Primer, printing set, printing method, and printer
A primer composition with cationic resin, polyvalent metal salt, and diethylene glycol alkyl ether compound addresses beading and adhesion issues, ensuring high image quality and gloss on various recording media.
Patent Information
- Application Number
- JP2024028771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-01
AI Technical Summary
Existing primers fail to suppress beading, maintain high image quality, and ensure adequate adhesion to various recording media, particularly non-permeable surfaces, due to insufficient drying of ink, leading to image unevenness.
A primer composition comprising water, a cationic resin, a polyvalent metal salt, and a diethylene glycol alkyl ether compound, with specific drying and formulation conditions to achieve a breaking energy of 20 mJ to 1,000 mJ and elongation of 500% to 2,500%, enhancing adhesion and gloss.
The primer effectively suppresses beading, improves image adhesion, and maintains excellent gloss on diverse recording media, including non-permeable surfaces, by optimizing the primer's mechanical properties.
Smart Images

Figure 2024132919000012 
Figure 2024132919000001 
Figure 2024132919000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a primer, a printing set, a printing method, and a printing apparatus. [Background technology]
[0002] In recent years, as printer speeds have increased, it is expected that image quality degradation such as image unevenness will become an issue due to beading caused by insufficient drying of the ink. Therefore, there is a demand for a new primer that can suppress the occurrence of beading and achieve both high productivity and high image quality. For example, a liquid composition for surface treatment of printed materials, which contains nonionic resin particles and a polyvalent metal salt, has been proposed (see, for example, Patent Document 1). In addition, a reaction liquid has been proposed that contains one or more organic solvents selected from esters, alkylene glycol ethers, cyclic esters, and alkoxyalkylamides, and an aggregating agent that aggregates the components of the ink composition, and is used in a recording method that uses the ink composition (see, for example, Patent Document 2). Summary of the Invention [Problem to be solved by the invention]
[0003] An object of the present invention is to provide a primer that can suppress the occurrence of beading, form an image having excellent glossiness, and improve adhesion between the image and different types of recording media. [Means for solving the problem]
[0004] The primer of the present invention as a means for solving the above-mentioned problems is a primer containing water, a cationic resin, a polyvalent metal salt, and a diethylene glycol alkyl ether compound, and 6 g of the primer is placed in a Teflon (registered trademark) petri dish having a diameter of 50 mm, and dried in a hot air circulating thermostatic chamber at 40°C for one day and then in a hot air circulating thermostatic chamber at 70°C for three days to obtain a dried and solid film, which has a breaking energy of 20 mJ or more and 1,000 mJ or less and a breaking elongation of 500% or more and 2,500% or less, measured as described below. <Measurement of breaking energy and breaking elongation> The dried film is cut into a sample having a size of 5 mm×50 mm using a cutter, and a tensile test is carried out under the following conditions to measure the breaking energy and breaking elongation. -conditions- Equipment: Shimadzu Autograph AG-10N Load cell: 5kN Pull speed: 150mm / min Chuck distance: 4mm Sample width: 5mm Effect of the Invention
[0005] According to the present invention, it is possible to provide a primer that can suppress the occurrence of beading, can form an image having excellent glossiness, and can improve the adhesion of the image to different types of recording media. [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is a schematic diagram showing an example of a printing apparatus of the present invention used in the printing method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] (Primer) The primer of the present invention contains water, a cationic resin, a polyvalent metal salt, and a diethylene glycol alkyl ether compound, and preferably contains a surfactant, and further contains other components as required. In the present invention, the "primer" may be referred to as a "treatment liquid," a "pretreatment liquid," a "composition liquid," a "reaction liquid," or a "liquid composition."
[0008] The liquid composition for surface treatment of Patent Document 1 (JP 2021-000790 A), which is a conventional technology, contains nonionic resin particles and does not contain a diethylene glycol alkyl ether compound. In addition, the reaction liquid of Patent Document 2 (JP 2021-120219 A), which is a conventional technology, does not use a diethylene glycol alkyl ether compound and a cationic resin in combination. Therefore, in the conventional technology, the occurrence of beading cannot be suppressed, the glossiness of the image is reduced, and the adhesion of the image to different types of recording media cannot be improved.
[0009] In the present invention, 6 g of the primer is placed in a Teflon (registered trademark) petri dish having a diameter of 50 mm, and dried in a hot air circulating thermostatic chamber at 40°C for one day and then in a hot air circulating thermostatic chamber at 70°C for three days to obtain a dried and solid film, which has a breaking energy of 20 mJ or more and 1,000 mJ or less and a breaking elongation of 500% or more and 2,500% or less, measured as described below. The breaking energy is preferably 100 mJ or more and 500 mJ or less.The breaking elongation is preferably 500% or more and 1,000% or less. <Measurement of breaking energy and breaking elongation> The dried film is cut into a sample having a size of 5 mm×50 mm using a cutter, and a tensile test is carried out under the following conditions to measure the breaking energy and breaking elongation. -conditions- Equipment: Shimadzu Autograph AG-10N Load cell: 5kN Pull speed: 150mm / min Chuck distance: 4mm Sample width: 5mm
[0010] In the present invention, the breaking energy of the dried and solid film of the primer is 20 mJ or more and 1,000 mJ or less, and the breaking elongation is 500% or more and 2,500% or less, so that the occurrence of beading can be suppressed, an image with excellent glossiness can be formed, and the adhesion of the image to different types of recording media can be improved. The cationic resin contained in the primer preferably has a highly polar monomer in the resin skeleton in order to improve the adhesive energy between the image and a recording medium of a different type and to enhance the adhesion between the image and the recording medium of a different type. In addition, in order to prevent the image from cracking when a recording medium of a different type is used and to allow the image to follow the recording medium, the number average molecular weight of the cationic resin is preferably 10,000 or more and 200,000 or less. In addition, the cationic resin preferably contains a monomer having a rigid skeleton such as a phenyl group. Furthermore, in order to improve the flexibility of the primer layer and to enhance the adhesion between the image and the recording medium of a different type, it is preferable to select a resin having a low glass transition temperature, a low elastic modulus, or a high breaking elongation. By using such a cationic resin, the breaking energy and breaking elongation of the dried and solidified film of the primer can be adjusted to a breaking energy of 20 mJ or more and 1,000 mJ or less and a breaking elongation of 500% or more and 2,500% or less.
[0011] <Water> Examples of water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, and ultrapure water. The water content in the primer is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of drying property and ejection reliability of the primer, however, it is preferably 10% by mass or more and 80% by mass or less, and more preferably 30% by mass or more and 60% by mass or less.
[0012] <Diethylene glycol alkyl ether compound> A diethylene glycol alkyl ether compound is used as the organic solvent. Examples of the diethylene glycol alkyl ether compound include diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monopentyl ether, diethylene glycol monohexyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, and diethylene glycol butyl methyl ether. These may be used alone or in combination of two or more. Among these, diethylene glycol diethyl ether is preferred from the viewpoint of the glossiness of the image and the adhesion between the image and different types of recording media. The content of the diethylene glycol alkyl ether compound is preferably 5% by mass to 30% by mass, more preferably 15% by mass to 30% by mass, based on the total amount of the primer. When the content of the diethylene glycol alkyl ether compound is 5% by mass to 30% by mass, an image having excellent glossiness can be formed, and adhesion between the image and different types of recording media is improved.
[0013] The primer of the present invention can use other organic solvents in addition to the diethylene glycol alkyl ether compound. Examples of the other organic solvents include polyhydric alcohols, ethers such as polyhydric alcohol alkyl ethers and polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, and sulfur-containing compounds. Examples of the other organic solvents include ethylene glycol, diethylene glycol, propylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, 3-methoxy-3-methyl-1-butanol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, and the like. Polyhydric alcohols such as diol, 1,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol. Examples of the compounds include alcohols, polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether, polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether, nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone, amides such as formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide, amines such as monoethanolamine, diethanolamine, and triethylamine, sulfur-containing compounds such as dimethyl sulfoxide, sulfolane, and thiodiethanol, propylene carbonate, and ethylene carbonate. These compounds may be used alone or in combination of two or more.
