Method for producing polymer

The polycondensation of polymers with ketene acetal structural units under controlled pressure conditions addresses the challenges of recycling polyolefin polymers, producing high molecular weight copolymers with improved heat resistance and mechanical strength.

JP2024132971APending Publication Date: 2024-10-01MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024037023
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2024-03-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing polyolefin polymers, such as polyethylene, are difficult to decompose and recycle, requiring high energy and generating environmental burdens, and those with structural units derived from ketene acetal lack sufficient molecular weight and heat resistance, necessitating costly high-pressure polymerization equipment.

Method used

A method involving polycondensation of polymers containing specific structural units derived from ketene acetal under controlled pressure conditions, followed by hydrolysis and further polycondensation, to produce polymers with enhanced molecular weight and heat resistance.

Benefits of technology

The method enables the production of polyolefin copolymers with high molecular weight, excellent heat resistance, and mechanical strength, facilitating efficient recycling of waste polyolefin materials without significant environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132971000001
    Figure 2024132971000001
  • Figure 2024132971000002
    Figure 2024132971000002
  • Figure 2024132971000003
    Figure 2024132971000003
Patent Text Reader

Abstract

To provide a method for producing a polymer by reusing polyolefin polymers such as polyethylene and the like contained in waste and the like, the polymer having excellent heat resistance and superior mechanical strength due to high molecular weight.SOLUTION: A method for producing a polymer comprises a polycondensation step (X) to obtain a polymer (B) comprising a structural unit derived from a polymer (A) by polycondensation of the polymer (A) comprising a structural unit (1) represented by the following general formula (1). (In the formula, l and m are integers which satisfy 0.001≤l / (l+m)≤0.2; n is an integer of 1-3; Z is an arbitrary repeating unit; R1 and R1 are each a hydrogen atom, a C1-10 alkyl group which may have a branch, a C3-10 cycloalkyl group which may have a substituent, a C6-10 aryl group which may have a substituent, or a C7-10 aralkyl group which may have a substituent, where at least one of n R1's and n R1's is a group other than the hydrogen atom.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a process for producing a polymer. [Background technology]

[0002] Polyolefin polymers such as polyethylene are polymers that have excellent weather resistance, chemical resistance, and mechanical properties, and many products containing polyolefin polymers are used in our daily lives. In particular, polyethylene polymers are used as packaging materials for food, electronic components, and various daily necessities due to their stability and light weight, enriching our daily lives.

[0003] However, due to its stability, polyethylene polymers are hardly decomposed even if they are physically reduced to the smallest possible size. Therefore, if polyethylene polymers are disposed of in landfills, they will remain in the ground semi-permanently. Furthermore, if polyethylene polymers are dumped, they may become marine litter and have a negative impact on marine life.

[0004] Therefore, in order to reuse polyolefin polymers such as polyethylene contained in waste materials, a chemical recycling method is used in which raw material monomers obtained by decomposing the polyolefin polymers are reused. However, many polyolefin polymers require a huge amount of energy to decompose into the original raw material monomers due to their large molecular weight. Therefore, among chemical recycling methods, a thermal recycling method is used, but this method is not preferable from the viewpoint of global environmental conservation because it inevitably generates carbon dioxide and has a large environmental load.

[0005] In view of this, polyolefin-based polymers that can be easily chemically recycled without placing a burden on the environment have been proposed. For example, Patent Documents 1 to 5 and Non-Patent Documents 1 and 2 disclose polyolefin-based polymers that contain structural units derived from ketene acetal in the main chain. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 04-081450 [Patent Document 2] Japanese Patent Application Publication No. 58-015508 [Patent Document 3] Japanese Patent Application Publication No. 04-081450 [Patent Document 4] Special Publication No. 06-504086 [Patent Document 5] U.S. Patent No. 5,281,681 [Non-patent literature]

[0007] [Non-Patent Document 1] iScience.,Volume23,Issue3,27 / March / 2020,100904 [Non-Patent Document 2] J.Environ.Polym.Degrad.,Volume6,p23-29(1998) Summary of the Invention [Problem to be solved by the invention]

[0008] However, the polyolefin polymers containing a structural unit derived from a ketene acetal in the main chain disclosed in Patent Documents 1 to 5 and Non-Patent Documents 1 and 2 are insufficient in molecular weight or heat resistance. Furthermore, in the method for producing a polyolefin polymer disclosed in Patent Document 5, a polymerization reaction is carried out under ultra-high pressure, which requires special and large production equipment, posing a problem in terms of production costs. Furthermore, Patent Documents 1 to 5 and Non-Patent Documents 1 and 2 make no mention of decomposing a polyolefin polymer containing a structural unit derived from a ketene acetal in its main chain by chemical recycling to obtain a raw material monomer or an oligomer derived from the polymer, and then reusing the obtained raw material monomer or the oligomer derived from the polymer to obtain a new polyolefin polymer, in particular to obtain a polymer having a higher molecular weight or higher heat resistance than the polyolefin polymer before being chemically recycled.

[0009] Furthermore, even if a previously known polymer having structural units derived from an olefin (referred to as a "polymer having an olefin unit") is decomposed by chemical recycling to obtain a raw material monomer or an oligomer derived from the polymer, and then the obtained raw material monomer or the oligomer derived from the polymer is reused to obtain a new polymer having olefin units, there has been a problem that the degree of polymerization of the polymer is low, i.e., the molecular weight is small, and sufficient mechanical properties and heat resistance cannot be obtained.

[0010] The present invention has been made in consideration of the above-mentioned problems of the conventional technology, and an object of the present invention is to provide a method for producing a polymer having excellent heat resistance and excellent mechanical strength due to its high molecular weight, by reusing a polyolefin polymer such as polyethylene contained in waste or the like. [Means for solving the problem]

[0011] Means of the Invention The present inventors have conducted extensive research to solve the above problems and have found that the above problems can be solved by polycondensing a polymer containing a specific structural unit, such as a structural unit derived from a ketene acetal. The present invention has been achieved based on these findings, and has the following gist.

[0012] [1] A method for producing a polymer, comprising: a polycondensation step (X) of polycondensing a polymer (A) containing a structural unit (1) represented by the following general formula (1) to obtain a polymer (B) containing a structural unit derived from the polymer (A): [ka] (In the above formula (1), l and m represent integers satisfying 0.001≦l / (l+m)≦0.2, and n represents an integer of 1 to 3. Z represents any repeating unit. 1 and R 2 each represents a hydrogen atom, an optionally branched alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms which may have a substituent, an aryl group having 6 to 10 carbon atoms which may have a substituent, or an aralkyl group having 7 to 10 carbon atoms which may have a substituent. Also, R 1 and R 2 At least one of may contain at least one heteroatom selected from the group consisting of oxygen atoms, sulfur atoms, and nitrogen atoms. n is 2 or 3, and multiple R 1 and R 2 If there are multiple R 1 may be the same or different, and the R 2 may be the same or different.)

[0013] [2] The method for producing a polymer according to [1], wherein the polycondensation reaction in the polycondensation step (X) is carried out under a pressure of 0.1 mm or more and 1 mmHg or less. [3] The method for producing a polymer according to [1] or [2], wherein the polycondensation step (X) includes a hydrolysis step (X-1) of hydrolyzing the polymer (A) to obtain a hydrolysis product derived from the polymer (A), and a polycondensation step (X-2) of polycondensing the obtained hydrolysis product to obtain the polymer (B). [4] The method for producing a polymer according to [3], comprising a hydrolysis step (X-1-1) in which the hydrolysis step (X-1) comprises hydrolyzing the polymer (A) in the presence of a basic catalyst in an alcohol-based solvent at a temperature in the range of 130°C or higher and 200°C or lower to obtain an oligomer and / or monomer derived from the polymer (A). [5] The method for producing a polymer according to [4], wherein the oligomer and / or monomer obtained in the hydrolysis step (X-1-1) is polycondensed in the polycondensation step (X-2) in the presence of a metal catalyst within a temperature range of 170°C or higher and 250°C or lower.

[0014] [6] In the above formula (1), l represents an integer from 1 to 15, and m represents an integer from 85 to 99. The method for producing a polymer according to any one of [1] to [5]. [7] The method for producing a polymer according to any one of [1] to [6], wherein the structural unit (1) contains a structural unit derived from a cyclic ketene acetal. [8] The method for producing a polymer according to [7], wherein the cyclic ketene acetal is represented by the following general formula (2). [Chemical formula] (In the above formula (2), n, R 1 , R 2 are respectively synonymous with n, R 1 , R 2 in the above formula (1).) [9] The method for producing a polymer according to any one of [1] to [8], wherein Z is a structural unit derived from a radically polymerizable monomer.

[10] The method for producing a polymer according to [9], wherein the radically polymerizable monomer contains at least one selected from the group consisting of ethylene and olefins having 3 to 12 carbon atoms.

[11] The method for producing a polymer according to any one of [1] to

[10] , wherein the weight average molecular weight Mwa of the polymer (A) and the weight average molecular weight Mwb of the polymer (B) satisfy the relationship Mwa < Mwb.

[12] The method for producing a polymer according to any one of [1] to

[11] , wherein the weight average molecular weight of the polymer (B) is 5000 or more and 1000000 or less.

[13] The method for producing a polymer according to any one of [1] to

[12] , wherein the weight average molecular weight Mwb of the polymer (B) is 3 times or more and 50 times or less the weight average molecular weight Mwa of the polymer (A).

[0015]

[14] The method for producing a polymer according to any one of [1] to

[13] , wherein in the above formula (1), Z has a repeating unit having at least one alkyl group having 1 to 20 carbon atoms which may have a branch, and at least one cycloalkyl group having 3 to 20 carbon atoms which may have a substituent, in a side chain.

[15] In the above formula (1), l represents an integer of 1 to 15, and m represents an integer of 85 to 99, The structural unit (1) contains a structural unit derived from a compound represented by general formula (2), The method for producing a polymer according to any one of [1] to

[14] , wherein the Z is a structural unit derived from a radically polymerizable monomer. [ka] (In the above formula (2), n and R 1 , R 2 respectively represent n and R in the formula (1). 1 , R 2 is equivalent to

[16] In the above formula (1), l represents an integer of 1 to 15, and m represents an integer of 85 to 99, The structural unit (1) contains a structural unit derived from 2-methylene-1,3-dioxepane, Z is a structural unit derived from a radical polymerizable monomer, The method for producing a polymer according to any one of [1] to

[15] , wherein the radical polymerizable monomer comprises at least one selected from the group consisting of ethylene and olefins having 3 to 12 carbon atoms.

[0016]

[17] The method for producing a polymer according to any one of [1] to

[16] , wherein the polymer (B) is a polymer containing a structural unit (3) represented by general formula (3). [ka] (In the above formula (3), l, m, n, Z, R 1 and R 2 respectively represent l, m, n, Z, and R in the formula (1). 1 and R 2is equivalent to Effect of the Invention

[0017] According to the method for producing a polymer of the present invention, a polymer having excellent heat resistance and excellent mechanical strength due to its high molecular weight can be produced by polycondensation of a polymer containing a specific structural unit such as ketene acetal. Therefore, according to the method for producing a polymer of the present invention, a polyolefin-based copolymer containing a structural unit derived from ketene acetal, which is contained in waste or the like, can be reused to obtain a polyolefin-based copolymer which has excellent heat resistance and, due to its high molecular weight, excellent mechanical strength. More specifically, the polyolefin-based copolymer contained in waste or the like is hydrolyzed to obtain oligomers and / or monomers derived from the polyolefin-based copolymer, and the obtained oligomers and / or monomers can then be used to obtain a polyolefin-based copolymer that is again excellent in heat resistance and has a high molecular weight and therefore excellent in mechanical strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not limited to the following description, and can be modified and implemented as desired without departing from the gist of the present invention.

[0019] In this specification, the term "structural unit" refers to a unit derived from a raw material compound used in the production of a polymer, formed by polymerization of the raw material compound, and refers to a partial structure sandwiched between any linking groups in the resulting polymer. It also includes a partial structure at the end of the polymer, one of which is a linking group and the other of which is a polymerization reactive group. The structural unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by treating the resulting polymer. In this specification, the terms "repeating unit" and "structural unit" have the same meaning. In the following, a "structural unit derived from a raw material compound" may be simply referred to as a "raw material compound unit." For example, a "cyclic ketene acetal unit" means a "structural unit derived from a cyclic ketene acetal and introduced into a polymer." In addition, in this specification, "(co)polymer" means either or both of a polymer and a copolymer.

[0020] In this specification, unless otherwise specified, a numerical range expressed with "~" means a range that includes the numerical values ​​before and after "~" as the lower and upper limits, and "A~B" means A or more and B or less.

[0021] In this specification, "including A or B" means "including A," "including B," or "including A and B," unless otherwise specified.

[0022] In this specification, "% by mass" indicates the content of a given component in a total amount of 100% by mass. In this specification, "% by mass" and "% by weight", "ppm by mass" and "ppm by weight", and "parts by mass" and "parts by weight" are synonymous. In addition, when simply written as "ppm", it means "ppm by weight".

[0023] "Optional" or "optionally" means that the subsequently described circumstance may or may not occur, and so the description includes instances when the circumstance occurs and instances when it does not occur.

[0024] As used herein, the term "about" can mean above and below 20% of the stated value. For example, about 75°C encompasses the range of 60°C to 90°C. All steps described herein can be performed in any suitable order unless otherwise indicated herein or clearly contradicted by context.

[0025] <Method of Producing Polymer> The method for producing a polymer of the present invention includes a polycondensation step (X) of polycondensing a polymer (A) containing a structural unit (1) represented by the following general formula (1) to obtain a polymer (B) containing a structural unit derived from the polymer (A).

[0026] [ka]

[0027] In the above formula (1), l and m represent integers satisfying 0.001≦l / (l+m)≦0.2; The aforementioned l is preferably an integer of 1 to 15 from the viewpoint of excellent yield when obtaining polymer (B) by polycondensation of polymer (A), that is, excellent reusability. The above m is preferably an integer of 85 to 99 from the viewpoint of excellent yield when the polymer (B) is obtained by polycondensing the polymer (A), that is, excellent reusability. Z represents an arbitrary repeating unit. Details of "Z" and "arbitrary repeating unit" will be described later. R 1 and R 2 each represents a hydrogen atom, an optionally branched alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms which may have a substituent, an aryl group having 6 to 10 carbon atoms which may have a substituent, or an aralkyl group having 7 to 10 carbon atoms which may have a substituent. Also, R 1 and R 2 At least one of may contain at least one heteroatom selected from the group consisting of oxygen atoms, sulfur atoms, and nitrogen atoms. n is 2 or 3, and multiple R 1 and R 2 If there are multiple R 1 may be the same or different, and the R 2 may be the same or different from each other.

