Two-pack curable type epoxy resin composition

A two-component epoxy resin composition with specific components ensures adequate pot life, workability, and heat resistance, addressing the limitations of existing compositions for use in civil engineering and construction, especially in high-rise wooden buildings.

JP2024132983APending Publication Date: 2024-10-01SANYO CHEM IND LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024038216
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2024-03-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing two-component epoxy resin compositions used in civil engineering and construction lack sufficient pot life and workability at low temperatures, exhibit poor storage stability, and do not provide adequate heat resistance for applications in high-rise wooden buildings.

Method used

A two-component curable epoxy resin composition comprising a polyvalent epoxy compound, an inorganic filler, and fumed silica with specific hydrophobicity levels, along with a reaction product of polyalkylene polyamine and bisphenol A diglycidyl ether, which enhances workability, storage stability, and heat resistance.

Benefits of technology

The composition maintains sufficient pot life and good workability at low temperatures, exhibits excellent storage stability, and achieves high heat resistance in cured products, making it suitable for applications in civil engineering and construction, particularly in wooden buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132983000001
    Figure 2024132983000001
  • Figure 2024132983000002
    Figure 2024132983000002
  • Figure 2024132983000003
    Figure 2024132983000003
Patent Text Reader

Abstract

To provide a two-pack curable type epoxy resin composition which can give a cured product that has enough work life even under low temperature and good workability, and is excellent in storage stability and heat resistance.SOLUTION: A two-pack curable type epoxy resin composition is composed of a main agent containing a polyvalent epoxy compound (A) which is liquid at 5°C, an inorganic filler (D) and fumed silica (E1) having a hydrophobic degree of 55 or more and 75 or less, and a curing agent containing a reactant (B) of 1 mol of polyalkylene polyamine with 0.05 to 0.35 mol of bisphenol A diglycidyl ether, an inorganic filler (D) and fumed silica (E2) having a hydrophobic degree of 0 or more and less than 55, wherein the content of (B) in the curing agent is 10 to 40 pts.wt. with respect to 100 pts.wt. of (A) in the main agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a two-component curing type epoxy resin composition. [Background technology]

[0002] Due to its excellent chemical and physical properties, epoxy resins are used in a wide range of applications, such as civil engineering, casting materials, adhesives, etc. In the civil engineering and construction field, two-part curing epoxy resin compositions that cure at room temperature and do not require heating are widely used. For example, in the GIR (Glued-in Rod) method, which is one of the joining methods for wooden buildings, a joining tool such as a steel rod is inserted into a hole made in wood, and a resin adhesive is injected and filled into the gap using an injection gun or the like, and then cured to join the pieces of wood together. Since the GIR method is carried out outdoors, the resin adhesive used is required to ensure sufficient pot life and workability (injectability, filling ability, etc.) even at low temperatures such as in winter or in cold regions. In recent years, high-rise wooden buildings have been attracting attention from the viewpoint of environmental conservation, etc. Components used in high-rise wooden buildings are required to have higher heat resistance and fire resistance than conventional low-rise buildings in accordance with building standards, and for epoxy resin compositions used in wooden buildings, such as adhesives for the GIR method, there is a demand for improved heat resistance and fire resistance of the cured product.

[0003] As an epoxy resin composition for use in the civil engineering and construction fields, Patent Document 1 proposes a two-liquid type epoxy resin composition characterized by containing styrenated phenol. The composition described in Patent Document 1 cures even at temperatures below 0°C, reaches practical strength, has a pot life, and has a viscosity that allows injection even at low temperatures, but the heat resistance of the cured product is insufficient. Patent Document 2 proposes a room temperature curable epoxy resin composition containing, as essential components, an epoxy resin having at least two oxirane rings in the molecule, one or more compounds selected from the group consisting of amine compounds and modified compounds thereof, one or more compounds selected from at least one of compounds consisting of boron halides or complexes thereof, and a phenolic compound. The composition described in Patent Document 2 can achieve both mechanical properties of the cured product, curability at low temperatures, and sufficient pot life, but does not take into consideration the heat resistance of the cured product, and the storage stability of the composition is insufficient. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-88348 A [Patent Document 2] JP 2017-105995 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a two-component curing epoxy resin composition which has sufficient pot life and good workability even at low temperatures, and which is capable of giving a cured product having excellent storage stability and heat resistance. In the present invention, "good workability" means that the composition has excellent injectability and filling property during use. "Excellent heat resistance of the cured product" means that the cured product has a high strength retention rate at high temperatures and that the adhesive strength between members bonded with the epoxy resin composition is maintained even at high temperatures. The above-mentioned "high temperature" refers to, for example, the temperature of the heat resistance test (T h ), and for wooden building applications, the temperature is around 100°C. "Low temperature" refers to the outdoor temperature in winter or in cold regions, which is around 5 to 10°C. In the present invention, Tg means the temperature at which the loss tangent (tan δ=loss modulus / storage modulus) becomes maximum when the temperature dependency of dynamic viscoelasticity is measured under the conditions described below. [Means for solving the problem]

[0006] As a result of investigations aimed at achieving the above object, the present inventors arrived at the present invention. That is, the present invention relates to a two-component curing type epoxy resin composition comprising a base material containing a polyepoxy compound (A) which is liquid at 5°C, an inorganic filler (D), and fumed silica (E1) having a hydrophobicity of 55 or more and 75 or less, and a curing agent containing a reaction product (B) of 1 mole of polyalkylene polyamine and 0.05 to 0.35 moles of bisphenol A diglycidyl ether, an inorganic filler (D), and fumed silica (E2) having a hydrophobicity of 0 or more and less than 55, wherein the content of (B) in the curing agent is 10 to 40 parts by weight per 100 parts by weight of (A) in the base material; and a cured product obtained by curing the epoxy resin composition. Effect of the Invention

[0007] The two-component curing type epoxy resin composition of the present invention has the effects of having sufficient pot life and good workability (injectability, filling property, etc.) even at low temperatures, excellent storage stability, and excellent heat resistance of the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The two-component curing type epoxy resin composition of the present invention comprises a base agent containing a polyepoxy compound (A) that is liquid at 5°C, an inorganic filler (D), and fumed silica (E1) having a hydrophobicity of 55 or more and 75 or less, and a curing agent containing a reaction product (B) of 1 mol of polyalkylene polyamine and 0.05 to 0.35 mol of bisphenol A diglycidyl ether, an inorganic filler (D), and fumed silica (E2) having a hydrophobicity of 0 or more and less than 55.

[0009] <Polyepoxy compound (A) that is liquid at 5°C> The polyepoxy compound (A) in the present invention which is liquid at 5°C is a compound which has two or more epoxy groups in the molecule and is liquid at 5°C, or a mixture which is liquid at 5°C and is obtained by mixing compounds which have two or more epoxy groups in the molecule. Examples of the polyepoxy compound (A) include the following polyglycidyl ethers (A1), polyglycidyl esters (A2), polyamine polyglycidyl amines (A3), other polyepoxy compounds (A4), and mixtures of two or more of these. When the polyepoxy compound (A) is a mixture of two or more kinds, so long as the mixture is liquid at 5°C, it may contain one that is solid at 5°C alone. In addition, the determination of whether a substance is liquid at 5°C can be made in accordance with the "Method of Confirming Liquidity" in Appendix 2 of the Ministerial Ordinance on the Testing and Properties of Hazardous Materials (Ministry of Home Affairs Ordinance No. 1 of 1989), except for changing the test temperature from 20°C to 5°C.

[0010] (A1) Polyglycidyl ether The polyglycidyl ether (A1) is an ether compound consisting of a glycidyl group and a residue obtained by removing hydrogen atoms from two or more hydroxyl groups of a polyol compound, and examples thereof include the following polyglycidyl ethers (A11) to (A16). (A11) Diglycidyl ether of dihydric phenol [carbon number (hereinafter sometimes abbreviated as C) 6 to 30] diglycidyl ethers of bisphenols (such as bisphenol F, -A, -B, -AD and -S), diglycidyl ethers of halogenated bisphenol A (such as tetrachlorobisphenol A), diglycidyl ethers of monocyclic dihydric phenols (such as catechol, resorcinol, hydroquinone), diglycidyl ethers of condensed polycyclic dihydric phenols [1,5-dihydroxynaphthalene, dihydroxybiphenyl, octachloro-4,4'-dihydroxybiphenyl, 9,9'-bis(4-hydroxyphenyl)fluorene, etc.], diglycidyl ethers obtained by the reaction of 2 moles of bisphenol A with 3 moles of epichlorohydrin, etc.;

[0011] (A12) Polyglycidyl ether of polyhydric (trihydric to hexahydric or higher) phenols Polyglycidyl ethers of polyhydric phenols (C6 or more and Mn5,000 or less), such as triglycidyl ethers of trihydric phenols (pyrogallol, dihydroxynaphthyl cresol, tris(hydroxyphenyl)methane, dinaphthyltriol, p-glycidylphenyldimethyltriyl bisphenol A, etc.), tetraglycidyl ethers of tetrahydric phenols (tetrakis(4-hydroxyphenyl)ethane, 4,4'-oxybis(1,4-phenylethyl)tetracresol, bis(dihydroxynaphthalene, etc.), phenol novolac resins, etc. polyglycidyl ethers of polyphenols (Mn400-5,000) obtained by the condensation reaction of phenol with glyoxal, glutaraldehyde, or formaldehyde, and polyglycidyl ethers of polyphenols (Mn400-5,000) obtained by the condensation reaction of resorcinol with acetone;