[0014] The content of the organic solvent (including the diethylene glycol alkyl ether compound) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 10% by mass to 60% by mass, and more preferably from 20% by mass to 60% by mass, based on the total amount of the primer.
[0015] <Polyvalent metal salts> The polyvalent metal salt is composed of a divalent or higher polyvalent metal ion, preferably a carboxylate ion or a nitrate ion, and is soluble in water.
[0016] The carboxylic acid in the carboxylate ion is preferably a saturated aliphatic monocarboxylic acid. Examples of the saturated aliphatic monocarboxylic acid include formic acid, acetic acid, propionic acid, butyric acid, isobutyric acid, valeric acid, isovaleric acid, pivalic acid, and hexanoic acid. These may be used alone or in combination of two or more.
[0017] Examples of polyvalent metal ions include Ca. 2+ , Cu 2+ , Ni 2+ , Mg 2+ , Zn 2+ , B.A. 2+ Divalent metal ions such as Al 3+ , Fe 3+ , Cr 3+ and the like trivalent metal ions.
[0018] Examples of the polyvalent metal salt include calcium carbonate, calcium nitrate, calcium chloride, calcium acetate, calcium sulfate, magnesium chloride, magnesium acetate, magnesium nitrate, magnesium sulfate, barium sulfate, zinc sulfide, zinc carbonate, aluminum chloride, aluminum nitrate, and hydrates thereof, etc. Among these, magnesium acetate or a hydrate thereof is preferred from the viewpoints of the glossiness of the image and the adhesion between the image and different types of recording media. The content of the polyvalent metal salt is preferably from 0.25% by mass to 10% by mass, and more preferably from 0.5% by mass to 5% by mass, based on the total amount of the primer.
[0019] <Cationic resin> The resin used in the primer preferably has a highly polar monomer in the resin skeleton in order to improve the adhesive energy between the image and the recording medium and thereby increase the adhesion. In addition, it is preferable to select a resin having a low glass transition temperature, a low elastic modulus, or a high breaking elongation in order to improve the flexibility of the primer layer and increase the adhesion between the image and a different type of recording medium. Among these, cationic resins are preferably used in terms of the gloss of the image and the adhesion between the image and a different type of recording medium.
[0020] The cationic resin is a resin having a cationic substituent, and examples thereof include cationic urethane resins, cationic olefin resins, cationic allylamine resins, etc. Among these, cationic urethane resins are preferred from the viewpoints of the glossiness of the image and the adhesion between the image and different types of recording media. The cationic resin may be a commercially available product, such as Hydran CP-7010, CP-7020, CP-7030, CP-7040, CP-7050, CP-7060, or CP-7610 (all manufactured by DIC Corporation); or aqueous urethane dispersion WBR-2120C or WBR-2122C (all manufactured by Taisei Fine Chemical Co., Ltd.).
[0021] The cationic resin is preferably mixed with materials such as an organic solvent in a resin emulsion state in which the cationic resin is dispersed using water as a dispersion medium to obtain a primer. Considering the ease of preparation of the primer by blending with the organic solvent and water, and dispersing the resin as uniformly as possible in the primer, it is preferable to add the resin to the primer in a resin emulsion state in which the resin particles are stably dispersed using water as a dispersion medium.
[0022] The cationic resin can be easily formed into a film by dissolving it in an organic solvent added to the primer. The film formation of the resin particles is promoted with the evaporation of the organic solvent and water contained in the primer. When dispersing the cationic resin in water as a dispersion medium, the resin particles may be forced emulsification type resin particles using a dispersant, or so-called self-emulsification type resin particles having a cationic group in the molecular structure, etc. Among these, self-emulsification type resin particles having a cationic group in the molecular structure are preferred from the viewpoint of increasing the strength of the printed matter.
[0023] The number average molecular weight of the cationic resin is preferably from 10,000 to 200,000 in terms of adhesion between different types of recording media and images. The number average molecular weight of the cationic resin can be measured, for example, by gel permeation chromatography (GPC). The content of the cationic resin is preferably 2% by mass or more and 15% by mass or less based on the total amount of the primer.
[0024] <Surfactant> The surfactant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include a compound having a hydrophilic group or a hydrophilic polymer chain on the side chain of a compound (silicone compound) having a polysiloxane structure such as polydimethylsiloxane, and a compound having a hydrophilic group or a hydrophilic polymer chain on the end of a compound (silicone compound) having a polysiloxane structure such as polydimethylsiloxane. Note that the compound having a polysiloxane structure may have a polysiloxane structure in its structure, and includes polysiloxane surfactants.
[0025] Examples of the hydrophilic group or the hydrophilic polymer chain include a polyether group (polyethylene oxide, polypropylene oxide, or a copolymer thereof, etc.), polyglycerin (CHO(CHCH(OH)CHO) n -H, etc.), pyrrolidone, betaine (C3H6N + (C2H4)2-CH2COO-, etc.), sulfates (C3H6O(C2H4O) n -SO3Na, etc.), phosphates (C3H6O(C2H4O) n -P(=O)OHONa, etc.), quaternary salts (C3H6N + (C2H4)3Cl- In the above chemical formula, n represents an integer of 1 or more. Among these, polyether groups are preferred. Other suitable examples include vinyl copolymers having silicone compound chains such as polydimethylsiloxane in their side chains, which are obtained by copolymerizing polydimethylsiloxane or the like having a polymerizable vinyl group at the end with other copolymerizable monomers (at least a portion of the monomers preferably contains a hydrophilic monomer such as (meth)acrylic acid or a salt thereof). Among these, a compound having a polysiloxane structure and a hydrophilic polymer chain is preferred, and it is more preferred that the hydrophilic polymer chain contains a polyether group. Particularly preferred is a polysiloxane surfactant having a methylpolysiloxane structure as a hydrophobic group and a nonionic surfactant having a polyoxyethylene structure as a hydrophilic group.
[0026] Examples of the polysiloxane surfactant include polyether-modified silicones and polyoxyalkylene group-containing silicone compounds. As the polysiloxane surfactant, commercially available products can be used. Examples of the commercially available products include Silface SAG503A, Silface SAG005, and Silface SAG008 (all manufactured by Nissin Chemical Industry Co., Ltd.); FZ2110, FZ2166, SH-3772M, L7001, and SH-3773M (all manufactured by Toray Dow Co., Ltd.); KF-353, KF-945, and KF-6017 (all manufactured by Shin-Etsu Chemical Co., Ltd.); and FormBan MS-575 (manufactured by Ultra Additives Inc.). These may be used alone or in combination of two or more.
[0027] The content of the surfactant is preferably 0.1% by mass to 4% by mass, more preferably 1% by mass to 2% by mass, based on the total amount of the primer. When the content is 0.1% by mass to 4% by mass, the combined use of the surfactant and the diethylene glycol alkyl ether compound can improve the adhesion between different types of recording media and the image, and can also improve the image quality such as gloss. The mass ratio of the surfactant to the cationic resin (surfactant:cationic resin) is preferably 1:4 to 1:20, and more preferably 1:5 to 1:10, from the viewpoints of the glossiness of the image and the adhesion between the image and different types of recording media.
[0028] <Other ingredients> The other components are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other components include antiseptic and antifungal agents, antifoaming agents, rust inhibitors, and pH adjusters.
[0029] - Defoaming agent - The defoaming agent is not particularly limited, and examples thereof include silicone-based defoaming agents, polyether-based defoaming agents, and fatty acid ester-based defoaming agents. These may be used alone or in combination of two or more. Among these, silicone-based defoaming agents are preferred because of their excellent foam breaking effect.
[0030] -Preservative and fungicidal agent- The antiseptic and antifungal agent is not particularly limited, and examples thereof include 1,2-benzisothiazolin-3-one.
[0031] -Rust inhibitor- The rust inhibitor is not particularly limited, and examples thereof include acid sulfite and sodium thiosulfate.
[0032] -pH adjuster- There are no particular limitations on the pH adjuster, so long as it is capable of adjusting the pH to 7 or higher, and examples of the pH adjuster include amines such as diethanolamine and triethanolamine.
