Liquid crystal aligning agent, liquid crystal alignment film and production method of the same, liquid crystal element, polymer, and compound
A liquid crystal aligning agent with specific structural units improves liquid crystal alignment, slimming resistance, and seal adhesion, addressing the challenges of external force-induced deterioration in mobile and automotive applications.
Patent Information
- Application Number
- JP2024006946
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-01
AI Technical Summary
Existing liquid crystal elements face challenges in achieving balanced improvements in liquid crystal orientation, mechanical properties such as slimming resistance and vibration resistance, and seal adhesion, particularly in mobile and automotive applications where external forces can cause deterioration in display quality.
A liquid crystal aligning agent containing specific structural units derived from diamines with aromatic ring structures, which form a polymer that enhances liquid crystal alignment, slimming resistance, and seal adhesion when used to create a liquid crystal alignment film through light irradiation treatment.
The solution results in liquid crystal elements with improved alignment, resistance to external forces, and enhanced adhesion, ensuring stable operation in mobile and automotive environments.
Smart Images

Figure 2024132878000001 
Figure 2024132878000002 
Figure 2024132878000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film and a method for producing the same, a liquid crystal element, a polymer, and a compound. [Background technology]
[0002] Liquid crystal elements are used in a wide range of applications, from relatively large display devices such as liquid crystal televisions and information displays to small display devices such as smartphones. The performance of a liquid crystal element is determined by various characteristics such as the alignment of liquid crystals, the magnitude of the pretilt angle, and the voltage holding ratio. In order to improve the performance of liquid crystal elements, improvements have been made to liquid crystal materials as well as liquid crystal alignment films for aligning liquid crystals in a certain direction (see, for example, Patent Document 1 and Patent Document 2).
[0003] Patent Document 1 discloses that, in a liquid crystal aligning agent containing a polyamic acid, which is a reaction product of a tetracarboxylic dianhydride and a diamine, and a derivative thereof, a polyamic acid obtained by using bis(4-aminophenoxy)adipamide as a diamine is contained in the liquid crystal aligning agent. Patent Document 2 discloses that a polyimide obtained by using di-tert-butyl adipoylbis[(4-aminophenethyl)carbamate] as a diamine is contained in the liquid crystal aligning agent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-132326 A [Patent Document 2] JP 2016-145954 A Summary of the Invention [Problem to be solved by the invention]
[0005] In order to meet the demand for higher resolution in recent years, further improvements in the liquid crystal alignment properties of liquid crystal elements have been made. In addition, in recent years, importance has been attached to the mechanical properties of liquid crystal elements, and there is a demand for a well-balanced improvement in the liquid crystal alignment properties and the mechanical properties.
[0006] For example, liquid crystal display devices are rapidly becoming popular for mobile and in-vehicle applications. Liquid crystal elements for mobile applications such as smartphones are required to have excellent display quality, as well as to be resistant to degradation of display quality caused by external forces and to have good touch panel characteristics, i.e., touch panel resistance (also called "slimming resistance").
[0007] In addition, in order to achieve both a larger operating area of the touch panel and a smaller display device, efforts are being made to narrow the frame of liquid crystal display devices. One method for narrowing the frame is to form a liquid crystal alignment film on the entire surface of the substrate, and then apply a sealant onto the liquid crystal alignment film to bond the substrates together. On the other hand, when the sealant is placed on the liquid crystal alignment film, force is likely to be applied to the alignment film portion where the sealant is placed. For this reason, if the mechanical properties of the liquid crystal alignment film or its adhesion to the substrate are poor, the adhesion between the substrates (hereinafter also referred to as "sealing adhesion") will decrease, and there is a concern that the substrates will be more likely to peel off due to the action of an external force or the like.
[0008] Furthermore, in addition to having excellent display quality, liquid crystal elements for in-vehicle use are required to have a property (hereinafter also referred to as "vibration resistance") that makes them less susceptible to degradation of display quality caused by external forces due to vibrations while the vehicle is in motion.
[0009] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a liquid crystal aligning agent which can provide a liquid crystal element having excellent liquid crystal alignment properties, slimming resistance, vibration resistance and seal adhesion. [Means for solving the problem]
[0010] The present invention employs the following means to solve the above problems.
[0011] <1> A liquid crystal aligning agent comprising a polymer [P] containing the following structural unit (U1) and structural unit (U2), and the content ratio of the structural unit (U1) is 5 mol % or more and 45 mol % or less with respect to the total amount of structural units derived from a diamine compound. Structural unit (U1): A structural unit derived from a diamine (D1) having at least one partial structure (A) selected from the group consisting of a ring structure in which two or more monocyclic aromatic rings are directly bonded and a condensed ring structure in which two or more monocyclic aromatic rings are condensed, and in which the total number of monocyclic aromatic rings constituting the partial structure (A) and the number of monocyclic aromatic rings constituting a portion other than the partial structure (A) is 3 or more. Structural unit (U2): A structural unit derived from a diamine (D2) having a partial structure represented by the following formula (1) (excluding those corresponding to the diamine (D1)). [ka] (In formula (1), Ar 1 and Ar 2 are each independently a divalent aromatic ring group. 1 and Z 2 are, independently of each other, a single bond, -NR 1 -, -O-, -S-, -CO-, * 1 -NR 1 -CO-, * 1 -CO-NR 1 -, * 1 -NR 1 -CO-NR 2 -, * 1 -CO-O- or * 1 -O-CO-. However, Z 1 and Z 2 R cannot be a single bond at the same time. 1 R is a monovalent organic group. 2 is a hydrogen atom or a monovalent organic group. 1 " is Ar 1 Or Ar 2 It represents a bond with L. 1 -NR 3-, -O-, -S-, -CO-, * 2 -NR 3 -CO-, * 2 -CO-NR 3 -, -NR 3 -CO-NR 4 -, * 2 -CO-O- or * 2 -O-CO-. 3 and R 4 are each independently a hydrogen atom or a monovalent organic group. 2 " is B 1 B 1 is a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. 2 is a divalent aliphatic hydrocarbon group having 3 to 20 carbon atoms. n is an integer of 0 to 3. When n is 2 or 3, multiple B 1 are the same or different, and multiple L 1 are the same or different. "*" represents a bond.)
[0012] <2> the above <1> A liquid crystal alignment film formed by the liquid crystal alignment agent. <3> the above <1> A method for producing a liquid crystal alignment film, comprising forming a coating film using the liquid crystal alignment agent of the above-mentioned formula (1) and subjecting the coating film to a light irradiation treatment to impart liquid crystal alignment ability. <4> the above <2> A liquid crystal element comprising a liquid crystal alignment film. <5> A polymer which is a polyamic acid, a polyamic acid ester or a polyimide and contains a structural unit derived from a diamine represented by the following formula (4): [ka] (In formula (4), Ar 3 and Ar 4 are each independently a divalent aromatic ring group, provided that Ar 3 and Ar 4 At least one of Z has a biphenyl structure or a fused ring structure. 3 and Z 4 are, independently of each other, a single bond, -NR 5 -, -O-, -S-, -CO-, * 3 -NR 5 -CO-, * 3-CO-NR 5 -, -NR 5 -CO-NR 6 -, * 3 -CO-O- or * 3 -O-CO-. 5 and R 6 are each independently a hydrogen atom or a monovalent organic group. 3 " is Ar 3 Or Ar 4 It represents a bond with L. 2 -NR 7 -, -O-, -S-, -CO-, * 4 -NR 7 -CO-, * 4 -CO-NR 7 -, -NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-. 7 and R 8 are each independently a hydrogen atom or a monovalent organic group. 4 " is B 3 B 3 and B. 4 are each independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. m1 is an integer of 1 to 3. When m1 is 2 or 3, multiple B 3 are the same or different, and multiple L 2 are the same or different.) <6> A diamine represented by the above formula (4). Effect of the Invention
[0013] According to the liquid crystal aligning agent of the present invention, a liquid crystal element having excellent liquid crystal alignment properties, slimming resistance, vibration resistance and seal adhesion can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Liquid crystal alignment agent Hereinafter, each component contained in the liquid crystal aligning agent of the present disclosure and other components that are optionally blended as necessary will be described.
[0015] In this specification, the term "hydrocarbon group" includes chain-shaped hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. The term "chain-shaped hydrocarbon group" refers to a straight-chain hydrocarbon group and a branched hydrocarbon group that do not include a cyclic structure in the main chain and are composed only of a chain structure. However, the chain-shaped hydrocarbon group may be saturated or unsaturated. The term "alicyclic hydrocarbon group" refers to a hydrocarbon group that includes only an alicyclic hydrocarbon structure as a ring structure and does not include an aromatic ring structure. However, the alicyclic hydrocarbon group does not necessarily have to be composed only of an alicyclic hydrocarbon structure, and also includes those that have a chain structure as a part of it. The term "aromatic hydrocarbon group" refers to a hydrocarbon group that includes an aromatic ring structure as a ring structure. However, the aromatic hydrocarbon group does not necessarily have to be composed only of an aromatic ring structure, and may include a chain structure or an alicyclic hydrocarbon structure as a part of it. The term "aliphatic hydrocarbon group" refers to a chain-shaped hydrocarbon group and an alicyclic hydrocarbon group. The term "aromatic ring" refers to an aromatic hydrocarbon ring and an aromatic heterocycle. The term "organic group" refers to an atomic group formed by removing any hydrogen atom from a carbon-containing compound (i.e., an organic compound).
[0016] The liquid crystal alignment agent of the present disclosure contains a polymer [P] that includes a structural unit (U1) having a specific aromatic ring structure and a structural unit (U2) having a specific aliphatic structure. The polymer [P] contained in the liquid crystal alignment agent of the present disclosure and components that are blended as necessary will be described below.
[0017] <Polymer [P]> Structural unit (U1) The structural unit (U1) of the polymer [P] is a structural unit derived from a diamine (D1) having at least one partial structure (A) selected from the group consisting of a ring structure in which two or more monocyclic aromatic rings are directly linked and a fused ring structure in which two or more monocyclic aromatic rings are fused, and in which the total number of the monocyclic aromatic rings constituting the partial structure (A) and the number of the monocyclic aromatic rings constituting a portion other than the partial structure (A) is 3 or more.
[0018] The monocyclic aromatic ring constituting the partial structure (A) may be an aromatic hydrocarbon ring or an aromatic heterocycle, specific examples of which include a benzene ring, a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a furan ring, and a thiophene ring.
[0019] Of the partial structure (A), the ring structure in which two or more monocyclic aromatic rings are directly linked is preferably a biphenyl ring structure or a triphenyl ring structure, and more preferably a biphenyl ring structure, from the viewpoints of ease of synthesis of the diamine (D1) and the interaction with the liquid crystal.
[0020] The condensed ring structure in which two or more monocyclic aromatic rings are condensed has a ring structure in which two or more monocyclic aromatic rings are bonded by sharing two or more atoms. Specific examples thereof include a naphthalene ring structure, an anthracene ring structure, a phenanthrene ring structure, a quinoline ring structure, an isoquinoline ring structure, an acridine ring structure, a benzofuran ring structure, and a benzothiophene ring structure. From the viewpoint of ease of synthesis of the diamine (D1) and interaction with liquid crystal, the condensed ring structure of the structural unit (U1) is preferably a naphthalene ring structure or an anthracene ring structure. In the condensed ring structure in which two or more monocyclic aromatic rings are condensed, for example, the number of monocyclic aromatic rings (specifically, benzene rings) constituting the naphthalene ring structure is two, and the number of monocyclic aromatic rings (specifically, benzene rings) constituting the anthracene ring structure is three.
[0021] From the viewpoint of the ease of synthesis of the diamine (D1) and the interaction with the liquid crystal, the partial structure (A) is preferably at least one selected from the group consisting of a biphenyl ring structure, a triphenyl ring structure, a naphthalene ring structure, an anthracene ring structure, a phenanthrene ring structure, a quinoline ring structure, an isoquinoline ring structure, an acridine ring structure, a benzofuran ring structure, and a benzothiophene ring structure, more preferably at least one selected from the group consisting of a biphenyl ring structure, a triphenyl ring structure, a naphthalene ring structure, an anthracene ring structure, and a phenanthrene ring structure, and even more preferably at least one selected from the group consisting of a biphenyl ring structure, a naphthalene ring structure, and an anthracene ring structure. The ring constituting the partial structure (A) may have a substituent. Examples of the substituent include an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a halogen atom, and a hydroxyl group.
