Woven or knitted fabric and clothing

The use of eccentric core-sheath type polyamide conjugate fibers in fabrics addresses the issues of shape change and breathability, providing enhanced comfort and quick-drying properties in clothing.

JP2024132976APending Publication Date: 2024-10-01TORAY INDUSTRIES INC

Patent Information

Application Number
JP2024037768
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-14
Filing Date
2024-03-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing fabrics fail to adequately improve comfort by insufficiently changing shape and breathability when wet, and lack quick-drying properties, leading to discomfort from stickiness and potential dimensional instability.

Method used

A woven or knitted fabric using eccentric core-sheath type polyamide conjugate fibers, with specific compositions and structures, that allow for significant shape change when wet, enhancing breathability and quick-drying capabilities.

Benefits of technology

The fabric exhibits improved breathability and quick-drying properties, maintaining comfort and dimensional stability even when wet, suitable for clothing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132976000001_ABST
    Figure 2024132976000001_ABST
Patent Text Reader

Abstract

To provide a fabric that is excellent in quick drying property and capable of further improving air permeability during wet than during dry due to change in form of the fabric during wet, and has a small dimensional change ratio when the fabric returned to a dry state from a wet state.SOLUTION: A woven or knitted fabric uses two or more types of yarns. At least one type of yarn of the yarns is an eccentric sheath-core polyamide conjugate fiber. Mass ratio of the polyamide conjugate fiber in the woven or knitted fabric is 10% to 60%. Stretch elongation ratio of the polyamide conjugate fiber is 3.0% or more. In the polyamide conjugate fiber, polyamide A constituting a core component includes 20 mass% or more in total of at least one type selected from a group consisting of polyether amide, polyether ester amide, and polyvinyl pyrrolidone, while polyamide B constituting a sheath component includes 50 mass% or more in total of at one type selected from a group consisting of nylon 6, nylon 66, nylon 4, nylon 610, nylon 410 and others.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to woven or knitted fabrics and clothing that can have high functionality by changing their shape. [Background technology]

[0002] It has long been known that natural fibers such as cotton and animal hairs such as wool change their fiber morphology, for example the rate of shrinkage, when the temperature and humidity change. Research is being conducted into synthetic fibers or fabrics that mimic these characteristics and further pursue comfort.

[0003] For example, it has been studied to improve breathability by using a composite fiber in which a high swelling component and a low swelling component are joined in a parallel arrangement structure, and by absorbing water, the crimp disappears and the spaces in the woven or knitted stitches open up (for example, Patent Document 1), and it has been studied to suppress stuffiness by applying a false twist process to a fiber in which a polyester component and a polyamide component are combined in a side-by-side type or eccentric core-sheath structure, and expanding the stitches due to the difference in the wet and dry crimp rates (for example, Patent Document 2).In addition, it has been attempted to improve breathability by using a knitted fabric in which cellulose-based spun yarn and long fibers, which have different torque indices depending on whether they are wet or dry, are alternately knitted, and residual torque is more likely to appear when wet, changing the angle of the stitches, that is, widening (for example, Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-23431 A [Patent Document 2] International Publication No. 2006 / 025610 [Patent Document 3] JP 2013-96031 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, as in Patent Document 1 and Patent Document 2, there is no drastic change in the fabric in which the stitches or the hollow walls of the stitches are enlarged, and the effect of improving comfort is insufficient, being equal to or less than that of a general mesh material in which the stitches are arbitrarily enlarged. Patent Document 3 also has room for improvement, as the change in the stitch angle results in smaller stitch openings than in a general mesh material.

[0006] In addition, although Patent Documents 1 to 3 all mention the effect of suppressing stuffiness, there is no description regarding the quick-drying ability of moisture absorbed by the fibers, and it can be said that these are insufficient to suppress discomfort caused by stickiness when used in clothing.

[0007] Furthermore, Patent Documents 1 to 3 state that absorbing water opens up spaces in the stitches and expands the stitches, which suggests that the dimensions of the fabric will change. However, Patent Documents 1 and 3 are silent as to whether the fabric will return to its original dimensions when it goes from a wet state to a dry state, which may pose an issue with dimensional stability.

[0008] To provide a fabric which is excellent in quick drying, has improved breathability when wet compared with when dry by changing the shape of the fabric when wet, and has a small dimensional change rate when returning from a wet state to a dry state. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention has the following configuration.

[0010] (1) A woven or knitted fabric using two or more types of yarn, at least one of which is an eccentric core-sheath type polyamide conjugate fiber, the mass ratio of the polyamide conjugate fiber in the woven or knitted fabric is 10% to 60%, and the polyamide conjugate fiber has a stretch elongation of 3.0% or more when measured by Method C described in Section 8.11 of JIS L 1013:2021 "Testing Method for Chemical Fiber Filament Yarns", and in the polyamide conjugate fiber, the polyamide A constituting the core component contains at least one selected from the group consisting of polyetheramide, polyetheresteramide, and polyvinylpyrrolidone in total at least 20% by mass, and the polyamide B constituting the sheath component contains at least one selected from the group consisting of nylon 6, nylon 66, nylon 4, nylon 610, nylon 410, nylon 11, nylon 12, nylon 56, nylon 510, and nylon 1010 in total at least 50% by mass.

[0011] (2) The woven or knitted fabric according to claim 1, wherein in the cross section of the polyamide conjugate fiber, the ratio (S / D) of the minimum thickness (S) of the sheath component to the fiber diameter (D) is 0.01 to 0.10.

[0012] (3) The woven or knitted fabric according to (1) or (2), wherein in the polyamide composite fiber, the polyamide A constituting the core component contains 20% by mass or more of polyetheramide, and the polyamide B constituting the sheath component contains 50% by mass or more of nylon 6.

[0013] (4) A woven or knitted fabric according to any one of (1) to (3), which has a higher air permeability in a wet state than in a dry state when measured in accordance with Method A (Fragile method: differential pressure 125 Pa) described in Section 8.26 of JIS L 1096:2010 "Testing methods for woven and knitted fabrics."

[0014] (5) Weight per unit area: 70 to 300 g / m 2 The woven or knitted fabric according to any one of (1) to (4), having a thickness of 0.3 to 1.0 mm when dry.

