Semiconductor device
The semiconductor device addresses void-related fluctuations in oxide transistor performance by using silicon oxide and silicon nitride insulating films to cover voids, improving reliability and performance.
Patent Information
- Application Number
- JP2024112344
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2012-07-20
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2033-07-16
AI Technical Summary
Transistors using oxide semiconductors in semiconductor devices experience fluctuations in electrical characteristics due to voids in the interlayer insulating films, which affect the stability and performance of the devices.
The semiconductor device incorporates a configuration with a source and drain electrode on a semiconductor film, a first insulating film with silicon oxide, and a second insulating film of silicon nitride to cover voids in the stepped regions, preventing further expansion and infiltration of moisture and hydrogen-containing compounds.
This configuration suppresses fluctuations in electrical characteristics, enhancing the reliability and performance of the semiconductor device by maintaining high integration and speed while preventing moisture and hydrogen infiltration.
Smart Images

Figure 2024133232000001_ABST
Abstract
Description
[Technical field]
[0001] The invention disclosed in this specification and the like relates to a semiconductor device and a method for manufacturing the semiconductor device.
[0002] In this specification and the like, a semiconductor device is a device that can function by utilizing semiconductor characteristics. Electro-optical devices, image display devices, semiconductor circuits, and electronic equipment are all semiconductor devices. It is located. [Background technology]
[0003] A technology for constructing transistors using a semiconductor thin film formed on a substrate with an insulating surface. The transistor is being used in integrated circuits (ICs) and image display devices (not simply called display devices). Semiconductors that can be used in transistors are widely used in electronic devices such as Silicon-based semiconductor materials are widely known as conductive thin films, but other materials include oxides. Semiconductors are in the spotlight.
[0004] For example, zinc oxide or an In-Ga-Zn oxide semiconductor is used as the oxide semiconductor. A technique for fabricating a transistor using this has been disclosed (see Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-165528 A Summary of the Invention [Problem to be solved by the invention]
[0006] In addition, for example, a semiconductor device (such as a liquid crystal panel) using a transistor including an oxide semiconductor When making a transistor using an oxide semiconductor, it is necessary to provide an interlayer insulating film on the transistor. .
[0007] In integrated circuits, the interlayer insulating film not only provides insulation between transistors and wiring, and between wirings, This is an important factor in stabilizing the characteristics of a transistor.
[0008] In view of the above, the present invention provides a semiconductor device having an interlayer insulating film on a transistor using an oxide semiconductor. One object is to suppress fluctuations in the electrical characteristics of a device. [Means for solving the problem]
[0009] One embodiment of the present invention is a semiconductor device formed by a source electrode and a drain electrode on a semiconductor film. a first insulating film having a gap in a step region formed by the first insulating film and containing silicon oxide as a component; The insulating film is provided in contact with the first insulating film so as to fill the gaps in the insulating film. The second insulating film includes a first insulating film. It is possible to prevent the void from spreading further outward. The configuration may be as follows.
[0010] One aspect of the present invention is a semiconductor device that at least partially overlaps with a gate electrode via a gate insulating film. a source electrode and a drain electrode having an area contacting a part of the upper surface of the semiconductor film; , a source electrode, a drain electrode and a semiconductor film are covered, and the source electrode and the drain electrode on the semiconductor film are The step region formed by the drain electrode and the gate electrode has a gap, and the step region is made of silicon oxide. and a first insulating film including a first insulating film and a second insulating film provided in contact with the first insulating film so as to fill the void portion of the first insulating film. and a second insulating film containing silicon nitride as a component.
[0011] Another embodiment of the present invention is a semiconductor film having a region in contact with a part of an upper surface of the semiconductor film. A source electrode and a drain electrode, and a semiconductor film are covered with the source electrode, the drain electrode and the semiconductor film. A gap is provided in a step region formed by the source electrode and the drain electrode on the conductive film. The first insulating film contains silicon oxide as a component, and a second insulating film is formed so as to fill the gaps of the first insulating film. a second insulating film including silicon nitride as a component and provided in contact with the first insulating film; and a gate electrode overlapping the semiconductor film with an insulating film interposed therebetween.
[0012] Another embodiment of the present invention is a semiconductor device having the above structure, The doped electrode is a multilayer structure including a first conductive film in contact with the semiconductor film and a second conductive film on the first conductive film. It has a layered structure, and the side end surface of the second conductive film is on the upper surface of the first conductive film.
[0013] Another embodiment of the present invention is a semiconductor device having the above structure, is 2.26g / cm 3 More than 2.50g / cm 3 It is preferable that the following is true:
[0014] Another embodiment of the present invention is a semiconductor device having the above structure, wherein the first insulating film is an oxide film. It is preferable that the first insulating film is a silicon nitride film, and the second insulating film is a silicon nitride film.
[0015] Another embodiment of the present invention is a semiconductor device having the above structure, wherein the thickness of the first insulating film is , which is greater than the thickness of the second insulating film.