[0022] The diamine (D1) may further have a monocyclic aromatic ring in a portion different from the partial structure (A). The monocyclic aromatic ring in the diamine (D1) in a portion different from the partial structure (A) may be an aromatic hydrocarbon ring or an aromatic heterocycle. Specific examples of these include a benzene ring, a pyrrole ring, a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a furan ring, and a thiophene ring. Among these, at least one selected from the group consisting of a benzene ring, a pyridine ring, and a pyrimidine ring is preferred, and at least one selected from the group consisting of a benzene ring and a pyridine ring is more preferred. The monocyclic aromatic ring in the diamine (D1) may have a substituent. Examples of the substituent include an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a halogen atom, and a hydroxyl group. When diamine (D1) has a monocyclic aromatic ring in a portion other than the partial structure (A), the number of monocyclic aromatic rings in the portion other than the partial structure (A) is, for example, 1 to 4, and preferably 1 to 3.
[0023] The monocyclic aromatic ring constituting the partial structure (A) and the monocyclic aromatic ring present in a portion other than the partial structure (A) are preferably at least one selected from the group consisting of a benzene ring, a pyrrole ring, a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a furan ring, and a thiophene ring, more preferably at least one selected from the group consisting of a benzene ring, a pyridine ring, a pyrimidine ring, a pyridazine ring, and a pyrazine ring, and even more preferably at least one selected from the group consisting of a benzene ring and a pyridine ring.
[0024] The diamine (D1) may have only one or more partial structures (A) in one molecule, as long as the total number of the monocyclic aromatic rings constituting the partial structure (A) and the monocyclic aromatic rings constituting the part other than the partial structure (A) (hereinafter also referred to as the "number of aromatic rings in the molecule") is 3 or more. For example, when the diamine (D1) has one biphenyl ring structure (a structure in which two benzene rings are directly bonded) as the partial structure (A) in one molecule and one benzene ring structure in a part other than the partial structure (A) in one molecule, the number of aromatic rings in the molecule in this diamine (D1) is 3. In addition, when the diamine (D1) has one naphthalene ring structure (a structure in which two benzene rings are condensed) as the partial structure (A) in one molecule and one benzene ring structure in a part other than the partial structure (A) in one molecule, the number of aromatic rings in the molecule in this diamine (D1) is 3.
[0025] A preferred specific example of the diamine (D1) is at least one selected from the group consisting of the following diamines (D1-1) and (D1-2). Diamine (D1-1): Diamine having two or more partial structures (A) Diamine (D1-2): A diamine having one partial structure (A) and having at least one aromatic ring structure (specifically, a monocyclic aromatic ring) different from the partial structure (A) in a portion different from the partial structure (A). In order to fully improve the slimming resistance, liquid crystal alignment and seal adhesion of a liquid crystal element, it is preferable that the diamine (D1) has a structure that allows the partial structure (A) to be introduced into the main chain of the polymer [P] by having the partial structure (A) in the main chain.
[0026] From the viewpoint of further increasing the slimming resistance of the liquid crystal element, the number of aromatic rings in the molecule of the diamine (D1) is preferably 4 or more. From the viewpoint of ensuring the solubility of the polymer [P], the number of aromatic rings in the molecule of the diamine (D1) is preferably 8 or less, and more preferably 6 or less.
[0027] Specifically, the diamine (D1) preferably has a partial structure represented by the following formula (2). [ka] (In formula (2), Ar 3 and Ar 4 are each independently a divalent aromatic ring group, provided that Ar 3 and Ar 4 At least one of Z has a biphenyl structure or a fused ring structure. 3 and Z 4 are, independently of each other, a single bond, -NR 5 -, -O-, -S-, -CO-, * 3 -NR 5 -CO-, * 3 -CO-NR 5 -, -NR 5 -CO-NR 6 -, * 3 -CO-O- or * 3 -O-CO-. 5 and R 6 are each independently a hydrogen atom or a monovalent organic group. 3 " is Ar 3 Or Ar 4 It represents a bond with L. 2 -NR 7 -, -O-, -S-, -CO-, * 4 -NR 7 -CO-, * 4 -CO-NR7 -, -NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-. 7 and R 8 are each independently a hydrogen atom or a monovalent organic group. 4 " is B 3 B 3 and B. 4 are each independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. m is an integer of 0 to 3. When m is 2 or 3, multiple B 3 are the same or different, and multiple L 2 are the same or different. "*" represents a bond.)
[0028] In the above formula (2), Ar 3 Or Ar 4 Examples of the divalent aromatic ring group represented by the formula (I) include substituted or unsubstituted aromatic hydrocarbon groups and aromatic heterocyclic groups. 3 Or Ar 4 When Ar has a substituent in the aromatic ring portion, the substituent includes an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a hydroxy group, a halogen atom, and the like. 3 Or Ar 4 is preferably a substituted or unsubstituted aromatic hydrocarbon group, or a substituted or unsubstituted nitrogen-containing aromatic heterocyclic group, and more preferably a substituted or unsubstituted aromatic hydrocarbon group.
[0029] Ar 3 Or Ar 4 Specific examples of the divalent aromatic ring group represented by the formula (I) include, as the aromatic hydrocarbon group, a group obtained by removing any two hydrogen atoms bonded to a carbon atom constituting each of a benzene ring, a biphenyl ring, a naphthalene ring, and an anthracene ring; and, as the nitrogen-containing aromatic heterocyclic group, a group obtained by removing any two hydrogen atoms bonded to a carbon atom constituting each of a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a quinoline ring, an isoquinoline ring, and an acridine ring. 3 Or Ar4 When the divalent aromatic ring group represented by the formula (I) has a substituent, examples of the substituent include a monovalent organic group having 1 to 6 carbon atoms, a halogen atom, a hydroxy group, etc. Specific examples of the organic group having 1 to 6 carbon atoms include an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a protected amino group having 1 to 6 carbon atoms, an alkoxyalkyl group having 1 to 6 carbon atoms, etc.
[0030] Ar is preferred because it can improve the slimming resistance, vibration resistance, seal adhesion, and liquid crystal alignment of liquid crystal elements. 3 Or Ar 4 Among them, the divalent aromatic ring group represented by Ar 3 and Ar 4 It is preferable that one of the above is a group in which two hydrogen atoms have been removed from a ring portion of a substituted or unsubstituted benzene ring, biphenyl ring, naphthalene ring, or anthracene ring, and the other is a group in which two hydrogen atoms have been removed from a ring portion of a substituted or unsubstituted biphenyl ring, naphthalene ring, or anthracene ring.
[0031] Z 3 or Z 4 Ga-NR 5 -, * 3 -NR 5 -CO-, * 3 -CO-NR 5 -OR-NR 5 -CO-NR 6 -If R 5 or R 6 Examples of the monovalent organic group represented by the formula (I) include a monovalent hydrocarbon group having 1 to 10 carbon atoms and a monovalent leaving group. Examples of the monovalent hydrocarbon group having 1 to 10 carbon atoms include a monovalent chain hydrocarbon group having 1 to 10 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 10 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms. Among these, an alkyl group, a cyclohexyl group, or a phenyl group having 1 to 6 carbon atoms is preferred, and from the viewpoint of further increasing the film density, an alkyl group having 1 to 3 carbon atoms is more preferred.
[0032] A leaving group is a group that is released by heat or light and is replaced by a hydrogen atom. R 5 or R 6The monovalent leaving group represented by the following formula (R) is preferably a group which is released by heat and is replaced with a hydrogen atom (hereinafter, also referred to as a "thermally releasing group"). 5 or R 6 is a thermally detachable group, it can be detached during the process of forming a liquid crystal alignment film by applying a liquid crystal alignment agent to a substrate and heating it, which is preferable in terms of simplifying the process. From the viewpoint of causing detachment during the process of forming a liquid crystal alignment film, it is preferable that the thermally detachable group is a group that decomposes at a temperature of 120 to 300° C. and is replaced with a hydrogen atom.
[0033] Specific examples of the leaving group include a tert-butoxycarbonyl group (Boc group), a benzyloxycarbonyl group, a 1,1-dimethyl-2-haloethyloxycarbonyl group, an allyloxycarbonyl group, a 2-(trimethylsilyl)ethoxycarbonyl group, a 9-fluorenylmethyloxycarbonyl group, etc. Among these, the Boc group is preferred because it has excellent thermal releasability and can reduce the amount of the removed structure remaining in the film.
[0034] R 5 and R 6 From the viewpoint of increasing the solubility of the polymer [P], is preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms or a monovalent leaving group, more preferably an alkyl group having 1 to 3 carbon atoms or a monovalent leaving group, and even more preferably a monovalent leaving group.
[0035] When a photo-alignment site (preferably a cyclobutane ring structure) is introduced into the main chain of the polymer [P], from the viewpoint of enhancing the photoreactivity of the polymer [P], Z 3 and Z 4 is Z 3 or Z 4 The aromatic ring group (Ar 3 , Ar 4 ) is preferably an electron donating group that increases the electron density of Z 3 and Z 4 At least one of the groups is -O-, -S- or -NR 56 -(R 56 is a hydrogen atom or a monovalent organic group. 3In the case of R 5 and Z 4 In the case of R 6 It is preferable that the aryl group is -O-, and it is more preferable that the aryl group is -O-. 3 and Z 4 Both are -O-, -S- or -NR 56 It is more preferable that it is -, and even more preferable that it is -O-.
[0036] B 3 Or B 4 Examples of the divalent aliphatic hydrocarbon group represented by the formula (I) include a chain hydrocarbon group having 1 to 20 carbon atoms and an alicyclic hydrocarbon group having 3 to 20 carbon atoms. Of these, examples of the chain hydrocarbon group having 1 to 20 carbon atoms include a linear or branched saturated chain hydrocarbon group having 1 to 20 carbon atoms and a linear or branched unsaturated chain hydrocarbon group having 2 to 20 carbon atoms. The alicyclic hydrocarbon group having 3 to 20 carbon atoms may be saturated or unsaturated, and may be monocyclic or polycyclic. B 3 Or B 4 is an alicyclic hydrocarbon group, the alicyclic hydrocarbon group is preferably a monocyclic saturated alicyclic hydrocarbon group, and examples thereof include groups in which two hydrogen atoms have been removed from the ring portion of each of a cyclopentane ring and a cyclohexane ring.
[0037] B 3 Or B 4 Among these, a divalent linear or branched chain hydrocarbon group having 1 to 10 carbon atoms is preferred, and a linear alkanediyl group having 1 to 10 carbon atoms is more preferred, because the divalent aliphatic hydrocarbon group represented by the formula (I) can increase the film density and form a liquid crystal alignment film that is highly effective in improving slimming resistance, seal adhesion, and voltage retention characteristics of a liquid crystal element. 3 and B. 4 From the viewpoint of obtaining a liquid crystal element exhibiting good liquid crystal alignment while sufficiently improving slimming resistance and seal adhesion, the number of carbon atoms is preferably 8 or less, more preferably 5 or less, even more preferably 3 or less, and even more preferably 1 or 2.
[0038] L 2 Ga-NR 7-, * 4 -NR 7 -CO-, * 4 -CO-NR 7 -OR-NR 7 -CO-NR 8 -If R 7 or R 8 Specific and preferred examples of the monovalent organic group represented by the formula (I) are as described above for R 5 or R 6 Examples of the monovalent organic group include the same groups as those described above for the monovalent organic group represented by the following formula: m is preferably an integer of 0 to 2, and more preferably 0 or 1, from the viewpoint of obtaining a liquid crystal element that exhibits good liquid crystal alignment while sufficiently enhancing the effects of improving slimming resistance and seal adhesion.
[0039] As the diamine (D1), there may be mentioned Ar 3 and Ar 4 A compound having one primary amino group bonded to each of the following can be preferably used. Specific examples of the diamine (D1) include compounds represented by the following formulae (d1-1) to (d1-19). [ka] [ka] (In formulas (d1-1) to (d1-8) and formulas (d1-14) to (d1-19), r is an integer of 1 to 10.)
