Stereo molding apparatus, stereo molding method, control device, and recovery device
The three-dimensional modeling apparatus addresses the issue of deteriorating powder quality by controlling the mixing ratio of fresh and recovered powder, ensuring optimal characteristics for improved modeling quality and object integrity.
Patent Information
- Application Number
- JP2023122685
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2023-07-27
- Publication Date
- 2024-10-01
AI Technical Summary
Existing three-dimensional modeling methods using recovered powder face challenges in maintaining modeling quality due to changes in the state of the powder, such as decreased fluidity and altered particle size distribution, which affect the quality of the shaped articles.
A three-dimensional modeling apparatus that includes a powder mixing unit to mix fresh and recovered powder at a controlled ratio based on information about the state of the powder and modeling conditions, using a control unit to adjust the mixing ratio to maintain optimal modeling quality.
The apparatus improves the quality of three-dimensional modeling by ensuring that the mixed powder meets desired characteristics, such as fluidity, packing density, and particle size distribution, thereby enhancing the quality of the final three-dimensional objects.
Smart Images

Figure 2024132789000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a three-dimensional object forming apparatus, a three-dimensional object forming method, a control apparatus, and a recovery apparatus. [Background technology]
[0002] Known methods of 3D modeling using powder lamination (powder additive manufacturing) include the binder jet (BJ) method, in which a binding liquid (modeling liquid) is applied to the modeling area on the surface of the powder layer, and the high-speed sintering (HSS) method, in which a modeling liquid containing a radiant energy absorber is applied.
[0003] In these methods, the powder in the powder layer other than the modeling region may be collected and reused as recovered powder. The modeling quality of the reused recovered powder may be affected by, for example, a drying process in a high-temperature environment after the modeling process.
[0004] For example, Patent Document 1 describes measuring the fluidity of reused material powder (recycled material) and, based on the measurement results, changing the particle size distribution of the unused material powder (virgin material) before reuse, or adding silica particles to the virgin material to suppress a decrease in the fluidity of the recycled material (recovered powder). Summary of the Invention [Problem to be solved by the invention]
[0005] However, Patent Document 1 leaves room for improvement in terms of suppressing deterioration in quality of the molded product caused by the use of recovered powder.
[0006] The present invention aims to improve modeling quality in three-dimensional modeling using recovered powder. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, a three-dimensional modeling apparatus according to one aspect of the present invention includes a modeling unit that models a model containing metal powder, a recovery unit that recovers at least a portion of the powder as recovered powder, a powder mixing unit that generates a mixed powder containing at least the recovered powder, and a control unit that controls the mixing ratio of new powder and the recovered powder based on information regarding the state of at least one or more of the powder, the recovered powder, and the mixed powder. Effect of the Invention
[0008] In three-dimensional modeling using recovered powder, modeling quality can be improved. [Brief description of the drawings]
[0009] [Figure 1] 1 is a block diagram showing a schematic configuration of a three-dimensional object forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of a configuration of a modeling unit according to an embodiment of the present invention. [Diagram 3] 5A to 5C are schematic diagrams illustrating a modeling process in a modeling unit according to an embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram showing a cross section of a modeling tank according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing a cross section of a green body according to one embodiment of the present invention. [Figure 6] FIG. 2 is a diagram showing an example of a schematic configuration of a powder mixing section according to one embodiment of the present invention. [Figure 7] FIG. 13 is a diagram showing a modified example of the powder mixing section according to one embodiment of the present invention. [Figure 8] FIG. 2 is a functional block diagram of a control unit according to an embodiment of the present invention. [Figure 9] FIG. 2 is a diagram illustrating an example of a hardware configuration of a control unit according to an embodiment of the present invention. [Figure 10] 4 is a flowchart of a molding control of a three-dimensional object according to an embodiment of the present invention. [Figure 11] 4 is a flowchart of a mixture ratio adjustment control according to an embodiment of the present invention. [Figure 12] FIG. 1 is a diagram illustrating the influence of molding conditions on the state of a powder according to an embodiment of the present invention. [Figure 13] 1 is an example of a captured image for estimating fluidity according to an embodiment of the present invention. [Figure 14] 1 is an example of a captured image for packing density estimation according to an embodiment of the present invention. [Figure 15] 4 is an example of a captured image for particle size distribution measurement according to an embodiment of the present invention. [Figure 16] FIG. 1 is a diagram showing a dependency relationship between a powder, a powder layer, and a three-dimensional object according to an embodiment of the present invention. [Figure 17] FIG. 13 is a diagram showing a first modified example of a molding portion according to an embodiment of the present invention. [Figure 18] FIG. 13 is a diagram showing a second modified example of the molding portion according to the embodiment of the present invention. [Figure 19] FIG. 11 is a block diagram showing a modified example of the mixture ratio adjustment unit according to the embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment will be described with reference to the drawings. In order to facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals as much as possible, and duplicated description will be omitted.
[0011] In the following description, the layer of powder 50 formed in the modeling unit 3 is called the "powder layer 51". The powder layer 51 may be a flattened layer. The powder 50 includes metal, such as aluminum or an aluminum alloy, but may include other metals. The layer to which the modeling liquid 60 is applied to the powder layer 51 is called the "modeling layer 61". The modeling layer 61 is a layered model in which the powder 50 is bonded by applying the modeling liquid 60. The "powder layer 51" and the "modeling layer 61" each refer to a single layer. Furthermore, an assembly formed by stacking multiple modeling layers 61 and in a state before the modeling is completed is called a "modeled object". On the other hand, an object formed by stacking multiple modeling layers 61 and completing the modeling and sintering is called a "three-dimensional model".
[0012] In addition, the term "mixed powder" used in the following description refers to multiple powders mixed by the powder mixing unit 2. The mixed powder includes new powder (hereinafter referred to as "new powder") and recovered powder (hereinafter referred to as "recovered powder"). New powder is powder that has not been used for modeling in the modeling unit 3. Recovered powder is powder that has been used for modeling in the modeling unit 3. Recovered powder may be powder recovered from the modeling unit 3, powder recovered from the powder removal unit 5, or a combination of these. The "mixing ratio" refers to the ratio of new powder to recovered powder contained in the mixed powder. Any type of ratio, such as a volume ratio or a weight ratio, can be applied as the "mixing ratio."
[0013] <Basic configuration of 3D modeling device> A basic configuration of a three-dimensional object forming apparatus 1 according to an embodiment will be described with reference to FIGS.
[0014] 1 is a block diagram showing a schematic configuration of a three-dimensional modeling apparatus 1 according to an embodiment of the present invention. As the three-dimensional modeling apparatus 1 according to an embodiment of the present invention, a binder jet (BJ) method is described below, which applies a binder (modeling liquid 60) to a modeling region on the surface of a powder layer 51. In the BJ method, a three-dimensional object of any shape can be modeled by selectively applying the modeling liquid 60 to the powder layer 51, solidifying it, and sintering it. The modeling liquid 60 contains, for example, a resin such as a binder and an ink such as a solvent.
[0015] The three-dimensional modeling apparatus 1 includes a powder mixing unit 2, a modeling unit 3, a drying unit 4, a powder removing unit 5, a sintering unit 6, a collecting unit 7, and a control unit 8.
[0016] The powder mixing unit 2 mixes the powder 50. In this way, mixed powder is generated as the powder 50 to be supplied to the modeling unit 3. The powder mixing unit 2 mixes new powder (new powder) that has not yet been used for modeling with powder (recovered powder) that has already been used for modeling and collected by the collection unit 7. Furthermore, the powder mixing unit 2 can mix the mixed powder at a desired mixing ratio based on a control command from the control unit 8 and supply it to the modeling unit 3.
[0017] The modeling unit 3 models a model containing powder 50. The powder 50 contains at least mixed powder supplied from the powder mixing unit 2. In this embodiment, the modeling unit 3 performs modeling by the BJ method. Note that a portion of the powder 50 used in the modeling unit 3 is collected in the collection unit 7 as collected powder.
[0018] The drying unit 4 dries the object modeled by the modeling unit 3. Specifically, the drying unit 4 dries the solvent and the like contained in the modeling liquid 60 contained in the object. In the drying unit 4, the modeling tank 12 containing the object modeled by the modeling unit 3 is heated and decompressed to dry it. As a result, the powder 50 is fixed by the binder contained in the modeling liquid 60.
[0019] The powder removal unit 5 removes excess powder 50 from the model dried by the drying unit 4. For example, any method such as blowing air onto the model may be used. The powder removal unit 5 removes the powder 50 that has not been applied with the modeling liquid 60 from the modeling tank 12 and has not adhered thereto. As a result, the powder removal unit 5 obtains a three-dimensional object that is adhered with the binder, i.e., a green body (G body) 62. The powder 50 removed by the powder removal unit 5 is collected in the collection unit 7 as collected powder.
[0020] The sintering section 6 generates a final three-dimensional object (S body) by sintering the green body 62. The sintering section 6 removes binder from the green body 62 (degreasing) and sinters it in, for example, a sintering furnace.
[0021] The recovery unit 7 recovers at least a portion of the powder 50 in the modeling unit 3 as recovered powder. The recovery unit 7 also recovers the powder 50 from the powder removing unit 5. The recovery unit 7 supplies the recovered powder to the powder mixing unit 2.
[0022] The control unit 8 controls the operation of each unit of the three-dimensional modeling apparatus 1. In particular, in this embodiment, the control unit 8 performs a mixing ratio adjustment control to control the mixing ratio of the powder mixed in the powder mixing unit 2 based on at least one of information on the state of the powder 50 and information on the modeling conditions of the modeling unit 3. The control unit 8 outputs a command value (mixing ratio command) including information on the mixing ratio to the powder mixing unit 2. The information on the state of the powder 50 is, for example, information on the state of at least one of new powder, recovered powder, and mixed powder. In addition, the information on the state of the powder 50 may include one or more of the powder fluidity, packing density, particle size distribution, and driving force of the motor, or may be a combination of these. The modeling conditions may include one or more of the volume of the modeled object, the scanning speed of the flat part, the rotation speed of the flat part, and the layer thickness of the powder layer, or may be a combination of these. In addition, these pieces of information may be determined from an image, or may be measured by an existing measuring device.
[0023] An example of the operation of the BJ type modeling unit 3 will be described with reference to Fig. 2. Fig. 2 is a diagram showing an example of the configuration of the modeling unit 3 according to an embodiment of the present invention.
[0024] In the following description, the X, Y, and Z directions are perpendicular to each other. The X and Y directions are horizontal, and the Z direction is vertical. The X direction is the axial direction of the rotation axis of the flat section 31. The Y direction is the movement direction of the flat section 31, and is the arrangement direction of the supply tank 11, the modeling tank 12, and the surplus powder tank 15 in the powder tank 10. The Z direction is the ascending and descending direction of the supply stage 13 and the modeling stage 14. In the following description, for convenience of explanation, the positive Z direction may be referred to as the upper side, and the negative Z direction may be referred to as the lower side.
[0025] As shown in FIG. 2, the modeling section 3 includes a powder tank 10, a lamination unit 30, and an application section 40.
[0026] The powder tank 10 forms a powder layer 51 containing powder 50. The application unit 40 applies a modeling liquid 60 to the powder layer 51 to form a modeling layer 61. In the modeling unit 3, a plurality of modeling layers 61 are stacked to form a model.
[0027] The powder tank 10 includes a supply tank 11, a modeling tank 12, a supply stage 13, a modeling stage 14, and a surplus powder tank 15. The powder tank 10 has a box-like shape. The tops of the supply tank 11, the modeling tank 12, and the surplus powder tank 15 are open.
[0028] The supply tank 11 of the powder tank 10 is a tank that supplies the powder 50 to the modeling tank 12. The supply tank 11 holds the powder 50 to be supplied to the modeling tank 12. A supply stage 13 is provided at the bottom of the supply tank 11. The supply stage 13 moves up and down in the vertical direction (Z direction). The side of the supply stage 13 is disposed so as to contact the inner side of the supply tank 11.