[0033] The primer of the present invention can be prepared by mixing water, a cationic resin, a polyvalent metal salt, a diethylene glycol alkyl ether compound, a surfactant, and further other components as necessary, and stirring and mixing as necessary. Stirring and mixing can be performed, for example, with a stirrer having stirring blades, a magnetic stirrer, a high-speed disperser, or the like.
[0034] -Primer properties- The physical properties of the primer are not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferable that the surface free energy γ, viscosity, pH, etc. are within the following ranges. The surface free energy γ of the primer at 25°C is set to 45 mJ / m2 in terms of adhesion between different types of recording media and images. 2 It is preferable that the concentration is less than 40 mJ / m 2 The following is more preferred: The surface free energy γ was measured by measuring the contact angle at 25°C using a FAMAS automatic contact angle meter (DMo-501, manufactured by Kyowa Interface Science Co., Ltd.) using polyvinyl chloride (GIY-11Z5, manufactured by Lintec Corporation) as a recording medium, and creating a Zisman plot to obtain the surface tension γc (critical surface tension) when cosθ=1 (θ=0), i.e., the surface free energy (mJ / m 2 ) can be obtained. The viscosity of the primer at 25° C. is preferably from 5 mPa·s to 20 mPa·s, and more preferably from 5 mPa·s to 15 mPa·s, in order to obtain good dischargeability. Here, the viscosity can be measured using, for example, a rotational viscometer (RE-550L, manufactured by Toki Sangyo Co., Ltd.). The measurement conditions are 25°C, standard cone rotor (1°34' x R24), sample liquid volume 1.2 mL, rotation speed 50 rpm, and measurement can be performed for 3 minutes. The pH of the primer is preferably 7 to 12, and more preferably 8 to 11, from the viewpoint of preventing corrosion of metal members that come into contact with the liquid.
[0035] In addition, the qualitative and quantitative methods of the diethylene glycol alkyl ether compound, cationic resin, polyvalent metal salt, surfactant, and other components contained in the primer of the present invention include, for example, gas chromatography mass spectrometry (GC-MS). As a measuring device using gas chromatography mass spectrometry (GC-MS), for example, GCMS-QP2020NX (manufactured by Shimadzu Corporation) can be mentioned. In addition, the water contained in the primer can be measured by a general method such as the quantitative determination of volatile components by gas chromatography mass spectrometry (GC-MS) and mass fluctuation by thermogravimetry-differential thermal analysis (TG-DTA).
[0036] (Print set) The printing set of the present invention comprises the primer of the present invention and an ink containing a coloring material and an organic solvent. The printing set of the present invention can be suitably used in various printing devices using an inkjet printing method, such as printers, facsimile machines, copying machines, printer / fax / copier combination machines, and three-dimensional modeling devices.
[0037] <Ink> The ink contains a coloring material and an organic solvent, and preferably contains water, a resin, and additives, and may contain other components as necessary.
[0038] -Organic solvents- The organic solvent is not particularly limited, and any water-soluble organic solvent can be used. Examples of the organic solvent include polyhydric alcohols, ethers such as polyhydric alcohol alkyl ethers and polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, and sulfur-containing compounds.
[0039] Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, Examples of such glycerol include 2,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol. Examples of polyhydric alcohol alkyl ethers include ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether. Examples of polyhydric alcohol aryl ethers include ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether. Examples of the nitrogen-containing heterocyclic compound include 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone. Examples of amides include formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide. Examples of the amines include monoethanolamine, diethanolamine, and triethylamine. Examples of sulfur-containing compounds include dimethyl sulfoxide, sulfolane, and thiodiethanol. Other organic solvents include, for example, propylene carbonate, ethylene carbonate, and the like. It is preferable to use an organic solvent having a boiling point of 250° C. or less, since this not only functions as a wetting agent but also provides good drying properties.
[0040] As the organic solvent, polyol compounds having 8 or more carbon atoms and glycol ether compounds are also preferably used. Polyol compounds having 8 or more carbon atoms and glycol ether compounds can improve the permeability of the ink when paper is used as the recording medium.
[0041] Examples of polyol compounds having 8 or more carbon atoms include 2-ethyl-1,3-hexanediol and 2,2,4-trimethyl-1,3-pentanediol. Examples of glycol ether compounds include polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; and polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether.
[0042] The content of the organic solvent is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of the drying property and ejection reliability of the ink, however, the content is preferably from 10% by mass to 60% by mass, and more preferably from 20% by mass to 60% by mass, of the total amount of the ink.
[0043] -Coloring materials- The coloring material is not particularly limited and can be appropriately selected depending on the purpose. For example, a pigment, a pigment dispersion, a dye, etc. can be used.
[0044] --Pigments-- As the pigment, an inorganic pigment or an organic pigment can be used. These pigments can be used alone or in combination of two or more. Also, mixed crystals can be used as the pigment.
[0045] Examples of pigments that can be used include black pigments, yellow pigments, magenta pigments, cyan pigments, white pigments, green pigments, orange pigments, glossy pigments such as gold and silver pigments, and metallic pigments.
[0046] Examples of the inorganic pigment that can be used include titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, and chrome yellow, as well as carbon black produced by a known method such as a contact method, a furnace method, or a thermal method.
[0047] Examples of the organic pigment include azo pigments, polycyclic pigments (e.g., phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, etc.), dye chelates (e.g., basic dye type chelates, acid dye type chelates, etc.), nitro pigments, nitroso pigments, and aniline black.
[0048] Among these pigments, those having good affinity with solvents such as organic solvents and water are preferably used. In addition, resin hollow particles or inorganic hollow particles can also be used.
[0049] Specific examples of pigments for black colors include carbon blacks (CI Pigment Black 7) such as furnace black, lamp black, acetylene black, and channel black; metals such as copper, iron (CI Pigment Black 11), and titanium oxide; and organic pigments such as aniline black (CI Pigment Black 1). For color, CI Pigment Yellow 1, 3, 12, 13, 14, 17, 24, 34, 35, 37, 42 (yellow iron oxide), 53, 55, 74, 81, 83, 95, 97, 98, 100, 101, 104, 108, 109, 110, 117, 120, 138, 150, 153, 155, 180, 185, 213; CI Pigment Orange CI Pigment Red 1, 2, 3, 5, 17, 22, 23, 31, 38, 48:2 (Permanent Red 2B (Ca)), 48:3, 48:4, 49:1, 52:2, 53:1, 57:1 (Brilliant Carmine 6B), 60:1, 63:1, 63:2, 64:1, 81, 83, 88, 101 ( 104, 105, 106, 108 (Cadmium Red), 112, 114, 122 (Quinacridone Magenta), 123, 146, 149, 166, 168, 170, 172, 177, 178, 179, 184, 185, 190, 193, 202, 207, 208, 209, 213, 219, 224, 254, 264; CI Pigmen CI Pigment Blue 1, 2, 15 (Phthalocyanine Blue), 15:1, 15:2, 15:3, 15:4 (Phthalocyanine Blue), 16, 17:1, 56, 60, 63; CI Pigment Green 1, 4, 7, 8, 10, 17, 18, 36, etc.
[0050] --Pigment Dispersion-- The pigment dispersion can be obtained by mixing and dispersing water, an organic solvent, a pigment, a pigment dispersant, and, if necessary, other components, and adjusting the particle size. The method for dispersing the pigment to prepare the pigment dispersion is not particularly limited and may be appropriately selected from known methods. Examples of the method include a method in which the pigment is mixed with materials such as water and an organic solvent, and a method in which the pigment is mixed with other materials such as water and a pigment dispersant to prepare a pigment dispersion, and then the resulting mixture is mixed with materials such as water and an organic solvent. The dispersion is preferably carried out using a dispersing machine. In addition, it is preferable to filter out coarse particles from the pigment dispersion using a filter or a centrifugal separator, and to degas the pigment dispersion, if necessary.
