Composition for polishing, polishing method, and method for manufacturing semiconductor substrate
The polishing composition with abrasive grains and quaternary phosphonium salt at specific pH and zeta potential effectively polishes low-k materials and silicon nitride at high rates with controlled selectivity, addressing the inefficiencies of existing technologies.
Patent Information
- Application Number
- JP2024035117
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-14
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-01
AI Technical Summary
Existing polishing compositions fail to achieve a high polishing rate for low-k materials like SiOC and Si3N4 while maintaining an appropriate selectivity ratio between them.
A polishing composition containing abrasive grains with a zeta potential of -10 mV or less and a quaternary phosphonium salt at a pH less than 7.0, which enhances the polishing rate and selectivity of low-k materials and silicon nitride.
The composition achieves a high polishing rate of 300 Å/min or more for both low-k materials and silicon nitride with a selectivity ratio of 1.0 to 2.0, improving the polishing efficiency and surface quality.
Smart Images

Figure 2024132946000001 
Figure 2024132946000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing composition, a polishing method, and a method for producing a semiconductor substrate. [Background technology]
[0002] In recent years, new microfabrication technologies have been developed to accompany the high integration and high performance of LSI (Large Scale Integration). Chemical mechanical polishing (CMP) is one of these technologies, and is frequently used in the LSI manufacturing process, especially in the multi-layer wiring formation process, for planarizing interlayer insulating films, forming metal plugs, and forming buried wiring (damascene wiring).
[0003] In order to suppress the capacitance between wiring, low-dielectric constant (Low-k) materials are being adopted as materials for the interlayer insulating film in the multi-layer wiring formation process. SiOC (carbon-containing silicon oxide, SiO2 doped with C) formed by the plasma CVD method is widely used as a low-dielectric constant (Low-k) material.
[0004] As a technique for polishing SiOC, Patent Document 1 discloses a polishing composition containing cerium-containing abrasive grains and hydroxyalkyl cellulose, and having a pH of 6.0 or more. According to Patent Document 1, such a composition is said to improve the polishing rate of SiOC. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-139349 A Summary of the Invention [Problem to be solved by the invention]
[0006] Recently, substrates containing both low-k material, typically SiOC, and Si3N4 (silicon nitride) have been used. In such substrates, there is an increasing demand for polishing low-k material and silicon nitride at a high polishing rate while polishing at a moderate polishing rate selectivity (for example, polishing rate of low-k material / polishing rate of Si3N4=1.0 or more and 2.0 or less). However, the polishing composition described in Patent Document 1 has a problem of not satisfying such requirements.
[0007] Therefore, an object of the present invention is to provide a means capable of polishing low-k materials and silicon nitride at a high polishing rate, and capable of achieving an appropriate selectivity ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by a polishing composition that contains abrasive grains and a quaternary phosphonium salt, has a pH of less than 7.0, and has a zeta potential of the abrasive grains in the polishing composition of -10 mV or less, and have completed the present invention. Effect of the Invention
[0009] According to the present invention, a means can be provided that can polish low-k materials and silicon nitride at high polishing rates and can achieve an appropriate selectivity ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] According to one embodiment of the present invention, there is provided a polishing composition comprising an abrasive grain and a quaternary phosphonium salt, having a pH of less than 7.0, and a zeta potential of the abrasive grain in the polishing composition of -10 mV or less. According to such a polishing composition of the present invention, low-k materials and silicon nitride can be polished at a high polishing rate, and the selectivity of the polishing rate of the low-k material to the polishing rate of silicon nitride can be made appropriate (for example, the polishing rate of the low-k material / polishing rate of Si3N4=1.0 or more and 2.0 or less).
[0011] Although the details of why the polishing composition of the present invention provides the above-mentioned effects are unclear, it is believed that the mechanism is as follows. Note that the mechanism is based on speculation, and the technical scope of the present invention is not limited by the mechanism.
[0012] Although the surface of a low-k material is generally hydrophobic, a quaternary phosphonium salt having an organic group is easily adsorbed to the low-k material. The zeta potential of the surface of a low-k material is close to 0 under acidic conditions, but the zeta potential of the surface of a low-k material to which a quaternary phosphonium salt is adsorbed turns positive. This makes it easier for abrasive grains having a negative zeta potential of -10 mV or less to come into contact with the surface of a low-k material having a positive zeta potential, increasing the frequency of contact of the abrasive grains and increasing the polishing rate. In addition, a quaternary phosphonium salt does not adsorb well to the surface of silicon nitride, and a high polishing rate can be maintained. As a result, the polishing rates of the low-k material and silicon nitride are increased, and the selectivity of the polishing rate of the low-k material to the polishing rate of silicon nitride can be made moderate (for example, the polishing rate of the low-k material / polishing rate of Si3N4=1.0 or more and 2.0 or less).
[0013] The embodiments of the present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in various ways within the scope of the claims. The embodiments described in this specification can be combined in any way to form other embodiments. In this specification, unless otherwise specified, operations and measurements of physical properties are performed under conditions of room temperature (20°C to 25°C) and relative humidity of 40% RH to 50% RH.
[0014] [Abrasive grain] The polishing composition according to the present invention contains abrasive grains. The abrasive grains have the function of mechanically polishing an object to be polished, and increase the polishing rate of the object to be polished by the polishing composition.
[0015] In the polishing composition of the present invention, the abrasive grains have a zeta potential of -10mV or less. Here, the "zeta (ζ) potential" refers to the potential difference that occurs at the interface between a solid and a liquid that are in contact with each other when they move relative to each other. If the zeta potential of the abrasive grains exceeds -10mV, the polishing speed of low-k materials and silicon nitride decreases.
[0016] In the polishing composition of the present invention, the zeta potential of the abrasive grains is preferably -60 mV or more and -10 mV or less, more preferably -50 mV or more and -10 mV or less, even more preferably -45 mV or more and -15 mV or less, and particularly preferably -40 mV or more and -15 mV or less. When the abrasive grains have a zeta potential in such a range, the polishing speed of the object to be polished can be further improved. Here, the zeta potential of the abrasive grains in the polishing composition is a value measured by the method described in the Examples. In addition, the zeta potential of the abrasive grains can be adjusted by the amount of anionic groups (particularly organic acid groups) of the abrasive grains described below, the pH of the polishing composition, etc.
