Adhesive composition and application of the same

A plant-derived adhesive composition with a specific acrylic resin and additives enhances olefin adhesive strength and removability, addressing the limitations of fossil-based adhesives by maintaining performance under moist heat conditions.

JP2024132943APending Publication Date: 2024-10-01MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024034998
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2024-03-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing adhesives, particularly acrylic adhesives, rely on fossil resources and face issues with insufficient olefin adhesive strength and removability, especially under moist heat conditions, leading to contamination of adherends.

Method used

An adhesive composition using an acrylic resin with a specific monomer structure derived from plant materials, combined with a crosslinking agent and a tackifier, to enhance olefin adhesive strength and removability, even under high temperature and humidity.

Benefits of technology

The adhesive composition achieves excellent adhesive strength to low polarity materials and maintains removability, reducing contamination even after prolonged exposure to moist heat, making it suitable for applications like double-sided tapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132943000001
    Figure 2024132943000001
  • Figure 2024132943000002
    Figure 2024132943000002
  • Figure 2024132943000003
    Figure 2024132943000003
Patent Text Reader

Abstract

To provide an adhesive composition which is excellent in olefin adhesive force, prevents contamination in peeling even after having been stuck to various adherends including an adherend containing a low polar material such as olefin, and then been exposed to a high temperature or moisture and hot environment for a long time, and is excellent in re-peelability.SOLUTION: An adhesive composition contains an acrylic resin (A), a crosslinking agent (B) and a tackifier (C), wherein the acrylic resin (A) contains a structural unit derived from an alkyl (meth)acrylate-based monomer (a1) having a linear alkyl group having 8 to 10 carbon atoms as a main structural unit, and a structural unit derived from a functional group-containing monomer (a2) having a crosslinkable functional group, and has an acid value of 15 mgKOH / g or more, and the tackifier (C) contains 50 wt.% or more of a tackifier (C1) having a softening point of 130°C or lower based on the total tackifier (C).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive composition and its use, more specifically, to a pressure-sensitive adhesive composition that can be used in the pressure-sensitive adhesive layer of a pressure-sensitive adhesive film, a pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition, and a pressure-sensitive adhesive film having a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive, such as a pressure-sensitive adhesive film for double-sided tape. The pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition of the present invention has excellent olefin adhesion even when using raw materials derived from plants that suppress dependence on fossil resource materials, and is unlikely to cause contamination when peeled off from an adherend after use under moist and hot conditions, and can be used, for example, as a pressure-sensitive adhesive film for double-sided tape. Note that "olefin adhesion" refers to adhesion to an adherend containing a low-polarity material such as an olefin. [Background technology]

[0002] Conventionally, natural rubber-based adhesives and acrylic-based adhesives have been known as adhesives used in adhesive layers of adhesive tapes, adhesive sheets, etc. As acrylic-based adhesives, (co)polymers having specific alkyl (meth)acrylates as essential constituent units have been developed. However, acrylic adhesives often use petroleum as a raw material, and carbon dioxide is emitted during disposal after use. This raises concerns about the depletion of petroleum resources and their impact on global warming, and the use of plant-derived raw materials, which are renewable materials, is therefore recommended.

[0003] In this regard, Patent Document 1 discloses a pressure-sensitive adhesive that contains 48% by weight or more of an acrylic monomer having a biological carbon with 7 to 14 carbon atoms in the hydrocarbon chain portion and has a glass transition temperature of -20° C. or lower. However, the technology of Patent Document 1 has a problem in that it is not possible to exert sufficient olefin adhesive strength.

[0004] In addition, the invention of Patent Document 2 aims to provide an adhesive composition partially derived from a plant material, and the document discloses a pressure-sensitive adhesive containing a 2-octyl (meth)acrylate / (meth)acrylic acid copolymer. However, the technology of Patent Document 2 has a problem in that removability deteriorates after long-term humidity loading. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-218458 A [Patent Document 2] Special Publication No. 2010-506979 Summary of the Invention [Problem to be solved by the invention]

[0006] The problem to be solved by the present invention is to provide a pressure-sensitive adhesive composition that can use raw materials derived from plants to reduce dependency on fossil resource materials, and that has excellent olefin adhesion and excellent removability, i.e., is unlikely to cause contamination when removed even after being exposed to a high temperature or humid heat environment for a long period of time after being applied to various adherends including adherends containing low polarity materials such as olefins. The present invention also provides a pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition, a pressure-sensitive adhesive layer using the pressure-sensitive adhesive, and a film having the pressure-sensitive adhesive layer. [Means for solving the problem]

[0007] The present inventors have found that the above-mentioned problems can be solved by using, as a monomer component of the acrylic polymer forming the adhesive layer, an acrylic resin (A) having a specific acid value and a structural unit derived from a (meth)acrylic acid alkyl ester monomer (a1) having a long-chain, linear alkyl group, and further using a certain proportion of a tackifier (C1) having a specific softening point, and have thus completed the present invention.

[0008] That is, the present invention includes the following aspects. Aspect (1) of the present invention is a pressure-sensitive adhesive composition comprising an acrylic resin (A), a crosslinking agent (B) and a tackifier (C), the acrylic resin (A) contains, as a main structural unit, a structural unit derived from a (meth)acrylic acid alkyl ester monomer (a1) having a linear alkyl group having 8 to 10 carbon atoms, contains a structural unit derived from a functional group-containing monomer (a2) having a crosslinkable functional group, and has an acid value of 15 mgKOH / g or more; The tackifier (C) is a pressure-sensitive adhesive composition containing 50% by weight or more of a tackifier (C1) having a softening point of 130° C. or less, based on the total weight of the tackifier (C).

[0009] In an embodiment (2) of the present invention, in the pressure-sensitive adhesive composition of the embodiment (1), the proportion of plant-derived carbon in the entire pressure-sensitive adhesive composition is 50% or more.

[0010] In an embodiment (3) of the present invention, in the pressure-sensitive adhesive composition of the embodiment (1) or (2), the functional group-containing monomer (a2) is a hydroxyl group-containing monomer and / or a carboxy group-containing monomer.

[0011] A fourth aspect of the present invention is a pressure-sensitive adhesive composition according to any one of the first to third aspects, wherein the acid value is 20 mgKOH / g or more.

[0012] Aspect (5) of the present invention is the pressure-sensitive adhesive composition according to any one of aspects (1) to (4), wherein the crosslinking agent (B) contains at least two types of crosslinking agents selected from the group consisting of isocyanate-based crosslinking agents, epoxy-based crosslinking agents, metal chelate-based crosslinking agents, and aziridine-based crosslinking agents.

[0013] A sixth aspect of the present invention relates to the pressure-sensitive adhesive composition according to any one of the first to fifth aspects, wherein the tackifier (C) contains a rosin-based resin (C1-1) having a softening point of 130° C. or lower.

[0014] A seventh aspect of the present invention is a pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to any one of the first to sixth aspects.

[0015] An embodiment (8) of the present invention is the pressure-sensitive adhesive of the embodiment (7), wherein the pressure-sensitive adhesive has a gel fraction of 50 to 90%.

[0016] A ninth aspect of the present invention is a pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive according to the seventh or eighth aspect.

[0017] A tenth aspect of the present invention is a pressure-sensitive adhesive film having the pressure-sensitive adhesive layer of the nineth aspect on a film.