[0016] Another embodiment of the present invention is a semiconductor device having the above structure, in which the semiconductor film is an oxide semiconductor. A conductive film is preferable.
[0017] In another embodiment of the present invention, a gate insulating film is provided between the gate electrode and the semiconductor device. a source electrode having a region in contact with a portion of the upper surface of the semiconductor film; and forming a source electrode, a drain electrode, and a semiconductor film on the semiconductor film. The step region formed by the source electrode and the drain electrode has a gap, A first insulating film containing silicon dioxide as a component is formed, and a void portion of the first insulating film is filled with silicon dioxide. A second insulating film containing silicon nitride as a component is formed in contact with the first insulating film. A method for manufacturing a semiconductor device.
[0018] In another embodiment of the present invention, a semiconductor film is formed, and a contact hole is formed in contact with a part of an upper surface of the semiconductor film. forming a source electrode and a drain electrode having a region; A semiconductor film is covered and formed by a source electrode and a drain electrode on the semiconductor film. A first insulating film having a gap in a step region and containing silicon oxide as a component is formed, A silicon nitride film is provided in contact with the first insulating film to fill the gaps in the insulating film. forming a second insulating film including the semiconductor film, and forming a gate electrode on the second insulating film so as to overlap the semiconductor film; A method for manufacturing a semiconductor device.
[0019] Another embodiment of the present invention is a method for manufacturing a semiconductor device having the above structure, further comprising: The drain electrode is formed of a first conductive film in contact with the semiconductor film and a second conductive film on the first conductive film. The first conductive film and the second conductive film are etched to form an etched structure. The etching process causes the side end surfaces of the second conductive film to be on the upper surface of the first conductive film.
[0020] Another embodiment of the present invention is a method for manufacturing a semiconductor device having the above structure, further comprising: The film density is 2.26g / cm 3 More than 2.50g / cm 3 It is preferable that the following is true:
[0021] Another embodiment of the present invention is a method for manufacturing a semiconductor device having the above structure, further comprising: It is preferable that the first insulating film is a silicon oxynitride film, and the second insulating film is a silicon nitride film.
[0022] Another embodiment of the present invention is a method for manufacturing a semiconductor device having the above structure, further comprising: The thickness of the film is greater than the thickness of the second insulating film.
[0023] Another embodiment of the present invention is a method for manufacturing a semiconductor device having the above structure, An oxide semiconductor film is preferable. Effect of the Invention
[0024] According to one embodiment of the present invention, a highly reliable semiconductor device in which fluctuations in electrical characteristics are suppressed is provided. It is possible. [Brief description of the drawings]
[0025] [Figure 1] 1A and 1B are a plan view and a cross-sectional view illustrating one embodiment of a semiconductor device. [Diagram 2] 1A to 1C illustrate an example of a method for manufacturing a semiconductor device. [Diagram 3] 1A to 1C illustrate an example of a method for manufacturing a semiconductor device. [Figure 4] 1A and 1B are a plan view and a cross-sectional view illustrating one embodiment of a semiconductor device. [Diagram 5] 1A to 1C illustrate an example of a method for manufacturing a semiconductor device. [Figure 6] 1A to 1C illustrate an example of a method for manufacturing a semiconductor device. [Figure 7] FIG. 1 is a cross-sectional view illustrating one embodiment of a semiconductor device. [Figure 8]4A to 4C are cross-sectional views showing the process of void generation. [Figure 9] FIG. 1 is a cross-sectional view illustrating one embodiment of a display device. [Figure 10] FIG. 1 is a cross-sectional view illustrating one embodiment of a display device. [Figure 11] FIG. 1 is a cross-sectional view illustrating one embodiment of a display device. [Figure 12] 1A to 1C are diagrams illustrating one embodiment of a display device. [Figure 13] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 14] 1A to 1C are diagrams illustrating electronic devices. [Figure 15] 1A to 1C are diagrams illustrating electronic devices. [Figure 16] FIG. 2 shows a STEM image of an example sample in an example. [Figure 17] FIG. 2 shows a STEM image of an example sample in an example. [Figure 18] FIG. 2 shows a STEM image of an example sample in an example. [Figure 19] FIG. 13 is a diagram showing electrical characteristics of an example sample in an example. [Figure 20] FIG. 13 is a diagram showing electrical characteristics of an example sample in an example. [Figure 21] FIG. 2 is a diagram for explaining an example sample in an embodiment. [Figure 22] FIG. 13 shows SIMS data of an example sample in an example. [Figure 23] FIG. 2 is a diagram for explaining an example sample in an embodiment. [Figure 24] FIG. 13 shows SIMS data of an example sample in an example. [Diagram 25] FIG. 13 is a model diagram illustrating transfer of nitrogen, hydrogen, and water in a nitrogen-containing oxide insulating film during heat treatment. [Figure 26] 1A and 1B are model diagrams illustrating transfer of nitrogen, hydrogen, and water in an oxide semiconductor film during heat treatment. [Figure 27] 1A and 1B are model diagrams illustrating changes in oxygen vacancies in an oxide semiconductor film due to heat treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, the embodiment will be described in detail with reference to the drawings. The present invention is not limited to the above description, and the embodiments and details may be modified without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various modifications may be made to the details. However, it should not be construed as being limited to the description of the embodiments shown below.