[0015] (6) A knitted fabric having a single layer structure, the knitted fabric having a knitting structure comprising: The polyamide composite fiber is continuously arranged in three or more courses, and a yarn different from the polyamide composite fiber is continuously arranged in two to five courses, which are alternately repeated in the warp direction. The woven or knitted fabric according to any one of (1) to (5), wherein all wales of the polyamide composite fiber have a plain weave, 2 to 10 wales of a yarn different from the polyamide composite fiber have a welt weave, and 4 to 10 wales of a yarn different from the polyamide composite fiber have a plain weave.

[0016] (7) The woven or knitted fabric according to any one of (1) to (5), which has a two-layer structure consisting of a front layer and a back layer, and contains the polyamide composite fiber only on either the front layer or the back layer.

[0017] (8) A garment comprising, as a whole or part of an upper or lower garment, the woven or knitted fabric according to any one of (1) to (7). Effect of the Invention

[0018] The woven and knitted fabric of the present invention is not only quick-drying, but also capable of changing its shape by absorbing water, and has improved breathability when wet compared to when dry, so that comfort is not lost even when sweating. In addition, the dimensional change rate when returning from a wet state to a dry state is small. Furthermore, since various functionalities can be imparted depending on the structure of the woven and knitted fabric, it is particularly suitable for use in clothing applications, and clothes using the same can be obtained. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a cross-sectional view of a polyamide composite fiber used in the woven or knitted fabric of the present invention. [Diagram 2] FIG. 2 is a knitting structure diagram of a single mesh knitted fabric used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The woven or knitted fabric of the present invention is characterized in that the shape of the fabric changes when it is in a wet state. The wet state referred to here means a state in which moisture, including water and sweat, is attached to the fabric. Specifically, it means that 0.5 ml or more of moisture is contained per 10 cm square of the fabric. When moisture is added to confirm the manifestation of the effect, 0.5 ml of water may be dripped onto a single point, or 0.5 ml of water may be sprayed in a mist form over a 10 cm square area.

[0021] The change in the shape of the fabric here means that the area where the aforementioned amount of moisture has been added rises in the front or back direction of the fabric. There is no limit to the size of the rise, but as mentioned above, when 0.5 ml of water is added to a 10 cm square fabric, it is preferable that the area where moisture has been added rises in the front or back direction by 0.50 mm or more, and more preferably by 1.00 mm or more.

[0022] The mechanism by which the fabric rises when wet is that the shrinkage of the eccentric core-sheath type polyamide composite fiber used in the fabric approaches non-shrinkage, as described below. In other words, the highly hygroscopic polyamide, typically a polyether-based fiber, arranged in the core portion swells, causing the shrinkage of the polyamide composite fiber caused by heat treatment to approach non-shrinkage, resulting in a change in the form of the woven or knitted fabric. When the fabric rises, not only does the breathability improve when wet, but the area of ​​the fabric temporarily increases, and the drying speed increases. The drying speed can be measured using the diffusible residual moisture content described in Example F. When the moisture content of the fabric is measured in 5-minute intervals, it is preferable that the time for the moisture content to reach 10% by mass or less is 50 minutes or less, and more preferably 45 minutes or less. The woven or knitted fabric of the present invention is a woven or knitted fabric using two or more types of yarn, at least one of which is an eccentric core-sheath type polyamide composite fiber.

[0023] An eccentric sheath-core polyamide composite fiber is a composite fiber in which at least two or more types of polyamide form an eccentric sheath-core structure. Here, eccentricity means that in the cross section of the polyamide composite fiber, the position of the center of gravity of the polyamide constituting the new component is different from the center of the cross section of the composite fiber. To explain specifically using FIG. 1, the center of the sheath portion 11 and the center of the core portion 12 are at different positions. The sheath-core means that the polyamide, which is the core component, is covered by the polyamide, which is the sheath portion. In the side-by-side type, there is a concern that peeling may occur due to the effects of yarn and fabric processing and aging deterioration caused by using the textile product, but by using the eccentric sheath-core type, these concerns are reduced and excellent quality can be obtained. In addition, if the core component and the sheath component peel off, the occurrence of shrinkage due to heat treatment is inhibited, and the morphological change of the fabric when wet, which will be described later, is inhibited, and the quick-drying property and breathability when wet are reduced, but the eccentric sheath-core structure can eliminate the concern of peeling.

[0024] In the cross section of the polyamide composite fiber, the ratio (S / D) of the minimum thickness (S) of the sheath component to the fiber diameter (D) is preferably 0.01 to 0.10. When S / D is 0.10 or less, the fiber shrinks after heat treatment at about 100°C, and the fiber can exhibit more significant crimping. Therefore, the fiber has excellent stretchability, and the morphological change when wet, which will be described later, is more effectively exhibited, and the breathability when wet is further improved. S / D is more preferably 0.03 or less. When S / D is 0.01 or more, the fiber has excellent abrasion resistance. S / D is more preferably 0.02 or more. The fiber can be prevented from being exposed to the outside due to insufficient durability of the sheath component. S / D can be measured by the method described in the Examples.

[0025] The stretching extension rate of the polyamide composite fiber measured by the C method described in 8.11 of JIS L 1013:2021 "Testing method for chemical fiber filament yarn" is 3.0% or more, and preferably 6.0% or more. The stretching extension rate is calculated using the following formula 1 from the length (L0) of the yarn taken from the woven or knitted fabric and the length (L1) of the yarn stretched by applying a certain load to the above yarn, so it can be said that the higher the stretching extension rate, the higher the shrinkage rate and the stronger the crimping. In addition, a high stretching extension rate means that the yarn stretches without being inhibited by crimping, which is suitable for the shape change when wetted, which will be described later. Stretching and elongation rate = ((L1-L0) / L0)×100 (Equation 1).

[0026] In polyamide composite fibers, the core portion has better hygroscopicity than the sheath portion. A hygroscopic fiber incorporates water molecules by physical adsorption or by forming an interaction between functional groups in the molecular structure of the fiber components and water molecules. In particular, when the fiber has high hygroscopicity, many water molecules are incorporated into the fiber, resulting in a large volumetric swelling. That is, the high hygroscopicity of the core portion results in a larger volumetric swelling than the sheath portion, and the shrinkage developed by heat treatment is more likely to extend. As the fiber elongates, the stitches become partially larger in knitted fabrics, and voids are formed between the warp and weft threads in woven fabrics, resulting in a change in the shape of the woven or knitted fabric when wet, improving breathability.