[0051] The particle size of the pigment in the pigment dispersion is not particularly limited and may be appropriately selected depending on the purpose. However, in terms of improving the dispersion stability of the pigment and improving the ejection stability and image quality such as image density, the maximum frequency of the particle size of the pigment in the pigment dispersion, calculated in terms of the maximum number, is preferably from 20 nm to 500 nm, and more preferably from 20 nm to 150 nm. The particle size of the pigment in the pigment dispersion can be measured using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrack Bell Co., Ltd.).
[0052] The content of the pigment in the pigment dispersion is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of obtaining good ejection stability and increasing image density, the content is preferably from 0.1% by mass to 60% by mass, and more preferably from 0.1% by mass to 50% by mass.
[0053] --dye-- The dye is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include acid dyes, direct dyes, reactive dyes, basic dyes, etc. These may be used alone or in combination of two or more kinds.
[0054] Specific examples of dyes include CI Acid Yellow 17, 23, 42, 44, 79, 142; CI Acid Red 52, 80, 82, 249, 254, 289; CI Acid Blue 9, 45, 249; CI Acid Black 1, 2, 24, 94; CI Food Black 1, 2; CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 14 4, 173; CI Direct Red 1, 4, 9, 80, 81, 225, 227; CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202; CI Directed Black 19, 38, 51, 71, 154, 168, 171, 195; CI Reactive Red 14, 32, 55, 79, 249; CI Reactive Black 3, 4, 35, etc.
[0055] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of good fixation, color development, and ejection stability, the content is preferably from 0.1% by mass to 15% by mass, and more preferably from 1% by mass to 10% by mass, based on the total amount of the ink.
[0056] The method of dispersing a pigment to obtain an ink is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method of introducing a hydrophilic functional group into a pigment to make it a self-dispersing pigment, a method of coating the surface of the pigment with a resin and dispersing it, and a method of dispersing the pigment using a dispersant.
[0057] Examples of methods for introducing a hydrophilic functional group into a pigment to make it a self-dispersing pigment include a method in which a functional group such as a sulfone group or a carboxyl group is added to a pigment (e.g., carbon) to make it dispersible in water.
[0058] Examples of the method for dispersing a pigment by coating its surface with a resin include a method for encapsulating the pigment in a microcapsule to make it dispersible in water. This can be called a resin-coated pigment. In this case, the pigment to be blended in the ink does not need to be entirely coated with a resin, and pigments that are not coated with a resin or pigments that are partially coated with a resin may be dispersed in the ink as long as the effect of the present invention is not impaired.
[0059] Examples of the method for dispersing a pigment using a dispersant include a method for dispersing a pigment using a known low molecular weight dispersant, such as a surfactant, and a method for dispersing a pigment using a known polymeric dispersant. The dispersant is not particularly limited and can be appropriately selected depending on the pigment, and can be, for example, anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. These can be used alone or in combination of two or more kinds. The dispersant may be a synthetic one or a commercially available one. The commercially available dispersant may be, for example, New Calgen D-1203 (Takemoto Oil & Fat Co., Ltd., nonionic surfactant). Na naphthalenesulfonate formalin condensate may also be suitably used as the dispersant.
[0060] -water- As the water, for example, pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, or ultrapure water can be used. The water content is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of the drying property and ejection reliability of the ink, however, the water content is preferably from 10% by mass to 90% by mass, and more preferably from 20% by mass to 60% by mass, of the total amount of the ink.
[0061] -resin- The type of resin contained in the ink is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include urethane resin, polyester resin, acrylic resin, vinyl acetate resin, styrene resin, butadiene resin, styrene-butadiene resin, vinyl chloride resin, acrylic styrene resin, acrylic silicone resin, etc. Resin particles made of these resins may also be used. Ink can be obtained by mixing resin particles in a resin emulsion state, in which the resin particles are dispersed in water as a dispersion medium, with materials such as coloring materials and organic solvents. As the resin particles, appropriately synthesized ones or commercially available ones may be used.
[0062] The volume average particle size of the resin particles is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of obtaining good fixing property and high image hardness, however, it is preferably from 10 nm to 1,000 nm, more preferably from 10 nm to 200 nm, and particularly preferably from 10 nm to 100 nm.
[0063] The resin content is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of fixation property and storage stability of the ink, however, the resin content is preferably from 1% by mass to 30% by mass, and more preferably from 5% by mass to 20% by mass, of the total amount of the ink.
[0064] There are no particular limitations on the particle size of the solid content in the ink and it can be appropriately selected depending on the purpose. However, from the viewpoint of improving image quality such as ejection stability and image density, the maximum frequency calculated in terms of the maximum number is preferably 20 nm or more and 1,000 nm or less, and more preferably 20 nm or more and 150 nm or less. The solid content includes resin particles, pigment particles, etc. The volume average particle size and the maximum frequency in terms of the maximum number can be measured, for example, using a particle size analyzer (Microtrac MODEL UPA9340, manufactured by Nikkiso Co., Ltd.).
[0065] -Additives- If necessary, surfactants, antifoaming agents, antiseptic and antifungal agents, rust inhibitors, pH adjusters, etc. may be added to the ink.
[0066] --Surfactant-- As the surfactant, a silicone-based surfactant, a fluorine-based surfactant, an amphoteric surfactant, a nonionic surfactant, etc. can be used. The silicone surfactant is not particularly limited and can be appropriately selected according to the purpose. Among them, those that do not decompose even at high pH are preferable. Examples of silicone surfactants include side chain modified polydimethylsiloxane, both end modified polydimethylsiloxane, one end modified polydimethylsiloxane, and both end modified polydimethylsiloxane of side chain. Those having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modified group are particularly preferable because they show good properties as an aqueous surfactant. In addition, polyether modified silicone surfactants can also be used as silicone surfactants, and examples thereof include compounds in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylsiloxane.
[0067] As the fluorosurfactant, for example, perfluoroalkylsulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in the side chain are particularly preferred because they have low foaming properties. As the perfluoroalkylsulfonic acid compounds, for example, perfluoroalkylsulfonic acid, perfluoroalkyl sulfonate, etc. are included. As the perfluoroalkyl carboxylic acid compounds, for example, perfluoroalkyl carboxylic acid, perfluoroalkyl carboxylate, etc. are included. As the polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in the side chain, sulfate ester salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups in the side chains, salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups in the side chains, etc. are included. As the counter ions of the salts in these fluorosurfactants, Li, Na, K, NH4, NH3CH2CH2OH, NH2(CH2CH2OH)2, NH(CH2CH2OH)3, etc. are included.
[0068] Examples of amphoteric surfactants include lauryl aminopropionate, lauryl dimethyl betaine, stearyl dimethyl betaine, and lauryl dihydroxyethyl betaine. Examples of nonionic surfactants include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyoxyethylene propylene block polymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and ethylene oxide adducts of acetylene alcohol.
[0069] The content of the surfactant is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of achieving excellent wettability and ejection stability and improving image quality, the content is preferably from 0.001% by mass to 5% by mass, and more preferably from 0.05% by mass to 5% by mass, relative to the total amount of ink.
[0070] --Antifoaming agent-- The defoaming agent is not particularly limited, and examples thereof include silicone-based defoaming agents, polyether-based defoaming agents, and fatty acid ester-based defoaming agents. These may be used alone or in combination of two or more. Among these, silicone-based defoaming agents are preferred because of their excellent foam breaking effect.
[0071] --Preservative and fungicidal agent-- The antiseptic and antifungal agent is not particularly limited and can be appropriately selected depending on the purpose. For example, 1,2-benzisothiazolin-3-one and the like can be mentioned.
[0072] --Rust inhibitor-- The rust inhibitor is not particularly limited and can be appropriately selected depending on the purpose. Examples of the rust inhibitor include acid sulfite and sodium thiosulfate.
[0073] --pH adjuster-- There are no particular limitations on the pH adjuster, so long as it is capable of adjusting the pH to 7 or higher, and examples of the pH adjuster include amines such as diethanolamine and triethanolamine.