[0028] In the general formula (1), m structural units represented by Z and l other structural units (referred to as structural units L) are usually randomly polymerized. In particular, it is preferable that m structural units Z are not consecutively bonded to the structural units L randomly. That is, the polymer (A) in the present invention is -(Z) m1 -L-(Z) m2 In this case, it is preferable that Σmx, which is the sum of m1 and m2, is m in general formula (1). Hereinafter, the same applies to the polymer (B).

[0029] (Polycondensation step (X)) The polycondensation step (X) in the production method of the present invention is a step of polycondensing the polymer (A) to obtain the polymer (B). The embodiment of the polycondensation step (X) is not particularly limited, and examples thereof include a method in which the polymer (A) is directly polycondensed using a known polycondensation method to obtain a polymer with a higher molecular weight, or a method in which the polymer (A) is first decomposed into monomers and / or oligomers derived from the polymer (A) using a known polymer decomposition method such as a hydrolysis method, and then the obtained monomers and / or oligomers are polycondensed using a known polycondensation method or a known ring-opening polymerization method to obtain a polymer. The polycondensation step (X) may be either batch polymerization or continuous polymerization, and either a transesterification reaction or a direct polymerization reaction may be used.

[0030] Examples of the metal catalyst (transesterification catalyst) used in the transesterification reaction include alkoxides and acetates of at least one metal selected from Mg, Mn, Zn, Ca, Li, Sn, and Ti, and dialkyl oxides of Sn. Examples of the polycondensation catalyst include compounds such as alkoxides and acetates of at least one metal selected from Sb, Ti, Ge, Sn, and Al, dialkyl oxides of Sn, and organic sulfonic acid compounds. When a product containing the polymer (B) obtained by the production method of the present invention may come into direct contact with food, it is preferable that the product does not contain an Sb compound or an organic sulfonic acid compound. Therefore, it is preferable to perform polycondensation using a Ti or Ge compound as the polycondensation catalyst. Since the polymer (B) after polycondensation contains monomers, oligomers, and various by-products, it is preferable to perform solid-phase polymerization at a temperature of 170°C or higher under reduced pressure or in a flowing inert gas.

[0031] As one embodiment of the polycondensation step (X), there is a method of subjecting the polymer (A) or a hydrolysis product of the polymer (A) to a polycondensation reaction in the presence of a catalyst within a temperature range of 170 to 250°C to obtain a polymer (B) having a higher weight average molecular weight Mwb.

[0032] In the polycondensation step (X), it is preferable that the weight average molecular weight Mwa of the polymer (A) and the weight average molecular weight Mwb of the polymer (B) satisfy the relationship Mwa < Mwb from the viewpoint that the mechanical strength and heat resistance of the obtained polymer (B) are better. From the viewpoint that the mechanical strength and heat resistance of the obtained polymer (B) are better, the weight average molecular weight Mwb of the polymer (B) is preferably 3 times or more, more preferably 4 times or more, with respect to the weight average molecular weight Mwa of the polymer (A), and preferably 50 times or less, more preferably 40 times or less. More specifically, it is preferably 3 times or more and 50 times or less, and more preferably 4 times or more and 40 times or less.

[0033] The method for controlling the weight average molecular weight Mwa and the weight average molecular weight Mwb such that Mwa < Mwb is not particularly limited. For example, the structure of the structural unit (1) in the polymer (A), the content ratio of the structural unit (1), further, the structure and type of the cyclic ketene acetal unit contained in the structural unit (1) and the content ratio of the cyclic ketene acetal unit can be controlled by those skilled in the art by appropriately selecting and adjusting them. Alternatively, the method for controlling such that Mwa < Mwb is the conditions of the polycondensation reaction in the polycondensation step (X), and the hydrolysis reaction of the hydrolysis step (X-1) which may be included in the polycondensation step (X) and the polycondensation reaction conditions of the polycondensation step (X-2) described later, and the hydrolysis step (X-1-1) described later included in the hydrolysis step (X-1), and further, the conditions of the purification step (X-1-2) described later provided as necessary, and it may be a method controlled by those skilled in the art by appropriately selecting and adjusting them.

[0034] In the present invention, in particular, it is preferable to perform the polycondensation step (X) (particularly, the polycondensation step (X-2) after hydrolysis) under high vacuum. By performing the polycondensation step (X) under high vacuum, the polymer (A) can be made to have a higher molecular weight without using equipment for applying high pressure. Conventionally, in order to increase the molecular weight of the polymer, high pressure has been applied. However, when applying high pressure, there are also problems with manufacturing equipment and the like. Under such circumstances, in the present invention, by deliberately advancing the polycondensation reaction under high vacuum, the polymer has been successfully made to have a higher molecular weight. The pressure in the polycondensation step (X) (particularly, the polycondensation step (X-2) after hydrolysis) is preferably 1 mmHg or less, more preferably 0.8 mmHg or less, and even more preferably 0.5 mmHg or less. The pressure in the polycondensation step (X) means the final pressure. Also, the lower limit of the pressure in the polycondensation step (X) is not particularly defined, but 0.1 mmHg or more is practical. Therefore, the pressure in the polycondensation step (X) (particularly the polycondensation step (X-2) after hydrolysis) is preferably 0.1 mm or more and 1 mmHg or less, more preferably 0.1 mm or more and 0.8 mmHg or less, and even more preferably 0.1 mm or more and 0.5 mmHg or less.

[0035] An example of the polycondensation step (X) of the present invention will be described below. It goes without saying that the polycondensation step (X) of the present invention is not limited to the one described below. The following scheme (1) shows an embodiment in which the polycondensation step (X) includes a hydrolysis step (X-1) of hydrolyzing a polymer (A) to obtain a hydrolysis product derived from the polymer (A), and a polycondensation step (X-2) of polycondensing the obtained hydrolysis product to obtain the polymer (B). By hydrolyzing the polymer (A), a hydrolyzate of the polymer (A) is obtained. The hydrolyzate of the polymer (A) in scheme (1) is obtained by decomposing a part of the ester bonds of the polymer (A), and it is presumed that the hydrolyzate may be an oligomer molecule having an OH group at one end and a COOH group at the other end, a decomposition product having an OH group at one end and not a COOH group at the other end, or a decomposition product having a COOH group at one end and not an OH group at the other end. Of these, the low molecular weight components are easily dissolved in water, and therefore are presumed to be removed before moving to the subsequent polycondensation step (X-2). In scheme (1), the polycondensation step (X-2) is carried out in the presence of the hydrolyzate. At this time, it is presumed that by carrying out the polycondensation step (X-2) under high vacuum, the remaining decomposition products having one end as an OH group and the other as a COOH group, or the remaining decomposition products having one end as a COOH group and the other as a OH group, are distilled off under reduced pressure. As a result, it is presumed that oligomer molecules having a relatively high molecular weight and one end as an OH group and the other as a COOH group are preferentially left as raw materials for the polycondensation reaction (X-2). As a result, it is presumed that the molecular weight of the resulting polymer (B) can be increased. [ka]

[0036] In the above scheme (1), R x are each independently a hydrogen atom, -OH, or -COOH. An example of the compound obtained in the above hydrolysis step (X-1) is presumed to be the following compound. [ka]

[0037] Furthermore, as shown in scheme (2), polymer (B) may be obtained from polymer (A) without going through a hydrolysis step. The following scheme (2) shows a scheme for obtaining a polymer (B) by polycondensing a polymer (A). In scheme (2), the polymer (A) also contains a low molecular weight polymer component to begin with. Therefore, even if the polycondensation reaction is performed without passing through the hydrolysis step of the polymer (A), it is presumed that the low molecular weight polymer will be distilled off under reduced pressure by performing the polycondensation step (X) under high vacuum. As a result, it is presumed that the molecular weight of the obtained polymer (B) can be increased. [ka]

[0038] The production method of the polymer (B) of the present invention will be described in more detail below. In the polycondensation step (X), the method for polycondensing the polymer (A) is not particularly limited. For example, a method in which the temperature is raised under normal pressure and an inert gas to carry out a first-stage initial polymerization of the polymer (A), and then the pressure is reduced to carry out a second-stage polymerization to obtain a high molecular weight polymer (B) can be mentioned. Furthermore, after the first and second polymerization reactions, a polymer (B) having a higher molecular weight can be obtained by further carrying out solid-phase polymerization or the like.

[0039] The conditions for the first stage initial polymerization are not particularly limited, but it is preferable to raise the temperature from room temperature at a rate of 0.5 to 10° C. / min, and when the temperature reaches 170 to 250° C., keep the temperature constant and continue the reaction for another 30 minutes to 24 hours. The conditions for the second stage polymerization, which is further carried out under reduced pressure, are not particularly limited, but it is preferable to maintain the temperature raised in the initial polymerization and carry out the polymerization under pressure conditions of 10 mmHg or less, preferably 3 mmHg or less.

[0040] The timing of adding the transesterification catalyst and the polycondensation catalyst is not particularly limited. They may be added together with the polymer (A) or may be added under reduced pressure after the completion of the initial polymerization. When the polymer (A) is a solution, it is preferable to add them after the completion of concentration under reduced pressure.

[0041] Furthermore, the polycondensation step (X) preferably includes a hydrolysis step (X-1) described later for hydrolyzing the polymer (A) to obtain a hydrolysis product derived from the polymer (A), and a polycondensation step (X-2) described later for polycondensing the obtained hydrolysis product to obtain the polymer (B). Unless otherwise specified, the various conditions in the polycondensation step (X-2) are the same for the polycondensation step (X) without the hydrolysis step (X-1).

[0042] (Hydrolysis process (X-1)) The hydrolysis step (X-1) in the production method of the present invention is a step for hydrolyzing the polymer (A) in the polycondensation step (X) to obtain a hydrolysis product derived from the polymer (A).

[0043] In the hydrolysis step (X-1), the structural unit (1) introduced into the main chain of the polymer (A) is hydrolyzed by a known hydrolysis method, whereby the polymer (A) can be decomposed into hydrolysis products derived from the polymer (A). The hydrolysis product obtained after hydrolysis here refers to an oligomer and / or monomer derived from the raw material of the polymer (A). Specifically, it refers to an oligomer and / or monomer containing one or more units of the structural unit (1), cyclic ketene acetal unit, and radically polymerizable monomer unit contained in the polymer (A). In addition, a (co)polymer formed from the oligomer and / or monomer generated by hydrolysis is also called a hydrolysis product.

[0044] Further, from the viewpoint of obtaining a polymer (B) having a higher molecular weight, the hydrolysis step (X-1) preferably includes a hydrolysis step (X-1-1) including hydrolyzing the polymer (A) in the presence of a basic catalyst in an alcohol solvent at a temperature in the range of 130° C. or higher and 200° C. or lower to obtain an oligomer and / or monomer derived from the polymer (A).

[0045] The basic catalyst is not particularly limited, and may be any known basic catalyst used in a typical hydrolysis reaction, such as potassium hydroxide, sodium hydroxide, lithium hydroxide, etc. The basic catalyst may be used alone or in combination of two or more kinds.

[0046] The alcohol solvent is not particularly limited, and may be any known alcohol such as methanol, ethanol, isopropyl alcohol, etc., particularly a lower alcohol having a carbon number of 1 to 3. The alcohol solvent may be used alone or in combination of two or more kinds.

[0047] The lower limit of the amount of the basic catalyst used in the hydrolysis step (X-1), particularly in the hydrolysis step (X-1-1), is not particularly limited, and is usually preferably 0.8 equivalents or more, more preferably 1.0 equivalents or more, relative to the polymer (A). On the other hand, the upper limit of the amount of the basic catalyst used is not particularly limited, and is usually preferably 20 equivalents or less, particularly preferably 10 equivalents or less. If the amount of the basic catalyst used is the above lower limit or more, hydrolysis can be performed at a sufficient hydrolysis rate. If the amount of the basic catalyst used is the above upper limit or less, post-treatment is easy and economical. The lower limit of the amount of the alcohol-based solvent used in the hydrolysis step (X-1), particularly in the hydrolysis step (X-1-1), is not particularly limited, and is usually preferably 500 parts by mass or more, more preferably 600 parts by mass or more, per 100 parts by mass of the total mass of the polymer (A). On the other hand, the upper limit of the amount of the alcohol-based solvent used is not particularly limited, and is usually preferably 4000 parts by mass or less, more preferably 3000 parts by mass or less, per 100 parts by mass of the total mass of the polymer (A). If the amount of the alcohol-based solvent used is the lower limit or more, hydrolysis proceeds sufficiently, and if it is the upper limit or less, hydrolysis can be efficiently performed.

[0048] The basic catalyst is usually used as an aqueous solution of about 1 to 6N. Therefore, water is present together with the alcohol-based solvent in the reaction system of the hydrolysis step (X-1), particularly the hydrolysis step (X-1-1). The upper limit of the amount of water present is not particularly limited, and is usually preferably 1000 parts by mass or less, more preferably 700 parts by mass or less, relative to 100 parts by mass of the total mass of the polymer (A). On the other hand, the lower limit of the amount of water present is not particularly limited, and is usually preferably 100 parts by mass or more, more preferably 200 parts by mass or more, relative to 100 parts by mass of the total mass of the polymer (A). If the amount of water present is equal to or more than the lower limit, hydrolysis proceeds sufficiently, and if it is equal to or less than the upper limit, hydrolysis can be efficiently performed.

[0049] The hydrolysis step (X-1), particularly the hydrolysis step (X-1-1), is preferably carried out under an inert gas atmosphere such as nitrogen since the steps are carried out at high temperatures.

[0050] Furthermore, from the viewpoint of obtaining a polymer (B) having a higher molecular weight, it is preferred that the oligomer and / or monomer derived from the polymer (A) obtained in the hydrolysis step (X-1), particularly the hydrolysis step (X-1-1), is polycondensed in the polycondensation step (X-2) in the presence of a metal catalyst at a temperature in the range of 170° C. or more and 250° C. or less.

[0051] Furthermore, the production method of the present invention may, as necessary, from the viewpoint of obtaining a polymer (B) with a higher molecular weight, comprise a purification step (X-1-2) after performing the hydrolysis step (X-1-1) and before performing the polycondensation step (X-2), in which the oligomer and / or monomer derived from the polymer (A) obtained in the hydrolysis step (X-1-1) is purified in the presence of a basic compound at a temperature within a range of 60°C or more and 120°C or less to obtain a purified product of the oligomer and / or monomer derived from the polymer (A). By carrying out the purification step (X-1-2), it is possible to remove catalyst residue components and components that inhibit polycondensation contained in the oligomer and / or monomer derived from the polymer (A) obtained in the hydrolysis step (X-1-1), and therefore it is possible to obtain a polymer (B) with a higher molecular weight in the subsequent polycondensation step (X-2).

