Carbon dioxide adsorption-reduction catalyst
A catalyst with a porous metal oxide carrier and specific ruthenium and lithium content addresses high energy consumption and low storage density issues, ensuring efficient carbon dioxide processing and methane generation even at low temperatures.
Patent Information
- Application Number
- JP2023043415
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing carbon dioxide storage reduction catalysts face issues with high energy consumption, reduced Ru activity due to high temperatures, low storage density, and insufficient processing capacity, particularly when using CaO or Li as storage materials.
A catalyst comprising a porous metal oxide carrier with ruthenium and lithium within specific content ranges, supporting excellent carbon dioxide storage and methanation performance, even at low temperatures.
The catalyst achieves enhanced processing capacity and storage density, reducing energy requirements and maintaining performance across varying temperatures, including startup conditions.
Smart Images

Figure 2024132582000002 
Figure 2024132582000003 
Figure 2024132582000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon dioxide (CO2) storage-reduction catalyst, and more particularly to a lithium-containing CO2 storage-reduction catalyst. [Background technology]
[0002] Methanation reactions using carbon dioxide (CO2) as a raw material have been attracting attention in recent years from the perspective of reducing CO2 emissions to curb global warming. Catalysts used in such methanation reactions include CO2 occlusion / reduction catalysts in which calcium oxide (CaO) as a CO2 occlusion material and ruthenium (Ru) as a methanation catalyst are supported on a support such as alumina (for example, JP 2020-110769 A (Patent Document 1)), and CO2 occlusion / reduction catalysts in which an alkali metal oxide as a CO2 occlusion material and ruthenium (Ru) as a methanation catalyst are supported on an alumina support (for example, A. Porta et al., Ind. Eng. Chem. Res., 2021, Vol. 60, pp. 6706-6718 (Non-Patent Document 1) and S. Cimino et al., J. CO2 Utilization, 2020, Vol. 37, pp. 195-203 (Non-Patent Document 2)). Such a CO2 storage reduction catalyst stores CO2 by passing a gas containing CO2 through it, and reduces the stored CO2 by passing a reducing gas (e.g., H2) through it to produce methane (CH4).
[0003] However, in the case of CO2 storage reduction catalysts using CaO as a CO2 storage material, the start temperature during storage / reduction is as high as 320°C, so excessive heat energy must be input when the CO2 storage reduction catalyst system is operating, resulting in a problem of reduced energy efficiency of the system. In addition, at high temperatures, O2 contained in the exhaust gas reacts with Ru, which may permanently reduce the activity of Ru. Furthermore, because CaO has a low CO2 storage density, a large amount of catalyst must be used, which requires a large reactor size, and the amount of Ru also increases, resulting in high equipment costs.
[0004] Furthermore, Non-Patent Document 1 describes that a CO2 storage reduction catalyst that uses Li as an alkali metal for the CO2 storage material has lower catalytic activity than a CO2 storage reduction catalyst that uses other alkali metals, and in the CO2 storage reduction catalyst described in Non-Patent Document 2, when Li is used as the alkali metal, the catalytic activity is improved compared to when other alkali metals are used, but the CO2 processing capacity in exhaust gas is still not sufficient. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-110769 A [Non-patent literature]
[0006] [Non-Patent Document 1] A. Porta et al., Ind. Eng. Chem. Res. 2021, vol. 60, pp. 6706-6718 [Non-Patent Document 2] S. Cimino et al., J. CO2 Utilization, 2020, Vol. 37, pp. 195-203 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the problems associated with the above-mentioned conventional technology, and aims to provide a CO2 storage-reduction catalyst that contains lithium (Li) as a CO2 storage material and has excellent CO2 storage performance and methanation catalytic performance (hereinafter, collectively referred to as "CO2 processing capacity"). [Means for solving the problem]
[0008] As a result of extensive research to achieve the above-mentioned object, the inventors discovered that in a CO2 storage-reduction catalyst in which lithium (Li) as a CO2 storage material and ruthenium (Ru) as a methanation catalyst are supported on a carrier such as alumina, excellent CO2 processing capacity can be achieved by setting the Ru content and Li content within specific ranges, and thus completed the present invention.
[0009] That is, the present invention provides the following aspects.