[0017] The type of abrasive grains is not particularly limited, and examples thereof include metal oxides such as silica, alumina, zirconia, and titania. The abrasive grains can be used alone or in combination of two or more kinds. The abrasive grains may be either commercially available products or synthetic products.
[0018] The type of abrasive grain is preferably silica, more preferably colloidal silica.The method for producing colloidal silica includes sodium silicate method and sol-gel method, and the colloidal silica produced by any method can be suitably used as the abrasive grain of the present invention.However, from the viewpoint of reducing metal impurities, the colloidal silica produced by the sol-gel method is preferred because it can be produced with high purity.
[0019] Colloidal silica can be produced by the sol-gel method using a conventionally known method. Specifically, colloidal silica can be obtained by using a hydrolyzable silicon compound (e.g., alkoxysilane or a derivative thereof) as a raw material and carrying out a hydrolysis-condensation reaction.
[0020] In some embodiments of the present invention, the colloidal silica contained in the polishing composition is preferably anion-modified colloidal silica (anion-modified colloidal silica), more preferably colloidal silica with organic acid fixed on the surface. Colloidal silica with organic acid fixed on the surface tends to have a larger absolute value of zeta potential in the polishing composition than normal colloidal silica with no organic acid fixed on the surface. Therefore, the zeta potential of colloidal silica in the polishing composition is easily adjusted to a negative value (for example, in the range of -40 mV to -15 mV).
[0021] Preferred examples of colloidal silica having an organic acid fixed to its surface include colloidal silica having an organic acid group, such as a carboxylic acid group, a sulfonic acid group, a phosphonic acid group, or an aluminic acid group, fixed to its surface. Among these, from the viewpoint of ease of production, colloidal silica having a sulfonic acid or a carboxylic acid fixed to its surface is preferred, and colloidal silica having a sulfonic acid fixed to its surface is more preferred.
[0022] The immobilization of an organic acid on the surface of colloidal silica cannot be achieved by simply allowing colloidal silica and an organic acid to coexist. For example, if sulfonic acid, which is a type of organic acid, is to be immobilized on colloidal silica, it can be achieved by the method described in, for example, “Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups”, Chem. Commun. 246-247 (2003). Specifically, a silane coupling agent having a thiol group, such as 3-mercaptopropyltrimethoxysilane, is coupled to colloidal silica, and then the thiol group is oxidized with hydrogen peroxide to obtain colloidal silica with sulfonic acid immobilized on the surface (sulfonic acid-modified colloidal silica, sulfonic acid-modified colloidal silica).
[0023] Alternatively, when a carboxylic acid, which is a type of organic acid, is immobilized on colloidal silica, it can be carried out by, for example, the method described in “Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel”, Chemistry Letters, 3, 228-229 (2000). Specifically, a silane coupling agent containing a photoreactive 2-nitrobenzyl ester is coupled to colloidal silica, followed by light irradiation, to obtain colloidal silica with a carboxylic acid immobilized on the surface (carboxylic acid-modified colloidal silica, carboxylic acid-modified colloidal silica).
[0024] The shape of the abrasive grains is not particularly limited, and may be spherical or non-spherical. Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and square prisms, cylinders, bales in which the center of a cylinder is bulged out more than the ends, donut shapes in which the center of a disk is penetrated, plates, so-called cocoon shapes with a constriction in the center, so-called association-type spheres in which multiple particles are integrated, so-called confetti shapes with multiple protrusions on the surface, and rugby ball shapes, and various other shapes are not particularly limited.
[0025] The size of the abrasive grains is not particularly limited. For example, the average primary particle diameter of the abrasive grains is preferably 5 nm or more, more preferably 8 nm or more, even more preferably 10 nm or more, and particularly preferably 12 nm or more. As the average primary particle diameter of the abrasive grains increases, the polishing speed of the object to be polished by the polishing composition increases. In addition, the average primary particle diameter of the abrasive grains is preferably 100 nm or less, more preferably 50 nm or less, even more preferably 30 nm or less, and particularly preferably 20 nm or less. As the average primary particle diameter of the abrasive grains decreases, it becomes easier to obtain a surface with fewer defects by polishing using the polishing composition. That is, the average primary particle diameter of the abrasive grains is preferably 5 nm or more and 100 nm or less, more preferably 8 nm or more and 50 nm or less, even more preferably 10 nm or more and 30 nm or less, and particularly preferably 12 nm or more and 20 nm or less. The average primary particle diameter of the abrasive grains can be calculated, for example, based on the specific surface area (SA) of the abrasive grains calculated by the BET method, assuming that the shape of the abrasive grains is a true sphere. In this specification, the average primary particle size of the abrasive grains is a value measured by the method described in the Examples.
[0026] In addition, the average secondary particle diameter of the abrasive grains is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm or more, and particularly preferably 25 nm or more. As the average secondary particle diameter of the abrasive grains increases, the resistance during polishing decreases, and stable polishing becomes possible. In addition, the average secondary particle diameter of the abrasive grains is preferably 400 nm or less, more preferably 300 nm or less, even more preferably 200 nm or less, particularly preferably 100 nm or less, and most preferably 50 nm or less. As the average secondary particle diameter of the abrasive grains decreases, the surface area per unit mass of the abrasive grains increases, the frequency of contact with the object to be polished increases, and the polishing speed increases. That is, the average secondary particle diameter of the abrasive grains is preferably 10 nm or more and 400 nm or less, more preferably 15 nm or more and 300 nm or less, even more preferably 20 nm or more and 200 nm or less, particularly preferably 25 nm or more and 100 nm or less, and particularly preferably 25 nm or more and 50 nm or less. The average secondary particle size of the abrasive grains can be measured by, for example, a dynamic light scattering method such as a laser diffraction scattering method.
[0027] The average degree of association of the abrasive grains is preferably 5.0 or less, more preferably 4.0 or less, even more preferably 3.0 or less, and particularly preferably 2.5 or less. As the average degree of association of the abrasive grains decreases, defects can be reduced more. The average degree of association of the abrasive grains is also preferably 1.0 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. This average degree of association is obtained by dividing the value of the average secondary particle diameter of the abrasive grains by the value of the average primary particle diameter. As the average degree of association of the abrasive grains increases, there is an advantageous effect that the polishing speed of the object to be polished by the polishing composition improves.