[0074] -Ink properties- The physical properties of the ink are not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferable that the viscosity, surface tension, pH, etc. are within the following ranges. The viscosity of the ink at 25° C. is preferably from 5 mPa·s to 30 mPa·s, and more preferably from 5 mPa·s to 25 mPa·s, in order to improve the print density and character quality and to obtain good ejection properties. Here, the viscosity can be measured using, for example, a rotational viscometer (RE-80L, manufactured by Toki Sangyo Co., Ltd.). The measurement conditions are 25°C, standard cone rotor (1°34' x R24), sample liquid volume 1.2 mL, rotation speed 50 rpm, and measurement can be performed for 3 minutes. The surface tension of the ink is preferably 35 mN / m or less, and more preferably 32 mN / m or less at 25° C., in order to ensure that the ink is appropriately leveled on the recording medium and the drying time of the ink is shortened. The pH of the ink is preferably from 7 to 12, and more preferably from 8 to 11, from the viewpoint of preventing corrosion of metal members that come into contact with the ink.
[0075] Examples of the qualitative and quantitative methods for the organic solvents, resins, coloring materials, and other components contained in the ink include gas chromatography mass spectrometry (GC-MS). Examples of measuring devices using gas chromatography mass spectrometry (GC-MS) include GCMS-QP2020NX (manufactured by Shimadzu Corporation). In addition, the water contained in the ink can be measured by general methods such as the quantitative determination of volatile components using gas chromatography mass spectrometry (GC-MS) and mass fluctuation using thermogravimetry-differential thermal analysis (TG-DTA).
[0076] <Printed material> The printed matter used in the present invention has an image formed on a recording medium using the printing set of the present invention. The printed matter can be obtained by printing on the recording medium using the printing device and printing method of the present invention.
[0077] <Recording Media> The recording medium is not particularly limited, and normal paper, glossy paper, special paper, cloth, etc. can be used, but good images can also be formed using non-permeable recording media. There are recording media obtained using various materials as non-permeable recording media, and the wettability when a primer is applied varies depending on the material present on the surface. According to the present invention, even when using such recording media with different wettability, it is possible to form a primer layer with good adhesion. The wettability of the recording medium can be evaluated, for example, by measuring the contact angle between the recording medium and the primer, or by the method disclosed in JP2012-78190A. A non-permeable recording medium is a recording medium with a surface that is low in water permeability and absorbency. It also includes materials that have many cavities inside but are not open to the outside. More quantitatively, in the Bristow method, 1 / 2 Water absorption up to 10mL / m 2 This refers to a recording medium that is: As the non-permeable recording medium, for example, a plastic film such as a polyvinyl chloride resin film, a polyethylene terephthalate (PET) film, a polypropylene film, a polyethylene film, or a polycarbonate film can be suitably used.
[0078] Examples of polypropylene and polyethylene include AR1025, AR1056, AR1082, EC1082, 1082D, 1073D, 1056D, 1025D, and FR1073 (all of which are manufactured by Asahi DuPont Flashspan). P2002, P2102, P2108, P2161, P2171, P2111, P4266, P5767, P3162, P6181, P8121, P1162, P1111, P1128, P1181, P1153, P1157, P1146, P1147, P1171 (all manufactured by Toyobo Co., Ltd.); YPI, Aqua Yupo, Super Yupo, Ultra Yupo, New Yupo, Yupo Illumination Paper, Yupo Building Materials Paper, Yupo High Gloss, Yupo Jet, Metallic Yupo (all manufactured by Yupo Corporation). These may be used alone or in combination of two or more.
[0079] (Printing method and printing device) The printing method of the present invention includes a primer applying step and an ink applying step, and may further include other steps as necessary. The printing apparatus of the present invention comprises a primer applying means and an ink applying means, and further comprises other means as required.
[0080] The printing method of the present invention can be suitably carried out by the printing apparatus of the present invention, and the primer application step can be carried out by a primer application means, the ink application step can be carried out by an ink application means, and the other steps can be carried out by other means.
[0081] Printing devices and printing methods also include desktop or wide-width printing devices capable of printing on A0-sized recording media, such as continuous feed printers that can use continuous paper wound into a roll as the recording medium.
[0082] <Primer application step and primer application means> The primer application step is a step of applying the primer of the present invention onto a recording medium, and is carried out by a primer application means.
[0083] The method of applying the primer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include the inkjet method, blade coating method, gravure coating method, gravure offset coating method, bar coating method, roll coating method, spray coating method, knife coating method, air knife coating method, comma coating method, U comma coating method, AKKU coating method, smoothing coating method, microgravure coating method, reverse roll coating method, four-roll coating method, five-roll coating method, dip coating method, curtain coating method, slide coating method, and die coating method. Among these, the inkjet method is preferred because it can apply the primer uniformly over the entire recording medium and can apply the minimum amount required by adjusting the droplet size.
[0084] The recording medium to which the primer has been applied may be heated to dry the primer as necessary, but heating is not required.
[0085] The amount of primer applied to the recording medium is 1 g / m 2 More than 15g / m 2 Less than 3 g / m is preferred. 2 More than 10g / m 2 The following is more preferred:
[0086] <Ink application process and ink application means> The ink application step is a step of applying an ink containing a coloring material and an organic solvent onto the recording medium to which the primer has been applied, and is carried out by an ink application unit. In the present invention, a primer is applied onto a recording medium, and then an ink is applied to the recording medium. Note that the ink may be applied before or after the primer has dried.
[0087] The method of applying the ink is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include an inkjet method, a blade coating method, a gravure coating method, a gravure offset coating method, a bar coating method, a roll coating method, a knife coating method, an air knife coating method, a comma coating method, a U comma coating method, an AKKU coating method, a smoothing coating method, a microgravure coating method, a reverse roll coating method, a four-roll coating method, a five-roll coating method, a dip coating method, a curtain coating method, a slide coating method, a die coating method, etc. Among these, the inkjet method is preferred from the viewpoints of the maintainability of the equipment and the working efficiency.
[0088] <Other steps and other means> The other means are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other means include a heating means and a transport means. The other steps are not particularly limited and can be appropriately selected depending on the purpose. For example, a heating step, a transporting step, etc. can be mentioned.
[0089] -Heating process and heating means- In the printing method of the present invention, it is preferable to have a heating step after the ink application step. Examples of the heating means include a roll heater, a drum heater, hot air, a hot plate, and the like. The heating step is preferably performed at a temperature of 60° C. to 80° C. in order to obtain a sufficient drying effect and not to damage the recording medium. The heating time is preferably from 10 seconds to 10 minutes, more preferably from 1 minute to 2 minutes, in order to obtain a sufficient drying effect and not to damage the recording medium.
[0090] Here, an embodiment of the printing device of the present invention used in the printing method of the present invention will be described in detail with reference to the drawings. Note that in each drawing, the same components are given the same reference numerals, and duplicated explanations may be omitted. In addition, the number, position, shape, etc. of the following components are not limited to this embodiment, and may be any number, position, shape, etc. that is preferable for implementing the present invention.
[0091] 1 is a schematic diagram showing an example of a printing apparatus of the present invention used in the printing method of the present invention. Note that the ink application step and the primer application step in the printing method of the present invention may be performed in the same printing apparatus or in separate printing apparatuses.
[0092] 1 includes a primer application unit 110, an ink application unit 120, a post-treatment liquid application unit 130, a drying unit 140, and a transport unit 150, and the primer application unit 110 applies a primer to the recording medium M. Note that the primer application unit 110, the post-treatment liquid application unit 130, the drying unit 140, and the transport unit 150 may be omitted.
[0093] The method of applying the primer is not particularly limited and can be appropriately selected depending on the purpose, but the inkjet method is preferable. Note that the primer may be applied to the recording medium manually in advance by a bar coating method or the like, and then printed using a printing device, so the primer application unit 110 may be omitted.
[0094] The recording medium M used for recording is not particularly limited and can be appropriately selected depending on the purpose. Examples include plain paper, glossy paper, special paper, cardboard, cloth, film, OHP sheets, and general-purpose printing paper. The present invention is particularly effective in non-permeable recording media where beading is likely to occur. In the present invention, the term "non-permeable recording medium" refers to a recording medium having a surface with low water permeability and low absorbency, and includes materials that have many cavities inside but are not open to the outside. More quantitatively, the Bristow method is used to determine the degree of penetration of the material within 30 msec from the start of contact. 1 / 2 Water absorption up to 10mL / m 2 The present invention refers to a recording medium that is: As the non-permeable recording medium, for example, polyvinyl chloride resin film, polyethylene terephthalate (PET) film, polypropylene, polyethylene, polycarbonate film, nylon film, and the like can be suitably used.