[0018] In the present invention, the term "adhesive film" conceptually includes an adhesive sheet, an adhesive film, and an adhesive tape.

[0019] The adhesive composition of the present invention is excellent in adhesion and removability. The reason why the adhesive composition of the present invention exhibits these effects is not clear, but the following reasons are presumed. By using a (meth)acrylic acid alkyl ester monomer (a1) having a linear alkyl group with a larger carbon number than butyl acrylate and 2-ethylhexyl acrylate, which are alkyl acid ester monomers used in general adhesives, the glass transition temperature (Tg) can be relatively high while maintaining the polarity of the entire polymer low, and by using a certain proportion of a tackifier (C1) having a specific softening point, the balance between the wettability and viscoelasticity of the polymer can be adjusted, and the interfacial interaction between a low-polarity adherend and the adhesive layer can be adjusted. It is considered that this makes it possible to achieve two features at the same time: increasing the olefin adhesion while suppressing the contamination of the adherend after long-term exposure to a high-temperature and high-humidity environment. Effect of the Invention

[0020] The adhesive obtained by crosslinking the adhesive composition of the present invention can reduce the dependency on fossil resource-based materials, has excellent adhesion to low-polarity adherends such as olefin adherends, and has excellent stain resistance when peeled off even after long-term exposure to a humid and hot environment. Therefore, an adhesive film having excellent adhesion to olefins and excellent removability from various adherends including olefin adherends can be obtained. The adhesive film of the present invention is particularly useful as a double-sided adhesive film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the embodiments of the present invention will be described in detail, however, these are merely examples of preferable embodiments and the present invention is not limited to these embodiments. In the present invention, "(meth)acrylic" means acrylic or methacrylic, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate, respectively. In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more, Y or less", as well as "preferably larger than X" or "preferably smaller than Y". Furthermore, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the meaning that "it is preferably greater than X" or "it is preferably less than Y". Furthermore, "y and / or z (y and z are optional configurations)" means at least one of y and z, and means the following three cases: y only, z only, and y and z. In the present specification, in which multiple numerical ranges are described in stages, each upper limit and each lower limit can be the upper limit or lower limit of any combination of numerical ranges. For example, when the content of a certain component is described as "5-20 mass%, 10-15 mass%, "it can be each of the numerical ranges of "5-15 mass%, " "10-20 mass%, " "5-10 mass%, " and "15-20 mass%. Furthermore, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical ranges can be replaced with values ​​shown in the examples or values ​​that are uniquely derived from the examples.

[0022] [Adhesive composition] The pressure-sensitive adhesive composition of the present invention contains at least an acrylic resin (A), a crosslinking agent (B) and a tackifier (C). First, the acrylic resin (A) will be described.

[0023] <Acrylic resin (A)> The acrylic resin (A) used in the present invention is a polymer of a copolymerization component (a), and the copolymerization component (a) contains at least a (meth)acrylic acid alkyl ester monomer (a1) having a linear alkyl group having 8 to 10 carbon atoms, and a functional group-containing monomer (a2) having a functional group.

[0024] [(Meth)acrylic acid alkyl ester monomer (a1)] Examples of the (meth)acrylic acid alkyl ester monomer (a1) having a linear alkyl group having 8 to 10 carbon atoms include n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, etc. One selected from these may be used alone, or two or more may be used in combination. Among these monomers (a1), it is preferable to use a plant-derived monomer from the viewpoint of carbon circulation. Examples of the plant-derived monomer include n-octyl(meth)acrylate and n-decyl(meth)acrylate.

[0025] The (meth)acrylic acid alkyl ester monomer (a1) is the main component of the copolymerization component (a). Here, the term "main component" refers to the monomer with the largest content among the two or more monomers contained in the copolymerization component (a). Furthermore, as a preferred content ratio, the content of the (meth)acrylic acid alkyl ester monomer (a1) is preferably 60% by weight or more, more preferably 65% ​​by weight or more, and particularly preferably 70% by weight or more, when the total amount of the copolymerization component (a) is taken as 100% by weight. In addition to the above, when a monomer derived from a plant is used, it is preferably 80% by weight or more, more preferably 90% by weight or more, and particularly preferably 95 parts by weight or more, from the viewpoint of carbon circulation. The upper limit is usually 99.9% by weight. If the content is too small, the effects of the present invention tend not to be obtained.

[0026] [Functional group-containing monomer (a2)] The functional group in the functional group-containing monomer (a2) is a crosslinkable functional group capable of forming a crosslinked structure with the crosslinking agent (B). Examples of such functional groups include a hydroxyl group, a carboxyl group, an epoxy group, an oxetane group, a glycidyl group, a sulfone group, an acetoacetyl group, and an acid anhydride group.

[0027] The functional group-containing monomer (a2) is preferably a hydroxyl group-containing monomer (a2-1) and / or a carboxy group-containing monomer (a2-2). Examples of the hydroxyl group-containing monomer (a2-1) include hydroxyalkyl (meth)acrylate monomers such as hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; oxyalkylene-modified mono(meth)acrylate monomers such as diethylene glycol mono(meth)acrylate and polyethylene glycol mono(meth)acrylate; and other primary hydroxyl group-containing (meth)acrylate monomers (e.g., 2-acryloyloxyethyl-2-hydroxyethylphthalic acid, N-methylol (meth)acrylamide, and hydroxyethylacrylamide). Among these, hydroxyethyl acrylate is particularly preferred. Examples of the carboxyl group-containing monomer (a2-2) include monomers having an acidic functional group such as a carboxyl group or an acid anhydride group, and specific examples thereof include (meth)acrylic acid, (meth)acrylic anhydride, maleic anhydride, itaconic anhydride, etc. Among these, acrylic acid is particularly preferred. One selected from these may be used alone, but it is preferable to use two or more of them in combination, as this tends to improve the cohesive strength of the pressure-sensitive adhesive.

[0028] The content of the functional group-containing monomer (a2) is preferably 0.1% by weight or more, more preferably 1% by weight or more, and particularly preferably 5% by weight or more, based on the total amount of the copolymerization component (a) being 100% by weight. The upper limit of the content of the functional group-containing monomer (a2) is preferably 40% by weight, more preferably 30% by weight, and particularly preferably 20% by weight. If the content is too low, the stain resistance tends to decrease, and if the content is too high, the adhesive strength tends to decrease.

[0029] [Other copolymerizable monomers (a3)] The copolymerization component (a) in the present invention may contain other copolymerizable monomers (a3) ​​within the scope of not impairing the effects of the present invention. Examples of the other copolymerizable monomers include (a3-1) (meth)acrylic acid alkyl ester monomers having a linear or branched alkyl group with 7 or less carbon atoms, (a3-2) (meth)acrylic acid alkyl ester monomers having a branched alkyl group with 8 to 12 carbon atoms, (meth)acrylic acid alkyl ester monomers having a linear or branched alkyl group with 13 or more carbon atoms, alicyclic structure-containing monomers, aromatic monomers, alkoxy group-containing monomers, amino group-containing monomers, and amide group-containing monomers.

[0030] Examples of the (meth)acrylic acid alkyl ester monomer (a3-1) having a linear or branched alkyl group having 7 or less carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl acrylate, etc. One selected from these may be used alone, or two or more may be used in combination. The content of the (meth)acrylic acid alkyl ester monomer (a3-1) having a linear or branched alkyl group having 7 or less carbon atoms is preferably 50% by weight or less, more preferably 40% by weight or less, and particularly preferably 30% by weight or less, when the total amount of the copolymerization component (a) is 100% by weight.