[0052] The hydrolysis step (X-1), particularly the hydrolysis step (X-1-1) and the purification step (X-1-2) which is provided as needed, can be carried out in the presence of a solvent, while the polycondensation step (X-2) can be carried out using a solid-phase polymerization method.

[0053] The purification temperature in the purification step (X-1-2) is preferably within the range of 60° C. or higher and 120° C. or lower, from the viewpoint of obtaining a polymer (B) with a higher molecular weight. The basic compound used in the purification step (X-1-2) is not particularly limited, and may be any known basic compound used in a typical hydrolysis reaction, such as potassium hydroxide, sodium hydroxide, lithium hydroxide, etc. These may be used alone or in combination of two or more. The solvent used in the purification step (X-1-2) is not particularly limited, and may be one or more of known solvents, such as methanol, ethanol, isopropyl alcohol, aromatic hydrocarbon compounds such as toluene and xylene, and polar solvents such as methyl isobutyl ketone.

[0054] The basic compound, the amount of solvent used, the amount of water present, and the reaction atmosphere in the purification step (X-1-2) may be the same as those in the hydrolysis step (X-1-1).

[0055] The purification step (X-1-2) may be carried out in the same reaction vessel subsequent to the hydrolysis step (X-1-1), or may be carried out by transferring the hydrolysis product after the hydrolysis step (X-1-1) to a separate reaction vessel.

[0056] Even in the case where the hydrolysis step (X-1) is not performed, it is preferable to produce the polymer (A), purify it, and then carry out the polycondensation reaction.

[0057] The reaction time of the hydrolysis step (X-1) may be any time that allows oligomers and / or monomers having the desired molecular weight to be obtained from the polymer (A), and varies depending on the type of polymer (A), the reaction temperature, and other reaction conditions, but is usually about 1 to 20 hours. When the hydrolysis step (X-1) is carried out only by the hydrolysis step (X-1-1), the above reaction time is preferably the reaction time of the hydrolysis step (X-1-1) (about 1 to 20 hours). Furthermore, when the hydrolysis step (X-1) includes the hydrolysis step (X-1-1) and, if necessary, the purification step (X-1-2), it is preferable that the total reaction time of these steps is the above-mentioned reaction time (about 1 to 20 hours).

[0058] After completion of the hydrolysis step (X-1), the temperature is lowered, and then the pH is adjusted to 1 to 4 using an acid such as hydrochloric acid to facilitate post-treatment. The precipitated oligomer and / or monomer of the polymer (A) is subjected to solid-liquid separation, washed with a polar solvent such as acetone as necessary, and then dried to recover the powdery oligomer and / or monomer of the polymer (A). The molecular weight of the oligomer and / or monomer is not particularly limited, and the conditions for hydrolysis, etc. may be appropriately adjusted according to known techniques to control the molecular weight so that the mechanical strength of the finally obtained polymer (B) satisfies the desired performance. However, the hydrolysis product obtained in the hydrolysis step (X-1) can also be directly subjected to the subsequent polycondensation step (X-2) without separating and recovering the oligomers and / or monomers of the polymer (A).

[0059] (Polycondensation step (X-2)) The polycondensation step (X-2) in the production method of the present invention is a step for obtaining the polymer (B) by polycondensing the oligomer and / or monomer of the polymer (A), which is the hydrolysis product obtained in the hydrolysis step (X-1).

[0060] The embodiment of the polycondensation step (X-2) is not particularly limited, and examples thereof include known polycondensation methods and ring-opening polymerization methods. Either batch polymerization or continuous polymerization may be used, and either a transesterification reaction or a direct polymerization reaction may be used.

[0061] As one embodiment of the polycondensation step (X-2), a method in which the hydrolysis product of the polymer (A) obtained in the hydrolysis step (X-1) is subjected to a polycondensation reaction in the presence of a catalyst at a temperature in the range of 170 to 250°C to obtain a polymer (B) having a higher molecular weight can be mentioned.

[0062] Among the catalysts used in the polycondensation step (X-2), the transesterification catalyst used in the transesterification reaction includes an alkoxide of at least one metal selected from Mg, Mn, Zn, Ca, Li, Sn, and Ti, an acetate, and a dialkyl oxide of Sn, with an alkoxide of at least one metal selected from Mg, Mn, Zn, Ca, Li, and Ti being preferred, and an alkoxide of Ti being more preferred.

[0063] In addition, examples of the polycondensation catalyst include compounds such as alkoxides and acetates of at least one metal selected from Sb, Ti, Ge, Sn, and Al, organic sulfonic acid compounds, and dialkyl oxides of Sn. Alkoxides of at least one metal selected from Mg, Mn, Zn, Ca, Li, and Ti are preferred, and alkoxides of Ti are more preferred. When a product containing the polymer (B) obtained by the production method of the present invention may come into direct contact with food, it is preferable that the product does not contain an Sb compound or an organic sulfonic acid compound, and therefore it is preferable to carry out polycondensation using a Ti or Ge compound as a polycondensation catalyst.

[0064] The lower limit of the amount of the polycondensation catalyst used in the polycondensation step (X-2) is not particularly limited, and is preferably 100 ppm by mass or more, more preferably 300 ppm by mass or more, based on 100 parts by mass of the total mass of the oligomer and / or monomer of the polymer (A), which is usually a hydrolysis product. On the other hand, the upper limit of the amount of the polycondensation catalyst used is not particularly limited, and is preferably 5000 ppm by mass or less, more preferably 3000 ppm by mass or less, based on 100 parts by mass of the total mass of the oligomer and / or monomer of the polymer (A), which is usually a hydrolysis product. If the amount of the polycondensation catalyst used is the above lower limit or more, the polycondensation reaction can be carried out at a sufficient reaction rate. If the amount of the polycondensation catalyst used is the above upper limit or less, coloration is suppressed and the cost efficiency is also excellent.

[0065] In addition, when the oligomer and / or monomer of the polymer (A) is obtained in a solid state as a hydrolysis product from the hydrolysis step (X-1), it is preferable to carry out a polycondensation reaction of the oligomer and / or monomer by using a solid-phase polymerization method. Alternatively, the polycondensation reaction can be carried out in a liquid phase by adding a solvent to the oligomer and / or monomer obtained in a solid state. When performing polycondensation reaction in liquid phase, any solvent used in general polycondensation reaction can be suitably used as the polycondensation reaction solvent, specifically, known organic solvents such as butanol and toluene can be used. These solvents may be used alone or in combination of two or more. In addition, it is preferable to use a small amount of these solvents.

[0066] In the polycondensation step (X-2), the method for polycondensing the hydrolysis product is not particularly limited. For example, a method in which the temperature is raised under normal pressure and in an inert gas to carry out a first-stage initial polymerization of the hydrolysis product, and then the pressure is reduced to carry out a second-stage polymerization to obtain a high molecular weight polymer (B) can be mentioned. Furthermore, after the first and second polymerization reactions, a polymer (B) having a higher molecular weight can be obtained by further carrying out solid-phase polymerization or the like.

[0067] Conditions for the first stage initial polymerization are not particularly limited, but it is desirable to raise the temperature from room temperature at a rate of 0.5 to 10° C. / min, and when the temperature reaches 170 to 250° C., keep the temperature constant and continue the reaction for another 30 minutes to 24 hours. Conditions for the second stage polymerization, which is further carried out under reduced pressure, are not particularly limited, but it is desirable to polymerize for 1 to 24 hours at a pressure of 10 mmHg or less, preferably 3 mmHg or less, while maintaining the temperature raised in the initial polymerization or at a temperature 5 to 20° C. higher than that. Since the polymerized polymer (B) obtained by the polycondensation reaction contains monomers, oligomers, and various by-products, it is also a preferred embodiment to further carry out solid-phase polymerization at a temperature of 170°C or higher, specifically, 170 to 230°C, under reduced pressure or in an inert gas flow after the second-stage polymerization.

[0068] The timing of adding the ester exchange catalyst and the polycondensation catalyst is not particularly limited, and they may be charged together with the hydrolysis product or may be added during the reduced pressure state after the completion of the initial polymerization. When the hydrolysis product is a solution, it is preferable to add them after the completion of concentration under reduced pressure.

[0069] After the polycondensation reaction is completed, an aromatic hydrocarbon solvent such as toluene or xylene is added to the resulting polycondensation reaction product and refluxed. The polycondensation reaction product after reflux is then added to a polar solvent such as acetone or methanol to precipitate, and the precipitate is collected by filtration to obtain the polymer (B).

[0070] In the polycondensation step (X-2), it is preferable that the weight average molecular weight Mwa and the weight average molecular weight Mwb satisfy the relationship Mwa < Mwb from the viewpoint that the mechanical strength and heat resistance of the obtained polymer (B) are better. The method for controlling the weight average molecular weight Mwa and the weight average molecular weight Mwb so as to satisfy the relationship Mwa < Mwb is not particularly limited. For example, the structure of the structural unit (1) in the polymer (A), the content ratio of the structural unit (1), further, the structure and type of the cyclic ketene acetal unit contained in the structural unit (1) and the content ratio of the cyclic ketene acetal unit can be controlled by those skilled in the art appropriately selecting and adjusting. Alternatively, the method for controlling so as to satisfy the relationship Mwa < Mwb may be a method in which those skilled in the art appropriately select and adjust the conditions of the hydrolysis reaction in the hydrolysis step (X-1) and the polycondensation reaction in the polycondensation step (X-2), and the treatment conditions of the hydrolysis step (X-1-1) and the purification step (X-1-2) provided as necessary included in the hydrolysis step (X-1).

[0071] Regarding the matters described in the above (polycondensation step (X-2)), in the case where the hydrolysis step (X-1) is not obtained, the polycondensation step (X) can be carried out in the same manner, and the same range is preferable.

[0072] <Polymer (A)> In the method for producing the polymer of the present invention, the polymer (A) is a polymer containing a structural unit (1) represented by the following general formula (1).

[0073]

Chemical formula

[0074] In the above formula (1), l and m represent integers satisfying 0.001≦l / (l+m)≦0.2; The aforementioned 1 is preferably an integer of 1 to 15, and more preferably an integer of 1 to 10, from the viewpoint of excellent yield when obtaining polymer (B) by polycondensing polymer (A), ie, excellent reusability. The above m is preferably an integer of 85 to 99, and more preferably an integer of 90 to 99, from the viewpoint of excellent yield when obtaining polymer (B) by polycondensing polymer (A), ie, excellent reusability. Z represents any repeating unit.

[0075] R 1 and R 2 each represents a hydrogen atom, an optionally branched alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms which may have a substituent, an aryl group having 6 to 10 carbon atoms which may have a substituent, or an aralkyl group having 7 to 10 carbon atoms which may have a substituent, and is preferably an optionally branched alkyl group having 1 to 10 carbon atoms. Also, R 1 and R 2At least one of R may contain at least one heteroatom selected from the group consisting of oxygen, sulfur, and nitrogen atoms. 1 and R 2 It is preferred that does not contain any heteroatoms. Also, n R 1 and R 2 At least one of these is preferably a hydrogen atom, and more preferably all of them are hydrogen atoms. n is 2 or 3, and multiple R 1 and R 2 If there are multiple R 1 may be the same or different, and the R 2 may be the same or different from each other.

[0076] R 1 and R 2 The alkyl group is preferably an alkyl group having 1 to 5 carbon atoms which may be branched. R 1 and R 2 The cycloalkyl group is preferably a cycloalkyl group having 3 to 5 carbon atoms which may have a substituent.

[0077] R 1 and R 2 Examples of the substituent that the cycloalkyl group, aryl group and aralkyl group may have include an alkyl group having 1 to 4 carbon atoms and an alkoxy group having 1 to 4 carbon atoms.

[0078] R 1 and R 2 Examples of the alkyl group having 1 to 10 carbon atoms which may have a branch include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, an n-hexyl group, and a 2-ethylhexyl group.

[0079] R 1 and R 2Examples of the cycloalkyl group having 3 to 10 carbon atoms (if the cycloalkyl group has a substituent, the number of carbon atoms of the substituent is not included in this carbon number) which may have a substituent include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group.

[0080] R 1 and R 2 Examples of the aryl group having 6 to 10 carbon atoms (if the aryl group has a substituent, the number of carbon atoms of the substituent is not included in this carbon number) which may have a substituent include a phenyl group, an o-methylphenyl group, an m-methylphenyl group, a p-methylphenyl group, a p-tert-butylphenyl group, and a p-methoxyphenyl group.

[0081] R 1 and R 2 Examples of the aralkyl group having 7 to 10 carbon atoms (if the aralkyl group has a substituent, the number of carbon atoms of the substituent is not included in this carbon number) which may have a substituent include a benzyl group, a phenylethyl group, and the like.

[0082] R other than hydrogen atom 1 and R 2 From the viewpoint of the balance between heat resistance and ductility of the resulting copolymer of polymer (B), preferred are methyl, tert-butyl, cyclohexyl and phenyl groups, with methyl being more preferred.

[0083] Among the structural units (1) represented by the above formula (1), the structural unit (1) in which n=2 is one preferred embodiment. Among the structural units (1) represented by the above formula (1), R 1 and R 2 Among these, the structural unit (1) is preferably a structural unit having 3 or less groups other than hydrogen atoms (however, when n=1, the number of groups is 2 or less), and R 1 and R 2 are preferably all hydrogen atoms. In the general formula (1), n ​​is preferably 2, and R 1 and R 2 is preferably a hydrogen atom.

[0084] In the polymer (A) of the present invention, the structural unit (1) preferably contains a structural unit derived from a cyclic ketene acetal (hereinafter referred to as a “cyclic ketene acetal unit”) from the viewpoint of excellent yield when the polymer (A) is polycondensed to obtain the polymer (B), i.e., excellent reusability.

[0085] Furthermore, it is preferable that the cyclic ketene acetal is represented by the following general formula (2) from the viewpoint of improving the yield when the polymer (A) is polycondensed to obtain the polymer (B), that is, the reusability.

