Multilayer electronic component

By incorporating Sn and a transition metal in the side margin portions with a specific ratio, the multilayer ceramic capacitors enhance insulation resistance and moisture resistance, addressing the issue of moisture penetration and enabling miniaturization and higher capacitance in electronic components.

JP2024132898APending Publication Date: 2024-10-01SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024022777
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-14
Filing Date
2024-02-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The insulation resistance of multilayer ceramic capacitors deteriorates due to moisture penetration through the side margin section, which is a common issue in highly integrated electronic components.

Method used

The side margin portions of the multilayer electronic component are made of Sn and a transition metal, with a ratio of transition metal content to Sn content of 10 or more, to trap moisture and prevent hydration, thereby enhancing insulation resistance.

Benefits of technology

This configuration effectively prevents the reversible deterioration of insulation resistance, improving moisture resistance reliability and enabling miniaturization and higher capacitance in electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132898000001_ABST
    Figure 2024132898000001_ABST
Patent Text Reader

Abstract

To provide a multilayer electronic component capable of preventing a reversible deterioration of an insulation resistance by preventing hydration by trapping a positive hole in a side margin part.SOLUTION: A multilayer electronic component 100 includes: a main body 110 that contains a dielectric layer, and an internal electrode which is alternately arranged with the dielectric layer, a first surface 1 and a second surface 2 that are opposite to a first direction, a third surface 3 and a fourth surface 4 that are connected to the first surface and the second surface and are opposite to a second direction, and a fifth surface 5 and a sixth surface 6 that are connected to the first to fourth surfaces and are opposite to a third direction; side margin parts 114 and 115 that are arranged onto the fifth surface and the sixth surface of the main body; and external electrodes 131 and 132 that are arranged onto the third surface and the fourth surface. Each side margin part contains Sn and a transition metal, and a ratio of a content of the transition metal to the content of Sn is 10 or larger.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer electronic component. [Background technology]

[0002] Multilayer ceramic capacitors (MLCCs), which are one type of multilayer electronic component, are chip-type capacitors that are mounted on printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones, and serve to charge and discharge electricity.

[0003] As electronic products become smaller, slimmer, and more multifunctional, there is a demand for smaller chip components as well, and the packaging of electronic components is becoming more highly integrated. In response to this trend, the space between the mounted electronic components is becoming smaller.

[0004] In particular, in the case of a structure in which a separate side margin portion is formed on the side of the main body to improve the capacitance, the probability of moisture penetration through the side margin portion increases, and structural improvements are required to prevent deterioration of the insulation resistance due to moisture penetration. Summary of the Invention [Problem to be solved by the invention]

[0005] One of several objects of the present invention is to suppress a phenomenon in which, when a separate side margin portion is formed on a side surface of a body, the insulation resistance is deteriorated due to moisture penetration through the side margin portion.

[0006] However, the scope of the present invention is not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Means for solving the problem]

[0007] According to an embodiment of the present invention, there is provided a multilayer electronic component comprising: a body including dielectric layers and internal electrodes alternately arranged with the dielectric layers, the body including first and second sides facing a first direction, third and fourth sides connected to the first and second sides and facing a second direction, and fifth and sixth sides connected to the first to fourth sides and facing a third direction; side margin portions disposed on the fifth and sixth sides; and external electrodes disposed on the third and fourth sides, the side margin portions including Sn and a transition metal, and a ratio of the transition metal content to the Sn content in the side margin portions being 10 or more. Effect of the Invention

[0008] One of the advantages of the present invention is that the ratio of the transition metal content to the Sn content in the side margin is adjusted to 10 or more, trapping holes in the side margin and preventing hydration, thereby preventing reversible deterioration of insulation resistance.

[0009] However, the various and beneficial advantages and effects of the present invention are not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0010] [Figure 1] 1 is a perspective view showing a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a perspective view showing a main body according to an embodiment; [Diagram 3] 2 is a cross-sectional view taken along line II' in FIG. [Figure 4] 2 is a cross-sectional view taken along line II-II' in FIG. [Diagram 5] FIG. 5 is an enlarged view of region P in FIG. [Figure 6] 1A to 1C are diagrams illustrating an example of a method for manufacturing a multilayer electronic component according to an embodiment of the present invention. [Figure 7]1A to 1C are diagrams illustrating an example of a method for manufacturing a multilayer electronic component according to an embodiment of the present invention. [Figure 8] 1A to 1C are diagrams illustrating an example of a method for manufacturing a multilayer electronic component according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shapes and sizes of elements in the drawings may be exaggerated for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0012] In order to clearly explain the present invention in the drawings, parts that are not relevant to the explanation are omitted, and the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited to those shown in the drawings. Components having the same function within the same concept are described using the same reference numerals. Furthermore, throughout the specification, when a part is said to "include" a certain component, this does not mean that other components are excluded, but that the part may further include other components, unless otherwise specified.