[0031] Examples of the (meth)acrylic acid alkyl ester monomer (a3-2) having a branched alkyl group having 8 to 12 carbon atoms include 2-ethylhexyl acrylate. The content of the (meth)acrylic acid alkyl ester monomer (a3-2) having a branched alkyl group having 8 to 12 carbon atoms is preferably 50% by weight or less, more preferably 40% by weight or less, and particularly preferably 30% by weight or less, when the total amount of the copolymerization component (a) is 100% by weight.

[0032] Examples of the (meth)acrylic acid alkyl ester monomer having a linear or branched alkyl group having 13 or more carbon atoms include tridecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, etc. One selected from these may be used alone, or two or more may be used in combination.

[0033] Examples of the alicyclic structure-containing monomer include (meth)acrylates having an alicyclic structure, such as cyclohexyl (meth)acrylate, isobornyl acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, 2-adamantyl (meth)acrylate, etc. One selected from these may be used alone, or two or more may be used in combination.

[0034] Examples of the aromatic monomer include (meth)acrylates having one aromatic ring such as phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxydipropylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypolypropylene glycol-(meth)acrylate, and (meth)acrylates having two aromatic rings such as phenoxybenzyl (meth)acrylate and ethoxylated o-phenylphenol (meth)acrylate. One selected from these may be used alone, or two or more may be used in combination.

[0035] Examples of the alkoxy group-containing monomer include alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, etc. One selected from these may be used alone, or two or more may be used in combination.

[0036] Examples of the amino group-containing monomer include primary amino group-containing (meth)acrylate monomers such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate, secondary amino group-containing (meth)acrylate monomers such as t-butylaminoethyl (meth)acrylate, and tertiary amino group-containing (meth)acrylate monomers such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate. One selected from these may be used alone, or two or more may be used in combination.

[0037] Examples of the amide group-containing monomer include (meth)acrylamide; alkoxyalkyl (meth)acrylamide monomers such as methoxymethyl (meth)acrylamide, ethoxymethyl (meth)acrylamide, propoxymethyl (meth)acrylamide, isopropoxymethyl (meth)acrylamide, n-butoxymethyl (meth)acrylamide, and isobutoxymethyl (meth)acrylamide; dialkyl (meth)acrylamide monomers such as dimethyl (meth)acrylamide and diethyl (meth)acrylamide; etc. One selected from these may be used alone, or two or more may be used in combination.

[0038] [Production of acrylic resin (A)] The polymerization method of the acrylic resin (A) may be a conventionally known method such as solution radical polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. For example, a method of mixing or dropping an appropriately selected copolymerization component (a) and a polymerization initiator into an organic solvent and polymerizing under a predetermined polymerization condition may be mentioned. Among them, solution radical polymerization and bulk polymerization are preferred, and solution radical polymerization is more preferred because the acrylic resin (A) can be stably obtained.

[0039] Examples of organic solvents used in the polymerization reaction include aromatic hydrocarbons such as toluene and xylene, aliphatic hydrocarbons such as hexane, esters such as ethyl acetate and butyl acetate, aliphatic alcohols such as n-propyl alcohol and isopropyl alcohol, and ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc. Among these organic solvents, in terms of ease of polymerization reaction, chain transfer effect, ease of drying during adhesive coating, and safety, ethyl acetate, acetone, methyl ethyl ketone, butyl acetate, toluene, and methyl isobutyl ketone are preferred, and more preferred are ethyl acetate, acetone, and methyl ethyl ketone.

[0040] Examples of the polymerization initiator used in the solution radical polymerization include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis(methylpropionic acid), which are normal radical polymerization initiators; and organic peroxides such as benzoyl peroxide, lauroyl peroxide, di-t-butyl peroxide, and cumene hydroperoxide, which can be appropriately selected and used according to the monomer to be used. One selected from these polymerization initiators may be used alone, or two or more may be used in combination.

[0041] Thus, an acrylic resin (A) is obtained which contains, as a main structural unit, a structural unit derived from a (meth)acrylic acid alkyl ester monomer (a1) having a linear alkyl group having 8 to 10 carbon atoms, a structural unit derived from a functional group-containing monomer (a2) having a crosslinkable functional group, and which may further contain a structural unit derived from another copolymerizable monomer (a3).

[0042] [Physical properties of acrylic resin (A)] The acid value of the acrylic resin (A) is 15 mgKOH / g or more, preferably 20 mgKOH / g or more, more preferably 25 mgKOH / g or less. If the acid value is too high, the stain resistance of the adherend after high heat load tends to decrease and the adhesive strength tends to increase too much. In the present invention, the acid value is determined by neutralization titration based on JIS K0070, and the resin content is 45% by weight. The acid value in the present invention is based on the acid content of the copolymerization component (a) of the acrylic resin (A). The acid in the present invention includes, for example, acrylic acid and carboxylate ion state in which the carboxy group is neutralized with a basic compound. The upper limit of the acid value of the acrylic resin (A) is usually 100 mgKOH / g.

[0043] The weight-average molecular weight of the acrylic resin (A) is preferably 200,000 to 2.5 million, more preferably 300,000 to 1.5 million, and particularly preferably 500,000 to 1 million. If the weight-average molecular weight is too low, appropriate adhesive strength cannot be obtained, the heat resistance of the adhesive layer decreases, and there is a tendency for contamination of the adherend after high heat load to increase, whereas if the weight-average molecular weight is too high, a large amount of dilution solvent is required, which tends to be disadvantageous in terms of coatability and cost.

[0044] The dispersity (weight average molecular weight / number average molecular weight) of the acrylic resin (A) is preferably 15 or less, more preferably 10 or less, and particularly preferably 6 or less. If the dispersity is too high, the cohesive force tends to decrease and the heat resistance tends to decrease. The lower limit of the dispersity is usually 1.

[0045] The weight average molecular weight of the acrylic resin (A) is a weight average molecular weight calculated based on the molecular weight of standard polystyrene. The weight average molecular weight was measured by a high performance liquid chromatography (Waters Japan, "Waters2695 (main body)" and "Waters2414 (detector)") using a Shodex GPCKF-806L column (molecular weight exclusion limit: 2×10 7 , Separation range: 100~2×10 7 The number average molecular weight can also be measured in a similar manner. The degree of dispersion can be calculated from the weight average molecular weight and the number average molecular weight.

[0046] The glass transition temperature (Tg) of the acrylic resin (A) is preferably −100 to 25° C., more preferably −60 to 0° C., particularly preferably −55 to −20° C., and even more preferably −50 to −30° C. If the glass transition temperature is too high, the tack tends to decrease, making lamination difficult, and zipping tends to occur during rework from a release film or adherend, while if the glass transition temperature is too low, the heat resistance tends to decrease.

[0047] The glass transition temperature is calculated by the following Fox formula.

number

[0048] The viscosity of the acrylic resin (A) is adjusted with a solvent etc., and the acrylic resin (A) solution is used in the pressure-sensitive adhesive composition of the present invention. From the viewpoint of ease of handling, the viscosity of the acrylic resin (A) solution is preferably 500 to 20,000 mPa·s, more preferably 1,000 to 18,000 mPa·s, and particularly preferably 2,000 to 15,000 mPa·s. If the viscosity is too high, the fluidity decreases and handling tends to become difficult, whereas if the viscosity is too low, coating tends to become difficult when forming the adhesive. The viscosity of the acrylic resin (A) solution can be determined by measuring the resin solution, whose temperature has been adjusted to 25° C., by a rotational viscometer method using a Brookfield viscometer.