[0040] Among the compounds represented by the above formulae (d1-1) to (d1-19), the compounds represented by the above formulae (d1-1), (d1-2), (d1-8) to (d1-9), (d1-13) to (d1-14) and (d1-16) correspond to diamines having a ring structure in which two or more monocyclic aromatic rings are directly linked as partial structure (A). The compounds represented by the above formulae (d1-3) to (d1-7), (d1-10) to (d1-12), (d1-15) and (d1-17) to (d1-19) correspond to diamines having a condensed ring structure in which two or more monocyclic aromatic rings are condensed as partial structure (A). Regarding the number of aromatic rings in the molecule, for example, the compound represented by the above formula (d1-1) has 3 aromatic rings, and the compound represented by the above formula (d1-4) has 4 aromatic rings. The compound represented by the above formula (d1-8) has 3 aromatic rings, and the compound represented by the above formula (d1-12) has 4 aromatic rings.
[0041] The content of the structural unit (U1) in the polymer [P] is 5 mol% or more and 45 mol% or less with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P]. If the content of the structural unit (U1) is less than 5 mol% with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P], the effect of improving the liquid crystal alignment and the seal adhesion of the liquid crystal element cannot be sufficiently obtained, and if it exceeds 45 mol%, the effect of improving the liquid crystal alignment of the liquid crystal element cannot be sufficiently obtained. From the viewpoint of improving the liquid crystal alignment and the seal adhesion of the liquid crystal element in a well-balanced manner, the content of the structural unit (U1) is preferably 10 mol% or more, more preferably 15 mol% or more, and even more preferably 20 mol% or more with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P]. In addition, the content of the structural unit (U1) is preferably 40 mol% or less, more preferably 35 mol% or less with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P]. The structural unit (U1) contained in the polymer [P] may be of only one type, or of two or more types.
[0042] Structural unit (U2) The structural unit (U2) of the polymer [P] is a structural unit derived from a diamine (D2) (excluding those corresponding to the diamine (D1)) having a partial structure represented by the following formula (1). [ka] (In formula (1), Ar 1 and Ar 2 are each independently a divalent aromatic ring group. 1 and Z 2 are, independently of each other, a single bond, -NR 1 -, -O-, -S-, -CO-, * 1 -NR 1 -CO-, * 1 -CO-NR 1 -, * 1 -NR 1 -CO-NR 2 -, * 1 -CO-O- or * 1 -O-CO-. However, Z 1 and Z 2 R cannot be a single bond at the same time. 1 R is a monovalent organic group. 2 is a hydrogen atom or a monovalent organic group. 1 " is Ar 1 Or Ar 2 It represents a bond with L. 1 -NR 3 -, -O-, -S-, -CO-, * 2 -NR 3 -CO-, * 2 -CO-NR 3 -, -NR 3 -CO-NR 4 -, * 2 -CO-O- or * 2 -O-CO-. 3 and R 4 are each independently a hydrogen atom or a monovalent organic group. 2 " is B 1 B 1 is a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. 2is a divalent aliphatic hydrocarbon group having 3 to 20 carbon atoms. n is an integer of 0 to 3. "*" represents a bond.
[0043] In the above formula (1), Ar 1 Or Ar 2 The divalent aromatic ring group represented by the formula (2) is 3 Or Ar 4 In order to improve the liquid crystal alignment property of the liquid crystal element, the divalent aromatic ring group represented by the formula (I) may be selected from the groups shown above. 1 Or Ar 2 The divalent aromatic ring group represented by the following formula (I) is preferably a substituted or unsubstituted monocyclic aromatic ring group, more preferably a substituted or unsubstituted phenylene group or pyridinediyl group, and still more preferably a substituted or unsubstituted phenylene group.
[0044] Z 1 or Z 2 Ga-NR 1 -, * 1 -NR 1 -CO-, * 1 -CO-NR 1 -OR-NR 1 -CO-NR 2 -If R 1 or R 2 Examples of the monovalent organic group represented by the formula (2) include a monovalent hydrocarbon group having 1 to 10 carbon atoms and a monovalent leaving group. Specific and preferred examples of these include R 5 or R 6 In the description of the monovalent organic group represented by the following formula, examples thereof include the monovalent hydrocarbon group having 1 to 10 carbon atoms and the monovalent leaving group.
[0045] In order to increase the solubility of the polymer [P], R 1 is preferably a monovalent hydrocarbon group or a monovalent leaving group having 1 to 10 carbon atoms, more preferably an alkyl group or a monovalent leaving group having 1 to 3 carbon atoms, and even more preferably a monovalent leaving group. R 2is preferably a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, or a monovalent leaving group from the viewpoint of further increasing the film density, and is preferably a monovalent hydrocarbon group or a monovalent leaving group having 1 to 10 carbon atoms, more preferably an alkyl group or a monovalent leaving group having 1 to 3 carbon atoms, and even more preferably a monovalent leaving group, from the viewpoint of further increasing the solubility of the polymer [P].
[0046] When a photo-alignment site (preferably a cyclobutane ring structure) is introduced into the main chain of the polymer [P], from the viewpoint of enhancing the photoreactivity of the polymer [P], Z 1 and Z 2 are preferably other than a single bond, and the adjacent aromatic ring groups (Ar 1 , Ar 2 ) is more preferably an electron donating group that increases the electron density of Z 1 and Z 2 At least one of the groups is -O-, -S- or -NR 12 -(R 12 is a hydrogen atom or a monovalent organic group. 1 In the case of R 1 and Z 2 In the case of R 2 ) is preferably -O- or -NR 12 From the above viewpoint, Z 1 and Z 2 Both are -O-, -S- or -NR 12 More preferably, it is -O- or -NR 12 It is even more preferred that -
[0047] B 1 Examples of the divalent aliphatic hydrocarbon group represented by the formula (I) include a chain hydrocarbon group having 1 to 20 carbon atoms and an alicyclic hydrocarbon group having 3 to 20 carbon atoms. 2 Examples of the divalent aliphatic hydrocarbon group represented by the formula (I) include a chain hydrocarbon group having 3 to 20 carbon atoms and an alicyclic hydrocarbon group having 3 to 20 carbon atoms. 1 Or B 2 In the above, specific examples of the divalent chain hydrocarbon group and alicyclic hydrocarbon group include B3 Or B 4 Examples of the groups include the same groups as those exemplified in the description of the above.
[0048] B 1 The divalent aliphatic hydrocarbon group represented by the formula (I) is preferably a divalent linear or branched chain hydrocarbon group having 1 to 10 carbon atoms, more preferably a linear alkanediyl group having 1 to 5 carbon atoms, and even more preferably a linear alkanediyl group having 1 to 3 carbon atoms, in that it can increase the film density and form a liquid crystal alignment film that is highly effective in improving the slimming resistance, seal adhesion, and voltage retention characteristics of a liquid crystal element.
[0049] B 2 From the viewpoint of obtaining a liquid crystal element exhibiting good liquid crystal alignment properties, the divalent aliphatic hydrocarbon group represented by the formula (I) is preferably a divalent linear or branched chain hydrocarbon group having 3 to 10 carbon atoms. In terms of being able to form a liquid crystal alignment film having a high film density and a high effect of improving slimming resistance, seal adhesion, and voltage retention characteristics of the liquid crystal element, the formula (I) is preferably a divalent aliphatic hydrocarbon group represented by the formula (I) in the formula (I). 1 is more preferably a linear alkanediyl group having 3 to 10 carbon atoms. 1 From the viewpoint of obtaining a liquid crystal element exhibiting good liquid crystal alignment while sufficiently improving slimming resistance and seal adhesion, the number of carbon atoms is preferably 8 or less, more preferably 6 or less, and even more preferably 5 or less.
[0050] L 1 Ga-NR 3 -, * 2 -NR 3 -CO-, * 2 -CO-NR 3 -OR-NR 3 -CO-NR 4 -If R 3 or R 4 Specific and preferred examples of the monovalent organic group represented by the formula (I) are as described above for R 5 or R 6 Examples of the monovalent organic group represented by the formula L 1 From the viewpoint of obtaining a liquid crystal element exhibiting good liquid crystal alignment, slimming resistance and seal adhesion, -NR 3 -, -O-, *2 -NR 3 -CO-, -NR 3 -CO-NR 4 -, * 2 -CO-O- or * 2 -O-CO- is preferred, and -NR 3 - is more preferred.
[0051] n is preferably 0 to 2, more preferably 0 or 1, and even more preferably 0, from the viewpoint of obtaining a liquid crystal element that exhibits good liquid crystal alignment while sufficiently enhancing the effect of improving slimming resistance and seal adhesion.
[0052] As the diamine (D2), there may be mentioned Ar 1 and Ar 2 A compound having one primary amino group bonded to each of the following can be preferably used. Specific examples of the diamine (D2) include compounds represented by the following formulas (d2-1) to (d2-14). [ka] (In formulas (d2-1) to (d2-14), k is an integer of 3 to 10. h is an integer of 2 to 10. Boc is a tert-butoxycarbonyl group.)
[0053] The content of the structural unit (U2) in the polymer [P] is preferably 10 mol% or more and 95 mol% or less with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P]. When the content of the structural unit (U2) is 10 mol% or more with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P], it is possible to obtain a liquid crystal element that exhibits good liquid crystal alignment while ensuring slimming resistance and vibration resistance of the liquid crystal element. In addition, when the content of the structural unit (U2) is 95 mol% or less with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P], it is possible to obtain a liquid crystal element that has a well-balanced improvement in slimming resistance, vibration resistance, liquid crystal alignment, and seal adhesion. From this viewpoint, the content of the structural unit (U2) is more preferably 15 mol% or more, more preferably 20 mol% or more, and even more preferably 25 mol% or more with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P]. The content of the structural unit (U2) is more preferably 90 mol % or less, and even more preferably 80 mol % or less, based on the total amount of the structural units derived from the diamine compound contained in the polymer [P]. The structural unit (U2) contained in the polymer [P] may be of one type or of two or more types.
[0054] In addition to the structural unit (U1) and the structural unit (U2), the polymer [P] may further contain a structural unit (hereinafter also referred to as "structural unit (U3)") derived from a diamine (hereinafter also referred to as "diamine (D3)") having a partial structure represented by the following formula (3). The polymer [P] further contains the structural unit (U3), which is advantageous in that a liquid crystal element having more excellent liquid crystal alignment properties can be obtained. [ka] (In formula (3), Ar 5 and Ar 6 are each independently a divalent aromatic ring group. 5 and Z 6 are, independently of each other, a single bond, -NR 9 -, -O-, -S-, -CO-, *5 -NR 9 -CO-, * 5 -CO-NR 9 -, * 5 -CO-O- or * 5 -O-CO-. However, Z 5 and Z 6 R cannot be a single bond at the same time. 9 is a hydrogen atom or a monovalent organic group. 5 " is Ar 5 Or Ar 6 B 5 is a methylene group or an ethylene group. "*" represents a bond.)
[0055] In the above formula (3), Ar 5 Or Ar 6 The divalent aromatic ring group represented by the formula (2) is 3 Or Ar 4 In order to improve the liquid crystal alignment property of the liquid crystal element, the divalent aromatic ring group represented by the formula (I) may be selected from the groups shown above. 5 Or Ar 6 The divalent aromatic ring group represented by the following formula (I) is preferably a substituted or unsubstituted monocyclic aromatic ring group, more preferably a substituted or unsubstituted phenylene group or pyridinediyl group, and still more preferably a substituted or unsubstituted phenylene group.
[0056] Z 5 or Z 6 Ga-NR 9 -, * 5 -NR 9 -CO- or * 5 -CO-NR 9 -If R 9 Examples of the monovalent organic group represented by the formula (2) include a monovalent hydrocarbon group having 1 to 10 carbon atoms and a monovalent leaving group. Specific and preferred examples of these include R 5 or R 6 In the description of the monovalent organic group represented by the formula (I), the monovalent hydrocarbon group having 1 to 10 carbon atoms and the monovalent leaving group are exemplified. From the viewpoint of increasing the solubility of the polymer [P], R 1is preferably a monovalent hydrocarbon group or a monovalent leaving group having 1 to 10 carbon atoms, more preferably an alkyl group or a monovalent leaving group having 1 to 3 carbon atoms, and even more preferably a monovalent leaving group.