[0095] The ink application section 120 applies ink to the surface of the recording medium M to which the primer has been applied. As the ink applying section 120, for example, a known inkjet head can be used. The ink application unit 120 may be an inkjet head that ejects ink of any color, and for example, inkjet heads that eject ink of the colors Y (yellow), M (magenta), C (cyan), K (black), and W (white) may be provided as necessary. The primer may be ejected from a part of the head that ejects the ink. In this case, the primer application unit 110 may be omitted.
[0096] The post-treatment liquid application unit 130 may be any device capable of applying the post-treatment liquid to the ink-applied area of the ink-applied surface of the recording medium M, and may be, for example, a spray or a roller other than an inkjet head. The post-treatment liquid application unit 130 may be omitted.
[0097] The method for applying the post-treatment liquid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include an inkjet method, a roller coating method, a blade coating method, a gravure coating method, a gravure offset coating method, a bar coating method, a roll coating method, a knife coating method, an air knife coating method, a comma coating method, a U comma coating method, an AKKU coating method, a smoothing coating method, a microgravure coating method, a reverse roll coating method, a four- to five-roll coating method, a dip coating method, a curtain coating method, a slide coating method, and a die coating method.
[0098] The drying section 140 dries, with hot air, the recording medium M to which the post-treatment liquid has been applied. If the recording medium M does not have a post-treatment liquid application section, the drying section 140 may be omitted. The drying section 140 may use infrared rays, microwaves, a roll heater, or the like instead of hot air to heat and dry the recording medium M to which the post-treatment liquid has been applied, or the drying section 140 may not be operated and the recording medium M to which the post-treatment liquid has been applied may be naturally dried.
[0099] The conveying unit 150 conveys the recording medium M. The conveying unit 150 is not particularly limited as long as it is capable of conveying the recording medium M, and can be appropriately selected depending on the purpose. For example, the conveying unit 150 may be a conveying belt, a platen, or the like.
[0100] The printing apparatus 100 may further include a fixing unit that heats and fixes the image formed on the recording medium M. The fixing unit is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a fixing roller.
[0101] When a desktop printer is used as the printing device, one embodiment of the primer application unit and post-treatment liquid application unit is to add a liquid storage unit having a primer or a post-treatment liquid and a liquid ejection head, and eject the primer or the post-treatment liquid by an inkjet method, as in the case of inks such as black (K), cyan (C), magenta (M), yellow (Y), and white (W).
[0102] In the present invention, the terms image formation, recording, printing, printing, etc. are all synonymous. Recording medium, media, and printed material are all synonymous. EXAMPLES
[0103] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0104] (Synthesis Example 1) <Synthesis of Resin A> In a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen blowing tube, 35 parts by mass of neopentyl glycol, 26 parts by mass of 1,6-hexanediol, 80 parts by mass of phthalic acid, 3 parts by mass of N-methyldiethanolamine, 215 parts by mass of hexamethylene diisocyanate, 31 parts by mass of isophorone diisocyanate, and 260 parts by mass of methyl ethyl ketone were added and reacted at 75°C for 4 hours to obtain a methyl ethyl ketone solution of a urethane prepolymer. Next, the obtained methyl ethyl ketone solution of a urethane prepolymer was cooled to 45°C and 34.9 parts by mass of dimethyl sulfate was added to quaternize it. Next, while gradually adding 1,760 parts by mass of water, it was emulsified and dispersed using a homogenizer, and the obtained emulsion dispersion was decompressed at 50°C to remove the solvent, and an aqueous dispersion of resin A with a non-volatile content of 25% was obtained.
[0105] (Synthesis Example 2) <Synthesis of Resin B> 126 parts by mass of 1,6-hexanediol, 33 parts by mass of N-methyldiethanolamine, 231 parts by mass of hexamethylene diisocyanate, and 260 parts by mass of methyl ethyl ketone were added to a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube, and the mixture was allowed to react at 75°C for 4 hours to obtain a methyl ethyl ketone solution of a urethane prepolymer. The solution was then cooled to 45° C. and 34.9 parts by mass of dimethyl sulfate was added to quaternize it. Next, 1760 parts by mass of water was gradually added while emulsifying and dispersing using a homogenizer, and the emulsified dispersion was subjected to reduced pressure at 50° C. to remove the solvent, thereby obtaining an aqueous dispersion of Resin B with a non-volatile content of 25%.
[0106] (Synthesis Example 3) <Synthesis of Resin C> A four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube was charged with 40 parts by mass of neopentyl glycol, 40 parts by mass of 1,6-hexanediol, 46 parts by mass of phthalic acid, 33 parts by mass of N-methyldiethanolamine, 200 parts by mass of hexamethylene diisocyanate, 31 parts by mass of isophorone diisocyanate, and 260 parts by mass of methyl ethyl ketone, and the mixture was allowed to react at 75° C. for 15 hours, thereby obtaining a methyl ethyl ketone solution of a urethane prepolymer. Next, the solution was cooled to 45°C and 34.9 parts by mass of dimethyl sulfate was added to quaternize it. Next, 1,760 parts by mass of water was gradually added while emulsifying and dispersing it using a homogenizer, and the emulsified dispersion was decompressed at 50°C to remove the solvent, obtaining an aqueous dispersion of resin C with a non-volatile content of 25%.
[0107] (Examples 1 to 20 and Comparative Examples 1 to 9) <Preparation of primer> The components and contents shown in Tables 1-1 to 1-3 and Tables 2-1 to 2-2 were mixed and stirred, and the resulting mixture was filtered through a filter with an average pore size of 10 μm (Minisart, manufactured by Sartorius) to prepare primers 1 to 29 of Examples 1 to 20 and Comparative Examples 1 to 9. The contents of each component of the primers in Tables 1-1 to 1-3 and Tables 2-1 to 2-2 are all in mass%, and the contents of resins (Hydran CP-7050, Superflex 126, Superflex 620, Mowinyl 6940, and Resins A to C) are calculated as solid contents.
[0108] Next, the surface free energy, breaking energy, and breaking elongation of each of the obtained primers were measured as follows. The results are shown in Tables 1-1 to 2-2.
[0109] <Measurement of surface free energy> Using each of the obtained primers and polyvinyl chloride (GIY-11Z5, manufactured by Lintec Corporation) as a recording medium, the contact angle was measured at 25°C using a FAMAS automatic contact angle meter (DMo-501, manufactured by Kyowa Interface Science Co., Ltd.), and a Zisman plot was created to calculate the surface tension γc (critical surface tension) when cosθ=1 (θ=0), that is, the surface free energy (mJ / m 2 ) was sought.
[0110] <Measurement of breaking energy and breaking elongation> 6 g of each of the obtained primers was placed in a Teflon (registered trademark) petri dish having a diameter of 50 mm, and dried in a hot air circulating thermostatic chamber at 40°C for one day, and then in a hot air circulating thermostatic chamber at 70°C for three days. The resulting dried film was cut with a cutter into samples having a size of 5 mm x 50 mm. A tensile test was performed under the following conditions to measure the breaking energy and breaking elongation. -conditions- Equipment: Shimadzu Autograph AG-10N Load cell: 5kN Pull speed: 150mm / min Chuck distance: 4mm Sample width: 5mm
[0111] [Table 1-1]
[0112] [Table 1-2]
[0113] [Table 1-3]
[0114] Details of each component in Tables 1-1 to 1-3 are as follows. SAG503A (siloxane surfactant, HLB value = 11, manufactured by Nissin Chemical Industry Co., Ltd.) Proxel LV (preservative, manufactured by Avecia) Hydran CP-7050 (cationic urethane resin particles, non-volatile content 30%, manufactured by DIC Corporation)
[0115] [Table 2-1]
[0116] [Table 2-2]
[0117] Details of each component in Tables 2-1 and 2-2 are as follows. Hydran CP-7050 (cationic urethane resin particles, non-volatile content 30%, manufactured by DIC Corporation) Superflex 126 (anionic urethane resin particles, non-volatile content 30%, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) Superflex 620 (cationic urethane resin particles, non-volatile content 30%, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) Movinyl 6940 (cationic acrylic resin particles, non-volatile content 30%, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) Superflex 650 (cationic urethane resin particles, non-volatile content 26%, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.)
