Semiconductor device and manufacturing method therefor

The semiconductor device addresses adhesion issues between insulating layers and wiring by using a rewiring layer with controlled oxygen permeability and multiple insulating layers, enhancing adhesion and preventing insulation defects.

JP2024133017APending Publication Date: 2024-10-01ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024040327
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2024-03-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Conventional fan-out type semiconductor devices face issues with insufficient adhesion between the insulating layer and wiring, leading to insulation defects during reliability tests, especially with finer wiring and harsh conditions.

Method used

The semiconductor device incorporates a rewiring layer with an insulating layer having controlled oxygen permeability (150 to 7000 cm³/m²·ATM) and a layer structure of three or more layers, using materials like polyimide and polybenzoxazole, to ensure adhesion and prevent insulation defects.

Benefits of technology

This configuration allows for the formation of fine via holes in the insulating layer while maintaining adhesion with the wiring, preventing insulation defects and ensuring reliability under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133017000001_ABST
    Figure 2024133017000001_ABST
Patent Text Reader

Abstract

To provide a semiconductor device capable of achieving all of capability of forming a fine via hole in an insulation layer, not causing poor insulation, and ensuring adhesion of the insulation layer and wiring after a reliability test and a semiconductor device in which improvement of chemical resistance of the insulation layer and ensuring adhesion of the insulation layer and the wiring after a thermal history can be implemented.SOLUTION: A semiconductor device 1 comprises a semiconductor chip 2, an encapsulation material 3 covering the semiconductor chip 2 so that at least part of it is exposed, and a rewiring layer 4 that is arranged on the side of a surface not covered with the encapsulation material 3 of the semiconductor chip 2 and has an area larger than that of the semiconductor chip 2 in plan view. The rewiring layer 4 includes wiring 5 electrically connected to the semiconductor chip 2 and an insulation layer 6 having the degree of oxygen permeation that is 150 to 7000 cm3 / m2 day atm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a manufacturing method thereof. [Background technology]

[0002] There are various methods for packaging semiconductor devices. For example, one of the semiconductor packaging methods is a packaging method in which a part of a semiconductor chip is covered with an encapsulant, and a rewiring layer that is electrically connected to the semiconductor chip is formed on the surface of the semiconductor chip that is not covered with the encapsulant. Among the semiconductor packaging methods, a semiconductor packaging method called Fan-Out has become mainstream in recent years.

[0003] In a fan-out type semiconductor package, a protective layer is formed on a predetermined surface of a semiconductor chip, and an encapsulant is disposed on the other surface of the semiconductor chip, thus forming a chip encapsulation body larger than the chip size of the semiconductor chip. Then, a rewiring layer is formed across the protective layer and encapsulant area. This rewiring layer is formed with a thin film thickness. Since the rewiring layer can be formed across the encapsulant area, the semiconductor package can hold many external connection terminals. For example, the device described in Patent Document 1 is known as a fan-out type semiconductor device. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-129767 A Summary of the Invention [Problem to be solved by the invention]

[0005] In a fan-out type semiconductor device, the rewiring layer is configured to include an insulating layer, and in this case, the wiring electrically connected to the semiconductor chip is often covered by the insulating layer. In addition, with the recent trend toward finer wiring, it has become necessary to form finer via holes in the insulating layer.

[0006] In addition, the present inventors have focused on the viewpoint that it is required to ensure high adhesion between the insulating layer and the wiring without causing insulation failure in the insulating layer after the wiring is formed, even under harsh conditions such as reliability tests, etc. However, in conventional semiconductor devices (fan-out type semiconductor devices) including the device described in Patent Document 1, the adhesion between the insulating layer in the redistribution layer and the wiring after the reliability test is insufficient.

[0007] The present invention has been made in consideration of the above-mentioned points, and aims to provide a semiconductor device and a manufacturing method thereof that can achieve all of the following: the ability to form fine via holes in an insulating layer, no insulation defects, and the ability to ensure adhesion between the insulating layer and wiring after reliability testing. [Means for solving the problem]

[0008] One aspect of the present invention is as follows. [1] A semiconductor chip; an encapsulant that covers the semiconductor chip so that at least a portion of the semiconductor chip is exposed; a redistribution layer disposed on a surface of the semiconductor chip that is not covered by the sealing material and has an area larger than that of the semiconductor chip in a plan view; The rewiring layer is electrically connected to the semiconductor chip and has an oxygen permeability of 150 to 7000 cm 3 / m 2 and an insulating layer having a temperature of 1000 nm to 1500 nm. [2] 2. The semiconductor device according to item 1, wherein the insulating layer has a layer structure of three or more layers. [3] Item 2. The semiconductor device according to item 1, wherein the semiconductor chip includes a plurality of chips. [4] 2. The semiconductor device according to claim 1, wherein the encapsulant is in contact with the insulating layer. [5] Item 2. The semiconductor device according to item 1, wherein the encapsulant comprises an epoxy resin. [6] The oxygen permeability is 250 to 5000 cm 3 / m 2 2. The semiconductor device according to item 1, wherein the semiconductor device has a thermal conductivity of 1000 stoichiometric ratio of 1:1. [7] The oxygen permeability is 150 to 400 cm 3 / m 2 2. The semiconductor device according to item 1, wherein the semiconductor device has a thermal conductivity of 1000 stoichiometric ratio of 1:1. [8] The oxygen permeability is 150 to 350 cm 3 / m 2 2. The semiconductor device according to item 1, wherein the semiconductor device has a thermal conductivity of 1000 stoichiometric ratio of 1:1. [9] The oxygen permeability is 150 to 300 cm 3 / m 2 2. The semiconductor device according to item 1, wherein the semiconductor device has a thermal conductivity of 1000 stoichiometric ratio of 1:1.

[10] The oxygen permeability is 400 to 7000 cm 3 / m 2 2. The semiconductor device according to item 1, wherein the semiconductor device has a thermal conductivity of 1000 stoichiometric ratio of 1:1.

[11] The oxygen permeability is 450 to 7000 cm 3 / m 2 2. The semiconductor device according to item 1, wherein the semiconductor device has a thermal conductivity of 1000 stoichiometric ratio of 1:1.

[12] The oxygen permeability is 500 to 7000 cm 3 / m 2 2. The semiconductor device according to item 1, wherein the semiconductor device has a thermal conductivity of 1000 stoichiometric ratio of 1:1.

[13] The insulating layer is made of carbon (C), hydrogen (H), nitrogen (N), oxygen (O), silicon (Si), and titanium (Ti), Semiconductor device.

[14] Item 2. The semiconductor device of item 1, wherein the insulating layer is halogen-free.

[15] 2. The semiconductor device according to item 1, wherein the insulating layer includes at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

[16] The insulating layer contains polyimide, and when IR spectrum measurement is performed by the attenuated total reflection method (ATR method), -1 The peak height near 1500cm -1 The peak height near the peak height and the peak ratio (1380cm -1 Near peak height / 1500cm -1 2. The semiconductor device according to item 1, wherein the peak height (absolute peak height) is 0.2 to 2.5.

[17] The semiconductor device optionally includes a protective layer for protecting the semiconductor chip; When the semiconductor device includes the protective layer, the protective layer is formed on the semiconductor chip, Item 2. The semiconductor device according to item 1, wherein the insulating layer is disposed between the semiconductor device and the insulating layer.

[18] Item 18. The semiconductor device according to item 17, wherein the protective layer is in contact with at least one of the semiconductor chip and the insulating layer.

[19] The protective layer has holes formed therein, Item 18. The semiconductor device according to item 17, wherein the semiconductor chip and a wiring electrically connected to the semiconductor chip are electrically connected through the hole.

[20] 20. The semiconductor device according to item 19, wherein a ratio of an opening area resulting from the holes to a surface of the protective layer on the semiconductor chip side is less than half. [twenty one] Item 18. The semiconductor device according to item 17, wherein the protective layer includes at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group. [twenty two] The protective layer contains polyimide, and when IR spectrum measurement is performed by an attenuated total reflection method (ATR method), the IR spectrum of the protective layer is 1380 cm -1 The peak height near 1500cm -1 The peak height near the peak height and the peak ratio (1380cm -1 Near peak height / 1500cm -1 Item 18. The semiconductor device according to item 17, wherein the peak height (absolute peak height) is 1.2 to 2.5. [twenty three] At least one of the protective layer and the insulating layer is formed of the following general formula (1): [ka] (In the formula, X 1 is a tetravalent organic group derived from a tetracarboxylic dianhydride, and Y 1 Is, Zia is a divalent organic group derived from amine, and m is an integer of 1 or greater. Item 18. The semiconductor device according to item 17, comprising a polyimide having a structure of [twenty four] In the general formula (1), X 1 is a tetravalent organic group containing an aromatic ring, Y in the general formula (1) 1 24. The semiconductor device according to item 23, wherein is a divalent organic group containing an aromatic ring. [twenty five] In the general formula (1), X 1 is represented by the following general formulas (2) to (5): [ka] [ka] [ka] (In the formula, R 9 teeth 、 is an oxygen atom, a sulfur atom, or a divalent organic group. [ka] 24. The semiconductor device according to item 23, comprising at least one structure represented by:

[26] In the general formula (1), X 1 is represented by the following general formula (6): [ka] 26. The semiconductor device according to item 25, comprising a structure represented by:

[27] Y in the general formula (1) 1 is represented by the following general formulas (7) to (9): [ka] (In the formula, R 10 , R 11 , R 12 and R 13 are each independently a hydrogen atom, a monovalent aliphatic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different. [ka] (In the formula, R 14 ~R 21 are each independently a hydrogen atom, a halogen atom, a monovalent organic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different. [ka] (In the formula, R 22 is a divalent group or an oxygen atom, R 23 ~R 30 are each independently a hydrogen atom, a halogen atom, a monovalent aliphatic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different from each other; k is an integer of 1 to 3, and when k is 2 or 3, R 22 , R 23 , R 24 ,R 27 , R 28 may be the same or different.) 24. The semiconductor device according to item 23, comprising at least one structure represented by:

[28] Y in the formula (1) 1 is represented by the following general formula (10): [ka] 24. The semiconductor device according to item 23, comprising a structure represented by:

[29] The insulating layer is formed of the following general formula (11): [ka] (In the formula, U and V are each independently a divalent organic group.) Item 16. The semiconductor device according to item 15, comprising the polybenzoxazole having the structure:

[30] Item 30. The semiconductor device according to item 29, wherein U in the general formula (11) is a divalent organic group having 1 to 30 carbon atoms.

[31] Item 30. The semiconductor device according to item 29, wherein U in the general formula (11) is a chain alkylene group having 1 to 8 carbon atoms and in which some or all of the hydrogen atoms are substituted with fluorine atoms.

[32] Item 30. The semiconductor device according to item 29, wherein V in the general formula (11) is a divalent organic group having 1 to 40 carbon atoms.

[33] Item 30. The semiconductor device according to item 29, wherein V in the general formula (11) is a divalent chain aliphatic group having 1 to 20 carbon atoms.

[34] Item 30. The semiconductor device according to item 29, wherein V in the general formula (11) is a divalent organic group containing an aromatic group.

[35] V in the general formula (11) is represented by the following general formulas (7) to (9): [ka] (In the formula, R 10 , R 11 , R 12 and R 13 are each independently a hydrogen atom or a group having 1 to 5 carbon atoms. are monovalent aliphatic groups, and may be the same or different. [ka] (In the formula, R 14 ~R 21 are each independently a hydrogen atom, a halogen atom, or a group having 1 to 5 carbon atoms. are monovalent organic groups, and may be the same or different. [ka] (In the formula, R 22 is a divalent group or an oxygen atom, R 23 ~R 30 are each independently hydrogen atoms, halogen atoms, and monovalent aliphatic groups having 1 to 5 carbon atoms, k is an integer from 1 to 3, and when k is 2 or 3, R 22 , R 23 , R 24 ,R 27 , R 28 may be the same or different.) 30. The semiconductor device according to item 29, comprising at least one structure represented by:

[36] V in the general formula (11) is represented by the following general formula (10): [ka] 30. The semiconductor device according to item 29, comprising a structure represented by:

[37] Item 16. The semiconductor device according to item 15, wherein the polymer having a phenolic hydroxyl group comprises a novolac type phenolic resin.

[38] Item 16. The semiconductor device according to item 15, wherein the polymer having a phenolic hydroxyl group includes a phenol resin having no unsaturated hydrocarbon group and a modified phenol resin having an unsaturated hydrocarbon group.

[39] 2. The semiconductor device of claim 1, wherein the insulating layer includes a first insulating layer and a second insulating layer having a different composition than the first insulating layer.

[40] 40. The semiconductor device according to any one of items 1 to 39, wherein the semiconductor device is a fan-out type, wafer level chip size package type semiconductor device.

[41] A first step of preparing a semiconductor chip; A second step of covering the prepared semiconductor chip with an encapsulant so that at least a portion of the semiconductor chip is exposed; and a third step of forming a redistribution layer having an area larger than that of the semiconductor chip in a plan view on the exposed surface side of the semiconductor chip. A method for manufacturing a semiconductor device, comprising: The redistribution layer has an oxygen permeability of 150 to 7000 cm 3 / m 2 A method for manufacturing a semiconductor device, comprising: an insulating layer having an insulating layer thickness of atm.