[0027] The functions of "source" and "drain" may differ when using transistors with different polarities. In some cases, such as when the direction of the current changes during circuit operation, the two may be interchanged. Therefore, in this specification, the terms "source" and "drain" are used interchangeably. It is possible to do so.
[0028] "Electrically connected" means that the device is connected via "something that has some kind of electrical effect." Here, "something that has some electrical effect" refers to the electrical effect between connected objects. There are no particular limitations as long as it is possible to transmit and receive signals.
[0029] The position, size, range, etc. of each component shown in the drawings are not necessarily the same as in the actual embodiment, in order to facilitate understanding. Therefore, the disclosed invention may not necessarily represent the actual position, size, range, etc. The present invention is not necessarily limited to the position, size, range, etc. disclosed in the drawings.
[0030] Ordinal numbers such as "first," "second," and "third" are used to avoid confusion of the components. That is why.
[0031] In this specification, "parallel" means that two straight lines are arranged at an angle of -10° or more and 10° or less. Therefore, it includes the case where the angle is between -5° and 5°. refers to the state in which two straight lines are arranged at an angle of 80° or more and 100° or less. , including cases where the angle is between 85° and 95°.
[0032] In this specification, when the crystal is a trigonal or rhombohedral crystal, it is represented as a hexagonal crystal system. vinegar.
[0033] (Embodiment 1) In this embodiment, a semiconductor device of one embodiment of the present invention will be described with reference to drawings. 1A and 1B are a top view and a cross-sectional view of a transistor 450, which is a semiconductor device of one embodiment of the present invention. FIG. 1A shows a top view of a transistor 450, and FIG. 1B shows a cross-sectional view of a portion of FIG. 1 shows a cross-sectional view taken along dashed line AB.
[0034] The transistor 450 shown in FIG. 1 has a gate electrode provided on a substrate 400 having an insulating surface. An electrode 402, a gate insulating film 404 provided on the gate electrode 402, and a gate insulating film 4 A semiconductor film 406 is provided on the gate electrode 404 and overlaps with the gate electrode 402. A source electrode 408a and a drain electrode 408b are provided. An insulating film 412 that covers the electrode 408a and the drain electrode 408b and is in contact with the semiconductor film 406 The insulating film 412 may be formed as a component of the transistor 450. 14, and an opening provided in the insulating film 412 and the interlayer insulating film 414 on the interlayer insulating film 414. An electrode 416 is provided which is electrically connected to the drain electrode 408b via a portion. In this embodiment, the electrode 416 is electrically connected to the drain electrode 408b. However, the electrode 416 may be electrically connected to the source electrode 408a.
[0035] In this embodiment, the gate insulating film 404 is a gate insulating film in contact with the gate electrode 402. The gate insulating film 404a and the semiconductor film 406 are in contact with each other. The insulating film 412 is a stacked structure of the semiconductor film 406, the source electrode 408a, and the The oxide insulating film 410 is a first insulating film that is in contact with the drain electrode 408b and the oxide insulating film 411. a nitride insulating film 411 which is a second insulating film functioning as a protective film on the film 410; The oxide insulating film 410 covers the semiconductor film 406, the source electrode 408a, and the drain electrode 408b. an oxide insulating film 410a that is in contact with the gate electrode 408b, is formed under low power conditions, and has high coverage; The oxide insulating film 410 has a stacked structure of an oxide insulating film 410a and an oxide insulating film 410b.
[0036] In addition, the step on the side end surface of the source electrode 408a and the drain electrode 408b is A void 413 is generated in the oxide insulating film 410 of the covering portion. Since the dielectric constant is lower than that of the film forming the portion 413, the dielectric constant between the wirings caused by the miniaturization of the semiconductor device is reduced. This reduces the capacitance required, enabling high speed operation while maintaining a high degree of integration. Moisture penetrates into the semiconductor film 406 through the gap 413, and the characteristics of the transistor 450 are deteriorated. However, by providing the nitride insulating film 411 over the oxide insulating film 410, The voids generated in the oxide insulating film 410 can be covered.
[0037] Furthermore, the gap 413 is blocked by the nitride insulating film 411, so that the oxide insulating film 41 In addition, the nitride insulating film 411 can prevent the void 413 from expanding outside the insulating film 411. Therefore, the voids 413 may be filled. Hydrogen or compounds containing hydrogen (such as water) are absorbed into the semiconductor film 4 It acts as a barrier membrane to prevent bacteria from penetrating into the bloodstream.
[0038] Next, a method for manufacturing the transistor 450 will be described with reference to FIGS.
[0039] First, a gate electrode 402 (formed in the same layer as the gate electrode 402) is formed on a substrate 400 having an insulating surface. The wiring is formed.