[0086] [ka]

[0087] (In the above formula (2), n and R 1 , R 2 respectively represent n and R in the above formula (1). 1 , R 2 is equivalent to

[0088] The cyclic ketene acetal represented by the general formula (2) is not particularly limited, and examples thereof include 2-methylene-1,3-dioxane, 2-methylene-1,3-dioxepane, 2-methylene-1,3-dioxocane, 5-methyl-2-methylene-1,3-dioxane, 5-methyl-2-methylene-1,3-dioxepane, 6-methyl-2-methylene-1,3-dioxocane, 5,6-dimethyl-2-methylene-1,3-dioxepane, 5-tert-butyl-2-methylene-1,3-dioxane, 5-tert-butyl-2-methylene-1,3-dioxepane, 6-tert-butyl-2-methylene-1,3-dioxocane, 5-cyclohexyl-2-methylene-1,3-dioxane, 5-cyclohexyl 6-cyclohexyl-2-methylene-1,3-dioxane, 2-methylene-5-phenyl-1,3-dioxane, 2-methylene-5-phenyl-1,3-dioxane, 2-methylene-6-phenyl-1,3-dioxane, 5,5-dimethyl-2-methylene-1,3-dioxane, 5-ethyl-5-methyl- Examples of the dioxane include 2-methylene-1,3-dioxane, 5-ethyl-2-methylene-1,3-dioxane, 5,5-dimethyl-2-methylene-1,3-dioxepane, 5-ethyl-5-methyl-2-methylene-1,3-dioxepane, 5,6-dimethyl-2-methylene-1,3-dioxocane, and 2-methylene-5,6,7-trimethyl-1,3-dioxocane.

[0089] Among these, from the viewpoint of excellent yield when polymer (B) is obtained by polycondensing polymer (A), i.e., excellent reusability, 2-methylene-1,3-dioxepane, 5-methyl-2-methylene-1,3-dioxepane, 5,6-dimethyl-2-methylene-1,3-dioxepane, 5-tert-butyl-2-methylene-1,3-dioxepane, 5-cyclohexyl-2-methylene-1,3-dioxepane, 2-methylene-5-phenyl-1,3-dioxepane, 5,5-dimethyl-2-methylene-1,3-dioxepane, and 5-ethyl-5-methyl-2-methylene-1,3-dioxepane are preferred, and 2-methylene-1,3-dioxepane (n=2 in formula (2)) is more preferred. These cyclic ketene acetals may be used alone or in combination of two or more.

[0090] Furthermore, in the polymer (A) of the present invention, Z represents any repeating unit. Examples of the any repeating unit include repeating units derived from non-crosslinking monomers. The non-crosslinking monomer is a monomer having one carbon-carbon double bond in one molecule, and is a monomer having no carbon-carbon double bond or reactive functional group in the side chain when copolymerized. Specific examples of the non-crosslinking monomer include olefins, and among them, α-olefins are preferred. Furthermore, in the polymer (A) of the present invention, it is preferable that Z is a structural unit derived from a radically polymerizable monomer (hereinafter referred to as a "radically polymerizable monomer unit"), from the viewpoints of excellent yield when the polymer (A) is polycondensed to obtain the polymer (B), i.e., excellent reusability, and further, excellent mechanical strength and heat resistance of the obtained polymer (B).

[0091] The radical polymerizable monomer is not particularly limited, and examples thereof include vinyl aromatic hydrocarbons such as styrene, α-methylstyrene, p-methylstyrene, and m-methylstyrene; vinyl alicyclic hydrocarbons such as vinylcyclohexane, vinylcyclopentane, vinylcyclohexene, vinylcycloheptane, vinylcycloheptane, and vinylnorbornane; ethylenically unsaturated carboxylic acids such as maleic anhydride, maleic acid, and itaconic acid; olefins having 2 to 12 carbon atoms such as ethylene, propylene, 1-butene, isobutylene, 1-pentene, 1-hexene, 1-octene, 1-decene, and 1-dodecene; conjugated dienes such as butadiene, isoprene, and myrcene; acrylamide, methacrylamide, acrylonitrile, methacrylonitrile, vinyl acetate, vinyl ketone, and vinyl chloride. acrylate, vinylidene chloride, vinylidene fluoride; (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, pentadecyl (meth)acrylate, and dodecyl (meth)acrylate; (meth)acrylic acid derivatives such as 2-hydroxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, glycidyl (meth)acrylate, allyl (meth)acrylate, and benzyl (meth)acrylate;2-vinylfuran, 2-isopropenylfuran, 2-vinylbenzofuran, 2-isopropenylbenzofuran, 2-vinyldibenzofuran, 2-vinylthiophene, 2-isopropenylthiophene, 2-vinyldibenzothiophene, 2-vinylpyrrole, N-vinylindole, N-vinylcarbazole, 2-vinyloxazole, 2-isopropenyloxazole, 2-vinylbenzoxazole, 3-vinylisoxazole, 3-isopropenylisoxazole, 2-vinylthiazole, 2-vinylimidazole, 4(5)-vinylimidazole, N-vinylimidazole, N-vinylimidazoline, 2-vinylbenzimidazole, 5(6)-vinylbenzimidazole, 5-isopropenylpyrazole, 2-isopropenyl1, Ethylenically unsaturated heterocyclic compounds such as 3,4-oxadiazole, vinyltetrazole, 2-vinylpyridine, 4-vinylpyridine, 2-isopropenylpyridine, 3-vinylpyridine, 3-isopropenylpyridine, 2-vinylquinoline, 2-isopropenylquinoline, 4-vinylquinoline, 4-vinylpyrimidine, 2,4-dimethyl-6-vinyl-S-triazine, 3-methylidenedihydrofuran-2(3H)-one, 4-methyl-3-methylidenedihydrofuran-2(3H)-one, and 4-decyl-3-methylidenedihydrofuran-2(3H)-one; ethylenically unsaturated group-containing phosphoric acid esters such as dimethyl methacryloyloxymethyl phosphate and 2-methacryloyloxy-1-methylethyl phosphate;

[0092] In the above general formula (1), Z preferably has a repeating unit having at least one alkyl group having 1 to 20 carbon atoms which may have a branch and at least one cycloalkyl group having 3 to 20 carbon atoms which may have a substituent on the side chain, and more preferably has a repeating unit having at least one alkyl group having 1 to 20 carbon atoms which may have a branch on the side chain. By having such a repeating unit with a branched structure, a polymer (B) having better transparency and strength tends to be obtained. Here, the side chain means, for example, a group bonded to a carbon atom in the main chain of a polymer consisting of a carbon-carbon double bond contained in a radical polymerizable monomer. Specific examples of Z include repeating units having a branched structure in a low density polyethylene structure called LDPE and a linear low density polyethylene structure called LLDPE.

[0093] Among these radical polymerizable monomers, from the viewpoints of excellent yield, i.e., reusability, when polymer (A) is polycondensed to obtain polymer (B), and further, better mechanical strength and heat resistance of the obtained polymer (B), at least one selected from ethylene, olefins having 3 to 12 carbon atoms, (meth)acrylic acid alkyl esters, vinyl norbornene, vinyl acetate, vinyl ketone, vinyl chloride, vinylidene chloride, and vinylidene fluoride is preferred, ethylene and olefins having 3 to 12 carbon atoms are more preferred, ethylene or α-olefins having 3 to 6 carbon atoms are particularly preferred, and ethylene is most preferred. These monomers may be used alone or in combination of two or more.

[0094] In the polymer (A) of the present invention, the lower limit of the content of the structural unit (1) is not particularly limited, and from the viewpoint of the yield when the polymer (A) is polycondensed to obtain the polymer (B), i.e., excellent reusability, it is preferably 60.0 mol% or more, more preferably 70.0 mol% or more, even more preferably 80.0 mol% or more, and particularly preferably 90.0 mol% or more, based on 100% of the total moles of the structural units of the polymer (A). On the other hand, the upper limit of the content of the structural unit (1) is not particularly limited, and from the viewpoint of the mechanical strength and heat resistance of the obtained polymer (B), it may be 100 mol% based on 100% of the total moles of the structural units of the polymer (A), or it may be preferably less than 100 mol%, more preferably 99.5 mol% or less, even more preferably 99.0 mol% or less, particularly preferably 98.0 mol% or less, and most preferably 95.0 mol% or less. The upper and lower limits can be combined arbitrarily. For example, the content of the structural unit (1) in the polymer (A) in the present invention may be 100 mol% relative to the total mole number of the structural units of the polymer (A), or it can be preferably 60.0 mol% or more and less than 100 mol%, more preferably 70.0 mol% or more and 99.5 mol% or less, even more preferably 80.0 mol% or more and 99.0 mol% or less, particularly preferably 90.0 mol% or more and 98.0 mol% or less, and most preferably 90.0 mol% or more and 95.0 mol% or less.

[0095] In the polymer (A) of the present invention, the lower limit of the content ratio (l) of the cyclic ketene acetal unit in the structural unit (1) is not particularly limited, and from the viewpoint of excellent yield when the polymer (A) is polycondensed to obtain the polymer (B), i.e., excellent reusability, the content is preferably 0.1 mol % or more, more preferably 0.5 mol % or more, still more preferably 0.8 mol % or more, still more preferably 0.9 mol % or more, still more preferably 1.0 mol % or more, and still more preferably 2.0 mol % or more, relative to the total number of moles of the structural units of the structural unit (1) (100%). On the other hand, the upper limit of the content of the cyclic ketene acetal is not particularly limited, and from the viewpoint of the mechanical strength and heat resistance of the obtained polymer (B), it is preferably 20.0 mol % or less, more preferably 17.0 mol % or less, even more preferably 15.0 mol % or less, still more preferably 13.0 mol % or less, still more preferably 10.0 mol % or less, even more preferably 9.0 mol % or less, particularly more preferably 8.5 mol % or less, and most preferably 8.0 mol % or less, relative to the total number of moles of the structural units of the structural unit (1) (100%). The upper and lower limits can be combined in any combination. For example, the content of the cyclic ketene acetal in the polymer (A) in the present invention is preferably 0.1 mol% to 20.0 mol%, more preferably 0.5 mol% to 18.0 mol%, even more preferably 0.8 mol% to 17.0 mol%, still more preferably 0.9 mol% to 16.0 mol%, and even more preferably 1.0 mol% to 15.0 mol%, based on the total moles of the structural units of the structural unit (1) (100%). As another example, the content of the cyclic ketene acetal in the polymer (A) of the present invention is more preferably 0.5 mol % or more and 10.0 mol % or less, still more preferably 0.8 mol % or more and 9.0 mol % or less, particularly preferably 0.9 mol % or more and 8.5 mol % or less, and most preferably 1.0 mol % or more and 8.0 mol % or less, relative to the total number of moles of the structural units of the structural unit (1) (100%).

[0096] In the polymer (A) of the present invention, the lower limit of the content ratio (m) of the repeating unit represented by Z in the structural unit (1) is not particularly limited, and from the viewpoint of mechanical strength and heat resistance of the obtained polymer (B), it is preferably 80.0 mol% or more, more preferably 85.0 mol% or more, more preferably 90.0 mol% or more, even more preferably 91.0 mol% or more, even more preferably 91.5 mol% or more, and most preferably 92.0 mol% or more, based on 100% of the total number of moles of the structural units of the structural unit (1). On the other hand, the upper limit of the content ratio of the repeating unit represented by Z is not particularly limited, and from the viewpoint of the yield when the polymer (A) is polycondensed to obtain the polymer (B), that is, excellent reusability, it is preferably 99.9 mol% or less, more preferably 99.5 mol% or less, even more preferably 99.2 mol% or less, particularly preferably 99.1 mol% or less, and most preferably 99.0 mol% or less, based on 100% of the total number of moles of the structural units of the structural unit (1). The upper and lower limits can be combined arbitrarily. For example, the content ratio of the radical polymerizable monomer unit in the polymer (A) in the present invention is preferably 80.0 mol% or more and 99.9 mol% or less, more preferably 85.0 mol% or more and 99.9 mol% or less, even more preferably 90.0 mol% or more and 99.5 mol% or less, even more preferably 91.0 mol% or more and 99.2 mol% or less, even more preferably 91.5 mol% or more and 99.1 mol% or less, and most preferably 92.0 mol% or more and 99.0 mol% or less, based on the total mole number of the structural unit of the structural unit (1) being 100%.

[0097] Furthermore, in the polymer (A) of the present invention, the lower limit of l / (l+m) is preferably 0.001 or more, more preferably 0.005 or more, even more preferably 0.08 or more, particularly preferably 0.09 or more, and most preferably 0.01 or more, from the viewpoint of the yield when the polymer (A) is polycondensed to obtain the polymer (B), i.e., excellent reusability. On the other hand, the upper limit of l / (l+m) is not particularly limited, and is preferably 0.200 or less, more preferably 0.100 or less, even more preferably 0.090 or less, particularly preferably 0.085 or less, and most preferably 0.080 or less, from the viewpoint of the mechanical strength and heat resistance of the obtained polymer (B). The upper and lower limits can be combined arbitrarily. For example, in the polymer (A) of the present invention, the molar ratio (l / (l+m)) of the cyclic ketene acetal unit / the radical polymerizable monomer unit is preferably 0.001 to 0.200, more preferably 0.100 to 0.100, even more preferably 0.08 to 0.090, particularly preferably 0.09 to 0.085, and most preferably 0.01 to 0.080.

[0098] In the polymer (A) of the present invention, the structural units derived from a cyclic ketene acetal (preferably a compound represented by formula (2)) and the structural units derived from a radically polymerizable monomer (preferably ethylene) preferably account for 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, still more preferably 95 mass% or more, even more preferably 97 mass% or more, and may be 100 mass% or less, based on 100 mass% of the polymer (A).

[0099] The lower limit of the weight average molecular weight (Mw) of the polymer (A) in the present invention is preferably 2,000 or more, more preferably 2,500 or more, and even more preferably 3,000 or more, from the viewpoint of the mechanical strength and heat resistance of the obtained polymer (B). On the other hand, the upper limit of the weight average molecular weight (Mw) is preferably 500,000 or less, more preferably 300,000 or less, even more preferably 20,000 or less, particularly preferably 100,000 or less, and most preferably 60,000 or less, from the viewpoint of the yield when the polymer (A) is polycondensed to obtain the polymer (B), i.e., excellent reusability. The above upper and lower limits can be combined in any combination. For example, the weight average molecular weight (Mw) of the polymer (A) in the present invention is preferably 2,000 to 500,000, more preferably 2,500 to 300,000, even more preferably 3,000 to 200,000, particularly preferably 3,000 to 100,000, and most preferably 3,000 to 60,000.

[0100] In addition, if the molecular weight distribution (weight average molecular weight / number average molecular weight: Mw / Mn) of the polymer (A) in the present invention is too small, the moldability of the obtained polymer (B) may be reduced, whereas if it is too large, the mechanical properties and heat resistance of the obtained polymer (B) may be reduced due to the low molecular weight components contained therein. Therefore, Mw / Mn is preferably from 1.7 to 20, more preferably from 1.8 to 15, and even more preferably from 1.9 to 10.