[42] Item 42. The method for producing a semiconductor device according to item 41, wherein the insulating layer is formed from a photosensitive resin composition capable of forming at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

[43] The second step comprises: forming a protective layer on the semiconductor chip; covering the semiconductor chip on which the protective layer is formed with a sealing material so that at least a portion of the protective layer is exposed; The third step comprises: Item 43. The method for manufacturing a semiconductor device according to item 41 or 42, further comprising forming the redistribution layer on the protective layer side.

[44] Item 44. The method for producing a semiconductor device according to item 43, wherein the protective layer is formed from a photosensitive resin composition capable of forming at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

[45] A semiconductor chip; an encapsulant that covers the semiconductor chip so that at least a portion of the semiconductor chip is exposed; a redistribution layer disposed on a surface side of the semiconductor chip that is not covered by the sealing material and has an area larger than that of the semiconductor chip in a plan view; Oxygen permeability is 150 to 7000 cm 3 / m 2 ·day·atm, insulating layer.

[46] A semiconductor chip; an encapsulant that covers the semiconductor chip so that at least a portion of the semiconductor chip is exposed; In a semiconductor chip comprising: a redistribution layer disposed on a surface side not covered by the sealing material and having an area larger than that of the semiconductor chip in a plan view; Wiring electrically connected to the semiconductor chip; The wiring is in contact with the oxygen permeability of 150 to 7000 cm 3 / m 2 An insulating layer, which is 100 nm thick, and a redistribution layer, which includes: Effect of the Invention

[0009] According to the present invention, it is possible to form a fine via hole in an insulating layer, and to prevent insulation failure. and that the adhesion between the insulating layer and the wiring after reliability testing can be ensured. It is therefore possible to provide a semiconductor device and a manufacturing method thereof. According to the present invention, there is provided an insulating layer and a rewiring layer capable of realizing the above-mentioned semiconductor device. It is possible. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view showing a configuration example of a semiconductor device according to an embodiment of the present invention; [Diagram 2] 1 is a schematic plan view showing a configuration example of a semiconductor device according to an embodiment of the present invention; [Diagram 3] 1 is a diagram showing an example of a manufacturing process for the semiconductor device of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described with reference to the drawings. The present invention is not limited to the following embodiment, and can be implemented in various modifications within the scope of the gist. In this specification, in a numerical range described in stages, the upper or lower limit value described in a certain numerical range may be replaced by the upper or lower limit value of another numerical range described in stages, or may be replaced by the corresponding value in the examples. The scale, shape, length, etc. shown in the drawings may be exaggerated to further improve clarity.

[0012] [Embodiment 1] Semiconductor device FIG. 1 is a schematic cross-sectional view showing a configuration example of a semiconductor device 1, and FIG. 2 is a schematic plan view showing a configuration example of the semiconductor device 1. As shown in the figure, the semiconductor device (semiconductor IC) 1 includes: A semiconductor chip 2; a sealing material that covers the semiconductor chip 2 so that at least a portion of the semiconductor chip 2 is exposed; a redistribution layer 4 disposed on a surface of the semiconductor chip 2 that is not covered by a sealing material and having an area larger than that of the semiconductor chip 2 in a plan view; The rewiring layer 4 is electrically connected to the semiconductor chip 2 and has an oxygen permeability of 150 to 7000 cm 3 / m 2 and an insulating layer (hereinafter, may be referred to as an "interlayer insulating film") 6 having a resistance of 100 MPa.

[0013] The semiconductor chip 2 may be configured to include multiple semiconductor chips (chips 2a). In Fig. 1, multiple chips 2a are arranged in parallel along the surface direction (direction perpendicular to the A direction in Fig. 1). The semiconductor chip 2 is made of a semiconductor such as silicon, and has a circuit formed therein. When the semiconductor chip 2 includes multiple chips 2a, the configuration of each chip 2a may be the same or different.

[0014] The redistribution layer 4 is formed larger than the semiconductor chip 2 in a plan view (as viewed from the arrow A in FIG. 1). That is, the semiconductor device 1 of the present embodiment is a fan-out type wafer-level chip size package (WLCSP) type semiconductor device.

[0015] [Rewiring layer] The redistribution layer 4 is configured to include wiring 5 and an insulating layer 6. Specifically, the redistribution layer 4 is configured to include a plurality of wirings 5 ​​electrically connected to a plurality of terminals 2a provided on the semiconductor chip 2, and an insulating layer 6 filling spaces between the wirings 5. The terminals 2a and the wirings 5 ​​are electrically connected. One end of the wiring 5 is connected to the terminals 2a, and the other end is connected to an external connection terminal 7. The wirings 5 ​​between the terminals 2a and the external connection terminals 7 are covered with the insulating layer 6.

[0016] The insulating layer 6 in the redistribution layer 4 has a layer structure of three or more layers. This makes it easier to ensure the flatness of each insulating layer, and therefore the finally obtained redistribution layer 4. The insulating layer 6 in the redistribution layer 4 may have nine layers or less. Here, the "rewiring layer" in this embodiment does not include a printed wiring board.

[0017] The thickness of the redistribution layer 4 is about 3 to 30 μm. The thickness of the redistribution layer 4 may be 1 μm or more, 5 μm or more, or 10 μm or more. The thickness of the redistribution layer 4 may be 40 μm or less, 30 μm or less, or 20 μm or less.

[0018] 2 shows a plan view (viewed in the direction of arrow A in FIG. 1) of the semiconductor device 1. However, the sealing material 3 is omitted from the illustration. The semiconductor device 1 is configured such that the area S1 of the redistribution layer 4 is larger than the area S2 of the semiconductor chip 2 in a plan view. From the viewpoint of increasing the number of external connection terminals, the area S1 of the redistribution layer 4 is preferably 1.05 times or more, more preferably 1.1 times or more, more preferably 1.2 times or more, and particularly preferably 1.3 times or more, of the area S2 of the semiconductor chip 2. The area S1 of the redistribution layer 4 may be 50 times or less, 25 times or less, 10 times or less, or 5 times or less of the area S2 of the semiconductor chip 2. The area S1 of the redistribution layer 4 of the part overlapping the semiconductor chip 2 in a plan view is also included in the area S1 of the redistribution layer 4.

[0019] The external shapes of the semiconductor chip 2 and the redistribution layer 4 may be the same or different. In Fig. 2, the external shapes of the semiconductor chip 2 and the redistribution layer 4 are both similar rectangular shapes, but the shapes may be other than rectangular.

[0020] (insulation layer and wiring) The insulating layer 6 is preferably made of a material with high insulating properties from the viewpoint of preventing unintended electrical connection with the wiring 5. The wiring 5 may be made of any material that has high electrical conductivity, and copper is generally used.

[0021] The insulating layer 6 has an oxygen permeability of 150 to 7000 cm 3 / m 2 The oxygen permeability can be measured by the method described in the Examples below. In this embodiment, if the oxygen permeability is within the above range, it is possible to achieve all of the following: a fine via hole can be formed in the insulating layer, insulation failure does not occur, and adhesion between the insulating layer and the wiring after a reliability test can be ensured. Although the reason for this is unclear, the present inventors believe it to be as follows. The reliability test is carried out under high temperature and high humidity conditions, for example, at 130°C and 85% relative humidity (RH). During this test, moisture and oxygen atoms penetrate the insulating layer, which causes oxidation of the wiring, which tends to corrode the wiring. As a result, migration occurs when voltage is applied, which leads to the formation of dendrites and other defects, which then lead to short circuits (insulation failure). In addition, when copper wiring is used as the wiring, copper ions diffuse into the insulating layer during the reliability test, which creates voids between the copper wiring and the insulating layer, resulting in reduced adhesion. In this case, it is difficult to form fine via holes (to obtain good developability). Therefore, oxygen permeability (cm 3 / m 2 ·day·atm) to 7000cm 3 / m 2 By controlling the temperature to 100° C. or less, the permeation of moisture and oxygen can be suppressed, thereby suppressing the above-mentioned phenomenon. The oxygen permeability is preferably 6500 or less, more preferably 6000 or less, and particularly preferably 5500 or less.

[0022] On the other hand, if the oxygen permeability is too low, the transmittance of the exposure light through the photosensitive resin composition is low. Therefore, when forming a via hole, i.e., when the coating film of the composition is irradiated with the exposure light, the light tends not to reach the bottom of the coating film sufficiently. Therefore, the oxygen permeability (cm 3 / m 2 By setting the oxygen permeability (cm ·day·atm) to 150 or more, good developability can be obtained, and in turn, good resolution can be obtained. 3 / m 2 The viscosity (days·atm) is preferably 200 or more, more preferably 250 or more, particularly preferably 300 or more, and even more preferably 350 or more. The oxygen permeability according to the present embodiment can be appropriately selected depending on the configuration of the semiconductor device to which it is applied. For example, in the case of a semiconductor device that requires strict reliability, it is preferable to use an insulating layer with a low oxygen permeability. In that case, the oxygen permeability (cm 3 / m 2The viscosity (°C / day / atm) is preferably from 150 to 450, more preferably from 150 to 400, particularly preferably from 150 to 350, and even more preferably from 150 to 300. In the case of a semiconductor device that requires strict resolution, it is preferable to use an insulating layer with high oxygen permeability. In this case, the oxygen permeability (cm 3 / m 2 The viscosity (°C·day·atm) is preferably from 350 to 7,000, more preferably from 400 to 7,000, particularly preferably from 450 to 7,000, and even more preferably from 500 to 7,000.

[0023] The oxygen permeability can be designed within the above range by selecting the polymer structure contained in the insulating layer and / or the amount and type of additive added to the insulating layer. For example, methods for increasing the oxygen permeability include introducing a compound with a large free volume into the polymer structure, and introducing such a compound into the insulating layer as an additive. For example, in the case of polyimide, a fluorine-based monomer (an acid dianhydride and / or a diamine containing a fluorine atom) can be selected as the raw material monomer. Also, an acid dianhydride and / or a diamine having a fluorene skeleton can be used as the raw material monomer. Methods for reducing oxygen permeability include producing an insulating layer using a plasticizer that volatilizes during curing of the coating of the composition and that can promote packing between polymers in the insulating layer (e.g., dicyclohexyl phthalate, diphenyl phthalate, di-2-ethylhexyl dicyclohexyl trimellitate, dicyclohexyl pyromellitate, dicyclohexyl adipate).

[0024] From the viewpoint of developability, the Young's modulus of the insulating layer 6 is preferably 5.0 GPa or less, more preferably 4.5 GPa or less, particularly preferably 4.1 GPa or less, or 4.0 GPa or less, and from the viewpoint of protecting the wiring, it is preferably 2.0 GPa or more, more preferably 2.5 GPa or more, particularly preferably 3.0 GPa or more, or 3.2 GPa or more.

[0025] The insulating layer 6 in the redistribution layer 4 may be multi-layered as described above. For example, the redistribution layer 4 may include a first insulating layer, a second insulating layer, and an intermediate layer that is different from the first insulating layer and the second insulating layer and is provided between the first insulating layer and the second insulating layer when the redistribution layer 4 is viewed in cross section. The intermediate layer is, for example, a wiring 5.

[0026] The composition, Young's modulus, and film thickness of the first insulating layer and the second insulating layer may be the same or different. When the first insulating layer and the second insulating layer have different compositions, it is possible to give each insulating layer different properties. In one embodiment, the insulating layer 6 includes a first insulating layer and a second insulating layer having a composition different from that of the first insulating layer.

[0027] The insulating layer 6 preferably contains at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group, for example, which makes it easier to achieve the effects of this embodiment.

[0028] The resin composition used to form the insulating layer 6 may be a photosensitive resin composition, and is preferably a photosensitive resin composition containing at least one selected from the group consisting of a polyimide precursor, a polybenzoxazole precursor, and a polymer having a phenolic hydroxyl group. Such a photosensitive resin composition may be either a negative type or a positive type. The resin composition used to form the insulating layer 6 may be in the form of a liquid or a film.

[0029] In this embodiment, the pattern obtained after exposing and developing the photosensitive resin composition is referred to as a “relief pattern,” and the relief pattern obtained by curing the same by heating is referred to as a “cured relief pattern.” This cured relief pattern constitutes the protective layer 8 and the insulating layer 6. In this embodiment, the insulating layer preferably contains at least one selected from the group consisting of carbon (C), hydrogen (H), nitrogen (N), oxygen (O), silicon (Si), and titanium (Ti), which makes it easier to achieve the effects of this embodiment. Here, the insulating layer 6 of this embodiment does not contain a halogen. By not introducing a functional group with a large free volume, such as a halogen, the chemical resistance of the insulating layer 6 can be easily prevented from decreasing.

[0030] (Sealing material) The sealing material 3 covers the surfaces (side and top surfaces) of the semiconductor chip 2, and is formed with an area larger than the region of the semiconductor chip 2 in a plan view (viewed in the direction of the arrow A in FIG. 1).

[0031] From the viewpoints of heat resistance and adhesion to the insulating layer 6, the sealing material 3 preferably contains an epoxy resin. Moreover, the sealing material 3 preferably contacts the semiconductor chip 2 and the rewiring layer 4. In particular, the sealing material 3 preferably contacts the insulating layer 6 in the rewiring layer 4. This makes it easy to effectively improve the sealing performance from the semiconductor chip 2 to the rewiring layer 4.

[0032] The sealing material 3 may be a single layer or multiple layers. When the sealing material 3 is multiple layers, the materials of the multiple layers may be the same or different.