[0012] (A13) Diglycidyl ether of aliphatic diol (C2 or higher and Mn 5,000 or lower) diglycidyl ethers of aliphatic diols (dihydric alcohols (e.g., ethylene glycol, propylene glycol, tetramethylene glycol, neopentyl glycol, 1,6-hexanediol (hereinafter abbreviated as EG, PG, TMG, NPG, and 1,6-HD, respectively)), polyalkylene glycols (e.g., polyethylene glycol (hereinafter abbreviated as PEG, having a molecular weight of 106 or more and Mn of 4,000 or less), polypropylene glycol (hereinafter abbreviated as PPG, having a molecular weight of 134 or more and Mn of 5,000 or less), polytetramethylene glycol (hereinafter abbreviated as PTMG, having a molecular weight of 162 or more and Mn of 5,000 or less)), etc.);

[0013] (A14) Polyglycidyl ether of aliphatic poly(trihydric to hexahydric or higher)ol (C6 or higher and Mn10,000 or lower) Polyglycidyl ethers of aliphatic polyols (polyhydric (3-6) alcohols [trimethylolpropane, glycerin, pentaerythritol, sorbitol (hereinafter abbreviated as TMP, GR, PE, SO, etc.)], intramolecular or intermolecular dehydration products of polyhydric alcohols [poly(n=2-5)GR], and alkylene oxides [hereinafter abbreviated as AO, C2-6, for example, ethylene oxide, 1,2-propylene oxide (hereinafter abbreviated as EO, PO, etc.)] adducts of these polyhydric alcohols, etc.);

[0014] (A15) Polyglycidyl ether of alicyclic ring-containing poly(dihydric to tetrahydric or higher)ol those with C3 or more and Mn of 5,000 or less, for example, polyglycidyl ethers such as 1,2-cyclopropanediol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 1,4-cyclohexanediol, hydrogenated bisphenol A, 1,2,3-cyclopropanetriol, 1,3,5-cyclohexanetriol, sucrose, and AO (1 to 20 mol) adducts thereof;

[0015] (A16) Polyglycidyl ether of aromatic ring-containing polyhydric (dihydric to tetrahydric or higher) alcohol Polyglycidyl ethers such as those with C8 or more and Mn of 5,000 or less, AO (1 to 20 moles) adducts of bisphenol A, m- and p-xylylene glycol, benzenediethanol, 1,2-diphenylethane-1,2-diol, 1,1,2,2,-tetraphenylethane-1,2-diol, and AO (1 to 20 moles) adducts thereof;

[0016] (A2) Polyglycidyl ester The polyglycidyl ether (A2) is an ester compound consisting of a glycidyl group and a residue formed by removing a hydrogen atom from a hydroxyl group contained in two or more carboxyl groups of a polycarboxylic acid compound, and examples thereof include the following polyglycidyl esters (A21) to (A22). (A21) Polyglycidyl esters of aromatic polyvalent (divalent to hexavalent or higher) carboxylic acids Polyglycidyl esters of aromatic polycarboxylic acids (C6 to C20 or more), such as diglycidyl esters of aromatic dicarboxylic acids (such as ortho-, iso-, and terephthalic acid), triglycidyl esters of aromatic tricarboxylic acids (such as trimellitic acid); (A22) Polyglycidyl esters of aliphatic or alicyclic polycarboxylic acids (C6 to C20 or more) For example, diglycidyl esters of aliphatic dicarboxylic acids (such as oxalic acid, maleic acid, succinic acid, glutaric acid, adipic acid, and pimelic acid), triglycidyl esters of aliphatic tricarboxylic acids (such as tricarballylic acid), (co)polymers (with a degree of polymerization of 2 to 10) of glycidyl (meth)acrylate, polyglycidyl esters of alicyclic-containing polyvalent carboxylic acids (such as dimer acid), and nuclear hydrogenations of the above (A21);

[0017] (A3) Polyamine Polyglycidylamine The polyglycidylamine (A3) of polyamine is a polyglycidyl compound having a structure in which hydrogen atoms bonded to nitrogen atoms contained in a polyamine are substituted with glycidyl groups. The polyamine constituting the polyglycidylamine (A3) of polyamine is preferably an amine having from C6 to C20 or more and having 2 to 10 or more active hydrogen atoms directly bonded to nitrogen atoms. Examples of the polyglycidylamine (A3) of polyamine include the following polyglycidylamines (A31) to (A33). (A31) Polyglycidylamines of aromatic amines For example, N,N-diglycidylaniline, N,N-diglycidyltoluidine, N,N,N',N'-tetraglycidyldiaminodiphenylmethane, N,N,N',N'-tetraglycidyldiaminodiphenylsulfone, N,N,N',N'-tetraglycidyldiaminoethylphenylmethane, and N,N,O-triglycidylaminophenol; (A32) Polyglycidylamines of Aliphatic Amines For example, N,N,N',N'-tetraglycidylxylylenediamine, N,N,N',N'-tetraglycidylhexamethylenediamine; (A33) Polyglycidylamines containing alicyclic or heterocyclic rings (C6-C20 or more and having 2-10 or more active hydrogen atoms directly bonded to nitrogen atoms) Polyglycidylamines of alicyclic ring-containing amines (e.g. hydrogenated N,N,N',N'-tetraglycidylxylylenediamine), polyglycidylamines of heterocyclic ring-containing amines (e.g. trisglycidylmelamine);

[0018] (A4) Other polyepoxy compounds The other polyfunctional epoxy compounds are polyfunctional epoxy compounds other than the above (A1) to (A3), and examples thereof include the following polyfunctional epoxy compounds (A41) to (A42). (A41) Aliphatic poly(2-6 or more) epoxides C6 or more and Mn2,500 or less, e.g., epoxidized polybutadiene, epoxidized soybean oil; (A42) Alicyclic poly(divalent to tetravalent or higher) epoxide Those with C6 or more and Mn of 2,500 or less, such as vinylcyclohexene dioxide, limonene dioxide, dicyclopentadiene dioxide, bis(2,3-epoxycyclopentyl)ether, ethylene glycol bisepoxydicyclopentyl ether, 3,4-epoxy-6-methylcyclohexylmethyl-3',4'-epoxy-6'-methylcyclohexanecarboxylate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, and bis(3,4-epoxy-6-methylcyclohexylmethyl)butylamine.

[0019] Of these polyepoxy compounds (A), from the viewpoint of the workability (injectability and filling property) of the epoxy resin composition, it is preferable to contain the diglycidyl ether of an aliphatic diol (A13) and the polyglycidyl ether of an aliphatic polyol (A14) having 2 to 4 epoxy groups in the molecule, and it is more preferable that the total weight of the diglycidyl ethers of (A13) and (A14) having 2 to 4 epoxy groups in the molecule is 5 to 20% by weight based on the weight of the polyepoxy compound (A). From the viewpoint of the mechanical strength and heat resistance of the cured product of the epoxy resin composition, it is preferable to contain a polyepoxy compound having a bisphenol A type structure or a bisphenol F type structure in the molecule, and it is more preferable to contain a polyepoxy compound having a bisphenol A type structure or a bisphenol F type structure among (A11) and (A12), and it is particularly preferable that the total weight of the polyepoxy compounds having a bisphenol A type structure or a bisphenol F type structure is 70 to 100% by weight based on the weight of the polyepoxy compound (A). The polyfunctional epoxy compound (A) may be used alone or in combination of two or more. When the polyfunctional epoxy compound (A) is a mixture of two or more kinds, as described above, the polyfunctional epoxy compound (A) may contain a compound that is solid at 5°C alone as long as the polyfunctional epoxy compound (A) as a whole is liquid at 5°C.

[0020] The epoxy equivalent (molecular weight per epoxy group) (g / eq) of the polyepoxy compound (A) is preferably 120 to 200 g / eq, more preferably 130 to 180 g / eq, and particularly preferably 140 to 180 g / eq, from the viewpoints of the workability (injectability, etc.) of the epoxy resin composition, the curability, and the mechanical strength of the cured product. The epoxy equivalent (g / eq) of the polyepoxy compound (A) is a value measured in accordance with JIS K 7236.

[0021] The viscosity (mPa·s) of the polyepoxy compound (A) at 25°C is preferably 500 to 10,000 mPa·s, and more preferably 1,000 to 7,000 mPa·s, from the viewpoints of the workability (injectability, etc.) and storage stability of the epoxy resin composition. The viscosity (mPa·s) of the polyepoxy compound (A) at 25°C can be measured using a B-type viscometer.

[0022] The viscosity (Pa·s) of the polyepoxy compound (A) at 5° C. is preferably 10 to 150 Pa·s, and more preferably 20 to 80 Pa·s, from the viewpoints of the workability (injectability, etc.) and storage stability of the epoxy resin composition. The viscosity (Pa·s) of the polyepoxy compound (A) at 5°C can be measured using a B-type viscometer.

[0023] <Reaction product (B) of 1 mol of polyalkylene polyamine and 0.05 to 0.35 mol of bisphenol A diglycidyl ether> (B) in the present invention is a reaction product of 1 mol of polyalkylene polyamine (b1) and 0.05 to 0.35 mol of bisphenol A diglycidyl ether. By reacting 1 mole of polyalkylene polyamine (b1) with 0.05 to 0.35 moles of bisphenol A diglycidyl ether, a reaction mixture is obtained which contains, as an essential component, a compound in which epoxy groups present at both ends of bisphenol A diglycidyl ether undergo ring-opening addition to amino groups contained in the polyalkylene polyamine (b1), and which further contains unreacted polyalkylene polyamine. That is, the reaction product (B) of 1 mole of polyalkylene polyamine (b1) and 0.05 to 0.35 moles of bisphenol A diglycidyl ether is a composition containing, as an essential component, a compound in which polyalkylene polyamine (b1) is added to both ends of 1 mole of bisphenol A diglycidyl ether, and further containing unreacted polyalkylene polyamine. The polyalkylene polyamines (b1) constituting the reactant (B) include those having C2 or more and Mn of 500 or less, and specific examples thereof include C2-12 alkylene diamines (ethylene diamine, propylene diamine, trimethylene diamine, tetramethylene diamine, hexamethylene diamine, etc.) and polyalkylene (C2-10) poly(trivalent to hexavalent or higher) amines (diethylene triamine, imino bis propyl amine, bis (hexamethylene) triamine, triethylene tetramine, tetraethylene pentamine, pentaethylene hexamine, hexaethylene heptamine, etc.). From the viewpoint of the heat resistance of the cured product, the active hydrogen equivalent of the polyalkylene polyamine (b1) is preferably 50 g / eq or less, and more preferably 40 g / eq or less. In the present invention, the active hydrogen equivalent of (b1) means the molecular weight per active hydrogen (hydrogen atom directly bonded to a N atom) possessed by (b1).