[0101] The Mw and Mw / Mn of the polymer (A) are values ​​measured by gel permeation chromatography (GPC), and the measurement conditions are as described in the examples below.

[0102] The Mw and Mw / Mn of the polymer (A) in the present invention can be arbitrarily controlled by appropriately optimizing known conditions such as the polymerization method and polymerization conditions for the polymer (A), the types and blending ratio of raw materials for the polymer (A), and the type and amount of the polymerization catalyst added.

[0103] The lower limit of the crystallization temperature of the polymer (A) in the present invention is not particularly limited, and from the viewpoint of improving the heat resistance and mechanical strength of the polymer (B) obtained by reusing the polymer (A), it is preferably 65° C. or higher, more preferably 70° C. or higher, even more preferably 75° C. or higher, and particularly preferably 80° C. or higher. The upper limit of the crystallization temperature is not particularly limited, and from the viewpoint that if the crystallization temperature is too high, the moldability of the obtained copolymer (B) becomes difficult, it is preferably 120° C. or lower, more preferably 117° C. or lower, even more preferably 113° C. or lower, and particularly preferably 110° C. or lower. The above upper and lower limits can be combined in any combination. For example, the suitable range of the crystallization temperature of the polymer (A) in the present invention is preferably 65 to 120°C, more preferably 70 to 117°C, further preferably 75 to 113°C, and particularly preferably 80 to 110°C. The method for measuring the crystallization temperature in the present invention will be described later in detail.

[0104] The lower limit of the melting point of the polymer (A) in the present invention is not particularly limited, and from the viewpoint of improving the heat resistance and mechanical strength of the polymer (B) obtained by reusing the polymer (A), it is preferably 80° C. or higher, more preferably 85° C. or higher, even more preferably 90° C. or higher, and particularly preferably 95° C. or higher. The upper limit of the melting point is not particularly limited, and from the viewpoint that if the melting point is too high, the resulting copolymer (B) becomes brittle and easily cracked, it is preferably 135° C. or lower, more preferably 130° C. or lower, even more preferably 125° C. or lower, and particularly preferably 120° C. or lower. The above upper and lower limits can be combined in any combination. For example, the suitable range of the melting point of the polymer (A) in the present invention is preferably 80 to 135°C, more preferably 85 to 130°C, further preferably 90 to 125°C, and particularly preferably 95 to 120°C. The method for measuring the melting point in the present invention will be described later in detail.

[0105] (Method for producing polymer (A)) The method for producing the polymer (A) in the present invention is not particularly limited, and in general, from the viewpoint of productivity, it is preferred to employ a known radical polymerization method, preferably a known high-pressure radical polymerization method (hereinafter simply referred to as a "radical polymerization method"), and produce the polymer (A) by adjusting the polymerization temperature, polymerization time, the type and amount of a chain transfer agent, the type and amount of a polymerization initiator, etc. As an example, polymer (A) can be produced by radically polymerizing a radically polymerizable monomer and a cyclic ketene acetal. More preferably, the polymer (A) is produced by polymerizing a radically polymerizable monomer and a cyclic ketene acetal in the presence of an azo-based initiator. The radical polymerization method is preferably carried out without a solvent or in a solvent, and is preferably carried out without a solvent from the viewpoint of obtaining a polymer (A) with a low impurity concentration. From the viewpoint of suppressing the occurrence of coloration in the polymer (A), the polymerization reaction is preferably carried out with a low dissolved oxygen content. In addition, the polymerization reaction is preferably carried out in an inert gas atmosphere such as nitrogen gas.

[0106] The polymerization initiator used in the radical polymerization method for producing the polymer (A) of the present invention is not particularly limited as long as it generates reactive radicals. As the polymerization initiator, a known metal complex and a known radical initiator can be used alone or in combination.

[0107] The radical polymerization performance of a metal complex depends on the metal species constituting the metal complex. Specific examples of the metal include iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), ruthenium (Ru), and palladium (Pd). Among these, iron, cobalt, copper, and ruthenium are preferred, and cobalt is more preferred. Furthermore, the radical polymerization performance of a metal complex is also affected by the type of compound that modifies the metal, called a ligand. By optimizing the combination of the metal and the ligand, the polymerization activity and polymerization stability as a polymerization initiator can be improved.

[0108] The method for forming a metal-ligand complex from the metal and the ligand is not particularly limited, and for example, the metal and the ligand may be mixed in advance to form a complex, or the metal and the ligand may be added separately to a polymerization system to form a complex within the polymerization system.

[0109] Specific examples of the metal complex include the following a) to c), where X represents a chlorine atom (Cl) or a bromine atom (Br). a) Copper-based complexes such as FeX2 / TACN (triazacyclononane), FeX2 / iPr3TACN (triisopropyl-1,4,7-triazacyclononane), CuX2 / PMDETA (pentamethyldiethylenetriamine), CuX2 / TPMA (tris(2-pyridylmethyl)amine), CuX2 / Me6TREN (tris(2-(dimethylamino)ethyl)amine), CuX2 / TPEN (tetrakis(2-pyridylmethyl)-1,2-ethylenediamine), and CuX2 / bpy (bipyridine). b) Ruthenium complexes such as chloro(indenyl)(triphenylphosphine)ruthenium, chloro(pentamethylcyclopentadiene)(bis(triphenylphosphine)ruthenium, and chloro(2-dimethylaminoindenyl)(bis(triphenylphosphine)ruthenium c) Cobalt complexes such as Co(tetraphenylporphyrin) and (-)-N,N'-bis(3,5-di-t-butylsalicylidene)-1,2-cyclohexanediaminocobalt

[0110] Among these, FeX2 / iPr3TACN (triisopropyl-1,4,7-triazacyclononane), CuX2 / TPMA, CuX2 / Me6TREN, chloro(2-dimethylaminoindenyl)(bis(triphenylphosphine)ruthenium, and (-)-N,N'-bis(3,5-di-t-butylsalicylidene)-1,2-cyclohexanediaminocobalt are preferred. These metal complexes can be used alone or in combination of two or more.

[0111] Specific examples of the radical initiator include known peroxide initiators such as di-t-butyl peroxide, t-hexylperoxyisopropyl monocarbonate, t-hexylperoxy 2-ethylhexanoate, t-butyl peroxypivalate, t-hexyl peroxypivalate, benzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, and lauroyl peroxide, and azo initiators such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), and dimethyl 2,2'-azobis(2-methylpropionate). Among these, di-t-butyl peroxide, t-hexylperoxy 2-ethylhexanoate, 1,1-bis(t-hexylperoxy)cyclohexane, dimethyl 2,2'-azobis(2-methylpropionate), and 2,2'-azobis(isobutyronitrile) are preferred. These polymerization initiators can be used alone or in combination of two or more.

[0112] The amount of the polymerization initiator used is not particularly limited, and is usually preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass, relative to 100 parts by mass of the cyclic ketene acetal monomer to be subjected to the polymerization reaction.

[0113] Examples of chain transfer agents used in the radical polymerization method for producing the polymer (A) of the present invention include alkyl mercaptans such as n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, 1,4-butanedithiol, 1,6-hexanedithiol, ethylene glycol bisthiopropionate, butanediol bisthioglycolate, butanediol bisthiopropionate, hexanediol bisthioglycolate, hexanediol bisthiopropionate, trimethylolpropane tris-(β-thiopropionate), and pentaerythritol tetrakisthiopropionate. Among these, monofunctional alkyl mercaptans such as n-octyl mercaptan and n-dodecyl mercaptan are preferred. These chain transfer agents can be used alone or in combination of two or more.

[0114] The amount of the chain transfer agent used is not particularly limited, and is usually 0.1 to 1 part by mass, preferably 0.15 to 0.8 parts by mass, more preferably 0.2 to 0.6 parts by mass, and even more preferably 0.2 to 0.5 parts by mass, relative to 100 parts by mass of the monomer to be subjected to the polymerization reaction. The amount of the chain transfer agent used is usually 2500 to 10000 parts by mass, preferably 3000 to 9000 parts by mass, and more preferably 3500 to 6000 parts by mass, relative to 100 parts by mass of the polymerization initiator. Alternatively, the reaction solvent or the like may also function as the chain transfer agent without using the chain transfer agent.

[0115] The solvent used in the radical polymerization method for producing the polymer (A) of the present invention is not particularly limited as long as it can dissolve the monomer and the polymer (A) and does not inhibit the radical polymerization. For example, a tertiary alcohol such as t-butanol or 2-methyl-2-butanol, or a solvent having low radical scavenging property such as dimethyl carbonate (DMC) can be used. These solvents can be used alone or in combination of two or more. The amount of the solvent used can be appropriately set in consideration of the viscosity of the reaction liquid and the productivity. The amount of the solvent used is not particularly limited, and is usually 300 to 50,000 parts by mass, and preferably 600 to 20,000 parts by mass, based on 100 parts by mass of the cyclic ketene acetal monomer used in the polymerization reaction.

[0116] In the radical polymerization method for producing the polymer (A) of the present invention, the temperature during the polymerization reaction is not particularly limited and is usually 50 to 85°C, more preferably 60 to 83°C, and even more preferably 65 to 80°C. A polymerization temperature of 50° C. or higher tends to improve productivity due to an increase in polymerization rate, a decrease in viscosity of the polymerization liquid, etc. Also, a polymerization temperature of 85° C. or lower makes it easy to control the polymerization rate, and furthermore, suppresses the generation of by-products, thereby suppressing coloration of the polymer (A).

[0117] In the radical polymerization method for producing the polymer (A) of the present invention, the polymerization reaction time is not particularly limited and is usually 0.5 to 10 hours, preferably 1.0 to 9 hours, and more preferably 1.0 to 8 hours.

[0118] In the radical polymerization method for producing the polymer (A) of the present invention, the pressure of the polymerization reaction is not particularly limited, and is usually 2 MPa or more, preferably 3 MPa or more, more preferably 3.5 MPa or more, and is preferably 25 MPa or less, 20 MPa or less, and further preferably 15 MPa or less. The pressure of the polymerization reaction is preferably 2 to 25 MPa, more preferably 3 to 25 MPa, and further preferably 3.5 to 20 MPa.

[0119] <Polymer (B)> In the method for producing a polymer of the present invention, the polymer (B) is a polymer containing structural units derived from the polymer (A) and is obtained by polycondensing the polymer (A).

[0120] In the method for producing the polymer of the present invention, it is preferable that the weight average molecular weight Mwa of the polymer (A) and the weight average molecular weight Mwb of the polymer (B) satisfy the relationship Mwa < Mwb from the viewpoint of better mechanical strength and heat resistance of the obtained polymer (B).

[0121] Also, from the viewpoint of the mechanical strength and heat resistance of the obtained polymer (B), the lower limit of the weight average molecular weight (Mw) of the polymer (B) in the present invention is preferably 5,000 or more, more preferably 8,000 or more, still more preferably 10,000 or more, and particularly preferably 15,000 or more. On the other hand, the upper limit of the weight average molecular weight (Mw) is preferably 1,000,000 or less, more preferably 500,000 or less, still more preferably 300,000 or less, and particularly preferably 200,000 or less from the viewpoint of the yield when polycondensing the polymer (A) to obtain the polymer (B), that is, excellent recyclability. The above upper and lower limits can be arbitrarily combined. For example, the weight average molecular weight (Mw) of the polymer (B) in the present invention is preferably 5,000 or more and 1,000,000 or less, more preferably 8,000 or more and 500,000 or less, still more preferably 10,000 or more and 300,000 or less, and particularly preferably 15,000 or more and 200,000 or less.

[0122] In addition, if the molecular weight distribution (weight average molecular weight / number average molecular weight: Mw / Mn) of the polymer (B) of the present invention is too small, the moldability of the obtained polymer (B) may decrease, and if it is too large, the mechanical properties and heat resistance of the obtained polymer (B) may decrease due to the contained low molecular weight components. Therefore, 1.7 to 20 is preferable, 1.8 to 15 is more preferable, and 1.9 to 10 is still more preferable.

[0123] Incidentally, Mw and Mw / Mn of the polymer (B) are values measured by gel permeation chromatography (GPC), and the measurement conditions are as described in the examples below.

[0124] The Mw and Mw / Mn of the polymer (B) of the present invention are determined by the conditions of the polycondensation reaction in the polycondensation step (X), the conditions of the hydrolysis reaction in the hydrolysis step (X-1) and the polycondensation reaction in the polycondensation step (X-2) included in the polycondensation step (X), and the conditions of the hydrolysis reaction in the hydrolysis step (X-1) and the hydrolysis step (X-1-1) and the hydrolysis step (X-1-2) included in the hydrolysis step (X-1) and the hydrolysis step (X-1-3) included in the hydrolysis step (X-1). The treatment conditions in the purification step (X-1-2) can be appropriately selected and adjusted to control the conditions as desired.

[0125] The polymer (B) is a polymer containing a structural unit (3) represented by the following general formula (3).

[0126] [ka]

[0127] (In the above formula (3), l, m, n, Z, R 1 and R 2 respectively represent l, m, n, Z, and R in the formula (1). 1 and R 2 is equivalent to

[0128] In the polymer (B) of the present invention, the structural unit (3) preferably contains a structural unit derived from a cyclic ketene acetal (hereinafter referred to as a "cyclic ketene acetal unit"). Furthermore, the cyclic ketene acetal is preferably represented by the following general formula (4).

[0129] [ka]

[0130] (In the above formula (4), n and R 1 and R 2 respectively represent n and R in the above formula (3). 1 and R 2 is equivalent to

[0131] The cyclic ketene acetal represented by the general formula (4) has the same meaning as the cyclic ketene acetal represented by the general formula (2).

[0132] Furthermore, in the polymer (B) of the present invention, it is preferable that the structural unit (3) further contains a structural unit derived from a radically polymerizable monomer (hereinafter referred to as a "radically polymerizable monomer unit"), from the viewpoint of improving the mechanical strength and heat resistance of the obtained polymer (B).

[0133] The radically polymerizable monomer forming the radically polymerizable monomer unit in the polymer (B) has the same meaning as the radically polymerizable monomer forming the radically polymerizable monomer unit in the polymer (A).

