Hard-coat composition, laminate film, and curable film
Patent Information
- Application Number
- JP2024090624
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-08-08
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2039-08-05
Smart Images

Figure 2024113051000001 
Figure 2024113051000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hard coat composition, in particular to a curable hard coat composition, and to a laminate film and the like that includes the hard coat composition. [Background technology]
[0002] Conventionally, resin film laminates having a hard coat layer have been used in various fields (see Patent Document 1). For example, such resin film laminates are used as front and back panels of mobile devices, automobile interior components, etc. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2017-508828 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0004] A hard coat layer that protects the surface of a resin film laminate requires a certain degree of hardness and high scratch resistance. On the other hand, in order to manufacture a resin film laminate having a desired shape, the resin films that constitute each layer require excellent moldability. It has been difficult to satisfy all of these different performances in a resin composition used to manufacture a laminate, particularly a hard coat layer.
[0005] Therefore, an object of the present invention is to provide a hard coat composition which, when cured, can produce a hard coat layer having excellent scratch resistance and high hardness and also has excellent formability during processing, and a laminate film and the like having such a hard coat composition. [Means for solving the problem]
[0006] The present inventors have discovered that a curable hard coat composition containing a specific polymer and nanoparticles has excellent characteristics that can solve the above-mentioned problems, and have completed the present invention.
[0007] That is, the present invention is as follows. (1) A curable hard coat composition comprising: (meth)acryloyl polymer and inorganic oxide nanoparticles, the (meth)acryloyl polymer has a (meth)acrylic equivalent of 200 to 500 g / eq and a weight average molecular weight of 5,000 to 200,000; The hard coat composition, wherein the inorganic oxide nanoparticles have an average particle size of 6 to less than 95 nm. (2) The hard coat composition according to the above (1), wherein the (meth)acryloyl polymer contains a repeating unit represented by the following formula (I): [ka] (In the above formula (I), m is an alkylene group having 1 to 4 carbon atoms or a single bond; n is an alkyl group having 1 to 4 carbon atoms or hydrogen; p is a single bond or an alkylene group having 1 or 2 carbon atoms; q is an alkyl group having a total of 1 to 12 carbon atoms which may contain at least one of the following substituents: an epoxy group, a hydroxyl group, an acryloyl group, and a methacryloyl group, or a hydrogen atom. (3) In the formula (I), m is an alkylene group having 1 or 2 carbon atoms; n is an alkyl group having 1 or 2 carbon atoms; p is a single bond or a methylene group; The hard coat composition according to the above (2), wherein q is hydrogen, or an alkyl group having a total of 1 to 6 carbon atoms which may contain at least one of the following substituents: a glycidyl group, a hydroxyl group, and an acryloyl group. (4) The hard coat composition according to the above (2), wherein the (meth)acryloyl polymer contains at least one of repeating units represented by the following formulae (II-a), (II-b), and (II-c): [ka] (5) The hard coat composition according to any one of (1) to (4) above, comprising 20 to 80% by weight of the (meth)acryloyl polymer and 80 to 20% by weight of inorganic oxide nanoparticles, based on the total weight of the hard coat composition. (6) The hard coat composition according to any one of (1) to (5) above, wherein the inorganic oxide nanoparticles contain silica having copolymerizable groups on the surface thereof. (7) The hard coat composition according to any one of the above (1) to (6), further comprising a leveling agent. (8) The hard coat composition according to the above (7), wherein the leveling agent contains a fluorine-based additive or a silicone-based additive. (9) The hard coat composition according to (7) or (8) above, wherein the hard coat composition contains 10% by weight or less of the leveling agent based on the total weight of the hard coat composition. (10) The hard coat composition according to any one of the above (1) to (9), which is energy ray curable. (11) The hard coat composition according to any one of the above (1) to (10), further comprising a photopolymerization initiator. (12) A laminate sample was obtained by applying the hard coat composition to the surface of the PMMA resin side of a substrate layer having a polycarbonate resin and a PMMA resin laminated thereon, so that a coating layer having a thickness of 7 μm was formed by the hard coat composition, drying the composition at 120° C. for 5 minutes, and cutting the sample to 210 mm×297 mm×0.3 mm (thickness). The laminate was preheated at 190°C for 40 seconds, and the sample was placed in a mold including a right-angled protrusion having a deep drawing height of 13 mm and dimensions of both length and width of 30 mm so that the surface of the polycarbonate resin side of the base layer was in contact with the molded product. The laminate sample was then pressure molded using high-pressure air of 3.5 MPa. The hard coat composition according to any one of the above (1) to (11), wherein the radius R of the region of the obtained pressure-molded body that contacts the right-angled protrusion of the die is 3 mm or less, and no cracks are generated in the coating layer on the pressure-molded body. (13) The hard coat composition is applied to the surface of the PMMA resin side of a substrate layer having a polycarbonate resin and a PMMA resin laminated thereon, so that a coating layer having a thickness of 7 μm is formed by the hard coat composition, and dried at 120° C. for 5 minutes. A masking film made of polypropylene having a thickness of 30 μm is attached to the surface of the uncured coating layer, and a pressure of 30 kg / m is applied to the masking film. 2 The hard coat composition according to any one of the above (1) to (12), wherein after applying a pressure of 0.1 μm for 24 hours and removing the masking film, the surface roughness Sa of the surface of the coating layer is less than 0.01 μm. (14) A laminate film comprising a substrate layer containing a resin and a coating layer having the hard coat composition according to any one of (1) to (13) above. (15) The laminate film according to the above (14), wherein the substrate layer has a thickness of 0.1 mm to 1.0 mm, and the coating layer has a thickness of 1.0 μm to 10 μm. (16) A cured film obtained by curing the laminate film according to (14) or (15) above. (17) The cured film according to (16) above, wherein the surface on the coating layer side has a pencil hardness of B or more. (18) On the surface of the coating layer, #0000 steel wool is applied at 100 gf / cm 2The cured film according to (16) or (17) above, wherein when the coating layer is scratched by reciprocating 15 times under a pressure of 0.1 mm, the change in haze (ΔH) between before and after scratching is less than 3.0%, as evaluated according to JIS K 7136:2000. (19) The cured film according to any one of (16) to (18) above, wherein the adhesion of the coating layer side is evaluated to be 0 according to JIS K 5600-5-6:1999. Effect of the Invention
[0008] The hard coat composition of the present invention contains a specific polymer and nanoparticles as described above, and when cured, it is capable of forming a hard coat layer with high hardness and scratch resistance, and has excellent moldability in the uncured state. Because of such excellent characteristics, the hard coat composition of the present invention is particularly suitable as a material for resin film laminates used in applications such as mobile devices and automobile interior parts. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a cross-sectional view showing a specific example of a laminate film including a coating layer having a hard coat composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and can be modified and carried out as desired within the scope of the effects of the invention.
[0011] [Hard Coat Composition] The hard coat composition of the present invention has a curing property of being cured by irradiation of energy rays, etc., and contains a (meth)acryloyl polymer and inorganic oxide nanoparticles. As will be described in detail later, the hard coat composition has excellent moldability and tack-free property before curing, and when cured to form, for example, a hard coat layer, it can realize high hardness and excellent scratch resistance.
[0012] The hard coat composition preferably contains 20-80% by weight of (meth)acryloyl polymer and 80-20% by weight of inorganic oxide nanoparticles based on the total weight of the hard coat composition, more preferably 30-70% by weight of (meth)acryloyl polymer and 70-30% by weight of inorganic oxide nanoparticles, and even more preferably 40-60% by weight of (meth)acryloyl polymer and 60-40% by weight of inorganic oxide nanoparticles.
[0013] <(Meth)acryloyl polymer> The (meth)acryloyl polymer has a (meth)acrylic equivalent of 200 to 500 g / eq. The (meth)acrylic equivalent of the (meth)acryloyl polymer is preferably 220 to 450 g / eq, and more preferably 250 to 400 g / eq. The (meth)acryloyl polymer also preferably has a double bond equivalent of 100 to 1000 g / eq, and the double bond equivalent of the (meth)acryloyl polymer is more preferably 150 to 800 g / eq, further preferably 200 to 600 g / eq, and particularly preferably 250 to 400 g / eq. The (meth)acryloyl polymer has a weight average molecular weight of 5,000 to 200,000. The weight average molecular weight of the (meth)acryloyl polymer is preferably 10,000 to 150,000, more preferably 15,000 to 100,000, and even more preferably 18,000 to 50,000. The weight average molecular weight can be measured based on the description in paragraphs 0061 to 0064 of JP-A-2007-179018. The details of the measurement method are shown below. [Table 1] That is, first, a calibration curve showing the relationship between the elution time and the molecular weight of polycarbonate was created by a universal calibration method using polystyrene as a standard polymer. Then, the elution curve (chromatogram) of polycarbonate was measured under the same conditions as in the case of the above-mentioned calibration curve. Furthermore, the weight average molecular weight (Mw) was calculated from the elution time (molecular weight) of polycarbonate and the peak area (number of molecules) at that elution time. The weight average molecular weight is represented by the following formula (A), in which Ni means the number of molecules having a molecular weight Mi. Mw = Σ(NiMi 2 ) / Σ(NiMi)···(A) In this specification, (meth)acrylic includes both acrylic and methacrylic.