[0024] Of the above (b1), from the viewpoints of pot life and heat resistance of the cured product, preferred are ethylenediamine, propylenediamine, trimethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine and hexaethyleneheptamine, and particularly preferred is pentaethylenehexamine. That is, it is particularly preferable that (B) contains a reaction product of pentaethylenehexamine and bisphenol A diglycidyl ether.

[0025] The molar number of bisphenol A diglycidyl ether reacted with 1 mole of polyalkylene polyamine in the above (B) is 0.05 to 0.35. If it is less than 0.05, the pot life tends to be shortened and storage stability tends to deteriorate, and if it exceeds 0.35, workability (injectability, etc.) at low temperatures tends to deteriorate. From the viewpoint of achieving both pot life, workability, and storage stability, the molar number of bisphenol A diglycidyl ether reacted with 1 mole of polyalkylene polyamine is preferably 0.05 to 0.30, and more preferably 0.07 to 0.20.

[0026] In the present invention, (B) not only functions as a curing agent in the room temperature curing reaction of the epoxy resin composition (hereinafter may be referred to as the first-stage curing), but also is presumed to function to further advance the curing reaction and improve the crosslink density when heated to a high temperature (for example, around 100°C) (hereinafter may be referred to as the second-stage curing reaction). Even in conventional room-temperature curable epoxy resin compositions, the curing reaction does not proceed completely at room temperature, and a second-stage curing reaction may occur when heated. However, since the epoxy resin composition of the present invention contains (B), it is presumed that the crosslink density is particularly likely to improve in the second-stage curing reaction, and a cured product with a higher Tg (glass transition temperature) can be obtained compared to conventional room-temperature curable epoxy resin compositions. For this reason, for example, when the composition of the present invention is used as a civil engineering adhesive for wooden buildings and the like, when it is heated to high temperatures due to a fire or the like, the crosslink density is effectively increased in the second-stage curing reaction described above, and it is presumed that one of the effects of the present invention, heat resistance (resin strength and adhesive strength are maintained even at high temperatures), is obtained. Furthermore, since the above (B) is a compound in which a polyalkylene polyamine and bisphenol A glycidyl ether are reacted in a specific molar ratio, it is possible to adjust the curing speed and pot life of the epoxy resin composition to appropriate ranges.

[0027] From the viewpoints of application ease and storage stability, the viscosity of (B) at 25°C is preferably 500 to 400,000 mPa·s, more preferably 500 to 200,000 mPa·s, particularly preferably 1,000 to 40,000 mPa·s, and most preferably 1,000 to 10,000 mPa·s. The viscosity (mPa·s) of (B) at 25°C can be measured using a Brookfield viscometer.

[0028] The (B) in the present invention can be obtained by mixing polyalkylene polyamine (b1) and bisphenol A diglycidyl ether, and reacting them by heating as necessary. The heating temperature may be appropriately adjusted depending on the type of (b1) and the number of moles of bisphenol A diglycidyl ether reacted with 1 mole of (b1), and is, for example, 20 to 100°C. The end point of the reaction in producing (B) can be confirmed by measuring the amine value. (B) may be used immediately after production (mixed with other components), or it may be stored after production and then used.

[0029] <Inorganic filler (D)> In the two-component curing epoxy resin composition of the present invention, from the viewpoints of handling property, storage stability, etc., each of the base agent and the curing agent contains the inorganic filler (D). In the present invention, the inorganic filler (D) may be any of the following (D1) to (D7) and mixtures of two or more of these. By incorporating the inorganic filler (D), the mechanical strength and heat resistance of the cured product of the epoxy resin composition can be improved. (D1) Silicates (e.g. talc, clay, mica, glass, quartz); (D2) Oxides [for example, titanium oxide, alumina, silica (excluding those falling under (E1) or (E2) below)]; (D3) Carbonates (e.g. calcium carbonate, magnesium carbonate, hydrotalcite); (D4) hydroxides (e.g., aluminum hydroxide, magnesium hydroxide, calcium hydroxide); (D5) Sulfites (e.g., barium sulfate, calcium sulfate, calcium sulfite); (D6) Borates (e.g. zinc borate, barium metaborate, aluminum borate, calcium borate, sodium borate); (D7) Nitrides (e.g., aluminum nitride, boron nitride, silicon nitride).

[0030] Of these (D), from the viewpoints of handleability, mechanical strength and heat resistance of the cured product, and industrial viewpoints, preferred are (D1), (D2), (D3) and (D4), more preferred are (D1), (D2) and (D3), and particularly preferred are silica and calcium carbonate.

[0031] The shape of (D) is preferably a powder from the viewpoint of the handleability of the epoxy resin composition, and the volume average particle size of (D) is preferably 0.1 to 800 μm, more preferably 0.5 to 250 μm, and particularly preferably 0.8 to 100 μm from the viewpoints of the viscosity and handleability of the epoxy resin composition.

[0032] <Fumed Silica (E1 and (E2)> The fumed silica in the present invention means powdered synthetic amorphous silica obtained by the combustion reaction or flame hydrolysis reaction of a silane compound, and is also called dry silica.Furthermore, it also includes silica particles obtained by the combustion reaction or flame hydrolysis reaction, the surface of which is hydrophobized. In the two-component curing epoxy resin composition of the present invention, the base agent contains fumed silica (E1) having a hydrophobicity degree of 55 or more and 75 or less, and the curing agent contains fumed silica (E2) having a hydrophobicity degree of 0 or more and less than 55. In this specification, the term "fumed silica (E)" means "fumed silica (E1) and fumed silica (E2)". The hydrophobicity of the fumed silica (E) in the present invention means the hydrophobicity by the methanol wettability method (methanol titration method), and is a value measured by the following method. The methanol wettability method evaluates the wettability with methanol, and the higher the hydrophobicity, the higher the hydrophobicity.

[0033] [Method for measuring the hydrophobicity of fumed silica (E)] 0.2 g of the silica particles to be measured (fumed silica) is weighed and added to 50 mL of distilled water in a 200 mL beaker. While stirring this with a magnetic stirrer at a speed of 150 rpm, methanol is slowly dripped from a burette with the tip immersed in the liquid until the entire silica particles are wet. The amount of methanol required to wet the entire silica particles is defined as Vm (mL), and the hydrophobicity is calculated using the following formula. The above phrase "the entire silica particles are wetted" means that the entire amount of the silica particles settles. Hydrophobicity = {Vm / (Vm+50)} x 100 For example, if the amount of methanol dropped Vm when the entire amount of silica particles has settled is 50 mL, the hydrophobicity of the silica particles is 50, and if the entire silica particles are wetted without dropping methanol, the hydrophobicity is 0. The larger the hydrophobicity number of the silica particles, the higher the hydrophobicity of the silica particles.

[0034] The hydrophobicity of the fumed silica (E) can be adjusted, for example, by the presence or absence of hydrophobic treatment of the silica particle surface, the type of surface treatment agent (organic silicon compound, etc., described later) used for the hydrophobic treatment, and the amount of the surface treatment agent used. Methods for increasing the hydrophobicity include using a surface treatment agent capable of introducing a highly hydrophobic surface modification group (long-chain alkylsilyl group, dimethylpolysiloxane group, etc.), and increasing the amount of the surface treatment agent used. Methods for decreasing the hydrophobicity include using a surface treatment agent capable of introducing a less hydrophobic surface modification group (containing a hydrophilic functional group, such as a methacryl group or an amino group), and decreasing the amount of the surface treatment agent used, but the hydrophobicity is lowest when no hydrophobic treatment is performed. As the above-mentioned surface treatment agent, an organosilicon compound can be suitably used. Representative organosilicon compounds include, in order of decreasing hydrophobicity, methacrylsilane {surface modifying group: methacryl group}, dimethyldichlorosilane {surface modifying group: dimethylsilyl group}, hexamethyldisilazane {surface modifying group: trimethylsilyl group}, monoalkylsilane {surface modifying group: alkylsilyl group (octylsilyl group, etc.)}, silicone oil {surface modifying group: dimethylpolysiloxane group}, and the like.

[0035] The fumed silica (E1) and the fumed silica (E2) can be produced by a known method, for example, by burning or hydrolyzing a silane compound in a flame formed by a combustible gas such as hydrogen gas and an oxygen-containing gas such as air, and then subjecting the surfaces of the resulting silica (silicon dioxide) particles to a hydrophobic treatment, if necessary, with a surface treatment agent (such as an organic silicon compound). Methods for hydrophobizing the surface treatment agent include a method in which the surface modifier is evaporated and brought into contact with the silica particles, a method in which the surface modifier is sprayed onto the surfaces of the silica particles with a spray or the like while the silica particles are flowing (dry contact method), and a method in which the surface modifier is dissolved in a specified solvent and the silica particles are dispersed in the solvent in which the surface modifier is dissolved.