[0134] In the polymer (B) of the present invention, the lower limit of the content of the structural unit (3) is not particularly limited, and is preferably 60.0 mol% or more, more preferably 70.0 mol% or more, even more preferably 80.0 mol% or more, and particularly preferably 90.0 mol% or more, based on 100% of the total number of moles of the structural units of the polymer (B). On the other hand, the upper limit of the content of the structural unit (3) is not particularly limited, and may be 100 mol% based on 100% of the total number of moles of the structural units of the polymer (B), or may be preferably less than 100 mol%, more preferably 99.5 mol% or less, even more preferably 99.0 mol% or less, particularly more preferably 98.0 mol% or less, and most preferably 95.0 mol% or less, based on the mechanical strength and heat resistance of the obtained polymer (B). The upper and lower limits can be combined arbitrarily. For example, the content of the structural unit (3) in the polymer (B) in the present invention may be 100 mol% relative to the total mole number of the structural units of the polymer (B), or it may be preferably 60.0 mol% or more and less than 100 mol%, more preferably 70.0 mol% or more and 99.5 mol% or less, even more preferably 80.0 mol% or more and 99.0 mol% or less, particularly preferably 90.0 mol% or more and 98.0 mol% or less, and most preferably 90.0 mol% or more and 95.0 mol% or less.

[0135] In the polymer (B) of the present invention, the lower limit of the content of the cyclic ketene acetal unit in the structural unit (3) is not particularly limited, and is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, even more preferably 0.8 mol% or more, particularly preferably 0.9 mol% or more, and most preferably 1.0 mol% or more, based on 100% of the total number of moles of the structural units of the structural unit (3). On the other hand, the upper limit of the content of the cyclic ketene acetal is not particularly limited, and is preferably 20.0 mol% or less, more preferably 10.0 mol% or less, even more preferably 9.0 mol% or less, particularly preferably 8.5 mol% or less, and most preferably 8.0 mol% or less, based on 100% of the total number of moles of the structural units of the structural unit (3), from the viewpoint of the mechanical strength and heat resistance of the obtained polymer (B). The upper and lower limits can be combined arbitrarily. For example, the content of the cyclic ketene acetal in the polymer (B) in the present invention is preferably 0.1 mol% to 20.0 mol%, more preferably 0.5 mol% to 10.0 mol%, even more preferably 0.8 mol% to 9.0 mol%, particularly preferably 0.9 mol% to 8.5 mol%, and most preferably 1.0 mol% to 8.0 mol%, based on the total moles of the structural units of the structural unit (3) (100%).

[0136] In the polymer (B) of the present invention, the lower limit of the content of the repeating unit represented by Z in the structural unit (3) is not particularly limited, and from the viewpoint of mechanical strength and heat resistance of the obtained polymer (B), it is preferably 80.0 mol% or more, more preferably 90.0 mol% or more, even more preferably 91.0 mol% or more, even more preferably 91.5 mol% or more, and most preferably 92.0 mol% or more, based on 100% of the total moles of the structural units of the structural unit (3). On the other hand, the upper limit of the content of the repeating unit represented by Z is not particularly limited, and from the viewpoint of the yield when the polymer (A) is polycondensed to obtain the polymer (B), that is, excellent reusability, it is preferably 99.9 mol% or less, more preferably 99.5 mol% or less, even more preferably 99.2 mol% or less, particularly preferably 99.1 mol% or less, and most preferably 99.0 mol% or less, based on 100% of the total moles of the structural units of the structural unit (1). The upper and lower limits can be combined arbitrarily. For example, the content ratio of the radical polymerizable monomer unit in the polymer (A) in the present invention is preferably 80.0 mol% or more and 99.9 mol% or less, more preferably 90.0 mol% or more and 99.5 mol% or less, still more preferably 91.0 mol% or more and 99.2 mol% or less, particularly preferably 91.5 mol% or more and 99.1 mol% or less, and most preferably 92.0 mol% or more and 99.0 mol% or less, based on the total mole number of the structural unit of the structural unit (1) being 100%.

[0137] Furthermore, in the polymer (B) of the present invention, the lower limit of the ratio of the number of moles of the cyclic ketene acetal units to the total number of moles of the cyclic ketene acetal units and the repeating units represented by Z is not particularly limited, and is preferably 0.001 or more, more preferably 0.005 or more, even more preferably 0.08 or more, particularly preferably 0.09 or more, and most preferably 0.01 or more. On the other hand, the upper limit of l / (l+m) is not particularly limited, and is preferably 0.200 or less, more preferably 0.100 or less, even more preferably 0.090 or less, and most preferably 0.085 or less, from the viewpoint of the mechanical strength and heat resistance of the obtained polymer (B). is particularly preferred, and 0.080 or less is most preferred. The upper and lower limits can be combined in any combination. For example, in the polymer (B) of the present invention, the ratio of the number of moles of the cyclic ketene acetal units to the total number of moles of the cyclic ketene acetal units and the repeating units represented by Z is preferably 0.001 to 0.200, more preferably 0.100 to 0.100, even more preferably 0.08 to 0.090, particularly preferably 0.09 to 0.085, and most preferably 0.01 to 0.080.

[0138] The lower limit of the crystallization temperature of the polymer (B) in the present invention is not particularly limited, and from the viewpoint of obtaining good heat resistance and mechanical strength, it is preferably 65° C. or higher, more preferably 70° C. or higher, even more preferably 75° C. or higher, and particularly preferably 80° C. or higher. The upper limit of the crystallization temperature is not particularly limited, and from the viewpoint that if the crystallization temperature is too high, the moldability of the obtained copolymer (B) becomes difficult, it is preferably 120° C. or lower, more preferably 117° C. or lower, even more preferably 113° C. or lower, and particularly preferably 110° C. or lower. The above upper and lower limits can be combined in any combination. For example, the suitable range of the crystallization temperature of the polymer (B) in the present invention is preferably 65 to 120°C, more preferably 70 to 117°C, further preferably 75 to 113°C, and particularly preferably 80 to 110°C. The method for measuring the crystallization temperature in the present invention will be described later in detail.

[0139] The lower limit of the melting point of the polymer (B) in the present invention is not particularly limited, and from the viewpoint of obtaining good heat resistance and mechanical strength, it is preferably 80° C. or higher, more preferably 85° C. or higher, even more preferably 90° C. or higher, and particularly preferably 95° C. or higher. The upper limit of the melting point is not particularly limited, and from the viewpoint that if the melting point is too high, the copolymer (B) becomes brittle and easily cracked, it is preferably 135° C. or lower, more preferably 130° C. or lower, even more preferably 125° C. or lower, and particularly preferably 120° C. or lower. The above upper and lower limits can be combined in any combination. For example, the suitable range of the melting point of the polymer (B) in the present invention is preferably 80 to 135°C, more preferably 85 to 130°C, further preferably 90 to 125°C, and particularly preferably 95 to 120°C. The method for measuring the melting point in the present invention will be described later in detail. EXAMPLES

[0140] The present invention will be explained in more detail below by way of experimental examples in place of the working examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. The following experimental examples are merely illustrative and are not intended to limit any of the embodiments described herein. The following experimental examples are not intended to limit the invention in any way. The values ​​of various manufacturing conditions and evaluation results in the following experimental examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and a preferred range may be a range defined by a combination of the above-mentioned upper or lower limit value and the values ​​of the following examples or values ​​between the examples.

[0141] [raw materials] The abbreviations for the raw materials used in the experimental examples are as follows. DMC: Dimethyl carbonate (product name: Dimethyl carbonate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 2-Methylene-1,3-dioxepane (CKA) (synthesized based on U.S. Patent Application Publication No. 2013 / 344159, U.S. Patent No. 5,455,361, and Journal of Organic Chemistry 1999, 64, 8386-8395) Co(salen) complex: a complex of cobalt and a salen ligand (product name: (R,R)-(-)-N,N'-bis(3,5-di-t-butylsalicylidene)-1,2-cyclohexanediaminocobalt(II), manufactured by Sigma-Aldrich Japan) AIBN: Azoisobutylnitrile (trade name: 2,2'-azobis(isobutyronitrile), manufactured by Tokyo Chemical Industry Co., Ltd.) Ti(OiPr)4: Tetraisopropyl orthotitanate (product name: Tetraisopropyl orthotitanate, manufactured by Tokyo Chemical Industry Co., Ltd.) tBuOH: tert-butyl alcohol (product name: tert-butyl alcohol, manufactured by Tokyo Chemical Industry Co., Ltd.) Ti(OBu)4: Tetrabutyl orthotitanate (product name: titanium tetrabutoxide monomer, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0142] In the following experimental examples, various physical properties were measured by the following methods.

[0143] [Evaluation method] <Melting point (Tm) and crystallization temperature (Tc)> The melting point (Tm) and crystallization temperature (Tc) of the polymer and hydrolysis product obtained in the experimental examples were measured using a differential scanning calorimeter (DSC) (manufactured by Hitachi High-Tech Science Corporation, model name: TA7000 DSC7020AS-3D) according to the following procedure. Approximately 1 mg of the polymer was placed in a sample container and held at 30°C for 3 minutes under a nitrogen gas atmosphere. Then, the temperature was increased from 30°C to 210°C at a rate of 10°C / min, and held at 210°C for 5 minutes. Then, the temperature was cooled from 210°C to -10°C at a rate of 10°C / min, and held at -10°C for 5 minutes. After that, the temperature was increased from -10°C to 210°C at a rate of 10°C / min, and the melting point (Tm) and crystallization temperature (Tc) (unit: °C) at this time were determined.

[0144] <Weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn)> For the polymers obtained in the experimental examples, the weight average molecular weight (Mw) and number average molecular weight (Mn) were determined by gel permeation chromatography (GPC measurement) according to the following procedure. A polymer sample (approximately 20 mg) was placed in a vial for a high-temperature GPC sample pretreatment device (manufactured by Polymer Laboratory, model name: PL-SP 260VS), and an o-dichlorobenzene solution containing BHT as a stabilizer (BHT concentration: 0.5 g / L) was added so that the polymer concentration became 0.1% by mass. Next, the vial containing the sample was placed in the high-temperature GPC sample pretreatment device and heated to 135° C. to dissolve the polymer, and then filtered using a glass filter to obtain a sample for GPC measurement. In any case, no polymer was observed trapped in the glass filter. Next, using a high-temperature GPC apparatus equipped with an RI detector (Tosoh Corporation, model name: HLC-8321GPC / HT, column: Tosoh Corporation TSKgel GMH-HT (30 cm × 4 columns)), GPC measurements were performed under the following measurement conditions: sample injection volume of approximately 300 μL, column temperature of 135°C, o-dichlorobenzene as the measurement solvent (mobile phase), and flow rate of 1.0 mL / min. The molecular weight of the polymer was calculated based on a calibration curve of retention time and molecular weight prepared from the viscosity equation of ethylene polymers using commercially available monodisperse polystyrene as a standard sample. The viscosity equation is [η] = K × M α For polystyrene, K=1.38E -4 , α=0.70, and for ethylene polymers, K=4.77E -4 , α = 0.70 was used.

[0145] <Polymer composition analysis> 13 The composition of the polymer obtained in the experimental example was analyzed using a C-NMR measurement device (manufactured by Bruker, model name: AVANCE500MHz) according to the following procedure. 30 mg of the polymer was dissolved in ODCB (orthodichlorobenzene)-d4 (0.6 mL) to prepare an NMR measurement sample. 13 Using a C-NMR measurement device, the measurement temperature was 130°C, pp:zgig (inverse gate decoupling 13C), the number of integrations was 3000 ns, and D1 was 14.8 seconds. 13 C-NMR measurements were performed.

[0146] [Experimental Example 1] (Synthesis of Polymer (A-1)) As the polymer (A-1), an ethylene / 2-methylene-1,3-dioxepane copolymer was synthesized by the following procedure. A 2L pressure reactor (AC) was charged with DMC (350mL) as a solvent, and then 2-methylene-1,3-dioxepane (50mL, 48.5g, 0.43mol) and a DMC solution (40mL) containing Co(salen) complex (0.75g, 1.24mmol) as a radical control agent (metal radical polymerization catalyst) were added. A DMC solution (10mL) containing AIBN (1.32g, 8.0mmol) was introduced into the catalyst inner cylinder of the AC. The air in the AC was replaced with nitrogen gas (pressure 0.5 MPa) three times, and then the air in the AC was replaced with ethylene gas (pressure 0.2 MPa) three times. The catalyst solution in the catalyst inner cylinder was put into the AC, and then ethylene gas was supplied to adjust the pressure in the AC to 2 MPa, and the temperature in the AC was raised to 72°C. The pressure in the AC was adjusted to 4.0 MPa while supplying ethylene gas, and the temperature in the AC was maintained at 75°C and stirred for 6 hours to carry out a polymerization reaction of ethylene and 2-methylene-1,3-dioxepane. Thereafter, the temperature in the AC was cooled to room temperature (25°C), and the AC was substituted with nitrogen. With the AC substituted with nitrogen, the polymerization solution was filtered from the bottom of the AC, washed with hexane and acetone (100 mL each), and dried to obtain a green ethylene / 2-methylene-1,3-dioxepane copolymer powder (25.02 g), which was named polymer (A-1). The obtained polymer (A-1) was a copolymer containing 6 mol % of structural units derived from 2-methylene-1,3-dioxepane and 94 mol % of structural units derived from ethylene, with the total structural units being 100 mol %. In addition, Mw=3,400, Mn=1,900, and Mw / Mn=1.9. In addition, two melting points (Tm) were observed, which were 87°C and 98°C. Two crystallization temperatures (Tc) were observed, which were 80°C and 91°C.

[0147] (Purification of Polymer (A-1)) The obtained polymer (A-1) (23.14 g) was placed in a flask, and the atmosphere in the flask was replaced with nitrogen. Toluene (200 mL) and 1N HCl (40 mL) were added thereto, and the mixture was stirred at 83°C for 2 hours. After stirring, the mixture in the flask was cooled to room temperature (25°C), added to acetone (200 mL), filtered, and washed with acetone (200 mL) twice, then naturally dried overnight and further vacuum dried at 25°C to obtain a light gray ethylene / 2-methylene-1,3-dioxepane copolymer powder (23.34 g, recovery rate 100%), which was used as the purified polymer (A). The resulting purified polymer (A-1) had Mw=3,400, Mn=1,900, and Mw / Mn=1.9. Two melting points (Tm) were observed, which were 89°C and 100°C. Two crystallization temperatures (Tc) were observed, which were 81°C and 91°C.

[0148] (Hydrolysis of purified polymer (A-1)) The purified polymer (A-1) (1.88 g) and MeOH / 1N KOH (40 mL / 8 mL) were placed in a 50 mL pressure reactor (AC) and purged with nitrogen. The mixture was stirred at 180°C for 4.5 hours. After the contents of the reactor were cooled to room temperature (25°C), the suspension was adjusted to acidic (pH 1) using 1N HCl, filtered, and the precipitate was washed with water. The precipitate was placed in a beaker of acetone (50 mL) and stirred for 10 minutes, then filtered. The resulting powder was air-dried overnight and then vacuum-dried to obtain a powder (1.32 g, recovery rate 70%). The obtained powder was a hydrolysis product of polymer (A-1). Two melting points (Tm) were observed, 94° C. and 104° C. Two crystallization temperatures (Tc) were observed, 85° C. and 96° C.