[0049] [Biomass content of acrylic resin (A)] The proportion of plant-derived carbon in the acrylic resin (A), i.e., the biomass ratio, is preferably 40% by weight or more, more preferably 50% by weight or more, and even more preferably 60% by weight or more, from the viewpoint of reducing the environmental load. The upper limit is 100% by weight. The biomass degree may be any value obtained by any one of the calculation methods shown below, as long as it falls within the above range.

[0050] (How to calculate biomass ratio) Biomass ratio (wt%) of acrylic resin (A)=[(biomass ratio of each biological raw material used in producing acrylic resin (A))×(weight of each biological raw material used in producing acrylic resin (A)] / (total weight of acrylic resin (A))×100]

[0051] The biomass degree is also called the content of carbon derived from living organisms, and can be determined by analyzing the composition ratio by NMR and calculating the carbon number of the living organism-derived monomer / total carbon number.

[0052] While carbon derived from living organisms contains a certain percentage of radioactive isotopes (C-14), carbon derived from petroleum contains almost no C-14. Therefore, the biomass content can also be calculated by measuring the concentration of C-14 contained in the adhesive. Specifically, it can be measured according to ASTM D6866, a standard used in many bioplastic industries.

[0053] <Crosslinking agent (B)> The crosslinking agent (B) used in the present invention is a compound that reacts with the functional group in the acrylic resin (A) to form a crosslinked structure, and examples of the crosslinking agent (B) include an isocyanate-based crosslinking agent (B1), an epoxy-based crosslinking agent (B2), a metal chelate-based crosslinking agent (B3) and an aziridine-based crosslinking agent (B4). By including the crosslinking agent (B), the crosslinking speed of the pressure-sensitive adhesive composition is increased, and the aging period during film production is also shortened, so that the pressure-sensitive adhesive film can be obtained economically and efficiently.

[0054] Examples of the isocyanate crosslinking agent (B1) include tolylene diisocyanate compounds such as 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate; xylylene diisocyanate compounds such as 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate and tetramethyl xylylene diisocyanate; aromatic isocyanate compounds such as 1,5-naphthalene diisocyanate and triphenylmethane triisocyanate; hexamethylene diisocyanate, isophorone diisocyanate, and adducts of these isocyanate compounds with polyol compounds such as trimethylolpropane, biuret compounds and isocyanurates of these polyisocyanate compounds, etc. One selected from these may be used alone, or two or more may be used in combination. Among these, from the viewpoints of high reactivity, improved heat resistance, and less contamination of the adherend, hexamethylene diisocyanate, isophorone diisocyanate, adducts of these isocyanate compounds with polyol compounds such as trimethylolpropane, biuret compounds or isocyanurate compounds of these polyisocyanate compounds, and rylene diisocyanate crosslinking agents are preferred, with nurate compounds of hexamethylene diisocyanate and adducts of 2,4-tolylene diisocyanate with trimethylolpropane being more preferred.

[0055] Examples of the epoxy crosslinking agent (B2) include bisphenol A-epichlorohydrin type epoxy resins, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl erythritol, diglycerol polyglycidyl ether, etc. One selected from these may be used alone, or two or more may be used in combination. Of these, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane is preferred.

[0056] Examples of the metal chelate crosslinking agent (B3) include acetylacetone and acetoacetyl ester coordination compounds of polyvalent metals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, zirconium, etc. One selected from these may be used alone, or two or more may be used in combination.

[0057] Examples of the aziridine crosslinking agent (B4) include tetramethylolmethane-tri-β-aziridinylpropionate, trimethylolpropane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), etc. One selected from these may be used alone, or two or more may be used in combination.

[0058] It is preferable to use at least two crosslinking agents selected from the group consisting of isocyanate-based crosslinking agents (B1), epoxy-based crosslinking agents (B2), metal chelate-based crosslinking agents (B3) and aziridine-based crosslinking agents (B4), and it is particularly preferable to use a combination of an isocyanate-based crosslinking agent (B1) and an epoxy-based crosslinking agent (B2).

[0059] The content of the crosslinking agent (B) is preferably 0.01 to 20 parts by weight, more preferably 0.1 to 15 parts by weight, and particularly preferably 1 to 10 parts by weight, relative to 100 parts by weight of the acrylic resin (A). In particular, when the isocyanate-based crosslinking agent (B1) and the epoxy-based crosslinking agent (B2) are used in combination, the content of the isocyanate-based crosslinking agent (B1) is preferably 1 to 10 parts by weight, more preferably 1.5 to 8 parts by weight, and particularly preferably 2 to 4 parts by weight, relative to 100 parts by weight of the acrylic resin (A), and the content of the epoxy-based crosslinking agent (B2) is preferably 0.01 to 1 part by weight, more preferably 0.02 to 0.5 parts by weight, and particularly preferably 0.02 to 0.2 parts by weight. If the content of crosslinking agent (B) is too low, the cohesive strength of the adhesive will decrease, and the staining resistance will tend to decrease. If the content is too high, unreacted crosslinking agent will remain, which will tend to cause staining of the adherend.

[0060] The pressure-sensitive adhesive composition of the present invention may contain a crosslinking agent other than the isocyanate-based crosslinking agent (B1), the epoxy-based crosslinking agent (B2), the metal chelate-based crosslinking agent (B3) and the aziridine-based crosslinking agent (B4), for example, a melamine-based crosslinking agent, an aldehyde-based crosslinking agent, an amine-based crosslinking agent, etc., within the range in which the effects of the present invention are not lost.

[0061] Examples of the melamine-based crosslinking agent include hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexaptoxymethylmelamine, hexapentyloxymethylmelamine, hexahexyloxymethylmelamine, melamine resins, and the like.

[0062] Examples of the aldehyde crosslinking agent include glyoxal, malondialdehyde, succindialdehyde, maleic dialdehyde, glutaric dialdehyde, formaldehyde, acetaldehyde, and benzaldehyde.

[0063] Examples of the amine-based crosslinking agent include hexamethylenediamine, triethyldiamine, polyethyleneimine, hexamethylenetetraamine, diethylenetriamine, triethyltetraamine, isophoronediamine, amino resins, and polyamides.

[0064] <Tackifier (C)> The tackifier (C) used in the present invention contains 50% by weight or more, preferably 70% by weight or more, more preferably 85% by weight or more, and particularly preferably 95% by weight or more of the tackifier (C1) having a softening point of 130° C. or less as a whole of the tackifier (C). The upper limit of the content of the tackifier (C1) is 100% by weight. If the content is too low, the removability is likely to decrease, making it difficult to obtain the effects of the present invention. Examples of such tackifiers (C1) include tackifiers such as rosin-based resins, phenol-based resins, terpene-based resins, modified terpene-based resins, hydrocarbon-based resins, epoxy-based resins, polyamide-based resins, elastomer-based resins, and ketone-based resins, which have a softening point of 130°C or less. Preferred examples include rosin-based resins (C1-1) having a softening point of 130°C or less. In addition, the tackifier (C) may contain a tackifier having a softening point of more than 130°C. In this case, the softening point of the tackifier (C) as a composition is preferably 180°C or lower, and more preferably 150°C or lower. The softening point of the tackifier (C) was determined by the following method (R&B (ring & ball) method) in accordance with JIS K5902 5.3 (1969). The softening point can be measured, for example, by an automatic softening point measuring device (manufactured by Elex Science Co., Ltd.) that automates heating and softening point measurement. In addition, when there is a range of softening points, the average value of the sum of the upper limit and the lower limit is regarded as the softening point.