[0027] As described above, from the viewpoint of high wettability, the polyamide A of the core portion contains at least one selected from the group consisting of polyetheramide, polyetheresteramide, and polyvinylpyrrolidone in a total amount of 20% by mass or more. When two or more of these components are contained, the polyamide A is a copolymer. When the polyamide A is a copolymer, it may contain other components other than polyetheramide, polyetheresteramide, or polyvinylpyrrolidone. Regarding the other components of the polyamide A, although there are no limitations, preferred examples include nylon 6, nylon 66, nylon 4, nylon 610, nylon 410, nylon 11, nylon 12, nylon 56, nylon 510, nylon 1010, etc. At least one selected from the group consisting of polyetheramide, polyetheresteramide, and polyvinylpyrrolidone is preferably contained in a total amount of 50% by mass or more, more preferably 80% by mass or more.

[0028] Moreover, polyetheramide is a block copolymer having an amide bond and an ether bond in the polymer structure. Specifically, it is a block copolymer obtained by polycondensation reaction of one or more polyamide forming components selected from lactam, aminocarboxylic acid, and salts of diamine and dicarboxylic acid, and a polyalkylene glycol component. The combination of the polyamide forming component and the polyalkylene glycol component is not limited, but a preferred example of the polyamide forming component includes lactams such as ε-caprolactam, ω-aminocarboxylic acid such as aminocaproic acid, nylon salts of diamine-dicarboxylic acid which are precursors of polyhexamethylene adipamide, polyhexamethylene sebacamide, etc., and a polyalkylene glycol component includes polyethylene glycol. More preferably, it is a polyetheramide in which ε-caprolactam is used as the polyamide forming component and polyethylene glycol is copolymerized from the viewpoint of heat resistance, fiber forming ability, and moisture absorption of the hygroscopic polymer.

[0029] Furthermore, polyetheresteramide is a block copolymer having an ether bond, an ester bond, and an amide bond in the polymer structure. Specifically, it is a block copolymer obtained by polycondensation reaction of one or more polyamide forming components selected from lactam, aminocarboxylic acid, and salts of diamine and dicarboxylic acid, and a polyetherester component consisting of dicarboxylic acid and polyalkylene oxide glycol. The combination of the polyamide forming component and the polyetherester component is not limited, but a preferred example of the polyamide forming component is one exemplified in the above polyetheramide, and the polyalkylene glycol component constituting the polyetherester component is polyethylene glycol from the viewpoint of hygroscopicity, and the dicarboxylic acid is adipic acid, sebacic acid, dodecadiacid, terephthalic acid, isophthalic acid.

[0030] On the other hand, the polyamide B of the sheath portion contains at least one selected from the group consisting of nylon 6, nylon 66, nylon 4, nylon 610, nylon 410, nylon 11, nylon 12, nylon 56, nylon 510 and nylon 1010 in a total amount of 50% by mass or more in order to make the polyamide B of the core portion less wettable. Among them, the type of nylon is preferably at least one selected from the group consisting of nylon 6, nylon 66, nylon 610, nylon 410, nylon 11, nylon 12, nylon 510 and nylon 1010 in order to have a lower moisture absorption. In addition, the content of the above-mentioned nylon is preferably 80% by mass or more in total. When two or more of these components are contained, the polyamide B is a copolymer. When the polyamide B is a copolymer, it may contain other components other than nylon 6, nylon 66, nylon 4, nylon 610, nylon 410, nylon 11, nylon 12, nylon 56, nylon 510 or nylon 1010. With regard to polyamide B, other components are not limited, but from the viewpoint of reducing wettability, the total content of polyetheramide, polyetheresteramide and polyvinylpyrrolidone is preferably 10% by mass or less, more preferably 5% by mass or less.

[0031] Among them, it is preferable that the polyamide A constituting the core component contains 20% by mass or more of polyetheramide, and the polyamide B constituting the sheath component contains 50% by mass or more of nylon 6. With this combination, the melting points of each are close to each other, and melt spinning can be performed more stably.

[0032] Each of the polyamide A and the polyamide B may contain various additives, if necessary.

[0033] As described above, in order to fully express the shrinkage caused by heat treatment and to change the shape of the fabric when wetted by the mechanism described below to improve breathability, the moisture absorption and release parameter ΔMR of polyamide A constituting the core component of the polyamide composite fiber is preferably 2.0% or more, more preferably 4.0% or more, and even more preferably 6.0% or more. If ΔMR is 2.0% or more, the shape of the fabric changes sufficiently when wetted, and the breathability when wetted is further improved. Here, the reason for the change in the shape of the fabric is that the shrinkage expressed in the eccentric core-sheath type polyamide composite fiber described above approaches non-shrinkage when wetted. When the highly hygroscopic polyamide, typically a polyether-based one, arranged in the core portion swells, the shrinkage approaches non-shrinkage, causing a change in the shape of the woven or knitted fabric. The higher the moisture absorption and release parameter ΔMR of polyamide A, the better, but the practical upper limit is 17.0%, and 10.0% or less is preferable. ΔMR can be measured by the method described in the Examples.

[0034] The yarn used in the woven or knitted fabric of the present invention must be other yarns in addition to the eccentric sheath-core composite fiber, and the mass ratio of the polyamide composite fiber in the woven or knitted fabric must be 10% to 60%. If the woven or knitted fabric is formed only from the above-mentioned eccentric sheath-core polyamide composite fiber, all yarns will become non-shrunk when the fabric is in a wet state, causing a large change in shape. However, the inventors have found that if the shape changes significantly overall, the fabric will not return to its original dimensions when dried, which is undesirable from the viewpoint of dimensional stability of the fabric. Therefore, when forming the woven or knitted fabric of the present invention, one or more types of yarns other than the eccentric sheath-core polyamide must be used. For example, if the mass ratio of the polyamide composite fiber is 100%, the shape of the fabric will change significantly when it absorbs water, but the influence of resistance at the stitches where the yarns cross will be large, making it difficult to return to its original state when dried, and it is prone to becoming so-called "stretched". In contrast, when the eccentric core-sheath type polyamide composite fiber changes shape as it approaches non-crimping when wet, the other yarns moderately suppress the shape change of the fabric, thereby suppressing the amount of shape change of the entire fabric, and the fabric can return to its original dimensions when dry.