[0029] The powder 50 required for modeling is supplied from the supply tank 11 to the modeling tank 12 of the powder tank 10. A powder layer 51 and a modeling layer 61 are formed in the modeling tank 12. Furthermore, a plurality of modeling layers 61 are stacked in the modeling tank 12 to form a model.
[0030] A supply stage 13 and a modeling stage 14 are provided at the bottom of the supply tank 11 and the modeling tank 12, respectively, and move up and down in the vertical direction (Z direction). The side of the modeling stage 14 is disposed so as to contact the inner side of the modeling tank 12. The upper surfaces of the supply stage 13 and the modeling stage 14 are kept horizontal.
[0031] The surplus powder tank 15 of the powder tank 10 is a tank that holds surplus powder 50 among the powder 50 flattened by the flat portion 31 when forming the powder layer 51. A means for sucking the powder 50 may be provided at the bottom of the surplus powder tank 15, or a means for removing the surplus powder tank 15 may be provided. The surplus powder tank 15 is disposed next to the modeling tank 12. The surplus powder 50 held in the surplus powder tank 15 is collected by the collection unit 7 using any of the above-mentioned methods, and is resupplied from the collection unit 7 to the powder mixing unit 2 as collected powder.
[0032] The powder 50 held in the supply tank 11 is appropriately replenished by the mixed powder supplied by the powder mixing unit 2 at any timing, such as before modeling in the modeling unit 3 starts or when the amount of powder 50 in the supply tank 11 decreases. Note that, although the powder tank 10 has been exemplified as having two tanks, the supply tank 11 and the modeling tank 12, the supply tank 11 may not be provided and the powder 50 may be directly supplied from the powder mixing unit 2 to the modeling tank 12.
[0033] Methods for transporting the powder 50 from the powder mixing section 2 to the supply tank 11 include a screw conveyor method using a screw, a pneumatic transport method using air, and the like.
[0034] In the example of FIG. 2, the powder tank 10 is configured such that the inner space of a single box is divided into three spaces along the Y direction to form the supply tank 11, the modeling tank 12, and the surplus powder tank 15. However, the configuration of the powder tank 10 is not limited to the example of FIG. 2. For example, the supply tank 11, the modeling tank 12, and the surplus powder tank 15 may be formed by separate boxes. In this configuration, it is preferable to install the supply tank 11 and the modeling tank 12 so that the surfaces facing the Y direction of the supply tank 11 and the modeling tank 12 are in close contact with the surfaces facing the Y direction of the modeling tank 12 and the surplus powder tank 15. This makes it possible to prevent the powder 50 from leaking to the outside when the powder 50 is moved between the tanks, and to make the movement of the powder 50 more reliable. In addition, as described with reference to FIG. 1, the modeling tank 12 containing the modeled object modeled in the modeling unit 3 can be easily transported to the drying unit 4 or the powder removing unit 5.
[0035] The lamination unit 30 also has a flat portion 31 and a powder removal portion 32 .
[0036] The flat part 31 of the lamination unit 30 flattens the modeling layer 61 and the powder layer 51. The flat part 31 flattens the modeling layer 61 and the powder layer 51 by scanning the recoater as a rotating body while rotating along the surface of the powder 50. The flat part 31 rotates and drives the powder 50 on the supply stage 13 of the supply tank 11 to the modeling tank 12, forming the powder layer 51. The flat part 31 moves back and forth in the Y direction along the stage surface (the surface on which the powder 50 is loaded) of the modeling stage 14. More specifically, the flat part 31 moves horizontally from the outside of the supply tank 11 to pass above the supply tank 11 and the modeling tank 12. As a result, the powder 50 is transferred and supplied onto the modeling tank 12, and the flat part 31 passes over the modeling tank 12 to flatten the powder 50, forming the powder layer 51. The flat part 31 is a member longer than the inner dimensions of the modeling tank 12 and the supply tank 11. The flat portion 31 may be a blade or a bar as a plate-like member.
[0037] Powder removing section 32 of lamination unit 30 removes powder adhering to flat section 31. Powder removing section 32 moves together with flat section 31 while being in contact with the peripheral surface of flat section 31.
[0038] The application unit 40 includes a carriage 41 and a head 42 .
[0039] The head 42 applies the modeling liquid 60 to the powder layer 51. The head 42 is, for example, an inkjet head, and is provided with a nozzle row in which a plurality of nozzles are arranged. A colored model may be formed by applying a cyan modeling liquid, a magenta modeling liquid, a yellow modeling liquid, and a black modeling liquid, or a modeling liquid of one color may be applied from a plurality of nozzles. The modeling liquid 60 may be applied by an inkjet method or a dispenser method.
[0040] At least one head 42 is mounted on a carriage 41, and moves back and forth in the X (main scanning), Y (sub-scanning), and Z directions by a motor, a guide member, and the like.
[0041] In particular, in this embodiment, the modeling unit 3 includes a photographing unit 16. The photographing unit 16 photographs the surface of the powder. The photographing unit 16 is installed, for example, above the modeling tank 12 so that the entire surface of the upper opening of the modeling tank 12 is included in the angle of view. The photographing unit 16 is not particularly limited to a specific position inside the modeling unit 3 as long as it is a position where the surface of the powder 50 can be photographed. The photographing unit 16 may also be installed outside the modeling unit 3 to photograph the state of the powder 50. The operation of the photographing unit 16 is controlled by the control unit 8, and the photographing unit 16 photographs the surface of the powder 50 on the modeling tank 12 when various tests are performed, and outputs image information, which is the photographed image, to the control unit 8. The photographing unit 16 uses, for example, a digital camera, a video camera, a CCD (Charge Coupled Device), a CMOS camera (Complementary Metal Oxide Semiconductor Camera), or the like. The photographing unit 16 may be a stereo camera that photographs the measurement object in overlapping photographing areas from different photographing positions. The number of imaging units is not limited, and may be more than one. The imaging unit 16 may function as a three-dimensional measuring device and measure a point cloud on the surface of the powder 50 from captured image information.
[0042] 3 is a schematic diagram illustrating a modeling process in the modeling unit 3 according to one embodiment of the present invention. The operation of the modeling unit 3 will be described with reference to FIG.
[0043] The modeling unit 3 starts modeling in a state where the supply tank 11 is filled with powder 50. The bottom surface (supply stage 13) of the supply tank 11 is raised, and the bottom surface (modeling stage 14) of the modeling tank 12 is lowered. The powder 50 overflows onto the supply tank 11 by the amount of rise of the bottom surface of the supply tank 11. The flat part 31 is rotated and scanned from above the supply tank 11 onto the modeling tank 12. As a result, the overflowing powder 50 on the supply tank 11 is transported to the modeling tank 12 and moves into the modeling tank 12. The powder 50 is laid in the modeling tank 12 by the amount of descent of the bottom surface of the modeling tank 12, and any powder beyond that overflows. Next, the flat part 31 is scanned from the modeling tank 12 to the surplus powder tank 15. As a result, the powder 50 overflowing from the modeling tank 12 is put into the surplus powder tank 15. The powder 50 in the surplus powder tank 15 is collected by the collection unit 7.
[0044] After that, as shown in FIG. 3, the inkjet head 42 of the application unit 40 is scanned over the modeling tank 12. As a result, the modeling liquid 60 is applied to the uppermost powder layer 51 of the powder 50 in the modeling tank 12 in an arbitrary image pattern. As a result, a modeling layer 61 is formed in the powder layer 51, in which the modeling liquid 60 has permeated into the powder 50. The above is the operation for one layer, and this is repeated many times to stack the layers. Finally, the modeling tank 12 is filled with the powder 50, and there are areas inside where the modeling liquid 60 has been selectively applied (multiple stacked modeling layers 61).
[0045] Fig. 4 is a schematic diagram showing a cross section of a modeling tank 12 according to an embodiment of the present invention. Fig. 5 is a schematic diagram showing a cross section of a green body 62 according to an embodiment of the present invention. The steps from the drying section 4 to the powder removing section 5 will be described with reference to Figs. 4 and 5.
[0046] Figure 4 shows a cross section of the modeling tank 12 after modeling in the modeling unit 3. The inside of the modeling tank 12 is filled with powder 50, and there are areas where the modeling liquid 60 has been applied (modeling layer 61) and areas where the modeling liquid 60 has not been applied. Immediately after the modeling liquid 60 is applied, the modeling liquid 60 has simply permeated between the particles of the powder 50 and has not yet solidified. Therefore, the modeling tank 12 is placed in the drying unit 4 and dried. The liquid components of the modeling liquid 60 evaporate, leaving only the binder components contained in the modeling liquid 60 behind, and the particles of the powder 50 are in a state of being solidified together.
[0047] In the powder removal unit 5, the powder 50 in the areas where the modeling liquid 60 was not applied and did not solidify is removed from the modeling layer 61. The powder 50 removed in the powder removal unit 5 is collected by the collection unit 7. Figure 5 shows a cross section of the modeled object (green body 62) remaining after the powder 50 around the modeling layer 61 has been removed and collected from the modeling tank 12.
[0048] The powder mixing section 2 will be described with reference to Fig. 6. Fig. 6 is a diagram showing an example of a schematic configuration of the powder mixing section 2 according to one embodiment of the present invention.
[0049] As shown in FIG. 6, the powder mixing section 2 has an agitation tank 21, a motor 22, a screw 23, tanks 24 and 25, a recovered powder tank 25, cocks 26, 27, and 28, and a mixed powder outlet 29.
[0050] The stirring tank 21 is a tank that holds and stirs the powder 50. The motor 22 drives the screw 23. The screw 23 is installed in the stirring tank 21, and is rotated at a predetermined rotation speed by driving the motor 22.
[0051] Therefore, the stirring tank 21 rotates the screw 23 by the motor 22 to stir and mix the powder uniformly. Depending on the amount of mixed powder held in the stirring tank 21 and the mixing ratio of the new powder and the mixed powder, the command value of the rotation speed of the screw 23 from the control unit 8 and the driving force of the motor 22 required for the rotation speed may differ. Therefore, for example, information on the power consumption of the motor 22 required to rotate the screw 23 at a predetermined rotation speed is transmitted to the control unit 8. Then, the control unit 8 estimates the driving force of the motor 22 based on the information on the power consumption. The control unit 8 determines information on the state of the powder based on the estimated driving force of the motor 22.
[0052] New powder is held in the new powder tank 24. Recovered powder is held in the recovered powder tank 25. The new powder tank 24 and the recovered powder tank 25 are connected to the stirring tank 21 via cocks 26 and 27, respectively. This allows powder to be supplied to the stirring tank 21 from each of the tanks 24 and 25.
[0053] Each of the cocks 26, 27 opens and closes in response to a command from the control unit 8. This allows the powder mixing unit 2 to adjust the mixing ratio of the mixed powder.
[0054] Furthermore, the new powder tank 24 and the recovered powder tank 25 have a weight measurement function. For example, the weight of the powder charged into the stirring tank 21, the weight ratio of new powder to recovered powder, etc. are measured from the difference in weight before and after the powder is supplied to the stirring tank 21. Note that the method of measuring the amount of new powder and recovered powder charged into the stirring tank 21 may be based on information other than weight, such as volume.
[0055] The mixed powder can be taken out from the mixed powder outlet 29 via a cock 28 at the bottom of the stirring tank 21. By opening and closing the cock 28 according to a command from the control unit 8, the amount of mixed powder supplied from the powder mixing unit 2 to the modeling unit 3 can be adjusted.
[0056] Here, we will add some details about the issues involved in reusing the recovered powder. The state of the powder 50 changes when it is used in modeling. For example, the powder 50 recovered from the modeling tank 12 of the modeling unit 3 may have even a small amount of modeling liquid 60 attached thereto, or may be oxidized by exposure to air during modeling, causing the state of the powder 50 to change. In addition, the powder 50 exposed to high temperatures in the drying unit 4 has its particle surfaces modified, causing the state of the powder 50 to change. Due to these changes, the recovered powder recovered from the modeling unit 3 or the powder removal unit 5 is in a different state from new powder. Therefore, even if the recovered powder is reused, it is necessary to improve the modeling quality.