[0013] FIG. 1 is a perspective view showing a multilayer electronic component according to one embodiment of the present invention, FIG. 2 is a perspective view generally showing a main body according to one embodiment, FIG. 3 is a cross-sectional view taken along line I-I' in FIG. 1, FIG. 4 is a cross-sectional view taken along line II-II' in FIG. 1, FIG. 5 is an enlarged view of region P in FIG. 4, and FIGS. 6 to 8 are diagrams showing an example of a method for manufacturing a multilayer electronic component according to one embodiment of the present invention.

[0014] Hereinafter, a multilayer electronic component according to one embodiment of the present invention will be described in detail with reference to FIGS.

[0015] In the figure, the first direction is the direction in which the first internal electrodes and the second internal electrodes are alternately arranged with the dielectric layer sandwiched therebetween or the thickness T direction, and of the second and third directions which are directions perpendicular to the first direction, the second direction can be defined as the length L direction and the third direction can be defined as the width W direction.

[0016] A multilayer electronic component 100 according to an embodiment of the present invention includes a body 110 including a dielectric layer 111 and internal electrodes 121, 122 arranged alternately with the dielectric layers, a first surface 1 and a second surface 2 facing in a first direction, a third surface 3 and a fourth surface 4 connected to the first and second surfaces and facing in the second direction, and a fifth surface 5 and a sixth surface 6 connected to the first to fourth surfaces and facing in the third direction, side margin portions 114, 115 arranged on the fifth and sixth surfaces, and external electrodes 131, 132 arranged on the third and fourth surfaces, the side margin portions including Sn and a transition metal, and a ratio of the transition metal content to the Sn content in the side margin portions is 10 or more.

[0017] The body 110 includes a dielectric layer 111 and a first internal electrode 121 and a second internal electrode 122 alternately arranged with the dielectric layer 111 .

[0018] Although there is no particular limitation on the specific shape of the body 110, the body 110 may have a hexahedral shape or a shape similar thereto, as shown in Fig. 2. Due to shrinkage of the ceramic powder contained in the body 110 during the firing process, the body 110 may have a substantially hexahedral shape, although it is not a hexahedral shape having perfectly straight lines.

[0019] The main body 110 may include a first surface 1 and a second surface 2 facing each other in a first direction, a third surface 3 and a fourth surface 4 connected to the first surface 1 and the second surface 2 and facing each other in the second direction, and a fifth surface 5 and a sixth surface 6 connected to the first surface 1 and the second surface 2, connected to the third surface 3 and the fourth surface 4, and facing each other in the third direction.

[0020] There is no particular limitation on the method of forming the body 110. For example, as shown in Fig. 6 to Fig. 8, a first ceramic green sheet 211a on which a plurality of parallel first internal electrode patterns 221 are printed and a second ceramic green sheet 211b on which a plurality of parallel second internal electrode patterns 222 are printed are alternately laminated, and the ceramic green sheet laminate 220 is cut into individual sizes along cutting lines C1-C1 and C2-C2 that are perpendicular to each other so as to cross a plurality of stripe-shaped first internal electrode patterns 221 and a stripe-shaped second internal electrode pattern 222 to form a laminated body 210, and then the laminated body 210 is fired to form the body 110, or side margin parts 114 and 115 described later are attached to the side surfaces of the laminated body 210 and then fired together to form the body 110, but the method is not limited thereto.

[0021] At this time, as shown in FIG. 2, in order to maximize the capacitance per unit volume of the multilayer electronic component 100 and minimize the step between the ends of the internal electrodes 121, 122 and the dielectric layer 111, both ends of the internal electrodes 121, 122 in the third direction can be in contact with the fifth surface 5 and the sixth surface 6 of the body 110, respectively.

[0022] The plurality of dielectric layers 111 are in a fired state, and the boundaries between adjacent dielectric layers 111 can be integrated to such an extent that they are difficult to confirm without using a scanning electron microscope (SEM).

[0023] According to an embodiment of the present invention, the raw material for forming the dielectric layer 111 is not particularly limited as long as a sufficient capacitance can be obtained. For example, a barium titanate-based material, a lead complex perovskite-based material, or a strontium titanate-based material can be used. The barium titanate-based material can include BaTiO3-based ceramic powder, and examples of the ceramic powder include BaTiO3, BaTiO3 partially solid-dissolved with Ca (calcium), Zr (zirconium), etc. 1-x Ca x )TiO3(0 <x<1)、Ba(Ti 1-y Ca y)O3 (0 < y < 1), (Ba 1-x Ca x )(Ti 1-y Zr y )O3 (0 < x < 1, 0 < y < 1) or Ba(Ti 1-y Zr y )O3 (0 < y < 1), etc. can be mentioned.