[0035] Considering the restoration to the original dimensions when dried, the mass ratio of the polyamide composite fiber in the woven or knitted fabric needs to be 60% or less, and preferably 40% or less. On the other hand, if the mass ratio of the polyamide composite fiber is too low, the shape change of the fabric when wet is insufficient and the breathability when wet is reduced, so the mass ratio of the polyamide composite fiber contained in the fabric needs to be 10% or more, and from the viewpoint of increasing the area in contact with air by the shape change and further increasing the drying speed, it is more preferable that it is 20%. As an index of restoration to the original state when dried, the G method (pulsator type domestic electric washing machine method) described in 8.39 of JIS L 1096 "Fabric test method for woven and knitted fabrics" can be used, and it is preferable that it is -5.0% to +3.0% of the original size.

[0036] Examples of yarns other than eccentric sheath-core polyamide include natural fibers such as cotton and silk, chemical fibers such as rayon and triacetate, polyester fibers such as polyethylene terephthalate, polyethylene naphthalate, polytrimethylene terephthalate, and polybutylene terephthalate, polyamide fibers such as nylon 6 and nylon 66, polyurethane fibers, polyphenylene sulfide fibers, and synthetic fibers such as polyimide fibers, but are not particularly limited thereto. Among them, polyamide fibers such as nylon 6 and nylon 66, which have the same components as the eccentric sheath-core composite fibers, are preferred from the viewpoint of being able to proceed with fabric processing such as dyeing under the same conditions as the eccentric sheath-core composite fibers. Although versatile polyethylene terephthalate may be used, it is necessary to pay attention to the fact that the hygroscopic polymer, which is the core part, is eluted out of the fiber depending on the temperature during dyeing.

[0037] When the fibers used for the woven or knitted fabric of the present invention are used for clothing applications, the fibers preferably have a fineness of 50 decitex (dtex) or more, more preferably 70 decitex or more, from the viewpoint of fabric strength, etc. From the viewpoint of texture, etc., the fibers have a fineness of 300 dtex or less, more preferably 200 dtex or less.

[0038] The woven and knitted fabrics of the present invention preferably have a higher air permeability when wet than when dry, as measured according to Method A (Fragile method: differential pressure 125 Pa) described in JIS L 1096:2010 "Testing methods for woven and knitted fabrics", section 8.26. Generally, in dry fabrics, air passes through the stitches in knitted fabrics and through the hollow spaces between yarns in woven fabrics, but in wet fabrics, the attached moisture forms a membrane that blocks the passage of air, decreasing the air permeability. On the other hand, in the woven and knitted fabrics of the present invention, the eccentric core-sheath type polyamide composite fiber that has developed crimp approaches non-crimping and the fiber extends, so that the stitches become partially larger in knitted fabrics and hollow spaces can be formed between warp and weft yarns in woven fabrics, thereby further improving the air permeability when wet. Here, the air permeability when dry can be determined by measuring the air permeability when the fabric is conditioned for 24 hours or more in a 20°C, 65% RH environment.

[0039] From the viewpoint of improving the breathability when wet compared to when dry, the thickness of the woven or knitted fabric of the present invention is preferably 0.3 mm to 1.0 mm. By making the thickness smaller than 1.0 mm, the breathability can be suppressed from being hindered by the influence of the thickness of the fabric, and the breathability when wet is further improved. By using an eccentric core-sheath type polyamide composite fiber, the breathability when wet is improved by the enlargement of the stitches in the knitted fabric and the hollow wall between the warp and weft in the woven fabric, but if the thickness is greater than 1.0 mm, the absolute value of the breathability is small, and the effect of improved breathability when wet may be difficult to feel. Therefore, the thickness is preferably 1.0 mm or less, and more preferably 0.8 mm or less. On the other hand, if the thickness of the fabric is thinner than 0.3 mm, the breathability is high regardless of whether it is dry or wet, so even if the breathability when wet is improved by using an eccentric core-sheath type polyamide composite fiber, the effect of improved breathability may be difficult to feel because the fabric originally had high breathability, but if it is 0.3 mm or more, the effect of improved breathability is more easily felt. Therefore, the thickness is preferably 0.3 mm or more, and from the viewpoint of transparency, etc., the thickness is more preferably 0.5 mm or more.

[0040] In addition, from the perspective of breathability, comfort when worn as clothing material, and light weight, the fabric has a basis weight of 300 g / m 2 It is preferable that the weight is less than 70 g / m from the viewpoint of strength and durability as a clothing material. 2 From the viewpoint of achieving both light weight, strength and durability, it is preferable that the thickness is 100 g / m 2 From 200 g / m 2 It is more preferable that the range is .

[0041] From the above viewpoints, the woven or knitted fabric of the present invention has a basis weight of 70 to 300 g / m 2 and the thickness when dry is preferably 0.3 to 1.0 mm.

[0042] In the present invention, when a knitted fabric is used, it may be either warp knitting or circular knitting. The structure of the knitted fabric is not particularly limited, but it may be a two-layer structure structure consisting of a front layer and a back layer that can be knitted by a double knitting machine, or a one-layer structure structure that can be knitted by a single knitting machine.

[0043] In the case of a single-layer structure, the knitted structure preferably has three or more consecutive courses of the polyamide composite fiber and two to five consecutive courses of a yarn different from the polyamide composite fiber, which are alternately repeated in the warp direction, and all wales of the polyamide composite fiber are in a plain weave, 2 to 10 wales of the yarn different from the polyamide composite fiber are in a welt weave, and 4 to 10 wales are in a plain weave. By using the above-mentioned knitted structure, the stitches in which the polyamide fiber is arranged become larger when wet, and the breathability is further improved. In addition, the larger stitches make it difficult for a moisture film to form, and the breathability is maintained even when the fabric is excessively wet. Note that the portion in which all wales of the polyamide composite fiber are in a plain weave may be four or more courses, but in order to maintain dimensional stability, the mass ratio of the polyamide composite fiber must be 60% or less, and six or less courses is preferable. In addition, for the yarn different from the polyamide composite fiber, if 11 or more wales are continuously formed in both the welt weave and plain weave, the fabric itself becomes more transparent, so it is preferable to knit 10 wales or less.