[0057] Therefore, it becomes effective for the control unit 8 to control the mixing ratio of new powder and recovered powder based on at least one of information regarding the molding conditions of the molding unit 3 and information regarding the state of the powder 50 so that the mixed powder supplied to the molding unit 3 has the desired characteristics.
[0058] Fig. 7 is a diagram showing a modified example of the powder mixing section 2 according to one embodiment of the present invention. As shown in Fig. 7, the powder mixing section 2 may be configured to mix a plurality of types of virgin powder together with recovered powder to generate mixed powder.
[0059] The powder mixing section 2 in Fig. 7 has a first new powder tank 24A and a second new powder tank 24B in which two types of new powder are respectively stored, in addition to the recovered powder tank 25 in Fig. 6. The first new powder tank 24A and the second new powder tank 24B are connected to the stirring tank 21 via cocks 26A and 26B, respectively. The opening and closing of the respective cocks 26A, 26B, 27 is adjusted according to a command from the control section 8. This allows three types of powder, including the two types of new powder and the recovered powder, to be supplied to the stirring tank 21 at a desired mixing ratio and mixed.
[0060] Here, the two types of new powder are two types of powder with different characteristics. For example, two types of powder, one with a pre-treatment and one without, two types of powder with different particle sizes, or a combination of these may be used. Note that, although the example in FIG. 7 illustrates a configuration in which the number of new powders is increased to two, a configuration in which three or more types of new powders are mixed with the recovered powder may also be used.
[0061] In this way, the powder mixing unit 2 mixes two or more types of new powder unused in the modeling unit 3 with the recovered powder. The control unit 8 controls the mixing ratio of each of the two or more types of new powder to the recovered powder. This improves modeling quality. For example, when powders of different particle sizes are mixed, it is easier to increase the density than when new powder of one type of powder size is used. This is because smaller particles can enter the gaps between larger particles. If the density can be increased, there is a higher possibility of creating a high-strength model.
[0062] The following describes the problems that arise when modeling using new powder A and new powder B as two or more types of new powder with different properties. When modeling for the first time using the three-dimensional modeling apparatus 1 of this embodiment, there is no recovered powder, and only new powder A and B (new powder AB) are mixed and used for modeling. For example, new powder A and new powder B are mixed in equal weights. However, the recovered powder is not necessarily new powder A and new powder B in equal weight. Since powder is scattered during modeling and is difficult to recover completely, it is possible that the recovery rates of new powder A and new powder B are different. For this reason, the recovered powder may have different properties from new powder AB. Therefore, the properties of the recovered powder will change from those of new powder AB, and even if the recovered powder is reused, it is still a problem to improve the modeling quality.
[0063] Therefore, it becomes effective to determine the mixing ratio between each of the multiple new powders and the recovered powder based on at least one of information regarding the molding conditions of the molding section 3 and information regarding the state of the powder 50 so that the mixed powder supplied to the molding section 3 has the desired characteristics.
[0064] <Mixing ratio adjustment control> Next, the mixture ratio adjustment control according to this embodiment will be described with reference to FIGS.
[0065] 8 is a functional block diagram of a control unit 8 according to an embodiment of the present invention. The control unit 8 has a modeling control unit 81, a modeling condition recording unit 82, a state estimating unit 83, and a mixing ratio adjusting unit 84.
[0066] The modeling control unit 81 controls the operation of the modeling unit 3. When modeling data on a three-dimensional object to be modeled is input from, for example, a modeling data creation device 104 outside the three-dimensional modeling apparatus 1, the modeling control unit 81 plans a modeling operation of the modeling unit 3 based on the modeling data. Then, the modeling control unit 81 outputs a modeling command based on the plan to the modeling unit 3 and operates the modeling unit 3 based on the modeling command, thereby causing the modeling unit 3 to perform a desired modeling operation. The modeling control unit 81 also outputs information on modeling conditions of the modeling unit 3, which is included in the modeling command, to the modeling condition recording unit 82.
[0067] The modeling condition recording unit 82 records information about the modeling conditions. Specifically, the modeling condition recording unit 82 records and stores information about the modeling conditions of the modeling unit 3 input from the modeling control unit 81. Here, the modeling conditions include information such as the volume of the modeled object, the scanning speed of the flat portion 31, the rotation speed of the flat portion 31, and the layer thickness of the powder layer 51.
[0068] The state estimation unit 83 estimates information related to the state of the powder 50. For example, an image of the powder 50 captured by the imaging unit 16 is input to the state estimation unit 83, and the state estimation unit 83 estimates information related to the state of the powder 50 based on the image. It is also possible to estimate information related to the state of the powder 50 based on measured values using an existing device without using an image. The state estimation unit 83 also receives the power consumption of the motor 22 of the powder mixing unit 2, and can estimate information related to the state of the powder 50 based on the power consumption. The state estimation unit 83 outputs information related to the state of the powder 50 (referred to as "powder state" in FIG. 8) to the mixing ratio adjustment unit 84.
[0069] The mixing ratio adjusting unit 84 adjusts the mixing ratio of the new powder and the mixed powder based on at least one of the information on the modeling conditions recorded in the modeling condition recording unit 82 and the information on the state of the powder 50 input from the state estimating unit 83. The mixing ratio adjusting unit 84 outputs a mixing ratio command to the powder mixing unit 2 to generate mixed powder at the adjusted mixing ratio.
[0070] FIG. 9 is a diagram showing an example of a hardware configuration of the control unit 8 according to an embodiment of the present invention.
[0071] As shown in FIG. 9, the control unit 8 of the 3D printing apparatus 1 includes a CPU 101 (Central Processing Unit), a ROM 102 (Read Only Memory) that stores programs for executing control and other fixed data, and a RAM 103 (Random Access Memory) that temporarily stores printing data and the like. The control unit 8 receives printing data from a printing data creation device 104 such as an external computer. The printing data creation device 104 creates printing data by slicing a final model into printing layers 61. The control unit 8 controls the printing operation for each printing layer 61. The printing data creation device 104 may be separate from the 3D printing apparatus 1 or may be integrated with it. The control unit 8 may be located inside the 3D printing apparatus 1 or outside it.
[0072] 10 is a flowchart of a process for controlling the formation of a three-dimensional object according to an embodiment of the present invention. The flowchart shown in FIG.
[0073] In step S1, an operation mode is selected by a user of the 3D modeling apparatus 1. The user performs an input operation to select a desired operation mode, for example, via an input device installed inside the 3D modeling apparatus 1 or connected to an external device for communication. Information on the selected operation mode is input to the mixture ratio adjustment unit 84 of the control unit 8.
[0074] Here, the user can select, for example, one of the following operation modes: shape accuracy priority mode, powder cost priority mode, or modeling speed priority mode. Depending on the selected operation mode, the mixing ratio of new powder and recovered powder after adjustment can be changed even under the same conditions. By implementing such mode selection, it is possible to perform optimal modeling according to the user. In modeling, there is a trade-off between shape accuracy, powder cost, and modeling speed. It is effective to be able to select which operation mode to prioritize according to the user.
[0075] In the "shape accuracy priority mode," the ratio of new powder in the mixed powder is increased. Generally, reuse of powder leads to deterioration, which leads to a decrease in modeling quality.
[0076] In the "Powder Cost Priority Mode", the proportion of recovered powder in the mixed powder is increased. Reuse reduces costs. Since powder deteriorates when reused, increasing the proportion of recovered powder may result in a decrease in modeling quality. However, the modeling quality can be kept constant by adjusting the speed of the flat section 31, for example.
[0077] In the "modeling speed priority mode", the ratio of new powder or recovered powder in the mixed powder is increased so that the fluidity of the powder 50 is increased when the flat portion 31 operates. This makes it possible to increase the speed of the flat portion 31.
[0078] In step S2, the mixing ratio adjustment unit 84 sets the mixing ratio of the new powder and the recovered powder based on at least one of information on the state of the powder 50 and information on the modeling conditions of the modeling unit 3 (mixing ratio adjustment step). The mixing ratio adjustment unit 84 can adjust and set the mixing ratio to suit the operation mode selected in step S1 by performing each process of the flowchart of the mixing ratio adjustment control. In the mixing ratio adjustment control, a subroutine process shown in FIG. 11 is executed. Details of the mixing ratio adjustment control will be described later with reference to FIG. 11. Alternatively, the operation mode may not be selected in step S1, and the mixing ratio may be set according to FIG. 11. The mixing ratio adjustment unit 84 outputs a mixing ratio command including information on the set mixing ratio to the powder mixing unit 2.
[0079] In step S3, the new powder and the collected powder are mixed by the powder mixing unit 2 based on the mixing ratio set in step S2 (powder mixing step). The mixed powder mixed in the powder mixing unit 2 is supplied to the modeling unit 3.
[0080] In step S4, the modeling unit 3 models a model using the mixed powder mixed in step S3 (modeling step). Here, the modeling control unit 81 controls the operation of the modeling unit 3. The modeling tank 12 in which the modeling object is accommodated is transported from the modeling unit 3 to the drying unit 4. In addition, surplus powder that has overflowed from the modeling tank 12 in the modeling unit 3 is collected by the collection unit 7 and supplied to the powder mixing unit 2 (collection step).
[0081] In step S4, the modeling control unit 81 outputs information about the modeling conditions of the modeling unit 3 used in the modeling process to the modeling condition recording unit 82, and records the information in the modeling condition recording unit 82. The modeling conditions recorded in the modeling condition recording unit 82 include information such as the volume of the modeled object, the scanning speed of the flat portion 31, the rotation speed of the flat portion 31, and the layer thickness of the powder layer 51.
[0082] In step S5, the model formed in step S4 is dried by the drying unit 4. The drying unit 4 dries the model at a drying temperature and for a drying time according to a control command from the control unit 8. The modeling tank 12 in which the model after drying is accommodated is transported from the drying unit 4 to the powder removing unit 5.
[0083] In step S6, the powder removing unit 5 removes excess powder from the molded object dried in step S4. The excess powder is collected by the collecting unit 7 (collection step). The molded object from which the excess powder has been removed is transported from the powder removing unit 5 to the sintering unit 6. In addition, the excess powder is collected by the collecting unit 7 and supplied to the powder mixing unit 2.
[0084] In step S7, the shaped object from which the excess powder has been removed in step S6 is sintered by the sintering unit 6. When the process of step S7 is completed, the main flow ends.
[0085] 11 is a flowchart of the mixing ratio adjustment control according to one embodiment of the present invention. Each process (mixing ratio adjustment step) of the mixing ratio adjustment control shown in FIG. 11 is executed as a subroutine process in step S2 of FIG.
[0086] In step S11, the mixture ratio adjustment unit 84 sets a target value and an allowable range based on the operation mode selected in step S1. The allowable range is, for example, a range in which deviation from a target value can be tolerated for the estimated value of the powder 50 estimated in steps S12 to S14 described below. For example, when the "shape accuracy priority mode" is selected, the target value of the packing density of the powder layer 51 is increased so as to improve the shape accuracy of the three-dimensional object. As a result, the ratio of new powder in the mixed powder is set to be relatively increased. Also, when the "powder cost priority mode" is selected, the allowable range of the fluidity of the powder 50 and the fluidity and packing density of the powder layer 51 are increased. As a result, the ratio of recovered powder in the mixed powder is set to be relatively increased. Also, when the "modeling speed priority mode" is selected, the allowable range of the packing density of the powder layer 51 is set to be large according to the current fluidity of the mixed powder. As a result, the lower limit of the ratio of new powder or recovered powder in the mixed powder becomes larger than the reference value. As a result, the fluidity of the mixed powder becomes relatively high.
[0087] Then, the control unit 8 controls the mixing ratio so as to change the mixing ratio of the powder 50 according to the operation mode selected in step S1. By configuring the target value and the allowable range to be changed according to the selected operation mode, an optimal modeling can be performed according to the user. Furthermore, the optimal mixing ratio can be adjusted under the constraints imposed by the selected operation mode.