[0036] As the fumed silica (E1) and the fumed silica (E2), commercially available products can be used. For example, the "AEROSIL (registered trademark)" series manufactured by Nippon Aerosil Co., Ltd., the "Reolosil (registered trademark)" series manufactured by Tokuyama Corporation, and the "Fumed Silica HDK (registered trademark)" series manufactured by Wacker Asahi Kasei Silicone Co., Ltd. can be suitably used. Commercially available products corresponding to fumed silica (E1) having a hydrophobicity of 55 or more and 75 or less include those whose particle surfaces have been hydrophobized with alkylsilanes [e.g., Aerosil R805 (surface treatment agent: alkylsilane, hydrophobicity: 55)], those whose particle surfaces have been hydrophobized with silicone oil (dimethylpolysiloxane) [e.g., Aerosil R202 (hydrophobicity: 70), Aerosil RY200 (hydrophobicity: 75), Aerosil RY200S (hydrophobicity: 75) and Aerosil RY300 (hydrophobicity: 75)], and those whose particle surfaces have trimethylsilyl groups derived from a surface treatment agent (trimethylsilane or hexamethyldisilazane) [e.g., Aerosil R812 (hydrophobicity: 60)], and the like. Commercially available products corresponding to fumed silica (E2) having a hydrophobicity of 0 or more and less than 55 include those that have not been hydrophobized [e.g., Aerosil 130, Aerosil 150, Aerosil 200, Aerosil 300 (all of which have a hydrophobicity of 0)], those whose particle surfaces have been hydrophobized with dimethyldichlorosilane [e.g., Aerosil R972 (hydrophobicity: 50)], and those whose particle surfaces have been hydrophobized with methacrylsilane [e.g., Aerosil R711 (hydrophobicity: 10) and Aerosil R7200 (hydrophobicity: 10)].

[0037] The hydrophobicity of the fumed silica (E1) contained in the base material of the two-component curing epoxy resin composition of the present invention is from 55 to 75. If the hydrophobicity is less than 55, it is difficult to adjust the thixotropic index and storage stability tends to deteriorate, while if it exceeds 75, it is not preferable from an industrial viewpoint. The hydrophobicity of (E1) contained in the base material is preferably from 55 to 70, more preferably from 60 to 70. The hydrophobicity of the fumed silica (E2) contained in the curing agent of the two-component curing type epoxy resin composition of the present invention is 0 or more and less than 55. If the hydrophobicity is 55 or more, the storage stability tends to deteriorate. The hydrophobicity of (E2) contained in the curing agent is preferably 0 or more and 50 or less.

[0038] Specific surface area (m2) of fumed silica (E) 2 / g) is preferably 50 to 400 m from the viewpoint of dispersibility in the epoxy resin composition. 2 / g, more preferably 100 to 300m 2 / g. The specific surface area of ​​the fumed silica (E) is a value measured by the BET method.

[0039] <Two-component curing epoxy resin composition> The two-component curing type epoxy resin composition of the present invention is a two-component curing type epoxy resin composition comprising a base agent containing the above-mentioned polyepoxy compound (A), inorganic filler (D), and fumed silica (E1) having a hydrophobicity of 55 or more and 75 or less, and a curing agent containing the above-mentioned (B), inorganic filler (D), and fumed silica (E2) having a hydrophobicity of 0 or more and less than 55, wherein the content of (B) in the curing agent is 10 to 40 parts by weight per 100 parts by weight of (A) in the base agent. If the content of (B) is less than 10 parts by weight per 100 parts by weight of (A), the heat resistance of the cured product will be insufficient, and if it exceeds 40 parts by weight, the workability will tend to deteriorate. The content of (B) per 100 parts by weight of (A) is preferably 12 to 35 parts by weight, more preferably 15 to 30 parts by weight, from the viewpoint of the heat resistance and workability of the cured product.

[0040] The weight ratio [D / A] of the (D) to the (A) in the base material is preferably 0.1 to 3.0, and more preferably 0.1 to 1.0, from the viewpoint of storage stability and the like. The weight ratio [D / (B+C)] of the weight of (D) in the curing agent to the total weight of (B) and (C) described below is preferably 0.1 to 3.0, and more preferably 0.1 to 1.0, from the viewpoint of storage stability, etc. The content of (D) in the two-component curing epoxy resin composition is preferably 10 to 50% by weight based on the weight of the epoxy resin composition, from the viewpoints of handleability and mechanical strength of the cured product.

[0041] The weight ratio [E1 / A] of the (E1) to the (A) in the base material is preferably 0.01 to 0.05 from the viewpoints of handling properties and storage stability. The weight ratio of the weight of the (E2) to the total weight of the (B) and (C) described below in the curing agent [E2 / (B+C)] is preferably 0.05 to 0.5 from the viewpoints of handling properties, storage stability, and the like. The content of (E) in the two-component curing epoxy resin composition [the total weight of (E1) and (E2)] is preferably 0.5 to 10% by weight, and more preferably 2 to 8% by weight, based on the weight of the epoxy resin composition, from the viewpoints of handleability, storage stability, and the like.

[0042] <Aliphatic polyamine (C)> The curing agent in the two-component curing epoxy resin composition of the present invention may further contain an aliphatic polyamine (C). By containing the aliphatic amine (C), the workability and pot life of the epoxy resin composition can be easily adjusted to a preferred range even at low temperatures. The aliphatic polyamine (C) in the present invention has 2 to 50 active hydrogens directly bonded to N atoms, and includes the following (C1) to (C11) and mixtures of two or more of these, provided that the following polyalkylene polyamine (C1) is a polyalkylene polyamine other than the polyalkylene polyamine (b1) constituting the above (B).

[0043] (C1): Polyalkylene polyamine polyalkylene polyamines having 2 or more carbon atoms and a number average molecular weight (hereinafter sometimes referred to as Mn) of 500 or less, other than the polyalkylene polyamine (b1) constituting the reactant (B), such as alkylene diamines having 2 to 12 carbon atoms (ethylene diamine, propylene diamine, trimethylene diamine, tetramethylene diamine, hexamethylene diamine, etc.) and polyalkylene (alkylene group having 2 to 10 carbon atoms) poly(trivalent to hexavalent or higher) amines [diethylene triamine, imino bis propyl amine, bis (hexamethylene) triamine, triethylene tetramine, tetraethylene pentamine, pentaethylene hexamine, hexaethylene heptamine, etc.];

[0044] (C2): Aliphatic polyamine other than (C1) Alkyl (alkyl group has 1 to 4 carbon atoms) or hydroxyalkyl (alkyl group has 2 to 4 carbon atoms) substituted derivatives of the above (C1), such as dialkyl (alkyl group has 1 to 3 carbon atoms) aminopropylamine, trimethylhexamethylenediamine, aminoethylethanolamine, 2,5-dimethyl-2,5-hexamethylenediamine, methyliminobispropylamine and N,N'-di-n-butyl-1,6-hexanediamine;

[0045] (C3) Alicyclic-containing poly(di- or trivalent)amine Those having 4 to 15 carbon atoms, such as 1,3-diaminocyclohexane, 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, menthenediamine and 4,4'-methylenedicyclohexanediamine (hydrogenated methylenedianiline);

[0046] (C4) Heterocycle-containing poly(di- or trivalent)amine those having 4 to 15 carbon atoms, such as piperazine, N-aminoethylpiperazine, 1,4-diaminoethylpiperazine and 1,4-bis(2-amino-2-methylpropyl)piperazine;

[0047] (C5) Aromatic ring-containing polyamine Those having 8 to 15 carbon atoms, such as xylylenediamine, tetrachloro-p-xylylenediamine, and styrene adducts of xylylenediamine;

[0048] (C6) Polyamidepolyamine having an imidazoline ring Those having a molecular weight of 200 or more and an Mn of 1,000 or less and having one or more imidazoline ring structures in the molecule, such as those available on the market under the trade name "Polymide L4051 (manufactured by Sanyo Chemical Industries, Ltd.)";

[0049] (C7): Polyamide polyamine other than (C6) Those with a molecular weight of 200 or more and Mn of 1,000 or less, such as polyamidepolyamines obtained by condensation of dicarboxylic acids (dimer acids, etc.) with an excess of [2 or more equivalents of the above (C1) or the like per equivalent of carboxyl group], except for those falling under the above (C6);

[0050] (C8) Polyether polyamine Those with a molecular weight of 100 or more and Mn of 1,000 or less, such as hydrogenated cyanoethylated polyether polyols [such as the above-mentioned polyalkylene glycols];

[0051] (C9) Epoxy-added polyamine The epoxy-added polyamine is one having a molecular weight of 100 or more and an Mn of 1,000 or less, for example, a reaction product of 1 mole of an epoxy compound with 1 to 30 moles of the above (C1) [a reaction product of 1 mole of an epoxy compound [the above polyepoxy compound (A) and a monoepoxide (butyl glycidyl ether, phenyl glycidyl ether, etc.)] with 1 to 30 moles of the above (C1) (molecular weight of 100 or more and Mn of 1,000 or less), etc.], other than the epoxy-added polyamine contained in the reaction product (B) of 1 mole of a polyalkylene polyamine with 0.05 to 0.35 moles of bisphenol A diglycidyl ether.

[0052] (C10) Cyanoethylated Polyamines Those with a molecular weight of 100 or more and Mn of 500 or less, such as the reaction product of acrylonitrile with the above (C1) (biscyanoethyldiethylenetriamine, etc.);

[0053] (C11) Other polyamines Hydrazine compounds (those with a molecular weight of 32 or more and Mn of 500 or less, such as hydrazine and monoalkylhydrazine), dihydrazide compounds [those with a molecular weight of 74 or more and Mn of 1,000 or less, such as dihydrazides of acids (succinic acid, adipic acid, isophthalic acid, terephthalic acid, etc.)] and guanidine compounds (those with a molecular weight of 59 or more and Mn of 500 or less, such as butylguanidine and 1-cyanoguanidine), etc.