[0024] Also, as the raw material for forming the dielectric layer 111, various ceramic additives, organic solvents, binders, dispersants, etc. can be added to powders such as barium titanate (BaTiO3) according to the object of the present invention. Therefore, according to one embodiment of the present invention, the dielectric layer 111 contains Ba and Ti.

[0025] On the other hand, the average thickness td of the dielectric layer 111 does not need to be particularly limited.

[0026] However, generally, when the dielectric layer 111 is formed thinly to a thickness of less than 0.6 μm, especially when the average thickness td of the dielectric layer 111 is 0.35 μm or less, there is a risk of deterioration in reliability.

[0027] According to one embodiment of the present invention, in the side margin portions 114 and 115, by adjusting the ratio of the content of the transition metal to the Sn content to 10 or more and suppressing the deterioration of the insulation resistance of the dielectric layer containing Ba and Ti even in a humid environment, the moisture resistance reliability can be improved. Therefore, even when the average thickness te of the dielectric layer 111 is 0.35 μm or less, excellent moisture resistance reliability of the multilayer electronic component 100 can be ensured.

[0028] Therefore, when the average thickness td of the dielectric layer 111 is 0.35 μm or less, the effect according to the present invention becomes more remarkable, and miniaturization and high capacitance of the multilayer electronic component 100 can be more easily achieved.

[0029] The average thickness td of the dielectric layer 111 may refer to an average size in a first direction of the dielectric layer 111 disposed between the first internal electrode 121 and the second internal electrode 122. Meanwhile, when the body 110 includes a plurality of dielectric layers 111, the average thickness td of the dielectric layer 111 may refer to an average thickness of at least one of the plurality of dielectric layers 111.

[0030] The average thickness td of the dielectric layer 111 can be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, in the scanned image, the thickness of one dielectric layer can be measured at 30 equally spaced points in the length direction to obtain an average value. The 30 equally spaced points can be designated as the capacitance forming part Ac. Furthermore, if such an average value measurement is extended to 10 dielectric layers to measure the average value, the average thickness of the dielectric layer can be further generalized.

[0031] 2 to 4, the body 110 may include a capacitance forming portion Ac that is disposed inside the body 110 and is a region where the first internal electrode 121 and the second internal electrode 122 overlap in a first direction.

[0032] The capacitance forming portion Ac is a portion that contributes to forming the capacitance of the capacitor, and can be formed by repeatedly laminating a plurality of first internal electrodes 121 and second internal electrodes 122 with the dielectric layer 111 interposed therebetween.

[0033] An upper cover part 112 may be disposed on one surface of the capacitance forming part Ac in the first direction, and a lower cover part 113 may be disposed on the other surface of the capacitance forming part Ac in the first direction.

[0034] The upper cover part and the lower cover part may be formed by stacking a single dielectric layer or two or more dielectric layers on the upper and lower surfaces of the capacitance forming part Ac in the thickness direction, respectively, and may basically serve to prevent damage to the internal electrodes due to physical or chemical stress.

[0035] The upper cover part 112 and the lower cover part 113 do not include an internal electrode and may include the same material as the dielectric layer 111 .

[0036] That is, the upper cover part 112 and the lower cover part 113 may include a ceramic material, for example, a barium titanate (BaTiO3) based ceramic material.

[0037] Meanwhile, the average thickness tc of the cover parts 112, 113 does not need to be particularly limited. However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the average thickness tc of the cover parts 112, 113 may be 15 μm or less. Here, the average thickness of the cover parts 112, 113 may mean the average thickness of each of the first cover part 112 and the second cover part 113.

[0038] The average thickness tc of the cover parts 112, 113 may mean the size in the first direction, and may be the average value of the size in the first direction of the cover parts 112, 113 measured at five equally spaced points on the upper or lower part of the capacitance forming part Ac.

[0039] The internal electrodes 121, 122 are alternately arranged with the dielectric layers 111. At this time, the internal electrodes and the dielectric layers are alternately arranged in the first direction.

[0040] The internal electrodes 121, 122 may include a first internal electrode 121 and a second internal electrode 122. The first internal electrodes 121 and the second internal electrodes 122 may be alternately arranged to face each other across the dielectric layer 111 constituting the body 110, and may be connected to the third surface 3 and the fourth surface 4 of the body 110, respectively. Specifically, one end of the first internal electrode 121 may be connected to the third surface, and one end of the second internal electrode 122 may be connected to the fourth surface. That is, in one embodiment, the internal electrodes 121, 122 may contact the third surface 3 or the fourth surface 4.