[0014] As described above, a hard coat composition containing a (meth)acryloyl polymer having a (meth)acrylic equivalent and weight average molecular weight within a specified range has good tack-free properties before curing and good scratch resistance after curing, and is also capable of easily progressing the curing and polymerization reaction.
[0015] The (meth)acryloyl polymer contained in the hard coat composition preferably has a repeating unit represented by the following formula (I). [ka] In formula (I), m is an alkylene group having 1 to 4 carbon atoms or a single bond, n is an alkyl group having 1 to 4 carbon atoms or hydrogen, p is a single bond or an alkylene group having 1 or 2 carbon atoms, and q is an alkyl group having a total of 1 to 12 carbon atoms which may contain at least one substituent selected from the group consisting of an epoxy group, a hydroxyl group, an acryloyl group, and a methacryloyl group, or hydrogen.
[0016] The (meth)acryloyl polymer more preferably contains the following repeating unit, that is, a repeating unit in which, in the above formula (I), m is an alkylene group having 1 or 2 carbon atoms, n is an alkyl group having 1 or 2 carbon atoms, p is a single bond or a methylene group, and q is an alkyl group having a total of 1 to 6 carbon atoms which may contain at least any one of substituents selected from a glycidyl group, a hydroxyl group, and an acryloyl group, or hydrogen. For example, in the above formula (I), m is a methylene group, n is a methyl group, p is a single bond, and q is a methyl group, an alkyl group having 5 or less carbon atoms and containing a glycidyl group (epoxy group), an alkyl group having 8 or less carbon atoms and containing a hydroxyl group and an acryloyl group, or the like.
[0017] Specific examples of the repeating units contained in the (meth)acryloyl polymer include those represented by the following formulae (II-a), (II-b), and (II-c). [ka] In the (meth)acryloyl polymer, the repeating unit of the formula (II-a) is preferably 30 to 85 mol %, more preferably 40 to 80 mol %, based on the total number of moles of the repeating unit of the formula (II-a), the repeating unit of the formula (II-b), and the repeating unit of the formula (II-c). The repeating unit of the formula (II-b) is preferably 5 to 30 mol %, more preferably 10 to 25 mol %, based on the total number of moles. The repeating unit of the formula (II-c) is preferably 10 to 40 mol %, more preferably 10 to 35 mol %, based on the total number of moles. The molar ratio of the repeating unit of the above formula (II-a), the repeating unit of the above formula (II-b), and the repeating unit of the above formula (II-c) is preferably 4.5-5.5:1.5-2.5:2.5-3.5, for example, 5:2:3.
[0018] A pentaerythritol-based polyfunctional acrylate compound may be added to the (meth)acryloyl polymer. Examples of the polyfunctional acrylate compound having a plurality of acrylate groups, preferably three or more acrylate groups, include pentaerythritol tetraacrylate and dipentaerythritol hexaacrylate, which are represented by the following formulae (III-a) and (III-b), respectively, as well as pentaerythritol triacrylate. [ka]
[0019] The polyfunctional acrylate compound is preferably contained in an amount of 70% by weight or less, more preferably 50% by weight or less, based on the total weight of the polyfunctional acrylate compound and the (meth)acryloyl polymer. In this way, by adding the polyfunctional acrylate compound to the hard coat composition and reacting it with the acryloyl group, glycidyl group (epoxy group), and hydroxyl group contained in the side chain of the (meth)acryloyl polymer, a hard coat film having higher scratch resistance can be formed.
[0020] <Inorganic oxide nanoparticles> As the inorganic oxide nanoparticles contained in the hard coat composition, silica particles, alumina particles, etc. can be used. Among these, it is preferable that the inorganic oxide nanoparticles contain silica particles, and it is preferable that the silica particles contain at least colloidal silica. The inorganic oxide nanoparticles contained in the hard coat are preferably treated with a surface treatment agent, which allows the inorganic oxide nanoparticles to be stably dispersed in the hard coat composition, particularly in the (meth)acryloyl polymer component.
[0021] As a surface treatment agent for inorganic oxide nanoparticles, a compound having a substituent that can be bonded to the surface of inorganic oxide nanoparticles and a substituent that is highly compatible with the components of the hard coat composition that disperses inorganic oxide nanoparticles, particularly with (meth)acryloyl polymers, is preferably used. For example, a silane compound, alcohol, amine, carboxylic acid, sulfonic acid, phosphonic acid, etc. are used as the surface treatment agent.