[0040] There are no significant limitations on the substrate that can be used for the substrate 400 having an insulating surface, but at least It is necessary to have at least a sufficient heat resistance to withstand the subsequent heat treatment. Glass substrates such as borosilicate glass and aluminoborosilicate glass, ceramic substrates, quartz A substrate, a sapphire substrate, etc. can be used. In addition, a single substrate such as silicon or silicon carbide can be used. Crystalline semiconductor substrates, polycrystalline semiconductor substrates, compound semiconductor substrates such as silicon germanium, SO A semiconductor device is provided on the substrate 40. It may be used as 0.
[0041] The material of the gate electrode 402 is molybdenum, titanium, tantalum, tungsten, aluminum, etc. Metallic materials such as aluminum, copper, chromium, neodymium, scandium, etc., or alloys containing these as their main components The gate electrode 402 can be formed using a gold material. Semiconductor films, such as polycrystalline silicon films doped with silicon, and silicon silicide films, such as nickel silicide, A silicide film may also be used.
[0042] The material of the gate electrode 402 includes indium oxide, tin oxide, and tungsten oxide. Indium oxide, indium zinc oxide with tungsten oxide, indium zinc oxide with titanium oxide Indium oxide, indium tin oxide with titanium oxide, indium oxide zinc oxide, acid Conductive materials such as indium tin oxide doped with silicon dioxide can also be applied.
[0043] Alternatively, the gate electrode 402 may be made of a nitrogen-containing In-Ga-Zn oxide, a nitrogen In-Sn oxides containing nitrogen, In-Ga oxides containing nitrogen, In-Zn oxides containing nitrogen oxides containing nitrogen, Sn-based oxides containing nitrogen, In-based oxides containing nitrogen, metal nitride films (indium nitride Alternatively, a film such as a tantalum nitride film, a zinc nitride film, a tantalum nitride film, or a tungsten nitride film may be used. Since the materials have a work function of 5 eV or more, it is possible to fabricate gate electrodes using these materials. By forming 402, the threshold voltage is made positive in the electrical characteristics of the transistor. A normally-off switching transistor can be realized. 402 may be a single layer structure or a laminated structure, for example, copper formed on tantalum nitride. The gate electrode 402 may have a tapered shape. For example, the taper angle may be The taper angle is set to 15° or more and 70° or less. This refers to the angle between the side edge of the layer and the bottom surface of the layer.
[0044] Next, a gate insulating film 404 is formed on the gate electrode 402 so as to cover the gate electrode 402. The gate insulating film 404 is formed by a plasma CVD method, a sputtering method, etc. Silicon oxide film, silicon oxynitride film, silicon nitride oxide film, silicon nitride film, etc. aluminum oxide film, hafnium oxide film, yttrium oxide film, zirconium oxide film aluminum oxide film, gallium oxide film, tantalum oxide film, magnesium oxide film, lanthanum oxide film, cerium oxide film In the present invention, an insulating film containing at least one of a lithium oxide film and a neodymium oxide film is used as a single layer or a laminated layer. In addition, a microwave plasma treatment is performed to repair oxygen vacancies after the gate insulating film 404 is formed. It is preferable to carry out the radical oxidation treatment by carrying out the above-mentioned procedure.
[0045] In this specification, the term "oxynitride" such as silicon oxynitride refers to a material having a specific composition and It refers to a material that contains more oxygen than nitrogen.
[0046] In this specification, the term "nitride oxide" such as silicon nitride oxide refers to a material having a specific composition. It refers to a material that contains more nitrogen than oxygen.
[0047] In the gate insulating film 404, a region in contact with a semiconductor film 406 to be formed later (this In the embodiment, the gate insulating film 404b) is preferably an oxide insulating film. .
[0048] Next, a semiconductor film 406 is formed over the gate insulating film 404 (see FIG. 2B).
[0049] The semiconductor film 406 may be an amorphous semiconductor film, a polycrystalline semiconductor film, or a microcrystalline semiconductor film. The material of the amorphous semiconductor film may be silicon or silicon germanium (S An i-Ge alloy or the like can be used. Also, an oxide semiconductor film can be used.
[0050] Next, a conductive film is formed on the semiconductor film 406, and this is processed by etching to form a semiconductor film. A source electrode 408a and a drain electrode 408b (including wiring formed in the same layer) (See FIG. 2(C)).
[0051] The source electrode 408a and the drain electrode 408b are made of, for example, Al, Cr, or Cu. A conductive film containing an element selected from the group consisting of Ta, Ti, Mo, and W, or a conductive film containing the above-mentioned elements as components. Metal nitride films (titanium nitride film, molybdenum nitride film, tungsten nitride film) that can In addition, Ti can be applied to either or both of the upper and lower sides of the conductive film such as Al or Cu. , Mo, W, etc., or their metal nitride films (titanium nitride film, molybdenum nitride film, etc.) The source electrode 408 may be a laminate of a tungsten film, a tungsten nitride film, etc. The a and drain electrodes 408b may be formed of a conductive metal oxide. The oxides include indium oxide (In2O3), tin oxide (SnO2), and zinc oxide (Zn O), indium tin oxide (In2O3-SnO2), indium zinc oxide (I n2O3-ZnO) or these metal oxide materials containing silicon oxide. It is possible.