[0065] [Rosin-based resin] Rosin resin is an amber-colored, amorphous natural resin obtained from pine trees, and its main component is a mixture of abietic acid and its isomers. In addition, rosin resins that have been modified by esterification, polymerization, hydrogenation, etc., utilizing the reactivity of abietic acid or its isomers are also included in the rosin resins. For example, unmodified rosin (e.g., tall rosin, gum rosin, and wood rosin), polymerized rosin, disproportionated rosin, hydrogenated rosin, maleic acid-modified rosin, fumaric acid-modified rosin, esters of these (e.g., glycerin ester, pentaerythritol ester, methyl ester, ethyl ester, butyl ester, and ethylene glycol ester), and those further modified by hydrogenation, etc., are included, and disproportionated rosin esters are preferably used from the viewpoints of heat resistance and color resistance.

[0066] Among rosin-based resins, those containing a high proportion of biologically derived raw materials are preferably used from the viewpoint of reducing the environmental load, and the biomass ratio of the rosin-based resin is preferably 70% by mass or more.

[0067] [Biomass content of tackifier (C)] From the viewpoint of reducing the environmental load, the biomass degree in the tackifier (C) is preferably 70% by weight or more, more preferably 75% by weight or more, even more preferably 80% by weight or more, and particularly preferably 90% by weight or more, with the upper limit being 100% by weight. The higher the content, the more renewable resources are increased, which is preferable. The biomass degree may be any value obtained by any one of the calculation methods shown below, as long as it falls within the above range.

[0068] (How to calculate biomass ratio) Biomass degree (wt%) of tackifier (C)=[(biomass degree of each biological raw material used in producing tackifier (C))×(weight of each biological raw material used in producing tackifier (C)] / (total weight of tackifier (C))×100]

[0069] The biomass ratio can also be determined by analyzing the composition ratio by NMR and calculating the carbon number of the biologically derived monomer / the total carbon number.

[0070] While carbon derived from living organisms contains a certain percentage of radioactive isotopes (C-14), carbon derived from petroleum contains almost no C-14. Therefore, the biomass content can also be calculated by measuring the concentration of C-14 contained in the adhesive. Specifically, it can be measured according to ASTM D6866, a standard used in many bioplastic industries.

[0071] As described above, the tackifier (C) used in the present invention may contain a tackifier other than the tackifier (C1) having a softening point of 130° C. or less, i.e., a tackifier having a softening point of more than 130° C. For example, it may contain a resin having a softening point of more than 130° C., such as a rosin-based resin, a phenol-based resin, a terpene-based resin, a modified terpene-based resin, a hydrocarbon-based resin, an epoxy-based resin, a polyamide-based resin, an elastomer-based resin, or a ketone-based resin. One selected from these tackifiers may be used alone, or two or more may be used in combination.

[0072] The content of the tackifier (C) is preferably 0.1 to 50 parts by weight, more preferably 1 to 40 parts by weight, particularly preferably 3 to 35 parts by weight, and further preferably 5 to 30 parts by weight, based on 100 parts by weight (solid content) of the acrylic resin (A). If the content is too small, the effects of the present invention tend to be difficult to obtain.

[0073] <Other ingredients> The adhesive composition of the present invention may further contain additives such as antioxidants, plasticizers, fillers, antistatic agents, pigments, diluents, antioxidants, UV absorbers, and UV stabilizers, within the scope of the present invention, and the antioxidants are particularly effective in maintaining the stability of the adhesive layer. One type selected from these additives may be used alone, or two or more types may be used in combination. In addition to the additives, the adhesive composition may contain a small amount of impurities contained in the manufacturing raw materials of the components of the adhesive composition.

[0074] When the above additives are used, the content is preferably 5 parts by mass or less, more preferably 1 part by mass or less, and particularly preferably 0.5 parts by mass or less, based on 100 parts by mass of the acrylic resin (A). The lower limit is usually 0 parts by mass. If the content is too high, the effect of the present invention tends to be impaired.

[0075] The pressure-sensitive adhesive composition of the present invention contains at least the above-mentioned acrylic resin (A), crosslinking agent (B) and tackifier (C), and can be obtained by mixing additives as necessary.

[0076] The method for mixing these components is not particularly limited, and various methods can be used, such as a method in which the components are mixed together at once, or a method in which any component is mixed and then the remaining components are mixed together or sequentially.

[0077] The proportion of plant-derived carbon in the entire pressure-sensitive adhesive composition of the present invention, i.e., the biomass ratio, is preferably 30% by weight or more, more preferably 40% by weight or more, particularly preferably 50% by weight or more, and particularly preferably 60% by weight or more, from the viewpoint of reducing the environmental load, with the upper limit being 100% by weight.

[0078] The biomass degree of the PSA composition is the ratio of the mass of the biologically derived raw materials used in producing the PSA composition to the total mass of the PSA composition, and can be calculated, for example, by the following formula. Biomass ratio (wt%) of adhesive composition=[(biomass ratio of each biological raw material used in producing the adhesive composition)×(weight of each biological raw material used in producing the adhesive composition)] / (total weight of the adhesive composition)×100]

[0079] The biomass degree of the pressure-sensitive adhesive composition can also be measured by the above-mentioned method using NMR or method using natural radioactive carbon C-14. The biomass degree may be determined by any of the above-mentioned calculation methods as long as the value obtained by the method falls within the above-mentioned range.

[0080] [Adhesive] When the adhesive composition of the present invention contains a solvent, it can be dried to form an adhesive. The adhesive composition of the present invention can also be crosslinked to form the adhesive of the present invention. The adhesive of the present invention has the following physical properties.

[0081] <Gel fraction> The gel fraction of the pressure-sensitive adhesive of the present invention is usually 40 to 100%, preferably 50 to 90%, more preferably 60 to 85%, and particularly preferably 65 to 80%. If the gel fraction is too low, the cohesive strength of the pressure-sensitive adhesive decreases, causing adhesive residue and tending to cause contamination of the adherend.

[0082] The gel fraction of the pressure-sensitive adhesive can be adjusted to the above range by, for example, adjusting the type and amount of the crosslinking agent (B), adjusting the composition ratio of hydroxyl groups in the composition, etc. The content of the crosslinking agent (B) and the ratio of the amount of functional groups contained in the acrylic resin (A) need to be balanced because the gel fraction changes due to the interaction between them.

[0083] The gel fraction is an indication of the degree of crosslinking, and is calculated, for example, by the following method. An adhesive sheet (without a separator) consisting of an adhesive layer formed on a polymer sheet (e.g., polyethylene terephthalate film, etc.) as a substrate is wrapped in a 200-mesh SUS wire netting and immersed in toluene at 23°C for 24 hours, and the weight percentage of the insoluble adhesive component remaining in the wire netting is taken as the gel fraction. The weight of the adhesive component is calculated by subtracting the weight of the substrate from the weight of the adhesive sheet.