[0022] The inorganic oxide nanoparticles preferably have a copolymerizable group on the surface. The copolymerizable group can be introduced by surface treatment of the inorganic oxide nanoparticles. Specific examples of the copolymerizable group include a vinyl group, a (meth)acrylic group, and a free radical polymerizable group. The average particle size of the inorganic oxide nanoparticles is from 6 to less than 95 nm, more preferably from 7 to 50 nm, and further preferably from 8 to 20 nm. In order to prevent the occurrence of irregularities on the surface of the hard coat composition after curing and to obtain a good surface appearance, it is preferable to use inorganic oxide nanoparticles that are in a state of as little aggregation as possible.
[0023] <Other components in the hard coat composition> The hard coat composition preferably further contains a leveling agent in addition to the above-mentioned (meth)acryloyl polymer and inorganic oxide nanoparticles. As the leveling agent, for example, a fluorine-based additive or a silicone-based additive is used. As the fluorine-based additive, MEGAFAC RS-56, RS-75, RS-76-E, RS-76-NS, RS-78, RS-90 manufactured by DIC, FTERGENT 710FL, 220P, 208G, 601AD, 602A, 650A, 228P, FTERGENT 240GFTX-218 manufactured by NEOS (all of which are fluorine-containing UV-reactive group-containing oligomers), etc. are used, and among these, FTERGENT 601AD, etc. is preferred as the fluorine-based additive. As the silicone additive, BYK-UV3500 and BYK-UV3505 (both of which are acrylic group-containing polyether-modified polydimethylsiloxanes) manufactured by BYK-Chemie AG are used, and among these, BYK-UV3500 and the like are preferred as the silicone additive.
[0024] The hard coat composition preferably contains 0.1 wt % or more and 10 wt % or less of a leveling agent based on the total weight of the hard coat composition, and the content of the leveling agent in the hard coat composition is more preferably 0.5 wt % or more and 7 wt % or less, and even more preferably 1 wt % or more and 5 wt % or less.
[0025] The curable hard coat composition may be energy ray curable or heat curable, but is preferably energy ray curable, more preferably ultraviolet curable. Therefore, it is preferable that the hard coat composition further contains a photopolymerization initiator. As the photopolymerization initiator, IRGACURE 184 (1-hydroxy-cyclohexyl-phenyl-ketone), IRGACURE 1173 (2-hydroxy-2-methyl-1-phenyl-propan-1-one), IRGACURE TPO (2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide), IRGACURE 819 (bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide), EsacureONE (oligo(2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone), etc. are used, and among these, IRGACURE TPO, etc. are preferred as the photopolymerization initiator from the viewpoint of heat resistance. The hard coat composition contains, for example, 1% by weight or more and 6% by weight or less of a photopolymerization initiator based on the total weight of the hard coat composition. The content of the photopolymerization initiator in the hard coat composition is more preferably 2% by weight or more and 5% by weight or less, and even more preferably 3% by weight or more and 4% by weight or less.
[0026] The hard coat composition may contain other additives, such as at least one additive selected from the group consisting of a heat stabilizer, an antioxidant, a flame retardant, a flame retardant assistant, an ultraviolet absorber, a release agent, and a colorant. As long as the desired physical properties are not significantly impaired, an antistatic agent, a fluorescent brightener, an antifogging agent, a flow improver, a plasticizer, a dispersant, an antibacterial agent, etc. may be added to the hard coat composition. In the hard coat composition, the (meth)acryloyl polymer and the inorganic oxide nanoparticles are preferably contained in an amount of 60% by mass or more, more preferably 80% by mass or more, and particularly preferably 90% by mass or more. Therefore, the content of components other than the above two main components in the hard coat composition is preferably less than 40% by mass, more preferably less than 20% by mass, and particularly preferably less than 10% by mass.
[0027] <Production of hard coat composition> The hard coat composition is produced by blending materials such as the above-mentioned (meth)acryloyl polymer and inorganic oxide nanoparticles. For example, each component such as the (meth)acryloyl polymer is mixed using a tumbler, and then melt-kneaded using an extruder to produce the (meth)acryloyl polymer. Here, the form of the resin composition is not limited to pellets, and may be flakes, powder, bulk, or the like.
[0028] <Properties of the hard coat composition> (i) Tack-free property The hard coat composition of the present invention has excellent tack-free properties. Therefore, even if the uncured hard coat composition comes into contact with other substances such as the hands of a worker, it can maintain a predetermined shape, and the adhesion of a part of the hard coat composition to the surface of the contacted substance is suppressed. In this way, according to the hard coat composition having excellent tack-free properties, it is easy to carry out the process of curing after molding into shapes suitable for various applications. In addition, it is easy to store or distribute the hard coat composition in a predetermined shape before curing.
[0029] In contrast, resin compositions with poor tack-free properties, for example, resin compositions mainly composed of low molecular weight oligomers, require a curing step before being molded into shapes suitable for various applications, and therefore tend to have poor moldability.