[0118] (Pigment Dispersion Preparation Example 1) <Preparation of Black Pigment Dispersion> 100 g of SRF-LS (carbon black, manufactured by Tokai Carbon Co., Ltd.) was added to 3,000 mL of 2.5N (normal) sodium hypochlorite solution, and the mixture was stirred at 60°C and 300 rpm for 10 hours to carry out oxidation treatment, obtaining a reaction liquid containing carbon black with carboxylic acid groups added to its surface. This reaction liquid was filtered, and the separated carbon black was neutralized with sodium hydroxide solution and ultrafiltered to obtain a pigment dispersion. Next, the obtained pigment dispersion was subjected to ultrafiltration using a dialysis membrane with ion-exchanged water, and further subjected to ultrasonic dispersion to obtain a black pigment dispersion having a volume average particle size of 100 nm and having a pigment solid content concentrated to 20 mass %.
[0119] (Ink Production Example 1) <Preparation of black ink> The components and contents shown in Table 3 were mixed and stirred, and the resulting mixture was filtered through a polypropylene filter with an average pore size of 0.2 μm to prepare black ink 1. Note that the contents of each component of the black ink in Table 3 are all in mass %, and the content of the resin (Boncoat CP-6450) is calculated as the solid content.
[0120] [Table 3]
[0121] Details of each component in Table 3 are as follows: Boncoat CP-6450 (acrylic resin emulsion, manufactured by DIC Corporation, solid content 40%) FS-300 (fluorosurfactant, manufactured by DuPont)
[0122] (Examples 21 to 40 and Comparative Examples 10 to 18) <Image formation> The prepared primers 1 to 29 and black ink 1 of Examples 1 to 20 and Comparative Examples 1 to 9 were filled into an inkjet printer (device name: modified IPSiO GXe5500, manufactured by Ricoh Co., Ltd.) based on the combinations shown in Tables 4-1 to 4-5. Next, a primer was applied to each recording medium shown in Tables 4-1 to 4-5 in an amount of 4.2 g / m 2 A solid image of primer was printed so that Next, within 10 minutes after printing the solid image of the primer, a solid image of Black Ink 1 was printed on top of the solid image of the primer, and the solid image of Black Ink 1 was dried at 80° C. for 3 minutes.
[0123] [Recording Media] Polyvinyl chloride (GIY-11Z5, manufactured by Lintec Corporation, hereafter referred to as "PVC sheet") Polyvinyl chloride foam plastic (KAPA (registered trademark) PLAST, manufactured by 3A Composites, hereinafter referred to as "foam plastic sheet") Polycarbonate (PC-2151, manufactured by Teijin Limited, hereinafter referred to as "polycarbonate film") Styrene (WB Tack, manufactured by Sekisui Plastics Co., Ltd., hereafter referred to as "styrene board") Polypropylene (Torayfan (registered trademark), manufactured by Toray Industries, Inc., hereinafter referred to as "polypropylene sheet") Acrylic (Acrylite TMS, manufactured by Mitsubishi Chemical Corporation, hereafter referred to as "acrylic board") Polyethylene terephthalate (Toyobo Ester (registered trademark) Film E3120, manufactured by Toyobo Co., Ltd., hereinafter referred to as "PET sheet") Polyethylene core aluminum composite plate (ALPOLIC (registered trademark), manufactured by Mitsubishi Chemical Infratec Corporation; hereinafter referred to as "aluminum composite plate") Polyester (Lumirror (registered trademark), manufactured by Toray Industries, Inc., hereinafter referred to as "polyester sheet")
[0124] Next, the fixability (beading resistance), glossiness, and adhesion of each of the obtained images were evaluated as follows. The results are shown in Tables 4-1 to 4-5.
[0125] <Fixation (beading resistance)> The presence or absence of beading (uneven recording) of the solid image of the primer alone formed on the "PVC sheet" and the ink image on the primer was visually observed, and the fixing property (beading resistance) was evaluated based on the following evaluation criteria. The evaluation of B or higher is preferable for practical use. [Evaluation Criteria] A: Very good (no beading at all) B: Good (slight beading observed) C: Normal (beading occurred)
[0126] <Adhesion> A cross-cut peel test was performed using a cloth adhesive tape (123LW-50, manufactured by Nichiban Co., Ltd.) on solid images formed on each of the recording media, namely "PVC sheet", "foamed plastic", "polycarbonate film", "styrene board", "polypropylene sheet", "acrylic board", "PET sheet", "aluminum sheet", and "polyester sheet". The number of remaining squares out of 100 test squares was counted, and the "adhesion" to the recording medium was evaluated based on the following evaluation criteria. A rating of B or higher is preferable for practical use. [Evaluation Criteria] A: 90 or more remaining squares B: 70 to less than 90 remaining squares C: Less than 70 remaining squares
[0127] <Glossiness> The 60° gloss of the solid image formed on the "PVC sheet" was measured four times using a gloss meter (BYK Gardener, 4501), the average 60° gloss was calculated, and the "glossiness" was evaluated based on the following evaluation criteria. The evaluation of B or higher is preferable for practical use. [Evaluation Criteria] A: Average 60° gloss level is 90 or more B: Average 60° gloss level is 80 or more and less than 90 C: Average 60° gloss level is less than 80
[0128] [Table 4-1]
[0129] [Table 4-2]
[0130] [Table 4-3]
[0131] [Table 4-4]
[0132] [Table 4-5]
[0133] It can be seen that Examples 21 to 28, which used Primers 1 to 8 of Examples 1 to 8, are preferred embodiments of the present invention, and provide images with excellent fixability, high gloss, and high adhesion. Example 29, which used Primer 9 of Example 9, had a diethylene glycol alkyl ether content of less than 5 mass %, and resulted in inferior adhesion compared to Examples 21-28. Example 30, which used the primer 10 of Example 10, is an example in which the content of diethylene glycol alkyl ether was more than 30 mass %, and the result was inferior to Examples 21-28 in adhesion. Example 31, which used primer 11 of Example 11, is an example in which diethylene glycol dimethyl ether was used as the diethylene glycol alkyl ether compound, and the result was inferior in gloss to Examples 21-28. Example 32, which used the primer 12 of Example 12, had a diethylene glycol diethyl ether content of less than 15 mass %, and was inferior in gloss and adhesion to Examples 21-28. Example 33, in which primer 13 of Example 13 was used, is an example in which magnesium nitrate was used as the polyvalent metal salt, and the results were inferior to Examples 21-28 in gloss and adhesion. Example 34, which used the primer 14 of Example 14, had a cationic resin content of less than 2 mass %, and resulted in inferior adhesion compared to Examples 21-28. Example 35, which used the primer 15 of Example 15, is an example in which the content of the cationic resin was more than 15 mass %, and the result was inferior to Examples 21-28 in gloss. Example 36, which used the primer 16 of Example 16, had a magnesium acetate content of less than 0.25 mass %, and resulted in inferior adhesion compared to Examples 21-28. Example 37, which used the primer 17 of Example 17, is an example in which the magnesium acetate content was more than 10 mass %, and the gloss was inferior to Examples 21-28. In Example 38, which used the primer 18 of Example 18, the surfactant content was less than 5 mass % relative to the cationic resin, and the adhesion was inferior to Examples 21-28. Example 39, which used the primer 19 of Example 19, had a surfactant content of more than 20% by mass relative to the cationic resin, and resulted in inferior fixing property compared to Examples 21-28. In Example 40, the primer 20 of Example 20 was used, and the surface free energy of the primer was 45 mJ / m 2 The results showed that the adhesion was inferior to those of Examples 21 to 28.