[0084] <Initial adhesive strength> The initial adhesive strength of the adhesive of the present invention is preferably 3N / 25mm or more, more preferably 5N / 25mm or more, and particularly preferably 8N / 25mm or more. When using the adhesive film of the present invention, if the adhesive strength becomes too large after high temperature or moist heat loading, peeling may not be possible, the substrate may break during peeling, or contamination due to adhesive residue may easily occur. The adhesive strength after high temperature or moist heat loading is preferably 8 times or less than the initial adhesive strength, more preferably 5 times or less, and particularly preferably 4 times or less. The adhesive strength is the 180° peel adhesive strength (N / 25mm) obtained according to the test method of [Initial adhesive strength] in the examples described later. Therefore, the pressure-sensitive adhesive of the present invention can be suitably used as a pressure-sensitive adhesive for double-sided tapes.

[0085] [Adhesive layer and adhesive film] The pressure-sensitive adhesive film of the present invention has a pressure-sensitive adhesive layer made of the above-mentioned pressure-sensitive adhesive, and can be obtained by laminating the pressure-sensitive adhesive layer on a film as a substrate. Examples of substrates on which the pressure-sensitive adhesive layer is laminated include single-layer or laminated films made of metals, polyester resins, polyethylene fluoride resins, polyimides and their derivatives, epoxy resins, etc., but from the standpoint of heat resistance and convenience in practical use, polyester films and polyimide films are preferred, and polyester films are more preferred. It is preferable that the adhesive film has a release film on the surface opposite to the substrate of the adhesive layer. When the adhesive film is put to practical use, the release film is peeled off before use. As the release film, a silicon-based release film, an olefin-based release film, a fluorine-based release film, a long-chain alkyl-based release film, or an alkyd-based release film can be used.

[0086] Examples of methods for producing the above-mentioned adhesive film using the adhesive composition of the present invention include [1] a method of applying the adhesive composition onto a substrate, drying to form an adhesive layer, laminating a release film onto the surface of the adhesive layer, and performing an aging treatment, and [2] a method of applying the adhesive composition onto a release film, drying to form an adhesive layer, laminating a substrate onto the surface of the adhesive layer, and performing an aging treatment. Among these, method [2] is preferred in terms of not damaging the substrate, workability, and stable production.

[0087] The aging treatment is carried out to balance the adhesive properties, and the aging conditions are that the temperature is usually 0 to 150°C, preferably 10 to 100°C, and more preferably 20 to 80°C, and the time is usually less than 30 days, preferably less than 14 days, and more preferably less than 7 days. Specifically, the aging can be carried out under conditions such as 23°C for 3 to 10 days and 40°C for 1 to 7 days. By using an isocyanate-based crosslinking agent (B1) as a crosslinking agent, the aging period can be shortened, and the adhesive film can be produced efficiently.

[0088] When applying the adhesive composition, it is preferable to dilute the adhesive composition in a solvent and apply it, and the dilution concentration is preferably 5 to 60% by weight, more preferably 10 to 50% by weight. The solvent used for dilution is not particularly limited as long as it dissolves the adhesive composition, and for example, ester-based solvents such as methyl acetate, ethyl acetate, methyl acetoacetate, and ethyl acetoacetate; ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; aromatic solvents such as toluene and xylene; and alcohol-based solvents such as methanol, ethanol, and propyl alcohol can be used. Among these, ethyl acetate, acetone, methyl ethyl ketone, and toluene are preferably used in terms of solubility, drying property, and price.

[0089] The pressure-sensitive adhesive composition can be applied by a conventional method such as roll coating, die coating, gravure coating, comma coating, or screen printing.

[0090] The thickness of the adhesive layer in the adhesive film is preferably 5 to 300 μm, more preferably 5 to 60 μm, and particularly preferably 10 to 30 μm. If the adhesive layer is too thin, the adhesive properties tend to be difficult to stabilize, whereas if it is too thick, the overall thickness of the adhesive film tends to increase, decreasing usability.

[0091] The pressure-sensitive adhesive film of the present invention can be used, for example, as a removable double-sided tape for fastening two types of items in daily life, or as a temporary double-sided tape used to temporarily hold or reinforce a product during the manufacturing process. In addition, since the pressure-sensitive adhesive film of the present invention can be attached to a metal adherend or an adherend made of a low-polarity material such as olefin, it can be preferably applied to metal adherends or low-polarity adherends used as structural members or exterior parts of transportation equipment, etc., in addition to the above-mentioned uses. Specific examples include automobiles (including passenger cars, trucks, buses, three-wheeled motor vehicles, tractors, snowmobiles, bulldozers, amphibious vehicles, etc.), railway vehicles (including trains such as Shinkansen, diesel cars, linear motor cars, cable cars, monorails, trolley buses, etc.), aircraft (including airplanes, helicopters, air cushion boats, etc.), ships (including large ships, small ships, water scooters, etc.), etc. As a preferred example, it can be preferably used for aluminum members (typically duralumin members) for structural members of aircraft. Examples of the adherend to which the pressure-sensitive adhesive film is to be attached include substrates made of the materials shown below.

[0092] Metal plates or foils such as aluminum, copper, iron, stainless steel, magnesium, nickel, and titanium; Stone materials such as marble, granite, artificial stone, terrazzo, ceramic tiles, etc.; Polyester resins such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene terephthalate / isophthalate copolymers, and ester acrylates; Polyolefin resins such as polyethylene, chlorinated polyethylene, chlorosulfonated polyethylene, ethylene propylene rubber, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, ethylene-isobutyl acrylate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, inonomer, polypropylene, polyallomer polybutylene, and polymethylpentene; Polyfluoroethylene resins such as polyvinyl fluoride, polyvinylidene fluoride, polyethylene tetrafluoride, and ethylene-ethylene tetrafluoride copolymers; Polystyrene, poly-alpha-methylstyrene, acrylonitrile-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, acrylonitrile-styrene-acrylate copolymers; polyalkyl (meth)acrylates such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; acrylic resins such as methyl methacrylate-styrene copolymers and methyl methacrylate-α-methylstyrene copolymers; Polyvinyl chloride polymers and their derivatives, such as polyvinyl chloride, plasticized polyvinyl chloride, ABS modified polyvinyl chloride, post-chlorinated polyvinyl chloride, polyvinyl chloride-acrylic resin alloy, vinyl chloride-propylene copolymer, vinyl chloride-vinyl acetate copolymer, polyvinylidene chloride, etc.; Polyvinyl acetate, polyvinyl alcohol, polyvinyl formal, polyvinyl butyral, ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, vinylon, and other polyvinyl acetates and their derivatives; Polyvinyl methyl ether, polyvinyl methyl ketone; Polyethers such as polyformaldehyde, acetal copolymers, polyethylene oxide, polypropylene oxide, chlorinated polyethers, phenoxy resins, and polyphenylene oxide; Fluorinated resins such as polytetrafluoroethylene, polychlorotrifluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, polyvinylidene fluoride, and chlorotrifluoroethylene-vinylidene fluoride copolymer; Polycarbonate, Polycarbonate ABS Alloy; Nylons (polyamides) such as nylon, nylon-6, nylon-6,6, nylon-6 / 6,6 copolymer, nylon-6,10, nylon-6,12, nylon-11, nylon-12, etc.; Butadiene-styrene copolymers, butadiene-based plastics; Polyimides and their derivatives, polysulfones, polyphenylene sulfides, high acrylonitrile copolymers; Silicone resins, semi-inorganic and inorganic polymers; Phenolic resins and their derivatives, such as phenolic resin, phenol-furfural resin, modified phenolic resin, etc.; Formalin resins such as furan resins, xylene resins, aniline resins, acetone formaldehyde resins; Unsaturated polyester and alkyd resins; Epoxy resins such as bisphenol type epoxy resins, epoxy resin composite materials, alicyclic epoxy resins, epoxy novolacs, biphenyl type epoxy resins, and epoxy acrylates; Polyurethanes such as polyurethane, urethane foam, and urethane acrylate; Allyl resins such as diallyl phthalate resin, triallyl cyanurate resin, polyallyl sulfone, allyl diglycol carbonate, polyallyl ether, and polyarylate; Cellulosic plastics, cellulose resins such as cellulose acetate, cellulose propionate, cellulose acetate butyrate, ethyl cellulose, nitrocellulose and cellulosic resins such as cellulosic plastics ...cellulose propionate, cellulose acetate butyrate, cellulose acetate butyrate butyrate butyrate butyrate butyrate butyrate but