[0052] The source electrode 408a and the drain electrode 408b are made of In-Ga- Zn-O film, In-Sn-O film containing nitrogen, In-Ga-O film containing nitrogen, I Metal nitride films such as n-Zn-O film, nitrogen-containing Sn-O film, and nitrogen-containing In-O film are used. The ends of the source electrode 408a and the drain electrode 408b can be tapered. It is preferable that the insulating film has a bar shape. By doing so, the insulating film can be more easily covered and the step can be easily formed. The taper angle is, for example, 30° to 70°. Preferably, the angle is between 30° and 60°.
[0053] In addition, the source electrode 408a and the drain electrode 408b are formed by adjusting the adhesion and conductivity of the film. Due to the problem of surface characteristics, for example, as shown in FIG. 8(A), the conductive film 407a, the conductive film 407b, and In the case where the conductive film 407c is formed as a stacked structure, the stacked conductive films are etched. When processing by the method, the etching speed differs depending on the type of conductive film. As shown in FIG. 1B, the side end surface of the conductive film 407c is in contact with the upper surface of the conductive film 407b, and the conductive film 407 The side end surface of b is in contact with the upper surface of the conductive film 407a, whereby the source electrode 408a and the drain electrode A step occurs on the side end surface of the pole 408b.
[0054] Due to this step, as shown in FIG. 8C, a void is formed in the oxide insulating film 410 to be formed later. In this embodiment, the source electrode 408a and the drain electrode 408b Although the above description uses a laminated structure of a conductive film having a significant step on the side end surface, the present invention is not limited to this. Even with a single conductive film, gaps are generated in the oxide insulating film 410 that is formed later due to the corners of the side end faces. The voids in the oxide insulating film 410 will be described later.
[0055] Next, the gate insulating film 404, the semiconductor film 406, the source electrode 408a and the drain electrode The oxide insulating film 410, which is part of the insulating film 412, is formed so as to cover 408b (FIG. 3). (See (A)).
[0056] The oxide insulating film 410 is a stacked film of an oxide insulating film 410a and an oxide insulating film 410b. The semiconductor film 406 can be formed by plasma CVD or sputtering. It is preferable to use a film capable of supplying oxygen to the semiconductor film 406. The oxide insulating film 410 may be a single layer of a silicon oxide film, a silicon oxynitride film, or the like. Alternatively, a gallium oxide film or a gallium oxide film can be used as the oxide insulating film 410. Alternatively, an aluminum oxide film, an aluminum oxynitride film, or the like can be used.
[0057] The oxide insulating film 410a is placed in a vacuum evacuated processing chamber of a plasma CVD apparatus. The substrate is maintained at 300°C or higher and 400°C or lower, more preferably 320°C or higher and 370°C or lower. The raw material gas is introduced into the processing chamber to set the pressure in the processing chamber to 100 Pa or more and 250 Pa or less. Then, the oxide insulating film 410 is formed by supplying high frequency power to an electrode provided in the processing chamber. As a, a silicon oxide film or a silicon oxynitride film can be formed.
[0058] Under the film formation conditions, by setting the substrate temperature to the above temperature, the bond between silicon and oxygen As a result, the oxide insulating film 410a is oxygen-permeable, dense, and A hard oxide insulating film, typically etched with 0.5% by weight hydrofluoric acid at 25°C. A silicon oxide film or an oxide film having a dipping speed of 10 nm / min or less, preferably 8 nm / min or less. A silicon nitride film can be formed.
[0059] Here, the oxide insulating film 410a is made of silane at a flow rate of 30 sccm and SiO2 at a flow rate of 400 The source gas was dinitrogen monoxide at 0 sccm, the pressure in the processing chamber was 200 Pa, and the substrate temperature was 22 At 0°C, a 27.12MHz high-frequency power source was used to apply 150W of high-frequency power to parallel plate electrodes. A silicon oxynitride film with a thickness of 50 nm is formed by the plasma CVD method using the gas supplied to the source. Under these conditions, a silicon oxynitride film through which oxygen is transmitted can be formed.
[0060] The oxide insulating film 410b is placed in a processing chamber of a plasma CVD apparatus that has been evacuated to a vacuum. The substrate is kept at 180° C. or higher and 260° C. or lower, more preferably 200° C. or higher and 240° C. or lower. A raw material gas is introduced into the processing chamber to set the pressure in the processing chamber to 100 Pa or more and 250 Pa or less. More preferably, the pressure should be between 100 Pa and 200 Pa, and the pressure should be 0. 17W / cm 2 More than 0.5W / cm 2 Less than or equal to 0.25 W / cm 2 More than 0 .35W / cm 2 Silicon oxide or oxynitride is formed by supplying the following high frequency power. A silicon oxide film is formed.