[0088] In step S12, the state estimation unit 83 estimates information about the state of the powder 50 based on the power consumption of the motor of the powder mixing unit 2. For example, the fluidity of the mixed powder or the recovered powder is estimated as information about the state of the powder 50, and the mixing ratio is determined. The fluidity of the mixed powder or the recovered powder estimated by the state estimation unit 83 is estimated from the power consumption of the motor 22. The power consumption of the motor 22 also includes information such as the control value of the motor 22 (PWM ratio for controlling ON / OFF) and the current consumption of the motor 22.
[0089] An example of the method for estimating the fluidity in step S12 is as follows. The amounts of new powder and recovered powder fed into the stirring tank 21 and the rotation speed of the motor 22 are kept constant, and the power consumption of the motor 22 is measured. Alternatively, the amount of mixed powder fed into the stirring tank 21 is changed, and the amount of change in the power consumption of the motor 22 is measured. Next, it is determined whether the power consumption is below a predetermined value. Since the power consumption of the motor 22 and the fluidity of the powder 50 are proportional, the fluidity can be estimated from the power consumption of the motor 22. When the amount of change in the power consumption of the motor 22 is measured, it is determined whether all power consumption is below a predetermined value.
[0090] When the power consumption of motor 22 is equal to or less than a predetermined value, it is determined that the fluidity of powder 50 is high. On the other hand, when the power consumption of motor 22 is greater than the predetermined value, it is determined that the fluidity is low. With this method, it is possible to select a relatively large estimated value when the fluidity is determined to be high, and to select a relatively small estimated value when the fluidity is determined to be low.
[0091] In this way, the fluidity of the mixed powder and the recovered powder is estimated based on the driving force of the motor 22, such as the motor power consumption of the powder mixing unit 2. For example, by adjusting the mixing ratio of new powder and recovered powder so that the motor power consumption is constant, powder 50 within the range of fluidity required to improve the molding quality can be used for molding. In addition, since the motor power consumption can be easily obtained, information on the state of the powder 50 can be easily estimated.
[0092] If the deviation between the estimated value of the fluidity of the mixed powder or the recovered powder estimated in step S12 and the target value of the fluidity set in step S11 is within the allowable range set in step S11, the process proceeds to step S13. On the other hand, if the deviation exceeds the allowable range, the process proceeds to step S15, where the mixing ratio of the powder 50 is adjusted by the mixing ratio adjustment unit 84. Note that the estimation of the driving force of the motor 22 in S12 may be omitted and the process proceeds to S13.
[0093] In step S15, if the estimated value of fluidity is higher than the allowable range with respect to the target value, the mixing ratio of new powder is reduced. Thus, the mixing ratio is controlled so that the fluidity of the powder 50 decreases from the current fluidity. On the other hand, if the estimated value of fluidity is lower than the allowable range with respect to the target value, the mixing ratio of new powder is increased. Thus, the mixing ratio is controlled so that the fluidity of the powder 50 increases from the current fluidity.
[0094] In step S15, if multiple virgin powders are mixed, the mixing ratio of the multiple virgin powders may be changed. For example, to increase the fluidity, the ratio of virgin powder with a relatively high fluidity may be increased. To decrease the fluidity, the ratio of virgin powder with a relatively low fluidity may be increased. When the process of step S15 is completed, the process returns to the main flow of FIG. 10.
[0095] In step S13, the mixing ratio adjusting unit 84 estimates the characteristics of the powder 50 used in the modeling process based on the information on the modeling conditions of the modeling unit 3. The mixing ratio adjusting unit 84 obtains information on the modeling conditions in the most recent modeling process from, for example, the modeling condition recording unit 82, and estimates information on the state of the powder 50. For example, the particle size distribution of the powder 50 is estimated.
[0096] If the deviation between the estimated value of the particle size distribution of the powder 50 estimated in step S13 and the target value of the flow distribution set in step S11 is within the allowable range set in step S11, the process proceeds to step S14. On the other hand, if the deviation exceeds the allowable range, the process proceeds to step S16, where the mixing ratio of the powder 50 is adjusted by the mixing ratio adjustment unit 84. Note that the estimation of information related to the modeling conditions of the modeling unit 3 in S13 may be omitted, and the process may proceed to S14 or S16.
[0097] In step S16, the mixing ratio of the new powder and the recovered powder is controlled to bring the particle size distribution of the current powder 50 into a desired range. In addition, in step S16, in the case where a configuration is adopted in which a plurality of new powders are mixed, the mixing ratio of the plurality of new powders may be changed to control the mixing ratio so that the particle size distribution of the current powder 50 comes into a desired range. When the process of step S16 is completed, the process returns to the main flow of FIG.
[0098] In step S14, the state estimation unit 83 performs a test to estimate the state of the mixed powder used in the modeling unit 3. There are three types of tests: a "fluidity test (S14a)", a "packing density test (S14b)", and a "particle size distribution test (S14c)". In each test, the photographing unit 16 first photographs the surface of the powder 50. Next, the state estimation unit 83 estimates information regarding the state of the powder 50 based on the photographed image. For example, the fluidity, packing density, particle size distribution, etc. of the mixed powder are estimated as information regarding the state of the powder 50.
[0099] Here, an overview of each of the tests S14a to S14c performed in step S14 will be described with reference to FIGS.
[0100] <Liquidity test (S14a)> The molding quality is affected if the fluidity of the powder 50 is too poor or too good compared to the reference value. If the fluidity of the powder 50 is too poor, the powder 50 will not be uniform on the flat portion 31. In this case, voids may be formed in the powder layer 51, or cracks may occur in the powder layer 51 due to the shear force caused by the movement of the flat portion 31. On the other hand, if the fluidity of the powder 50 is too good, the powder 50 in the lower layer may flow together with the powder 50 each time the powder layer 51 is layered, thereby reducing the molding quality. For this reason, in the fluidity test in step S14a, the fluidity of the powder 50 is estimated from the image captured by the photographing unit 16, and the mixing ratio of the new powder and the recovered powder is determined so that the powder 50 falls within a predetermined range.
[0101] An outline of the fluidity test in step S14a will be described with reference to FIG. 13. FIG. 13 is an example of a captured image for estimating fluidity according to an embodiment of the present invention. In the fluidity test, for example, after changing one or more of the scanning speed or rotation speed of the flat portion 31, the photographing unit 16 photographs the surface of the powder 50. The fluidity of the powder 50 is estimated from the photographed image. This makes the unevenness P on the surface of the powder 50 occur more reliably and more conspicuously, making it easier to determine the occurrence of the unevenness P from the photographed image. In addition, since it is possible to determine at what level the scanning speed or rotation speed of the flat portion 31 causes the unevenness P, the fluidity of the powder 50 can be estimated. FIG. 13(A) is an example of an image of the surface of a normal powder 50. In FIG. 13(A), the surface of the powder 50 is uniform over the entire surface.
[0102] On the other hand, Fig. 13(B) is an example of an image capturing the surface of abnormal powder 50. Fig. 13(B) shows a state in which the fluidity of powder 50 is worse than that of Fig. 13(A). In Fig. 13(B), unevenness P occurs on the surface of powder 50.
[0103] In another method of fluidity testing, for example, the flat portion 31 is stopped midway through its operation, before the flat portion 31 reaches from one end to the other end in the scanning direction. This causes the powder 50 in the powder layer 51 that is in contact with the flat portion 31 to scatter in the scanning direction, and the fluidity of the powder 50 can be estimated from an image taken of the surface of the powder 50 in a scattered state.
[0104] It is considered that the better the fluidity of the powder 50, the greater the distance and area over which the powder 50 scatters when the flat portion 31 is stopped. In addition, the scattered powder 50 remains unevenly on the surface, so the state of scattering can be determined from the captured image. For this reason, for example, by measuring the distance the powder 50 reaches furthest from the stopping position of the flat portion 31 along the scanning direction, the area of the area of the scattered powder 50, and the like from the image, the fluidity of the powder 50 can be estimated. For example, the better the fluidity, the greater the distance the scattered powder 50 will travel, and the greater the area of the area of the scattered powder 50 will be.
[0105] If the fluidity test shows that the fluidity of the powder 50 is too poor, the mixing ratio of the new powder and the recycled powder is controlled so that the fluidity of the powder 50 is increased from the current fluidity of the powder 50. On the other hand, if the fluidity of the powder 50 is too good, the mixing ratio of the new powder and the recycled powder is controlled so that the fluidity of the powder 50 is decreased from the current fluidity of the powder 50.
[0106] 11, if the deviation between the estimated value of the fluidity of powder 50 estimated in step S14a and the target value of the fluidity set in step S11 is within the allowable range set in step S11, the process proceeds to step S14b. On the other hand, if the deviation exceeds the allowable range, the process proceeds to step S15, where the mixing ratio of powder 50 is adjusted by the mixing ratio adjustment unit 84.
[0107] In step S15, if the estimated value of fluidity is higher than the allowable range with respect to the target value, i.e., if the estimated fluidity of powder 50 is good, the mixing ratio of virgin powder is reduced. Thus, the mixing ratio is controlled so as to decrease the fluidity. On the other hand, if the estimated value of fluidity is lower than the allowable range with respect to the target value, i.e., if the estimated fluidity of powder 50 is poor, the mixing ratio of virgin powder is increased. Thus, the mixing ratio is controlled so as to increase the fluidity.
[0108] In step S15, if multiple virgin powders are mixed, the mixing ratio of the multiple virgin powders may be changed. For example, to increase the fluidity, the ratio of virgin powder with a relatively high fluidity may be increased. To decrease the fluidity, the ratio of virgin powder with a relatively low fluidity may be increased. When the process of step S15 is completed, the process returns to the main flow of FIG. 10.
[0109] <Packing density test (S14b)> An overview of the packing density test in step S14b will be described with reference to Fig. 14. Fig. 14 is an example of a captured image for packing density estimation according to an embodiment of the present invention. In the packing density test in step S14b, a larger amount of modeling liquid 60 than the specified amount is applied, and an image of the surface of the powder 50 after a predetermined time has passed is taken. The packing density is estimated from the captured image.
[0110] If the filling density is high, the modeling liquid 60 will penetrate and crush fine shapes, resulting in a deterioration in modeling quality. This may be due to changes in properties, such as an increase in the wettability of the powder 50 and the modeling liquid 60, or a decrease in the viscosity of the modeling liquid 60.
[0111] On the other hand, when the filling density is low, there is no deterioration in the modeling quality due to the penetration of the modeling liquid 60. However, there is a possibility that changes in characteristics such as a decrease in the wettability between the powder 50 and the modeling liquid 60 and an increase in the viscosity of the modeling liquid 60 may occur.
[0112] The penetration of the modeling liquid 60 takes time, and the viscosity of the modeling liquid 60 decreases in the drying unit 4, and the penetration progresses. Therefore, even if the surface of the powder 50 is photographed after the modeling liquid 60 is applied, the penetration of the modeling liquid 60 cannot be determined. For this reason, in the filling density test, the modeling liquid 60 is applied in an amount greater than the specified amount to accelerate the penetration of the modeling liquid 60 into the powder 50 and determine the filling density in a short time. For this reason, the bleeding of the modeling liquid 60 into the powder 50 is determined from the image captured by the photographing unit 16, and the filling density is estimated, thereby determining the mixing ratio of the powder 50. This adjusts the filling density of the powder 50 to a predetermined range, improving the modeling quality. The amount of the modeling liquid 60 applied may also be adjusted together with the determination of the mixing ratio of the powder 50.
[0113] FIG. 14 shows an image taken by the photographing unit 16 10 minutes after applying the modeling liquid 60 to the surface of the powder 50. FIG. 14(A) shows an image in which the modeling liquid 60 is applied twice as much as the specified amount, and FIG. 14(B) shows an image in which the modeling liquid 60 is applied four times as much as the specified amount. If the two images taken with the specified amount of the modeling liquid 60 are not blurred, the filling density is determined to be appropriate. If bleeding occurs in one or more of the two images, the filling density is determined to be high. For example, in FIG. 14(A), the character "A" in the test image 61A does not blur, but in FIG. 14(B), the character "A" in the test image 61B blurs. Therefore, FIG. 14 is determined to have a high filling density. In this way, in the filling density test, the amount of the modeling liquid 60 is changed from the specified amount, and the degree of bleeding is determined from the image. This makes it possible to estimate the filling density of the powder 50.