[0093] In particular, examples of heat-resistant materials include metal plates or foils such as aluminum, copper, iron, stainless steel, magnesium, nickel, and titanium; stone materials such as marble, granite, artificial stone, terrazzo, and ceramic tiles; polyester-based resins such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene terephthalate / isophthalate copolymer, and ester acrylate; polyfluoroethylene-based resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, and ethylene-tetrafluoroethylene copolymer; polyimide and its derivatives; and epoxy resins such as bisphenol-type epoxy resins, epoxy resin composite materials, alicyclic epoxy resins, epoxy novolac, biphenyl-type epoxy resins, and epoxy acrylates.

[0094] The adhesive film obtained by using the adhesive composition of the present invention is preferably used in various applications requiring moist heat resistance. For example, it can be used as a packaging bag for medicines; a protective film for preventing curling, wrinkling, and contamination of films and foils caused by moist heat load; a barrier film with excellent water vapor barrier properties; a film for fixing substrates and glass used in display panels, etc.; a masking film during the solder reflow process of electronic circuit boards; various temporary fixing and component protection films, etc., and it can be widely used in tape applications and temporary fixing applications requiring moist heat resistance.

[0095] The method of using the adhesive film of the present invention, particularly the adhesive film for double-sided tape, will be described. First, the adhesive film for double-sided tape of the present invention is attached to the surface of the adherend. For example, a rubber roller can be used as a means for attachment. Next, the adherend to which the adhesive film is attached is attached to another adherend and fixed. After use in the fixed state is finished, when it is no longer necessary to fix with the adhesive film for double-sided tape, the adhesive film for double-sided tape is peeled off from the surface of the adherend. The adhesive film for double-sided tape of the present invention is unlikely to become contaminated when peeled off from an adherend even after long-term use in a high-humidity environment, and has sufficiently high adhesive performance, making it effective for temporary fixing of adherends.

[0096] The biomass degree in the pressure-sensitive adhesive layer (pressure-sensitive adhesive) is almost the same as that in the pressure-sensitive adhesive composition, and therefore the preferred value is the same and can be calculated by the same method. The high biomass degree of the pressure-sensitive adhesive composition of the present invention makes the pressure-sensitive adhesive layer (pressure-sensitive adhesive) obtained by using such a pressure-sensitive adhesive composition environmentally friendly. EXAMPLES

[0097] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are by weight. In the following examples, the weight average molecular weight, dispersity, glass transition temperature and other physical properties of the acrylic resin (A) were measured according to the methods described above. First, prior to the examples, the following components were prepared.

[0098] <Acrylic resin (A)> The following were used as raw material monomers for the acrylic resin. Monomer (a1) NOAA: n-octyl acrylate (straight-chain alkyl group with 8 carbon atoms, manufactured by Osaka Organic Chemical Industry Co., Ltd.) Monomer (a2) Aac: Acrylic acid (Osaka Organic Industry Co., Ltd.) HEMA: Hydroxyethyl methacrylate (linear alkyl group with 2 carbon atoms, manufactured by Mitsubishi Gas Chemical Company, Inc.) Other copolymerizable monomers (a3) 2EHA: 2-ethylhexyl acrylate (branched alkyl group with 8 carbon atoms) BA: Butyl acrylate (alkyl group carbon number: 4)

[0099] [Production of acrylic resin (A-1)] A four-necked round-bottom flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet, and a thermometer was charged with 64 parts of ethyl acetate and 0.04 parts of azobisisobutyronitrile (AIBN) as a polymerization initiator, and heated until the internal temperature reached the boiling point. A mixed solution of 91.9 parts of NOAA, 8 parts of Aac, and 0.1 parts of HEMA was added dropwise over a period of 2 hours while maintaining the boiling state. One hour after the monomer addition was completed, 0.05 parts of polymerization initiator (AIBN) and 4 parts of ethyl acetate were added and the reaction was allowed to proceed for 2 hours. Further, 0.036 parts of a polymerization initiator (AIBN) and 4 parts of ethyl acetate were added and reacted for 2 hours, after which the mixture was diluted with 50.2 parts of ethyl acetate to obtain an acrylic resin (A-1) solution [solid concentration 45%, viscosity 3000 mPa·s / 25°C, acrylic resin (A-1): weight average molecular weight (Mw) 700,000, dispersity (Mw / Mn) 5.4, glass transition temperature (Tg) -49°C].

[0100] The ratio of each copolymerization component (a) in the acrylic resin (A-1) was changed as shown in Table 1, and acrylic resins (A'-2) to (A'-6) were produced using the same polymerization recipe.

[0101] [Table 1]

[0102] <Crosslinking agent (B)> As the crosslinking agent (B), the following was used. Isocyanate-based crosslinking agent (B1): Trimethylolpropane adduct of tolylene diisocyanate (Examples 1 to 3, Comparative Examples 1 to 14: Coronate L-55E, manufactured by Tosoh Corporation) (Comparative Examples 15 to 18: Takenate D-101E, manufactured by Mitsui Chemicals, Inc.) Epoxy crosslinking agent (B2): 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (Tetrad C, manufactured by Mitsubishi Gas Chemical Co., Ltd.)

[0103] <Tackifier (C)> The following was used as the tackifier (C). [Tackifier with a softening point of 130°C or less (C1)] Super Ester A-100: Disproportionated rosin ester resin (manufactured by Arakawa Chemical Industries, softening point: 100°C, biomass content: 95-100%) Pine Crystal KE-604: Hydrogenated rosin ester resin (manufactured by Arakawa Chemical Industries, softening point: 130°C, biomass content: 80-94%) Pine Crystal KE-359: Hydrogenated rosin ester resin (manufactured by Arakawa Chemical Industries, hydroxyl value: 40, softening point: 100°C, biomass ratio: 80-94%) [Other tackifiers] YS Polyster G-150: Terpene phenol resin (manufactured by Yasuhara Chemical Co., Ltd., softening point: 150°C) Pencel D-135: Polymerized rosin ester resin (manufactured by Arakawa Chemical Industries, softening point: 135°C, biomass content: 80-94%)

[0104] <Example 1> 2.8 parts of crosslinking agent (B1) (Coronate L-55E) and 10 parts of tackifier (C1) (Super Ester A-100) were mixed with 100 parts of solid content of the acrylic resin (A-1) obtained above, and further diluted with ethyl acetate to a solid content concentration of 20%. This adhesive composition solution was applied onto a polyethylene terephthalate (PET) film (thickness 38 μm) as a substrate so that the thickness after drying was about 10 μm, and dried at 100 ° C for 5 minutes. Thereafter, a release-treated PET film was attached to the coated surface for protection, and the film was aged for 7 days in an atmosphere at a temperature of 40 ° C to obtain an adhesive film.