[0030] (ii) Gloss (appearance) after removing the masking In the hard coat composition of the present invention, when the uncured hard coat composition is processed into a film, and a masking film is laminated thereon and then peeled off, the occurrence of unevenness on the film surface can be suppressed and good gloss can be maintained. As will be described in detail later, in such evaluation tests, it was confirmed that the hard coat composition of the present invention can keep the surface smooth and maintain good gloss after the masking film is peeled off.
[0031] (iii) Formability (pressure formability) The hard coat composition of the present invention is also excellent in moldability in an uncured state. The moldability of the hard coat composition is evaluated, for example, as follows. That is, after applying the hard coat composition on the surface of the substrate layer and drying it, the obtained laminate is placed on a mold having a convex portion and heated to perform pressure molding, and the hard coat composition in the form of a sheet can be evaluated by whether it is appropriately stretched while following the convex portion, and whether cracks occur, etc. As described in detail below, in such evaluation tests, it was confirmed that the hard coat composition of the present invention can be stretched while conforming to protrusions without causing cracks during pressure forming.
[0032] (iv) Scratch resistance When the hard coat composition of the present invention is cured, high scratch resistance is realized. As will be described in detail later, when a laminate having a layer of the hard coat composition is cured to form a hard coat layer, it has been confirmed that the scratch resistance of the surface of the hard coat layer is superior to that of cured PMMA resin (polymethyl methacrylate resin) and lens resin.
[0033] (v)Hardness The cured hard coat composition has high hardness. Specifically, when applied to a PMMA substrate and cured, it can achieve a pencil hardness of B or more according to the evaluation method of JIS K 5600-5-4:1999. The surface of the cured hard coat composition preferably achieves a pencil hardness of F or more, particularly preferably 2H or more.
[0034] (vi) Adhesion The cured hard coat composition also has excellent adhesion to resin substrates. Specifically, as described in detail below, when the composition was applied to a PMMA substrate and cured, the evaluation result determined by the evaluation method of JIS K 5600-5-6:1999 was 0, which is better than the evaluation results 1 to 5.
[0035] [Laminated film] The laminate film of the present invention is obtained by laminating a coating layer having the above-mentioned hard coat composition in an uncured state, preferably a coating layer consisting of the hard coat composition in an uncured state, on any surface of a base layer containing a resin.
[0036] The base layer of the laminate film preferably contains a resin, more preferably a thermoplastic resin. There is no particular limitation on the type of thermoplastic resin, but various resins such as polycarbonate (PC) resin, acrylic resin such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), polyimide (PI), cycloolefin copolymer (COC), norbornene-containing resin, polyethersulfone, cellophane, and aromatic polyamide are used. Of these options, the thermoplastic resin of the base layer preferably contains at least a polycarbonate resin.
[0037] The type of polycarbonate resin contained in the base layer of the laminate film is not particularly limited as long as it contains a -[OR-OCO]- unit (wherein R contains an aliphatic group, an aromatic group, or both an aliphatic group and an aromatic group, and further has a straight-chain structure or a branched structure) containing a carbonate bond in the molecular main chain, but polycarbonates having a bisphenol skeleton are preferred, and polycarbonates having a bisphenol A skeleton or a bisphenol C skeleton are particularly preferred. As the polycarbonate resin, a mixture or copolymer of bisphenol A and bisphenol C may be used. By using a bisphenol C-based polycarbonate resin, for example, a polycarbonate resin containing only bisphenol C, or a mixture or copolymer of bisphenol C and bisphenol A, the hardness of the base layer can be improved. The viscosity average molecular weight of the polycarbonate resin is preferably from 15,000 to 40,000, more preferably from 20,000 to 35,000, and further preferably from 22,500 to 25,000.
[0038] The acrylic resin contained in the base layer of the laminate film is not particularly limited, but may be, for example, a homopolymer of various (meth)acrylic acid esters such as polymethyl methacrylate (PMMA) or methyl methacrylate (MMA), or a copolymer of PMMA or MMA with one or more other monomers, or a mixture of a plurality of these resins. Among these, a (meth)acrylate containing a cyclic alkyl structure having low birefringence, low moisture absorption, and excellent heat resistance is preferred. Examples of such (meth)acrylic resins include, but are not limited to, Acrypet (manufactured by Mitsubishi Rayon), Delpet (manufactured by Asahi Kasei Chemicals), and Parapet (manufactured by Kuraray). It is preferable to use a laminate in which the above-mentioned acrylic resin is laminated on the surface layer of a polycarbonate resin as the substrate, since this can improve the hardness of the surface layer of the substrate layer.