[0041] 2, the first internal electrode 121 may be spaced apart from the fourth surface 4 and exposed through the third surface 3, and the second internal electrode 122 may be spaced apart from the third surface 3 and exposed through the fourth surface 4. A first external electrode 131 may be disposed on the third surface 3 of the body and connected to the first internal electrode 121, and a second external electrode 132 may be disposed on the fourth surface 4 of the body and connected to the second internal electrode 122.

[0042] That is, the first internal electrode 121 is not connected to the second external electrode 132 but is connected to the first external electrode 131, and the second internal electrode 122 is not connected to the first external electrode 131 but is connected to the second external electrode 132. Therefore, the first internal electrodes 121 may be formed at a certain distance apart on the fourth surface 4, and the second internal electrodes 122 may be formed at a certain distance apart on the third surface 3. In this case, the first internal electrodes 121 and the second internal electrodes 122 may be electrically separated from each other by a dielectric layer 111 disposed therebetween.

[0043] Furthermore, as described above, in order to maximize the capacitance per unit volume of the multilayer electronic component 100 and minimize the step between the ends of the internal electrodes 121, 122 and the dielectric layer 111, both ends of the internal electrodes 121, 122 in the third direction can be in contact with the fifth surface 5 and the sixth surface 6 of the main body 110, respectively.

[0044] There is no particular limitation on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity can be used. For example, the internal electrodes 121 and 122 can include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0045] The internal electrodes 121 and 122 may be formed by printing a conductive paste for internal electrodes, which contains at least one of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, on a ceramic green sheet. The method for printing the conductive paste for internal electrodes may be a screen printing method or a gravure printing method, but the present invention is not limited thereto.

[0046] On the other hand, the average thickness te of the internal electrodes 121, 122 does not need to be particularly limited.

[0047] However, in general, when the internal electrodes 121, 122 are formed to a thickness of less than 0.6 μm, particularly when the average thickness te of the internal electrodes 121, 122 is 0.35 μm or less, there is a risk of the reliability decreasing.

[0048] According to one embodiment of the present invention, in the side margin portions 114, 115, the ratio of the transition metal content to the Sn content is adjusted to 10 or more, and degradation of the insulation resistance of the dielectric layer containing Ba and Ti is suppressed even in a humid environment, thereby improving the moisture resistance reliability. Therefore, even when the average thickness te of the internal electrodes 121, 122 is 0.35 μm or less, excellent moisture resistance reliability of the multilayer electronic component 100 can be ensured.

[0049] Therefore, when the average thickness te of the internal electrodes 121, 122 is 0.35 μm or less, the effects of the present invention become more pronounced, and the multilayer electronic component 100 can be more easily reduced in size and increased in capacity.

[0050] The average thickness te of the internal electrodes 121, 122 may refer to the average size of the internal electrodes 121, 122 in the first direction. Meanwhile, when the body 110 includes a plurality of internal electrodes 121, 122, the average thickness td of the internal electrodes 121, 122 may refer to the average thickness of at least one of the plurality of internal electrodes 121, 122.

[0051] The average thickness te of the internal electrodes 121, 122 may be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, in the scanned image, the thickness of one internal electrode may be measured at 30 equally spaced points in the length direction to obtain an average value. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 internal electrodes and an average value is measured, the average thickness of the internal electrodes may be further generalized.

[0052] 1 and 4, side margins 114 and 115 may be disposed on the fifth and sixth surfaces 5 and 6 of the body 110.

[0053] The side margins 114 and 115 essentially serve to prevent damage to the internal electrodes due to physical or chemical stress.

[0054] The method for forming the side margins 114, 115 is not particularly limited. For example, they can be formed by applying a ceramic slurry for forming the side margins to the side surfaces of the laminated body 210 and then firing, or by pressing and adhering a ceramic green sheet for forming the side margins to the side surfaces of the laminated body 210 and then firing. The material for forming the side margins 114, 115 does not need to be particularly limited, and they may be formed of the same material as the dielectric layer 111, but is not limited thereto, and when they are formed of a material different from that of the dielectric layer 111, , can have different compositions.