[0028] The upper limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably less than 2.0, more preferably 1.8 or less, and even more preferably 1.5 or less. In such a range, defects on the surface of the object to be polished can be further reduced. The aspect ratio is the average of the values obtained by taking the smallest rectangle that circumscribes the image of the abrasive grains by a scanning electron microscope, and dividing the length of the long side of the rectangle by the length of the short side of the same rectangle, and can be determined using general image analysis software. The lower limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably 1.0 or more, and more preferably 1.2 or more.
[0029] In the particle size distribution of abrasive grains obtained by laser diffraction scattering method, the lower limit of D90 / D10, which is the ratio of the particle diameter (D90) when the cumulative particle mass from the fine particle side reaches 90% of the total particle mass and the particle diameter (D10) when the cumulative particle mass from the fine particle side reaches 10% of the total particle mass of all particles, is not particularly limited, but is preferably 1.1 or more, more preferably 1.4 or more, even more preferably 1.7 or more, and most preferably 2.0 or more. In addition, in the particle size distribution of abrasive grains in a polishing composition obtained by laser diffraction scattering method, the upper limit of the ratio D90 / D10, which is the particle diameter (D90) when the cumulative particle mass from the fine particle side reaches 90% of the total particle mass and the particle diameter (D10) when the cumulative particle mass from the fine particle side reaches 10% of the total particle mass of all particles, is not particularly limited, but is preferably 3.0 or less, more preferably 2.5 or less. Within such a range, defects on the surface of the object to be polished can be further reduced.
[0030] The size of the abrasive grains (average primary particle size, average secondary particle size, aspect ratio, D90 / D10, etc.) can be appropriately controlled by selecting the manufacturing method of the abrasive grains, etc.
[0031] The concentration (content) of the abrasive grains is not particularly limited, but is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, even more preferably 1% by mass or more, even more preferably more than 1% by mass, and particularly preferably 1.5% by mass or more, based on the total mass of the polishing composition. The upper limit of the concentration (content) of the abrasive grains is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less, based on the total mass of the polishing composition. That is, the concentration (content) of the abrasive grains is preferably 0.5% by mass or more and 20% by mass or less, more preferably 0.8% by mass or more and 20% by mass or less, even more preferably 1% by mass or more and 15% by mass or less, even more preferably more than 1% by mass and 10% by mass or less, and particularly preferably 1.5% by mass or more and 5% by mass or less, based on the total mass of the polishing composition. Within such a range, the polishing rate can be improved while suppressing costs. In addition, when the polishing composition contains two or more kinds of abrasive grains, the concentration (content) of the abrasive grains means the total amount of these.
[0032] [Quaternary phosphonium salts] The polishing composition according to the present invention contains a quaternary phosphonium salt. As described above, the quaternary phosphonium salt has the effect of shifting the zeta potential of the surface of the low-k material to a positive potential, and can improve the polishing rate of the low-k material.
[0033] From the viewpoint of further improving the effect of the present invention, the quaternary phosphonium salt according to the present invention preferably has at least one of a substituted or unsubstituted aryl group bonded to the phosphorus atom and a substituted or unsubstituted alkyl group bonded to the phosphorus atom. Examples of the substituents that the aryl group and the alkyl group may have include halogen atoms, hydroxyl groups, carboxyl groups, cyano groups, nitro groups, amino groups, monoalkylamino groups, dialkylamino groups, trialkylsilyl groups, aliphatic heterocyclic groups, aryl groups, alkyl groups, etc. The alkyl group bonded to the phosphorus atom is not substituted with an alkyl group.
[0034] The aryl group bonded to the phosphorus atom is not particularly limited, and examples thereof include aryl groups having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, an anthracenyl group, a tetracenyl group, a phenanthryl group, a chrysenyl group, a triphenylenyl group, and a biphenyl group.
[0035] The alkyl group bonded to the phosphorus atom is not particularly limited, and examples thereof include linear or branched alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, sec-butyl, n-pentyl, isopentyl, n-hexyl, isohexyl, n-octyl, isooctyl, n-nonyl, isononyl, n-decyl, isodecyl, n-dodecyl, isododecyl, undecyl, lauryl, myristyl, cetyl, stearyl, 2-ethylhexyl, and 4-butyloctyl groups; and cyclic alkyl groups (cycloalkyl groups) having 3 to 20 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl groups.
[0036] More specific examples of the quaternary phosphonium salt include, for example, tetraphenylphosphonium fluoride, tetrabutylphosphonium fluoride, methyltriphenylphosphonium fluoride, ethyltriphenylphosphonium fluoride, propyltriphenylphosphonium fluoride, benzyltriphenylphosphonium fluoride, dodecyltriphenylphosphonium fluoride, hexadecyltri(n-butyl)phosphonium fluoride, and tetradecyltriphenylphosphonium fluoride; Tetra n-butylphosphonium hydroxide, tetraethylphosphonium hydroxide, tetraphenylphosphonium hydroxide, methyltriphenylphosphonium hydroxide, ethyltriphenylphosphonium hydroxide, propyltriphenylphosphonium hydroxide, butyltriphenylphosphonium hydroxide, benzyltriphenylphosphonium hydroxide; Tetra n-butylphosphonium acetate, ethyltriphenylphosphonium acetate, tetramethylphosphonium acetate; Tetrakis(hydroxymethyl)phosphonium sulfate; benzyltriphenylphosphonium chloride, (4-chlorobenzyl)triphenylphosphonium chloride, (2-chlorobenzyl)triphenylphosphonium chloride, triphenyl(2-chlorobenzyl)phosphonium chloride, (chloromethyl)triphenylphosphonium