[0061] The source gas for the oxide insulating film 410b may be a deposition gas containing silicon and an oxidizing gas. Representative examples of deposition gases containing silicon include silane, disilane, and the like. Examples of oxidizing gases include oxygen, ozone, and monoxide. Examples include dinitrogen and nitrogen dioxide.
[0062] The oxide insulating film 410b was formed under the following conditions: Supplying high-frequency power increases the efficiency of decomposing the source gas in the plasma, resulting in oxygen radicals. As a result, the oxygen content in the oxide insulating film 410b increases and the oxidation of the source gas progresses. However, when the substrate temperature is the above temperature, the silicon and the oxide The bonding strength of the oxygen atoms is weak, so some of the oxygen is released when heated. The oxide insulating film contains more oxygen than the surface area, and some of the oxygen is released when heated. In addition, an oxide insulating film 410a is provided over the semiconductor film 406. For this reason, in the step of forming the oxide insulating film 410b, the oxide insulating film 410a is As a result, damage to the semiconductor film 406 is reduced while the The oxide insulating film 410b can be formed using high-frequency power with high power density.
[0063] In this manner, the oxide insulating film 410 is formed on the semiconductor film 406, the source electrode 408a, and the drain an oxide insulating film 410a that is in contact with the gate electrode 408b, is formed under low power conditions, and has high coverage; It is preferable to have a stacked structure of the oxide insulating film 410b over the oxide insulating film 410a.
[0064] In addition, if there are steps on the side end surfaces of the source electrode 408a and the drain electrode 408b, When the oxide insulating film 410 is formed, a void 413 as shown in FIG. The void 413 is formed by observing the cross-sectional shape of the insulating film 412 using a scanning transmission electron microscope (STEM). By observing using the mission electron microscopy method, It can be confirmed that the gap 413 has a lower dielectric constant than the film that forms the gap 413. Therefore, it is possible to reduce the capacitance between wirings that occurs with the miniaturization of semiconductor devices, and To enable high-speed operation while maintaining a high degree of integration.
[0065] The oxide insulating film 410 is a low-density film that includes voids in the film. 410 has voids (low density regions) and therefore has a lower film density as a whole. It has characteristics.
[0066] The insulating film 412 was formed by X-ray reflectometry (XRR). The preferred overall membrane density, as measured by 3 Over 2.50g / cm 3 The following is the result.
[0067] After the oxide insulating film 410 is formed, heat treatment may be performed. The temperature of the heat treatment is typically 150° C. or higher and lower than the substrate distortion point, preferably 200° C. or higher and 450° C. or lower, and more preferably The temperature must be between 300℃ and 450℃.
[0068] Next, a nitride insulating film 411 is formed so as to cover the oxide insulating film 410 (see FIG. 3(B)). (see).
[0069] The nitride insulating film 411 can be formed by a plasma CVD method or a sputtering method. Silicon nitride, silicon oxynitride, or the like can be used in a single layer or in a laminated layer. The nitride insulating film 411 is made of aluminum nitride, aluminum oxide nitride, or the like. In addition, if the nitride insulating film 411 is a film with high coverage, the source electrode 408 a and the step on the side end surface of the drain electrode 408b becomes gentler (the step portion becomes flat). This is preferable because it reduces the occurrence of voids due to steps. Instead of the insulating film 411, aluminum oxide may be used.
[0070] The nitride insulating film 411 is formed on the steps of the side end surfaces of the source electrode 408a and the drain electrode 408b. The nitride insulating film 410 has a function of covering voids generated in the oxide insulating film 410 due to the difference in thickness. The gap is blocked by 411, so that the gap extends outside the oxide insulating film 410. In addition, the gap may be filled with the nitride insulating film 411. In addition, the nitride insulating film 411 is protected from hydrogen or other impurities from the outside or the interlayer insulating film 414 that is formed later. The barrier film prevents hydrogen-containing compounds (such as water) from penetrating into the semiconductor film 406. Since the transistor functions as a gate, the reliability of the transistor can be improved.
[0071] In this manner, the transistor 450 of this embodiment can be formed.
[0072] Next, the interlayer insulating film 414 is formed over the transistor 450 .
[0073] The interlayer insulating film 414 is made of acrylic resin, epoxy resin, benzocyclobutene resin, or poly Organic materials such as imide and polyamide can be used. In addition, multiple insulating films made of these materials can be stacked. The interlayer insulating film 414 may be formed by layering.
[0074] Next, an opening is provided in the insulating film 412 and the interlayer insulating film 414, and the insulating film 412 is formed on the interlayer insulating film 414. An electrode 416 is formed which is electrically connected to the drain electrode 408b through the opening (FIG. 3( See C).
[0075] The electrode 416 is formed by appropriately using the material shown in the source electrode 408a or the drain electrode 408b. The electrode 416 can also be made of indium oxide with tungsten oxide, Indium zinc oxide containing tungsten, indium oxide containing titanium oxide, titanium oxide Indium tin oxide (ITO) containing tin Conductive materials with light-transmitting properties such as indium zinc oxide and indium tin oxide doped with silicon oxide Materials can be used.