[0149] (Purification of hydrolysis product of polymer (A-1)) The hydrolyzate (1.12 g) of the obtained polymer (A-1) and toluene (20 mL) were placed in a 100 mL eggplant flask. After stirring at 90°C for 20 minutes, 6N NaOH (2.0 mL) was added. The suspension was stirred at 90°C for 10 minutes, filtered, and the precipitate was washed with tBuOMe and water. The precipitate, water (20 mL), and toluene (20 mL) were added and heated to 85°C and stirred. 1N HCl was added to the aqueous layer until the pH became 1, and then 1N HCl (4 mL) and water (4 mL) were added. The toluene layer was washed with water three times and then cooled to room temperature. The precipitate was filtered and washed with water and acetone. The obtained powder was air-dried overnight and then vacuum-dried to obtain a granular solid (0.44 g, recovery rate 39%). The resulting granular solid was a purified hydrolysis product of polymer (A-1).

[0150] (Polycondensation of the purified product of the hydrolysis product of polymer (A-1)) As polymer (B), an ethylene / 2-methylene-1,3-dioxepane copolymer was produced by the following procedure. The purified product (0.33 g) of the hydrolysis product of the obtained polymer (A-1) was placed in a reactor, and the inside of the reactor was replaced with nitrogen. Then, a butanol solution (0.035 mol / L, 0.02 mL, 0.001 mmol) containing Ti(OiPr)4 was added, and the temperature in the reactor was raised from 25°C to 180°C over 20 minutes, and then stirred for 2 hours. Then, the temperature in the reactor was raised to 195°C over 10 minutes, and stirred for 4 hours with a vacuum pump, and the final pressure was 0.81 mmHg. After that, the viscous liquid obtained in the reactor was cooled to 130°C, and toluene (20 mL) was added and the polycondensate was dissolved while refluxing at 130°C. The obtained solution was slowly poured into acetone (50 mL), and a white suspension was obtained. This operation of adding toluene, refluxing, and pouring the obtained solution into acetone was repeated twice. The finally obtained white suspension was filtered, and the white filtrate was then collected in a tray and dried to obtain 0.31 g (94% recovery) of a white powder of ethylene / 2-methylene-1,3-dioxepane copolymer, which was designated as polymer (B-1). The resulting polymer (B-1) had an Mw of 16,200, an Mn of 3,800, and an Mw / Mn of 4.2, a melting point (Tm) of 106°C, and a crystallization temperature (Tc) of 96°C.

[0151] [Experimental Example 2] (Synthesis of Polymer (A-2)) As the polymer (A-2), an ethylene / 2-methylene-1,3-dioxepane copolymer was synthesized by the following procedure. In a 2-L pressure reactor (AC), DMC (350 mL) was added as a solvent, followed by the addition of 2-methylene-1,3-dioxepane (60 mL, 58.2 g, 0.51 mol) and a DMC solution (10 mL) containing a Co(salen) complex (0.75 g, 1.24 mmol) as a radical reaction promoter (metal radical polymerization catalyst). A DMC solution (5 mL) containing AIBN (1.32 g, 8.0 mmol) was introduced into the catalyst inner cylinder of the AC. The air in the AC was replaced with nitrogen gas (pressure 0.5 MPa) three times, and then the air in the AC was replaced with ethylene gas (pressure 0.2 MPa) three times. The catalyst solution in the catalyst inner cylinder was put into the AC, and then ethylene gas was supplied to adjust the pressure in the AC to 2 MPa, and the temperature in the AC was raised to 72°C. The pressure in the AC was adjusted to 4.0 MPa while supplying ethylene gas, and the temperature in the AC was maintained at 75°C and stirred for 6 hours to carry out a polymerization reaction of ethylene and 2-methylene-1,3-dioxepane. Thereafter, the temperature in the AC was cooled to room temperature (25°C), and the AC was substituted with nitrogen. With the AC substituted with nitrogen, the polymerization solution was filtered from the bottom of the AC, washed with hexane and acetone (100 mL each), and dried to obtain a green ethylene / 2-methylene-1,3-dioxepane copolymer powder (28.65 g), which was named polymer (A-2). The obtained polymer (A-2) was a copolymer containing 8 mol % of structural units derived from 2-methylene-1,3-dioxepane and 92 mol % of structural units derived from ethylene, with the total structural units being 100 mol %. In addition, Mw=4,200, Mn=2,100, and Mw / Mn=1.9. Two melting points (Tm) were observed, which were 85°C and 97°C. Two crystallization temperatures (Tc) were observed, which were 78°C and 89°C.

[0152] (Purification of Polymer (A-2)) The obtained polymer (A-2) (11.26 g) was placed in a flask and replaced with nitrogen. Toluene (100 mL) and 1N HCl (20 mL) were added thereto and stirred at 86 ° C for 2 hours. After stirring, the mixture in the flask was cooled to room temperature (25 ° C), and then added to acetone (300 mL), filtered, naturally dried, and dried under reduced pressure to obtain a light gray ethylene / 2-methylene-1,3-dioxepane copolymer powder (10.08 g, recovery rate 89.5%), which was used as the purified polymer (A-2). The resulting purified polymer (A-2) had Mw=4,000, Mn=2,100, and Mw / Mn=1.9. Two melting points (Tm) were observed, which were 85° C. and 97° C. Two crystallization temperatures (Tc) were observed, which were 78° C. and 88° C.

[0153] (Hydrolysis of purified polymer (A-2)) The purified polymer (A-2) (0.8 g) and MeOH / 1N KOH (16 mL / 3.2 mL) were placed in a 50 mL pressure reactor (AC) and purged with nitrogen. The mixture was stirred at 165°C for 5 hours. After the contents of the reactor were cooled to room temperature (25°C), the suspension was acidified (pH 1) with 1N HCl, filtered, and the precipitate was washed with water. The precipitate was placed in a beaker of acetone (50 mL) and stirred for 10 minutes, then filtered. The resulting powder was air-dried overnight and then vacuum-dried to obtain a powder (0.65 g, recovery rate 81%). The obtained powder was a hydrolysis product of polymer (A-2). Two melting points (Tm) of the hydrolysis product were observed, 89°C and 100°C. Two crystallization temperatures (Tc) were observed, 83°C and 94°C.

[0154] (Polycondensation of hydrolysis product of polymer (A-2)) As polymer (B), an ethylene / 2-methylene-1,3-dioxepane copolymer was produced by the following procedure. The hydrolysis product (0.61 g) of the obtained polymer (A-2) was placed in a reactor, and the inside of the reactor was replaced with nitrogen. Then, a butanol solution (0.035 mol / L, 0.08 mL, 0.003 mmol) containing Ti(OiPr)4 was added, and the temperature in the reactor was raised from 25°C to 200°C over 20 minutes, and then the mixture was stirred for 1 hour, and the mixture was stirred for another 1 hour while reducing the pressure in the reactor with a diaphragm pump. Then, the temperature in the reactor was raised to 220°C over 10 minutes, and the mixture was stirred for 3 hours with a vacuum pump, and the final pressure was 0.32 mmHg. After that, the viscous liquid obtained in the reactor was cooled to 130°C, toluene (20mL) was added, and the polycondensate was dissolved while refluxing at 130°C. The obtained solution was slowly poured into acetone (100mL), and a white suspension was obtained. This operation of adding toluene, refluxing, and pouring into acetone was repeated three times. The finally obtained white suspension was filtered, and the white filtrate was then collected in a tray and dried to obtain 0.44 g (75% recovery) of a white powder of ethylene / 2-methylene-1,3-dioxepane copolymer, which was designated as polymer (B-2). The resulting polymer (B-2) had Mw=17,500, Mn=4,000, and Mw / Mn=4.3, a melting point (Tm) of 94°C, and a crystallization temperature (Tc) of 86°C.

[0155] [Experimental Example 3] (Purification of hydrolysis product of polymer (A-2)) The hydrolysis product (0.7 g) of the polymer (A-2) obtained in Experimental Example 2 and KOH (0.4 g) were placed in a 100 mL eggplant flask, and water (8 mL) was added. The suspension was heated to 85°C in an oil bath and stirred for 2 hours. After stirring, it was vacuum dried, and toluene (25 mL) was added to the obtained solid. It was heated to 75°C in an oil bath, stirred for 15 minutes, left to stand, and the supernatant liquid was removed. The process of adding toluene, heating and stirring, leaving to stand, and removing the supernatant liquid was repeated two more times, and then vacuum dried at 85°C. 1N HCl was added to the obtained powder to adjust it to acidic (pH 1), and then it was filtered and the precipitate was washed with water and acetone. The obtained powder was air-dried overnight and then vacuum dried to obtain a granular solid (0.45 g, recovery rate 64%). The resulting granular solid was a purified hydrolysis product of polymer (A-2).

[0156] (Polycondensation of the purified product of the hydrolysis product of polymer (A-2)) As polymer (B), an ethylene / 2-methylene-1,3-dioxepane copolymer was produced by the following procedure. The purified product (0.50 g) of the hydrolysis product of the obtained polymer (A-2) was placed in a reactor, and the inside of the reactor was replaced with nitrogen. Then, a butanol solution (0.035 mol / L, 0.08 mL, 0.003 mmol) containing Ti(OiPr)4 was added, and the temperature in the reactor was raised from 25°C to 180°C over 20 minutes, and then stirred for 10 minutes, and stirred for another hour while reducing the pressure in the reactor with a diaphragm pump. Then, the temperature in the reactor was raised to 195°C over 10 minutes, and stirred for 2 hours with a vacuum pump, and the final pressure was 0.37 mmHg. After that, the viscous liquid obtained in the reactor was cooled to 130°C, toluene (20mL) was added, and the polycondensate was dissolved while refluxing at 130°C. The obtained solution was slowly poured into acetone (50mL), and a white suspension was obtained. This operation of adding toluene, refluxing, and pouring into acetone was repeated three times. The finally obtained white suspension was filtered, and the white filtrate was then collected in a tray and dried to obtain 0.47 g (94% recovery) of a white powder of ethylene / 2-methylene-1,3-dioxepane copolymer, which was designated as polymer (B-3). The resulting polymer (B-3) had Mw=22,600, Mn=3,700, and Mw / Mn=6.1, a melting point (Tm) of 103°C, and a crystallization temperature (Tc) of 96°C.

[0157] [Experimental Example 4] (Synthesis of Polymer (A-4)) As the polymer (A-4), an ethylene / 2-methylene-1,3-dioxepane (CKA) copolymer was synthesized by the following procedure. A mixture of CKA (30 mL, 29.1 g, 0.25 mol) and tBuOH (400 mL) was added to a 2 L pressure reactor (AC). Then, a solution (20 mL) of AIBN (0.66 g, 4.0 mmol) dissolved in CKA as a radical generator was introduced into the AC. The air in the AC was replaced with nitrogen gas (pressure 0.5 MPa) three times, and then the air in the AC was replaced with ethylene gas (pressure 0.2 MPa) three times. The temperature in the AC was raised, and while supplying ethylene gas, the pressure in the AC was maintained at 4.0 MPa and the temperature at 75°C, and stirring was continued for 3 hours. After that, the temperature in the AC was cooled to room temperature (25°C), and the AC was replaced with nitrogen. The AC was replaced with nitrogen, and the polymerization solution was filtered from the bottom of the AC, washed with acetone (100 mL), and dried to obtain a white powder (19.82 g) of ethylene / CKA copolymer, which was designated as polymer (A-4). The polymer (A-4) obtained had a CKA-derived structural unit content of 7.5 mol % and an ethylene-derived structural unit content of 92.5 mol % with respect to the total structural units being 100 mol %. In addition, Mw=12,700, Mn=5,800, and Mw / Mn=2.2. Two melting points (Tm) were observed, which were 89°C and 96°C. The crystallization temperature (Tc) was 85°C.

[0158] (Hydrolysis of Polymer (A-4)) Polymer (A-4) (23.23 g) and MeOH / 1N KOH (350 mL / 70 mL) were placed in a 2 L pressure reactor (AC) and purged with nitrogen. The mixture was stirred at 160°C for 5 hours, and then the temperature in the AC was cooled to room temperature (25°C). The resulting suspension was adjusted to pH 1-2 (acidic) using 1N HCl, and the resulting filtrate was added to distilled water (400 mL). Next, the distilled water containing the filtrate was stirred and then filtered, and the filtrate obtained was poured into acetone (400 mL). Next, the acetone containing the filtrate was stirred and then filtered, and the resulting filtrate was air-dried to obtain a white powder (15.9 g). The obtained powder was a hydrolysis product of polymer (A-4). Two melting points (Tm) of the hydrolysis product were observed, 94°C and 107°C. The crystallization temperatures (Tc) were 87°C and 97°C.

[0159] (Polycondensation of hydrolysis product of polymer (A-4)) The hydrolysis product (2.05 g) of polymer (A-4) was placed in a glass reactor and purged with nitrogen. The temperature was raised to 140°C and the atmosphere was purged with nitrogen again. A toluene solution of Ti(OBu)4 (31 mmol / L, 0.1 mL, 0.003 mmol) was added thereto, and the mixture was heated at 205°C. The mixture was stirred at the same temperature for 1 hour and reduced in pressure with a vacuum pump. Toluene (30 mL) was added thereto and refluxed, and the resulting solution was poured into acetone (200 mL). To the residue was again added toluene (20 mL) and refluxed, and the solution was poured into acetone again. The suspension was filtered, and the resulting precipitate was air-dried and dried up in a tray to obtain a white powder (1.80 g) as polymer B, which was named polymer (B-4).

[0160] The obtained polymer (B-4) had Mw=121,000, Mn=8,700, and Mw / Mn=13.9. The melting point (Tm) was 99°C, and two crystallization temperatures (Tc) were observed, which were 88°C and 56°C.

[0161] [Experimental Example 5] (Synthesis of Polymer (A-5)) As the polymer (A-5), an ethylene / 2-methylene-1,3-dioxepane (CKA) copolymer was synthesized by the following procedure. Polymerization was carried out in the same manner as in Experimental Example 4, except that CKA (66 mL) and tBuOH (800 mL) were used, to obtain a copolymer (16.7 g), which was designated as polymer (A-5). The polymer (A-5) obtained had a CKA-derived structural unit content of 5.1 mol% and an ethylene-derived structural unit content of 94.9 mol%, with the total structural units being 100 mol%. Mw=12,000, Mn=6,700, and Mw / Mn=1.8. Two melting points (Tm) were observed, 100°C and 104°C. The crystallization temperatures (Tc) were 92 and 57°C.