[0010] [1] A catalyst comprising a porous support made of a metal oxide, ruthenium supported on the porous support, and lithium supported on the porous support, The content of the ruthenium is 1 to 5 mass% based on the total amount of the catalyst, The content of the lithium is 6 to 9 mass% in terms of lithium oxide based on the entire catalyst. Carbon dioxide storage reduction catalyst.
[0011] [2] The specific surface area of the porous carrier is 100 to 500 m 2 / g of the carbon dioxide storage reduction catalyst according to [1].
[0012] [3] The carbon dioxide occlusion / reduction catalyst according to [1] or [2], wherein the porous support has a bulk density of 0.5 to 2 g / ml.
[0013] [4] The carbon dioxide occlusion / reduction catalyst according to any one of [1] to [3], wherein the average particle size of the granules of the porous carrier is 0.1 to 6 mm. Effect of the Invention
[0014] According to the present invention, in a CO2 occlusion reduction catalyst containing lithium (Li) as a CO2 occlusion material, it is possible to develop excellent CO2 treatment capacity and to maintain the excellent CO2 treatment capacity even at low temperatures. [Brief description of the drawings]
[0015] [Figure 1]1 is a graph showing temperature profiles in a performance evaluation test of catalysts obtained in Examples and Comparative Examples. [Diagram 2] 1 is a graph showing the relationship between the content of various CO2 occlusion materials and the CO2 processing capacity. [Diagram 3] 1 is a graph showing the relationship between evaluation temperature T1 and CO2 treatment capacity in a catalyst performance evaluation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below based on preferred embodiments thereof.
[0017] [CO2 storage reduction catalyst] The carbon dioxide (CO2) storage-reduction catalyst of the present invention is a catalyst containing a porous support made of a metal oxide, ruthenium supported on the porous support, and lithium supported on the porous support.
[0018] The carrier used in the present invention is a porous carrier made of a metal oxide. By using a porous carrier, gas components are well diffused, and the CO2 processing capacity is improved. The metal oxide is not particularly limited as long as it is used as a carrier for a CO2 storage reduction catalyst, and examples thereof include known metal oxides such as alumina (Al2O3), silica (SiO2), zirconia (ZrO2), titania (TiO2), ceria (CeO2), and zeolite. Among these metal oxides, alumina and titania are preferred, and alumina is more preferred, from the viewpoint of increasing the methanation catalytic performance. Moreover, such metal oxides may be used alone or in combination of two or more.
[0019] The specific surface area of the porous carrier is 100 to 500 m 2 / g is preferable, and 200 to 300m 2When the specific surface area of the porous carrier is less than the lower limit, the CO2 absorption rate decreases, and the CO2 processing capacity tends to decrease, whereas when the specific surface area of the porous carrier is more than the upper limit, the bulk density of the porous carrier decreases, and the CO2 absorption density tends to decrease.
[0020] The bulk density of the porous carrier is preferably 0.5 to 2 g / ml, more preferably 0.8 to 1.0 g / ml. If the bulk density of the porous carrier is less than the lower limit, the bulk density of the catalyst decreases, and the CO2 storage density tends to decrease, whereas if the bulk density exceeds the upper limit, the active area having the CO2 processing ability decreases, and the CO2 processing ability tends to decrease.
[0021] Furthermore, the average pore diameter of the porous carrier is preferably 3 to 50 nm, more preferably 5 to 20 nm. If the average pore diameter of the porous carrier is less than the lower limit, gas components do not diffuse sufficiently, and the CO2 treatment capacity tends to decrease, while if it exceeds the upper limit, the stability of the pore structure tends to decrease.
[0022] The pore volume of the porous carrier is 0.3 to 1.5 cm 3 / g is preferable, and 0.3 to 1.0 cm 3 When the pore volume of the porous carrier is less than the lower limit, the gas components do not diffuse sufficiently, and the CO2 treatment capacity tends to decrease, whereas when the pore volume of the porous carrier is more than the upper limit, the thermal stability of the porous carrier tends to decrease.
[0023] Furthermore, the porous carrier is preferably a granule, and the average particle size thereof is preferably 0.1 to 6 mm, more preferably 0.5 to 3 mm. If the average particle size of the granules of the porous carrier is less than the lower limit, the flow of gas components is hindered, and therefore, there is a tendency that surplus energy is required for pressurization for gas flow, whereas if the average particle size exceeds the upper limit, there is a tendency that gas diffusion into the inside of the granules is hindered, and therefore, CO2 processing capacity is reduced.