[0039] The substrate layer of the laminate film may contain additives other than the thermoplastic resin. For example, at least one additive selected from the group consisting of a heat stabilizer, an antioxidant, a flame retardant, a flame retardant assistant, an ultraviolet absorber, a release agent, and a colorant. In addition, an antistatic agent, a fluorescent brightener, an antifogging agent, a flow improver, a plasticizer, a dispersant, an antibacterial agent, etc. may be added to the substrate layer.
[0040] The base layer of the laminate film preferably contains 80% by mass or more of thermoplastic resin, more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The base layer preferably contains 80% by mass or more of polycarbonate resin, more preferably 90% by mass or more, and particularly preferably 95% by mass or more of polycarbonate resin.
[0041] The thickness of the base layer of the laminate film is not particularly limited, but is preferably 30 to 1000 μm (1 mm), more preferably 50 to 700 μm, and particularly preferably 100 to 500 μm. Two or more base layers may be provided, and when a plurality of base layers are provided, the total thickness of the base layers is, for example, 100 to 1000 μm, preferably about 200 to 500 μm.
[0042] The laminate film of the present invention is manufactured as follows. First, in the manufacture of the base layer, a material such as a resin composition is processed into a layer (sheet) by a conventional method. For example, this is a method using extrusion molding or cast molding. An example of extrusion molding is a method in which pellets, flakes or powder of a resin composition are melted and kneaded in an extruder, then extruded from a T-die or the like, and the resulting semi-molten sheet is cooled and solidified while being pressed between rolls to form a sheet.
[0043] The coating composition is then applied to the outer surface of the substrate layer having a single layer or a plurality of layers and dried to form a coating layer.
[0044] In the laminate film, the thickness of the base layer is preferably 0.1 mm to 1.0 mm, for example, 0.2 mm to 0.8 mm, or 0.3 mm to 0.7 mm. In the laminate film, the coating layer preferably has a thickness of 1.0 μm to 10 μm. The coating layer has a thickness of, for example, 2.0 μm to 8.0 μm, or 3.0 μm to 5.0 μm.
[0045] The structure of the laminate film is, for example, as shown in Fig. 1. In the laminate film 10 illustrated in Fig. 1, a coating layer 12 formed mainly of a hard coat composition, preferably only of a hard coat composition, is laminated on the surface of the PMMA layer side of a base layer having a polymethyl methacrylate layer (PMMA resin layer) 20 and a polycarbonate layer (PC resin layer) 22.
[0046] [Hardened film] The cured film of the present invention is obtained by curing the above-mentioned laminate film. That is, the laminate film has a curable coating layer, and the cured film can be obtained by curing the coating layer of the laminate film. The curing method may be photocuring or heat curing.
[0047] As is clear from the properties of the hard coat composition after curing described above, the surface of the coating layer side of the cured film of the present invention has excellent properties. That is, the surface of the coating layer side of the cured film realizes high pencil hardness, preferably pencil hardness of B or higher based on JIS K 5600-5-4:1999, high scratch resistance, and excellent adhesion, for example, adhesion evaluated as level 0 in JIS K 5600-5-6:1999. EXAMPLES
[0048] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and can be modified as desired without departing from the gist of the present invention.
[0049] [Laminate manufacturing] First, a coating composition (coating solution) was prepared by mixing the components shown in Table 2 below. The acryloyl polymers used here are as follows. (a) Acryloyl polymer A: Artcure RA-3602MI manufactured by Negami Chemical Industries (Acrylic polymer containing double bonds in the side chain: (meth)acrylic equivalent 300g / eq: double bond equivalent 300g / eq) (b) Acryloyl polymer B: Star-501 manufactured by Osaka Organic Chemical Industry Co., Ltd. (Dendrimer polyacrylate (multi-branched (dipentaerythritol hexaacrylate (DPHA) linked type) polyacrylate with acrylate groups at the ends: (meth)acrylic equivalent 120g / eq) (c) Acryloyl polymer C: Artcure OAP-5000 manufactured by Negami Chemical Industries (Acrylic polymer containing double bonds in the side chain: (meth)acrylic equivalent 2000g / eq: double bond equivalent 2000g / eq) (d) Acryloyl polymer D: Negami Chemical Industries Art Resin UN-3320HC (Urethane acrylate oligomer: (meth)acrylic equivalent 250g / eq) The inorganic oxide particles (nanosilica) added to the coating solution are as follows: Nanosilica: MEK-AC-2140Z (organosilica sol (average particle size 10-15 nm: surface-modified silica sol) manufactured by Nissan Chemical Co., Ltd. Furthermore, MEK was added to the obtained mixture as a dilution solvent, and the coating solution adjusted to a solid content of 30 wt% was coated onto the PMMA side of a PC / PMMA co-extruded film (PC: Iupilon E-2000, manufactured by Mitsubishi Engineering Plastics Corporation; PMMA: Altoglass V020, manufactured by Arkema; PMMA layer thickness 45 μm: total thickness 0.3 mm). The coating process was performed using a #16 wire wound rod and the applied coating solution was dried at 120°C for 5 minutes. The dried coating solution formed a coating layer approximately 7 micrometers thick. The coating layer was then cured using a Fusion H bulb (Fusion UV Systems) at 90% power with air blowing at 1.8 m / min. The UV exposure conditions were 1000 mJ / cm. 2 It was.