[0057] When a photo-alignment site (preferably a cyclobutane ring structure) is introduced into the main chain of the polymer [P], from the viewpoint of enhancing the photoreactivity of the polymer [P], Z 5 and Z 6 is an adjacent aromatic ring group (Ar 5 , Ar 6 ) is preferably an electron donating group that increases the electron density of Z 5 and Z 6 At least one of the groups is -O-, -S- or -NR 9 - is preferred, and -O- or -NR 9 From the above viewpoint, Z 5 and Z 6 Both are -O-, -S- or -NR 9 More preferably, it is -O- or -NR 9 It is even more preferred that -
[0058] As the diamine (D3), there may be mentioned Ar 5 and Ar 6 A compound having one primary amino group bonded to each of the following can be preferably used. Specific examples of the diamine (D3) include compounds represented by the following formulae (d3-1) to (d3-10). [ka]
[0059] When the polymer [P] contains the structural unit (U3), the content of the structural unit (U3) is preferably 1 mol% or more with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P], from the viewpoint of obtaining a sufficient effect of improving the liquid crystal alignment. The content of the structural unit (U3) is more preferably 2 mol% or more, and even more preferably 5 mol% or more with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P]. In addition, the content of the structural unit (U3) is preferably 20 mol% or less, and more preferably 15 mol% or less with respect to the total amount of the structural units derived from the diamine compound contained in the polymer [P], from the viewpoint of suppressing the decrease in slimming resistance, vibration resistance, and seal adhesion of the liquid crystal element. The structural unit (U3) contained in the polymer [P] may be only one type, or may be two or more types.
[0060] The polymer [P] may be a polycondensate of a diamine compound and a carboxylic acid or a derivative thereof. In terms of being able to form a liquid crystal alignment film having high affinity with liquid crystals, high mechanical strength, and excellent voltage retention characteristics, the polymer [P] is preferably a polycondensate of a tetracarboxylic acid derivative and a diamine compound, and more specifically, is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide. Here, the "tetracarboxylic acid derivative" includes tetracarboxylic acid dianhydride, tetracarboxylic acid diester, and tetracarboxylic acid diester dihalide.
[0061] (Polyamic acid) When the polymer [P] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [P]") can be produced by a method of reacting a tetracarboxylic dianhydride with a diamine compound including a diamine (D1) and a diamine (D2).
[0062] Tetracarboxylic acid dianhydride As the tetracarboxylic acid dianhydride used in the synthesis of the polyamic acid [P], a compound known as a tetracarboxylic acid derivative that can be used in the production of polyamic acid, polyamic acid ester, and polyimide can be used. As the tetracarboxylic acid dianhydride used in the synthesis of the polyamic acid [P], for example, an aliphatic tetracarboxylic acid dianhydride, an aromatic tetracarboxylic acid dianhydride, etc. can be mentioned. As the aliphatic tetracarboxylic acid dianhydride, a chain tetracarboxylic acid dianhydride and an alicyclic tetracarboxylic acid dianhydride can be mentioned.
[0063] Specific examples of these include chain tetracarboxylic dianhydrides such as 1,2,3,4-butanetetracarboxylic dianhydride and ethylenediaminetetraacetic dianhydride. Examples of the alicyclic tetracarboxylic dianhydride include 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentane tetracarboxylic dianhydride, and cyclohexane tetracarboxylic dianhydride. Examples of aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, ethylene glycol bisanhydrotrimate, 4,4'-carbonyldiphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 3,3',4,4'-diphenylethertetracarboxylic dianhydride. In addition to the above, the tetracarboxylic dianhydride described in JP-A-2010-97188 can be used. The tetracarboxylic dianhydride can be used alone or in combination of two or more.
[0064] From the viewpoints of the availability of the compound and the ease of production of the polymer, the tetracarboxylic acid dianhydride used in the synthesis of the polyamic acid [P] is preferably at least one selected from the group consisting of 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-butanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, cyclohexanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, pyromellitic dianhydride, and 3,3',4,4'-biphenyltetracarboxylic dianhydride.
[0065] In addition, when a liquid crystal alignment film is formed by a photoalignment method, the tetracarboxylic acid derivative used in the synthesis of the polymer [P] preferably contains a tetracarboxylic acid derivative having a cyclobutane ring structure, and more preferably contains 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride and its derivatives (specifically, tetracarboxylic acid diesters and tetracarboxylic acid diester dihalides). In the synthesis of the polymer [P], the proportion of the tetracarboxylic acid derivative having a cyclobutane ring structure used is preferably 20 mol % or more, more preferably 30 mol % or more, and even more preferably 50 mol % or more, based on the total amount of the tetracarboxylic acid derivative used in the synthesis of the polymer [P].
[0066] Diamine compounds The diamine compounds used in the synthesis of the polyamic acid [P] may be only diamine (D1) and diamine (D2), or only diamine (D1), diamine (D2), and diamine (D3). In addition, when synthesizing the polyamic acid [P], a diamine other than the diamine (D1), diamine (D2), and diamine (D3) (hereinafter, also referred to as "other diamines") may be used in combination as the diamine compound. Examples of other diamines include aliphatic diamines, aromatic diamines, and diaminoorganosiloxanes. Aliphatic diamines include chain diamines and alicyclic diamines.
[0067] Specific examples of other diamines include chain diamines such as m-xylylenediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, and 1,3-bis(aminomethyl)cyclohexane; alicyclic diamines such as 1,4-diaminocyclohexane and 4,4'-methylenebis(cyclohexylamine); Aromatic diamines include dodecanoxydiaminobenzene, tetradecanoxydiaminobenzene, pentadecanoxydiaminobenzene, hexadecanoxydiaminobenzene, octadecanoxydiaminobenzene, cholestanyloxydiaminobenzene, cholesteryloxydiaminobenzene, cholestanyl diaminobenzoate, cholesteryl diaminobenzoate, lanostannyl diaminobenzoate, 3,6-bis(4-aminobenzoyloxy)cholestane, 3,6-bis(4-aminophenoxy)cholestane, 1,1 -bis(4-((aminophenyl)methyl)phenyl)-4-butylcyclohexane, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-heptylcyclohexane, 1,1-bis(4-((aminophenoxy)methyl)phenyl)-4-heptylcyclohexane, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-(4-heptylcyclohexyl)cyclohexane, N-(2,4-diaminophenyl)-4-(4-heptylcyclohexyl)benzamide, the following formula (E-1): [ka] (In formula (E-1), X I and X II are each independently a single bond, -O-, *-COO-, or *-OCO- (wherein "*" represents a bond to the diaminophenyl group). I R is an alkanediyl group having 1 to 3 carbon atoms. II R is a single bond or an alkanediyl group having 1 to 3 carbon atoms. III is an alkyl group, an alkoxy group, a fluoroalkyl group or a fluoroalkoxy group having 1 to 20 carbon atoms. a is 0 or 1. b is an integer of 0 to 3. c is an integer of 0 to 2. d is 0 or 1, provided that 1≦a+b+c≦3. Directing group-containing diamines such as compounds represented by the formula: p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 4,4'-diaminodiphenylamine, 4,4'-diaminodiphenylsulfide, 4-aminophenyl-4'-aminobenzoate, 4,4'-diaminoazobenzene, bis[2-(4-aminophenyl)ethyl]hexanedioic acid, N,N-bis(4-aminophenyl)methylamine, 1,5-diaminonaphthalene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-di Aminobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 9,9-bis(4-aminophenyl)fluorene, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-(p-phenylenediisopropylidene)bisaniline, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis-(4-aminophenyl)-piperazine, 3,5-diaminobenzoic acid, 4,4'-diaminodiphenethylurea, etc.; Examples of diaminoorganosiloxanes include 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, and the like. In addition, the diamines described in JP-A-2010-97188 can also be used.
[0068] In the above formula (E-1), "-X I -(R I -X II ) d Examples of the divalent group represented by "-" include an alkanediyl group having 1 to 3 carbon atoms, -O-, *-COO-, and -O-C2H4-O- (wherein the bond marked with "*" is bonded to a diaminophenyl group). III The two amino groups in the diaminophenyl group are preferably in the 2,4- or 3,5-position relative to the other group.
[0069] Specific examples of the compound represented by formula (E-1) above include the compounds represented by formulas (E-1-1) to (E-1-4) below. [ka]
[0070] In the synthesis of the polyamic acid [P], the proportion of the other diamine used is preferably 70 mol % or less, more preferably 60 mol % or less, even more preferably 50 mol % or less, and even more preferably 30 mol % or less, based on the total amount of the diamine compounds used in the synthesis of the polyamic acid [P]. As the other diamine, one type may be used alone, or two or more types may be used in combination.
[0071] (Synthesis of polyamic acid) The polyamic acid [P] can be obtained by reacting a tetracarboxylic dianhydride with a diamine compound, optionally together with a molecular weight modifier. In the synthesis reaction of the polyamic acid [P], the ratio of the tetracarboxylic dianhydride to the diamine compound is preferably such that the acid anhydride group of the tetracarboxylic dianhydride is 0.2 to 2 equivalents per equivalent of the amino group of the diamine compound. Examples of the molecular weight modifier include acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride, monoamine compounds such as aniline, cyclohexylamine, and n-butylamine, and monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate. The ratio of the molecular weight modifier to be used is preferably 20 parts by mass or less per 100 parts by mass of the total of the tetracarboxylic dianhydride and diamine compound used.
[0072] The synthesis reaction of the polyamic acid [P] is preferably carried out in an organic solvent. The reaction temperature is preferably -20°C to 150°C, and the reaction time is preferably 0.1 to 24 hours. Examples of the organic solvent used in the reaction include aprotic polar solvents, phenolic solvents, alcoholic solvents, ketone solvents, ester solvents, ether solvents, halogenated hydrocarbons, and hydrocarbons. Specific examples of these include one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphortriamide, m-cresol, xylenol, and halogenated phenols, or a mixture of one or more of these with another organic solvent (e.g., butyl cellosolve, diethylene glycol diethyl ether, etc.). The amount of the organic solvent used is preferably an amount such that the total amount of the tetracarboxylic dianhydride and the diamine is 0.1 to 50 mass% based on the total amount of the reaction solution.
[0073] In this manner, a polymer solution in which the polyamic acid [P] is dissolved is obtained. This polymer solution may be used as it is for the preparation of a liquid crystal alignment agent, or the polyamic acid [P] contained in the polymer solution may be isolated and then used for the preparation of a liquid crystal alignment agent.
[0074] Polyamic acid ester When the polymer [P] is a polyamic acid ester, the polyamic acid ester (hereinafter also referred to as "polyamic acid ester [P]") can be obtained, for example, by a method of reacting a polyamic acid [P] with an esterifying agent, a method of reacting a tetracarboxylic acid diester with a diamine compound containing diamine (D1) and diamine (D2), or a method of reacting a tetracarboxylic acid diester dihalide with a diamine compound containing diamine (D1) and diamine (D2). The polyamic acid ester [P] may have only an amic acid ester structure, or may be a partially esterified product in which an amic acid structure and an amic acid ester structure coexist. The reaction solution in which the polyamic acid ester [P] is dissolved may be used as it is for the preparation of a liquid crystal alignment agent, or the polyamic acid ester [P] contained in the reaction solution may be isolated and then used for the preparation of a liquid crystal alignment agent.
[0075] Polyimide When the polymer [P] is a polyimide, the polyimide (hereinafter also referred to as "polyimide [P]") can be obtained, for example, by dehydrating and cyclizing the polyamic acid [P] synthesized as described above to convert it into an imidized product. The polyimide [P] may be a complete imidized product in which all of the amic acid structures of the precursor polyamic acid [P] are dehydrated and cyclized, or a partial imidized product in which only a part of the amic acid structures are dehydrated and cyclized, and an amic acid structure and an imide ring structure coexist. The polyimide [P] preferably has an imidization rate of 20 to 99%, more preferably 30 to 90%. The imidization rate is the ratio of the number of imide ring structures to the total number of amic acid structures and the number of imide ring structures of the polyimide, expressed as a percentage. Here, a part of the imide rings may be isoimide rings.
[0076] The dehydration ring-closing of the polyamic acid [P] is preferably carried out by dissolving the polyamic acid [P] in an organic solvent, adding a dehydrating agent and a dehydration ring-closing catalyst to the solution, and heating as necessary. In this method, the dehydrating agent may be, for example, an acid anhydride such as acetic anhydride, propionic anhydride, or trifluoroacetic anhydride. The amount of the dehydrating agent used is preferably 0.01 to 20 moles per mole of the amic acid structure of the polyamic acid [P]. The dehydration ring-closing catalyst may be, for example, a tertiary amine such as pyridine, collidine, lutidine, or triethylamine. The amount of the dehydration ring-closing catalyst used is preferably 0.01 to 10 moles per mole of the dehydrating agent used. The organic solvent used in the dehydration ring-closing reaction may be the organic solvent exemplified as the one used in the synthesis of the polyamic acid [P]. The reaction temperature in the dehydration ring-closing reaction is preferably 0 to 180° C. The reaction time is preferably 1.0 to 120 hours. The reaction solution containing the polyimide [P] may be used for the preparation of a liquid crystal aligning agent as it is, or the polyimide [P] may be isolated and then used for the preparation of a liquid crystal aligning agent.