[0024] In the CO2 storage reduction catalyst of the present invention, ruthenium (Ru) is supported on the porous carrier. This Ru acts as a methanation catalyst, specifically, it promotes the reduction reaction of CO2 when the CO2 stored in the CO2 storage material reacts with a reducing gas (e.g., H2) and is reduced to produce methane (CH4).
[0025] In the CO2 storage reduction catalyst of the present invention, the Ru content is 1 to 5 mass% based on the total catalyst. When the Ru content is within the above range, the reduction reaction of CO2 is promoted, and the methanation catalytic activity is improved. On the other hand, when the Ru content is below the above lower limit, the reduction reaction of CO2 is not promoted sufficiently, and the methanation catalytic activity is reduced. On the other hand, when the Ru content exceeds the above upper limit, the pores of the porous support are blocked, reducing the amount of CO2 storage, thereby reducing the CO2 storage performance, or the Ru grains grow, thereby reducing the methanation catalytic activity.
[0026] In the CO2 storage-reduction catalyst of the present invention, lithium (Li) is supported on the porous support. Li acts as a CO2 storage material. Such Li is usually supported on the porous support in the form of an oxide.
[0027] The reason why a CO2 occlusion reduction catalyst using Li as a CO2 occlusion material has a higher CO2 processing capacity than a CO2 occlusion reduction catalyst using other alkali metals is not entirely clear, but the inventors speculate as follows. That is, when a gas containing CO2 is contacted with a CO2 occlusion reduction catalyst containing an alkali metal as a CO2 occlusion material, the CO2 reacts with the alkali metal to form a carbonate and is occluded in the catalyst [CO2 occlusion process]. When a gas containing H2 is contacted with the catalyst that has occluded CO2, the CO2 is reduced by the H2 to produce methane (CH4) [reduction process].
[0028] When Li is used as an alkali metal, lithium carbonate (Li2CO3) formed by reacting with CO2 is thermodynamically moderate, so the CO2 absorption process and the reduction process proceed in a well-balanced manner, and good CO2 absorption performance and good methanation catalytic performance are compatible, so it is presumed that the CO2 treatment capacity will be high. In addition, since the reduction process proceeds even at low temperatures, good methanation catalytic performance is maintained, and high CO2 treatment capacity is expressed.
[0029] On the other hand, when potassium (K) or sodium (Na) is used as the alkali metal, potassium carbonate (K2CO3) or sodium carbonate (Na2CO3) formed by the reaction with CO2 is thermodynamically more stable than Li2CO3, so it is presumed that the reduction process does not proceed easily, the methanation catalyst performance decreases, and the CO2 treatment capacity decreases. In particular, at low temperatures, the reduction process proceeds significantly slower, so it is presumed that the methanation catalyst performance decreases further and the CO2 treatment capacity decreases further.
[0030] On the other hand, when magnesium (Mg) is used as the alkali metal, magnesium carbonate (MgO) formed by reacting with CO2 is thermodynamically unstable compared to Li2CO3. Therefore, it is presumed that the absorption process does not proceed easily, the CO2 absorption performance decreases, and the CO2 processing capacity decreases.
[0031] In the CO2 storage-reduction catalyst of the present invention, the Li content is 6 to 9 mass% in terms of lithium oxide with respect to the entire catalyst. When the Li content is within the above range, excellent CO2 storage performance is exhibited and high CO2 processing capacity is obtained. On the other hand, when the Li content is less than the above lower limit, the CO2 storage site is small, and the CO2 storage performance is reduced. On the other hand, when the Li content exceeds the above upper limit, the pores of the porous support are blocked, and the amount of CO2 storage is reduced, and the CO2 storage performance is reduced. The Li content is preferably 7 to 9 mass% in terms of lithium oxide, and more preferably 7.5 to 8.5 mass%, from the viewpoint of exhibiting even better CO2 storage performance and improving CO2 processing capacity.