[0055] Meanwhile, the width of the margin parts 114, 115 is not particularly limited. However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the average width of the margin parts 114, 115 may be 15 μm or less. In addition, according to an embodiment of the present invention, the ratio of the transition metal content to the Sn content in the side margin parts 114, 115 is adjusted to 10 or more, and the insulation resistance deterioration of the dielectric layer containing Ba and Ti is suppressed even in a humid environment, thereby improving the moisture resistance reliability. Therefore, even if the average width of the margin parts 114, 115 is 15 μm or less, excellent reliability can be ensured. The average width of the side margin parts 114, 115 may mean the average size of the side margin parts 114, 115 in the third direction, and may be the average value of the size of the side margin parts 114, 115 in the third direction measured at five equally spaced points on the side of the capacitance forming part Ac.

[0056] According to one embodiment of the present invention, the side margin portions 114, 115 may include Sn and a transition metal.

[0057] In the past, there have been attempts to include Sn in the side margins in order to reduce the grain size of the dielectric grains in the side margins and thereby achieve high toughness.

[0058] However, if the side margin portion is damaged by an external impact, moisture penetrates into the damaged area and affects the dielectric layer 111 included in the capacitance forming portion Ac, so that there is a limit to the extent to which the insulation resistance deterioration in the dielectric layer 111 can be fundamentally prevented in a humid environment.

[0059] Therefore, according to one embodiment of the present invention, the side margin portions 114, 115 further contain a transition metal in addition to Sn, thereby suppressing deterioration of the insulation resistance of the dielectric layer 111 even in a humid environment, thereby improving the moisture resistance reliability of the multilayer electronic component 100.

[0060] If the molar ratio of the transition metal to Sn in the side margin portions 114, 115 is less than 10, there is a possibility that the effect of trapping holes in the ceramic of the dielectric layer 111 described below and suppressing the insulation resistance of the dielectric layer 111 may be insufficient. Therefore, as in one embodiment of the present invention, the molar ratio of the transition metal to Sn in the side margin portions 114, 115 is preferably 10 or more, which can significantly improve the moisture resistance reliability of the multilayer electronic component 100.

[0061] On the other hand, the upper limit of the molar ratio of transition metal to Sn in the side margin portions 114 and 115 is not particularly limited, but since excessive addition of transition metal may lead to deterioration of the reliability of the dielectric layer due to the generation of oxygen vacancies, it is preferable that the upper limit be 25 or less.

[0062] There is no particular limitation on the type of transition metal contained in the side margin portions 114, 115. For example, the transition metal may be one or more of Mn, Co, V, Ni, Fe, and alloys thereof.

[0063] Meanwhile, in order to improve the strength and toughness of the side margin parts 114, 115, the content of Sn contained in the side margin parts 114, 115 can be adjusted. In this case, the side margin parts 114, 115 may further contain Ba and Ti, and the content of Sn in the side margin parts 114, 115 is preferably 0.1 moles or more and 3.0 moles or less per 100 moles of Ba. If the content of Sn in the side margin parts 114, 115 is less than 0.1 moles per 100 moles of Ba, the substantial effect of adding Sn is unlikely to be exhibited, and if the content of Sn in the side margin parts 114, 115 is more than 3.0 moles per 100 moles of Ba, the formation of a network between Sn and excessive suppression of grain growth of the dielectric layer may cause a problem of deterioration of impact resistance.

[0064] Meanwhile, the side margin parts 114, 115 may include one or more dielectric grains having a core-shell structure. In this case, a part of Ti in the shell part of the core-shell structure may be substituted with Sn, and the substituted Sn may suppress grain growth of the dielectric grains in the side margin parts 114, 115. This may improve the density of the side margin parts 114, 115.

[0065] In addition, the method of measuring the molar ratio of the transition metal to Sn contained in the side margin portion is not particularly limited. For example, the laminated electronic component 100 is polished to the center in the second direction to expose cross sections in the first and third directions, and then the average Sn content and the average transition metal content are measured in any five or more 5 μm×5 μm regions spaced apart in the first direction of the side margin portions 114 and 115 by SEM-EDX (Scanning Electron Microscope Energy-Dispersive X-ray spectroscopy), and the average molar ratio of the transition metal to Sn is calculated. In this case, the content of each element may be measured in at% or mol%.

[0066] As described above, the dielectric layer 111 may be made of a BaTiO3-based ceramic material, and therefore may contain Ba and Ti. In this case, if moisture from the outside penetrates into the dielectric layer 111, the dielectric layer 111 may reversibly deteriorate in insulation resistance in a hydrated state.

[0067] The hydration of the dielectric ceramic of the dielectric layer 111 containing Ba and Ti is carried out by forming holes (holes, represented by the following chemical formula 1) as follows: [ka] ) is consumed and occurs reversibly, so if the dielectric ceramic has n-type properties, the insulation resistance will deteriorate in a humid environment, whereas if it has p-type properties, the insulation resistance may increase in a humid environment.