[0033] (protective layer) The protective layer 8 protects the semiconductor chip 2. From the viewpoint of protecting the semiconductor chip 2 against physical impact, the Young's modulus of the protective layer 8 is preferably 4.0 GPa or more, more preferably 4.5 GPa or more, and particularly preferably 5 GPa or more. When the protective layer is made of a photosensitive resin composition, from the viewpoint of developability, the Young's modulus of the protective layer 8 is preferably 9.0 GPa or less, more preferably 8.5 GPa or less, and particularly preferably 8.0 GPa or less. The Young's modulus can be calculated by a tensile test, a nanoindentation test, or the like.

[0034] The protective layer 8 is provided on the surface of the semiconductor chip 2 that is not covered by the encapsulant 3. When the semiconductor chip 2 is viewed in plan (as viewed from the side covered by the encapsulant 3 in FIG. 1 ) the protective layer 8 is in the shadow of the semiconductor chip 2 and therefore cannot be observed.

[0035] The protective layer 8 is in contact with at least one of the semiconductor chip 2 and the insulating layer 6. This makes it easier to protect the semiconductor chip 2 in a suitable manner. This configuration is an embodiment in which improved adhesion between the protective layer 8 and the insulating layer 6 is desired, and even in the case of the semiconductor device 1 having such an embodiment, it is possible to improve the adhesion between the protective layer 8 and the insulating layer 6. In particular, in the semiconductor device 1, the protective layer 8 is in contact with both the semiconductor chip 2 and the insulating layer 6, which is a more preferable embodiment from the above viewpoint. Although omitted in the semiconductor device 1, other members may be interposed between the semiconductor chip 2 and the insulating layer 6 as long as the effects of this embodiment can be obtained.

[0036] Holes 8a are formed in the protective layer 8, and the semiconductor chip 2 side and the wiring 5 side are electrically connected through the holes 8a. This makes it easier to further protect the semiconductor chip 2 while ensuring the electrical connection between the semiconductor chip 2 side and the wiring 5 side. A plurality of holes 8a are provided in the protective layer 8 corresponding to the terminals 2a of the semiconductor chip 2, and the terminals 2a are inserted into each of the plurality of holes 8a.

[0037] In the semiconductor device 1, the ratio of the opening area resulting from the holes 8a to the surface of the protective layer 8 facing the semiconductor chip 2 is less than half. This ensures a protective area for protecting the semiconductor chip 2, making it easier to further protect the semiconductor chip 2. Here, the "opening area" refers to the total area of ​​the opening entrances on the surface facing the semiconductor chip 2.

[0038] The protective layer preferably contains at least one selected from the group consisting of, for example, polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

[0039] The resin composition used to form the protective layer 8 may be any photosensitive resin composition, and is preferably a photosensitive resin composition containing at least one selected from the group consisting of a polyimide precursor, a polymer having a polyimide moiety and a polyimide precursor moiety in the polymer structure, a solvent-soluble polyimide, a polybenzoxazole precursor, and a polymer having a phenolic hydroxyl group. Such a photosensitive resin composition may be either negative or positive. The resin composition used to form the protective layer 8 may be in the form of a liquid or a film.

[0040] <Polyimide precursor> (A) Photosensitive resin Examples of the photosensitive resin (A) used to prepare the polyimide precursor include polyamide and polyamic acid ester. Examples of the polyamic acid ester include those represented by the following general formula (12): [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom, a saturated aliphatic group having 1 to 30 carbon atoms, an aromatic group, a monovalent organic group having a carbon-carbon unsaturated double bond, or a monovalent ion having a carbon-carbon unsaturated double bond; X 1 is a tetravalent organic group derived from a tetracarboxylic dianhydride, and Y 1 is a divalent organic group derived from a diamine, and m is an integer of 1 or greater. It is possible to use a polyamic acid ester containing a repeating unit represented by the following formula: In the formula, m is preferably 2 or more, and more preferably 5 or more.

[0041] In the above formula (12), R 1 and R 2 When exists as a monovalent cation, O is negatively charged, i.e., exists as -O-. 1 and Y 1 may contain a hydroxyl group. R 1 and R 2 is represented by the following general formula (13): [ka] (In the formula, R 3 , R 4 and R 5 are each independently a hydrogen atom or an organic group having 1 to 5 carbon atoms, and m1 is an integer of 1 to 20. It is more preferable that the aryl group is a monovalent organic group represented by the following general formula (14): [ka] (In the formula, R 6 , R 7 and R 8 are each independently a hydrogen atom or an organic group having 1 to 5 carbon atoms, and m2 is an integer of 1 to 20. It is also preferable that the structure has an ammonium ion at the end of a monovalent organic group represented by the formula: I wish.

[0042] A plurality of polyamic acid esters represented by the general formula (12) may be mixed together, or a polyamic acid ester obtained by copolymerizing two or more polyamic acid esters represented by the general formula (12) may be used.

[0043] X 1 From the viewpoints of Young's modulus and chemical resistance, X is preferably a tetravalent organic group containing an aromatic group. 1 is represented by the following general formulas (2) to (5): [ka] [ka] [ka] (In the formula, R 9 teeth 、 is an oxygen atom, a sulfur atom, or a divalent organic group. [ka] It is preferable that the aryl group is a tetravalent organic group containing at least one structure represented by the following formula:

[0044] R in general formula (4) 9 may be, for example, a divalent organic group having 1 to 40 carbon atoms or a halogen atom. 9 may contain a hydroxyl group.

[0045] X in general formula (1) 1 From the viewpoint of developability, the compound represented by the following general formula (6): [ka] A tetravalent organic group containing a structure represented by the following formula is particularly preferred.

[0046] Y 1 From the viewpoints of Young's modulus and chemical resistance, Y is preferably a divalent organic group containing an aromatic group. 1 is represented by the following general formulas (7) to (9): [ka] (In the formula, R 10 , R 11 , R 12 and R 13 are each independently a hydrogen atom, a monovalent aliphatic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different. [ka] (In the formula, R 14 ~R 21 are each independently a hydrogen atom, a halogen atom, a monovalent organic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different. [ka] (In the formula, R 22 is a divalent organic group or an oxygen atom, R 23 ~R 30are each independently a hydrogen atom, a halogen atom, a monovalent aliphatic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different from each other; k is an integer of 1 to 3, and when k is 2 or 3, R 22 , R 23 , R 24 ,R 27 , R 28 may be the same or different.) It is preferable that the divalent organic group contains at least one structure represented by the following formula:

[0047] R in general formula (9) 22 is, for example, a divalent organic group having 1 to 40 carbon atoms or a halogen atom.

[0048] From the viewpoint of developability, Y 1 is represented by the following general formula (10): [ka] A divalent organic group containing a structure represented by the following formula is particularly preferred.

[0049] In the polyamic acid ester, X in the repeating unit 1 is derived from the tetracarboxylic dianhydride used as a raw material, and Y 1 is derived from the diamine used as a raw material.

[0050] Examples of tetracarboxylic dianhydrides used as raw materials include pyromellitic anhydride (PMDA), diphenylether-3,3',4,4'-tetracarboxylic dianhydride (4,4'-oxydiphthalic dianhydride: ODPA), benzophenone-3,3',4,4'-tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA), etc. These may be used alone or in combination.

[0051] Examples of diamines used as raw materials include p-phenylenediamine (PPD), m-phenylenediamine, 4,4'-diaminodiphenyl ether (DADPE), 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diamino-2,2'-dimethylbiphenyl (m-TB), 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, and 3,3'-diaminodiphenyl sulfide. sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diamino Aminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy) phenyl] ether, bis[4-(3-aminophenoxy)phenyl] ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4- Examples of such compounds include 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), and 2,2-bis[4-(4-aminophenoxy)-3-methylphenyl]propane (MBAPP). Some of the hydrogen atoms on these benzene rings may be substituted. These compounds may be used alone or in combination.

[0052] By using 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, fluorene dianhydride, or the like as the acid anhydride, the oxygen permeability in the insulating layer tends to be increased. By using diamines such as 9,9-bis(4-aminophenyl)fluorene (BAFL) and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, the oxygen permeability in the insulating layer tends to be increased.

[0053] In the synthesis of the polyamic acid ester (A), a method can be preferably used in which a tetracarboxylic acid diester obtained by an esterification reaction of a tetracarboxylic acid dianhydride, which will be described later, is directly subjected to a condensation reaction with a diamine.

[0054] The alcohols used in the esterification reaction of the tetracarboxylic dianhydride are alcohols having an olefinic double bond. Specific examples include 2-hydroxyethyl methacrylate, 2-methacryloyloxyethyl alcohol, glycerin diacrylate, and glycerin dimethacrylate. These alcohols may be used alone or in combination of two or more.

[0055] Concerning the specific synthesis method of the polyamic acid ester (A), a conventionally known method can be adopted. As the synthesis method, for example, the method shown in the pamphlet of International Publication No. 00 / 43439 can be mentioned. That is, a method can be mentioned in which a tetracarboxylic acid diester is once converted into a tetracarboxylic acid diester diacid chloride, and the tetracarboxylic acid diester diacid chloride and a diamine are subjected to a condensation reaction in the presence of a basic compound, and further a polyamic acid ester is produced. Also, a method can be mentioned in which a polyamic acid ester is produced by a method in which a tetracarboxylic acid diester and a diamine are subjected to a condensation reaction in the presence of an organic dehydrating agent.

[0056] Examples of organic dehydrating agents include dicyclohexylcarbodiimide (DCC), diethylcarbodiimide, diisopropylcarbodiimide, ethylcyclohexylcarbodiimide, diphenylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, 1-cyclohexyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, and the like.

[0057] The weight average molecular weight of the polyamic acid ester (A) is preferably from 6,000 to 150,000, more preferably from 7,000 to 50,000, and still more preferably from 7,000 to 20,000.

[0058] <Polymer having polyimide moiety and polyimide precursor moiety in the polymer structure> As a polymer having a polyimide portion and a polyimide precursor portion in the polymer structure, a polyimide precursor having a polyimide portion in part can be used. Such a precursor can be, for example, a polyimide precursor represented by the following general formula (15): [ka] (In the formula, X 1 , X 2 and X 3 are each independently a tetravalent organic group having 6 to 40 carbon atoms; Y 1 and Y 2are each independently a divalent organic group having 6 to 40 carbon atoms, 1 is an integer from 2 to 30, and n 2 and n 3 are each independently an integer of 2 to 150, R 1 , R 2 , R 3 , and R 4 are each independently a hydrogen atom or a monovalent organic group having 1 to 40 carbon atoms, and R 1 , R 2 , R 3 , and R 4 At least one of the above has a structure containing the general formula (13) or (14). The structure includes:

[0059] In the above general formula (15), n 2 / (n 2 +n 3 ) is 0.05≦n 2 / (n 2 +n 3 )≦0.95. From the viewpoint of flatness, it is preferably 0.1 or more, more preferably 0.2 or more, and particularly preferably 0.45 or more. From the viewpoint of resolution, it is preferably 0.9 or less, more preferably 0.8 or less, and particularly preferably 0.7 or less. X in formula (15) 1 , X 2 and X 3 The preferred range of X in formula (12) is 1 The preferred range of Y in formula (15) is the same as that of 1 and Y 2 The preferred range of Y in formula (12) is 1 The preferred range is the same as that of the above.

[0060] <Solvent-soluble polyimide> The solvent-soluble polyimide of the present embodiment may be any polyimide that is soluble in a solvent. [ka] (In the formula, X 1is a tetravalent organic group derived from a tetracarboxylic dianhydride, and Y 1 is a divalent organic group derived from a diamine, and m is an integer of 1 or greater. It is preferable that the polyimide includes a polyimide having the structure:

[0061] In formula (1), X 1 In addition to the above, Y may be a tetravalent organic group having 6 to 40 carbon atoms. 1 In addition to the above, may be a divalent organic group having 6 to 40 carbon atoms, and m is preferably 2 or more, more preferably 5 or more. For example, X in formula (1) 1 is preferably a tetravalent organic group containing an aromatic ring, and Y 1 is preferably a divalent organic group containing an aromatic ring.

[0062] X in formula (1) 1 The preferred range of X in formula (12) is 1 The preferred range is the same as that of Y in formula (1). 1 The preferred range of Y in formula (12) is 1 The preferred range is the same as that of the above. From the viewpoint of resolution, the solvent-soluble polyimide of the present embodiment preferably contains a radically reactive functional group at its terminal.

[0063] (B1) Photoinitiator When the resin composition used to form the protective layer and the insulating layer is a negative photosensitive resin composition, the composition may contain a photoinitiator. Examples of the photoinitiator (B1) include benzophenone derivatives such as benzophenone, o-benzoyl methyl benzoate, 4-benzoyl-4'-methyldiphenyl ketone, dibenzyl ketone, and fluorenone, acetophenone derivatives such as 2,2'-diethoxyacetophenone and 2-hydroxy-2-methylpropiophenone, 1-hydroxycyclohexyl phenyl ketone, thioxanthone derivatives such as thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, and diethylthioxanthone, benzil derivatives such as benzil, benzil dimethyl ketal, and benzyl-β-methoxyethyl acetal, benzoin derivatives such as benzoin methyl ether, 2,6-di(4'-diazidobenzal)-4-methylcyclohexanthone, and 2,6-di(4'-diazidobenzal)-4-methylcyclohexanthone. Azides such as xanone and 2,6'-di(4'-diazidobenzal)cyclohexanone, oximes such as 1-phenyl-1,2-butanedione-2-(O-methoxycarbonyl)oxime, 1-phenylpropanedione-2-(O-methoxycarbonyl)oxime, 1-phenylpropanedione-2-(O-ethoxycarbonyl)oxime, 1-phenylpropanedione-2-(O-benzoyl)oxime, 1,3-diphenylpropanetrione-2-(O-ethoxycarbonyl)oxime, 1-phenyl-3-ethoxypropanetrione-2-(O-benzoyl)oxime, N-arylglycines such as N-phenylglycine, peroxides such as benzoyl peroxide, aromatic biimidazoles, and titanocenes are used. Among these, the above oximes are preferred from the viewpoint of photosensitivity. The photoinitiator (B1) may be used alone or in combination of two or more.