chloride, (2,4-dichlorobenzyl)triphenylphosphonium chloride, (1-naphthylmethyl)triphenylphosphonium chloride, tetra-n-butylphosphonium chloride, tetrakis(hydroxymethyl)phosphonium chloride, tetraphenylphosphonium chloride; amyltriphenylphosphonium bromide, benzyltriphenylphosphonium bromide, (bromomethyl)triphenylphosphonium bromide, 3-bromopropyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, cyclopropyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, heptyltriphenylphosphonium bromide, hexyltriphenylphosphonium bromide, (2-hydroxybenzyl)triphenylphosphonium bromide, methyltriphenylphosphonium bromide, (4-nitrobenzyl)triphenylphosphonium bromide, tetraethylphosphonium bromide, tetra-n-octylphosphonium bromide, tetraphenylphosphonium bromide, tri(n-butyl)dodecylphosphonium bromide, tri(n-butyl)hexadecylphosphonium bromide, tri(n-butyl)n-octylphosphonium bromide, triphenylpropylphosphonium bromide, triphenyl(tetradecyl)phosphonium bromide; Ethyltriphenylphosphonium iodide, isopropyltriphenylphosphonium iodide, methyltriphenylphosphonium iodide, tetraphenylphosphonium iodide, tri(n-butyl)methylphosphonium iodide; Di-tert-butylmethylphosphonium tetraphenylborate, μ-oxo-bis[tris(dimethylamino)phosphonium]bis(tetrafluoroborate), tetra-n-butylphosphonium benzotriazolate, tetraethylphosphonium tetrafluoroborate, tetrakis(hydroxymethyl)phosphonium sulfate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, tributyl(2-methoxyethyl)phosphonium bis(trifluoromethanesulfonyl)imide, tri-tert-butylphosphonium tetrafluoroborate, tri-tert-butylphosphonium tetraphenylborate, tricyclohexylphosphonium tetrafluoroborate, acetonyltriphenylphosphonium chloride, allyltriphenylphosphonium chloride, trans-2-butene-1,4-bis(triphenylphosphonium chloride), (cyanomethyl)triphenylphosphonium chloride, (formylmethyl)triphenylphosphine phosphonium chloride, (methoxymethyl)triphenylphosphonium chloride, tributyl(cyanomethyl)phosphonium chloride, 2-(trimethylsilyl)ethoxymethyltriphenylphosphonium chloride, allyltriphenylphosphonium bromide, (4-carboxybutyl)triphenylphosphonium bromide, (3-carboxypropyl)triphenylphosphonium bromide, cinnamyltriphenylphosphonium bromide, (3,4-dimethoxybenzyl)triphenylphosphonium bromide, 2-dimethylaminoethyltriphenylphosphonium bromide, 2-(1,3-dioxolan-2-yl)ethyltriphenylphosphonium bromide, (1,3-dioxolan-2-yl)methyltriphenylphosphonium bromide, 4-ethoxybenzyltriphenylphosphonium bromide, ethoxycarbonylmethyl(triphenyl)phosphonium bromide, methoxycarbonylmethyl(triphenyl)phosphonium bromide, phenacyltriphenylphosphonium bromide, tributyl(1,3-dioxolan-2-ylmethyl)phosphonium bromide, (3-trimethylsilyl-2-propynyl)triphenylphosphonium bromide, triphenylpropargylphosphonium bromide, triphenylvinylphosphonium bromide, (N-methyl-N-phenylamino)triphenylphosphonium iodide, (2-trimethylsilylethyl)triphenylphosphonium iodide;, These quaternary phosphonium salts can be used alone or in combination of two or more. In addition, the quaternary phosphonium salts may be commercially available products or synthetic products.
[0037] Among these quaternary phosphonium salts, compounds having a substituted or unsubstituted linear or branched alkyl group bonded to the phosphorus atom are preferred. More preferably, the compounds have a tetraalkylphosphonium cation in which all four organic groups bonded to the phosphorus atom are alkyl groups. The alkyl group is more preferably linear. The maximum carbon number of the alkyl group of the tetraalkylphosphonium cation is particularly preferably 2 or more and 10 or less. If the maximum carbon number of the alkyl group is within this range, the adsorption of the quaternary phosphonium salt to the low-k material becomes appropriate, and the effect of shifting the zeta potential of the low-k material surface to positive is efficiently exerted, and the desired effect is more effectively exerted.
[0038] When the maximum number of carbon atoms in the alkyl group of the tetraalkylphosphonium cation is 1, adsorption to the low-k material is unlikely to occur, and it may be difficult to improve the removal rate of the low-k material.
[0039] If the maximum number of carbon atoms in the alkyl group of the tetraalkylphosphonium cation exceeds 10, it will be more likely to be adsorbed onto the surface of silicon nitride, acting as a protective film for silicon nitride, which may decrease the polishing speed of silicon nitride. It may also cause aggregation of abrasive grains.
[0040] From the above viewpoints, the quaternary phosphonium salt used in the present invention is more preferably tetra-n-butylphosphonium fluoride, tetra-n-butylphosphonium hydroxide, tetraethylphosphonium hydroxide, tetra-n-butylphosphonium acetate, tetra-n-butylphosphonium chloride, tetraethylphosphonium bromide, tetra-n-octylphosphonium bromide, tri(n-butyl)n-octylphosphonium bromide, tri(n-butyl)methylphosphonium iodide, tetra-n-butylphosphonium benzotriazolate, tetraethylphosphonium tetrafluoroborate, and even more preferably at least one selected from the group consisting of tetra-n-butylphosphonium hydroxide, tetraethylphosphonium bromide, and tetra-n-octylphosphonium bromide.The quaternary phosphonium salt is particularly preferably at least one of tetra-n-butylphosphonium hydroxide and tetraethylphosphonium bromide.
[0041] The lower limit of the concentration (content) of quaternary phosphonium salt in the polishing composition is preferably 0.001 mass% (10 mass ppm) or more, more preferably 0.005 mass% (50 mass ppm) or more, and even more preferably 0.01 mass% (100 mass ppm) or more.In addition, the upper limit of the concentration (content) of quaternary phosphonium salt in the polishing composition is preferably 1 mass% (10000 mass ppm) or less, more preferably 0.5 mass% (5000 mass ppm) or less, even more preferably 0.3 mass% (3000 mass ppm) or less, and particularly preferably 0.1 mass% (1000 mass ppm) or less. That is, the concentration (content) of the quaternary phosphonium salt in the polishing composition is preferably 0.001% by mass (10 ppm by mass) or more and 1% by mass (10,000 ppm by mass) or less, more preferably 0.005% by mass (50 ppm by mass) or more and 0.5% by mass (5,000 ppm by mass) or less, even more preferably 0.01% by mass (100 ppm by mass) or more and 0.3% by mass (3,000 ppm by mass) or less, and particularly preferably 0.01% by mass (100 ppm by mass) or more and 0.1% by mass (1,000 ppm by mass) or less.