[0076] As a result, the voids in the oxide insulating film 410 have a lower dielectric constant than the film that forms the voids. Therefore, it is possible to reduce the capacitance between wirings that occurs with the miniaturization of semiconductor devices, and to achieve high integration. The nitride insulating film 411 blocks the gap. This can prevent voids from expanding outside the oxide insulating film 410. The gap may be filled with the nitride insulating film 411. Hydrogen or compounds containing hydrogen (such as water) may enter the insulating interlayer 414 from the outside or from the insulating interlayer 414 that will be formed later. Since it functions as a barrier film that prevents the penetration of the impurities into the semiconductor film 406, The reliability of the 450 can be improved.
[0077] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0078] (Embodiment 2) In this embodiment mode, a semiconductor device different from that in Embodiment Mode 1 will be described with reference to the drawings. 4A and 4B are a top view and a cross-sectional view of a transistor 550, which is a semiconductor device of one embodiment of the present invention. FIG. 4A shows a top view of a transistor 550, and FIG. 4B shows the top view of the transistor 550 shown in FIG. 1 is a cross-sectional view taken along dashed line CD. The transistor 50 has a top-gate structure in comparison with the transistor 450 described in the first embodiment. The difference is that it is a gyroscope.
[0079] The transistor 550 shown in FIG. 4 is a transistor having a base insulating layer provided on a substrate 400 having an insulating surface. The insulating film 401 and the semiconductor film 406 provided on the insulating base film 401 are and a source electrode 408a and a drain electrode 408b provided on the semiconductor film 406; A gate electrode 408a covers the source electrode 408a and the drain electrode 408b and is in contact with the semiconductor film 406. An insulating film 512 and a gate electrode provided on the gate insulating film 512 and overlapping with the semiconductor film 406 The electrode 402 is also provided. The interlayer insulating film 414 covers the transistor 550. A drain is formed on the film 414 through an opening provided in the insulating film 412 and the interlayer insulating film 414. An electrode 416 is provided to electrically connect to the first electrode 408b. The electrode 416 is electrically connected to the drain electrode 408b, but is not limited to this. 416 may be in electrical contact with the source electrode 408a.
[0080] In this embodiment, the gate insulating film 512 is formed on the semiconductor film 406 and the source electrode 408a. The oxide insulating film 510, which is the first insulating film in contact with the drain electrode 408b, and the oxide A laminated structure of a nitride insulating film 511 which is a second insulating film functioning as a protective film on the insulating film 510. The oxide insulating film 510 covers the semiconductor film 406, the source electrode 408a, and the drain electrode 408b. An oxide insulating film 510a that is in contact with the rain electrode 408b, is formed under low power conditions, and has high coverage. The oxide insulating film 510a has a stacked structure of the oxide insulating film 510b over the oxide insulating film 510a.
[0081] In addition, the step on the side end surface of the source electrode 408a and the drain electrode 408b is A void 413 is generated in the oxide insulating film 510 of the covering portion. Since the dielectric constant is lower than that of the film forming the gap 413, the dielectric constant is reduced due to the miniaturization of semiconductor devices. This reduces the capacitance generated by the semiconductor device, enabling high speed operation while maintaining a high degree of integration. Moisture penetrates into the semiconductor film 406 through the gap 413, and the characteristics of the transistor 550 are deteriorated. Although there is a possibility that the nitride insulating film 511 may be provided on the oxide insulating film 510, The voids generated in the oxide insulating film 510 can be covered with the above-mentioned.
[0082] Furthermore, the gap 413 is blocked by the nitride insulating film 511, so that the oxide insulating film 51 In addition, the nitride insulating film 511 can prevent the void 413 from expanding outside the insulating film 511. Therefore, the voids 413 may be filled. Hydrogen or compounds containing hydrogen (such as water) are absorbed into the semiconductor film 4 It acts as a barrier membrane to prevent bacteria from penetrating into the bloodstream.
[0083] Next, a method for manufacturing the transistor 550 will be described with reference to FIGS.
[0084] First, a base insulating film 401 is formed on a substrate 400 having an insulating surface. The material and manufacturing method of the base insulating film 401 are the same as those of the substrate 400 and the gate insulating film 401 in the first embodiment. The gate insulating film 404 can be taken into consideration.
[0085] Next, a semiconductor film 406 is formed on the base insulating film 401 (see FIG. 5A). The material and manufacturing method of the semiconductor film 406 can be referred to in the embodiment mode 1. Cut.
[0086] Next, a conductive film is formed on the semiconductor film 406, and this is processed by etching to form a semiconductor film. A source electrode 408a and a drain electrode 408b (including wiring formed in the same layer) (see FIG. 5B). Materials for the source electrode 408a and the drain electrode 408b The manufacturing method and the like are the same as those of the source electrode 408a and the drain electrode 408b in the first embodiment. can be taken into consideration.