[0064] The amount of the photoinitiator (B1) added is preferably 1 to 40 parts by mass, more preferably 2 to 20 parts by mass, based on 100 parts by mass of the polyamic acid ester (A). By adding 1 part by mass or more of the photoinitiator (B1) based on 100 parts by mass of the polyamic acid ester (A), the photosensitivity tends to be excellent. Also, by adding 40 parts by mass or less, the thick-film curing property tends to be excellent.

[0065] (B2) Photoacid generator The photoacid generator (B2) has the function of increasing the solubility of the light irradiated portion in an aqueous alkaline solution. When the resin composition used to form the protective layer and the insulating layer is a positive-type photosensitive resin, the composition may contain a photoacid generator. By containing the photoacid generator, an acid is generated in the ultraviolet-exposed portion, and therefore the solubility of the exposed portion in an alkaline aqueous solution is increased. This allows the composition to be used as a positive-type photosensitive resin composition.

[0066] Examples of the photoacid generator (B2) include quinone diazide compounds, sulfonium salts, phosphonium salts, diazonium salts, iodonium salts, etc. Among these, quinone diazide compounds are preferably used from the viewpoint of exhibiting an excellent dissolution suppression effect and obtaining a highly sensitive positive-type photosensitive resin composition.

[0067] (C) Additives As described above, the oxygen permeability of the insulating layer can be adjusted by the polymer structure in the insulating layer, and can also be adjusted by the type or amount of additives. By using a (meth)acrylate compound containing a halogen such as a fluorine atom as an additive, the oxygen permeability tends to be increased. Examples of such compounds include methyl 2-fluoroacrylate, 2,2,2-trifluoroethyl acrylate, 2,2,3,3,3-pentafluoropropyl acrylate, 2-(perfluorobutyl)ethyl acrylate, 3-perfluorohexyl-2-hydroxypropyl acrylate, 1H,1H,3H-tetrafluoropropyl acrylate, 1H,1H,5H-octafluoropentyl acrylate, 1H,1H,7H-dodecafluoroheptyl acrylate, 1H-1-(trifluoromethyl)trifluoroethyl acrylate, 1H,1H,3H-hexafluorobutyl acrylate, and the like. In addition to the above, examples of compounds capable of increasing oxygen permeability include fluorene (meth)acrylate, which has a large free volume.

[0068] There is a tendency that oxygen permeability can be reduced by using a compound such as a plasticizer as an additive that can improve the packing between polymers during heat curing. Examples of such plasticizers include dicyclohexyl phthalate, diphenyl phthalate, di-2-ethylhexyl dicyclohexyl trimellitate, dicyclohexyl pyromellitate, and dicyclohexyl adipate.

[0069] (D) Solvent The solvent may be any solvent capable of dissolving or dispersing each component. Examples include N-methyl-2-pyrrolidone (NMP), γ-butyrolactone (GBL), acetone, methyl ethyl ketone, dimethyl sulfoxide (DMSO), etc. These solvents can be used in the range of 30 to 1500 parts by mass per 100 parts by mass of the photosensitive resin (A) depending on the coating film thickness and viscosity.

[0070] (E) Other The photosensitive resin (A) may have a crosslinking agent. As the crosslinking agent, a crosslinking agent capable of crosslinking the photosensitive resin (A) or capable of forming a crosslinked network by itself when the polyimide precursor composition is exposed to light, developed, and then cured by heating can be used. By using the crosslinking agent, the heat resistance and chemical resistance of the cured film (insulating layer) can be further enhanced.

[0071] In addition, the photosensitive resin (A) may contain a sensitizer for improving photosensitivity, an adhesion aid for improving adhesion to a substrate, and the like.

[0072] (Exposure and development) After the polyimide precursor is exposed to light, unnecessary parts are washed away with a developer. In the case of polyimide precursors that are developed with a solvent, the developer used may be a good solvent such as N,N-dimethylformamide, dimethylsulfoxide (DMSO), N,N-dimethylacetamide, N-methyl-2-pyrrolidone (NMP), cyclopentanone, γ-butyrolactone (GBL), or acetate esters, or a mixture of these good solvents with poor solvents such as lower alcohols, water, or aromatic hydrocarbons. After development, rinse cleaning is performed with a poor solvent, etc., as necessary.

[0073] In the case of a polyimide precursor that is developed with an alkaline aqueous solution, preferred are aqueous solutions of compounds that exhibit alkalinity, such as an aqueous solution of tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and hexamethylenediamine.

[0074] (thermal curing) After development, the exposed polyimide precursor can be heated to close the ring of the polyimide precursor, thereby forming a polyimide, which becomes the cured relief pattern, i.e., the insulating layer.

[0075] Regarding the heating temperature for thermal curing of the polyimide precursor, generally, the higher the heat curing temperature, the larger the Young's modulus tends to be. From the viewpoint of making the Young's modulus of the insulating layer of the present embodiment a desired value, the heating temperature is preferably 160°C or more, more preferably 180°C or more, and particularly preferably 200°C or more. From the viewpoint of the influence on other members, the heating temperature is preferably 400°C or less.

[0076] <Polyimide> The structure of the cured relief pattern formed from the polyimide precursor, for example, at least one of the protective layer and the insulating layer, may be represented by the following general formula (1): [ka] (In the formula, X 1 is a tetravalent organic group derived from a tetracarboxylic dianhydride, and Y 1 is a divalent organic group derived from a diamine, and m is an integer of 1 or greater. The preferred X in the general formula (12) includes polyimides having the structure: 1 , Y 1 For the same reason, m is also preferred in the polyimide represented by general formula (1).

[0077] In the case of an alkali-soluble polyimide, the polyimide may be terminated with a hydroxyl group. When the protective layer of the present embodiment contains polyimide, the IR spectrum measured by the attenuated total reflection (ATR) method has a peak at 1380 cm -1 The peak height near 1500cm -1 The peak height near the peak height and the peak ratio (1380cm -1 Near peak height / 1500cm -1 From the viewpoint of chemical resistance, it is preferably 1.3 or more, more preferably 1.4 or more, and particularly preferably 1.5 or more. From the viewpoint of developability, it is preferably 2.4 or less, more preferably 2.3 or less, and particularly preferably 2.2 or less. The "1380cm" -1 The peak height in the vicinity of 1330 to 1430 cm -1 The maximum peak height within the range of 1500 cm -1 The peak height in the vicinity of 1450 to 1550 cm -1 is the maximum peak height within the range.

[0078] When the insulating layer of this embodiment contains polyimide, the IR spectrum measurement is performed by the attenuated total reflection (ATR) method. -1 The peak height near 1500cm -1The peak height near the peak height and the peak ratio (1380cm -1 Near peak height / 1500cm -1 In view of chemical resistance, it is preferably 0.3 or more, more preferably 0.4 or more, and particularly preferably 0.5 or more. In view of developability, it is preferably 1.0 or less, more preferably 0.7 or less, and particularly preferably 0.6 or less. The "1380cm" -1 The peak height in the vicinity of 1330 to 1430 cm -1 The maximum peak height within the range of 1500 cm -1 The peak height in the vicinity of 1450 to 1550 cm -1 is the maximum peak height within the range.

[0079] <Polybenzoxazole precursor> (A) Photosensitive resin The photosensitive resin used for the polybenzoxazole precursor may be a resin represented by the following general formula (11A): [ka] (In the formula, Y 2 and Y 3 is a divalent organic group. Poly(o-hydroxyamide) containing a repeating unit represented by the following formula can be used.

[0080] From the viewpoint of adhesion between the insulating layer and the sealing material, Y 2 is preferably a divalent organic group having 1 to 30 carbon atoms, more preferably a chain alkylene group having 1 to 15 carbon atoms (however, the hydrogen atoms of the chain alkylene may be substituted with halogen atoms), and particularly preferably a chain alkylene group having 1 to 8 carbon atoms and some or all of the hydrogen atoms being substituted with fluorine atoms.

[0081] In addition, from the viewpoint of adhesion between the insulating layer and the sealing material, Y 3 is preferably a divalent organic group containing an aromatic group, and more preferably represented by the following general formulas (7) to (9):

[0082] [ka] (In the formula, R 10 , R 11 , R 12 and R 13 are each independently a hydrogen atom or a monovalent aliphatic group having 1 to 5 carbon atoms, and may be the same or different.)

[0083] [ka] (In the formula, R 14 ~R 21 are each independently a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 5 carbon atoms, and may be the same or different.

[0084] [ka] (In the formula, R 22 is a divalent organic group or an oxygen atom, R 23 ~R 30 are each independently a hydrogen atom, a halogen atom, or a monovalent aliphatic group having 1 to 5 carbon atoms, and may be the same or different from each other; k is an integer of 1 to 3, and when k is 2 or 3, R 22 , R 23 , R 24 ,R 27 , R 28 may be the same or different.) It is preferable that the divalent organic group contains at least one structure represented by the following formula:

[0085] R in general formula (9) 22 may be, for example, a divalent organic group having 1 to 40 carbon atoms or a halogen atom.

[0086] From the viewpoint of adhesion between the insulating layer and the sealing material, Y 3 is represented by the following general formula (10): [ka] A divalent organic group containing a structure represented by the following formula is particularly preferred.

[0087] In addition, from the viewpoint of adhesion between the insulating layer and the sealing material, Y 3 is preferably a divalent organic group having 1 to 40 carbon atoms, more preferably a divalent chain aliphatic group having 1 to 40 carbon atoms, and particularly preferably a divalent chain aliphatic group having 1 to 20 carbon atoms.

[0088] The polybenzoxazole precursor can generally be synthesized from a dicarboxylic acid derivative and a hydroxyl group-containing diamine. Specifically, the polybenzoxazole precursor can be synthesized by converting the dicarboxylic acid derivative into a dihalide derivative and then reacting it with a diamine. As the dihalide derivative, a dichloride derivative is preferable.

[0089] The dichloride derivative can be synthesized by reacting a dicarboxylic acid derivative with a halogenating agent, such as thionyl chloride, phosphoryl chloride, phosphorus oxychloride, or phosphorus pentachloride, which are commonly used in acid chloride reactions of carboxylic acids.

[0090] The dichloride derivative can be synthesized by reacting a dicarboxylic acid derivative with the above-mentioned halogenating agent in a solvent, or by carrying out the reaction in an excess of the halogenating agent and then distilling off the excess.

[0091] Examples of dicarboxylic acids used in the dicarboxylic acid derivative include isophthalic acid, terephthalic acid, 2,2-bis(4-carboxyphenyl)-1,1,1,3,3,3-hexafluoropropane, 4,4'-dicarboxybiphenyl, 4,4'-dicarboxydiphenyl ether (4,4'-diphenyl ether dicarboxylic acid), 4,4'-dicarboxytetraphenylsilane, bis(4-carboxyphenyl)sulfone, 2,2-bis(p-carboxyphenyl)propane, 5-tert-butylisophthalic acid, 5-bromoisophthalic acid, 5-fluoroisophthalic acid, 5-chloroisophthalic acid, 2,6-naphthalenedicarboxylic acid, malonic acid, dimethylmalonic acid, ethylmalonic acid, isopropylmalonic acid, di-n-butylmalonic acid, succinic acid, tetrafluorosuccinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, dimethylmethylsuccinic acid, glutaric acid, hexafluoroglutarate, and the like. Glutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 3-ethyl-3-methylglutaric acid, adipic acid, octafluoroadipic acid, 3-methyladipic acid, octafluoroadipic acid, pimelic acid, 2,2,6,6-tetramethylpimelic acid, suberic acid, dodecafluorosuberic acid, azelaic acid, sebacic acid, hexadecafluorosebacic acid, 1,9-nonanedioic acid, dodecanedioic acid, tridecafluorosebacic acid, hexadecafluorosebacic acid, 1,9-nonanedioic acid, dodecafluorosebacic acid, tridecafluorosebacic acid, hexadecafluorosebacic acid, hexadecafluorosebacic acid, hexadecafluorosebacic acid, hexadecafluorosebacic acid, hexadecafluorosebacic acid, hexadecafluorosebacic acid, trideca ... Examples of the dicarboxylic acids include tetracosane diacid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosane diacid, heneicosane diacid, docosane diacid, tricosane diacid, tetracosane diacid, pentacosane diacid, hexacosane diacid, heptacosane diacid, octacosane diacid, nonacosane diacid, triacontanedioic acid, hentriacontanedioic acid, dotriacontanedioic acid, diglycolic acid, and dicyclopentadiene carboxylic acid. These may be used in combination.