[0042] When the polishing composition contains two or more kinds of quaternary phosphonium salts, the concentration (content) of the quaternary phosphonium salts means the total amount thereof.
[0043] [pH and pH adjusters] The pH of the polishing composition according to the present invention is less than 7.0. If the pH is 7.0 or more, the polishing rate of silicon nitride in particular is low, and the desired effect of the present invention cannot be obtained. The pH is preferably 1.0 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. The pH is preferably 6.0 or less, more preferably 5.0 or less, and even more preferably 4.5 or less. That is, the pH of the polishing composition according to the present invention is preferably 1.0 or more and 6.0 or less, more preferably 1.5 or more and 5.0 or less, and even more preferably 2.0 or more and 4.5 or less.
[0044] The polishing composition of the present invention preferably contains a pH adjuster for adjusting pH.The pH adjuster may be either an acid or a base, and may be either an inorganic compound or an organic compound.The pH adjuster may be used alone or in combination of two or more kinds.
[0045] Specific examples of acids that can be used as a pH adjuster include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid; and organic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid.
[0046] Examples of bases that can be used as pH adjusters include amines such as aliphatic amines and aromatic amines, organic bases such as quaternary ammonium hydroxides, hydroxides of alkali metals such as sodium hydroxide and potassium hydroxide, hydroxides of Group 2 elements, and ammonia.
[0047] The amount of pH adjuster to be added is not particularly limited, and can be appropriately adjusted so that the polishing composition has a desired pH. The pH of the polishing composition can be measured, for example, by a pH meter, and specifically, can be measured by the method described in Examples.
[0048] [Dispersion medium] The polishing composition according to the present invention preferably further contains a dispersion medium. Examples of the dispersion medium include water; alcohols such as methanol, ethanol, and ethylene glycol; ketones such as acetone, and mixtures thereof. Of these, water is preferable as the dispersion medium. That is, according to a more preferred embodiment of the present invention, the dispersion medium contains water. According to a more preferred embodiment of the present invention, the dispersion medium is substantially composed of water. Note that the above "substantially" means that a dispersion medium other than water may be included as long as the objective effect of the present invention can be achieved, and more specifically, the dispersion medium is preferably composed of 90% by mass or more and 100% by mass or less of water and 0% by mass or more and 10% by mass or less of a dispersion medium other than water, and more preferably composed of 99% by mass or more and 100% by mass or less of water and 0% by mass or more and 1% by mass or less of a dispersion medium other than water. Most preferably, the dispersion medium is water.
[0049] From the viewpoint of not inhibiting the action of the components contained in the polishing composition, it is preferable for the dispersion medium to be water that contains as few impurities as possible. Specifically, pure water or ultrapure water from which impurity ions have been removed with an ion exchange resin and then foreign matter has been removed through a filter, or distilled water is more preferable.
[0050] [Electrical Conductivity of Polishing Composition] The electrical conductivity (EC) of the polishing composition according to the present invention is not particularly limited, but is preferably 1 mS / cm or more, more preferably 1.5 mS / cm or more. The electrical conductivity (EC) of the polishing composition according to the present invention is preferably 20 mS / cm or less, more preferably 15 mS / cm or less. That is, the electrical conductivity (EC) of the polishing composition according to the present invention is preferably 1 mS / cm or more and 20 mS / cm or less, more preferably 1.5 mS / cm or more and 15 mS / cm or less. If the electrical conductivity (EC) of the polishing composition is in such a range, the polishing rate of the low-k material and silicon nitride can be maintained high, and the repulsion between the abrasive grains can be appropriately adjusted to ensure stability. The electrical conductivity of the polishing composition can be adjusted by the type and amount of a pH adjuster, etc., and the electrical conductivity can be measured by the method described in the Examples.
[0051] [Other ingredients] The polishing composition of the present invention may further contain known additives that can be used in polishing compositions, such as water-soluble polymers, complexing agents, metal corrosion inhibitors, preservatives, antifungal agents, oxidizing agents, reducing agents, and surfactants, as necessary. Among these, the polishing composition preferably contains an antifungal agent. The polishing composition of the present invention is acidic. For this reason, it is more preferable that the polishing composition contains an antifungal agent. That is, in one embodiment of the present invention, the polishing composition is substantially composed of abrasive grains, a quaternary phosphonium salt, a dispersion medium, and at least one of a pH adjuster and an antifungal agent. Here, "the polishing composition is substantially composed of abrasive grains, a quaternary phosphonium salt, a dispersion medium, and at least one of a pH adjuster and an antifungal agent" means that the total content of the abrasive grains, the quaternary phosphonium salt, the dispersion medium, and at least one of a pH adjuster and an antifungal agent is more than 99% by mass (upper limit: 100% by mass) with respect to the total mass of the polishing composition. Preferably, the polishing composition comprises an abrasive grain, a quaternary phosphonium salt, a dispersion medium, a pH adjuster, and an antifungal agent (the above total content=100% by mass).
[0052] The following describes the antifungal agent (preservative), which is a preferred other component, and the oxidizing agent.
[0053] (Anti-mold agent) Examples of the antifungal agent (preservative) that can be added to the polishing composition of the present invention include isothiazoline-based preservatives such as 2-methyl-4-isothiazolin-3-one and 5-chloro-2-methyl-4-isothiazolin-3-one, paraoxybenzoic acid esters, and phenoxyethanol, etc. These antifungal agents (preservatives) may be used alone or in combination of two or more.
[0054] (Oxidizing agent) The polishing composition according to the present invention preferably does not substantially contain an oxidizing agent. If an oxidizing agent is contained in the polishing composition, the surface of the object to be polished may be oxidized to generate an oxide film, which may result in a longer polishing time. Specific examples of the oxidizing agent include hydrogen peroxide (H2O2), sodium persulfate, ammonium persulfate, and sodium dichloroisocyanurate. The polishing composition substantially does not contain an oxidizing agent means that the oxidizing agent is not intentionally contained at least. Therefore, a polishing composition that inevitably contains a small amount of an oxidizing agent due to raw materials, manufacturing method, etc. is included in the concept of a polishing composition that does not substantially contain an oxidizing agent. For example, the concentration (content) of the oxidizing agent in the polishing composition is preferably 0.01 mass% (100 mass ppm) or less, more preferably less than 0.01 mass% (100 mass ppm), and even more preferably 0.005 mass% (50 mass ppm) or less. The lower limit of the concentration (content) of the oxidizing agent is preferably 0% by mass or more, and more preferably 0.0005% by mass (5 ppm by mass) or more.