[0162] (Hydrolysis of Polymer (A-5)) Polymer (A-5) (45.77 g) and MeOH / 1N KOH (350 mL / 70 mL) were placed in a 2 L pressure reactor (AC) and purged with nitrogen. The mixture was stirred at 160° C. for 5 hours, and then the temperature in the AC was cooled to room temperature (25° C.). The resulting suspension was adjusted to pH 1-2 (acidic) using 1N HCl, and the filtrate obtained by filtering the suspension was poured into distilled water (400 mL). Next, the distilled water containing the filtrate was stirred and then filtered, and the filtrate obtained was poured into acetone (400 mL). Next, the acetone containing the filtrate was stirred and then filtered, and the resulting filtrate was air-dried to obtain a white powder (36.7 g). The obtained powder was a hydrolysis product of polymer (A-5). Two melting points (Tm) of the hydrolysis product were observed, which were 98°C and 110°C. The glass transition points (Tc) were 89°C and 99°C.

[0163] (Polycondensation of hydrolysis product of polymer (A-5)) The hydrolysis product (4.34 g) of polymer (A-5) was placed in a glass reactor and purged with nitrogen. The temperature was raised to 140°C and the atmosphere was purged with nitrogen again. A toluene solution of Ti(OBu)4 (31 mmol / L, 0.2 mL, 0.006 mmol) was added thereto, and the mixture was heated to 205°C, stirred at the same temperature for 1.5 hours, and the pressure was reduced by a vacuum pump. Toluene (20 mL) was added thereto and refluxed, and the resulting solution was poured into acetone (400 mL), and toluene (10 mL) was added to the residue and refluxed, and poured into acetone again. The suspension was filtered, and the precipitate was air-dried and dried up to obtain a white powder (4.16 g) as polymer B, which was named polymer (B-5). The obtained polymer (B-5) had Mw=91,300, Mn=8,700, and Mw / Mn=10.5. The melting point (Tm) was 101°C, and two crystallization temperatures (Tc) were observed, which were 91°C and 56°C.

[0164] [Experimental Example 6] (Synthesis of Polymer (A-7)) As the polymer (A-7), an ethylene / 2-methylene-1,3-dioxepane (CKA) copolymer was synthesized by the following procedure. Polymerization was carried out in the same manner as in Experimental Example 4 except that CKA (149 mL) and tBuOH (800 mL) were used and the polymerization time was changed to 5 hours, to obtain a copolymer (36.5 g), which was designated as polymer (A-7). The polymer (A-7) obtained had a CKA-derived structural unit content of 10.6 mol % and an ethylene-derived structural unit content of 89.4 mol % with respect to the total structural units being 100 mol %. Mw=12,100, Mn=5,900, Mw / Mn=2.1. Two melting points (Tm) were observed, 81°C and 90°C. The crystallization temperatures (Tc) were 79 and 46°C.

[0165] (Hydrolysis of Polymer (A-7)) Polymer (A-7) (34.33 g) and MeOH / 1N KOH (350 mL / 70 mL) were placed in a 2 L pressure reactor (AC) and purged with nitrogen. The mixture was stirred at 160°C for 5 hours, and then the temperature in the AC was cooled to room temperature (25°C). The resulting suspension was adjusted to pH 1-2 (acidic) using 1N HCl, and the resulting filtrate was added to distilled water (400 mL). Next, the distilled water containing the filtrate was stirred and then filtered, and the filtrate obtained was poured into acetone (500 mL). Next, the acetone containing the filtrate was stirred and then filtered, and the resulting filtrate was air-dried to obtain a white powder (23.08 g). The obtained powder was a hydrolysis product of polymer (A-7). Two melting points (Tm) of the hydrolysis product were observed, which were 92°C and 103°C. The crystallization temperatures (Tc) were 85°C and 91°C.

[0166] (Polycondensation of hydrolysis product of polymer (A-7)) The hydrolysis product (1.58g) was placed in a glass reactor and purged with nitrogen. It was heated to 140°C and purged with nitrogen again. A toluene solution of Ti(OBu)4 (31mmol / L, 0.10mL, 0.003mmol) was added thereto, and the mixture was heated to 190°C. It was stirred for 30 minutes while flowing nitrogen at the same temperature. It was stirred for 20 minutes at the same temperature, 15 minutes at 200°C, and 1.5 hours at 205°C while reducing the pressure. After cooling it to 130°C, toluene (20mL) was added and refluxed, the solution was added to acetone (200mL), toluene (20mL) was added to the residue, refluxed, and added to acetone again. The suspension was filtered, and the white powder was placed in a tray and air-dried and dried up to obtain a white powder (1.34g), which was used as polymer (B-7). The obtained polymer (B-7) had Mw=97,400, Mn=7,900, and Mw / Mn=13.5. The melting point (Tm) was 97°C, and two crystallization temperatures (Tc) were observed, which were 85°C and 55°C.

[0167] [Experimental Example 7] (Polycondensation of Polymer (A-4)) Polymer (A-4) (2.14g) was placed in a glass reactor and purged with nitrogen. A toluene solution of Ti(OiPr)4 (30mmol / L, 0.1mL, 0.003mmol) was added. The mixture was heated to 185℃, and a toluene solution of Ti(OiPr)4 (30mmol / L, 0.1mL, 0.003mmol) was added. The mixture was heated to 195℃ and stirred for 1.5 hours while reducing the pressure with a vacuum pump. The mixture was further stirred at 200℃ for 1.5 hours and at 205℃ for 3.5 hours. The mixture was cooled to 130℃, and toluene (15mL) was added and refluxed. The resulting solution was poured into acetone (150mL). The suspension was filtered, and the precipitate was air-dried and dried up to obtain a white powder (1.72g), which was named polymer (B-8). The obtained polymer (B-8) had Mw=65,900, Mn=4,400, and Mw / Mn=15.0. The melting point (Tm) was 91°C, and two crystallization temperatures (Tc) were observed, which were 81°C and 48°C.

[0168] [Experimental Example 8] (Polycondensation of Polymer (A-5)) Polymer (A-5) (6.50 g) was placed in a glass reactor and replaced with nitrogen. It was heated to 150°C, and a toluene solution of Ti(OBu)4 (30 mmol / L, 0.2 mL, 0.006 mmol) was added. It was heated to 195°C, and stirred for 10 minutes while reducing the pressure with a vacuum pump, and at 205°C for 5 hours. After cooling to 130°C, toluene (30 mL) was added and refluxed. The resulting solution was poured into acetone (150 mL). After filtering the suspension, the precipitate was air-dried and dried up to obtain a white powder (5.05 g), which was named polymer (B-9). The obtained polymer (B-9) had Mw=65,900, Mn=4,400, and Mw / Mn=15.0. The melting point (Tm) was 91°C, and two crystallization temperatures (Tc) were observed, which were 81°C and 48°C.

[0169] [Experimental Example 9] (Synthesis of Polymer (A-6)) As the polymer (A-6), an ethylene / 2-methylene-1,3-dioxepane (CKA) copolymer was synthesized by the following procedure. Polymerization was carried out in the same manner as in Experimental Example 4 except that CKA (30 mL) and tBuOH (800 mL) were used and the polymerization time was changed to 6 hours, to obtain a copolymer (5.9 g), which was designated as polymer (A-6). The polymer (A-6) obtained had a CKA-derived structural unit content of 2.4 mol % and an ethylene-derived structural unit content of 97.6 mol % with respect to the total structural units being 100 mol %. Mw=16,400, Mn=8,800, Mw / Mn=1.9. Two melting points (Tm) were observed, 104°C and 108°C. The crystallization temperatures (Tc) were 96 and 59°C.

[0170] (Polycondensation of Polymer (A-6)) Polymer (A-6) (1.87g) was placed in a glass reactor and purged with nitrogen. It was heated to 160℃, and a toluene solution of Ti(OBu)4 (30mmol / L, 0.2mL, 0.006mmol) was added. The mixture was heated to 205℃ and stirred for 40 minutes while flowing nitrogen at the same temperature. After that, the pressure was reduced by a vacuum pump and the mixture was stirred for 2 hours. After cooling to 130℃, toluene (30mL) was added and refluxed. The obtained solution was poured into acetone (200mL). After filtering the suspension, the precipitate was air-dried and dried up to obtain a white powder (1.35g), which was named polymer (B-10). The obtained polymer (B-10) had Mw=79,300, Mn=9,900, and Mw / Mn=8.0. The melting point (Tm) was 103°C, and two crystallization temperatures (Tc) were observed, which were 93°C and 54°C.

[0171] [Table 1]

[0172] The polymer (B) obtained under the production conditions of Experimental Examples 1 to 10 had a higher molecular weight (Mw, Mn) than the polymer (A). In particular, the polymer (B) obtained under the production conditions of Experimental Examples 1 and 3 had a higher melting point (Tm) and crystallization temperature (Tc) than the polymer (A). That is, according to the production method of the present invention, polymer (A) can be chemically recycled to obtain polymer (B) which is more excellent in mechanical properties and heat resistance than polymer (A). It was found that the melting point of the polymer (B) having a plurality of branches was lower than that of the polymer having no branches.

Claims

1. A method for producing a polymer, comprising: a polycondensation step (X) of polycondensing a polymer (A) containing a structural unit (1) represented by the following general formula (1) to obtain a polymer (B) containing a structural unit derived from the polymer (A): [Formula 1] (In the above formula (1), l and m represent integers satisfying 0.001≦l / (l+m)≦0.2, and n represents an integer of 1 to 3. Z represents any repeating unit. 1 and R 2 each represents a hydrogen atom, an optionally branched alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms which may have a substituent, an aryl group having 6 to 10 carbon atoms which may have a substituent, or an aralkyl group having 7 to 10 carbon atoms which may have a substituent. Also, R 1 and R 2 At least one of may contain at least one heteroatom selected from the group consisting of oxygen atoms, sulfur atoms, and nitrogen atoms. n is 2 or 3, and a plurality of R 1 and R 2 If R exists, 1 may be the same or different, and the plurality of R 2 may be the same or different.)

2. The method for producing a polymer according to claim 1, wherein the polycondensation reaction in the polycondensation step (X) is carried out under a pressure of 0.1 mm or more and 1 mmHg or less.

3. The method for producing a polymer according to claim 1, wherein the polycondensation step (X) includes a hydrolysis step (X-1) of hydrolyzing the polymer (A) to obtain a hydrolysis product derived from the polymer (A), and a polycondensation step (X-2) of polycondensing the obtained hydrolysis product to obtain the polymer (B).

4. The method for producing a polymer according to claim 3, wherein the hydrolysis step (X-1) comprises a hydrolysis step (X-1-1) in which the polymer (A) is hydrolyzed in an alcohol-based solvent in the presence of a basic catalyst at a temperature in the range of 130° C. or more and 200° C. or less to obtain an oligomer and / or a monomer derived from the polymer (A).

5. The method for producing a polymer according to claim 4, wherein the oligomer and / or monomer obtained in the hydrolysis step (X-1-1) is polycondensed in the presence of a metal catalyst in the polycondensation step (X-2) at a temperature in the range of 170° C. or more and 250° C. or less.

6. The method for producing a polymer according to any one of claims 1 to 4, wherein in the above formula (1), l represents an integer of 1 to 15, and m represents an integer of 85 to 99.

7. The method for producing a polymer according to any one of claims 1 to 4, wherein the structural unit (1) includes a structural unit derived from a cyclic ketene acetal.

8. The method for producing a polymer according to claim 7 , wherein the cyclic ketene acetal is represented by the following general formula (2): [chemical 2] (In the above formula (2), n, R 1 , R 2 respectively represent n and R in the formula (1). 1 , R 2 (Same meaning as above.)

9. The method for producing a polymer according to any one of claims 1 to 5, wherein the Z is a structural unit derived from a radically polymerizable monomer.

10. The method for producing a polymer according to claim 9, wherein the radical polymerizable monomer comprises at least one selected from the group consisting of ethylene and olefins having 3 to 12 carbon atoms.

11. The method for producing a polymer according to any one of claims 1 to 5, wherein the weight average molecular weight Mwa of the polymer (A) and the weight average molecular weight Mwb of the polymer (B) satisfy the relationship Mwa < Mwb.

12. The method for producing a polymer according to any one of claims 1 to 5, wherein the weight average molecular weight of the polymer (B) is 5,000 or more and 1,000,000 or less.

13. The method for producing a polymer according to any one of claims 1 to 5, wherein the weight average molecular weight Mwb of the polymer (B) is 3 to 50 times the weight average molecular weight Mwa of the polymer (A).

14. The method for producing a polymer according to any one of claims 1 to 5, wherein in the above formula (1), Z has a repeating unit having at least one alkyl group having 1 to 20 carbon atoms which may have a branch, and at least one cycloalkyl group having 3 to 20 carbon atoms which may have a substituent, in a side chain.

15. In the above formula (1), l represents an integer of 1 to 15, and m represents an integer of 85 to 99. The structural unit (1) contains a structural unit derived from a compound represented by general formula (2), The method for producing a polymer according to any one of claims 1 to 5, wherein the Z is a structural unit derived from a radically polymerizable monomer. [C3] (In the above formula (2), n, R 1 , R 2 respectively represent n and R in the formula (1). 1 , R 2 (Same meaning as above.)

16. In the above formula (1), l represents an integer of 1 to 15, and m represents an integer of 85 to 99. The structural unit (1) contains a structural unit derived from 2-methylene-1,3-dioxepane, Z is a structural unit derived from a radical polymerizable monomer, The method for producing a polymer according to any one of claims 1 to 5, wherein the radical polymerizable monomer comprises at least one selected from the group consisting of ethylene and olefins having 3 to 12 carbon atoms.

17. The method for producing a polymer according to any one of claims 1 to 5, wherein the polymer (B) is a polymer containing a structural unit (3) represented by general formula (3). [C4] (In the above formula (3), l, m, n, Z, R 1 and R 2 respectively represent l, m, n, Z, and R in formula (1). 1 and R 2 (Same meaning as above.)

Citation Information

Patent Citations

  • Production of ethylene copolymer

    JP1983015508A

  • Decomposable ethylene copolymer composition

    JP1992081450A

  • Photodegradable and biodegradable polyethylene

    JP1994504086A

  • Photodegradable and biodegradable polyethylene

    US5281681A