[0092] Examples of hydroxyl group-containing diamines include 3,3'-diamino-4,4'-dihydroxybiphenyl, 4,4'-diamino-3,3'-dihydroxybiphenyl, bis(3-amino-4-hydroxyphenyl)propane, bis(4-amino-3-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(4-amino-3-hydroxyphenyl)sulfone, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-amino-3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, etc. These may be used in combination.

[0093] (B2) Photoacid generator Examples of the photoacid generator (B2) include diazonaphthoquinone compounds, aryl diazonium salts, diaryliodonium salts, triarylsulfonium salts, etc. Among these, diazonaphthoquinone compounds are preferred because of their high sensitivity.

[0094] (C) Additives The preferred types and amounts of the additive (C) are the same as those described in relation to the polyimide.

[0095] (D) Solvent The solvent (D) may be any solvent capable of dissolving or dispersing each of the components.

[0096] (E) Other The polybenzoxazole precursor may contain a crosslinking agent, a sensitizer, an adhesion promoter, a thermal acid generator, etc. The polybenzoxazole precursor may contain necessary additives in addition to the above.

[0097] (Exposure and development) After the polybenzoxazole precursor is exposed to light, unnecessary portions are washed away with a developer, such as an aqueous alkali solution of sodium hydroxide, potassium hydroxide, sodium silicate, ammonia, ethylamine, diethylamine, triethylamine, triethanolamine, or tetramethylammonium hydroxide.

[0098] Although the above description has focused on positive-type polybenzoxazole precursors, negative-type polybenzoxazole precursors may also be used.

[0099] (thermal curing) After development, the polybenzoxazole precursor can be heated to close the ring of the polybenzoxazole precursor, thereby forming the polybenzoxazole, which becomes the cured relief pattern, i.e., the insulating layer 6.

[0100] The heating temperature for thermal curing of the polybenzoxazole precursor is preferably low from the viewpoint of the influence on other members, and is preferably 250° C. or less, more preferably 230° C. or less, still more preferably 200° C. or less, and particularly preferably 180° C. or less.

[0101] <Polybenzoxazole> The structure of the cured relief pattern formed from the polybenzoxazole precursor has the following general formula (11): [ka] (In the formula, U and V are each independently a divalent organic group.) The polybenzoxazole includes the polybenzoxazole having the structure:

[0102] U in the general formula (11) is Y in the general formula (11A). 2 V in the general formula (11) may be the same as Y in the general formula (11A). 3 The preferred Y in the general formula (11A) is 2 , Y3 For the same reason, is also preferred for U and V in the general formula (11).

[0103] <Polymer having phenolic hydroxyl group> (A) Photosensitive resin The polymer having a phenolic hydroxyl group of the present embodiment is a resin having a phenolic hydroxyl group in the molecule, and is soluble in alkali. Specific examples include vinyl polymers containing a monomer unit having a phenolic hydroxyl group, such as poly(hydroxystyrene), phenol resins, poly(hydroxyamide), poly(hydroxyphenylene) ether, and polynaphthol. Among these, phenolic resins are preferred because of their low cost and small volumetric shrinkage during curing, and novolac-type phenolic resins are particularly preferred.

[0104] Phenolic resins are polycondensation products of phenol or its derivatives with aldehydes. The polycondensation is carried out in the presence of a catalyst such as an acid or a base. Phenolic resins obtained using an acid catalyst are called novolak-type phenolic resins.

[0105] Examples of phenol derivatives include phenol, cresol, ethylphenol, propylphenol, butylphenol, amylphenol, benzylphenol, adamantanephenol, benzyloxyphenol, xylenol, catechol, resorcinol, ethylresorcinol, hexylresorcinol, hydroquinone, pyrogallol, phloroglucinol, 1,2,4-trihydroxybenzene, pararosolic acid, biphenol, bisphenol A, bisphenol AF, bisphenol B, bisphenol F, and bisphenol S. , dihydroxydiphenylmethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,4-bis(3-hydroxyphenoxybenzene), 2,2-bis(4-hydroxy-3-methylphenyl)propane, α,α'-bis(4-hydroxyphenyl)-1,4-diisopropylbenzene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 2,2-bis(2-hydroxy-5-biphenylyl)propane, and dihydroxybenzoic acid.

[0106] Examples of aldehyde compounds include formaldehyde, paraformaldehyde, acetaldehyde, propionaldehyde, pivalaldehyde, butyraldehyde, pentanal, hexanal, trioxane, glyoxal, cyclohexylaldehyde, diphenylacetaldehyde, ethylbutyraldehyde, benzaldehyde, glyoxylic acid, 5-norbornene-2-carboxaldehyde, malondialdehyde, succindialdehyde, glutaraldehyde, salicylaldehyde, naphthaldehyde, and terephthalaldehyde.

[0107] The photosensitive resin (A) preferably contains component (a), a phenolic resin having no unsaturated hydrocarbon groups, and component (b), a modified phenolic resin having unsaturated hydrocarbon groups. It is more preferable that the component (b) is further modified by a reaction between a phenolic hydroxyl group and a polybasic acid anhydride.

[0108] From the viewpoint of further improving the mechanical properties (elongation at break, elastic modulus, and residual stress), it is preferable to use a phenolic resin modified with a compound having an unsaturated hydrocarbon group having 4 to 100 carbon atoms as the component (b).

[0109] (b) The modified phenolic resin having an unsaturated hydrocarbon group is generally a reaction product of phenol or a derivative thereof with a compound having an unsaturated hydrocarbon group (preferably having 4 to 100 carbon atoms) (hereinafter sometimes simply referred to as an "unsaturated hydrocarbon group-containing compound") (hereinafter referred to as an "unsaturated hydrocarbon group-modified phenol derivative") and an aldehyde, or a reaction product of a phenolic resin and an unsaturated hydrocarbon group-containing compound.

[0110] The phenol derivatives used here may be the same as the phenol derivatives described above as the raw material for the phenol resin as the (A) photosensitive resin.

[0111] From the viewpoints of adhesion and thermal shock resistance of a resist pattern, the unsaturated hydrocarbon group of the unsaturated hydrocarbon group-containing compound preferably contains two or more unsaturated groups. From the viewpoints of compatibility when made into a resin composition and flexibility of a cured film, the unsaturated hydrocarbon group-containing compound preferably has 8 to 80 carbon atoms, more preferably has 10 to 60 carbon atoms.

[0112] Examples of the unsaturated hydrocarbon group-containing compound include unsaturated hydrocarbons having 4 to 100 carbon atoms, polybutadiene having a carboxyl group, epoxidized polybutadiene, linoleyl alcohol, oleyl alcohol, unsaturated fatty acids, and unsaturated fatty acid esters. Suitable unsaturated fatty acids include crotonic acid, myristoleic acid, palmitoleic acid, oleic acid, elaidic acid, vaccenic acid, gadoleic acid, erucic acid, nervonic acid, linoleic acid, α-linolenic acid, eleostearic acid, stearidonic acid, arachidonic acid, eicosapentaenoic acid, sardine acid, and docosahexaenoic acid. Among these, esters of unsaturated fatty acids having 8 to 30 carbon atoms and monohydric to trihydric alcohols having 1 to 10 carbon atoms are more preferred, and esters of unsaturated fatty acids having 8 to 30 carbon atoms and glycerin, which is a trihydric alcohol, are particularly preferred.

[0113] Esters of unsaturated fatty acids having 8 to 30 carbon atoms and glycerin are commercially available as vegetable oils. Vegetable oils include non-drying oils with an iodine value of 100 or less, semi-drying oils with an iodine value of more than 100 and less than 130, and drying oils with an iodine value of 130 or more. Examples of non-drying oils include olive oil, morning glory seed oil, cashew seed oil, camellia oil, camellia oil, castor oil, and peanut oil. Examples of semi-drying oils include corn oil, cottonseed oil, and sesame oil. Examples of drying oils include tung oil, linseed oil, soybean oil, walnut oil, safflower oil, sunflower oil, perilla oil, and mustard oil. In addition, processed vegetable oils obtained by processing these vegetable oils may be used.

[0114] Among the above vegetable oils, it is preferable to use non-drying oils in order to prevent gelation caused by excessive reaction in the reaction between phenol or its derivatives or phenol resin and vegetable oil, and to improve yield.On the other hand, it is preferable to use drying oils in order to improve the adhesion, mechanical properties and thermal shock resistance of the resist pattern.Among the drying oils, tung oil, linseed oil, soybean oil, walnut oil and safflower oil are preferable, and tung oil and linseed oil are more preferable, because they can more effectively and reliably exhibit the effects of the present invention.

[0115] These unsaturated hydrocarbon group-containing compounds may be used alone or in combination of two or more.

[0116] In preparing the component (b), first, the phenol derivative and the unsaturated hydrocarbon group-containing compound are reacted to prepare an unsaturated hydrocarbon group-modified phenol derivative. The reaction is preferably carried out at 50 to 130°C. From the viewpoint of improving the flexibility of the cured film (resist pattern), the reaction ratio of the phenol derivative and the unsaturated hydrocarbon group-containing compound is preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, of the unsaturated hydrocarbon group-containing compound per 100 parts by mass of the phenol derivative. If the amount of the unsaturated hydrocarbon group-containing compound is less than 1 part by mass, the flexibility of the cured film tends to decrease, and if it exceeds 100 parts by mass, the heat resistance of the cured film tends to decrease. In the above reaction, p-toluenesulfonic acid, trifluoromethanesulfonic acid, or the like may be used as a catalyst as necessary.

[0117] The unsaturated hydrocarbon group-modified phenol derivative produced by the above reaction is polycondensed with aldehydes to produce a phenol resin modified with an unsaturated hydrocarbon group-containing compound. The aldehydes may be the same as those mentioned above for obtaining the phenol resin.

[0118] The reaction between the aldehydes and the unsaturated hydrocarbon group-modified phenol derivative is a polycondensation reaction, and conventionally known synthesis conditions for phenolic resins can be used. The reaction is preferably carried out in the presence of a catalyst such as an acid or a base, and more preferably an acid catalyst is used. Examples of the acid catalyst include hydrochloric acid, sulfuric acid, formic acid, acetic acid, p-toluenesulfonic acid, and oxalic acid. These acid catalysts can be used alone or in combination of two or more.

[0119] The reaction is preferably carried out at a reaction temperature of 100 to 120°C. The reaction time varies depending on the type and amount of the catalyst used, but is usually 1 to 50 hours. After the reaction is completed, the reaction product is dehydrated under reduced pressure at a temperature of 200°C or less to obtain a phenolic resin modified with an unsaturated hydrocarbon group-containing compound. In addition, a solvent such as toluene, xylene, or methanol can be used for the reaction.

[0120] The phenol resin modified with an unsaturated hydrocarbon group-containing compound can also be obtained by polycondensing the above-mentioned unsaturated hydrocarbon group-modified phenol derivative with an aldehyde together with a compound other than phenol such as m-xylene. In this case, the molar ratio of the compound other than phenol to the compound obtained by reacting the phenol derivative with the unsaturated hydrocarbon group-containing compound is preferably less than 0.5.

[0121] The component (b) can also be obtained by reacting the phenolic resin of the component (a) with an unsaturated hydrocarbon group-containing compound. The unsaturated hydrocarbon group-containing compound to be reacted with the phenolic resin can be the same as the unsaturated hydrocarbon group-containing compound described above.

[0122] The reaction between the phenolic resin and the unsaturated hydrocarbon group-containing compound is preferably carried out at 50 to 130°C. In addition, the reaction ratio between the phenolic resin and the unsaturated hydrocarbon group-containing compound is preferably 1 to 100 parts by mass of the unsaturated hydrocarbon group-containing compound, more preferably 2 to 70 parts by mass, and even more preferably 5 to 50 parts by mass, per 100 parts by mass of the phenolic resin, from the viewpoint of improving the flexibility of the cured film (resist pattern). If the amount of the unsaturated hydrocarbon group-containing compound is less than 1 part by mass, the flexibility of the cured film tends to decrease, and if it exceeds 100 parts by mass, the possibility of gelation during the reaction tends to increase, and the heat resistance of the cured film tends to decrease. At this time, p-toluenesulfonic acid, trifluoromethanesulfonic acid, or the like may be used as a catalyst, if necessary. In addition, a solvent such as toluene, xylene, methanol, or tetrahydrofuran can be used for the reaction.

[0123] The phenolic hydroxyl groups remaining in the phenolic resin modified by the unsaturated hydrocarbon group-containing compound produced by the above method are further reacted with a polybasic acid anhydride. This allows the acid-modified phenolic resin to be used as component (b). By acid-modifying with a polybasic acid anhydride, a carboxyl group is introduced, further improving the solubility of component (b) in an alkaline aqueous solution (developer).

[0124] The polybasic acid anhydride may have an acid anhydride group formed by dehydration condensation of the carboxyl groups of a polybasic acid having a plurality of carboxyl groups. Examples of the polybasic acid anhydride include dibasic acid anhydrides such as phthalic anhydride, succinic anhydride, octenyl succinic anhydride, pentadodecenyl succinic anhydride, maleic anhydride, itaconic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, nadic anhydride, 3,6-endomethylenetetrahydrophthalic anhydride, methylendomethylenetetrahydrophthalic anhydride, tetrabromophthalic anhydride and trimellitic anhydride, and aromatic tetrabasic acid dianhydrides such as biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, diphenylethertetracarboxylic dianhydride, butanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, pyromellitic anhydride and benzophenonetetracarboxylic dianhydride. These may be used alone or in combination of two or more. Among these, the polybasic acid anhydride is preferably a dibasic acid anhydride, more preferably one or more selected from the group consisting of tetrahydrophthalic anhydride, succinic anhydride, and hexahydrophthalic anhydride. In this case, there is an advantage that a resist pattern having a better shape can be formed.