[0054] From the viewpoints of adhesion (adhesion under normal temperature and high temperature conditions) and heat resistance of the cured product, it is preferable that the aliphatic polyamine (C) further contains a polyamidepolyamine (C6) having an imidazoline ring, and it is particularly preferable that the content of (C6) is 5 to 75% by weight based on the weight of the aliphatic polyamine (C).

[0055] The number average molecular weight of the aliphatic polyamine (C) is preferably 100-1,500, more preferably 100-800, and particularly preferably 100-500, from the viewpoint of handleability. In the present invention, the number average molecular weight of the aliphatic polyamine (C) is the molecular weight calculated from the chemical formula when (C) is a single compound, and is the value obtained by adding up the products of the molecular weights calculated from the chemical formulas of each compound and the ratio of the number of molecules of each compound (molar ratio) when (C) is a mixture of two or more compounds.

[0056] From the viewpoints of pot life and heat resistance of the cured product, the active hydrogen equivalent of the aliphatic polyamine (C) is preferably from 30 to 200 g / eq, and more preferably from 40 to 180 g / eq. In the present invention, the active hydrogen equivalent of (C) means the molecular weight per active hydrogen (hydrogen atom directly bonded to a N atom) possessed by (C). From the viewpoint of heat resistance of the cured product, the active hydrogen equivalent of the amine contained in the curing agent is preferably 60 g / eq or less, and more preferably 50 g / eq or less. The active hydrogen equivalent of the amine contained in the curing agent is the weighted average of the active hydrogen equivalents of (B) and (C) contained in the curing agent, calculated by the content (parts by weight) of each component.

[0057] When the curing agent for the epoxy resin composition of the present invention contains an aliphatic polyamine (C), the contents of (B) and (C) in the curing agent are preferably as follows, based on the weight of the curing agent. From the viewpoint of heat resistance, the content of (B) is preferably 20 to 80% by weight, more preferably 20 to 70% by weight, and particularly preferably 30 to 60% by weight. The content of (C) is preferably 5 to 30% by weight, and more preferably 5 to 20% by weight, from the viewpoints of workability at low temperatures and pot life.

[0058] The contents of (A), (B) and (C) in the epoxy resin composition of the present invention are preferably as follows, based on the total weight of (A), (B) and (C): From the viewpoints of the workability of the epoxy resin composition and the heat resistance of the cured product, the content of (A) is preferably 40 to 70% by weight, more preferably 45 to 68% by weight, and particularly preferably 50 to 65% by weight. From the viewpoints of the heat resistance and workability of the epoxy resin composition, the content of (B) is preferably 5 to 40% by weight, more preferably 7 to 35% by weight, and particularly preferably 11 to 30% by weight. From the viewpoints of the workability of the epoxy resin composition and the heat resistance of the cured product, the content of (C) is preferably 1 to 10% by weight, more preferably 2 to 10% by weight, and particularly preferably 3 to 10% by weight.

[0059] The molar ratio of the epoxy groups of (A) in the base resin to the active hydrogens of (B) and (C) in the curing agent (active hydrogens directly bonded to N atoms of (B) and (C)) [active hydrogens / epoxy groups] is preferably 0.5 to 2.0, more preferably 0.8 to 1.5, and particularly preferably 1.0 to 1.2, from the viewpoint of the physical properties (mechanical strength) of the cured product.

[0060] <Monofunctional epoxide (F)> The epoxy resin composition of the present invention may further contain a monofunctional epoxide (F) having one epoxy group in the molecule. By containing (F), it may be easier to adjust the viscosity and pot life of the epoxy resin composition. (F) is not particularly limited as long as it is a compound having one epoxy group in the molecule, but examples of (F) include alkyl monoglycidyl ethers (butyl glycidyl ether, 2-ethylhexyl glycidyl ether, etc.), allyl glycidyl ether, glycerol monoglycidyl ether, alkylphenol monoglycidyl ether, styrene oxide, phenyl glycidyl ether, cresyl glycidyl ether, glycidyl methacrylate, and mixtures of two or more of these.

[0061] The amount of the monofunctional epoxide (F) used is preferably 3% by weight or less based on the total weight of (A), (B) and (C) from the viewpoint of the heat resistance of the cured product of the epoxy resin composition.

[0062] The epoxy resin composition of the present invention may further contain, as necessary, within a range that does not impair the effects of the present invention, (1) curing accelerators (tertiary amino compounds, alkali compounds other than the above (B) and (C), Lewis base compounds, phenol group-containing compounds, etc.), (2) adhesion promoters (titanium coupling agents, etc.), (3) antioxidants (hindered amines, hydroquinones, hindered phenols, sulfur-containing compounds, etc.), (4) ultraviolet absorbers (benzophenones, benzotriazoles, salicylic acid esters, metal complex salts, etc.), (5) plasticizers (phthalic acid esters, phosphate esters, fatty acid esters, epoxidized soybean oil, castor oil, liquid paraffin alkyl polycyclic aromatic hydrocarbons, etc.), (6) waxes (paraffin wax, microcrystalline wax, polymerized wax, beeswax, spermaceti wax, low molecular weight polyolefins, etc.), and (7) carboxylic acids (carboxylic acids, ... (7) non-reactive diluents (benzyl alcohol, tar, picumen, etc.), (8) reactive diluents (low molecular weight aliphatic glycidyl ethers, aromatic monoglycidyl ethers, etc.), (9) organic fillers [aramid fiber powder, nylon fiber powder, acrylic fiber powder, acrylic resin powder, phenolic resin powder, etc.], (10) deodorants [activated carbon, zeolite, etc.], (11) pigments or dyes [carbon black, red lead, para red, Prussian blue, etc.], (12) thixotropic agents [bentonite, hydrogenated castor oil wax, calcium stearate, etc.], (13) solvents (ethyl acetate, toluene, alcohol, ether, ketone, etc.), (14) foaming agents, (15) defoamers, (16) antistatic agents, (17) antibacterial agents, (18) fungicides, (19) viscosity modifiers, (20) fragrances, and (21) flame retardants. (G)

[0063] The epoxy resin composition of the present invention can be produced and used in the following manner. The epoxy resin composition is prepared separately in the form of two liquids [a base agent containing (A), (D) and (E1) and a curing agent containing (B), (D) and (E2)] and mixed at the time of use to obtain an epoxy resin composition. (C), which is added as needed, is preferably mixed in advance with the curing agent. (F) and (G), which are added as needed, are preferably mixed in advance with the base agent and / or the curing agent from the viewpoints of the curability and workability of the composition. In the present invention, the method for mixing (A), (B), (D), and (E), and optionally containing (C), (F), and (G), is not particularly limited, and examples thereof include a method using a mixer such as a universal mixer and a method using a mixer.

[0064] The initial viscosity (Pa·s) of the epoxy resin composition of the present invention at 25° C. is preferably 100 Pa·s or less, and more preferably 20 to 70 Pa·s, from the viewpoint of workability (injectability, filling property, etc.). The initial viscosity (Pa·s) at 5° C. is preferably 200 Pa·s or less, and more preferably 70 to 180 Pa·s. The initial viscosity of an epoxy resin composition refers to the viscosity measured after the base agent and the curing agent are adjusted to a predetermined temperature, the base agent and the curing agent are mixed in a predetermined mixing ratio and mixed for 2 minutes, and then the viscosity is set in a B-type viscometer and measured several minutes later (e.g., 6 minutes after the start of mixing) while the temperature is adjusted to the predetermined temperature in a thermostatic bath.

[0065] The initial viscosity can be measured, for example, under the following conditions. Equipment: BH type viscometer [Model number "TVB-22H", manufactured by Toki Sangyo Co., Ltd.] Rotation speed: 20 rpm Spindle No.: No. 7

[0066] The thixotropic index of the base material of the epoxy resin composition of the present invention is preferably 5 to 8 from the viewpoint of storage stability, etc. Also, the thixotropic index of the curing agent of the epoxy resin composition of the present invention is preferably 4 to 8 from the viewpoint of storage stability, etc. The thixotropic index in the present invention is the value obtained by dividing the viscosity (mPa s) measured at 25°C using a Brookfield viscometer at a rotation speed of 2 rpm by the viscosity (mPa s) measured at 25°C using a Brookfield viscometer at a rotation speed of 20 rpm [viscosity measured at 2 rpm (mPa s) / viscosity measured at 20 rpm (mPa s)]. The thixotropic index of the base resin tends to increase by increasing the hydrophobicity of the fumed silica (E1) and by increasing the amount of fumed silica (E1) added. The thixotropic index of the epoxy resin composition can be adjusted to the above-mentioned range by adjusting the hydrophobicity and the amount of the fumed silica (E) added, and by selecting the type of the aliphatic polyamine (C) used, if necessary. However, in the case of using an aliphatic polyamine (C) having a functional group capable of interacting with the silanol group of the fumed silica (E), the opposite tendency may be observed.

[0067] <Cured product obtained by curing two-component curing type epoxy resin composition> The cured product of the present invention is a cured product obtained by curing the above-mentioned epoxy resin composition. It can be obtained by mixing the base agent containing the above-mentioned (A), (D) and (E1) with the curing agent containing the above-mentioned (B), (D) and (E2) as described above, and curing it as necessary to proceed with the curing reaction. When used as a civil engineering and construction adhesive, since it is applied on-site without temperature control, the curing temperature is not particularly limited, but is preferably 5 to 40°C, and more preferably 15 to 30°C. The curing time of the epoxy resin composition at 5 to 40° C. is preferably 100 to 340 hours, and more preferably 120 to 240 hours. The curing time means the time required for the resin strength (compressive strength at 25°C) to reach the strength required for practical use (for example, 60 MPa or more when used as a civil engineering and construction adhesive) when cured at a specified temperature. The compressive strength at 25°C can be measured in accordance with JIS K 7181.