[0114] If the result of the packing density test indicates that the degree of penetration is large, the mixing ratio of new powder and recovered powder is adjusted so as to reduce the packing density of the current powder 50.
[0115] 11, if the deviation between the estimated value of the filling density of powder 50 estimated in step S14b and the target value of the filling density set in step S11 is within the allowable range set in step S11, the process proceeds to step S14c. On the other hand, if the deviation exceeds the allowable range, the process proceeds to step S17, where the mixing ratio of powder 50 is adjusted by the mixing ratio adjustment unit 84.
[0116] In step S17, if the estimated value of the filling density is higher than the allowable range with respect to the target value, i.e., if the estimated filling density of the powder 50 is high and the penetration is relatively small, the mixing ratio of the new powder is reduced. Therefore, the mixing ratio is controlled so that the filling density of the powder 50 decreases from the current value and the penetration is increased to an appropriate value. On the other hand, if the estimated value of the filling density is lower than the allowable range with respect to the target value, i.e., if the estimated filling density of the powder 50 is low and the penetration is relatively large, the mixing ratio of the new powder is increased. Therefore, the mixing ratio is controlled so that the filling density of the powder 50 increases from the current value and the penetration is decreased to an appropriate value.
[0117] In step S17, in the case where a plurality of virgin powders are mixed, the mixing ratio of the plurality of virgin powders may be changed. For example, to increase the packing density, the ratio of virgin powder with a relatively high packing density may be increased to decrease the packing density. Also, the ratio of virgin powder with a relatively low packing density may be increased. When the process of step S17 is completed, the process returns to the main flow of FIG. 10.
[0118] <Particle size distribution test (S14c)> An overview of the particle size distribution test in step S14c will be described with reference to Fig. 15. Fig. 15 is an example of a captured image for measuring particle size distribution according to one embodiment of the present invention. In the particle size distribution test in step S14c, powder 50 is scattered on glass surface 17, and the scattered powder 50 is photographed. From the captured image, the size of particles contained in powder 50 is measured, and the particle size distribution is estimated.
[0119] The particle size distribution of the powder 50 affects the presence or absence of defects in the molded object, its strength, and the progress of sintering, and thus affects the molding quality. If the particle size distribution of the powder 50 is outside a predetermined range, the molding quality will decrease. For this reason, the particle size distribution of the powder 50 is determined from the captured image, and the mixing ratio of new powder and recovered powder is determined so that the particle size distribution falls within the predetermined range.
[0120] FIG. 15(A) is an example of an image taken by scattering powder 50 on a glass surface 17 and switching to a magnifying lens. Since light is applied from below the glass surface 17, each particle of the powder 50 can be identified, and the number of particles of the powder 50 included in the image can be counted. FIG. 15(B) is an image in which the image of FIG. 15(A) is partially enlarged. In FIG. 15(B), two particles, particles 50A and 50B, are enlarged, and the diameters of the particles can be seen. In FIG. 15(B), particle 50A has a diameter equivalent to 7 pixels in the captured image, and particle 50B has a diameter equivalent to 4 pixels. In this way, the diameters of the particles of the powder 50 included in the captured image are measured, the number of particles is counted, and a histogram is created, and thus the particle size distribution is determined.
[0121] In the flowchart of Fig. 11, if the deviation between the estimated value of the particle size distribution of powder 50 estimated in step S14c and the target value of the flow distribution set in step S11 is within the allowable range set in step S11, the process returns to the main flow of Fig. 10. On the other hand, if the deviation exceeds the allowable range, the process proceeds to step S16, where the mixing ratio of powder 50 is adjusted by the mixing ratio adjustment unit 84.
[0122] In step S16, the mixing ratio of the new powder and the recovered powder is controlled so that the particle size distribution of the current powder 50 falls within a desired particle size distribution range. In addition, in step S16, in the case of a configuration in which a plurality of new powders are mixed, the mixing ratio of the plurality of new powders may be changed so that the particle size distribution of the current powder 50 falls within a desired particle size distribution range. When the process of step S16 is completed, the process returns to the main flow of FIG.
[0123] The glass surface 17 used in the particle size distribution test is installed, for example, at a location different from the modeling tank 12 in the modeling unit 3. The glass surface 17 is installed within the range of the angle of view of the photographing unit 16, or is set at a position where the photographing unit 16 can move and photograph during the particle size distribution test.
[0124] In this embodiment, the powder 50 is scattered on the glass surface 17 with a transparent background so that the particle size distribution can be easily determined from the powder surface image, but an image of the powder surface on the surface of the modeling tank 12 may be used. In this case, the particle size distribution can be measured by performing preprocessing such as extracting the powder 50 on the surface from the powder surface image using, for example, a well-known image processing method.
[0125] Thus, in step S14, the state estimation unit 83 estimates the fluidity, packing density, and particle size distribution of the powder 50 and the powder layer 51 as information on the state of the powder 50 based on the image of the surface of the powder 50 captured by the photographing unit 16. With this configuration, it is possible to accurately estimate the state of the powder 50 using the image captured by the photographing unit 16, and the estimation can be performed with a simple configuration and at low cost. Furthermore, based on the information on the state of the powder 50 estimated in this way, the mixing ratio is determined so that one or more of the fluidity, packing density, and particle size distribution are within a predetermined range. This improves the modeling quality even if the recovered powder is reused.
[0126] The information on the state of the powder 50 estimated by the state estimation unit 83 in step S14 may be at least one of the fluidity, packing density, and particle size distribution of the powder 50, or a combination of these. Also, a configuration may be used in which something other than the fluidity, packing density, and particle size distribution is estimated. Also, the fluidity, packing density, and particle size distribution of the powder 50 are estimated based on an image, but they may be measured using an existing measuring device. In this case, one or more of the new powder, the recovered powder, and the mixed powder may be measured, and the mixing ratio may be determined based on the measured value.
[0127] The three types of tests, namely, "fluidity test (S14a)", "filling density test (S14b)" and "particle size distribution test (S14c)", which are performed by the state estimation unit 83 in step S14, are preferably performed in advance before the actual modeling operation, although the timing of performing the tests is not particularly limited. It may be difficult to perform the tests during the actual modeling operation of the modeling unit 3. For example, there are conditions for performing the tests, such as intentionally making it easier for unevenness P to occur on the powder surface in the fluidity test, applying more modeling liquid 60 than usual in the filling density test, and scattering powder 50 on a glass surface 17 other than the modeling tank 12 in the particle size distribution test. Examples of the timing include, before the start of modeling with the three-dimensional modeling apparatus 1, when the three-dimensional modeling apparatus 1 is started, when the three-dimensional modeling apparatus 1 receives new modeling data from the modeling data creation device 104, and the like. Alternatively, examples of the timing include, during modeling with the three-dimensional modeling apparatus 1, when modeling of one three-dimensional object is completed and the modeling operation of another three-dimensional object is started. Moreover, each test may be performed periodically or at an arbitrary timing, or in response to an operation command from a user, regardless of the modeling operation of the 3D modeling apparatus 1.
[0128] In this manner, in the flowchart of the mixing ratio adjustment control shown in FIG. 11, the mixing ratio adjustment unit 84 uses (1) to (4) as four types of judgment indexes to adjust the mixing ratio of new powder to recovered powder so that the mixing ratio is optimized. (1) The mixture ratio is determined based on the operation mode set in step S11. (2) In step S12, the mixing ratio is determined from information on the fluidity of the collected powder based on the power consumption of the motor 22 of the powder mixer 2 estimated by the state estimator 83. (3) In step S13, a mixture ratio is determined based on the information on the modeling conditions of the modeling unit 3 recorded in the modeling condition recording unit 82. (4) In step S14, the state estimation unit 83 determines the mixing ratio from one or more pieces of information on the state of the powder 50 based on the image captured by the imaging unit 16, including fluidity, packing density, and particle size distribution.
[0129] The mixing ratio adjustment unit 84 can grasp the current characteristics of the powder 50 by referring to the judgment indexes (1) to (4). Then, the mixing ratio of the new powder and the recovered powder is adjusted so that the powder 50 has the desired characteristics. For example, a predetermined range is determined for each of the information on the state of the powder 50, such as the fluidity, packing density, and particle size distribution of the powder 50, and the information on the state of the powder 50 is set to fall within the predetermined range. By adjusting the mixing ratio so that the powder 50 has the desired characteristics, the modeling quality is improved.
[0130] Here, the effect of applying the judgment index (3) will be described with reference to FIG. 12. FIG. 12 is a diagram for explaining the influence of the molding conditions according to one embodiment of the present invention on the state of the powder 50. FIGS. 12(A) and (B) show the particle size distribution of the recovered powder when the powder layer 51 is formed with a layer thickness of 102 μm and 66 μm, respectively. The horizontal axis of the particle size distribution shows the diameter (μm) of the particles contained in the recovered powder, and the vertical axis shows the ratio (volume %) of each powder diameter to the entire recovered powder. In other words, the vertical axis shows the volume ratio of each particle to the volume of the entire recovered powder. Moreover, the particle size distribution D1 of the recovered powder in the powder removal unit 5 is shown by a solid line, and the particle size distribution D2 of the recovered powder in the molding unit 3 is shown by a dotted line.
[0131] If the particle size distribution of the mixed powder used in the modeling unit 3, the scanning speed and rotation speed of the flat portion 31, and the layer thickness of the powder layer 51 are the same, the particle size distribution of the powder recovered by the modeling unit 3 and the particle size distribution of the powder recovered by the powder removal unit 5 will be almost the same every time. For this reason, if modeling is performed in advance under various modeling conditions and the particle size distribution of the powder recovered by the modeling unit 3 and the powder removal unit 5 are recorded, the particle size distribution of the powder recovered by each of the modeling unit 3 and the powder removal unit 5 can be estimated from the modeling conditions during actual modeling.
[0132] In Fig. 12(A), the particle size distribution D2 of the powder 50 collected in the modeling unit 3 is almost the same as the particle size distribution D1 of the powder 50 collected in the powder removal unit 5. On the other hand, in Fig. 12(B), the particle size distribution D2 of the powder 50 collected in the modeling unit 3 has a high proportion of powder 50 with large particle sizes, and the particle size distribution D1 of the powder 50 collected in the powder removal unit 5 has a high proportion of powder 50 with small particle sizes. In this way, the particle size distributions D1, D2 of the powder 50 collected from the modeling unit 3 and the powder 50 collected from the powder removal unit 5 may differ, and this depends on the layer thickness.
[0133] 12 illustrates the effect on the particle size distribution when the lamination thickness of the powder layer 51, which is one of the modeling conditions of the modeling unit 3, is changed, but the particle size distribution may also be affected by changing other modeling condition parameters such as the scanning speed and rotation speed of the flat unit 31 and the volume of the modeled object. In addition, effects on the packing density, fluidity, and other parameters other than the particle size distribution may also occur.
[0134] Therefore, by taking into account the molding conditions of the molding section 3, as in the above judgment indicator (3), it is possible to grasp changes in the state of the mixed powder, such as particle size distribution, and therefore it is possible to more appropriately adjust the mixing ratio.
[0135] The procedure for estimating the powder 50 based on the molding conditions in the judgment index (3) and adjusting the mixing ratio is, for example, as follows. First, the relationship between the scanning speed of the flat portion 31, the rotation speed of the flat portion 31, the layer thickness of the powder layer 51, and the characteristics of the powder 50 recovered by the molding unit 3 and the powder 50 recovered by the powder removal unit 5 when molding is performed under those conditions (here, particle size distribution is used as an example). The relationship between the molding conditions acquired in this way and the characteristics of the powder 50 is stored, for example, in the mixing ratio adjustment unit 84.
[0136] Next, using the relationship thus obtained, in step S13 of Fig. 11, the particle size distribution of the powder 50 recovered in the modeling unit 3 and the particle size distribution of the powder 50 recovered in the powder removal unit 5 under the actual modeling conditions are estimated. Note that, if there is no data under the exactly same conditions as the modeling conditions previously investigated, the particle size distribution may be estimated by interpolation.