[0134] Comparative Example 10, which used primer 21 of Comparative Example 1, is an example that does not contain a diethylene glycol alkyl ether compound, but contains triethylene glycol monobutyl ether instead of the diethylene glycol alkyl ether compound, and the fixing property was inferior to that of the Examples. Comparative Example 11, which used primer 22 of Comparative Example 2, is an example in which the diethylene glycol alkyl ether compound was not contained and ethyl acetate was used instead of the diethylene glycol alkyl ether compound, and the fixing property was inferior to that of the Examples. Comparative Example 12, which used primer 23 of Comparative Example 3, is an example that did not contain a diethylene glycol alkyl ether compound and used γ-butyrolactone instead of the diethylene glycol alkyl ether compound, and the results showed inferior fixation and adhesion compared to the examples. Comparative Example 13, which used Primer 24 from Comparative Example 4, is an example that does not contain a cationic resin and uses Superflex 126, an anionic resin, instead of a cationic resin, and the results showed inferior fixation, gloss, and adhesion compared to the Examples. Comparative Example 14, which used primer 25 of Comparative Example 5, is an example that does not contain a polyvalent metal salt and uses sodium acetate, a monovalent metal salt, instead of the polyvalent metal salt, and the results showed inferior fixation, gloss, and adhesion compared to the Examples. Comparative Example 15, which used the primer 26 of Comparative Example 6, had a breaking elongation of less than 500% because it used Superflex 620 as the cationic resin, resulting in poorer fixability and adhesion than the Examples. Comparative Example 16, which used the primer 27 of Comparative Example 7, is an example in which a resin having a breaking elongation of more than 2,500% was used, and the results showed inferior fixability and adhesion compared to the Examples. Comparative Example 17, which used the primer 28 of Comparative Example 8, is an example in which a resin with a breaking energy of less than 20 mJ was used, and the results showed inferior fixability and adhesion compared to the Examples. Comparative Example 18, which used the primer 29 of Comparative Example 9, is an example in which a resin having a breaking energy of more than 1,000 mJ was used, and the results showed inferior fixability and adhesion compared to the Examples.
[0135] For example, aspects of the present invention are as follows. <1> A primer comprising water, a cationic resin, a polyvalent metal salt, and a diethylene glycol alkyl ether compound, The primer is characterized in that 6 g of the primer is placed in a Teflon (registered trademark) petri dish having a diameter of 50 mm, and dried in a hot air circulating thermostatic chamber at 40°C for one day and then in a hot air circulating thermostatic chamber at 70°C for three days to obtain a dried and solid film, which has a breaking energy of 20 mJ or more and 1,000 mJ or less and a breaking elongation of 500% or more and 2,500% or less, measured as described below. <Measurement of breaking energy and breaking elongation> The dried film is cut into a sample having a size of 5 mm×50 mm using a cutter, and a tensile test is carried out under the following conditions to measure the breaking energy and breaking elongation. -conditions- Equipment: Shimadzu Autograph AG-10N Load cell: 5kN Pull speed: 150mm / min Chuck distance: 4mm Sample width: 5mm <2> The content of the diethylene glycol alkyl ether compound is 5% by mass or more and 30% by mass or less. <1> It is a primer described in <3> The diethylene glycol alkyl ether compound is diethylene glycol diethyl ether. <1> It is a primer described in <4> The polyvalent metal salt comprises magnesium acetate. <1> It is a primer described in <5> The content of the polyvalent metal salt is 0.25% by mass or more and 10% by mass or less. <1> It is a primer described in <6> The cationic resin is a cationic urethane resin. <1> It is a primer described in <7> The content of the cationic resin is 2% by mass or more and 15% by mass or less. <1> It is a primer described in <8> Further comprising a surfactant, The mass ratio of the surfactant to the cationic resin (surfactant:cationic resin) is 1:4 to 1:20. <1> It is a primer described in <9> Surface free energy γ at 25°C is 45mJ / m 2 The above-mentioned <1> It is a primer described in <10> The above <1> from <9> A primer according to any one of the above. an ink containing a coloring material and an organic solvent; The printing set is characterized by having the following features. <11> On a recording medium, <1> from <9> A primer application step of applying a primer according to any one of the above. an ink application step of applying an ink containing a coloring material and an organic solvent onto the recording medium to which the primer has been applied; A printing method comprising the steps of: <12> The recording medium is a non-permeable recording medium. <11> 2 is a printing method according to the present invention. <13> On a recording medium, <1> from <9> A primer applying means for applying the primer according to any one of the above items; an ink applying means for applying an ink containing a coloring material and an organic solvent onto the recording medium to which the primer has been applied; The printing device is characterized by having: <14> The recording medium is a non-permeable recording medium. <13> The printing apparatus according to the present invention is
[0136] The above <1> from <9> The primer according to any one of <10> The printing set according to <11> from <12> The printing method according to any one of the preceding claims, <13> from <14> According to the printing apparatus described in any one of the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0137] 100 Printing device 110 Primer application section 120 Ink application section 130 Post-processing liquid application section 140 Drying section 150 Conveyor M Recording medium [Prior art documents] [Patent documents]
[0138] [Patent Document 1] Patent Publication No. 2021-000790 [Patent Document 2] JP 2021-120219 A
Claims
1. A primer comprising water, a cationic resin, a polyvalent metal salt, and a diethylene glycol alkyl ether compound, A primer characterized in that 6 g of the primer is placed in a Teflon (registered trademark) petri dish having a diameter of 50 mm, and dried in a hot air circulating thermostatic chamber at 40°C for one day and then in a hot air circulating thermostatic chamber at 70°C for three days, to obtain a dried and solid film, which has a breaking energy of 20 mJ or more and 1,000 mJ or less and a breaking elongation of 500% or more and 2,500% or less, measured as described below. <Measurement of Breaking Energy and Breaking Elongation> The dried film is cut into a sample having a size of 5 mm×50 mm using a cutter, and a tensile test is carried out under the following conditions to measure the breaking energy and breaking elongation. -conditions- Equipment: Shimadzu Autograph AG-10N Load cell: 5kN Pull speed: 150 mm / min ・Chuck distance: 4mm ・Sample width: 5 mm
2. The primer according to claim 1 , wherein the content of the diethylene glycol alkyl ether compound is 5% by mass or more and 30% by mass or less.
3. The primer of claim 1 , wherein the diethylene glycol alkyl ether compound is diethylene glycol diethyl ether.
4. The primer of claim 1 , wherein the polyvalent metal salt comprises magnesium acetate.
5. The primer according to claim 1 , wherein the content of the polyvalent metal salt is 0.25% by mass or more and 10% by mass or less.
6. The primer according to claim 1 , wherein the cationic resin is a cationic urethane resin.
7. The primer according to claim 1 , wherein the content of the cationic resin is from 2% by mass to 15% by mass.
8. Further comprising a surfactant, 2. The primer according to claim 1, wherein a mass ratio of the surfactant to the cationic resin (surfactant:cationic resin) is from 1:4 to 1:
20.
9. Surface free energy γ at 25°C is 45 mJ / m 2 2. The primer of claim 1, wherein:
10. A primer according to any one of claims 1 to 9; an ink containing a coloring material and an organic solvent; A printing set comprising:
11. a primer applying step of applying the primer according to any one of claims 1 to 9 onto a recording medium; an ink application step of applying an ink containing a coloring material and an organic solvent onto the recording medium to which the primer has been applied; A printing method comprising:
12. The printing method of claim 11 , wherein the recording medium is a non-permeable recording medium.
13. A primer applying means for applying the primer according to any one of claims 1 to 9 onto a recording medium; an ink applying means for applying an ink containing a coloring material and an organic solvent onto the recording medium to which the primer has been applied; A printing device comprising:
14. The printing apparatus of claim 13 , wherein the recording medium is a non-permeable recording medium.
Citation Information
Patent Citations
Surface treatment liquid composition, printing method and printing apparatus
JP2021000790A
Reaction liquid, inkjet recording method, and set of ink and reaction liquid
JP2021120219A