[0044] An example of the knitted structure is shown in Figure 2. In Figure 2, the first yarn 15, which is the polyamide composite fiber, is made up of three consecutive courses (first to third courses), and the second yarn 16, which is a yarn different from the polyamide composite fiber, is made up of five consecutive courses (fourth to eighth courses). All wales of the first yarn 15 are made up of a plain weave, and two wales (first and second wales) of the second yarn 16 are made up of a welt weave and four wales (third to sixth wales) are made up of a plain weave.

[0045] In the case of a two-layer structure consisting of a front surface and a back surface, it is preferable that only one of the front surface or the back surface contains the polyamide composite fiber. By disposing the polyamide composite fiber on either the front surface or the back surface, the shape change when wet, which will be described later, becomes large, and the breathability and quick-drying property when wet can be further improved. On the other hand, since the opposite surface does not contain the polyamide composite fiber, no shape change occurs when wet, and the woven / knitted fabric as a whole can suppress excessive dimensional change when wet, and the dimensional stability can be further improved. The structure is preferably an inlay structure, a cardboard structure, a smooth structure, or a structure based on these structures with a part of the structure knitted in a mesh. When the woven / knitted fabric of the present invention is used to make clothing, it is preferable that the surface containing the eccentric core-sheath type polyamide composite fiber is placed on the skin side from the viewpoint of absorbing sweat and causing the above-mentioned shape change. In addition, in the case of a smooth knit where the same structure is seen from either the front or back direction, either side may be the surface.

[0046] The woven fabric is not particularly limited, but a two-layer structure or three-layer structure consisting of a surface layer and a back layer is preferable. Examples of the woven fabric include plain weave, twill weave, and satin weave.

[0047] In the present invention, it is also preferable to control the density of the woven or knitted fabric in order to make the morphological change when wet more remarkable, as described below.

[0048] In the case of plain stitch knitting, which is a typical knitted fabric structure, the wale number (hereinafter sometimes abbreviated as W), which indicates the warp density, is preferably 20 to 60 per inch. A wale number greater than 20 per inch makes it easier to maintain the shape of the knitted fabric, while a wale number less than 60 per inch, preferably less than 50 per inch, is a preferred embodiment because it results in significant changes in shape when wet, as described below. The course number (hereinafter sometimes abbreviated as C), which indicates the weft density, is preferably 30 to 150 per inch, more preferably 30 to 60 per inch.

[0049] For the same reason, in the case of a woven fabric, the ratio of the cover factors CF of the warp and weft yarns (warp yarn CF / weft yarn CF) calculated by the following formula 2 is 0.8 to 2.0, and preferably 1.0 to 1.7. CF=density (strands / 2.54cm) x (fineness (dtex) x 0.9)^(1 / 2) (formula 2).

[0050] For the reasons mentioned above, the woven or knitted fabric of the present invention can be suitably used as clothing, and can be provided as a textile product which is more comfortable than conventional upper or lower garments.

[0051] Next, an example of a method for producing the eccentric core-sheath structure composite fiber of the present invention will be described.

[0052] First, a manufacturing method by high-speed direct spinning will be described as an example of melt spinning of polyamide composite fibers. The selected polyamides are melted separately, metered and transported using a gear pump, and a composite flow is formed to have a core-sheath structure in a normal manner, and discharged from a spinneret for eccentric core-sheath composite fibers. In this case, in order to obtain a desired composite fiber cross section, each polymer flow path and discharge cross section are controlled by the spinneret. The discharged polyamide composite fiber thread is cooled to 30°C by blowing cooling air using a thread cooling device such as a chimney, and is oiled and converged by an oiling device. Next, it is taken up by a take-up roller at 1500 to 4000 m / min, and passed through a take-up roller and a stretching roller. At this time, it is stretched at 1.0 to 3.0 times according to the ratio of the peripheral speed of the take-up roller and the stretching roller. Furthermore, the thread is heat-set by a stretching roller, and wound into a package at a take-up speed of 3000 m / min or more.

[0053] Separately, a method for producing polyamide composite fiber by high-speed direct melt spinning will be described below. The first polyamide and the second polyamide are melted separately, metered and transported using a gear pump, and a composite flow is formed as it is so as to have a core-sheath structure in a normal manner, and discharged from a spinneret using an eccentric core-sheath type composite fiber spinneret. The discharged polyamide composite fiber thread is cooled to 30°C by blowing cooling air using a thread cooling device such as a chimney, oiled by an oiling device, and converged, taken up by a take-up roller at 3000 to 4500 m / min, passes through the take-up roller and the stretching roller, and is slightly stretched at 1.0 to 1.2 times according to the ratio of the peripheral speed of the take-up roller and the stretching roller. Furthermore, it is wound up on a package at a take-up speed of 3000 m / min or more.

[0054] Generally, in the case of a side-by-side type composite cross section, yarn bending is likely to occur due to differences in flow speed, resulting in poor operability. However, by using an eccentric core-sheath type composite cross section, spinning properties are improved and fine single yarns can be easily obtained.

[0055] It is also possible to perform entanglement using a known entanglement device in the process up to winding. If necessary, it is also possible to increase the number of entanglements by performing entanglement multiple times. Furthermore, it is also possible to additionally apply an oil just before winding. The method for producing false twist textured yarn is not limited, but for example, it is preferable to perform false twisting using a pin type, friction type, belt type, etc. depending on the fineness and number of twists.

[0056] When the obtained yarn is used to produce a woven fabric, the manufacturing method is not particularly limited. For the woven fabric, the warp yarn is warped and placed on a loom. Similarly, the weft yarn is placed on the loom, but the polyamide composite fiber may be used for both the warp yarn and the weft yarn, or for either one of them, as long as the mass ratio is within the above-mentioned range. The loom is not particularly limited, and examples thereof include air jet looms and rapier looms. Among these, air jet looms are particularly preferred because high-speed weaving is relatively easy and productivity is easily increased. In addition, when producing a knitted fabric, the manufacturing method is not particularly limited. The knitting machine may be either a warp knitting machine or a weft knitting machine. Examples of warp knitting machines include tricot machines and Raschel machines, and examples of weft knitting machines include flat knitting machines and circular knitting machines, but circular knitting machines are particularly preferred because high-speed knitting is relatively easy and productivity is easily increased.