[0032] [Method for manufacturing CO2 storage reduction catalyst] The CO2 occlusion reduction catalyst of the present invention can be prepared, for example, as follows. That is, an aqueous solution containing a Li salt is prepared, a predetermined amount of a porous carrier made of a metal oxide supporting Ru is added to the aqueous solution, and then the solution is dried and fired to obtain a CO2 occlusion reduction catalyst in which Ru and Li are supported on the porous carrier made of the metal oxide. The metal oxide supporting Ru may be prepared by adding a predetermined amount of a metal oxide to an aqueous solution containing a Ru salt, followed by drying and firing, or may be a commercially available product. In addition, an aqueous solution containing a Li salt is prepared, a predetermined amount of a porous carrier made of a metal oxide is added to the aqueous solution, followed by drying and firing to prepare a CO2 occlusion material in which lithium oxide is supported on the porous carrier made of the metal oxide, and the CO2 occlusion material is added to an aqueous solution in which a predetermined amount of Ru salt is dissolved, followed by drying and firing to obtain a CO2 occlusion reduction catalyst in which Ru and Li are supported on the porous carrier made of the metal oxide. Furthermore, a CO2 storage reduction catalyst in which Ru and Li are supported on a porous support made of a metal oxide can also be obtained by preparing an aqueous solution containing a Ru salt and a Li salt in a predetermined mass ratio, adding a predetermined amount of a porous support made of a metal oxide to this aqueous solution, and then drying and calcining the solution.
[0033] The firing conditions are not particularly limited as long as the Li salt is converted into an oxide state and the Ru salt is converted into Ru. For example, the firing temperature is preferably 400 to 600°C, and more preferably 450 to 550°C, and the firing time is preferably 1 to 10 hours, and more preferably 3 to 8 hours.
[0034] Examples of Li salts include lithium nitrate (LiNO3), lithium carbonate (Li2CO3), and lithium acetate (CH3COOLi). Examples of Ru salts include ruthenium nitrosyl nitrate, ruthenium nitrate, ruthenium chloride, and dodecacarbonyl triruthenium.
[0035] [CO2 storage and reduction process] Such a CO2 occlusion reduction catalyst of the present invention can be applied to, for example, the following CO2 occlusion reduction process. That is, after a gas containing CO2 is brought into contact with the CO2 occlusion reduction catalyst of the present invention to occlude CO2, the occluded CO2 is reduced to produce CH4 by bringing a reducing gas (e.g., H2) into contact with the CO2 occlusion reduction catalyst with the occluded CO2. Also, while a gas containing CO2 and H2 is brought into contact with the CO2 occlusion reduction catalyst of the present invention to occlude CO2, the occluded CO2 is reacted with a reducing gas (e.g., H2) to reduce the occluded CO2 to produce CH4.
[0036] The CO2 storage-reduction catalyst of the present invention exhibits excellent CO2 processing ability because it has both good CO2 storage performance and good methanation catalytic performance. In particular, since the CO2 storage-reduction catalyst of the present invention maintains good methanation catalytic performance even at low temperatures, it enables reduction of CO2 and production of CH4 without supplying excessive heat energy even at low temperatures such as at the start of the above-mentioned CO2 storage-reduction process, and can maintain excellent CO2 processing ability. EXAMPLES
[0037] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0038] Example 1 First, a ruthenium nitrosyl nitrate nitric acid solution (Ru(NO)(NO3)3HNO3 soln., Furuya Metal Co., Ltd., Ru concentration: 18.73 mass% (metal base)) was diluted with ion-exchanged water to prepare an aqueous solution of ruthenium nitrosyl nitrate nitric acid. The aqueous solution was then poured into spherical activated alumina (Al2O3, Sumika Alchem Co., Ltd., product number: KHO-12, granules (particle size: 1 to 2 mm), specific surface area: 210 m 2The catalyst was added to a 100-milligram catalyst (Ru content: 3.0 mass% relative to the total mass of the catalyst, 0.01 mass / g, bulk density: 0.85 g / ml, pore volume: 0.43 ml / g) in such a way that the Ru content in the resulting catalyst was 3.0 mass% relative to the total mass of the catalyst. The resulting solid-liquid mixture was left to stand at room temperature for 12 hours in a vacuum desiccator whose pressure was reduced using a vacuum pump, and the solid component was recovered and dried at 90°C for 12 hours under normal pressure.