[0068] [Chemical formula 1] [ka]

[0069] In one embodiment, the dielectric layer 111 may further include one or more of Dy, Ho, Tb, La, Yb, and Er. This reduces the average grain size of the dielectric grains included in the dielectric layer 111, thereby improving the dielectric constant and improving the high temperature reliability. However, when the dielectric layer 111 further includes one or more additives such as Dy, Ho, Tb, La, Yb, and Er to have n-type properties, the insulation resistance may deteriorate due to hydration of the dielectric ceramic in the dielectric layer 111 as described above. However, according to an embodiment of the present invention, the side margin parts 114 and 115 include Sn and a transition metal, and the molar ratio of the transition metal to Sn in the side margin parts 114 and 115 is 10 or more, so that even if the dielectric layer 111 includes one or more of Dy, Ho, Tb, La, Yb, and Er, the phenomenon of the insulation resistance deteriorating in a hydrated state can be prevented.

[0070] Specifically, when moisture penetrates into the capacitance forming portion Ac, holes in the dielectric ceramic are consumed at the end of the dielectric layer 111 in the third direction, causing hydration and deteriorating the insulation resistance, but when the side margin portions 114, 115 are disposed on the fifth and sixth faces 5, 6 of the body 110 as in one embodiment of the present invention, the transition metal contained in the side margin portions 114, 115 traps holes in the dielectric ceramic of the dielectric layer 111, preventing the hydration reaction. This makes it possible to significantly improve the moisture resistance reliability of the multilayer electronic component 100.

[0071] In one embodiment, the dielectric layer 111 may contain a transition metal. In this case, the transition metal contained in the dielectric layer 111 may be formed by diffusing the transition metal element contained in the side margin portions 114 and 115 to both ends in the third direction of the dielectric layer 111. In this way, by including the transition metal at both ends in the third direction of the dielectric layer 111, which are portions vulnerable to moisture penetration, it is possible to suppress deterioration of the insulation resistance of the dielectric layer 111.

[0072] 5, in one embodiment, the dielectric layer 111 may be divided into a first region 111a adjacent to the fifth and sixth faces and a second region 111b disposed between the first region 111a by the transition metal diffused to both ends in the third direction of the dielectric layer 111, and the molar ratio of the transition metal to Ba contained in the first region 111a may be higher than the molar ratio of the transition metal to Ba contained in the second region 111b. This prevents the occurrence of oxygen vacancies throughout the entire region of the dielectric layer 111, thereby reducing reliability, and improves the moisture resistance reliability of the entire laminated electronic component 100 by trapping holes in the first region 111a, which is vulnerable to moisture penetration.

[0073] Meanwhile, when the content of the transition metal in the dielectric layer 111 including Ba and Ti is excessive, the concentration of oxygen vacancies may increase, and the reliability may be deteriorated. Therefore, rather than controlling the content of the transition metal in the entire region of the dielectric layer 111, it may be advantageous to form the content of the transition metal high only in the regions adjacent to both ends in the third direction of the dielectric layer 111, in order to reduce the concentration of oxygen vacancies in the entire dielectric layer 111 while maintaining the moisture resistance reliability. That is, it is preferable to appropriately control the formation degree of the first region 111a of the dielectric layer, and preferably, the average size of the first region 111a in the third direction may be 50 μm or less.

[0074] The method of dividing the first region 111a and the second region 111b is not particularly limited. For example, in a cross section in the first and third directions polished to the center in the second direction of the laminated electronic component 100, the transition metal content can be measured by SEM-EDX (Scanning Electron Microscope Energy-Dispersive X-ray spectroscopy) analysis from an end in the third direction of an arbitrary dielectric layer to the center in the third direction, and the region with a high transition metal content can be divided into the first region 111a and the region with a low transition metal content can be divided into the second region 111b. In this case, if the dielectric layer 111 further contains Sn, the region at both ends in the third direction of the dielectric layer 111 where the molar ratio of the transition metal to Sn is 10 or more can be divided into the first region 111a, and the other region can be divided into the second region 111b. In this case, the size in the third direction of the dielectric layer 111 is measured from both ends in the third direction to the point where the molar ratio of the transition metal to Sn decreases to less than 10, and this measurement is repeated for any five or more dielectric layers 111 and the average value is taken, thereby measuring the average size in the third direction of the first region 111a.