[0077] The solution viscosity of the polymer [P] used in preparing the liquid crystal alignment agent is preferably 10 to 800 mPa·s when made into a 10% by mass solution, and more preferably 15 to 500 mPa·s. The solution viscosity (mPa·s) is a value measured at 25°C using an E-type rotational viscometer for a 10% by mass polymer solution prepared using a good solvent for the polymer [P] (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).
[0078] The weight average molecular weight (Mw) of the polymer [P] measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, more preferably 2,000 to 300,000. The molecular weight distribution (Mw / Mn) expressed as the ratio of Mw to the number average molecular weight (Mn) measured by GPC in terms of polystyrene is preferably 7 or less, more preferably 5 or less.
[0079] The content of the polymer [P] in the liquid crystal alignment agent is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of the total amount of solids contained in the liquid crystal alignment agent (i.e., the total mass of the components other than the solvent of the liquid crystal alignment agent). In addition, when preparing the liquid crystal alignment agent, one type of polymer [P] may be used alone, or two or more types may be used in combination.
[0080] <Other ingredients> The liquid crystal aligning agent of the present disclosure may contain, in addition to the polymer [P], components different from the polymer [P] (hereinafter also referred to as "other components"), if necessary.
[0081] Polymer [Q] The liquid crystal alignment agent of the present disclosure may further contain a polymer (hereinafter also referred to as "polymer [Q]") that does not contain either the structural unit (U1) or the structural unit (U2) as a polymer component. The main skeleton of the polymer [Q] is not particularly limited. Examples of the polymer [Q] include polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, polyester, polyenamine, polyurea, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivative, polyacetal, and addition polymer. Examples of the addition polymer include (meth)acrylic polymer, styrene polymer, maleimide polymer, and styrene-maleimide copolymer.
[0082] From the viewpoint of obtaining a highly reliable liquid crystal element, the polymer [Q] is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, and addition polymer, among the above. From the viewpoint of easily distributing the polymer [P] in the upper layer, sufficiently enhancing the effect of improving the liquid crystal alignment, and easily adjusting the electrical properties, the polymer [Q] is particularly preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.
[0083] When the polymer [Q] is contained in the liquid crystal alignment agent, the content of the polymer [Q] is preferably 1 part by mass or more, more preferably 2 parts by mass or more, based on 100 parts by mass of the total amount of the polymer [P] and the polymer [Q]. The content of the polymer [Q] is preferably 95 parts by mass or less, more preferably 90 parts by mass or less, based on 100 parts by mass of the total amount of the polymer [P] and the polymer [Q]. As the polymer [Q], one type can be used alone, or two or more types can be used in combination.
[0084] Crosslinking agent The liquid crystal aligning agent of the present disclosure may further contain a crosslinking agent as another component. Examples of the crosslinking agent include a group having a polymerizable carbon-carbon bond, a cyclic ether group, a cyclic thioether group, an isocyanate group, a protected isocyanate group, a methylol group, a protected methylol group, a hydroxyalkylamide group, a protected hydroxyalkylamide group, a cyclic carbonate group, a group "-CR 9 =CR 10 -R 11 -" (but R 9 R is a monovalent organic group that is eliminated by reaction with an amino group. 10 is a hydrogen atom or an alkyl group, R 11 is an electron-withdrawing group), a compound having at least one crosslinkable group selected from the group consisting of a silanol group, an amino group, a protected amino group, and an alkoxysilyl group (hereinafter also referred to as "compound [C]").
[0085] Among the above-mentioned crosslinkable groups, examples of groups having a polymerizable carbon-carbon bond include a (meth)acryloyl group, a maleimide group, an alkenyl group, a vinylphenyl group, a vinyl ether group, and a 3-methylenetetrahydrofuran-2(3H)-one-5-yl group. 9 =CR 10 -R 11 -" in R 9 Examples of the monovalent organic group represented by the formula (1) include an alkoxy group having 1 to 5 carbon atoms, a pyrrolidone-1-yl group, and a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom). 11 Examples of the electron-withdrawing group include a carbonyl group and a sulfonyl group.
[0086] From the viewpoints of improving the liquid crystal alignment property, voltage retention property and film strength of a liquid crystal element in a well-balanced manner and suppressing a decrease in reworkability, the number of crosslinkable groups that compound [C] has in one molecule is preferably 2 to 12, more preferably 2 to 10. From the viewpoint of storage stability, the molecular weight of compound [C] is preferably 3,000 or less, more preferably 2,000 or less, and even more preferably 1,000 or less.
[0087] As the compound [C], among the above, a compound having a functional group capable of reacting with an amino group can be preferably used, and among them, a compound having a total of two or more of at least one type selected from the group consisting of a cyclic ether group, a hydroxyalkylamide group, a protected hydroxyalkylamide group, a methylol group, a protected methylol group, and a protected isocyanate group in one molecule can be more preferably used.
[0088] Specific examples of the compound [C] include compounds having a polymerizable carbon-carbon bond, such as ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and compounds represented by the following formulae (c-1) to (c-6): Examples of compounds having a cyclic (thio)ether group include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, triglycidyl isocyanurate, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N-diglycidyl-benzylamine, N,N-diglycidyl-aminomethylcyclohexane, and N,N-diglycidyl-cyclohexylamine; Examples of the compound having an isocyanate group or a protected isocyanate group include compounds represented by the following formulas (c-7) to (c-11): Examples of the compound having a methylol group or a protected methylol group include compounds represented by the following formulas (c-12) to (c-17): Examples of compounds having a hydroxyalkylamide group or a protected hydroxyalkylamide group include compounds represented by the following formulae (c-18) to (c-20): Examples of the compound having a cyclic carbonate group include compounds represented by the following formulas (c-21) and (c-22): Base “-CR 9 =CR 10 -R 11 -" includes, for example, compounds represented by each of the following formulas (c-23) to (c-29); As the compound having an amino group or a protected amino group, the compounds represented by each of the following formulae (c-30) to (c-33) are mentioned; Examples of compounds having an alkoxysilyl group or a silanol group include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, vinyltriethoxysilane, and trimethoxysilylpropylsuccinic anhydride. [ka] [ka] [ka] (In formula (c-7) and formula (c-8), R 13 is a tert-butoxy group.) [ka] (In formula (c-16), Ac is an acetyl group.) [ka] [ka] [ka] [ka]
[0089] When the liquid crystal alignment agent of the present disclosure contains a crosslinking agent, the content ratio is preferably 0.2 parts by mass or more relative to 100 parts by mass of the total amount of the polymer components contained in the liquid crystal alignment agent (i.e., the total amount of the polymer [P] and the polymer [Q]) from the viewpoint of increasing the seal adhesion of the liquid crystal element and improving the liquid crystal alignment and voltage retention characteristics. The content ratio of the crosslinking agent is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the total amount of the polymer components. In addition, from the viewpoint of satisfying the liquid crystal alignment and voltage retention characteristics of the liquid crystal element, the storage stability of the liquid crystal alignment agent, and the reworkability of the liquid crystal alignment film, the content ratio of the crosslinking agent is preferably 20 parts by mass or less, and more preferably 15 parts by mass or less, relative to 100 parts by mass of the total amount of the polymer components. As the crosslinking agent, one type may be used alone, or two or more types may be used in combination.
[0090] ·solvent The liquid crystal aligning agent of the present disclosure is prepared as a liquid composition in which the polymer [P] and other components used as necessary are preferably dispersed or dissolved in a suitable solvent.
[0091] As the solvent, an organic solvent is preferably used.Specific examples thereof include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,2-dimethyl-2-imidazolidinone, 1,3-dimethyl-2-imidazolidinone, phenol, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone, diacetone alcohol, 1-hexanol, 2-hexanol, propane-1,2-diol, 3-methoxy-1-butanol, ethylene glycol monomethyl ether, methyl lactate, ethyl lactate, butyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, ethyl acetoacetate, ethyl propionate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol-n-propyl ether, and ethylene glycol-i-propyl ether. Examples of the solvent include ethylene glycol-n-butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisopentyl ether, ethylene carbonate, propylene carbonate, propylene glycol monomethyl ether (PGME), diethylene glycol diethyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol diacetate, cyclopentanone, cyclohexanone, etc. As the solvent, one type can be used alone or two or more types can be mixed and used.
[0092] Other components contained in the liquid crystal alignment agent include, in addition to the above, for example, a crosslinking agent, an antioxidant, a metal chelate compound, a curing accelerator, a surfactant, a filler, a dispersant, a photosensitizer, etc. The blending ratio of the other components can be appropriately selected according to each compound within a range that does not impair the effects of the present disclosure.
[0093] The solid content concentration in the liquid crystal alignment agent (the ratio of the total mass of the components other than the solvent of the liquid crystal alignment agent to the total mass of the liquid crystal alignment agent) is appropriately selected in consideration of viscosity, volatility, etc., and is preferably in the range of 1 to 10 mass %. If the solid content concentration is 1 mass % or more, it is preferable in that the thickness of the coating film can be sufficiently ensured and a liquid crystal alignment film showing better liquid crystal alignment properties can be obtained. On the other hand, if the solid content concentration is 10 mass % or less, the coating film can be made to an appropriate thickness, and a liquid crystal alignment film showing good liquid crystal alignment properties tends to be easily obtained. In addition, the viscosity of the liquid crystal alignment agent becomes appropriate, and the coating property tends to be good.
[0094] Polymers and Compounds According to the present disclosure, there is provided a polymer which is a polyamic acid, a polyamic acid ester, or a polyimide and which includes a structural unit derived from a diamine represented by the following formula (4). Also, according to the present disclosure, there is provided a diamine represented by the following formula (4). [ka] (In formula (4), Ar 3 and Ar 4 are each independently a divalent aromatic ring group, provided that Ar 3 and Ar 4 At least one of Z has a biphenyl structure or a fused ring structure. 3 and Z 4 are, independently of each other, a single bond, -NR 5 -, -O-, -S-, -CO-, * 3 -NR 5 -CO-, * 3 -CO-NR 5 -, -NR 5 -CO-NR 6 -, * 3 -CO-O- or *3 -O-CO-. 5 and R 6 are each independently a hydrogen atom or a monovalent organic group. 3 " is Ar 3 Or Ar 4 It represents a bond with L. 2 -NR 7 -, -O-, -S-, -CO-, * 4 -NR 7 -CO-, * 4 -CO-NR 7 -, -NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-. 7 and R 8 are each independently a hydrogen atom or a monovalent organic group. 4 " is B 3 B 3 and B. 4 are each independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. m1 is an integer of 1 to 3. When m1 is 2 or 3, multiple B 3 are the same or different, and multiple L 2 are the same or different.)
[0095] All of these compounds are suitable as materials for forming a liquid crystal alignment film. In the above formula (4), m1 is preferably 1 or 2, more preferably 1, from the viewpoint of obtaining a liquid crystal element that exhibits good liquid crystal alignment while sufficiently enhancing the effect of improving slimming resistance and seal adhesion. Ar 3 , Ar 4 , Z 3 , Z 4 , L 2 , B 3 and B. 4 Specific and preferred examples of Ar 3 , Ar 4 , Z 3 , Z 4 , L 2 , B 3 and B. 4Specific examples of the compound represented by formula (4) include the compounds represented by formulas (d1-9) to (d1-13) above.
[0096] The synthesis method of the diamine represented by the above formula (4) is not particularly limited, and it can be synthesized by appropriately combining standard methods in organic chemistry. One example is a method in which a dinitro compound having a nitro group instead of a primary amino group in the diamine represented by the above formula (4) is synthesized, and then the nitro group of the obtained dinitro compound is aminated using an appropriate reduction system. The method for synthesizing the dinitro compound can be appropriately selected depending on the target compound. For example, as described in the examples below, -Ar 3 -Z 3 A compound having a partial structure represented by - and a nitro group, -(B 3 -L 2 ) m1 -B 4 - can be obtained by reacting a compound having a partial structure represented by the formula:
[0097] The reduction reaction of the dinitro compound can be preferably carried out in an organic solvent using a catalyst such as palladium carbon, platinum carbon, zinc, iron, tin, nickel, etc. Examples of the organic solvent used here include one or more of toluene, tetrahydrofuran, N,N-dimethylformamide, alcohols, etc. However, the synthesis procedure of the diamine represented by the above formula (4) is not limited to the above method.