[0137] The particle size distribution of all the recovered powder is determined by taking a weighted average of the particle size distribution of the powder 50 recovered in the modeling unit 3 and the particle size distribution of the powder 50 recovered in the powder removal unit 5, based on the ratio of the amounts of the powder 50. The amount of powder 50 recovered in the modeling unit 3 is the amount of powder 50 overflowing from the modeling tank 12, and can be estimated from the amount of vertical movement of the bottoms of the supply tank 11 and the modeling tank 12. The amount of powder 50 recovered in the powder removal unit 5 can be estimated from the volume of the modeling tank 12 excluding the volume of the modeled object.
[0138] In this way, the particle size distribution of the recovered powder can be estimated, and the amount of new powder to be mixed in is determined so that the particle size distribution becomes the desired particle size distribution. That is, in step S16 of Fig. 11, if the particle size distribution of the recovered powder has changed significantly from the original particle size distribution, more new powder is mixed in than the specified amount. On the other hand, if the particle size distribution of the recovered powder has not changed significantly from the original particle size distribution, less new powder is mixed in than the specified amount.
[0139] Furthermore, when a plurality of types of virgin powder, for example, a plurality of virgin powders having different particle sizes is mixed, the mixing ratio of the plurality of virgin powders is adjusted so as to obtain a desired particle size distribution.
[0140] In step S13 of Fig. 11, a configuration for estimating the particle size distribution of the powder 50 from the modeling conditions of the modeling unit 3 is illustrated based on the example of Fig. 12, but it is also possible to estimate, in addition to the particle size distribution, for example, packing density and fluidity from the modeling conditions. For example, in step S13, when a configuration for estimating packing density from modeling conditions is applied, the flowchart of Fig. 11 may be modified to proceed to step S17 when the deviation between the estimated value and the target value exceeds the allowable range. Similarly, in step S13, when a configuration for estimating fluidity from modeling conditions is applied, the flowchart of Fig. 11 may be modified to proceed to step S15 when the deviation between the estimated value and the target value exceeds the allowable range.
[0141] By adjusting the mixing ratio based on such molding conditions, the molding quality can be improved even when using recycled powder.
[0142] The mixing ratio adjusting unit 84 outputs information on the adjusted mixing ratio as a mixing ratio command to the powder mixing unit 2. In step S2 of Fig. 10, a desired mixing ratio is set based on the mixing ratio command input from the mixing ratio adjusting unit 84. Then, in step S3, the mixing ratio adjusting unit 84 produces mixed powder so as to have the desired adjusted mixing ratio.
[0143] The effects of the three-dimensional modeling apparatus 1 according to this embodiment will be described below. The three-dimensional modeling apparatus 1 includes a modeling unit 3 that models a model containing powder 50, a recovery unit 7 that recovers at least a portion of the powder 50 as recovered powder, a powder mixing unit 2 that mixes two or more types of powder including the recovered powder, and a control unit 8 that controls the mixing ratio of the two or more types of powder mixed in the powder mixing unit 2 based on information on the state of the powder 50 and information on the modeling conditions of the modeling unit 3.
[0144] In the three-dimensional modeling apparatus 1 of this embodiment, surplus powder around the modeled object is collected after the modeling process and drying process in three-dimensional modeling, and this collected powder is reused. The state of the collected powder may change from that of the powder before modeling, such as decreasing in fluidity. On the other hand, in order to maintain constant modeling quality, it is desirable that the mixed powder generated by mixing new powder and collected powder in the powder mixing unit 2 satisfies a desired standard value. Therefore, it is necessary to appropriately adjust the mixing ratio of new powder and collected powder in the powder mixing unit 2 according to the state of the collected powder.
[0145] Therefore, in this embodiment, the mixing ratio of the new powder and the recovered powder is adjusted using two types of information: the first information on the state of the powder 50 and the second information on the modeling conditions of the modeling unit 3. By adjusting the mixing ratio based on multiple types of information in this manner, the modeling quality is improved.
[0146] In this embodiment, the mixing ratio adjustment unit 84 of the control unit 8 adjusts the mixing ratio of two or more types of powder mixed in the powder mixing unit 2 by using both information on the state of the powder 50 and information on the modeling conditions of the modeling unit 3, but the information referred to for adjusting the mixing ratio may be at least one of the information on the state of the powder 50 and the information on the modeling conditions of the modeling unit 3. In other words, a configuration may be used in which the mixing ratio is adjusted by using at least a part of the four judgment indexes (1) to (4) listed in the above-mentioned step S15.
[0147] In the 3D modeling apparatus 1 of this embodiment, the mixing ratio adjusting unit 84 of the control unit 8 adjusts the mixing ratio of new powder and recovered powder to an optimal ratio, thereby improving modeling quality. Here, the influence of the powder 50, the powder layer 51, and the mixing ratio on 3D modeling will be described with reference to Fig. 16. Fig. 16 is a diagram showing the dependency relationship between the powder 50 and the powder layer 51 and the 3D modeled object according to one embodiment of the present invention.
[0148] The new powder and the recovered powder are mixed at an arbitrary mixing ratio in the powder mixing section 2 to generate a mixed powder. Therefore, the bulk density, fluidity, and particle size distribution as information 113 on the state of the mixed powder depend on the information 110 on the state of the new powder, the information 111 on the state of the recovered powder, and the mixing ratio 112 of the mixed powder. The powder layer 51 is formed in the modeling section 3 using this mixed powder. Therefore, the packing density and the presence or absence of a result as information 115 on the state of the powder layer 51 depend on the information 113 on the state of the mixed powder, and the layer thickness, scanning speed, and rotation speed as information 114 on the modeling conditions of the modeling section 3. The model passes through the drying section 4, the powder removing section 5, and the sintering section 6 to complete a three-dimensional model. Therefore, the density, strength, and shape accuracy as information 116 on the modeled object and the three-dimensional modeled object depend on the information 113 on the state of the mixed powder and the information 115 on the state of the powder layer 51.
[0149] The factors that cause fluctuations in the information 116 on the state of the modeled object and the three-dimensional modeled object will be described. The information 111 on the state of the recovered powder varies greatly because it deteriorates with repeated modeling. The information 110 on the state of the new powder does not vary as much as the properties of the recovered powder, but it does vary depending on the production lot. The information 113 on the state of the mixed powder depends on the information 110 on the state of the new powder, the information 111 on the state of the recovered powder, and the mixing ratio 112, but these are not in a linear relationship. In other words, even if the information 110 on the state of the new powder and the information 111 on the state of the recovered powder are accurately known, it is difficult to accurately predict the information 113 on the state of the mixed powder.
[0150] It is sufficient for the 3D modeling apparatus 1 to model the object so that information 116 on the state of the 3D object falls within an allowable range. The dependency shown in Fig. 16 is modeled in advance (hereinafter, referred to as "powder 50 and 3D object model"). The mixture ratio adjustment unit 84 controls the mixture ratio 112 so that information 113 on the state of the mixed powder and information 115 on the state of the powder layer 51 reach target values.
[0151] Here, the four types of judgment indexes (1) to (4) used by the mixture ratio adjustment unit 84 and their correspondence with FIG. 16 will be described.
[0152] The judgment index (1) is a target value and an allowable range of the mixing ratio based on the operation mode set in step S11 in Fig. 11. In Fig. 16, it corresponds to adjusting the target values of the information 113 on the state of the mixed powder and the information 115 on the state of the powder layer 51, and adjusting the settable range of the information 114 on the modeling conditions.
[0153] The judgment index (2) is information on the fluidity of the powder 50 estimated in step S12 in Fig. 11. In Fig. 16, it corresponds to the information 113 on the state of the mixed powder or the information 111 on the state of the collected powder.
[0154] The judgment index (3) is information on the modeling condition used in step S13 in Fig. 11. In Fig. 16, it corresponds to information 111 on the state of the collected powder.
[0155] The judgment index (4) is the fluidity, packing density, and particle size distribution of the mixed powder estimated in step S14 in Fig. 11. In Fig. 16, it corresponds to information 113 on the state of the mixed powder and information 115 on the state of the powder layer 51.
[0156] A specific method in which the mixture ratio adjusting unit 84 adjusts the mixture ratio to an optimum one will be described.
[0157] The target values and allowable ranges of the information 113 on the state of the mixed powder and the information 115 on the state of the powder layer 51, and the set values of the information 114 on the modeling conditions are determined in advance. By selecting the operation mode in step S11, these ranges are adjusted.
[0158] For example, when the "shape accuracy priority mode" is selected, the allowable range of the particle size distribution in the information 113 on the state of the mixed powder is set narrow, and the target value of the packing density in the information 115 on the state of the powder layer 51 is set high. The mixing ratio 112 is determined so as to satisfy these set values.
[0159] For example, when the "powder cost priority mode" is selected, the target values of information 113 regarding the state of the mixed powder, information 115 regarding the state of the powder layer 51, and the set values of information 114 regarding the molding conditions are within the allowable range, and the mixing ratio 112 is determined so as to increase the amount of recovered powder.
[0160] For example, when the “modeling speed priority mode” is selected, the allowable range of the scanning speed of the information 114 on the modeling conditions is set to be wide. The mixing ratio 112 is determined in consideration of the information 113 on the state of the mixed powder and the information 115 on the state of the powder layer 51 so as to satisfy this setting.
[0161] In step S12, the fluidity is estimated as information 113 on the state of the mixed powder. Alternatively, the fluidity is measured as information 111 on the state of the collected powder by the method described in the "characteristic acquisition mode" described later. The difference between the measured fluidity and a target value is calculated, and the mixing ratio 112 is changed based on the three-dimensional object model so as to reduce the difference.
[0162] Since the modeling conditions of the modeling unit 3 are recorded in step S13, information 111 on the state of the recovered powder can be estimated. From the estimated information 111 on the state of the recovered powder, the mixing ratio 112 is changed based on the three-dimensional object model so that information 113 on the state of the mixed powder with new powder becomes equal to a target value.
[0163] In step S14, information 113 on the state of the mixed powder and information 115 on the state of the powder layer 51 are estimated, and the mixture ratio 112 is changed based on the powder 50 and the three-dimensional object model so that these become equal to the target values.
[0164] Moreover, the three-dimensional modeling apparatus 1 of this embodiment includes a state estimation unit 83 that estimates information on the state of the powder 50. A mixing ratio adjustment unit 84 of the control unit 8 adjusts the mixing ratio based on the information estimated by the state estimation unit 83. With this configuration, the mixing ratio can be adjusted using the information on the state of the powder 50 estimated by the state estimation unit 83, so that the mixing ratio can be adjusted to a more appropriate value.
[0165] <First Modification of Mixing Ratio Adjustment Control> The mixing ratio adjustment control may be configured to have a mode in which the powder mixing unit 2 mixes new powder or recovered powder at a predetermined ratio. Specifically, a "calibration mode" that uses only new powder and a "characteristics acquisition mode" that uses only recovered powder to acquire the characteristics of the recovered powder can be added.
[0166] (Calibration mode) In the calibration mode, the powder mixing unit 2 supplies only new powder to the modeling unit 3. Then, information on the state of the new powder at this time is obtained. For example, each test in step S14 is performed to estimate the fluidity, packing density, and particle size distribution from the image captured by the imaging unit 16. Also, as in step S12, the fluidity is estimated from the driving force of the motor 22 of the powder mixing unit 2. The information on the state of the new powder is considered to be known, and the state estimation unit 83 is calibrated by comparing the estimated information with the known information.
[0167] 7 has a first pattern in which only virgin powder A is supplied to the modeling unit 3, and a second pattern in which only virgin powder B is supplied to the modeling unit 3. Information on the state of the powder 50 may be estimated for each pattern to calibrate the state estimation unit 83.
[0168] By providing such a calibration mode, the modeling quality is improved even when using recovered powder.