[0075] The transition metal contained in the dielectric layer 111 can dissolve in the dielectric ceramic of the dielectric layer 111 to generate holes in the lattice, and can increase the trap energy, thereby improving the reliability of the multilayer electronic component 100. However, if the dielectric layer 111 contains an excessive amount of transition metal, the concentration of oxygen vacancies increases, and the reliability may deteriorate. Therefore, in one embodiment, rather than adjusting only the content of the transition metal contained in the dielectric layer 111, the molar ratio of the transition metal to Sn in the side margin parts 114 and 115 is adjusted to be higher than the molar ratio of the transition metal to Sn in the dielectric layer 111, so that the transition metal is concentrated and distributed in the side margin parts 114 and 115 that do not contribute to the formation of capacitance and both ends in the third direction of the dielectric layer 111, thereby suppressing the deterioration of the insulation resistance of the dielectric layer 111 and improving the high-temperature reliability of the multilayer electronic component 100.

[0076] In one embodiment, the dielectric layer 111 and the side margin portions 114, 115 include dielectric grains, and the average grain size of the dielectric grains in the side margin portions 114, 115 may be smaller than the average grain size of the dielectric grains in the dielectric layer 111. This allows the side margin portions 114, 115 to have higher moisture resistance and toughness than the dielectric layer 111. This allows the moisture resistance reliability of the multilayer electronic component 100 to be improved, and the occurrence of cracks to be suppressed.

[0077] The external electrodes 131, 132 may be disposed on a third or fourth surface of the body 110. Specifically, the first external electrode 131 is disposed on the third surface 3 and connected to the first internal electrode 121, and the second external electrode 132 is disposed on the fourth surface 4 and connected to the second internal electrode 122.

[0078] In this embodiment, a structure in which the multilayer electronic component 100 has two external electrodes 131, 132 is described, but the number and shapes of the external electrodes 131, 132 can be changed depending on the configuration of the internal electrodes 121, 122 and other purposes.

[0079] Meanwhile, the external electrodes 131 and 132 may be formed using any material having electrical conductivity, such as a metal, and the specific material may be determined taking into consideration electrical characteristics, structural stability, etc., and may further have a multi-layer structure.

[0080] For example, the external electrodes 131 and 132 may include electrode layers 131a and 132a disposed on the body 110, and plating layers 131b and 132b formed on the electrode layers 131a and 132a.

[0081] As a more specific example of the electrode layers 131a and 132a, the electrode layers may be fired electrodes containing a conductive metal and glass, or may be resin-based electrodes containing a conductive metal and resin.

[0082] Also, the electrode layers 131a and 132a may be in a form in which a fired electrode and a resin-based electrode are sequentially formed on the main body 110. Also, the electrode layers 131a and 132a may be formed by transferring a sheet containing a conductive metal onto the main body 110, or may be formed by transferring a sheet containing a conductive metal onto a fired electrode.

[0083] Materials having excellent electrical conductivity can be used as the conductive metal contained in the electrode layers 131a and 132, but are not particularly limited thereto. For example, the conductive metal may be one or more of nickel (Ni), copper (Cu), and alloys thereof.

[0084] The plating layers 131b and 132b can serve to improve the sealing property or mounting characteristics of the multilayer electronic component 100. The type of the plating layers 131b and 132b is not particularly limited, and may be a plating layer containing one or more of Ni, Sn, Pd, and alloys thereof, or may be formed of a plurality of layers.

[0085] As a more specific example of the plating layers 131b, 132b, the plating layers 131b, 132b may be Ni-containing plating layers or Sn-containing plating layers, and may be in a form in which a Ni-containing plating layer and a Sn-containing plating layer are sequentially formed on the electrode layers 131a, 132a, or in a form in which a Sn-containing plating layer, a Ni-containing plating layer and a Sn-containing plating layer are sequentially formed. The plating layers may also include a plurality of Ni plating layers and / or a plurality of Sn plating layers.

[0086] (Example) In this example, samples were prepared so that the molar ratio of the transition metal to Sn contained in the side margin portion was 1.0, 5.0, and 10.0.

[0087] Specifically, after attaching the ceramic green sheets for forming the side margin portions to the side surfaces of the laminated body 210, they were thermocompressed at a temperature of 50°C to 120°C and sintered in a hydrogen atmosphere. Thereafter, the external electrodes containing Cu were fired, and a plating layer containing Ni and a plating layer containing Sn were formed in this order.

[0088] Table 1 below shows the results of evaluating the moisture resistance reliability of 1200 samples for each test number. The moisture resistance reliability was evaluated by applying a voltage of 4V for 1 hour under conditions of 85℃ and 85% relative humidity, and judging the insulation resistance value to be defective if it decreased by 10^7 times or more of the initial insulation resistance value.

[0089] [Table 1]

[0090] In the results in Table 1 above, Mn was used as the transition metal, but the results can also be applied to Co, V, Ni, and Fe.