[0098] <Liquid crystal alignment film and liquid crystal element> The liquid crystal alignment film of the present disclosure is manufactured by the liquid crystal alignment agent prepared as described above. The liquid crystal element of the present disclosure includes a liquid crystal alignment film formed by using the liquid crystal alignment agent described above. The driving method of the liquid crystal in the liquid crystal element is not particularly limited, and can be applied to various modes such as TN (Twisted Nematic) type, STN (Super-twisted Nematic) type, VA (Vertical Alignment) type (including VA-MVA type, VA-PVA type, etc.), IPS (In-Plane Switching) type, FFS (Fringe Field Switching) type, OCB (Optically Compensated Bend) type, PSA (Polymer Sustained Alignment) type, etc. The liquid crystal element can be manufactured by a method including, for example, the following steps 1 to 3. In step 1, the substrate used differs depending on the desired operation mode. Steps 2 and 3 are common to each operation mode.
[0099] <Step 1: Formation of coating film> First, a liquid crystal alignment agent is applied onto a substrate, and a coating film is formed on the substrate, preferably by heating the applied surface. As the substrate, for example, a transparent substrate made of glass such as float glass or soda glass; or plastic such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, or poly(alicyclic olefin) can be used. When manufacturing a TN-type, STN-type, or VA-type liquid crystal element, two substrates on which a patterned transparent conductive film is provided are used. On the other hand, when manufacturing an IPS-type or FFS-type liquid crystal element, a substrate on which an electrode patterned in a comb-tooth shape is provided and an opposing substrate on which no electrode is provided are used. As the transparent conductive film, a NESA film (registered trademark of US PPG) made of tin oxide (SnO2), an ITO film made of indium oxide-tin oxide (In2O3-SnO2), or the like can be used.
[0100] The method of applying the liquid crystal alignment agent to the substrate is not particularly limited. The liquid crystal alignment agent can be applied to the substrate by, for example, a spin coat method, a printing method (for example, an offset printing method, a flexographic printing method, etc.), an inkjet method, a slit coat method, a bar coater method, an extrusion die method, a direct gravure coater method, a chamber doctor coater method, an offset gravure coater method, an impregnation coater method, an MB coater method, etc.
[0101] After the liquid crystal alignment agent is applied, preheating (prebaking) is preferably performed for the purpose of preventing dripping of the applied liquid crystal alignment agent. The prebaking temperature is preferably 30 to 200° C., and the prebaking time is preferably 0.25 to 10 minutes. Thereafter, the solvent is completely removed, and a baking (postbaking) step is performed, if necessary, for the purpose of thermally imidizing the amic acid structure present in the polymer. The baking temperature (postbaking temperature) at this time is preferably 80 to 280° C., more preferably 80 to 250° C. The postbaking time is preferably 5 to 200 minutes. The thickness of the film formed is preferably 0.001 to 1 μm.
[0102] <Step 2: Alignment Treatment> When manufacturing a TN-type, STN-type, IPS-type or FFS-type liquid crystal element, the coating film formed in the above step 1 is subjected to a treatment (alignment treatment) for imparting liquid crystal alignment ability. This imparts the alignment ability of liquid crystal molecules to the coating film, forming a liquid crystal alignment film. As the alignment treatment, it is preferable to use a rubbing treatment in which the surface of the coating film formed on the substrate is rubbed with cotton, nylon or the like, or a photo-alignment treatment in which the coating film is subjected to a light irradiation treatment to impart liquid crystal alignment ability. When manufacturing a vertical alignment type liquid crystal element, the coating film formed in step 1 may be used as it is as a liquid crystal alignment film, or the coating film formed in step 1 may be subjected to an alignment treatment in order to further enhance the liquid crystal alignment ability.
[0103] The light irradiation for photo-alignment can be performed by a method of irradiating the coating film after the post-bake step, a method of irradiating the coating film after the pre-bake step but before the post-bake step, or a method of irradiating the coating film during heating in at least one of the pre-bake step and the post-bake step. For example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm can be used as the radiation to be irradiated to the coating film. Preferably, ultraviolet light containing light with a wavelength of 200 to 400 nm is used. When the radiation is polarized, it may be linearly polarized or partially polarized. When the radiation used is linearly polarized or partially polarized, the radiation may be performed from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. When the radiation is non-polarized, the radiation is irradiated in an oblique direction.
[0104] Examples of the light source used include a low pressure mercury lamp, a high pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. The radiation dose is preferably 200 to 30,000 J / m 2 and more preferably 500 to 10,000 J / m 2 After the light irradiation for imparting the alignment ability, the surface of the substrate may be washed with, for example, water, an organic solvent (e.g., methanol, isopropyl alcohol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated.
[0105] <Step 3: Construction of liquid crystal cell> A pair of substrates on which liquid crystal alignment films are formed are arranged opposite to each other, and liquid crystal is arranged between the two substrates arranged opposite to each other to manufacture a liquid crystal cell. For example, the liquid crystal cell can be manufactured by arranging two substrates opposite to each other with a gap therebetween so that the liquid crystal alignment films face each other, bonding the peripheries of the two substrates with a sealant, injecting liquid crystal into the cell gap surrounded by the substrate surfaces and the sealant, and sealing the injection hole, or by a method using the ODF method. For example, an epoxy resin containing a hardener and aluminum oxide spheres as a spacer can be used as the sealant. For example, nematic liquid crystal and smectic liquid crystal can be used as the liquid crystal, and among these, nematic liquid crystal is preferred.
[0106] When manufacturing a liquid crystal display device, a polarizing plate is subsequently attached to the outer surface of the liquid crystal cell. Examples of the polarizing plate include a polarizing film called an "H film" made by absorbing iodine while stretching and aligning polyvinyl alcohol, sandwiched between cellulose acetate protective films, and a polarizing plate made of the H film itself.
[0107] The liquid crystal element of the present disclosure can be effectively applied to various applications, specifically, for example, it can be used as various display devices such as clocks, portable game machines, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, and information displays, as well as light control devices, retardation films, and the like.
[0108] According to the present disclosure described above in detail, the following means are provided. [Means 1] A liquid crystal aligning agent comprising a polymer [P] containing the following structural unit (U1) and structural unit (U2), and the content ratio of the structural unit (U1) is 5 mol % or more and 45 mol % or less based on the total amount of structural units derived from a diamine compound. Structural unit (U1): A structural unit derived from a diamine (D1) having at least one partial structure (A) selected from the group consisting of a ring structure in which two or more monocyclic aromatic rings are directly bonded and a condensed ring structure in which two or more monocyclic aromatic rings are condensed, and in which the total number of monocyclic aromatic rings constituting the partial structure (A) and the number of monocyclic aromatic rings constituting a portion other than the partial structure (A) is 3 or more. Structural unit (U2): A structural unit derived from a diamine (D2) having a partial structure represented by the above formula (1) (excluding those corresponding to the above diamine (D1)). [Means 2] The liquid crystal aligning agent according to [Means 1], wherein the diamine (D1) has a partial structure represented by the above formula (2). [Means 3] The liquid crystal aligning agent according to [Means 1] or [Means 2], wherein the polymer [P] is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide. [Means 4] The liquid crystal aligning agent according to any one of [Means 1] to [Means 3], wherein the polymer [P] further contains a structural unit derived from a diamine having a partial structure represented by the above formula (3). [Means 5] The liquid crystal aligning agent according to any one of [Means 1] to [Means 4], further comprising a polymer [Q] containing neither the structural unit (U1) nor the structural unit (U2). [Means 6] The liquid crystal aligning agent according to [Means 5], wherein the polymer [Q] is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide. [Means 7] The liquid crystal aligning agent according to any one of [Means 1] to [Means 6], further comprising a crosslinking agent. [Measure 8] A liquid crystal alignment film formed by using the liquid crystal aligning agent according to any one of [Measure 1] to [Measure 7]. [Measure 9] A method for producing a liquid crystal alignment film, comprising forming a coating film using the liquid crystal aligning agent according to any one of [Measure 1] to [Measure 7], and subjecting the coating film to a light irradiation treatment to impart liquid crystal aligning ability. [Means 10] A liquid crystal element comprising the liquid crystal alignment film according to [Means 8]. [Means 11] A polymer which is a polyamic acid, a polyamic acid ester or a polyimide and contains a structural unit derived from a diamine represented by the above formula (4). [Means 12] A diamine represented by the above formula (4). EXAMPLES
[0109] Hereinafter, the embodiments will be described in more detail with reference to examples, but the present invention should not be construed as being limited to the following examples.
[0110] In the following examples, the imidization rate of the polyimide in the polymer solution was measured by the following method. [Imidization rate of polyimide] The polyimide solution was poured into pure water, and the resulting precipitate was thoroughly dried under reduced pressure at room temperature. It was then dissolved in deuterated dimethyl sulfoxide and measured at room temperature using tetramethylsilane as a standard substance. 1 H-NMR measurement was performed. 1 The imidization rate [%] was calculated from the H-NMR spectrum using the following formula (F-1). Imidization rate [%] = (1-(A 1 / (A 2 ×α)))×100 …(F-1) (In formula (F-1), A 1 is the peak area due to the proton of the NH group that appears at a chemical shift of around 10 ppm, and A 2 is the peak area due to other protons, and α is the ratio of the number of other protons to one proton of the NH group in the polymer precursor (polyamic acid).
[0111] The abbreviations of the compounds are as follows. In the following, the "compound represented by formula (X)" may be simply referred to as "compound (X)".
[0112] (Tetracarboxylic acid dianhydride) [ka]
[0113] (Diamine compounds) [ka] [ka] [ka]
[0114] (Additives) [ka]
[0115] <Synthesis of diamine> [Synthesis example] Compound (DA-8) was synthesized according to the following scheme. [ka]
[0116] Synthesis of intermediate [1] 4-Hydroxy-4'-nitrobiphenyl (9.29 mmol), bis(2-chloroethyl) ether (23.2 mmol), potassium carbonate (23.2 mmol) and N,N-dimethylformamide (41 g) were added to a three-neck flask equipped with a nitrogen inlet tube and stirred at 80°C for 48 hours. After the reaction was completed, ethyl acetate was added and the mixture was separated and washed with water. The organic phase was concentrated under reduced pressure to obtain a crude product. The obtained crude product was subjected to column chromatography using ethyl acetate and hexane to obtain intermediate [1] (yield: 65%). The amount of intermediate [1] was 100%. 1 The results of H-NMR measurement are as follows: 1 H-NMR (400MHz, CDCl3-d6, δ(ppm)): 8.27(d, 2H), 7.68(d, 2H), 7.57(d, 2H), 7.03(d, 2H), 4.22(m, 2H), 3.93(m, 2H), 3.86(m, 2H), 3.68(m, 2H).
[0117] Synthesis of intermediate [2] Intermediate [1] (6.06 mmol), 4-nitrophenol (6.66 mmol), potassium carbonate (12.1 mmol) and dimethylformamide (27 g) were added to a three-neck flask equipped with a nitrogen inlet tube and stirred at 100°C for 20 hours. After cooling to room temperature, the salt was removed by filtration and the filtrate was concentrated under reduced pressure. Isopropyl alcohol was added thereto to precipitate crystals. The crystals were filtered, washed with water and isopropyl alcohol, and dried to obtain intermediate [2] (yield: 81%). The amount of intermediate [2] was 100%. 1 The results of H-NMR measurement are as follows: 1 H-NMR (400MHz, DMSO-d6, δ(ppm)): 8.26(d, 2H), 8.18(d, 2H), 7.92(d, 2H), 7. 74(d, 2H), 7.17(d, 2H), 7.09(d, 2H), 4.28(m, 2H), 4.19(m, 2H), 3.85(m, 4H).
[0118] Synthesis of compound (DA-8) Intermediate [2] (4.97 mmol), 10% palladium carbon (0.26 g), hydrazine monohydrate (30.0 mmol), tetrahydrofuran (7 g) and isopropyl alcohol (6 g) were placed in a three-neck flask equipped with a nitrogen inlet tube and stirred at 60°C for 2 hours. After the reaction was completed, the reaction solution was filtered through Celite, concentrated under reduced pressure, and isopropyl alcohol was added to precipitate crystals. The crystals were collected by filtration, washed with isopropyl alcohol, and dried to obtain compound (DA-8) (yield: 95%). Compound (DA-8) 1 The results of H-NMR measurement are as follows: 1 H-NMR (400MHz, DMSO-d6, δ(ppm)): 7.42(d, 2H), 7.27(d, 2H), 6.93(d, 2H), 6.65(d, 2H), 6.62(d, 2H), 6.48(d, 2H), 5.20(s, 2H), 4.58(s, 2H), 4.10(m, 2H), 3.95(m, 2H), 3.78(m, 2H), 3.74(m, 2H).