[0057] The processing of the obtained woven or knitted fabric may be the same as that of general nylon products, but the woven or knitted fabric of the present invention requires attention to the temperature when heat-treating with hot water, such as scouring or dyeing, in order to induce shrinkage. As an example of processing, scouring can be performed at a temperature of 80°C or higher to remove excess dirt and oil, and coloring can be performed by acid dyeing at about 100°C using an acid dye. After dyeing, the fabric can be finished by setting the density as desired and drying with hot air. EXAMPLES

[0058] The present invention will be described in more detail below with reference to examples.

[0059] [Various tests and evaluation methods] A. ΔMR (ΔMR before hot water treatment) About 1 to 2 g of a fiber sample or fabric sample was weighed into a weighing bottle, dried at 110°C for 2 hours, and then the mass was measured and this mass was designated as w0. Next, the dried fiber sample was held at a temperature of 20°C and a relative humidity of 65% for 24 hours, and then the mass was measured and this mass was designated as w65%. Next, the temperature was adjusted to 30°C and the relative humidity to 90%, and the fiber sample was held at this temperature for 24 hours, and then the mass was measured and this mass was designated as w90%. MR1=[(w65%-w0) / w0]×100...(3) MR2=[(w90%-w0) / w0]×100...(4) ΔMR = MR2 - MR1 (5) At this time, the value calculated using the formulas (3) to (5) was defined as ΔMR.

[0060] B. The minimum thickness of the sheath (S), the fiber diameter (D) and the ratio (S / D) A multifilament made of composite fibers was embedded in an embedding agent such as epoxy resin at 10 consecutive points at 1 cm intervals in the fiber axis direction to prepare a sample, and images of each sample were taken at a magnification where 10 or more fibers could be observed with a transmission electron microscope (TEM). At this time, metal staining was applied to clarify the contrast of the joint between the core component and the sheath component. The fiber diameter D and the minimum thickness S of the sheath component were measured from all single yarns in the observed image using "WinROOF2015" manufactured by Mitani Shoji Co., Ltd. as image analysis software. In addition, if the fiber cross section was not a perfect circle, the fiber diameter in the same direction as the minimum thickness S of the sheath component was taken as D. In the 10 samples, the average value of the minimum thickness S of the sheath component and the fiber diameter D of all fibers that could be observed in each image was calculated, and 10 sets of the average fiber diameter D and the average minimum thickness S of the sheath component for each sample were prepared, and these were further averaged to obtain the fiber diameter D and the minimum thickness S of the sheath component of the present invention. The fiber diameter D and the minimum thickness S of the sheath component were measured in μm units to four decimal places, and the values ​​were averaged by rounding off the fourth decimal place to the third decimal place. The ratio (S / D) of the minimum thickness S of the sheath component and the fiber diameter D thus obtained was rounded off to the second decimal place.

[0061] C.Stretching and elongation rate The stretching and elongation rate of the fiber samples was measured according to Method C (simplified method) described in Section 8.11 of JIS L 1013:2021 "Test methods for chemical fiber filament yarns." The average value was calculated with an N number of 5 and rounded to the nearest tenth.

[0062] D. Changes in the shape of the dough A piece of fabric measuring 10 cm square was prepared and left in an environment of 20°C and 65% RH for 24 hours, and then the height was measured using a 3D shape measuring instrument (manufactured by Keyence Corporation) with a height measurement range of 1.5 mm. Next, using the same piece of fabric, 1.0 ml of distilled water was dropped with a syringe and left for 30 seconds, and the height was measured using the same measuring instrument. The height when dry was A and the height when wet was B, and the height BA was obtained. The number of N was set to 5, and the average value was calculated, measured to the third decimal place, and rounded off to the second decimal place.

[0063] E. Breathability A piece of fabric consisting of 15 cm square was prepared, and left in an environment of 20°C and 65% RH for 24 hours, and then the air permeability in the dry state was measured according to the A method (Fragile type method: differential pressure 125 Pa) described in JIS L 1096:2010 "Fabric test method for woven and knitted fabrics" 8.26. Next, for Examples 1 to 3 and Comparative Examples 1 to 5 described later, 1.5 ml of distilled water was dropped with a syringe and left for 30 seconds, and then the air permeability in the wet state was measured in the same manner. Also, for Examples 4 to 6 and Comparative Examples 6 and 7, 0.5 ml of distilled water was sprayed in a mist form over a 10 cm square, and the air permeability in the wet state was measured in the same manner. Then, the difference was calculated as (air permeability in the wet state) - (air permeability in the dry state). Also, for Examples 4 to 6 and Comparative Examples 6 and 7, assuming a state of sweating a lot, 2.0 ml of distilled water was sprayed in a mist form over a 10 cm square, and the air permeability in the excessively wet state was measured in the same manner.

[0064] F.Quick drying 0.3 ml of water was dropped onto the centre of a 10 cm x 10 cm piece of fabric, and the mass of the test piece was measured at 5 minute intervals as the water diffused and dried. The time required for the diffusible residual moisture content to reach 10 mass% or less was calculated using the following formula 6. Diffusible residual moisture content (mass%) = moisture content at any time (g) / moisture content at the start of measurement (g) × 100 (Equation 6).

[0065] G. Dimensional change rate Measurements were performed according to the G method (method for pulsator-type household electric washing machines) described in Section 8.39 of JIS L 1096:2010 "Testing methods for woven and knitted fabrics," and values ​​within the range of -5.0% to +3.0% from the size before the test were determined as acceptable values. The larger the rate of change, the larger the dimensions after the test were compared to before the test. Ta.

[0066] H. Thickness A piece of fabric measuring 15 cm square was prepared and left in an environment of 20°C and 65% RH for 24 hours. It was then measured in accordance with Method A (JIS method) described in Section 8.4 of JIS L 1096:2010 "Testing methods for woven and knitted fabrics." Five different points on the sample were measured and the average value was calculated to three decimal places, and the third decimal place was rounded off to the nearest two decimal places.