[0050] [Evaluation of properties] The properties of the thus obtained cured laminate and the laminate in a state before the coating layer was dried and cured (uncured laminate) were evaluated as follows.
[0051] <Tack-free in uncured state> The tack-free properties of the uncured laminate were evaluated by finger touch evaluation.
[0052] <Gloss (appearance) after removing masking in uncured state> A test piece having a substrate layer in which polycarbonate resin and PMMA resin were laminated was prepared, and the hard coat composition was applied to the surface of the substrate layer of the test piece on the PMMA resin side so that a coating layer having a thickness of 7 μm was formed by the hard coat composition, followed by drying at 120° C. for 5 minutes. A 30 μm thick masking film made of polypropylene was then attached to the surface of the uncured coating layer, and a 30 kg / m 2After applying this pressure for 24 hours, the masking film was peeled off, and the surface roughness Sa (based on ISO25178) of the surface of the coating layer was measured using a scanning white light interference microscope VS1530 manufactured by Hitachi High-Technologies Corporation. The examples and comparative examples having a surface roughness Sa value of less than 0.01 μm were evaluated as having good appearance.
[0053] <Moldability in uncured state (compressed air moldability)> A test piece having a substrate layer in which polycarbonate resin and PMMA resin were laminated was prepared, and the hard coat composition was applied to the surface of the substrate layer of the test piece on the PMMA resin side so that a coating layer having a thickness of 7 μm was formed by the hard coat composition, followed by drying at 120° C. for 5 minutes. Then, for the laminate sample obtained by cutting to 210 mm x 297 mm x 0.3 mm (thickness), the laminate was preheated at 190°C for 40 seconds, and the sample was placed in a mold containing a right-angled protrusion having a deep drawing height of 13 mm and dimensions of both length and width of 30 mm so that the surface of the polycarbonate resin side of the base layer was in contact with the mold, and the laminate sample was subjected to pressure molding using high-pressure air of 3.5 MPa. The moldability of the examples and comparative examples in which the radius R of the area of the pressure-molded body in contact with the right-angled portion of the mold was within 3 mm and no cracks occurred in the coating layer on the pressure-molded body was evaluated as good. In the base layer which was a laminate of polycarbonate resin and PMMA resin, as described above, the thickness of the PMMA layer was 45 μm, and the total thickness was 0.3 mm.
[0054] <Scratch resistance after curing> After curing, apply 100gf / cm of #0000 steel wool to the surface of the coating. 2The sample was scratched by moving it back and forth 15 times under a pressure of 1.0 mm. Based on JIS K 7136:2000, the absolute value of the haze change (ΔH), which is the difference between the haze value measured before the scratch test and the haze value measured after the scratch test based on JIS K 7136:2000, was calculated and evaluated. For the examples and comparative examples in which the ΔH value was less than 3.0%, the scratch resistance was evaluated as good.
[0055] <Chemical resistance after curing> Neutrogena SPF100 was applied to the surface of the cured coating layer, and the appearance was visually observed after 1 hour at 80° C. Examples and comparative examples with no abnormalities on the surface were evaluated as having good chemical resistance.
[0056] <Pencil hardness after curing> Measurements were carried out based on the conditions of JIS K 5600-5-4:1999, and the evaluation was based on the hardest pencil grit that did not cause scratches. <Adhesion> The adhesion was evaluated according to the evaluation method of JIS K5600-5-6: 1999. For the examples and comparative examples with an evaluation result of 0, the adhesion was evaluated as good. The measurement results of the properties of the film of the laminates of each of the Examples and Comparative Examples are shown in Table 2. [Table 2] [Explanation of symbols]
[0057] 10. Laminated film 12 Coating Layer 20 Polymethyl methacrylate layer (PMMA resin layer) 22 Polycarbonate layer (PC resin layer)
Claims
1. A hard coat composition is applied onto a surface of the PMMA resin side of a substrate layer in which a polycarbonate resin and a PMMA resin are laminated, so that a coating layer having a thickness of 7 μm is formed by the hard coat composition, and the hard coat composition is dried at 120° C. for 5 minutes; A masking film made of polypropylene and having a thickness of 30 μm is attached to the surface of the uncured coating layer, and a pressure of 30 kg / m2 is applied to the masking film. After 24 hours have passed, the surface roughness Sa of the surface of the coating layer after the masking film is peeled off is less than 0.01 μm.