[0068] The Tg (glass transition temperature) Tg1 of the cured product (the cured product of the first-stage curing reaction) obtained by curing the epoxy resin composition of the present invention at 25°C for 5 days is preferably 40 to 80°C, and more preferably 70 to 80°C, from the viewpoint of mechanical strength, etc. Furthermore, the cured product obtained by further heating the cured product at high temperature (at 100°C for 180 minutes) to cure (the cured product of the second-stage curing reaction; hereinafter, sometimes referred to as a completely cured product) has a Tg of Tg2, which is the Tg of the cured product, and the above Tg1 (Tg2 / Tg1), from the viewpoint of heat resistance, preferably from 1.2 to 4.0, more preferably from 1.5 to 4.0, and particularly preferably from 2.0 to 4.0. The (Tg2 / Tg1) ratio can be adjusted to fall within the above range mainly by adjusting Tg2. Specifically, Tg2 can be increased by, for example, decreasing the epoxy equivalent of the polyepoxy compound (A), decreasing the active hydrogen equivalent of (C), or increasing the content of aromatic ring structures or structures that form hydrogen bonds in the polyepoxy compounds (A) and (C). In the present invention, Tg means the temperature at which the loss tangent (tan δ=loss modulus / storage modulus) becomes maximum when the temperature dependency of dynamic viscoelasticity is measured under the conditions described below.

[0069] The compressive strength P1 at 25°C of the cured product (the cured product of the first-stage curing reaction) obtained by curing the epoxy resin composition of the present invention at the above-mentioned curing temperature (25°C) for 5 days is preferably 60 to 120 MPa, and more preferably 70 to 120 MPa, from the viewpoint of mechanical strength, etc. In addition, the temperature for heat resistance testing (T h The strength retention (%) of the cured product at high temperatures calculated by the following formula from P2, which is the compressive strength of the cured product at 200° C., and the above P1, is preferably 50% or more, and more preferably 60% or more. Strength retention rate of cured material at high temperatures (%) = (P2 / P1) x 100 In addition, the temperature of the above heat resistance test (T h When used in civil engineering and construction applications, the heat resistance or fire resistance standards are set according to the structure of the building and the location where it is used. For example, when used in wooden buildings, wood contains water, so the temperature rise during a fire is relatively gradual and the temperature reached inside the wood is around 100°C. h is, for example, 100°C. The strength retention rate of the cured product at high temperatures is such that the ratio of Tg2 to Tg1 (Tg2 / Tg1) falls within the above-mentioned preferred range and the above-mentioned Tg2 is the temperature of the heat resistance test (T h The Tg2 and (Tg2 / Tg1) ratio can be adjusted by the above-mentioned methods. The compressive strength of the cured product in the present invention can be measured in accordance with JIS K 7181 by the method described below.

[0070] The two-component curing epoxy resin composition of the present invention has sufficient pot life and good workability (injectability, filling property, etc.) even at low temperatures, and is also excellent in storage stability and heat resistance of the cured product, so it can be used for various applications such as adhesives, resin fillers, and molded products, and is particularly suitable for use as adhesives and resin fillers for civil engineering and construction. Furthermore, since the cured product has high heat resistance (high strength retention rate at high temperatures, and the adhesive strength between members bonded with the epoxy resin composition is maintained even at high temperatures), it is particularly useful as an adhesive for the GIR method in wooden buildings where heat resistance and fire resistance are required. The GIR (glued-in rod) method is a method of bonding wood pieces together by drilling holes in wood, inserting a connector such as a steel rod into the hole, injecting and filling the void with a resin adhesive, and then curing it.

[0071] The epoxy resin composition of the present invention can also be used as an adhesive and resin filler for civil engineering and construction other than the GIR method (for repair and reinforcement work of structures such as concrete structures and steel structures, crack injection, adhesive for post-installed anchors, etc.), and is particularly useful as an adhesive for post-installed anchors. The term "post-installed anchor" refers to a construction method in which an anchor member such as an anchor bolt or a reinforcing bar is embedded in an already manufactured concrete structure (hereinafter referred to as a base material) in the fields of civil engineering, architecture, machinery, etc., and the epoxy resin composition of the present invention can be used as an adhesive between the base material and the metal anchor member when embedding the metal anchor member in the base material. Specifically, the anchor member is inserted into a hole drilled in the base material, and the epoxy resin composition of the present invention is poured into the hole, thereby firmly bonding the hole wall and the anchor member. As described above, the epoxy resin composition of the present invention gives a cured product with excellent heat resistance and fire resistance, so that the resin strength and the adhesive strength between the joined members can be maintained even when the temperature rises due to a fire or the like.

[0072] The present specification discloses the following:

[0073] The present disclosure (1) is a two-component curing type epoxy resin composition comprising a base material containing a polyepoxy compound (A) that is liquid at 5°C, an inorganic filler (D), and fumed silica (E1) having a hydrophobicity of 55 or more and 75 or less, and a curing agent containing a reaction product (B) of 1 mole of polyalkylene polyamine and 0.05 to 0.35 moles of bisphenol A diglycidyl ether, an inorganic filler (D), and fumed silica (E2) having a hydrophobicity of 0 or more and less than 55, wherein the content of (B) in the curing agent is 10 to 40 parts by weight per 100 parts by weight of (A) in the base material.

[0074] The present disclosure (2) is the two-component curing type epoxy resin composition according to the present disclosure (1), in which the viscosity of (B) at 25° C. is 500 to 400,000 mPa·s.

[0075] The present disclosure (3) is the two-component curing type epoxy resin composition according to the present disclosure (1) or (2), in which (B) contains a reaction product of pentaethylenehexamine and bisphenol A diglycidyl ether.

[0076] The present disclosure (4) is a two-component curing type epoxy resin composition in any combination with any of the present disclosures (1) to (3), wherein the curing agent further contains an aliphatic polyamine (C), the number average molecular weight of the (C) is 100 to 1500, and the active hydrogen equivalent of the (C) is 30 to 200 g / eq.

[0077] The present disclosure (5) is a two-component curing type epoxy resin composition which is an adhesive for civil engineering and construction, and is any combination with any of the present disclosures (1) to (4).

[0078] The present disclosure (6) is a cured product obtained by curing the two-component curing type epoxy resin composition according to any one of the present disclosures (1) to (5). EXAMPLES

[0079] The present invention will be further described below with reference to examples, but the present invention is not limited to these.

[0080] <Production Example 1: Production of (B-1)> At room temperature, 37.8 g (0.10 mmol) of bisphenol A glycidyl ether was added to 454 g (1.96 mmol) of pentaethylenehexamine (b1-1), and the mixture was stirred for 5 minutes using a stirrer. The reaction temperature was then raised to 40°C and the mixture was allowed to react for 1 hour to obtain (B-1), a reaction product of pentaethylenehexamine and bisphenol A diglycidyl ether (the number of moles of bisphenol A diglycidyl ether reacted per mole of pentaethylenehexamine was 0.05). The viscosity of (B-1) at 25°C was measured using a BH type viscometer [model number "TVB-22H", manufactured by Toki Sangyo Co., Ltd.] at a rotation speed of 50 rpm and spindle No. 5, and was 500 mPa·s.

[0081] <Production Examples 2 to 7: Production of (B-2) to (B-7)> (B-2) to (B-7) were obtained in the same manner as in Production Example 1, except that the raw materials (g: grams) shown in Table 1 were used. The number of moles of bisphenol A diglycidyl ether reacted with 1 mole of polyalkylene polyamine (b1) in each of the obtained (B) and the viscosity (mPa s) at 25°C are shown in Table 1. The viscosity of each (B) was measured using the same viscometer as in Production Example 1, changing the spindle No. and rotation speed according to the viscosity as necessary.

[0082] <Comparative Preparation Example 1: Preparation of (Comparative B-1)> A comparative compound (Comparative B-1), which is a reaction product of pentaethylenehexamine and bisphenol A diglycidyl ether (the number of moles of bisphenol A diglycidyl ether reacted per mole of pentaethylenehexamine is 0.39 moles), was obtained in the same manner as in Production Example 1, except that the weight of pentaethylenehexamine (b1-1) was changed to 60.0 g (0.26 mmol) and the weight of bisphenol A glycidyl ether was changed to 37.8 g (0.1 mmol). The viscosity of (Comparative B-1) at 25°C was measured using a BH type viscometer [model number "TVB-22H", manufactured by Toki Sangyo Co., Ltd.] at a rotation speed of 2 rpm and spindle No. 7, and was 840,000 mPa·s.