[0125] The photosensitive resin (A) may further contain a phenolic resin that has been acid-modified by reacting it with a polybasic acid anhydride. When the photosensitive resin (A) contains a phenolic resin that has been acid-modified with a polybasic acid anhydride, the solubility of the photosensitive resin (A) in an aqueous alkaline solution (developer) is further improved.

[0126] Examples of the polybasic acid anhydride include dibasic acid anhydrides such as phthalic anhydride, succinic anhydride, octenyl succinic anhydride, pentadodecenyl succinic anhydride, maleic anhydride, itaconic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, methyl hexahydrophthalic anhydride, nadic anhydride, 3,6-endo methylene tetrahydrophthalic anhydride, methyl end methylene tetrahydrophthalic anhydride, tetrabromo phthalic anhydride, and trimellitic anhydride, and aliphatic and aromatic tetrabasic acid dianhydrides such as biphenyl tetracarboxylic acid dianhydride, naphthalene tetracarboxylic acid dianhydride, diphenyl ether tetracarboxylic acid dianhydride, butane tetracarboxylic acid dianhydride, cyclopentane tetracarboxylic acid dianhydride, pyromellitic anhydride, and benzophenone tetracarboxylic acid dianhydride. These may be used alone or in combination of two or more. Among these, the polybasic acid anhydride is preferably a dibasic acid anhydride, and more preferably, for example, one or more selected from the group consisting of tetrahydrophthalic anhydride, succinic anhydride, and hexahydrophthalic anhydride.

[0127] (B2) Photoacid generator Examples of the photoacid generator include diazonaphthoquinone compounds, aryl diazonium salts, diaryliodonium salts, triarylsulfonium salts, etc. Among these, diazonaphthoquinone compounds are preferred because of their high sensitivity.

[0128] (C) Additives The preferred types and amounts of the additive (C) are the same as those described in relation to the polyimide.

[0129] (D) Solvent The solvent (D) may be any solvent capable of dissolving or dispersing each of the components.

[0130] (E) Other It may contain a thermal crosslinking agent, a sensitizer, an adhesive assistant, a dye, a surfactant, a dissolution promoter, a crosslinking promoter, etc. Among these, by containing a thermal crosslinking agent, when the photosensitive resin film after pattern formation is heated and cured, the thermal crosslinking agent component reacts with the (A) photosensitive resin to form a crosslinked structure. This allows curing at a low temperature, and prevents the film from becoming brittle or melting. Specifically, the thermal crosslinking agent component may preferably be a compound having a phenolic hydroxyl group, a compound having a hydroxymethylamino group, or a compound having an epoxy group.

[0131] (Exposure and development) After the polymer having a phenolic hydroxyl group is exposed to light, unnecessary portions are washed away with a developer, such as an alkaline aqueous solution of sodium hydroxide, potassium hydroxide, sodium silicate, ammonia, ethylamine, diethylamine, triethylamine, triethanolamine, or tetramethylammonium hydroxide (TMAH).

[0132] (thermal curing) After development, the polymer having a phenolic hydroxyl group is heated to thermally crosslink the polymers having a phenolic hydroxyl group. The crosslinked polymer becomes a cured relief pattern, that is, the insulating layer 6.

[0133] The heating temperature for thermal curing of the polymer having a phenolic hydroxyl group is preferably low from the viewpoint of the influence on other members, and is preferably 250° C. or less, more preferably 230° C. or less, still more preferably 200° C. or less, and particularly preferably 180° C. or less.

[0134] <Method for manufacturing semiconductor device> The method for manufacturing the semiconductor device 1 of the present embodiment includes the steps of: A first step of preparing a semiconductor chip 2; a second step of covering the prepared semiconductor chip 2 with a sealing material so that at least a portion of the semiconductor chip 2 is exposed; A third step of forming a rewiring layer 4 having an area larger than that of the semiconductor chip 2 in a plan view on the exposed surface side of the semiconductor chip 2, The rewiring layer 4 has an oxygen permeability of 150 to 7000 cm 3 / m 2 Including an insulating layer 6 having a temperature of 100° C. to 350° C.

[0135] Here, the second step is A step of forming a protective layer on the semiconductor chip (protective layer forming step); It is preferable that the method further comprises a step of covering the semiconductor chip on which the protective layer has been formed with a sealing material so that at least a part of the protective layer is exposed (sealant forming step). The third step preferably includes a step of forming a redistribution layer on the protective layer side.

[0136] A manufacturing method of the semiconductor device 1 will be described with reference to FIG. 3. FIG. 3 shows an example of a manufacturing process of the semiconductor device 1. In FIG. 3A, a pre-processed wafer 10 is prepared. Then, a photosensitive resin composition (photosensitive composition for forming a protective layer) is applied, exposed and developed to form a relief pattern (protective layer forming process). Then, in FIG. 3B, the wafer is diced to form a plurality of semiconductor chips 2. The semiconductor chips 2 prepared in this manner are attached to a support 11 at a predetermined interval, as shown in FIG. 3C.

[0137] Next, the molding resin 12 is applied from above the semiconductor chip 2 onto the support 11, and mold sealing is performed as shown in FIG. 3D (sealing material forming step). Next, the support 11 is peeled off, and the molding resin 12 is inverted (see FIG. 3E). As shown in FIG. 3E, the semiconductor chip 2 and the molding resin 12 appear on approximately the same plane. Next, in the step shown in FIG. 3F, a photosensitive resin composition 13 is applied onto the semiconductor chip 2 and the molding resin 12. Then, the applied photosensitive resin composition 13 is exposed and developed to form a relief pattern (relief pattern forming step). The photosensitive resin composition 13 may be either a positive type or a negative type. Furthermore, the relief pattern is heated to form a cured relief pattern (insulating layer forming step). Furthermore, wiring is formed in the area where the cured relief pattern is not formed (wiring forming step).

[0138] In this embodiment, the relief pattern forming step, the insulating layer forming step, and the wiring forming step are combined into a rewiring layer forming step for forming a rewiring layer connected to the semiconductor chip 2.

[0139] The insulating layer in the redistribution layer may have multiple layers, and therefore the redistribution layer formation process may include a relief pattern formation process multiple times, an insulating layer formation process multiple times, and a wiring formation process multiple times.

[0140] Then, in Fig. 3G, a plurality of external connection terminals 7 corresponding to each semiconductor chip 2 are formed (bump formation), and dicing is performed between each semiconductor chip 2. This makes it possible to obtain a semiconductor device (semiconductor IC) 1 as shown in Fig. 3H. In this embodiment, a plurality of fan-out type semiconductor devices 1 can be obtained by the manufacturing method shown in Fig. 3.

[0141] In this embodiment, in the above-mentioned insulating layer forming process, it is preferable to form the insulating layer from a photosensitive resin composition capable of forming at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

[0142] In addition, when forming a protective layer, it is preferable to form such a protective layer from a photosensitive resin composition capable of forming at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

[0143] [Other embodiments] Although the present embodiment has been described above, the aspects of the present invention are not limited to the above.

[0144] For example, the encapsulant may include an encapsulating member that surrounds the side surface of the semiconductor chip and a tape that overlaps the top surface of the semiconductor chip (the surface opposite to the surface on which the insulating layer is disposed). The encapsulating member may be in contact with the insulating layer and may include an epoxy resin.

[0145] 1 shows the semiconductor chip 2 including two chips in parallel, the semiconductor chip may include three or more chips in parallel. Furthermore, the protective layer 8 may be omitted. In this case, the semiconductor chip and the sealing material form substantially the same surface, and the rewiring layer is disposed on this surface.

[0146] A further aspect of the present invention is A semiconductor chip 2; an encapsulant 3 that covers the semiconductor chip 2 so that at least a portion of the semiconductor chip 2 is exposed; A semiconductor device (1) including a redistribution layer (4) disposed on a surface side of a semiconductor chip (2) that is not covered by a sealing material (3) and having an area larger than that of the semiconductor chip (2) in a plan view, the semiconductor device (1) comprising an insulating layer (6) for use in forming the redistribution layer (4), Oxygen permeability is 150 to 7000 cm 3 / m 2 ·day·atm, and the insulating layer 6.

[0147] Furthermore, a further aspect of the present invention is A semiconductor chip 2; a sealing material that covers the semiconductor chip 2 so that at least a portion of the semiconductor chip 2 is exposed; In the semiconductor chip 2, a rewiring layer 4 is disposed on a surface side not covered by the sealing material and has an area larger than that of the semiconductor chip 2 in a plan view. Wiring 5 electrically connected to the semiconductor chip 2; In contact with the wiring 5 and having an oxygen permeability of 150 to 7000 cm 3 / m 2 and an insulating layer 6 having a thickness of 100 .mu.m and a redistribution layer 4 having a thickness of 100 .mu.m.

[0148] The requirements that can be adopted in the semiconductor device according to one embodiment of the present invention and that are preferable are also applicable and preferable in other embodiments (e.g., an insulating layer and a rewiring layer, and a method for manufacturing a semiconductor device) other than the semiconductor device. For example, the oxygen permeability (cm 3 / m 2 The above-mentioned range of 1000 nm to 1500 nm is also preferable for the insulating layer and the rewiring layer, and also for the manufacturing method of the semiconductor device. EXAMPLES

[0149] The present invention will be described below with reference to examples and comparative examples. In the examples and comparative examples, the following materials and measurement methods were used.

[0150] The abbreviations used in the examples and comparative examples are as follows. ODPA: 4,4'-oxydiphthalic dianhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride BPADA: 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic anhydride DADPE: 4,4'-diaminodiphenyl ether BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane m-TB: 4,4'-diamino-2,2'-dimethylbiphenyl MBAPP: 2,2-bis[4-(4-aminophenoxy)-3-methylphenyl]propane TFMB: 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl BAFL: 9,9'-bis(4-aminophenyl)fluorene DCC: dicyclohexylcarbodiimide HEMA: 2-hydroxyethyl methacrylate GBL: gamma-butyrolactone NMP: N-methyl-2-pyrrolidone

[0151] (Polymer A-1: ​​Synthesis of polyimide precursor) As tetracarboxylic dianhydride, 88.3 g of ODPA and 55.8 g of BPDA were placed in a 2-liter separable flask. Then, 128.4 g of HEMA and GBL were added, and pyridine (80 g) was further added while stirring at room temperature, thereby obtaining a reaction mixture. After the end of the heat generation due to the reaction, the mixture was allowed to cool to room temperature, and then left to stand for 16 hours.

[0152] Next, a solution of 192.7 g of DCC dissolved in GBL was added to the reaction mixture over 40 minutes while stirring under ice cooling. Then, 92.9 g of DADPE as a diamine suspended in GBL was added to the reaction mixture over 60 minutes while stirring. After stirring for 2 hours at room temperature, ethyl alcohol was further added and stirred for 1 hour, and then GBL was added. The precipitate formed in the reaction mixture was removed by filtration, thereby obtaining a reaction liquid.

[0153] Ethyl alcohol was added to the resulting reaction solution, thereby producing a precipitate consisting of a crude polymer. The produced crude polymer was filtered off and dissolved in tetrahydrofuran to obtain a crude polymer solution. The obtained crude polymer solution was dropped into water to precipitate the polymer, and the resulting precipitate was filtered off. The resulting polymer was then vacuum dried to obtain a powdered polymer (polyimide precursor (polymer A-1)). The weight average molecular weight (Mw) was 22,000.

[0154] (Polymer A-2: Synthesis of polyimide precursor) Polymer A-2 was obtained in the same manner as in the example of Polymer A-1, except that 246.8 g of BPADA was used as the tetracarboxylic dianhydride and 92.9 g of DADPE was used as the diamine. The weight average molecular weight (Mw) of Polymer A-2 was 21,000.

[0155] (Polymer A-3: Synthesis of polyimide precursor) Polymer A-3 was obtained in the same manner as in the example of Polymer A-1, except that 147.11 g of ODPA was used as the tetracarboxylic dianhydride and 190.5 g of BAPP was used as the diamine. The weight average molecular weight (Mw) of Polymer A-3 was 23,000.

[0156] (Polymer A-4: Synthesis of polyimide precursor) Polymer A-4 was obtained in the same manner as in the example of Polymer A-1, except that naphthalene dianhydride (127.2 g) was used as the tetracarboxylic dianhydride and m-TB (98.5 g) was used as the diamine. The weight average molecular weight (Mw) of Polymer A-4 was 20,000.

[0157] (Diamine Oligomer W-1: Synthesis of Polyimide) In a 0.5-liter separable flask equipped with a Dean-Stark tube and a cooling tube, 41.6 g of BPADA as an acid component, 34.0 g of m-TB as a diamine component, and 176.4 g of NMP as a solvent were added and stirred. 42.3 g of toluene was further added and stirred, and then the temperature was raised to 185°C under a nitrogen stream. After stirring at 185°C for 2.5 hours, the toluene in the system and the water generated by imidization were removed over 1.5 hours. Then, the solution was cooled to room temperature to obtain a solution of diamine oligomer W-1 having a repeating unit of a polyimide structure. The weight average molecular weight (Mw) of this diamine oligomer W-1 was 3,000. Diamine Oligomer W-1 1 The imide ring closure rate was confirmed by H-NMR measurement and comparing the peaks derived from the amide bonds with the peaks derived from the aromatic rings of the polyimide, and was found to be 99% or more.