[0169] Here, we will explain how the state estimation unit 83 estimates the fluidity based on the driving force of the motor 22 of the powder mixing unit 2. As the motor 22 is used, the proportional relationship between the driving force and the fluidity changes due to the adhesion of powder and wear, etc., which causes an estimation error. If this error can be eliminated, the estimation accuracy will increase.
[0170] Here, the control value and current consumption of the motor 22 when only virgin powder is stirred are recorded in advance.
[0171] First, in the calibration mode, only new powder is put into the stirring tank 21 of the powder mixing section 2. Next, the control value of the motor 22 or the current consumption of the motor 22 is measured. It is preferable that the pre-recorded value is the same as the measured value. On the other hand, if the values are different, a correction coefficient is calculated to correct the measured value.
[0172] When new powders A and B are used, the control value of motor 22 or the current consumption of motor 22 is measured in the first and second patterns. The fluidity, control value, and power consumption of new powder A and new powder B are recorded in advance. If the values measured in the first and second patterns differ from the recorded values, a correction coefficient is calculated to correct the measured values.
[0173] (Characteristics Acquisition Mode) In the characteristic acquisition mode, the powder mixing unit 2 supplies only the recovered powder to the modeling unit 3. Then, information about the state of the recovered powder at this time is estimated, and information about the state of the recovered powder is estimated based on the estimated information. As in the calibration mode, the information about the state of the recovered powder is estimated based on each test in step S14 and the driving force of the motor 22 of the powder mixing unit 2 in step S12. If the estimated information about the state of the recovered powder has changed significantly compared to the information about the state of the mixed powder, it is preferable to discard the recovered powder.
[0174] By providing such a characteristic acquisition mode, the molding quality is improved even if the recovered powder is reused.
[0175] <Second Modification of Mixing Ratio Adjustment Control> In the mixing ratio adjustment control, the control unit 8 may be configured to impose restrictions on the modeling conditions of the modeling unit 3 according to information on the state of the mixed powder.
[0176] As a specific example, the setting range of the modeling conditions is changed according to information on the estimated state of the powder 50. For example, the fluidity is acquired in step S12 or step S14. Depending on the fluidity, if the fluidity is high, the maximum value of the scanning speed of the flat portion 31 is increased, and if the fluidity is low, the maximum value of the scanning speed of the flat portion 31 is decreased.
[0177] In this way, by restricting the modeling conditions of the modeling unit 3 according to the information on the state of the powder 50, it is possible to prevent the setting of modeling conditions that do not match the information on the state of the powder 50, thereby improving the modeling quality.
[0178] The fluidity of the mixed powder affects the molding quality. Therefore, the maximum value of the recoating speed of the flat portion 31 changes depending on the fluidity. Therefore, the fluidity is estimated based on the image captured in step S14 and the power consumption in step S12, and the maximum value of the molding condition for the flat portion 31 is changed. This prevents the setting of molding conditions that do not match the information on the state of the powder 50, improving the molding quality.
[0179] <Third Modification of Mixing Ratio Adjustment Control> In addition, in the mixing ratio adjustment control, a communication unit that transmits information on the state of the powder 50 or information on the modeling conditions of the modeling unit 3 to an external device may be provided, and the control unit 8 may control the mixing ratio based on an instruction received from the external device via the communication unit. The external device may be a cloud.
[0180] The 3D modeling apparatus 1 is connected to a service provider that supports the operation of the apparatus via the communication unit. The 3D modeling apparatus 1 transmits information such as the modeling conditions in step S13, the image in step S14, and the measurement values in step S12 to an external device. The external device estimates information on the state of the powder 50 based on the information transmitted from the 3D modeling apparatus 1 and determines the mixing ratio. Then, it transmits the mixing ratio to the 3D modeling apparatus 1 via the communication unit. The 3D modeling apparatus 1 generates the mixed powder based on the transmitted mixing ratio.
[0181] The external device may store, for example, information on the modeling conditions, the state of the powder 50, and the like in advance.
[0182] Alternatively, the external device may perform a simulation to predict changes in the information regarding the modeling conditions and the state of the powder 50. From the transmitted information, the simulation predicts changes in the information regarding the state of the collected powder, and determines an optimal mixing ratio.
[0183] Fig. 17 is a diagram showing a first modified example 3A of the modeling unit according to one embodiment of the present invention. The modeling unit 3A according to the first modified example shown in Fig. 17 includes a powder supply unit 70 instead of the supply tank 11 of the modeling unit 3 shown in Fig. 1. Descriptions common to Fig. 1 will be omitted as appropriate.
[0184] The powder supplying unit 70 supplies powder 50 to the powder layer 51 in the modeling tank 12. The powder supplying unit 70 is movable in the horizontal direction (Y1 and Y2 directions) and scans above the modeling tank 12 to supply powder 50 to the modeling tank 12.
[0185] The powder supply section 70 includes a hopper 71 , a vibration source 72 , and a trough 73 .
[0186] The hopper 71 holds the powder 50 to be supplied to the modeling tank 12 .
[0187] The trough 73 supplies the powder 50 to the modeling tank 12. The trough 73 is a supply path that supplies the powder 50 held in the hopper 71 to the modeling tank 12. It is preferable that the length (width) of the trough 73 in the X direction is the same as the length (width) of the modeling tank 12 in the X direction. The vibration source 72 vibrates the trough 73. As the trough 73 is vibrated by the vibration source 72, the powder 50 falls from the opening of the trough 73 into the modeling tank 12.
[0188] 1, the modeling section 3A includes an application section 40, a lamination unit 30, and an excess powder tank 15. As part of the modeling section, the powder supply section 70 supplies powder to form a powder layer 51 containing powder 50. The application section 40 applies modeling liquid 60 to the powder layer 51 to form a modeling layer 61. In the modeling section 3A, a plurality of modeling layers 61 are laminated to form a modeled object.
[0189] Fig. 18 is a diagram showing a second modified example 3B of the modeling unit according to an embodiment of the present invention. Unlike the modeling unit 3 shown in Fig. 1, the modeling unit 3B according to the second modified example shown in Fig. 18 uses a high-speed sintering (HSS) method in which a modeling solution containing a radiant energy absorber is applied.
[0190] In the modeling unit 3B of the second modified example, unlike the modeling unit 3 of the above embodiment, the application unit 40B applies a modeling liquid 60B containing a radiant energy absorbent, and further includes a radiant energy source 90. Descriptions of the means denoted by the same reference numerals as those in FIG. 1 will be omitted as appropriate.
[0191] The application unit 40B applies a modeling liquid 60B containing a radiant energy absorber to a powder layer 51 containing the powder 50.
[0192] The application unit 40B includes a radiant energy source 90. The radiant energy source 90 is driven to the region of the powder layer 51 to which the modeling liquid 60B containing a radiant energy absorbent is applied. The radiant energy source 90 may be anything that activates the radiant energy absorbent, such as light or electromagnetic radiation. The radiant energy source 90 may be installed on only one side of the head 42, or on both the left and right sides. The radiant energy source 90 may be connected to the carriage 41 and driven integrally with the head 42. Alternatively, the radiant energy source 90 may be a separate entity from the head 52 and driven separately.
[0193] The radiant energy source 90 includes a light source 91 and a reflector 92 .
[0194] Examples of the light source 91 include a halogen lamp, an LED, an LD, a flash lamp, a xenon lamp, and a spherical lamp.
[0195] Reflecting section 92 reflects light emitted from light source 91. For example, reflecting section 92 is generally dome-shaped with an opening at one end and a curved surface, and light source 91 is disposed within the area of the opening. The curved surface of reflecting section 92 condenses the light so that the area of the light irradiated from light source 91 to powder layer 51 is smaller than the area of the opening of reflecting section 92.
[0196] For example, when the radiant energy absorber is a near-infrared dye (NIRD) or a near-infrared pigment (NIRP), electromagnetic radiation having a wavelength of, for example, about 800 nm to about 1400 nm is irradiated from a radiant energy source 90 onto the powder layer 51 to which the modeling liquid 60B containing the radiant energy absorber has been applied. This allows the radiant energy absorber to absorb the electromagnetic radiation and convert the absorbed energy into thermal energy. In addition to the radiant energy absorber, a colorant may be applied to the powder layer 51 containing the powder 50.
[0197] 19 is a block diagram showing a modified example 84A of the mixing ratio adjustment unit according to one embodiment of the present invention. The mixing ratio adjustment unit 84 shown in FIG. 8 can be replaced with the mixing ratio adjustment unit 84A according to the modified example shown in FIG.
[0198] The mixing ratio adjustment unit 84A may be implemented with a machine learning program. The mixing ratio adjustment unit 84A can execute optimal modeling control for similar modeling data and similar device conditions (powder surface conditions, powder characteristics used) by learning the correspondence between the modeling data, powder surface / powder characteristic information, and optimal control of each part of the three-dimensional modeling apparatus 1. The machine learning program includes a data accumulation unit 85, a learning unit 86, and an estimation unit 87.
[0199] The data storage unit 85 stores data such as the shape of the object, information about the state of the powder 50, information about the state of the modeling tank 12, the modeling conditions of the 3D modeling apparatus 1, the mixing ratio and the modeling results (characteristic values such as the accuracy, density, and strength of the object, the presence or absence of damage to the object or internal defects during the process or after completion, etc.).
[0200] The learning unit 86 learns, for example, to detect conditions that have a high probability of causing modeling failure from the data stored in the data storage unit 85. The algorithm used by the learning unit 86 is not particularly limited, and deep learning using a neural network, an unsupervised learning model, a supervised learning model, a reinforcement learning model, etc. can be applied. The teacher data input to the algorithm used by the learning unit 86 are, for example, the image captured by the imaging unit 16, the modeling conditions of the three-dimensional modeling device 1, and the mixture ratio.
[0201] The estimation unit 87 estimates the validity of the mixing ratio by utilizing the learned learning unit 86. For example, an image, modeling conditions, a mixing ratio, etc. are input to the estimation unit 87. The estimation unit 87 outputs a predetermined numerical value. The numerical value indicates, for example, the possibility of deterioration of accuracy or the possibility of internal defects occurring in the modeled object, from 0 to 10.
[0202] For example, if the estimation unit 87 outputs a high numerical value, the modeling quality may be degraded.
[0203] For example, when the estimation unit 87 outputs a low numerical value, it is determined that the modeling quality satisfies a certain standard.
[0204] <Modification of the imaging unit 16> A 3D scanner may be used as the imaging unit 16 included in the modeling unit 3. A method using a 3D scanner will be described.
[0205] A 3D scanner, for example, shines crossed lasers on the target, captures the reflected light with a sensor, and then uses the principle of triangulation to measure distance. This makes it possible to observe the powder surface more accurately as a three-dimensional point cloud. Specifically, it makes it possible to clearly observe the edges of the target.
[0206] In other words, in the filling density test (S14b) described with reference to Figure 14, when a 3D scanner is used as the photographing unit 16, more precise images can be obtained than with a digital camera, video camera, or CCD, thereby reducing the risk of incorrect judgment.
[0207] For example, in the case of Figure 14, "bleeding" is measured, but a slight step is created at the boundary between the area where bleeding occurs, that is, the area where ink (modeling liquid 60) is present, and the area where ink is not present. Since a 3D scanner uses a laser and measures the distance, this step can be clearly extracted. Therefore, it is possible to accurately determine the standard for whether bleeding is OK or NG.
[0208] In this way, by using a 3D scanner as the imaging unit 16, it is possible to optimize the amount of virgin powder mixed when virgin powder and recovered powder are mixed to generate mixed powder in the powder mixing unit 2. This eliminates the waste of virgin powder, thereby contributing to the SDGs.
[0209] In other words, compared to using a digital camera, video camera, or CCD as the photographing unit 16, using a 3D scanner improves the accuracy of determining the boundary of the bleeding, thereby eliminating the waste of new powder.
[0210] For the fluidity test (S14a) described with reference to Fig. 13 and the particle size distribution test (S14c) described with reference to Fig. 15, the same effect can be obtained by using a 3D scanner as the imaging unit 16 in the same manner as for the packing density test (S14b) in Fig. 14. In other words, the accuracy of the judgment is improved.