[0055] [Form of polishing composition] The polishing composition according to the present invention is typically supplied to an object to be polished in the form of a polishing liquid containing the polishing composition, and is used to polish the object to be polished. The polishing composition according to the present invention may be used as a polishing liquid after dilution (typically diluted with water), or may be used as a polishing liquid as it is. That is, the concept of the polishing composition according to the present invention includes both a polishing composition (working slurry) that is supplied to an object to be polished and used to polish the object to be polished, and a concentrated liquid (original working slurry liquid) that is diluted and used for polishing. The concentration ratio of the concentrated liquid can be, for example, about 2 to 100 times on a volume basis, and is usually about 3 to 50 times.
[0056] [Polished object] The object to be polished according to the present invention is not particularly limited, and examples thereof include single crystal silicon, polycrystalline silicon (polysilicon), polycrystalline silicon doped with n-type or p-type impurities, amorphous silicon, amorphous silicon doped with n-type or p-type impurities, silicon oxide, silicon nitride, silicon carbonitride (SiCN), metals, SiGe, carbon-containing materials, low dielectric constant materials (Low-k materials), and the like.
[0057] Examples of objects to be polished that contain silicon oxide include a TEOS-type silicon oxide film (hereinafter simply referred to as "TEOS" or "TEOS film") produced using tetraethyl orthosilicate as a precursor, a high density plasma (HDP) film, an undoped silicate glass (USG) film, a phosphorus silicate glass (PSG) film, a boron-phosphorus silicate glass (BPSG) film, and a rapid thermal oxidation (RTO) film.
[0058] Examples of metals include tungsten, copper, aluminum, cobalt, hafnium, nickel, gold, silver, platinum, palladium, rhodium, ruthenium, iridium, and osmium.
[0059] Examples of carbon-containing materials include amorphous carbon, spin-on carbon (SOC), diamond-like carbon (DLC), nanocrystalline diamond, graphene, and other materials other than low-k materials.
[0060] A low-dielectric constant material (Low-k material) is a material with a relative dielectric constant k lower than that of silicon oxide, and is preferably a material with a relative dielectric constant k of 3.0 or less. Specific examples include silicon carbide (SiC), carbon-containing silicon oxide (SiOC), silicon oxide containing a methyl group, benzocyclobutene (BCB), fluorinated silicon oxide (SiOF), HSQ (hydrogen silsesquioxane), MSQ (methyl silsesquioxane), HMSQ (hydride-methyl silsesquioxane), polyimide-based polymers, arylene ether-based polymers, cyclobutene-based polymers, and perfluorocyclobutene (PFCB).
[0061] The object to be polished may be a commercially available product or may be produced by a known method.
[0062] Among these, the object to be polished is preferably one that contains a low-k material and silicon nitride. Therefore, according to a preferred embodiment of the present invention, the polishing composition is used to polish an object to be polished that contains a low-k material and silicon nitride. The low-k material is preferably silicon oxide containing carbon (SiOC).
[0063] [Method of manufacturing the polishing composition] The method for producing the polishing composition according to the present embodiment is not particularly limited, and can be obtained by, for example, stirring and mixing abrasive grains, quaternary phosphonium salt, dispersion medium, and other additives added as necessary. The details of each component are as described above.
[0064] The temperature at which the components are mixed is not particularly limited, but is preferably 10° C. to 40° C., and may be heated to increase the dissolution rate. The mixing time is also not particularly limited as long as the components can be mixed uniformly.
[0065] [Polishing method and semiconductor substrate manufacturing method] As described above, the polishing composition according to this embodiment is particularly suitable for polishing an object to be polished that has a low-k material and silicon nitride.Therefore, the present invention provides a polishing method for polishing an object to be polished that includes a low-k material and silicon nitride with the polishing composition according to this embodiment.The present invention also provides a method for producing a semiconductor substrate, which comprises polishing a semiconductor substrate that includes a low-k material and silicon nitride by the above-mentioned polishing method.
[0066] As a polishing device, a general polishing device can be used that is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.
[0067] The polishing pad may be made of any material, including general nonwoven fabric, polyurethane, porous fluororesin, etc. It is preferable that the polishing pad has grooves formed thereon to allow the polishing liquid to accumulate.
[0068] Regarding the polishing conditions, for example, the rotation speed of the polishing table (platen) and carrier (head) was 10 rpm (0.17 s -1 ) or more 500rpm (8.33s -1 The pressure applied to the substrate having the object to be polished (polishing pressure) is preferably 0.5 psi (3.45 kPa) or more and 10 psi (68.9 kPa) or less.
[0069] The method of supplying the polishing composition to the polishing pad is not particularly limited, and for example, a method of continuously supplying the composition using a pump, etc. is adopted. There is no limit to the amount of the composition supplied, but it is preferable that the surface of the polishing pad is always covered with the polishing composition according to the present invention.
[0070] The polishing composition according to the present embodiment may be a one-liquid type or a multi-liquid type such as a two-liquid type. The polishing composition according to the present invention may be prepared by diluting the stock solution of the polishing composition, for example, three times or more, with a diluent such as water.
[0071] [Polishing speed] As described above, the polishing composition of the present invention is capable of polishing low-k materials and silicon nitride at a high polishing rate.
[0072] In the present invention, the polishing speed of the low-k material is preferably 300 Å / min or more, more preferably 400 Å / min or more, and even more preferably 450 Å / min or more, and the polishing speed of silicon nitride is preferably 300 Å / min or more, more preferably 330 Å / min or more, and even more preferably 360 Å / min or more.
[0073] [Selection ratio] As described above, the polishing composition of the present invention can control the ratio (selectivity) of the polishing rate for low-k material to the polishing rate for silicon nitride within an appropriate range.