[0158] (Diamine Oligomer W-2: Synthesis of Polyimide) In the synthesis method of the diamine oligomer W-1, except that 52.6g of MBAPP was used instead of 34.0g of m-TB, 220g of NMP as a solvent, and 52.8g of toluene were used, the same method as that of the example of the diamine oligomer W-1 was used to obtain a solution of diamine oligomer W-2. The weight average molecular weight (Mw) of this diamine oligomer W-2 was 5,000. As with diamine oligomer W-1, 1 The imide ring closure rate was confirmed by H-NMR measurement, which was found to be 99% or more.

[0159] (Polymer B-1: Synthesis of polyimide precursor having polyimide moiety) As an acid component, 20.9 g of BPADA was placed in a 1-liter separable flask, and 10.9 g of HEMA and 42 g of GBL were added. 6.4 g of pyridine was added while stirring at room temperature, and the mixture was heated at 50°C for 4 hours. After the heat generation by the reaction had ceased, the mixture was allowed to cool to room temperature. The mixture was then allowed to stand for another 16 hours to obtain a reaction mixture.

[0160] Next, under ice cooling, a solution in which 16.3 g of DCC was dissolved in 16.3 g of GBL was added to the reaction mixture over 40 minutes while stirring. Then, 91.0 g of GBL was added. Next, a solution in which 101.7 g of the NMP solution of the diamine oligomer W-2 prepared above was mixed with 66.5 g of GBL as the diamine component was added over 20 minutes while stirring. Next, a solution in which 2.4 g of m-TB was dissolved in 7 g of GBL was added over 5 minutes while stirring. After further stirring at room temperature for 4 hours, 6.4 g of ethyl alcohol was added and stirred for 30 minutes, and then 49.0 g of GBL was added. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction solution.

[0161] The reaction solution thus obtained was added to 1000 g of ethyl alcohol to produce a precipitate consisting of a crude polymer. The crude polymer thus produced was filtered and dissolved in 270 g of GBL to obtain a crude polymer solution. The crude polymer solution thus obtained was eluted with an anion exchange resin ("Amberlyst" manufactured by Organo Corporation) and then cooled to 30° C. for 1 hour. TM The polymer was purified using a 15JWET filter to obtain a polymer solution. The obtained polymer solution was dropped into 3800 g of water to precipitate the polymer, and the obtained precipitate was collected by filtration. The polymer was then dried in a vacuum to obtain a powdered polymer B-1. The weight average molecular weight (Mw) of this polymer B-1 was 30,000, and the imide group introduction rate was 0.43. The imide group concentration U per repeating unit of the polyimide obtained from the polymer B-1 was 16.0 wt %. The "imide group concentration U" was calculated by converting it to the polyimide of the polyimide cured film obtained by heating and curing at 350°C (hereinafter the same).

[0162] (Polymer B-2: Synthesis of polyimide precursor having polyimide moiety) As an acid component, 15.2 g of BPADA was placed in a 1-liter separable flask, and 7.9 g of HEMA and 30.8 g of GBL were added. 4.6 g of pyridine was added while stirring at room temperature, and the mixture was heated at 50°C for 4 hours. After the heat generation caused by the reaction had ceased, the mixture was allowed to cool to room temperature. The mixture was then left to stand for another 16 hours to obtain a reaction mixture.

[0163] Next, under ice cooling, a solution of 11.9 g of DCC dissolved in 11.9 g of GBL was added to the reaction mixture over 40 minutes while stirring. Then, 91.0 g of GBL was added. Next, a solution of 111.5 g of the NMP solution of the diamine oligomer W-1 prepared above mixed with 72.9 g of GBL was added as the diamine component over 20 minutes while stirring. After further stirring at room temperature for 4 hours, 49.0 g of GBL was added. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction liquid.

[0164] The subsequent purification steps were carried out in the same manner as in the case of polymer B-1 to obtain polymer B-2. The weight average molecular weight (Mw) of this polymer B-2 was 24,000, and the imide group introduction rate was 0.58. The imide group concentration U per repeating unit of the polyimide obtained from polymer B-2 was 20.1 wt%.

[0165] (Polymer C-1: Synthesis of solvent-soluble polyimide) In a nitrogen-purged three-neck flask equipped with a Dean-Stark extractor, 100.0 g of NMP and 34.9 g (0.1 mol) of BAFL were added and dissolved, and 15.6 g (0.05 mol) of ODPA and 25.0 g of toluene were added thereto and heated to 180°C.

[0166] After it was confirmed that the theoretical amounts of water (1.80 g) and the added toluene (25.0 g) had been extracted in the Dean-Stark extraction apparatus, the heating was stopped and the mixture was cooled to room temperature.

[0167] To the resulting reaction solution, 15.5 g (0.1 mol) of Karenz (registered trademark) MOI (product name; manufactured by Showa Denko K.K.) was added and stirred to obtain a polymer solution. The resulting polymer solution was dropped into 3 kg of water to precipitate the polymer, which was then filtered off. The resulting solution was then vacuum dried to obtain polyimide C-1 with modified ends in powder form. The weight average molecular weight (Mw) of this polyimide C-1 was 4,400, the number average molecular weight (Mn) was 3,400, and the polydispersity (Mw / Mn) was 1.29. Based on the integral ratio of proton NMR, it was confirmed that the modification rate of the polyimide main chain terminals was 95%.

[0168] (Polymer C-2: Synthesis of solvent-soluble polyimide) Polyimide C-2 was obtained in the same manner as in Production Example 1, except that the amount of BAFL was changed to 26.2 g and the amount of Karenz MOI was changed to 7.8 g. The weight average molecular weight (Mw) of polyimide C-2 was 6,900, the number average molecular weight (Mn) was 5,200, and the polydispersity (Mw / Mn) was 1.33. Moreover, it was confirmed from the integral ratio of proton NMR that the modification rate of the above-mentioned terminal was 94%.

[0169] (Polymer C-3: Synthesis of solvent-soluble polyimide) 64.1g of TFMB was placed in a 1-liter separable flask, and 400ml of GBL was added under a nitrogen atmosphere. 97.7g of 6FDA was added while stirring at room temperature, and the mixture was stirred at room temperature for 6 hours to obtain a polyamic acid solution. Then, 15g of pyridine and 80g of acetic anhydride were added, and 40g of toluene was added. The mixture was then stirred at 185°C for 4 hours, and it was confirmed that the theoretical amount of water was removed. After removing the toluene, the mixture was cooled to room temperature to obtain a solution containing polyimide (polymer C-3). The obtained solution was subjected to post-treatment based on the same method as in the example of polymer C-1 (polymer precipitation, filtration, and vacuum drying), to obtain polymer C-3. The weight average molecular weight (Mw) of this polymer C-3 was 22,000.

[0170] [Formulation examples 1-12] The components were mixed as shown in the table below to obtain a solution of a photosensitive resin composition. Note that the unit of the amount of each component in Table 1 is parts by mass. The oxygen permeability, short circuit time after a BHAST (Biased Highly Accelerated temperature and humidity Stress Test) test, developability, and adhesion shown in the table were measured by the following methods.

[0171] [Table 1]

[0172] The symbols in Table 1 represent the following compounds. Photoinitiator D-1: 1,2-propanedione-3-cyclopentyl-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime) (trade name: PBG-305, manufactured by Changzhou Strong Electronics Co., Ltd.) D-2: 1-[4-(phenylthio)phenyl]-3-propane-1,2-dione-2-(O-acetyloxime) (trade name: PBG-3057, Changzhou Strong Electronics Co., Ltd.) Silane Coupling Agent E-1: 3-glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd.) Radical Polymerizable Compound F-1: Polyethylene glycol #200 dimethacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.) Fluorine-Based Monomers G-1: 2,2,2-trifluoroethyl methacrylate solvent H-1: γ-butyrolactone (GML) H-2: Dimethyl sulfoxide (DMSO)

[0173] (Oxygen permeability) The photosensitive resin composition prepared above was spin-coated onto a 6-inch silicon wafer substrate having an aluminum deposition layer on its surface so that the film thickness after curing was 10 μm, and the substrate was pre-baked at 110° C. for 4 minutes. The substrate was then subjected to a heat curing treatment at 230° C. for 2 hours using a vertical curing furnace (Koyo Lindberg, model name VF-2000B), thereby producing a wafer on which a resin film (insulating layer) was formed. The wafer was immersed overnight in a dilute hydrochloric acid solution to peel off the resin film pieces, which were then dried. The pieces were cut into pieces 50 mm long x 50 mm long and used as samples. The samples obtained above were subjected to oxygen transmission rate (cm 3 / m 2 That is, the measurement was performed using the measurement device GTR-10XF, with the measurement environment at 23°C, relative humidity (RH) at 65%, gas type at 23°C, and cell diameter at 35 mmΦ.

[0174] (Short circuit duration after BHAST test) A TEG (Test Element Group) with a line / space (L / S) of 5 μm / 5 μm was prepared, and oxygen plasma treatment was performed for 2 minutes at 40 mL / min, 133 W, 50 Pa using a low pressure plasma (EXAM, manufactured by Shinko Seiki Co., Ltd.). The resin composition was then spin-coated using a coater developer (D-Spin60A, manufactured by SOKUDO Co., Ltd.), pre-baked on a hot plate at 110°C for 240 seconds, and a coating film was formed so that the final film thickness was 7 μm. After the coating film was formed, the substrate was immediately exposed to light with an exposure dose of 300 to 600 mJ / cm2 (here, within 5 minutes after the coating film was formed). 2 After development, the film was heated at 230° C. for 2 hours in a nitrogen atmosphere using a temperature-rising programmable curing furnace (VF-2000 type, manufactured by Koyo Lindberg Co., Ltd.) to prepare a sample.

[0175] This sample was tested at 130°C and 85% RH with an applied voltage of 1 V using a BHAST test device (Highly Accelerated Life Test Device, Espec Corp.: EMS-222M, Electrochemical Migration Evaluation System, Espec Corp.: AMI-025-U-5). The insulation resistance between the copper wirings arranged in the insulating layer was measured at 30-minute intervals, and the insulation resistance was 1×10 4 The time when the resistance became equal to or less than Ω was regarded as the time when the dielectric breakdown occurred. The time from the start of the test to the dielectric breakdown was calculated and evaluated according to the following criteria. "Excellent": 500+ hours "Good": 200 to 500 hours "OK": 24 hours or more but less than 200 hours "Not possible": Less than 24 hours

[0176] [Example 1] (Fabrication of insulating layers, rewiring layers and semiconductor devices) The top and side surfaces of a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) serving as a semiconductor chip were covered with epoxy resin serving as a molding resin to form a sealing material.

[0177] (developability) On the lower surface of the wafer (the surface of the wafer not covered with the encapsulant), a 200 nm thick Ti layer and a 400 nm thick Cu layer were sputtered in this order using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Next, the resin composition of Formulation Example 1 was spin-coated on the wafer using a coater developer (D-Spin60A model, manufactured by SOKUDO Corporation), and then pre-baked on a hot plate at 110°C for 180 seconds, thus forming a coating film with a final thickness of 5 μm.

[0178] After the coating film was formed, the coating film was irradiated with energy of 400 mJ / cm2 using a test pattern mask by Prisma GHI (manufactured by Ultratech Co., Ltd.) immediately (here, less than 5 minutes after the coating film was formed). Next, the coating film was spray-developed with a coater developer (D-Spin60A type, manufactured by SOKUDO Co., Ltd.) using cyclopentanone as a developer for a time multiplied by 1.4 the time until the unexposed part was completely dissolved and disappeared. After that, a relief pattern (Example 1A) on Cu was obtained by rotating and spray-rinsing with propylene glycol methyl ether acetate for 10 seconds (relief pattern formation process). Then, it was evaluated according to the following criteria. "Good": A 7μm via hole was formed in this process. "OK": A 10μm via hole was formed in this process. "Not acceptable": Via holes of 10 μm or less could not be formed using this process. In the above evaluation, "a via hole was formed" means that when the cross section of the relief pattern was observed with a field emission scanning electron microscope (FE-SEM) S-4800 (manufactured by Hitachi High-Technologies Corporation), the via hole was observed to have no residue, bridging, or footing at the bottom of the via hole.

[0179] The wafer with the relief pattern formed on Cu was heated in a temperature-programmable curing furnace (VF-2000, manufactured by Koyo Lindberg) at 230°C for 2 hours in a nitrogen atmosphere to obtain a cured relief pattern of about 5 μm thickness made of resin on Cu (insulating layer forming step; first insulating layer). On the obtained relief pattern, 200 nm thick Ti and 400 nm thick Cu were sputtered in this order using the above-mentioned sputtering device (wiring forming step; wiring).

[0180] The photosensitive resin composition obtained in Formulation Example 1 was spin-coated on the relief pattern after sputtering using a coater developer (D-Spin60A type, manufactured by SOKUDO Co., Ltd.) in the same manner, and then pre-baked on a hot plate at 110°C for 180 seconds, thus forming a coating film. The obtained coating film was heat-treated at 230°C for 2 hours under a nitrogen atmosphere using a temperature-rise programmable curing furnace (VF-2000 type, manufactured by Koyo Lindberg Co., Ltd.), thereby obtaining a cured film made of a resin having a thickness of about 5 μm on the relief pattern of the cured product of Formulation Example 1 (second insulating layer). This formed a rewiring layer including the first insulating layer, wiring, and the second insulating layer.