[0067] [Example 1] To determine the ΔMR, nylon 6 (melt viscosity 160 Pa·s, melting point 220°C) and polyether-based nylon (melt viscosity 55 Pa·s, melting point 200°C) were melted and extruded from a spinneret (spinning temperature 270°C). The yarn extruded from the spinneret was cooled and solidified in a yarn cooling device, taken up at 3700 m / min on a take-up roller (room temperature 25°C), stretched 1.1 times between stretching rollers (room temperature 25°C), and then wound up on a package at a take-up speed of 4000 m / min to obtain nylon 6 filament yarn and polyether-based amide filament yarn with a fineness of 56 dtex and filament count of 24. Each of the obtained yarns was used to make a cylindrical knitted fabric on a 28G cylindrical knitting machine (manufactured by Eiko Sangyo Co., Ltd.) and the ΔMR was measured, which was 2.2% for nylon 6 and 8.6% for polyether-based nylon.

[0068] Next, nylon 6 as the polyamide of the sheath portion and polyetheramide as the polyamide of the core portion were arranged using a spinneret for eccentric core-sheath type composite fiber, and melt-extruded at a composite ratio (mass ratio) of 5:5 (spinning temperature 270°C). The yarn extruded from the spinneret was cooled and solidified by a yarn cooling device, oiled with a water-containing oil agent by an oiling device, and then entangled by a fluid entanglement nozzle device. The yarn was then taken up at 3700 m / min by a take-up roller (room temperature 25°C), stretched 1.1 times between stretching rollers (room temperature 25°C), and wound up on a package at a take-up speed of 4000 m / min to obtain a core-sheath type composite nylon yarn with a fineness of 56 dtex and a filament count of 24 (first yarn). The obtained yarn was made into a cylindrical knitted fabric using a 28G cylindrical knitting machine (manufactured by Eiko Sangyo Co., Ltd.), and the ΔMR was measured to be 6.8%. Next, using a 28-gauge single circular knitting machine (manufactured by Fukuhara Seiki Seisakusho Co., Ltd.), a plain weave was formed on the front side with a 78 dtex-24 filament nylon yarn (second yarn) that is not a core-sheath type and whose main component is nylon 6, and an inlay weave knit fabric was obtained with a core-sheath type composite nylon yarn (first yarn) on the back side. The resulting fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, after which it was polished to a wale (W) / course (C) ratio of 48 / 56 and a basis weight of 112 g / m 2 The results are shown in Table 1.

[0069] [Example 2] Using the core-sheath composite nylon yarn (first yarn) obtained in Example 1 and a non-core-sheath polyester yarn (second yarn) of 84 dtex-36 filament, a striped knit fabric was obtained with both yarns arranged in parallel in the wale direction using a 28-gauge single circular knitting machine (manufactured by Fukuhara Seiki Seisakusho Co., Ltd.). The resulting fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then knitted to a W / C of 50 / 52 and a basis weight of 100 g / m. 2 The results are shown in Table 1.

[0070] [Example 3] Using the sheath-core composite nylon yarn (first yarn) obtained in Example 1 and a non-sheath-core nylon yarn (second yarn) of 56 dtex-40 filament mainly composed of nylon 6, a double circular knit fabric was obtained by knitting the 56 dtex-40 filament nylon yarn in a plain weave on the front side using a 28-gauge double circular knitting machine (manufactured by Fukuhara Seiki Seisakusho Co., Ltd.) and knitting the sheath-core composite nylon yarn in a mesh weave with openings on the back side. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then the fabric was spun to a W / C of 48 / 58 and a basis weight of 130 gm. 2 The results are shown in Table 1.

[0071] [Example 4] Using the sheath-core composite nylon yarn (first yarn) obtained in Example 1 and a non-sheath-core nylon yarn (second yarn) of 78 dtex-24 filament, a waffle-shaped single mesh knitted fabric with the knitting structure shown in FIG. 2 was obtained on a 36-gauge single circular knitting machine (manufactured by Fukuhara Seiki Seisakusho Co., Ltd.). The obtained knitted fabric had three continuous courses of the first yarn and five continuous courses of the second yarn, with all wales of the first yarn being in a plain weave, two wales of the second yarn being in a welt weave, and four wales being in a plain weave. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then had a W / C of 58 / 122 and a basis weight of 152 g / m. 2 The results are shown in Table 2.

[0072] [Example 5] A knitted fabric with the same structure as in Example 4 was obtained using the core-sheath composite nylon yarn (first yarn) obtained in Example 1 and a non-core-sheath polyester yarn (second yarn) of 84 dtex-36 filament. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then the W / C was 56 / 122 and the basis weight was 151 g / m. 2 The results are shown in Table 2.

[0073] [Example 6] A waffle-shaped single mesh knitted fabric was obtained using the sheath-core composite nylon yarn (first yarn) obtained in Example 1 and a non-sheath-core polyester yarn (second yarn) of 84 dtex-36 filament on a 36-gauge single circular knitting machine (manufactured by Fukuhara Seiki Seisakusho Co., Ltd.). The obtained knitted fabric had two continuous courses of the first yarn and five continuous courses of the second yarn, with all wales of the first yarn being in a plain weave, one wale of the second yarn being in a welt weave, and three wales being in a plain weave. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then had a W / C of 56 / 112 and a basis weight of 145 g / m 2 The results are shown in Table 2.

[0074] [Comparative Example 1] A 56 dtex-40 filament non-core sheath nylon yarn (first yarn) mainly composed of nylon 6 and a 78 dtex-24 filament non-core sheath nylon yarn (second yarn) were used to obtain a knitted fabric with the same structure as in Example 1, with the second yarn on the face and the first yarn on the back. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, after which it was found to have a W / C of 42 / 66 and a basis weight of 119 g / m. 2 The results are shown in Table 1.

[0075] [Comparative Example 2] A knitted fabric with the same structure as in Example 2 was obtained using a nylon yarn (first yarn) with a non-core-sheath structure of 56 dtex-48 filaments, mainly composed of nylon 6, and a polyester yarn of 84 dtex-36 filaments (second yarn). The obtained fabric was scoured at 80°C for 20 minutes, dyed at 100°C for 30 minutes, and then spun to a size of 46 / 60 W / C and 110 g / m2. 2 The results are shown in Table 1.