1. A curable hard coat composition comprising: Based on the total weight of the hard coat composition, the hard coat composition comprises 20 to 80 weight percent (meth)acryloyl polymer and 80 to 20 weight percent inorganic oxide nanoparticles; the (meth)acryloyl polymer has a double bond equivalent of 100 to 1000 g / eq and a weight average molecular weight of 5,000 to 200,000; The inorganic oxide nanoparticles have an average particle size of 6 to less than 95 nm; In the hard coat composition, the content of components other than the two components of the (meth)acryloyl polymer and the inorganic oxide nanoparticles is less than 40 mass %. Hardcoat Composition.
2. The hard coat composition of claim 1, wherein the (meth)acryloyl polymer comprises a repeating unit represented by the following formula (I): [Formula 1] (In the above formula (I), m is an alkylene group having 1 to 4 carbon atoms or a single bond; n is an alkyl group having 1 to 4 carbon atoms or hydrogen; p is a single bond or an alkylene group having 1 or 2 carbon atoms; q is an alkyl group having a total of 1 to 12 carbon atoms which may contain at least one of the following substituents: an epoxy group, a hydroxyl group, an acryloyl group, and a methacryloyl group, or a hydrogen atom.
3. In the formula (I), m is an alkylene group having 1 or 2 carbon atoms; n is an alkyl group having 1 or 2 carbon atoms; p is a single bond or a methylene group; 3. The hard coat composition according to claim 2, wherein q is an alkyl group having a total of 1 to 6 carbon atoms which may contain at least one of a glycidyl group, a hydroxyl group, and an acryloyl group, or a hydrogen atom.
4. The hard coat composition of claim 2, wherein the (meth)acryloyl polymer contains at least one of repeating units represented by the following formulas (II-a), (II-b), and (II-c): [chemical 2] 5. The hard coat composition of claim 1, wherein the inorganic oxide nanoparticles comprise silica having copolymerizable groups on the surface thereof.
6. The hard coat composition of claim 1, further comprising a leveling agent.
7. The hard coat composition of claim 6, wherein the leveling agent comprises a fluorine-based additive or a silicone-based additive.
8. The hard coat composition of claim 6 or 7, wherein the hard coat composition comprises 10 wt. % or less of the leveling agent based on the total weight of the hard coat composition.
9. The hard coat composition of claim 1, wherein the (meth)acryloyl polymer has a (meth)acrylic equivalent of 200 to 500 g / eq.
10. The hard coat composition according to any one of claims 1 to 9, which is energy ray curable.
11. The hard coat composition according to claim 1, further comprising a photopolymerization initiator.
12. A laminate sample obtained by applying a hard coat composition to a surface of the PMMA resin side of a substrate layer having a polycarbonate resin and a PMMA resin laminated thereon so that a coating layer having a thickness of 7 μm is formed by the hard coat composition, drying the composition at 120° C. for 5 minutes, and cutting the resulting sample to a size of 210 mm x 297 mm x 0.3 mm (thickness), The laminate was preheated at 190°C for 40 seconds, and the sample was placed in a mold including a right-angled protrusion having a deep drawing height of 13 mm and a length and width of 30 mm so that the surface of the polycarbonate resin side of the base layer was in contact with the molded product. The laminate sample was then subjected to pressure molding using high-pressure air of 3.5 MPa. The hard coat composition according to any one of claims 1 to 11, wherein the radius R of a region of the obtained pressure-molded body that contacts the right-angled protrusion of the die is 3 mm or less, and no cracks are generated in the coating layer on the pressure-molded body.
13. A laminate film comprising a coating layer having the hard coat composition according to any one of claims 1 to 12 on a substrate layer comprising a resin.
14. A laminate film as described in claim 13, wherein the thickness of the substrate layer is 0.1 mm to 1.0 mm, and the thickness of the coating layer is 1.0 μm to 10 μm.
15. A cured film obtained by curing the laminate film described in claim 13 or 14.
16. The cured film described in claim 15, wherein the pencil hardness of the surface on the coating layer side is B or higher.
17. A cured film as described in claim 15 or 16, wherein when the surface of the coating layer side is scratched by moving #0000 steel wool back and forth 15 times under a pressure of 100 gf / cm2, the change in haze (ΔH) of the coating layer before and after scratching, evaluated in accordance with JIS K 7136:2000, is less than 3.0%.
18. The cured film according to claim 15, wherein the adhesion of the coating layer side is evaluated as 0 according to JIS K 5600-5-6:1999.
19. The hard coat composition according to claim 1, which does not contain an isocyanate compound.