[0074] In the present invention, the ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride (low-k material / silicon nitride) is preferably 1.0 or more, more preferably 1.1 or more. The ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride (low-k material / silicon nitride) is preferably 2.0 or less, more preferably 1.9 or less, and even more preferably 1.7 or less. That is, the selectivity may be 1.0 or more and 2.0 or less, 1.0 or more and 1.9 or less, or 1.0 or more and 1.7 or less. The selectivity may be 1.1 or more and 2.0 or less, 1.1 or more and 1.9 or less, or 1.1 or more and 1.7 or less. If the selectivity is out of the above range, the surface condition of the polished object finally obtained may be poor.
[0075] Although the embodiments of the present invention have been described in detail, it is apparent that the same are illustrative and exemplary, not restrictive, and the scope of the present invention should be interpreted by the appended claims.
[0076] The present invention encompasses the following aspects and configurations. 1. A polishing composition comprising an abrasive grain and a quaternary phosphonium salt, the pH of which is less than 7.0, and the zeta potential of the abrasive grain in the polishing composition is -10 mV or less; 2. The polishing composition according to 1 above, wherein the quaternary phosphonium salt has at least one of a substituted or unsubstituted aryl group bonded to the phosphorus atom and a substituted or unsubstituted alkyl group bonded to the phosphorus atom; 3. The polishing composition according to 1. or 2. above, wherein the quaternary phosphonium salt has a substituted or unsubstituted alkyl group bonded to the phosphorus atom; 4. The polishing composition according to any one of 1. to 3. above, wherein the quaternary phosphonium salt has a tetraalkylphosphonium cation, and the maximum number of carbon atoms in the alkyl group of the tetraalkylphosphonium cation is 2 or more and 10 or less; 5. The polishing composition according to any one of 1. to 4. above, wherein the quaternary phosphonium salt is at least one of tetra-n-butylphosphonium hydroxide and tetraethylphosphonium bromide; 6. The polishing composition according to any one of 1. to 5. above, wherein the abrasive grains are anion-modified colloidal silica; 7. The polishing composition according to any one of 1. to 6. above, further comprising a pH adjuster; 8. The polishing composition according to any one of 1. to 7. above, further comprising a dispersion medium; 9. The polishing composition according to any one of 1. to 8. above, wherein the concentration of the oxidizing agent in the polishing composition is less than 100 ppm by mass; 10. The polishing composition according to any one of 1. to 9. above, wherein the abrasive grains in the polishing composition have a zeta potential of -40 mV or more and -15 mV or less; 11. The polishing composition according to any one of 1. to 10. above, which is used for polishing an object to be polished, including a low-k material and silicon nitride; 12. The polishing composition according to claim 11, wherein the low-k material is SiOC; 13. The polishing composition according to 11 or 12 above, wherein the ratio of the polishing rate of the low-k material to the polishing rate of the silicon nitride (low-k material / silicon nitride) is 1.0 or more and 2.0 or less; 14. A polishing method, comprising a step of polishing an object containing a low-k material and silicon nitride with the polishing composition according to any one of 1. to 13. above; 15. A method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing a low-k material and silicon nitride by the polishing method described in 14 above. EXAMPLES
[0077] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively. In the following examples, unless otherwise specified, the operations were performed under the conditions of room temperature (20°C to 25°C) / relative humidity 40% RH to 50% RH. Each physical property was measured as follows.
[0078] <Average secondary particle size of abrasive grains> The average secondary particle diameter of the abrasive grains was measured as the volume average particle diameter (arithmetic mean diameter based on volume; Mv) using a dynamic light scattering particle size / particle size distribution analyzer UPA-UT151 (manufactured by Nikkiso Co., Ltd.).
[0079] <Zeta potential of abrasive grains> The zeta potential of the abrasive grains in the polishing composition was measured using a zeta potential measuring device manufactured by Otsuka Electronics Co., Ltd. (device name "ELS-Z2").
[0080] <pH of polishing composition> The pH of the polishing composition was measured with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA).
[0081] <Electrical Conductivity of Polishing Composition> The electrical conductivity (EC) of the polishing composition was measured with a tabletop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71 LAQUA (registered trademark)).
[0082] <Sulfonic acid immobilized colloidal silica> [Production Example 1] Sulfonic acid-modified silica particles (surface-modified silica 1) were obtained as abrasive grains according to the following procedure.
[0083] (Preparation process of raw colloidal silica dispersion (unmodified silica particles)) In a flask, 4080g of methanol, 610g of water, and 168g of 29% by mass aqueous ammonia solution were mixed, the liquid temperature was kept at 20°C, and a mixed liquid of 135g of methanol and 508g of tetramethoxysilane (TMOS) was added dropwise over a period of 25 minutes. After that, thermally concentrated water replacement was performed under conditions of pH 7 or higher, and 1000g of 19.5% by mass silica sol was obtained (average secondary particle size: 34nm).
[0084] (Surface modification process) Next, 1.2 g (silane coupling agent concentration relative to the total mass of silica solids: 0.6 mass%) of 3-mercaptopropyltrimethoxysilane (MPS, silane coupling agent, product name: KBM-803, Shin-Etsu Chemical Co., Ltd.) mixed with 4.8 g of methanol was dropped at a flow rate of 1 mL / min to 1000 g of the silica sol obtained above (195 g in terms of silica solids). After that, it was heated and boiled, and then replaced with pure water for 3 hours.
[0085] Next, the reaction solution was left to stand overnight to cool, and 0.0343 g of 30% by mass hydrogen peroxide solution (3 moles per mole of silane coupling agent) was added and boiled again. After that, the mixture was replaced with pure water for 2 hours, and then cooled to room temperature (25°C) to obtain sulfonic acid-modified colloidal silica (surface-modified silica 1).
[0086] [Production Example 2] A sulfonic acid-modified colloidal silica (surface-modified silica 2) was obtained in the same manner as in the above Production Example 1, except that in the section (Surface modification step) of the above Production Example 1, the amount of 3-mercaptopropyltrimethoxysilane (MPS) added as a silane coupling agent was changed to 0.12 g (silane coupling agent concentration relative to the total mass of silica solids: 0.06 mass%).
[0087] Example 1 <Preparation of Polishing Composition> Abrasive grains, sulfonic acid modified colloidal silica (surface modified silica 1, average secondary particle diameter: 34 nm), were added to water as a dispersion medium so that the final concentration was 2 mass%. Furthermore, tetra-n-octylphosphonium bromide (Tokyo Chemical Industry Co., Ltd.) was added to a final concentration of 200 mass ppm, and the mixture was stirred and mixed (stirring temperature: 25°C, stirring time: 20 minutes). The pH of the polishing composition was adjusted to 2.5 using nitric acid, and the polishing composition was completed.
