospinning, wet spinning, dry spinning, dry jet wet spinning, solution blowing, or centrifugal spinning.

9. The step of spinning the dissolved lignin into fibers comprises: Thermally stabilizing the fibrous morphology in an oxidizing atmosphere while heating to 250° C. at a heating rate of greater than 3° C. / min to provide fibers; and Carbonizing the fibers at a temperature greater than 450° C. to provide a fibrous carbon material. The method of any one of claims 6 to 8, comprising producing a fibrous carbon material comprising:

10. Dissolving the lignin derivative according to any one of claims 1 to 5 in a solvent to produce dissolved lignin; and Casting the molten lignin into the shape or form of a material. A method of solution forming a material comprising:

11. The method of claim 10, wherein the solvent comprises one or more co-solvents, fiber-forming polymers, fiber-forming additives, fiber-forming fillers, fiber-forming catalysts or thermal stability modifiers.