[0039] Next, the solid component after drying was added to an aqueous solution of lithium nitrate prepared by dissolving lithium nitrate (LiNO3, Fujifilm Wako Pure Chemical Industries, Ltd., product number: 128-01232) in ion-exchanged water so that the Li2O content in the resulting catalyst was 6.0 mass% relative to the entire catalyst, and the resulting solid-liquid mixture was left to stand at room temperature for 12 hours in a vacuum desiccator that was depressurized using a vacuum pump to recover the solid component. This solid component was dried at 90°C for 12 hours under normal pressure, and then calcined at 500°C for 5 hours. The resulting calcined product was used to remove the powdery residue using a sieve with a mesh size of 0.5 mm to obtain a granular catalyst [Ru(3) / Li2O(6) / Al2O3(91)] with a particle size of 1 mm or more, in which Ru and Li2O are supported on Al2O3.
[0040] Example 2 A granular catalyst [Ru(3) / Li2O(7) / Al2O3(90)] having a particle size of 1 mm or more and in which Ru and Li2O are supported on Al2O3 was obtained in the same manner as in Example 1, except that the dried solid component was added to the lithium nitrate aqueous solution so that the Li2O content in the resulting catalyst was 7.0 mass% based on the total mass of the catalyst.
[0041] Example 3 A granular catalyst [Ru(3) / Li2O(8) / Al2O3(89)] having a particle size of 1 mm or more and in which Ru and Li2O are supported on Al2O3 was obtained in the same manner as in Example 1, except that the dried solid component was added to the lithium nitrate aqueous solution so that the Li2O content in the resulting catalyst was 8.0 mass% based on the total mass of the catalyst.
[0042] Example 4 A granular catalyst [Ru(3) / Li2O(9) / Al2O3(88)] with a particle size of 1 mm or more, in which Ru and Li2O were supported on Al2O3, was obtained in the same manner as in Example 1, except that the dried solid component was added to the lithium nitrate aqueous solution so that the Li2O content in the resulting catalyst was 9.0 mass% based on the total mass of the catalyst.
[0043] Comparative Example 1 A granular catalyst [Ru(3) / Li2O(4) / Al2O3(93)] having a particle size of 1 mm or more and in which Ru and Li2O are supported on Al2O3 was obtained in the same manner as in Example 1, except that the dried solid component was added to the lithium nitrate aqueous solution so that the Li2O content in the resulting catalyst was 4.0 mass% based on the total mass of the catalyst.
[0044] Comparative Example 2 A granular catalyst [Ru(3) / Li2O(5) / Al2O3(92)] with a particle size of 1 mm or more, in which Ru and Li2O were supported on Al2O3, was obtained in the same manner as in Example 1, except that the dried solid component was added to the lithium nitrate aqueous solution so that the Li2O content in the resulting catalyst was 5.0 mass% based on the total mass of the catalyst.
[0045] Comparative Example 3 A granular catalyst [Ru(3) / Li2O(10) / Al2O3(87)] having a particle size of 1 mm or more and in which Ru and Li2O are supported on Al2O3 was obtained in the same manner as in Example 1, except that the dried solid component was added to the lithium nitrate aqueous solution so that the Li2O content in the resulting catalyst was 10.0 mass% based on the total mass of the catalyst.
[0046] Comparative Example 4 Calcium nitrate tetrahydrate (Ca(NO3)2·4H2O, Fujifilm Wako Pure Chemical Industries, Ltd., product number: 039-00735) was dissolved in ion-exchanged water to prepare an aqueous calcium nitrate solution. Ruthenium-loaded alumina powder (Ru / Al2O3, N.E. Chemcat Corporation, product number: HYAc-5E N-Type, Ru content: 5 mass%, alumina content: 95 mass%, average alumina pore size: 13 nm, alumina pore volume: 0.38 cm3) was added to the aqueous calcium nitrate solution.3 / g) was added so that the CaO content in the resulting catalyst was 8.7 mass% based on the total amount of the catalyst. The resulting solid-liquid mixture was stirred for about 1 hour, and then concentrated on a hot plate set at 350°C until it became a slurry. The resulting slurry was dried at 110°C for 12 hours, and then calcined at 500°C for 5 hours. The resulting calcined product was heated at a pressure of 1000 kg / cm. 2 After pressing at 400° C. for 1 minute, the mixture was crushed and classified using a sieve to obtain a pellet-shaped catalyst with a particle size of 0.5 to 1.0 mm, in which Ru and CaO are supported on Al2O3 [Ru(4.6) / Li2O(8.7) / Al2O3(86.7)].