[0083] [Table 1]

[0084] The abbreviations in Table 1 are as follows. <Polyalkylenepolyamine (b1)> b1-1: Pentaethylenehexamine [Product name: Pentaethylenehexamine, manufactured by Tosoh Corporation, active hydrogen equivalent: 29 g / eq, number of active hydrogen atoms directly bonded to N atoms: 8] b1-2: diethylenetriamine [Product name: Diethylenetriamine, manufactured by Tosoh Corporation, active hydrogen equivalent: 21 g / eq, number of active hydrogen atoms directly bonded to N atoms: 5] b1-3: ethylenediamine [Product name: "Ethylenediamine", manufactured by Tosoh Corporation, active hydrogen equivalent: 15g / eq, number of active hydrogen atoms directly bonded to N atoms: 4]

[0085] <Example 1: Preparation of two-component curing type epoxy resin composition (X-1)> Using a universal mixer [trade name "Universal Mixer 5DMV-01-r", Dalton Co., Ltd.], 72.0 parts by weight of bisphenol F diglycidyl ether (A-2), 3.0 parts by weight of neopentyl glycol diglycidyl ether (A-3), 3.0 parts by weight of trimethylolpropane polyglycidyl ether (A-4), 20.0 parts by weight of calcium carbonate (D-1) and 2.0 parts by weight of Aerosil RY200S (E1-2) were mixed under reduced pressure while defoaming (temperature 25°C, stirring time 60 minutes, pressure 4 kPa) to obtain a base agent. In addition, 15.6 parts by weight of (B-1), 15.8 parts by weight of calcium carbonate (D-1) and 4.0 parts by weight of Aerosil 972 (E2-2) were mixed under reduced pressure while defoaming (temperature 25°C, stirring time 60 minutes, pressure 4 kPa) to obtain a curing agent. The obtained base resins and curing agents were mixed (temperature 25°C, stirring time 3 minutes, rotation speed 1400 rpm) using a centrifugal defoamer (product name "Awatori Rentaro ARV930TWIN", manufactured by Thinky Corporation) to obtain an epoxy resin composition (X-1).

[0086] <Examples 2 to 19: Production of two-component curing type epoxy resin compositions (X-2) to (X-19)> Each base agent and each curing agent were obtained in the same manner as in Example 1, except that the raw materials (parts by weight) for each Example were used as shown in Table 2. Next, each base agent and each curing agent obtained were mixed (temperature 25°C, mixing time 3 minutes, rotation speed 1400 rpm) using a centrifugal defoamer [product name "Awatori Rentaro ARV930TWIN", manufactured by Thinky Corporation] to obtain epoxy resin compositions (X-2) to (X-19).

[0087] [Table 2]

[0088] <Comparative Examples 1 to 8: Production of Comparative Epoxy Resin Compositions (Comparative X-1) to (Comparative X-8)> For each comparative example, each base agent and each curing agent were obtained in the same manner as in Example 1, except that the raw materials (parts by weight) shown in Table 3 were used. Next, each of the base agents and curing agents obtained was mixed (temperature 25°C, mixing time 3 minutes, rotation speed 1400 rpm) using a centrifugal defoamer [product name "Awatori Rentaro ARV930TWIN", manufactured by Thinky Corporation] to obtain epoxy resin compositions (Comparative X-1) to (Comparative X-8).

[0089] [Table 3]

[0090] The abbreviations in Tables 2 and 3 are as follows. <Polyepoxy compound (A)> A-1: Bisphenol A diglycidyl ether [Product name: Epomic R140, manufactured by Mitsui Fine Chemicals, Inc., epoxy equivalent: 190g / eq] A-2: Bisphenol F diglycidyl ether [Product name "jER807", manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 175g / eq] A-3: Neopentyl glycol diglycidyl ether [Product name: "Denacol Ex-211", Nagase ChemteX Corporation, epoxy equivalent: 138g / eq] A-4: Trimethylolpropane polyglycidyl ether [Product name: "Denacol Ex-321", Nagase ChemteX Corporation, epoxy equivalent 140g / eq, mixture of epoxy groups with 2 and 3 in the molecule]

[0091] <(B) and ratio (B)> B-1: Obtained in Production Example 1 B-2: Obtained in Production Example 2 B-3: Obtained in Manufacturing Example 3 B-4: Obtained in Manufacturing Example 4 B-5: Obtained in Manufacturing Example 5 B-6: Obtained in Production Example 6 B-7: Obtained in Manufacturing Example 7 Comparison B-1: Obtained in Comparative Example 1 Ratio B-2: Pentaethylenehexamine [product name "Pentaethylenehexamine", manufactured by Tosoh Corporation, viscosity (25°C) 143 mPa·s, active hydrogen equivalent 29 g / eq]

[0092] <Aliphatic polyamine (C)> C-1: Polyamide polyamine having an imidazoline ring [Product name: Polymide L4051, manufactured by Sanyo Chemical Industries, Ltd., active hydrogen equivalent: 103 g / eq, number of active hydrogen atoms directly bonded to N atoms: 6, number average molecular weight: 470] C-2: Styrene adduct of xylylenediamine [Product name: Gaskamine ST 240, manufactured by Mitsubishi Gas Chemical Co., Ltd., active hydrogen equivalent: 103 g / eq, 2-3 active hydrogen atoms directly bonded to N atoms, number average molecular weight: 258] C-3: Xylylenediamine [Product name: Ankamine 2422, manufactured by Air Products Japan Co., Ltd., active hydrogen equivalent: 34 g / eq, number of active hydrogen atoms directly bonded to N atoms: 4, number average molecular weight: 136] C-4: 1,3-bis(aminomethyl)cyclohexane [Product name "1,3-BAC", manufactured by Mitsubishi Gas Chemical Co., Ltd., active hydrogen equivalent 36g / eq, number of active hydrogen atoms directly bonded to N atoms 4, number average molecular weight 142] C-5: Polyamide polyamine without imidazoline ring [Product name: Polymide L-15-3, manufactured by Sanyo Chemical Industries, Ltd., active hydrogen equivalent: 170 g / eq, number of active hydrogen atoms directly bonded to N atoms: 8 to 14, number average molecular weight: 1412]

[0093] <Inorganic filler (D)> D-1: Calcium carbonate [Product name "Softon 1200", manufactured by Shiraishi Calcium Co., Ltd., volume average particle size 1.8 μm] <Fumed silica (E1) with a hydrophobicity of 50 to 70> E1-1: Aerosil 805 [Product name: AEROSIL 805, manufactured by Nippon Aerosil Co., Ltd., hydrophobicity degree 55, specific surface area 200 m 2 / g] E1-2: Aerosil RY200S [Product name: AEROSIL RY200S, manufactured by Nippon Aerosil Co., Ltd., hydrophobicity level 70, specific surface area 130 m 2 / g] <Fumed silica (E2) with a hydrophobicity of 0 to 50> E2-1: Aerosil 200 [Product name: AEROSIL 200, manufactured by Nippon Aerosil Co., Ltd., hydrophobicity level 0, specific surface area 200 m 2 / g] E2-2: Aerosil R972 [Product name: AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd., hydrophobicity degree 50, specific surface area 130 m 2 / g]

[0094] The performance of each resin composition obtained in the Examples and Comparative Examples was evaluated by the following test methods. The initial viscosity (1) and (2) and the pot life (3) were measured by mixing each of the base agents and curing agents obtained above by the following methods. The thixotropic index (4) and storage stability (separation resistance) were measured by the following methods before mixing each of the base agents and curing agents obtained above. The measurement and evaluation results are shown in Tables 2 and 3.

[0095] <Test Method> (1) Initial viscosity (5°C) [unit: Pa s] After adjusting the temperature of the base agent and curing agent to 5°C, they were mixed for 2 minutes to a total of 120 g in the mixing ratios shown in Table 2 or Table 3 for each Example and Comparative Example. The viscosity of the resulting mixture (epoxy resin composition) was measured under the following conditions using a BH type viscometer [model number "TVB-22H", manufactured by Toki Sangyo Co., Ltd.] while adjusting the temperature in a thermostatic bath at 5°C, and the viscosity (Pa s) was measured 6 minutes after starting to mix the base agent and curing agent. <Measurement conditions> Temperature: 5℃ Rotation speed: 20 rpm Spindle No.: No. 7 When used as an adhesive for the GIR method in wooden buildings, the initial viscosity (Pa·s) at 5° C. must be 200 Pa·s or less, and is preferably 70 to 180 Pa·s.

[0096] Initial viscosity (25℃) [unit: Pa s] The initial viscosity (Pa s) at 25°C was measured in the same manner as in (1) above, except that the temperature was changed to 25°C. When used as an adhesive for the GIR method in wooden buildings, the initial viscosity (Pa s) at 25°C must be 100 Pa s or less, and is preferably 20 to 70 Pa s.

[0097] Pot life [unit: min] After measuring the initial viscosity (25°C) in (2) above, the viscosity was measured using a BH type viscometer [model number "TVB-22H", manufactured by Toki Sangyo Co., Ltd.] while controlling the temperature in a thermostatic bath at 25°C, and the time from the start of the initial viscosity measurement (6 minutes after the start of mixing the base agent and hardener) until the viscosity reached 200 (Pa·s) was defined as the pot life (minutes). When used as an adhesive for the GIR method in wooden buildings, the pot life must be 15 minutes or more from the viewpoint of workability, and is preferably 15 to 190 minutes, and more preferably 20 to 80 minutes.

[0098] Thixotropic index (25℃) Before mixing, the viscosity of each base agent and each hardener was measured using a BH type viscometer [model number "TVB-22H", manufactured by Toki Sangyo Co., Ltd.] under the following condition A while controlling the temperature in a thermostatic bath at 25°C, and this was recorded as "viscosity (mPa s) measured at a rotation speed of 2 rpm." Next, the viscosity was measured under the following condition B, and this was recorded as "viscosity (mPa s) measured at a rotation speed of 20 rpm." The thixotropic index (25°C) of each base resin and each curing agent was calculated using the following formula. Thixotropic index (25°C) = [viscosity measured at a rotation speed of 2 rpm (mPa s) / viscosity measured at a rotation speed of 20 rpm (mPa s)] <Measurement condition A> Temperature: 25℃ Rotation speed: 2rpm Spindle No.: No. 7 <Measurement condition B> Temperature: 25℃ Rotation speed: 20rpm Spindle No.: No. 7 The thixotropic index of the base material of the epoxy resin composition of the present invention is preferably 5 to 8 from the viewpoint of storage stability, etc. Also, the thixotropic index of the curing agent of the epoxy resin composition of the present invention is preferably 4 to 8 from the viewpoint of storage stability, etc.