[0076] [Comparative Example 3] A 56 dtex-40 filament nylon yarn (first yarn) that was not a core-sheath type was used to obtain a knitted fabric with the same structure as in Example 3. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then the W / C was 44 / 64 and the basis weight was 119 g / m2 The results are shown in Table 1.

[0077] [Comparative Example 4] Using the sheath-core composite nylon yarn (first yarn) obtained in Example 1 and a non-sheath-core nylon yarn (second yarn) of 56 dtex-40 filament mainly composed of nylon 6, a 28-gauge double circular knitting machine (manufactured by Fukuhara Seiki Seisakusho Co., Ltd.) was used to obtain a knitted fabric with the same structure as in Example 3, in which the sheath-core composite nylon yarn was used on the front and back sides and the non-sheath-core nylon yarn of 56 dtex-40 filament was used on part of the back side. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then the W / C was 48 / 60 and the basis weight was 126 g / m. 2 The results are shown in Table 1.

[0078] [Comparative Example 5] Using the sheath-core composite nylon yarn (first yarn) obtained in Example 1 and a non-sheath-core nylon yarn (second yarn) of 56 dtex-40 filament mainly composed of nylon 6, a single circular knitted fabric was obtained by knitting into a mesh structure with openings in some parts of the fabric using a 28-gauge double circular knitting machine (manufactured by Fukuhara Seiki Seisakusho Co., Ltd.). The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then the W / C was 44 / 52 and the basis weight was 109 g / m. 2 The results are shown in Table 1.

[0079] [Comparative Example 6] A 50 dtex-40 filament non-core-sheath nylon yarn (first yarn) and a 78 dtex-24 filament non-core-sheath nylon yarn (second yarn) were used to obtain a knitted fabric with the same structure as in Example 4. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then the W / C was 53 / 92 and the basis weight was 105 g / m. 2 The results are shown in Table 2.

[0080] [Comparative Example 7] A 56 dtex-36 filament non-core sheath polyester yarn (first yarn) and a 84 dtex-36 filament non-core sheath polyester yarn (second yarn) were used to obtain a knitted fabric with the same structure as in Example 4. The obtained fabric was scoured at 80°C for 20 minutes and dyed at 100°C for 30 minutes, and then the W / C was 51 / 90 and the basis weight was 91 g / m. 2 The results are shown in Table 2.

[0081] [Table 1]

[0082] [Table 2] [Industrial Applicability]

[0083] The woven or knitted fabric of the present invention changes its shape when it absorbs water, and can be used as clothing with excellent comfort due to improved breathability, and can also have various functions such as quick drying, which can increase the drying speed after washing. It can be particularly suitably used in clothing applications where comfort is required. [Explanation of symbols]

[0084] 11...Polyamide composite fiber sheath 12. Polyamide composite fiber core 13 Minimum thickness S of sheath component 14...Fiber diameter D 15...First thread 16...Second thread

Claims

1. A woven or knitted fabric using two or more types of yarn, at least one of which is an eccentric core-sheath type polyamide conjugate fiber, the mass ratio of the polyamide conjugate fiber in the woven or knitted fabric being 10% to 60%, the polyamide conjugate fiber having a stretch elongation of 3.0% or more when measured by Method C described in Section 8.11 of JIS L 1013:2021 "Testing methods for chemical fiber filament yarns", and in the polyamide conjugate fiber, polyamide A constituting a core component contains a total of 20% by mass or more of at least one type selected from the group consisting of polyetheramide, polyetheresteramide, and polyvinylpyrrolidone, and polyamide B constituting a sheath component contains a total of 50% by mass or more of at least one type selected from the group consisting of nylon 6, nylon 66, nylon 4, nylon 610, nylon 410, nylon 11, nylon 12, nylon 56, nylon 510, and nylon 1010.

2. 2. The woven or knitted fabric according to claim 1, wherein in a cross section of the polyamide conjugate fiber, the ratio (S / D) of the minimum thickness (S) of the sheath component to the fiber diameter (D) is 0.01 to 0.

10.

3. 3. The woven or knitted fabric according to claim 1, wherein in the polyamide composite fiber, the polyamide A constituting the core component contains 20% by mass or more of polyetheramide, and the polyamide B constituting the sheath component contains 50% by mass or more of nylon 6.

4. 3. The woven or knitted fabric according to claim 1, wherein the air permeability in a wet state is higher than the air permeability in a dry state when measured in accordance with Method A (Fragile method: differential pressure of 125 Pa) described in Section 8.26 of JIS L 1096:2010 "Testing methods for woven and knitted fabrics."

5. Weight per unit area: 70 to 300 g / m 2 The woven or knitted fabric according to claim 1 or 2, having a thickness of 0.3 to 1.0 mm when dry.

6. A knitted fabric having a single layer structure, wherein the knitted structure of the knitted fabric is The polyamide composite fiber is continuously arranged in three or more courses, and a yarn different from the polyamide composite fiber is continuously arranged in two to five courses, which are alternately repeated in the warp direction.

3. The woven or knitted fabric according to claim 1, wherein all wales of said polyamide composite fiber are in a plain weave, 2 to 10 wales of a yarn different from said polyamide composite fiber are in a welt weave, and 4 to 10 wales of said yarn are in a plain weave.

7. 3. The woven or knitted fabric according to claim 1, which has a two-layer structure consisting of a front layer and a back layer, and only one of the front layer or the back layer contains the polyamide composite fiber.

8. 3. A garment comprising, as a whole or part of an upper garment or a lower garment, the woven or knitted fabric according to claim 1 or 2.

Citation Information

Patent Citations

  • Reversible air-permeable fabric

    JP2005023431A

  • Fabric with excellent air permeability

    JP2013096031A

  • Composite fiber

    WO2006025610A1

Cited By

  • Machine-washable wool and real silk outdoor fabric and preparation method thereof

    CN119777053A

  • Intelligent quick-drying fabric

    CN120366959A

  • Smart quick-drying fabric

    WO2026218404A1