[0047] Comparative Example 5 A sodium nitrate aqueous solution prepared by dissolving sodium nitrate (NaNO3, FUJIFILM Wako Pure Chemical Industries, Ltd., product number: 195-02545) in ion-exchanged water was used instead of the lithium nitrate aqueous solution, and the solid component after drying was added to the sodium nitrate aqueous solution so that the Na2O content in the resulting catalyst was 4.0 mass% relative to the entire catalyst. In the same manner as in Example 1, a granular catalyst [Ru(3) / Na2O(4) / Al2O3(93)] with a particle size of 1 mm or more, in which Ru and Na2O were supported on Al2O3, was obtained.
[0048] Comparative Example 6 A granular catalyst [Ru(3) / Na2O(5) / Al2O3(92)] with a particle size of 1 mm or more, in which Ru and Na2O were supported on Al2O3, was obtained in the same manner as in Comparative Example 5, except that the dried solid component was added to the sodium nitrate aqueous solution so that the Na2O content in the resulting catalyst was 5.0 mass% based on the total mass of the catalyst.
[0049] Comparative Example 7 A granular catalyst [Ru(3) / Na2O(6) / Al2O3(91)] with a particle size of 1 mm or more, in which Ru and Na2O were supported on Al2O3, was obtained in the same manner as in Comparative Example 5, except that the dried solid component was added to the sodium nitrate aqueous solution so that the Na2O content in the resulting catalyst was 6.0 mass% based on the total mass of the catalyst.
[0050] Comparative Example 8 A granular catalyst [Ru(3) / Na2O(7) / Al2O3(90)] with a particle size of 1 mm or more, in which Ru and Na2O were supported on Al2O3, was obtained in the same manner as in Comparative Example 5, except that the dried solid component was added to the sodium nitrate aqueous solution so that the Na2O content in the resulting catalyst was 7.0 mass% relative to the total mass of the catalyst.
[0051] Comparative Example 9 A granular catalyst [Ru(3) / Na2O(8) / Al2O3(89)] with a particle size of 1 mm or more, in which Ru and Na2O are supported on Al2O3, was obtained in the same manner as in Comparative Example 5, except that the dried solid component was added to the sodium nitrate aqueous solution so that the Na2O content in the resulting catalyst was 8.0 mass% based on the total mass of the catalyst.
[0052] <Catalyst performance evaluation test> The performance evaluation test (CO2 treatment capacity evaluation test) of the obtained catalyst was carried out with the temperature profile shown in Figure 1. 3 A stainless steel (SUS) reaction tube (inner diameter: 8 mm) was filled with the mixture so that the above-mentioned mixture was obtained, and the reaction tube was attached to a temperature programmed desorption analyzer ("TP-5000" manufactured by Hemmi Slide Rule Co., Ltd.). The catalyst was heated to 320°C while flowing He through the catalyst bed at a flow rate of 40 ml / min (pretreatment step), and then, while heating the catalyst at 320°C, H2-containing gas of H2 (20%) + He (balance) was flowed through the catalyst bed at a flow rate of 40 ml / min for 60 minutes to activate the catalyst (activation step).
[0053] Next, while heating the catalyst at the evaluation temperature (T1) shown in Table 1, a CO2-containing gas of CO2 (10%) + He (balance) was fed into the catalyst bed at a flow rate of 40 ml / min for a predetermined cycle time (t i ) was passed through the reactor (CO2 absorption process), and then H2 (40%) + He (balance) H2-containing gas was passed through the reactor at a flow rate of 40 ml / min for a predetermined cycle time (t i) was passed through the catalyst (H2 reduction process), and this series of steps (CO2 absorption process → H2 reduction process) was repeated six times (evaluation process). The gas that had passed through the catalyst during this evaluation process was analyzed by a mass spectrometer.
[0054] The cycle time (t i The evaluation process was carried out four times by changing the time (t i indicates the cycle time in the i-th evaluation step (i = 1 to 4). Note that between each evaluation step, the catalyst was heated to the evaluation temperature (T1) shown in Table 1, while He was passed through the catalyst bed at a flow rate of 40 ml / min.