[0099] (5) Storage stability (separation resistance) After adjusting the temperature of each base agent and each hardener before mixing to 25℃, 50g of each was placed in a centrifuge tube and centrifuged at 2000rpm for 30 minutes using a centrifuge [tabletop centrifuge "H-36", manufactured by Kokusan Co., Ltd.]. The appearance was visually observed every 30 minutes to confirm whether or not the inorganic filler (D) had settled in each base agent and each hardener. The time (minutes) until the settling of (D) occurred was judged based on the following evaluation criteria, and the results are shown in Tables 2 and 3. This test, which involves centrifugation at a rotation speed of 2000 rpm for 30 minutes, is an accelerated test that reproduces the separation properties observed when the sample is stored for two months under normal storage conditions (25°C, static). <Evaluation criteria> ◎: 180 minutes or more ○: 120 minutes or more, less than 180 minutes △: 60 minutes or more, less than 120 minutes ×: Less than 60 minutes

[0100] (6) Tg1: Tg of the cured product (cured product of the first curing reaction) obtained by curing at 25°C for 5 days [unit: °C] The kneaded epoxy resin composition was molded into a plate with a thickness of about 10 mm and cured at 25° C. for 5 days. After curing, a rectangular parallelepiped test piece with a thickness of about 10 mm, a width of about 10 mm, and a length of about 3 mm was cut out, and the storage modulus E' and loss modulus E" were measured using a dynamic viscoelasticity device (Rheogel-E4000, manufactured by UBM Co., Ltd.) under conditions of a fundamental frequency of 1 Hz and a heating rate of 5° C. / min. The temperature at which E" / E' (tan δ) was maximum was defined as Tg1.

[0101] (7) Tg2: Tg of the cured product (completely cured product) after heating at high temperature (100°C) [unit: °C] The kneaded epoxy resin composition was molded into a plate with a thickness of about 10 mm, cured at 25°C for 5 days, and then heated in a thermostatic bath at 100°C for 60 minutes. After cooling at 25°C for 3 hours, a rectangular parallelepiped test piece with a thickness of about 10 mm, a width of about 10 mm, and a length of about 3 mm was cut out, and the storage modulus E' and loss modulus E" were measured using a dynamic viscoelasticity device (Rheogel-E4000, manufactured by UBM Co., Ltd.) under conditions of a fundamental frequency of 1 Hz and a heating rate of 5°C / min. The temperature at which E" / E' (tan δ) was at its maximum was defined as Tg2.

[0102] (8) P1: Compressive strength (compressive yield strength) at 25°C of the hardened product (hardened product of the first stage hardening reaction) obtained by hardening at 25°C for 5 days, [unit: MPa] The kneaded epoxy resin composition was molded into a plate with a thickness of about 10 mm, and cured by aging at 25°C for 5 days. A rectangular parallelepiped test piece with a thickness of about 10 mm, width of about 10 mm, and length of about 30 mm was cut out, and measurements were performed in a thermostatic chamber at 25°C using a universal material testing machine [AG-50kNXplus, manufactured by Shimadzu Corporation] in accordance with JIS K7181, except that the test speed was changed to 2 mm / min.

[0103] (9) P2: Compressive strength (compressive yield strength) of the cured material at heat resistance test temperature (test temperature 100°C), [unit: MPa] The kneaded epoxy resin composition was molded into a plate with a thickness of about 10 mm, and cured at 25°C for 5 days. A rectangular parallelepiped test piece with a thickness of about 10 mm, width of about 10 mm, and length of about 15 mm was cut out and left to stand for 1 hour in a thermostatic chamber set at a temperature of 100°C. After that, while controlling the temperature in the thermostatic chamber to 100°C, measurements were performed in accordance with JIS K7181 using a universal material testing machine [AG-50kNXplus, manufactured by Shimadzu Corporation], except that the test speed was changed to 2 mm / min.

[0104] (10) Strength retention of the cured product at high temperatures For each Example, the strength retention (%) of the cured product at high temperatures was calculated from the P1 and P2 measured above according to the following formula. Strength retention rate of cured material at high temperatures (%) = (P2 / P1) x 100

[0105] (11) Adhesive strength between steel plates (lap shear adhesive strength) (25°C) [unit: MPa] Cold-rolled steel plates of about 1.6 mm thick × about 25 mm wide × about 100 mm long as specified in JIS G3141 were washed with acetone, and two cold-rolled steel plates were bonded with each epoxy resin composition kneaded so that the overlap length was 12.5 mm and the thickness of the adhesive layer was 0.2 mm to obtain test pieces (curing conditions: 5 days of curing at 25°C). After curing, the adhesive strength (lap shear adhesive strength) at 25°C was measured according to JIS K6850 at a test speed of 10 mm / min using a universal material testing machine [AG-50kNXplus, manufactured by Shimadzu Corporation]. The average values ​​of the results of five tests were evaluated based on the following evaluation criteria, and the results are shown in Tables 2 and 3. <Evaluation criteria> ◎: 10MPa or more ○: 5MPa or more, less than 10MPa ×: Less than 5MPa

[0106] (12) Adhesive strength between steel plates (lap shear adhesive strength) (100°C) [unit: MPa] Cold-rolled steel plates of approximately 1.6 mm thick, approximately 25 mm wide, and approximately 100 mm long as specified in JIS G3141 were washed with acetone, and two cold-rolled steel plates were bonded together with each of the kneaded epoxy resin compositions so that the overlap length was 12.5 mm and the thickness of the adhesive layer was 0.2 mm to obtain test specimens (curing conditions: 25°C and curing for 5 days). The test specimens were heated at a temperature T h After leaving it for 1 hour in a thermostatic chamber set at (100°C), the temperature was increased to T h The adhesive strength (lap shear adhesive strength) at 25°C was measured using a universal material testing machine [AG-50kNXplus, manufactured by Shimadzu Corporation] in accordance with JIS K6850, while controlling the temperature at 100°C and testing at a speed of 10 mm / min. The average values ​​of the results of five tests were evaluated based on the following criteria, and the results are shown in Tables 2 and 3. <Evaluation criteria> ◎: 15MPa or more ○: 10MPa or more, less than 15MPa △: 5MPa or more, less than 10MPa ×: Less than 5MPa

[0107] The results in Table 2 show that the epoxy resin compositions of Examples 1 to 19 have a required pot life even at low temperatures and therefore have good workability, and further have excellent storage stability and heat resistance of the cured product. On the other hand, from the results of Table 3, the epoxy resin compositions of Comparative Examples 1 and 3 not containing (B) had a short pot life, poor workability, and poor storage stability of the curing agent. The epoxy resin composition of Comparative Example 3 also had insufficient heat resistance (strength retention rate and adhesive strength at high temperature) of the cured product. The epoxy resin composition of Comparative Example 2, which contains a comparative compound (ratio B-1) in which the number of moles of bisphenol A diglycidyl ether reacted with 1 mole of polyalkylene polyamine is outside the upper limit of the range specified in claim 1 instead of (B), had too high an initial viscosity and poor workability. The epoxy resin compositions of Comparative Example 4, in which the weight ratio [(B) / (A)] of (B) in the curing agent to (A) in the base resin is outside the lower limit of the range specified in claim 1, and Comparative Example 5, in which the weight ratio is outside the upper limit, had insufficient heat resistance (strength retention rate and adhesive strength at high temperature) of the cured product. In Comparative Examples 6 to 8, in which the hydrophobicity of the fumed silica (E1) and / or (E2) was outside the range specified in claim 1, the storage stability of the base resin and / or curing agent was poor. [Industrial Applicability]

[0108] The epoxy resin composition of the present invention has sufficient pot life even at low temperatures, good workability (injectability, filling property, etc.), excellent storage stability, and can give a cured product with excellent heat resistance, so it can be used for various applications such as adhesives, resin fillers, and molded products, and is particularly suitable for use as adhesives for civil engineering and construction and resin fillers for civil engineering and construction. It is particularly useful as an adhesive for the GIR method and an adhesive for post-installed anchors.

Claims

1. A two-component curing type epoxy resin composition comprising a base material containing a polyepoxy compound (A) which is liquid at 5°C, an inorganic filler (D), and fumed silica (E1) having a hydrophobicity of 55 or more and 75 or less, and a curing agent containing a reaction product (B) of 1 mole of polyalkylene polyamine and 0.05 to 0.35 moles of bisphenol A diglycidyl ether, an inorganic filler (D), and fumed silica (E2) having a hydrophobicity of 0 or more and less than 55, wherein the content of (B) in the curing agent is 10 to 40 parts by weight per 100 parts by weight of (A) in the base material.

2. 2. The two-component curing epoxy resin composition according to claim 1, wherein the viscosity of (B) at 25° C. is 500 to 400,000 mPa·s.

3. 2. The two-component curing epoxy resin composition according to claim 1, wherein (B) contains a reaction product of pentaethylenehexamine and bisphenol A diglycidyl ether.

4. The two-component curing epoxy resin composition according to claim 1, wherein the curing agent further contains an aliphatic polyamine (C), the number average molecular weight of the (C) is 100 to 1500, and the active hydrogen equivalent of the (C) is 30 to 200 g / eq.

5. 2. The two-component curing type epoxy resin composition according to claim 1, which is an adhesive for civil engineering and construction.

6. A cured product obtained by curing the two-component curing type epoxy resin composition according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Epoxy resin composition

    JP2008088348A

  • Ordinary temperature curable epoxy resin composition

    JP2017105995A