[0091] With reference to Test Nos. 1 and 2, when the molar ratio of transition metal to Sn contained in the side margin portion is less than 10.0, the effect of improving moisture resistance reliability increases as the molar ratio of transition metal to Sn increases, but it can be confirmed that this is not sufficient.

[0092] In the case of test number 3, in which the molar ratio of the transition metal to Sn contained in the side margin portion is 10.0, the moisture resistance failure rate is 0 ppm, and it is confirmed that the moisture resistance reliability is significantly improved. Therefore, it can be confirmed that when the molar ratio of the transition metal to Sn contained in the side margin portion is 10.0 or more as in one embodiment of the present invention, the moisture resistance reliability of the multilayer electronic component can be significantly improved.

[0093] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment and the accompanying drawings, but is limited by the scope of the accompanying claims. Therefore, various substitutions, modifications and changes can be made by a person having ordinary knowledge in the art within the scope of the technical idea of ​​the present invention described in the claims, and these also belong to the scope of the present invention.

[0094] In addition, the expression "one embodiment" used in the present invention does not mean the same embodiment, but is provided to emphasize and describe each unique feature that is different from the others. However, the above-mentioned one embodiment does not exclude being realized in combination with the features of another embodiment. For example, even if a matter described in a specific embodiment is not described in another embodiment, it can be understood as a description related to the other embodiment, unless there is a description in the other embodiment that is opposite or contradictory to the matter.

[0095] The terms used in the present invention are merely used to describe one embodiment and are not intended to limit the present invention. In this case, a singular expression includes a plural expression unless the context clearly indicates otherwise. [Explanation of symbols]

[0096] 100: Multilayer electronic components 110: Main unit 111: Dielectric layer 121, 122: Internal electrode 131, 132: External electrode 112, 113: Cover part 114, 115: Side margin 210: Laminated body 220: Ceramic green sheet laminate 211: Ceramic green sheet 221, 222: Internal electrode pattern

Claims

1. a body including dielectric layers including Ba and Ti and internal electrodes alternately disposed with the dielectric layers, the body including a first surface and a second surface facing a first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing a second direction, and a fifth surface and a sixth surface connected to the first surface to the fourth surface and facing a third direction; side margin portions disposed on the fifth surface and the sixth surface; external electrodes disposed on the third surface and the fourth surface; the side margin portion contains Sn and a transition metal, A multilayer electronic component, wherein in the side margin portion, a molar ratio of the transition metal to Sn is 10 or more.

2. the dielectric layer further comprises a transition metal; In the dielectric layer, a region adjacent to the fifth surface and the sixth surface is defined as a first region, and a region disposed between the first regions is defined as a second region.

2. The multilayer electronic component according to claim 1, wherein a molar ratio of the transition metal to Ba contained in said first region is higher than a molar ratio of the transition metal to Ba contained in said second region.

3. 3. The multilayer electronic component according to claim 2, wherein an average size of the first regions in the third direction is 50 μm or less.

4. 2. The multilayer electronic component according to claim 1, wherein the dielectric layer further contains Sn and a transition metal, and includes at least one region at both ends of the dielectric layer in the third direction in which a molar ratio of the transition metal to Sn is 10 or more.

5. The multilayer electronic component according to claim 1 , wherein the dielectric layer further includes at least one of Dy, Ho, Tb, La, Yb, and Er.

6. 2. The multilayer electronic component according to claim 1, wherein the transition metal is at least one of Mn, Co, V, Ni, Fe, and alloys thereof.

7. The side margin portion further contains Ba and Ti, 2. The multilayer electronic component according to claim 1, wherein the content of the Sn in the side margin portion is 0.1 moles or more and 3.0 moles or less per 100 moles of the Ba.

8. the dielectric layer further comprises Sn and a transition metal; 2. The multilayer electronic component according to claim 1, wherein a molar ratio of the transition metal to Sn in said side margin portion is higher than a molar ratio of the transition metal to Sn in said dielectric layer.

9. the dielectric layer and the side margin portion include dielectric grains, 2. The multilayer electronic component according to claim 1, wherein an average grain size of the dielectric grains in the side margin portion is smaller than an average grain size of the dielectric grains in the dielectric layer.

10. 2. The multilayer electronic component according to claim 1, wherein the side margin portion includes one or more dielectric grains having a core-shell structure.

11. The multilayer electronic component according to claim 1 , wherein an average size of the side margin portion in the third direction is 20 μm or less.

12. 11. The multilayer electronic component according to claim 1, wherein the dielectric layers have an average thickness of 0.35 μm or less.

13. 11. The multilayer electronic component according to claim 1, wherein the internal electrodes have an average thickness of 0.35 μm or less.