[0088] Example 2 A polishing composition was prepared in the same manner as in Example 1, except that tetra-n-butylphosphonium hydroxide (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of tetra-n-octylphosphonium bromide.
[0089] Example 3 A polishing composition was prepared in the same manner as in Example 1, except that tetraethylphosphonium bromide (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of tetra-n-octylphosphonium bromide.
[0090] Comparative Example 1 A polishing composition was prepared in the same manner as in Example 1, except that no quaternary phosphonium salt was used.
[0091] Comparative Example 2 A polishing composition was prepared in the same manner as in Example 1, except that 1-hydroxyethane-1,1-diphosphonic acid (HEDP, etidronic acid, manufactured by Italmatch Japan Co., Ltd.) was used instead of tetra-n-octylphosphonium bromide.
[0092] Comparative Example 3 A polishing composition was prepared in the same manner as in Example 2, except that no abrasive grains were used.
[0093] Comparative Example 4 A polishing composition was prepared in the same manner as in Example 2, except that the sulfonic acid-modified colloidal silica (surface-modified silica 2, average secondary particle diameter: 34 nm) obtained in Production Example 2 was used as the abrasive grains.
[0094] [evaluation] The objects to be polished (substrates) were a 300 mm wafer (SiOC film, manufactured by Advanced Materials Technology Corp., product name: BD2x 5kA Blanket) and a 300 mm wafer (Si3N4 (silicon nitride film), manufactured by Advanced Materials Technology Corp., product name: LP-SiN 3.5KA Blanket), each of which was cut into 60 mm x 60 mm chip coupons to be used as test pieces.
[0095] Using the polishing composition obtained above, the prepared substrate was polished under the following polishing conditions, and the removal rate was measured: (polishing conditions) Polishing machine: EJ-380IN-CH (Engis Japan Co., Ltd.) Polishing pad: Hard polyurethane pad (Nitta DuPont, IC1010) Polishing pressure: 2.0psi (1psi=6894.76Pa) Platen rotation speed: 60 rpm Head (carrier) rotation speed: 60 rpm Flow rate of polishing composition: 100ml / min Polishing time: 30 seconds.
[0096] (polishing speed) The film thickness was measured using an optical interference film thickness measuring device (SCREEN Holdings Co., Ltd., model number: Lambda Ace VM-2030), and the polishing rate was evaluated by dividing the difference in film thickness before and after polishing by the polishing time (see the formula below). The polishing rate for both SiOC film and Si3N4 film is preferably 300 Å / min or more.
[0097]
number
[0098] (Selectivity) The selectivity was determined by dividing the polishing speed of the SiOC film obtained above by the polishing speed of the Si3N4 film (silicon nitride film). The selectivity is preferably 1.0 or more and 2.0 or less.
[0099] The composition and evaluation results of the polishing compositions of the Examples and Comparative Examples are shown in the following Table 1. In addition, "-" in Table 1 indicates that the agent was not used.
[0100] [Table 1]
[0101] As is clear from Table 1 above, when the polishing composition of the embodiment is used, the polishing speed of the low-k materials, SiOC and silicon nitride, is both 300 Å / min or more, and it is found that a high polishing speed can be obtained. In addition, the ratio (selectivity) of the polishing speed of SiOC to the polishing speed of silicon nitride is 1.0 or more and 2.0 or less, and it is found that an appropriate selectivity can be obtained. On the other hand, when the polishing composition of the comparative example is used, the polishing speed of SiOC is low, and the selectivity is reduced, especially in the cases of Comparative Examples 1 and 2.
[0102] The results shown in Table 1 were obtained by polishing an object having a low-k material (SiOC) and an object having silicon nitride separately. However, it is expected that the polishing speed and selectivity similar to those shown in Table 1 will be obtained even when an object having both a low-k material and silicon nitride is polished.
Claims
1. Abrasive grains and A quaternary phosphonium salt; and having a pH of less than 7.0; The polishing composition, wherein the abrasive grains in the polishing composition have a zeta potential of -10 mV or less.
2. The polishing composition according to claim 1 , wherein the quaternary phosphonium salt has at least one of a substituted or unsubstituted aryl group bonded to the phosphorus atom and a substituted or unsubstituted alkyl group bonded to the phosphorus atom.
3. The polishing composition of claim 1 , wherein the quaternary phosphonium salt has a substituted or unsubstituted alkyl group bonded to the phosphorus atom.
4. 2. The polishing composition according to claim 1, wherein the quaternary phosphonium salt has a tetraalkylphosphonium cation, and the maximum number of carbon atoms in an alkyl group of the tetraalkylphosphonium cation is 2 or more and 10 or less.
5. 5. The polishing composition according to claim 4, wherein the quaternary phosphonium salt is at least one of tetra-n-butylphosphonium hydroxide and tetraethylphosphonium bromide.
6. The polishing composition according to claim 1 , wherein the abrasive grains are anion-modified colloidal silica.
7. The polishing composition of claim 1 , further comprising a pH adjuster.
8. The polishing composition according to claim 1 , further comprising a dispersion medium.
9. The polishing composition according to claim 1 , wherein the concentration of the oxidizing agent in the polishing composition is less than 100 ppm by mass.
10. 2. The polishing composition according to claim 1, wherein the abrasive grains in the polishing composition have a zeta potential of −40 mV or more and −15 mV or less.
11. 2. The polishing composition according to claim 1, which is used in polishing an object containing a low-k material and silicon nitride.
12. The polishing composition according to claim 11, wherein the low-k material is SiOC.
13. 12. The polishing composition according to claim 11, wherein the ratio of the polishing rate of the low-k material to the polishing rate of the silicon nitride (low-k material / silicon nitride) is 1.0 or more and 2.0 or less.
14. 14. A polishing method comprising the step of polishing an object containing a low-k material and silicon nitride with the polishing composition according to claim 1.
15. A method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing a low-k material and silicon nitride by the polishing method according to claim 14.
Citation Information
Patent Citations
Polishing liquid, polishing liquid set, and substrate polishing method
JP2017139349A