[0055] For the sixth cycle of each evaluation step (cycle time: t1 to t4), the amount of unreacted CO2 that had passed through the catalyst was determined based on the mass spectrometry results (signal intensity of CO2 (m / e = 44)) of the gas after passing through the catalyst, and the CO2 conversion rate for each cycle time (t1 to t4) was calculated using the following formula. CO2 conversion rate [%] = (CO2 supply amount - unreacted CO2 amount) / CO2 supply amount x 100 The calculated CO2 conversion rate was plotted against the cycle time (t1 to t4). From the graph showing the correlation between the cycle time and the CO2 conversion rate, the cycle time (t(99)) at which the CO2 conversion rate reached 99% was determined. Using this cycle time (t(99)), the amount of CO2 processed by the catalyst within t(99) was calculated according to the following formula. CO2 processing amount (mol-CO2) = time t(99) x CO2 supply amount per unit time The obtained CO2 treatment amount (mol-CO2) was divided by the catalyst volume (2.4 ml) to calculate the CO2 treatment capacity of the catalyst (unit: mol-CO2 / L-cat). The results are shown in Table 1.
[0056] [Table 1]
[0057] Based on the results shown in Table 1, the CO2 treatment capacity of the catalyst when the evaluation temperature (T1) was 250°C and 320°C was plotted against the content of the CO2 storage material. The results are shown in Figure 2. As is clear from these results, the catalysts (Examples 1 to 4) supporting a predetermined amount of Li as an alkali metal had a significantly higher CO2 treatment capacity than the catalyst (Comparative Example 4) supporting Ca instead of Li. In addition, it was found that they had a higher CO2 treatment capacity than the catalysts (Comparative Examples 5 to 9) supporting Na.
[0058] Furthermore, as shown in FIG. 2, in the catalysts supporting Li as an alkali metal, when the Li content becomes smaller or larger than a predetermined amount, it was found that the CO2 treatment capacity significantly decreases (Comparative Examples 1 to 3), and is lower than that of the catalysts supporting Na (Comparative Examples 5 to 9).
[0059] Based on the results shown in Table 1, the CO2 treatment capabilities of the catalysts obtained in Example 3, Comparative Example 4, and Comparative Example 7 were plotted against the evaluation temperature (T1). The results are shown in Figure 3. As is clear from these results, the catalyst supporting a predetermined amount of Li as an alkali metal (Example 3) showed a smaller rate of decrease in CO2 treatment capability due to a decrease in temperature than the catalyst supporting Ca instead of Li (Comparative Example 4) and the catalyst supporting Na (Comparative Example 7), and it was confirmed that excellent CO2 treatment capability was maintained even at low temperatures. [Industrial Applicability]
[0060] As described above, according to the present invention, in a CO2 occlusion reduction catalyst containing lithium (Li) as a CO2 occlusion material, it is possible to realize excellent CO2 processing ability and maintain excellent CO2 processing ability even at low temperatures. Therefore, the CO2 occlusion reduction catalyst of the present invention is useful as a catalyst that can efficiently occlude CO2 and reduce it to CH4 not only during normal operation of a CO2 purification system but also in low temperature conditions such as at the start of operation.
[0061] In addition, the CO2 storage reduction catalyst of the present invention has a large CO2 storage capacity, which makes it possible to reduce the volume of the reactor, thereby reducing costs. In addition, because of its excellent methanation catalytic performance, it is expected to improve the purity of the methane produced.
[0062] Furthermore, because excellent CO2 processing capacity is maintained even at low temperatures, it is possible to lower the operating temperature of the reactor, which is expected to reduce the external energy required to maintain the reactor temperature and make the process more efficient.
Claims
1. A catalyst comprising a porous support made of a metal oxide, ruthenium supported on the porous support, and lithium supported on the porous support, The content of the ruthenium is 1 to 5 mass% based on the total amount of the catalyst, The lithium content is 6 to 9 mass% in terms of lithium oxide based on the entire catalyst. A carbon dioxide storage reduction catalyst.
2. The specific surface area of the porous carrier is 100 to 500 m 2 2. The carbon dioxide storage reduction catalyst according to claim 1, wherein the carbon dioxide storage reduction catalyst has a molecular weight of 1.0 to 1.0 g.
3. 2. The carbon dioxide occlusion reduction catalyst according to claim 1, wherein the porous carrier has a bulk density of 0.5 to 2 g / ml.
4. 2. The carbon dioxide occlusion reduction catalyst according to claim 1, wherein the average particle size of the granules of the porous carrier is 0.1 to 6 mm.
Citation Information
Patent Citations
Carbon dioxide occlusion reduction catalyst and methane production system
JP2020110769A