[0181] Then, a plurality of external connection terminals corresponding to each semiconductor chip were formed (bump formation) on the side opposite to the sealing material of the rewiring layer, and each semiconductor chip was diced to produce the semiconductor device of Example 1. This semiconductor device is a fan-out type wafer-level chip size package type semiconductor device.

[0182] (Adhesion) For the semiconductor device of Example 1 prepared above, the cured film (second insulating layer) having a thickness of about 5 μm formed on the relief pattern of the cured product (first insulating layer) in the rewiring layer was treated at 130° C. and 85% RH for 168 hours, and then the adhesion properties between the copper substrate and the insulating layer (cured resin coating film) were evaluated based on the following criteria in accordance with the cross-cut method of JIS K 5600-5-6 standard. "Excellent": The lattice number of the insulating layer attached to the substrate is 80 to 100. "Good": The number of lattices in the insulating layer attached to the substrate is 60 or more but less than 80. "Acceptable": The number of lattices in the insulating layer attached to the substrate is between 40 and 60. "Not acceptable": The number of lattices in the insulating layer attached to the substrate is less than 40

[0183] [Examples 2 to 10, Comparative Examples 1 and 2] Using Blending Examples 2 to 12, tests were carried out in the same manner as in Example 1. The results are shown in Table 1. Note that for each Blending Example, the optimal exposure dose and development time were calculated before preparation, and then each test was carried out.

[0184] [Table 2]

[0185] As is clear from the table, according to the examples, good results were obtained in all of the evaluations of "oxygen permeability," "short circuit time after BHAST test," "developability," and "adhesion." In addition, as is clear from the table, by appropriately changing the types and contents of the polymer, fluorine-based monomer, photopolymerization initiator, silane coupling agent, and radical polymerization initiator in Example 1 using Blending Example 1, the oxygen permeability (cm 3 / m 2 It was confirmed that the temperature (days·atm) could be appropriately controlled. [Industrial Applicability]

[0186] The present invention is preferably applied to a semiconductor device having a semiconductor chip and a rewiring layer connected to the semiconductor chip, and in particular to a fan-out type wafer level chip size package type semiconductor device. [Explanation of symbols]

[0187] 1 Semiconductor device 2. Semiconductor chips 2a terminal 3. Encapsulating material 4 Redistribution layer 5. Wiring 6 Insulating layer (interlayer insulating film) 7 External connection terminal 8 Protective layer 8a hole 10 Wafers 11 Support 12 Molding resin 13 Photosensitive resin composition

Claims

1. A semiconductor chip; an encapsulant that covers the semiconductor chip so that at least a portion of the semiconductor chip is exposed; a redistribution layer disposed on a surface of the semiconductor chip that is not covered by the sealing material and has an area larger than that of the semiconductor chip in a plan view; The rewiring layer has an oxygen permeability of 150 to 7000 cm 3 / m 2 .An insulating layer having a thermal conductivity of 100 .mu.m.

2. The semiconductor device according to claim 1 , wherein the insulating layer has a layer structure of three or more layers.

3. The semiconductor device according to claim 1 , wherein the semiconductor chip comprises a plurality of chips.

4. The semiconductor device according to claim 1 , wherein the sealing material is in contact with the insulating layer.

5. The semiconductor device according to claim 1 , wherein the sealing material includes an epoxy resin.

6. The oxygen permeability is 250 to 5000 cm 3 / m 2 2. The semiconductor device according to claim 1, wherein the temperature is 0.5° C.-1 ...

7. The oxygen permeability is 150 to 400 cm 3 / m 2 2. The semiconductor device according to claim 1, wherein the temperature is 0.5° C.-1 ...

8. The oxygen permeability is 150 to 350 cm 3 / m 2 2. The semiconductor device according to claim 1, wherein the temperature is 0.5° C.-1 ...

9. The oxygen permeability is 150 to 300 cm 3 / m 2 2. The semiconductor device according to claim 1, wherein the temperature is 0.5° C.-1 ...

10. The oxygen permeability is 400 to 7000 cm 3 / m 2 2. The semiconductor device according to claim 1, wherein the temperature is 0.5° C.-1 ...

11. The oxygen permeability is 450 to 7000 cm 3 / m 2 2. The semiconductor device according to claim 1, wherein the temperature is 0.5° C.-1 ...

12. The oxygen permeability is 500 to 7000 cm 3 / m 2 2. The semiconductor device according to claim 1, wherein the temperature is 0.5° C.-1 ...

13. The insulating layer is made of carbon (C), hydrogen (H), nitrogen (N), oxygen (O), silicon (Si), and titanium (Ti). Semiconductor device.

14. The semiconductor device according to claim 1 , wherein the insulating layer is halogen-free.

15. 2. The semiconductor device according to claim 1, wherein said insulating layer includes at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

16. The insulating layer contains polyimide, and when IR spectrum measurement is performed by an attenuated total reflection method (ATR method), -1 The peak height near 1500 cm -1 The peak height near the peak height and the peak ratio (1380 cm -1 Near peak height: 1500 cm -1 2. The semiconductor device according to claim 1, wherein the peak height (above peak height) is 0.2 to 2.

5.

17. The semiconductor device optionally includes a protective layer for protecting the semiconductor chip; When the semiconductor device includes the protective layer, the protective layer is formed on the semiconductor chip, The semiconductor device according to claim 1 , wherein the insulating layer is disposed between the first and second electrodes.

18. The semiconductor device according to claim 17 , wherein the protective layer is in contact with at least one of the semiconductor chip and the insulating layer.

19. The protective layer has holes formed therein, The semiconductor device according to claim 17 , wherein the semiconductor chip and a wiring electrically connected to the semiconductor chip are electrically connected to each other through the hole.

20. 20. The semiconductor device according to claim 19, wherein a ratio of an opening area resulting from the holes to a surface of the protective layer on the semiconductor chip side is less than half.

21. 18. The semiconductor device according to claim 17, wherein the protective layer includes at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

22. The protective layer contains polyimide, and when IR spectrum measurement is performed by an attenuated total reflection method (ATR method), -1 The peak height near 1500 cm -1 The peak height near the peak height and the peak ratio (1380 cm -1 Near peak height: 1500 cm -1 18. The semiconductor device according to claim 17, wherein the peak height (above peak height) is 1.2 to 2.

5.

23. At least one of the protective layer and the insulating layer is represented by the following general formula (1): 【Chemistry 1】 (In the formula, X 1 is a tetravalent organic group derived from a tetracarboxylic dianhydride, Y 1 Is, Zia is a divalent organic group derived from amine, and m is an integer of 1 or more.

20. The semiconductor device of claim 17, comprising a polyimide having a structure of:

24. X in the general formula (1) 1 is a tetravalent organic group containing an aromatic ring, Y in the general formula (1) 1 The semiconductor device according to claim 23 , wherein is a divalent organic group containing an aromatic ring.

25. X in the general formula (1) 1 is represented by the following general formulas (2) to (5): 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 (In the formula, R 9 teeth 、 is an oxygen atom, a sulfur atom, or a divalent organic group. 【Chemistry 5】 24. The semiconductor device of claim 23, comprising at least one structure represented by:

26. X in the general formula (1) 1 is represented by the following general formula (6): 【Chemistry 6】 26. The semiconductor device of claim 25, comprising a structure represented by:

27. Y in the general formula (1) 1 is represented by the following general formulas (7) to (9): 【Chemistry 7】 (In the formula, R 10 , R 11 , R 12 and R 13 are each independently a hydrogen atom, a monovalent aliphatic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different. 【Chemistry 8】 (In the formula, R 14 ~R 21 are each independently a hydrogen atom, a halogen atom, a monovalent organic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different. 【Chemistry 9】 (In the formula, R 22 is a divalent group or an oxygen atom, R 23 ~R 30 are each independently a hydrogen atom, a halogen atom, a monovalent aliphatic group having 1 to 5 carbon atoms, or a hydroxyl group, and may be the same or different from each other; k is an integer of 1 to 3, and when k is 2 or 3, R 22 , R 23 , R 24 , R 27 , R 28 may be the same or different.) 24. The semiconductor device of claim 23, comprising at least one structure represented by:

28. Y in the formula (1) 1 is represented by the following general formula (10): 【Chemistry 10】 24. The semiconductor device of claim 23, comprising a structure represented by:

29. The insulating layer is formed of the following general formula (11): 【Chemistry 11】 (In the formula, U and V are each independently a divalent organic group.) 16. The semiconductor device of claim 15, comprising the polybenzoxazole having the structure:

30. 30. The semiconductor device according to claim 29, wherein U in the general formula (11) is a divalent organic group having 1 to 30 carbon atoms.

31. 30. The semiconductor device according to claim 29, wherein U in said general formula (11) is a chain alkylene group having 1 to 8 carbon atoms and in which some or all of the hydrogen atoms are substituted with fluorine atoms.

32. 30. The semiconductor device according to claim 29, wherein V in the general formula (11) is a divalent organic group having 1 to 40 carbon atoms.

33. 30. The semiconductor device according to claim 29, wherein V in the general formula (11) is a divalent chain aliphatic group having 1 to 20 carbon atoms.

34. 30. The semiconductor device according to claim 29, wherein V in the general formula (11) is a divalent organic group containing an aromatic group.

35. V in the general formula (11) is represented by the following general formulas (7) to (9): 【Chemistry 12】 (In the formula, R 10 , R 11 , R 12 and R 13 are each independently a hydrogen atom or a group having 1 to 5 carbon atoms. are monovalent aliphatic groups, and may be the same or different. 【Chemistry 13】 (In the formula, R 14 ~R 21 are each independently a hydrogen atom, a halogen atom, or a group having 1 to 5 carbon atoms. are monovalent organic groups, and may be the same or different. 【Chemistry 14】 (In the formula, R 22 is a divalent group or an oxygen atom, R 23 ~R 30 are each independently hydrogen atoms, halogen atoms, and monovalent aliphatic groups having 1 to 5 carbon atoms, k is an integer from 1 to 3, and when k is 2 or 3, R 22 , R 23 , R 24 , R 27 , R 28 may be the same or different.) 30. The semiconductor device of claim 29, comprising at least one structure represented by:

36. V in the general formula (11) is represented by the following general formula (10): 【Chemistry 15】 30. The semiconductor device of claim 29, comprising a structure represented by:

37. The semiconductor device according to claim 15 , wherein the polymer having a phenolic hydroxyl group includes a novolac type phenolic resin.

38. 16. The semiconductor device according to claim 15, wherein the polymer having a phenolic hydroxyl group includes a phenol resin having no unsaturated hydrocarbon group and a modified phenol resin having an unsaturated hydrocarbon group.

39. 2. The semiconductor device according to claim 1, wherein said insulating layer includes a first insulating layer and a second insulating layer having a different composition from said first insulating layer.

40. The semiconductor device according to any one of claims 1 to 39, wherein the semiconductor device is a fan-out type, wafer level chip size package type semiconductor device.

41. A first step of preparing a semiconductor chip; a second step of covering the prepared semiconductor chip with an encapsulant so that at least a portion of the semiconductor chip is exposed; and a third step of forming a redistribution layer having an area larger than that of the semiconductor chip in a plan view on the exposed surface side of the semiconductor chip. A method for manufacturing a semiconductor device, comprising: The redistribution layer has an oxygen permeability of 150 to 7000 cm 3 / m 2 A method for manufacturing a semiconductor device including an insulating layer having a temperature of 100° C. to 300° C.

42. 42. The method for producing a semiconductor device according to claim 41, wherein the insulating layer is formed from a photosensitive resin composition capable of forming at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

43. The second step comprises: forming a protective layer on the semiconductor chip; covering the semiconductor chip on which the protective layer is formed with an encapsulant so that at least a portion of the protective layer is exposed; The third step comprises:

43. The method for manufacturing a semiconductor device according to claim 41, further comprising the step of forming the redistribution layer on the protective layer side.

44. 44. The method for producing a semiconductor device according to claim 43, wherein the protective layer is formed from a photosensitive resin composition capable of forming at least one selected from the group consisting of polyimide, polybenzoxazole, and a polymer having a phenolic hydroxyl group.

45. A semiconductor chip; an encapsulant that covers the semiconductor chip so that at least a portion of the semiconductor chip is exposed; a redistribution layer disposed on a surface side of the semiconductor chip that is not covered by the sealing material and has an area larger than that of the semiconductor chip in a plan view; Oxygen permeability is 150 to 7000 cm 3 / m 2 An insulating layer, which is .days.atm.

46. A semiconductor chip; an encapsulant that covers the semiconductor chip so that at least a portion of the semiconductor chip is exposed; In a semiconductor chip comprising: a redistribution layer disposed on a surface side not covered by the sealing material and having an area larger than that of the semiconductor chip in a plan view; Wiring electrically connected to the semiconductor chip; The wiring is in contact with the oxygen permeability of 150 to 7000 cm 3 / m 2 and an insulating layer having a conductivity of 100 .mu.m.

Citation Information

Patent Citations

  • Manufacturing method for semiconductor device

    JP2011129767A