[0119] <Polymer synthesis> 1. Synthesis of polyamic acid [Synthesis Example 1] 100 parts by mole of compound (TA-2) as a tetracarboxylic dianhydride, 20 parts by mole of compound (DA-1) as a diamine compound, and 80 parts by mole of compound (DB-1) were dissolved in N-methyl-2-pyrrolidone (NMP), and the mixture was allowed to react at room temperature for 6 hours to obtain a solution containing 15% by mass of polyamic acid (referred to as polymer (PA-1)).
[0120] [Synthesis Examples 2-17] Polyamic acids (polymers (PA-2) to (PA-17)) were obtained by the same operation as in Synthesis Example 1, except that the types and amounts of the tetracarboxylic dianhydrides and diamine compounds used were changed as shown in Table 1. In Table 1, the values of the tetracarboxylic dianhydrides (acid dianhydride 1 and acid dianhydride 2) represent the ratio (molar parts) of the use of each compound relative to 100 parts by mole of the total amount of the tetracarboxylic dianhydrides used in the synthesis of each polymer. The values of the diamine compounds (diamine 1, diamine 2, and diamine 3) represent the ratio (molar parts) of the use of each compound relative to 100 parts by mole of the total amount of the diamine compounds used in the synthesis of each polymer (the same applies to Table 2 below).
[0121] [Table 1]
[0122] 2. Synthesis of Polyimide [Synthesis Example 18] 100 mol parts of compound (TA-2) as tetracarboxylic dianhydride, 30 mol parts of compound (DA-2) and 50 mol parts of compound (DB-2) as diamine compounds, and 20 mol parts of compound (DC-8) were dissolved in NMP and reacted at room temperature for 6 hours to obtain a solution containing 15% by mass of polyamic acid. Next, NMP was added to the obtained polyamic acid solution to obtain a solution with a polyamic acid concentration of 10% by mass, and pyridine and acetic anhydride were added to perform a dehydration ring-closing reaction at 60° C. for 4 hours. After the dehydration ring-closing reaction, the solvent in the system was replaced with fresh NMP to obtain a solution containing 15% by mass of polyimide with an imidization rate of about 60% (this is referred to as polymer (PI-1)).
[0123] [Synthesis Examples 19 and 20] Polyimides (polymers (PI-2) and (PI-3)) were obtained in the same manner as in Synthesis Example 18, except that the types and amounts of the tetracarboxylic dianhydride and diamine compound used were changed as shown in Table 2, and the amounts of pyridine and acetic anhydride were adjusted to make the imidization rate as shown in Table 2.
[0124] [Table 2]
[0125] <Preparation and Evaluation of Liquid Crystal Alignment Agent> [Example 1: Optical FFS type liquid crystal display element] 1. Preparation of Liquid Crystal Alignment Agent The solution containing the polymer (PA-3) obtained in Synthesis Example 3 was diluted with NMP and butyl cellosolve (BC) to obtain a solution with a solvent composition of NMP / BC=80 / 20 (mass ratio) and a solid content concentration of 3.5 mass%. The solution was filtered through a filter with a pore size of 0.2 μm to prepare a liquid crystal alignment agent (AL-1).
[0126] 2. Fabrication of FFS-type LCD elements using the photoalignment method A glass substrate (first substrate) having a flat electrode (bottom electrode), an insulating layer, and a comb-shaped electrode (top electrode) laminated in this order on one side thereof, and a glass substrate (second substrate) without an electrode were prepared. Next, a liquid crystal alignment agent (AL-1) was applied to each of the electrode-forming surface of the first substrate and one substrate surface of the second substrate using a spinner, and heated (pre-baked) on a hot plate at 80°C for 1 minute. Thereafter, the substrate was dried (post-baked) for 30 minutes in an oven at 230°C with the interior replaced with nitrogen, forming a coating film with an average thickness of 0.1 μm. The obtained coating film was irradiated with 1,000 J / m2 of linearly polarized ultraviolet light containing a 254 nm emission line using a Hg-Xe lamp. 2 The coating film was irradiated with light from the normal direction of the substrate to perform a photo-alignment treatment. The amount of irradiation was measured using an actinometer that measures at a wavelength of 254 nm. Next, the coating film that had been subjected to the photo-alignment treatment was heated in a clean oven at 230°C for 30 minutes to perform a heat treatment, thereby forming a liquid crystal alignment film. Next, for one of the pair of substrates on which the liquid crystal alignment film was formed, an epoxy resin adhesive containing aluminum oxide spheres with a diameter of 3.5 μm was applied by screen printing to the outer edge of the surface having the liquid crystal alignment film. Then, the substrates were overlapped and pressed together so that the projection direction of the polarization axis on the substrate surface during light irradiation was antiparallel, and the adhesive was thermally cured at 150°C for 1 hour. Next, negative liquid crystal (MLC-6608, manufactured by Merck) was filled between the pair of substrates through the liquid crystal injection port, and the liquid crystal injection port was sealed with an epoxy adhesive to obtain a liquid crystal cell. Furthermore, in order to remove the flow alignment during liquid crystal injection, the liquid crystal cell was heated at 120°C and then slowly cooled to room temperature. Then, polarizing plates were attached to both outer surfaces of the substrate in the liquid crystal cell to obtain a liquid crystal display element. In addition, the above series of operations was performed with a UV irradiation dose of 100 to 10,000 J / m after post-baking. 2 Three or more liquid crystal display elements with different amounts of ultraviolet light irradiation were manufactured by changing the exposure amount within the range of 1, and the liquid crystal display element with the exposure amount (optimum exposure amount) that showed the best alignment characteristics was used for the following evaluation.
[0127] 3. Evaluation of liquid crystal alignment (evaluation by retardation change rate) The LCD device manufactured in 2 above was rated at 27,000 cd / m2 The liquid crystal alignment was evaluated by the retardation change rate before and after backlight irradiation. The retardation of the liquid crystal display element manufactured in 2 above was measured by Axoscan manufactured by Optoscience, the retardation change rate α before and after backlight irradiation was calculated by the following formula (F-2), and the change rate α was compared with the judgment value. The smaller the change rate α, the less likely the liquid crystal alignment to deteriorate due to backlight irradiation, and the better the liquid crystal alignment. The change rate α was 0.5% or less and was evaluated as "excellent (◎)", 0.5% or more and 1% or less and was evaluated as "good (○)", 1% or more and 2% or less and was evaluated as "fair (△)", and 2% or more and was evaluated as "poor (×)". α=Δθ / θ1 …(F-2) (In formula (F-2), Δθ represents the retardation difference before and after irradiation, and θ1 represents the retardation value before irradiation.) As a result, the liquid crystal alignment property of this example was evaluated as "good (◯)".
[0128] 4. Evaluation of liquid crystal alignment after vibration test (evaluation by number of bright spots) A vibration test was carried out using the liquid crystal display element manufactured in 2 above. The vibration test was carried out by moving the vibration test device in the direction opposite to the liquid crystal display element while the liquid crystal display element was fixed to the vibration test device to vibrate the liquid crystal display element. Specifically, the vibration test was carried out by applying a sine vibration in which the vibration frequency was modulated (swept) from 50 Hz to 100 Hz in 5 minutes to the liquid crystal display element for 30 minutes at an acceleration of 1.0 G. As a result of the vibration test, in the liquid crystal display element of this embodiment, when the number of minute bright spots caused by scraping of the alignment film was 0 to 5, it was rated as "excellent (◎)", when it was 6 to 10, it was rated as "good (○)", when it was 11 to 20, it was rated as "fair (△)", and when it was 21 or more, it was rated as "poor (×)". As a result, the liquid crystal alignment of this embodiment was evaluated as "good (○)".
[0129] 5. Evaluation of slimming resistance (evaluation of haze after slimming test) The liquid crystal alignment agent prepared in 1 above was filtered through a 1.0 μm filter and then applied by spin coating to the second substrate prepared above. Next, it was heated (pre-baked) on a hot plate at 80°C for 1 minute. After that, it was dried (post-baked) for 30 minutes in an oven at 230°C with the inside of the oven replaced with nitrogen, forming a coating film with an average thickness of 0.1 μm. The obtained coating film was irradiated with 1,000 J / m2 of linearly polarized ultraviolet light containing a 254 nm emission line using an Hg-Xe lamp. 2 The substrate was irradiated with light from the normal direction to perform a photo-alignment treatment. The amount of irradiation was measured using an actinometer that measures at a wavelength of 254 nm. The photo-aligned coating was then heated in a clean oven at 230°C for 30 minutes to perform a heat treatment, and a substrate with a liquid crystal alignment film was obtained. The alignment film was rubbed with rayon cloth: YA-20-R manufactured by Yoshikawa Kako Co., Ltd. (roller diameter 120 mm, roller rotation speed 1000 rpm, moving speed 20 mm / sec, indentation length 0.3 mm). The presence or absence of scratches or scrapes on the surface of the alignment film was measured by measuring the haze (cloudiness). At this time, the haze was measured using a haze meter (HZ-V3, manufactured by Suga Test Instruments Co., Ltd.) in accordance with JIS K 7136. As a result of the slimming test, in the liquid crystal alignment agent of this embodiment, if the haze caused by the scraping of the alignment film was 0% or more and 0.2% or less, it was rated as "good (○)", if it was more than 0.2% and 0.4% or less, it was rated as "fair (△)", and if it was more than 0.4%, it was rated as "poor (×)". As a result, the slimming resistance of this embodiment was rated as "good (○)".
[0130] 6. Evaluation of seal adhesion The liquid crystal alignment agent (AL-1) prepared in 1 above was applied to a glass substrate using a spinner, pre-baked for 2 minutes on a hot plate at 80°C, and then heated (post-baked) for 30 minutes in an oven at 230°C with the interior replaced with nitrogen, forming a coating film with an average thickness of 0.10 μm. By repeating the same operation, two glass substrates with coating films were produced. On the coating film of one of the glass substrates with the coating film formed, an ODF sealant (S-WB42, manufactured by Sekisui Chemical Co., Ltd.) was applied to a width of 1 mm, and the other glass substrate was laminated so that the coating film and the ODF sealant were in contact with each other. After that, a metal halide lamp was used to apply 30,000 J / m 2 After irradiating the film with light (equivalent to 365 nm), the film was heated in an oven at 120°C for 1 hour. The adhesion strength was then measured using a compression and tensile tester (model number: SDWS-0201-100SL) manufactured by Imada Seisakusho, to evaluate the adhesion of the film to the sealant. The greater the adhesion strength, the more the film's cohesive failure was suppressed. The evaluation was conducted when the adhesion strength was 175 N / cm 2 If it is more than 125N / cm, it is considered to be "Good (○)". 2 More than 175N / cm 2 If it is less than 125N / cm, it is marked as "Fair (△)". 2 If the adhesion was less than 175 N / cm, it was rated as "poor (x)". 2 The seal adhesion was evaluated as "good (○)."
[0131] [Examples 2 to 11 and Comparative Examples 1 to 4] A liquid crystal alignment agent was prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. Using the obtained liquid crystal alignment agent, an FFS-type liquid crystal display element was manufactured by a photoalignment method in the same manner as in Example 1, and the liquid crystal alignment property, alignment property after a vibration test, slimming resistance, and seal adhesion were evaluated. The results are shown in Table 3. In Table 3, the numerical values in the columns for polymer components (polymer 1 and polymer 2) and additives indicate the blending ratio (parts by mass) of the solid content of each compound relative to 100 parts by mass of the total amount of the polymer components used in the preparation of the liquid crystal alignment agent.
[0132] [Table 3]
[0133] As shown in Table 3, Examples 1 to 11, which used a liquid crystal alignment agent containing the polymer [P], showed a good balance of improvements in liquid crystal alignment, liquid crystal alignment after vibration test, slimming resistance, and adhesion, compared to Comparative Examples 1 to 4, which used a liquid crystal alignment agent not containing the polymer [P], and showed good results. Among them, Examples 1, 2, 4, 5, 7, 8, 10, and 11 were all evaluated as "○" or "◎", and Examples 4 and 10 were particularly excellent, with the liquid crystal alignment evaluated as "◎".