[0105] <Examples 2 and 3, Comparative Examples 1 to 18> As shown in Table 2, pressure-sensitive adhesive films were obtained in the same manner as in Example 1 using the acrylic resins (A'-2) to (A'-6), the crosslinking agent (B), and the tackifier (C).

[0106] The adhesive films obtained in Examples 1 to 3 and Comparative Examples 1 to 18 were evaluated for olefin adhesion and removability to various adherends, and the results are summarized in Tables 3 and 4. The release-treated PET film was peeled off when various measurement tests were carried out. The gel fraction of the adhesive was also measured for each adhesive film, and the results are summarized in Table 2.

[0107] [Table 2]

[0108] [Olefin Adhesion] The adhesive film obtained above was cut to a width of 25 mm and a length of 150 mm to prepare a test piece. Next, a polypropylene (PP) plate (manufactured by Nippon Test Panel Co., Ltd.) was used as an adherend, and the film was pressed and attached with a 2 kg rubber roller in two passes in an atmosphere of 23°C and 50% relative humidity, and then left for 30 minutes in the same atmosphere, after which the 180° peel adhesion (N / 25 mm) was measured at a peel speed of 300 mm / min in accordance with JIS Z0237. The adhesive strength was evaluated according to the following criteria. ○: 8.0N / 25mm or more, △: Less than 8.0N / 25mm, 5.0N / 25mm or more ×: Less than 5.0N / 25mm

[0109] [Evaluation of removability from various adherends] (Adhesive strength after heating) The adhesive film obtained above was cut to a width of 25 mm and a length of 150 mm to prepare a test piece. Next, stainless steel (SUS) plate (SUS304BA plate, manufactured by Engineering Test Services, JIS standard compliant), polypropylene (PP) plate (manufactured by Nippon Test Panel), acrylonitrile butadiene styrene (ABS) plate (manufactured by Engineering Test Services), and polyvinyl chloride (PVC) plate (manufactured by Nippon Test Panel) were used as adherends, and the plates were pressed and attached with a 2 kg rubber roller in two strokes at 23°C and 50% relative humidity, and left in the same atmosphere for 30 minutes. The plates were then left to stand for 360 hours in an 80°C environment, and then left to stand for 2 hours in an atmosphere at 23°C and 50% relative humidity. In accordance with JIS Z0237, the 180° peel adhesion (N / 25mm) was measured at a peel speed of 300mm / min. In addition, the contamination (glue residue) on the adherend surface after peeling was visually confirmed and evaluated as follows. ○: No contamination was observed. △: Slight contamination was observed. ×: Contamination was clearly confirmed.

[0110] (Adhesive strength after heat and humidity) The adhesive film obtained above was cut to a width of 25 mm and a length of 150 mm to prepare a test piece. Next, the above-mentioned SUS, PP, ABS, and PVC test plates were used as adherends, and the test pieces were pressed and attached with a 2 kg rubber roller in two passes in an atmosphere of 23°C and 50% relative humidity, and left in the same atmosphere for 30 minutes. Next, the test pieces were left to stand for 720 hours in an environment of 60°C and 90% RH, and then left for 2 hours in an atmosphere of 23°C and 50% relative humidity. In accordance with JIS Z0237, the 180° peel adhesion (N / 25mm) was measured at a peel speed of 300mm / min. In addition, the contamination (glue residue) on the adherend surface after peeling was visually confirmed and evaluated as follows. ○: No contamination was observed. △: Slight contamination was observed. ×: Contamination was clearly confirmed.

[0111] [Table 3]

[0112] [Table 4]

[0113] The pressure-sensitive adhesive films of Examples 1 to 3 using the pressure-sensitive adhesive composition of the present invention had excellent olefin adhesion and also excellent removability from various adherends. On the other hand, the adhesive films of Comparative Examples 1 and 8 to 14, which used an acrylic resin (A'-4) with an acid value of less than 15 mgKOH / g, had poor removability after heating and after moist heat. The adhesive films of Comparative Examples 2 to 7, which used an adhesive composition not containing a tackifier (C), and the adhesive films of Comparative Examples 11 to 18, which used an adhesive composition in which the tackifier (C1) having a softening point of 130°C or less accounts for less than 50% by weight of the total tackifier (C), had low olefin adhesion and were also poor in removability. [Industrial Applicability]

[0114] The pressure-sensitive adhesive composition of the present invention can be suitably used as a composition for forming a pressure-sensitive adhesive layer in various pressure-sensitive adhesive films, and can be particularly suitably used in applications where the adherend is an olefin-based material. The pressure-sensitive adhesive film of the present invention can be used, for example, as a removable double-sided tape for fastening two types of items in daily life, or as a temporary double-sided tape used to temporarily hold or reinforce a product during the manufacturing process.

Claims

1. A pressure-sensitive adhesive composition comprising an acrylic resin (A), a crosslinking agent (B) and a tackifier (C), the acrylic resin (A) contains, as a main structural unit, a structural unit derived from a (meth)acrylic acid alkyl ester monomer (a1) having a linear alkyl group having 8 to 10 carbon atoms, contains a structural unit derived from a functional group-containing monomer (a2) having a crosslinkable functional group, and has an acid value of 15 mgKOH / g or more; The pressure-sensitive adhesive composition, wherein the tackifier (C) contains a tackifier (C1) having a softening point of 130° C. or less in an amount of 50% by weight or more of the total tackifier (C).

2. The pressure-sensitive adhesive composition according to claim 1 , wherein the proportion of plant-derived carbon in the entire pressure-sensitive adhesive composition is 50% or more.

3. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the functional group-containing monomer (a2) is a hydroxyl group-containing monomer and / or a carboxyl group-containing monomer.

4. 3. The pressure-sensitive adhesive composition according to claim 1, having an acid value of 20 mgKOH / g or more.

5. 3. The pressure-sensitive adhesive composition according to claim 1, wherein the crosslinking agent (B) contains at least two types of crosslinking agents selected from the group consisting of an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a metal chelate-based crosslinking agent, and an aziridine-based crosslinking agent.

6. 3. The pressure-sensitive adhesive composition according to claim 1, wherein the tackifier (C) contains a rosin-based resin (C1-1) having a softening point of 130° C. or lower.

7. A pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to claim 1 or 2.

8. The pressure-sensitive adhesive according to claim 7, wherein the pressure-sensitive adhesive has a gel fraction of 50 to 90%.

9. A pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive according to claim 7 .

10. A pressure-sensitive adhesive film having the pressure-sensitive adhesive layer according to claim 9 thereon.

Citation Information

Patent Citations

  • 2-Octyl (meth)acrylate adhesive composition

    JP2010506979A

  • Adhesive tape

    JP2019218458A