[0211] 13, the area and shape of unevenness P occurring on the surface of powder 50 are measured, and a slight step is generated at the boundary between the area where unevenness P exists and the area where unevenness P does not exist. By using a 3D scanner as the imaging unit 16, the accuracy of the judgment is improved, as in the packing density test (S14b) in FIG.
[0212] In the particle size distribution test (S14c) of Figure 15, by taking advantage of the advantage of using a 3D scanner as the imaging unit 16, which enables clear edge detection, the sizes of the particles 50A, 50B can be measured more accurately, and the particle size distribution can also be estimated more accurately.
[0213] Therefore, in the fluidity test (S14a) and particle size distribution test (S14c), when a 3D scanner is used as the imaging unit 16, the criteria for the test results being OK / NG can be accurately determined.
[0214] Incidentally, even when a 3D scanner is used as the photographing unit 16, in the flowchart of the mixing ratio adjustment control in FIG. 11, the processes other than the tests in step S14 may be the same as when a digital camera, video camera, or CCD is used as the photographing unit 16.
[0215] The present embodiment has been described above with reference to specific examples. However, the present disclosure is not limited to these specific examples. Any design modifications made by a person skilled in the art to these specific examples are also included within the scope of the present disclosure as long as they have the features of the present disclosure. The elements of each of the above-mentioned specific examples and their arrangements, conditions, shapes, etc. are not limited to those exemplified and can be changed as appropriate. The combination of each of the elements of each of the above-mentioned specific examples can be changed as appropriate as long as no technical contradiction occurs.
[0216] In the above embodiment, a single 3D modeling apparatus 1 has been described as an example, but the 3D modeling system may include multiple 3D modeling apparatuses 1. In the 3D modeling system, the multiple 3D modeling apparatuses 1 are connected to each other so that they can communicate with each other, and the multiple 3D modeling apparatuses 1 can operate in conjunction with each other.
[0217] In addition, a control device having a modeling control unit 81, a modeling condition recording unit 82, a state estimation unit 83, and a mixing ratio adjustment unit 84 may be connected to a three-dimensional modeling apparatus including the powder mixing unit 2, the modeling unit 3, the drying unit 4, the powder removal unit 5, the sintering unit 6, and the recovery unit 7, or the control device may be included in the three-dimensional modeling apparatus.
[0218] <Contribution to the United Nations-led Sustainable Development Goals (SDGs)> Each embodiment of the present invention can use recovered powder to create three-dimensional objects, thereby contributing to goals 12 and 13 of the SDGs. Furthermore, if the powder contains metals such as aluminum, iron, or copper, it can also contribute to recycling.
[0219] For example, aspects of the present invention are as follows. <1> A molding unit that molds a molded object containing metal powder; A recovery unit that recovers at least a portion of the powder as recovered powder; A powder mixing section for generating a mixed powder containing at least the recovered powder; A control unit that controls a mixing ratio of the new powder and the recovered powder based on information on at least one of the states of the powder, the recovered powder, and the mixed powder; A three-dimensional modeling apparatus comprising: <2> The molding unit is The modeling liquid is applied to the powder. <1> The three-dimensional modeling apparatus according to claim 1 . <3> The recovery section includes: At least a part of the powder used in the modeling unit or the powder removed in the powder removing unit is collected. <1> or <2> The three-dimensional modeling apparatus according to claim 1 . <4> The powder mixing section includes: The unused new powder is mixed with the recovered powder in the molding section. <1> ~ <3> 3. The three-dimensional object forming apparatus according to claim 1 . <5> The information regarding one or more states of the powder, the recovered powder, and the mixed powder is The flowability, packing density, and particle size distribution of the powder <1> ~ <4> 3. The three-dimensional object forming apparatus according to claim 1 . <6> The control unit is Further, the mixing ratio is controlled based on information regarding the molding conditions of the molding unit. <1> ~ <5> 3. The three-dimensional object forming apparatus according to claim 1 . <7> A state estimation unit that estimates information regarding one or more states of the powder, the recovered powder, and the mixed powder, The control unit controls the mixture ratio based on the information estimated by the state estimation unit. The above <1> ~ <6> 3. The three-dimensional object forming apparatus according to claim 1 . <8> a photographing unit that photographs a surface of the powder in the modeling unit; determining information regarding one or more states of the powder, the recovered powder, and the mixed powder based on the image captured by the imaging unit; The above <1> ~ <7> 3. The three-dimensional object forming apparatus according to claim 1 . <9> The powder mixing unit has a motor that stirs the mixed powder, The control unit determines information regarding one or more states of the powder, the collected powder, and the mixed powder based on the driving force of the motor. The above <1> ~ <8> 3. The three-dimensional object forming apparatus according to claim 1 . <10> The 3D modeling device is capable of selecting operations including accuracy, cost, and speed; The control unit determines information regarding one or more states of the powder, the recovered powder, and the mixed powder in response to the selected operation. The above <1> ~ <9> 3. The three-dimensional object forming apparatus according to claim 1 . <11> A forming unit that forms a layer containing powder; An application unit that applies a modeling liquid to the layer; A recovery unit that recovers at least a portion of the powder as recovered powder; A powder mixing section for generating a mixed powder containing at least the recovered powder; A control unit that controls a mixing ratio of the new powder and the recovered powder based on information about the molding conditions of the forming unit; A three-dimensional modeling apparatus comprising: <12> The powder contains a metal. <11> The three-dimensional modeling apparatus according to claim 1 . <13> the forming unit includes a flattening unit that is rotated and scanned along a surface of the powder to flatten the surface and form a powder layer; The molding conditions include any one of a volume of the object, a scanning speed of the flat portion, a rotation speed of the flat portion, and a layer thickness of the powder layer. The above <11> or <12> The three-dimensional modeling apparatus according to claim 1 . <14> The control unit Further, the mixing ratio of the mixed powder is controlled based on information on one or more states of the powder, the recovered powder, and the mixed powder. <11> ~ <13> 3. The three-dimensional object forming apparatus according to claim 1 . <15> A molding step of forming an object containing metal powder; A recovery step of recovering at least a portion of the powder as recovered powder; A powder mixing step of generating a mixed powder containing at least the recovered powder; A mixing ratio adjustment step of controlling a mixing ratio of the new powder and the recycled powder based on information on at least one of the states of the powder, the recycled powder, and the mixed powder; A three-dimensional modeling method comprising the steps of: <16> A sintering unit that sinters the shaped object, The above <1> ~ <14> 3. The three-dimensional object forming apparatus according to claim 1 . <17> A molding unit that molds a molded object containing metal powder; A recovery unit that recovers at least a portion of the powder as recovered powder; a powder mixing unit that generates a mixed powder including at least the recovered powder, A control device that controls the mixing ratio of the new powder and the recycled powder based on information regarding at least one or more states of the powder, the recycled powder, and the mixed powder. <18> A recovery apparatus that recovers, as recovered powder, a portion of powder used in a molding apparatus that forms a molded object containing metal powder, the recovery apparatus comprising: A control unit is provided that controls a mixing ratio of the new powder and the recovered powder based on information on one or more states of at least the powder, the recovered powder, and a mixed powder generated containing at least the recovered powder. Recovery device. [Explanation of symbols]
[0220] 1 Three-dimensional modeling device 2 Powder mixing section 22 Motor 3. Modeling Department 31 Flat area 6 Sintering section 7. Collection Section 8 Control unit (control device) 82 Modeling Condition Recording Section (Recording Section) 83 State Estimation Unit 16. Photography Department 50 powder (mixed powder) 51 Powder layer [Prior art documents] [Patent documents]
[0221] [Patent Document 1] Patent Publication No. 2021-025062
Claims
1. A molding unit that molds a molded object containing metal powder; A recovery unit that recovers at least a portion of the powder as recovered powder; A powder mixing section for generating a mixed powder containing at least the recovered powder; A control unit that controls a mixing ratio of the new powder and the recovered powder based on information on at least one of the states of the powder, the recovered powder, and the mixed powder; A three-dimensional modeling apparatus comprising:
2. The molding unit is The three-dimensional object fabrication apparatus according to claim 1 , further comprising an application unit that applies a modeling liquid to the powder.
3. The recovery section includes: The three-dimensional object fabrication apparatus according to claim 1 , wherein at least a part of the powder used in the modeling unit or the powder removed in a powder removing unit is recovered.
4. The powder mixing section includes: The three-dimensional object fabrication apparatus according to claim 1 , wherein the recovered powder is mixed with the unused new powder in the modeling unit.
5. The information regarding one or more states of the powder, the recycled powder, and the mixed powder is The three-dimensional modeling apparatus according to claim 1 , further comprising flowability, packing density, and particle size distribution of the powder.
6. The control unit is The three-dimensional object forming apparatus according to claim 1 , further comprising: a mixing ratio control unit that controls the mixing ratio based on information regarding a modeling condition of the modeling unit.
7. a state estimation unit that estimates information regarding one or more states of the powder, the recovered powder, and the mixed powder, The control unit controls the mixture ratio based on the information estimated by the state estimation unit. The three-dimensional object forming apparatus according to claim 1 .
8. a photographing unit that photographs a surface of the powder in the modeling unit; determining information regarding one or more states of the powder, the collected powder, and the mixed powder based on the image captured by the imaging unit; The three-dimensional object forming apparatus according to claim 1 .
9. The powder mixing unit has a motor that stirs the mixed powder, The control unit determines information regarding one or more states of the powder, the collected powder, and the mixed powder based on the driving force of the motor. The three-dimensional object forming apparatus according to claim 1 .
10. The 3D modeling device is capable of selecting operations including accuracy, cost, and speed; The control unit determines information regarding one or more states of the powder, the recovered powder, and the mixed powder in response to the selected operation. The three-dimensional object forming apparatus according to claim 1 .
11. A forming unit that forms a layer containing powder; An application unit that applies a modeling liquid to the layer; A recovery unit that recovers at least a portion of the powder as recovered powder; A powder mixing section for generating a mixed powder containing at least the recovered powder; A control unit that controls a mixing ratio of the new powder and the recovered powder based on information about the molding conditions of the forming unit; A three-dimensional modeling apparatus comprising:
12. The three-dimensional object fabrication apparatus according to claim 11 , wherein the powder contains a metal.
13. the forming unit includes a flattening unit that is rotated and scanned along a surface of the powder to flatten the surface and form a powder layer; The molding conditions include any one of a volume of a molded object, a scanning speed of the flat portion, a rotation speed of the flat portion, and a layer thickness of the powder layer. The three-dimensional object forming apparatus according to claim 11.
14. The control unit The three-dimensional object fabrication apparatus according to claim 11 , further comprising: a mixing ratio of the mixed powder being controlled based on information regarding at least one of states of the powder, the collected powder, and the mixed powder.
15. A molding step of forming an object containing metal powder; A recovery step of recovering at least a portion of the powder as recovered powder; A powder mixing step of generating a mixed powder containing at least the recovered powder; A mixing ratio adjustment step of controlling a mixing ratio of the new powder and the recycled powder based on information on at least one of the states of the powder, the recycled powder, and the mixed powder; A three-dimensional modeling method comprising the steps of:
16. A sintering unit that sinters the shaped object, The three-dimensional object forming apparatus according to claim 1 .
17. A molding unit that molds a molded object containing metal powder; A recovery unit that recovers at least a portion of the powder as recovered powder; a powder mixing unit that generates a mixed powder including at least the recovered powder, A control device that controls the mixing ratio of the new powder and the recycled powder based on information regarding at least one or more states of the powder, the recycled powder, and the mixed powder.
18. A recovery apparatus that recovers, as recovered powder, a portion of powder used in a molding apparatus that forms a molded object containing metal powder, the recovery apparatus comprising: A control unit is provided for controlling a mixing ratio of the new powder and the recovered powder based on information on one or more states of at least the powder, the recovered powder, and a mixed powder generated containing at least the recovered powder. Recovery device.
Citation Information
Patent Citations
Material powder for metal additive manufacturing, and method for manufacturing the same
JP2021025062A
Cited By
Process compensation method and system for characteristic evolution of additive manufacturing recovery powder
CN120839093A