[0134] [Example 12: Rubbed FFS type liquid crystal display element] 1. Preparation of Liquid Crystal Alignment Agent The solution containing the polymer (PA-8) obtained in Synthesis Example 8 was diluted with NMP and BC to obtain a solution with a solvent composition of NMP / BC=80 / 20 (mass ratio) and a solid content concentration of 3.5 mass%. This solution was filtered through a filter with a pore size of 0.2 μm to prepare a liquid crystal alignment agent (AL-12).
[0135] 2. Fabrication of FFS-type LCD elements using the rubbing method The first and second substrates were prepared in the same manner as in Example 1. Next, a liquid crystal alignment agent (AL-12) was applied to the electrode-formed surface of the first substrate and one surface of the second substrate by a spinner, and heated (pre-baked) on a hot plate at 110°C for 3 minutes. Then, the liquid crystal alignment agent (AL-12) was applied to the electrode-formed surface of the first substrate and one surface of the second substrate by a spinner, and heated (pre-baked) on a hot plate at 110°C for 30 ... in a nitrogen-substituted oven at 230°C for 30 minutes to form a coating film having an average thickness of 0.08 μm. Next, the coating film surface was subjected to a rubbing treatment by a rubbing machine having a roll wrapped with rayon cloth at a roll rotation speed of 1000 rpm, a stage moving speed of 3 cm / sec, and a pile pressing length of 0.3 mm. Then, ultrasonic cleaning was performed in ultrapure water for 1 minute, and then drying was performed in a clean oven at 100°C for 10 minutes to obtain a pair of substrates having a liquid crystal alignment film. Next, a pair of substrates having a liquid crystal alignment film was screen-printed with an epoxy resin adhesive containing aluminum oxide spheres having a diameter of 3.5 μm, leaving a liquid crystal injection port at the edge of the surface on which the liquid crystal alignment film was formed. The substrates were then superimposed and pressed together, and the adhesive was thermally cured at 150°C for 1 hour. Next, a negative liquid crystal (MLC-6608, manufactured by Merck) was filled into the gap between the pair of substrates through the liquid crystal injection port, and the liquid crystal injection port was then sealed with an epoxy adhesive. Furthermore, in order to remove the flow orientation during liquid crystal injection, the substrate was heated at 120°C and then slowly cooled to room temperature to produce a liquid crystal cell. Note that when the pair of substrates were superimposed, the rubbing methods of the respective substrates were set to be antiparallel. Next, polarizing plates were attached to both outer surfaces of the substrates in the liquid crystal cell to obtain an FFS-type liquid crystal display element.
[0136] 3. Evaluation The liquid crystal display element manufactured in the above 2. was evaluated for liquid crystal alignment and liquid crystal alignment after vibration test by the same method as in Example 1. In addition, the liquid crystal alignment agent (AL-12) prepared in the above 1. was used to evaluate slimming resistance and seal adhesion of the liquid crystal alignment film to the substrate by the same method as in Example 1. These results are shown in Table 4.
[0137] [Examples 13 to 15 and Comparative Example 5] A liquid crystal alignment agent was prepared in the same manner as in Example 12, except that the composition of the liquid crystal alignment agent was changed as shown in Table 4. In addition, using the obtained liquid crystal alignment agent, an FFS-type liquid crystal display element was manufactured by a rubbing method in the same manner as in Example 12, and the liquid crystal alignment property, alignment property after a vibration test, slimming resistance, and seal adhesion were evaluated. The results are shown in Table 4. In Table 4, the numerical value in the polymer column indicates the blending ratio (parts by mass) of the solid content of each polymer relative to 100 parts by mass of the total amount of the polymer components used in the preparation of the liquid crystal alignment agent.
[0138] [Table 4]
[0139] As shown in Table 4, in Examples 12 to 15 using a liquid crystal alignment agent containing the polymer [P], the liquid crystal alignment, the liquid crystal alignment after the vibration test, the slimming resistance and the adhesion were improved in a well-balanced manner, and the results were good, compared to Comparative Example 5 using a liquid crystal alignment agent not containing the polymer [P]. Among them, in Examples 12, 13 and 15, the evaluations of the liquid crystal alignment, the liquid crystal alignment after the vibration test, the slimming resistance and the seal adhesion were all "○" or higher, and various properties were improved in a well-balanced manner. In addition, in Example 14, the evaluations of the slimming resistance and the seal adhesion were "△", but the evaluations of the liquid crystal alignment and the alignment after the vibration test were "○" or higher. In contrast, in Comparative Example 5 using a liquid crystal alignment agent not containing the polymer [P], the evaluation of the liquid crystal alignment after the vibration test was "×", and the evaluation of the seal adhesion was "△".
[0140] From the above results, it is clear that a liquid crystal aligning agent containing the polymer [P] can provide a liquid crystal device excellent in liquid crystal alignment property, slimming resistance, vibration resistance and seal adhesion.
Claims
1. A liquid crystal aligning agent comprising a polymer [P] containing the following structural unit (U1) and structural unit (U2), and a content ratio of the structural unit (U1) being 5 mol % or more and 45 mol % or less with respect to the total amount of structural units derived from a diamine compound. Structural unit (U1): A structural unit derived from a diamine (D1) having at least one partial structure (A) selected from the group consisting of a ring structure in which two or more monocyclic aromatic rings are directly bonded and a condensed ring structure in which two or more monocyclic aromatic rings are condensed, and in which the total number of monocyclic aromatic rings constituting the partial structure (A) and the number of monocyclic aromatic rings constituting a portion other than the partial structure (A) is 3 or more. Structural unit (U2): a structural unit derived from a diamine (D2) having a partial structure represented by the following formula (1) (excluding those corresponding to the diamine (D1)) 【Chemistry 1】 (In formula (1), Ar 1 and Ar 2 are each independently a divalent aromatic ring group. 1 and Z 2 are each independently a single bond, -NR 1 -, -O-, -S-, -CO-, * 1 -NR 1 -CO-, * 1 -CO-NR 1 -, * 1 -NR 1 -CO-NR 2 -, * 1 -CO-O- or * 1 -O-CO-. However, Z 1 and Z 2 cannot be a single bond at the same time. 1 R is a monovalent organic group. 2 is a hydrogen atom or a monovalent organic group. 1 " is Ar 1 Or Ar 2 It represents a bond with L. 1 is -NR 3 -, -O-, -S-, -CO-, * 2 -NR 3 -CO-, * 2 -CO-NR 3 --, --NR 3 -CO-NR 4 -, * 2 -CO-O- or * 2 -O-CO-. 3 and R 4 are each independently a hydrogen atom or a monovalent organic group. 2 " is B 1 It represents a bond with . 1 is a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. 2 is a divalent aliphatic hydrocarbon group having 3 to 20 carbon atoms. n is an integer of 0 to 3. When n is 2 or 3, multiple B 1 are the same or different, and multiple L 1 are the same or different. "*" represents a bond.)
2. The liquid crystal aligning agent according to claim 1 , wherein the diamine (D1) has a partial structure represented by the following formula (2): 【Chemistry 2】 (In formula (2), Ar 3 and Ar 4 are each independently a divalent aromatic ring group. 3 and Ar 4 At least one of Z has a biphenyl structure or a condensed ring structure. 3 and Z 4 are each independently a single bond, -NR 5 -, -O-, -S-, -CO-, * 3 -NR 5 -CO-, * 3 -CO-NR 5 --, --NR 5 -CO-NR 6 -, * 3 -CO-O- or * 3 -O-CO-. 5 and R 6 are each independently a hydrogen atom or a monovalent organic group. 3 " is Ar 3 Or Ar 4 It represents a bond with L. 2 is -NR 7 -, -O-, -S-, -CO-, * 4 -NR 7 -CO-, * 4 -CO-NR 7 --, --NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-. 7 and R 8 are each independently a hydrogen atom or a monovalent organic group. 4 " is B 3 It represents a bond with . 3 and B 4 are each independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. m is an integer of 0 to 3. When m is 2 or 3, multiple B 3 are the same or different, and multiple L 2 are the same or different. "*" represents a bond.)
3. The liquid crystal aligning agent according to claim 1 , wherein the polymer [P] is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.
4. The liquid crystal aligning agent according to claim 1 , wherein the polymer [P] further contains a structural unit derived from a diamine having a partial structure represented by the following formula (3): 【Chemistry 3】 (In formula (3), Ar 5 and Ar 6 are each independently a divalent aromatic ring group. 5 and Z 6 are each independently a single bond, -NR 9 -, -O-, -S-, -CO-, * 5 -NR 9 -CO-, * 5 -CO-NR 9 -, * 5 -CO-O- or * 5 -O-CO-. However, Z 5 and Z 6 cannot be a single bond at the same time. 9 is a hydrogen atom or a monovalent organic group. 5 " is Ar 5 Or Ar 6 It represents a bond with . 5 is a methylene group or an ethylene group. "*" represents a bond.)
5. The liquid crystal aligning agent according to claim 1 , further comprising a polymer [Q] that does not contain either the structural unit (U1) or the structural unit (U2).
6. The liquid crystal aligning agent according to claim 5 , wherein the polymer [Q] is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.
7. The liquid crystal aligning agent according to claim 1 , further comprising a crosslinking agent.
8. A liquid crystal alignment film formed by the liquid crystal aligning agent according to any one of claims 1 to 7.
9. A method for producing a liquid crystal alignment film, comprising forming a coating film from the liquid crystal aligning agent according to any one of claims 1 to 7, and subjecting the coating film to a light irradiation treatment to impart liquid crystal alignment ability.
10. A liquid crystal element comprising the liquid crystal alignment film according to claim 8 .
11. A polymer which is a polyamic acid, a polyamic acid ester or a polyimide and contains a structural unit derived from a diamine represented by the following formula (4): 【Chemistry 4】 (In formula (4), Ar 3 and Ar 4 are each independently a divalent aromatic ring group. 3 and Ar 4 At least one of Z has a biphenyl structure or a condensed ring structure. 3 and Z 4 are each independently a single bond, -NR 5 -, -O-, -S-, -CO-, * 3 -NR 5 -CO-, * 3 -CO-NR 5 --, --NR 5 -CO-NR 6 -, * 3 -CO-O- or * 3 -O-CO-. 5 and R 6 are each independently a hydrogen atom or a monovalent organic group. 3 " is Ar 3 Or Ar 4 It represents a bond with L. 2 is -NR 7 -, -O-, -S-, -CO-, * 4 -NR 7 -CO-, * 4 -CO-NR 7 --, --NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-. 7 and R 8 are each independently a hydrogen atom or a monovalent organic group. 4 " is B 3 It represents a bond with . 3 and B 4 are each independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. m1 is an integer of 1 to 3. When m1 is 2 or 3, multiple B 3 are the same or different, and multiple L 2 are the same or different.)
12. A diamine represented by the following formula (4): 【Chemistry 5】 (In formula (4), Ar 3 and Ar 4 are each independently a divalent aromatic ring group. 3 and Ar 4 At least one of Z has a biphenyl structure or a condensed ring structure. 3 and Z 4 are each independently a single bond, -NR 5 -, -O-, -S-, -CO-, * 3 -NR 5 -CO-, * 3 -CO-NR 5 --, --NR 5 -CO-NR 6 -, * 3 -CO-O- or * 3 -O-CO-. 5 and R 6 are each independently a hydrogen atom or a monovalent organic group. 3 " is Ar 3 Or Ar 4 It represents a bond with L. 2 is -NR 7 -, -O-, -S-, -CO-, * 4 -NR 7 -CO-, * 4 -CO-NR 7 --, --NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-. 7 and R 8 are each independently a hydrogen atom or a monovalent organic group. 4 " is B 3 It represents a bond with . 3 and B 4 are each independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. m1 is an integer of 1 to 3. When m1 is 2 or 3, multiple B 3 are the same or different, and multiple L 2 are the same or different.)
Citation Information
Patent Citations
Liquid crystal aligning agent, liquid crystal alignment film, liquid crystal display element, phase difference film, manufacturing method for phase difference film, polymer, and compound
JP2014132326A
Liquid crystal alignment agent, liquid crystal alignment film, liquid crystal display element, polymer, and compound
JP2016145954A
Cited By
Liquid crystal alignment agent for forming liquid crystal alignment film and liquid crystal display element
CN122302280A