[0087] As shown in the first embodiment, the source electrode 408a and the drain electrode 408b A step occurs on the side end surface, and this step causes a void in the gate insulating film 512 to be formed later. The void portion in the gate insulating film 512 will be described later.
[0088] Next, the base insulating film 401, the semiconductor film 406, the source electrode 408a and the drain electrode 408 are An oxide insulating film 510, which is a part of the gate insulating film 512, is formed so as to cover the gate insulating film 08b. See Figure 5(C).
[0089] The oxide insulating film 510 is formed on the base insulating film 401, the semiconductor film 406, and the source electrode 408. a and the drain electrode 408b, and is formed under low power conditions. It is preferable that the oxide insulating film 510a and the oxide insulating film 510b be stacked over the oxide insulating film 510a. The material and the formation method of the oxide insulating film 510 are the same as those of the oxide insulating film 41 in Embodiment 1. 0 can be taken into consideration.
[0090] In addition, if there are steps on the side end surfaces of the source electrode 408a and the drain electrode 408b, When the oxide insulating film 510 is formed, the void 413 as described in Embodiment 1 is generated. Since the gap 413 has a lower dielectric constant than the film that forms the gap 413, the semiconductor device This reduces the capacitance between wiring that occurs with miniaturization of semiconductor devices, and enables high integration while maintaining high density. Enables fast operation.
[0091] The oxide insulating film 510b is a low-density film that includes voids 413 in the film. The insulating film 510b has a low density region, and hence has a low film density as a whole. has.
[0092] The gate insulating film 512 was obtained by X-ray reflectometry (XRR). The preferred overall membrane density, as measured by the FT-IR method, is 2.26 g / cm 3 2. That's it. 50g / cm 3 The following is the result.
[0093] Next, a nitride insulating film 511 is formed so as to cover the oxide insulating film 510 (see FIG. 6(A)). The material and the method of manufacturing the nitride insulating film 511 are the same as those of the nitride insulating film 4 in the first embodiment. 11 may be taken into consideration.
[0094] The nitride insulating film 511 is formed on the steps of the side end surfaces of the source electrode 408a and the drain electrode 408b. The nitride insulating film 510 has a function of covering voids generated in the oxide insulating film 510 due to the difference in thickness. The gap is blocked by 511, so that the gap spreads to the outside of the oxide insulating film 510. In addition, the gap may be filled with the nitride insulating film 511. In addition, the nitride insulating film 511 is protected from hydrogen or other impurities from the outside or the interlayer insulating film 414 that is formed later. The barrier film prevents hydrogen-containing compounds (such as water) from penetrating into the semiconductor film 406. Since the transistor functions as a gate, the reliability of the transistor can be improved.
[0095] Next, the gate electrode 402 is formed on the gate insulating film 512 overlapping with the semiconductor film 406. (See FIG. 6B.) The material and manufacturing method of the gate electrode 402 are the same as those of the gate electrode in Embodiment 1. The port electrode 402 can be taken into consideration.
[0096] In this manner, the transistor 550 of this embodiment can be formed.
[0097] Next, the interlayer insulating film 414 is formed over the transistor 550, and the insulating film 412 and the interlayer insulating film 413 are An opening is provided in the insulating film 414, and the drain electrode 408 is formed on the interlayer insulating film 414 through the opening. An electrode 416 is formed to be electrically connected to the interlayer insulating film 414 and the The materials and manufacturing methods of the interlayer insulating film 414 and the electrode 416 are the same as those of the first embodiment. 416 may be taken into consideration.
[0098] As shown in FIG. 6D, an oxide insulating film and a nitride insulating film are formed on the gate electrode 402. An insulating film 530 made of a nitride insulating film may be provided. As a result, a gap is generated in the insulating film 530 due to the corners of the side end faces of the gate electrode 402. By forming the nitride insulating film, the voids are blocked by the nitride insulating film, and the voids are formed on the outside of the oxide insulating film. In addition, the gate insulating film 512 is formed by covering the oxide insulating film. Instead of using a stacked structure of a nitride insulating film, the insulating film 530 is formed of a nitride insulating film covering an oxide insulating film. A laminated structure may also be used.
[0099] As a result, the gaps in the oxide insulating film 510 have a lower dielectric constant than the film that forms the gaps. Therefore, it is possible to reduce the capacitance between wirings that occurs with the miniaturization of semiconductor devices, and to achieve high integration. The nitride insulating film 511 blocks the gap. By cutting the insulating film 510, it is possible to prevent voids from expanding outside the oxide insulating film 510. In some cases, the gap is filled with the nitride insulating film 511. 11 is a compound containing hydrogen (such as water) from the outside or from the interlayer insulating film 414 formed later. The barrier film prevents the penetration of the ions (e.g., fluorine) into the semiconductor film 406. The reliability of the resistor 550 can be improved.
[0100] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0101] (Embodiment 3) In this embodiment, a semiconductor device different from those in the first and second embodiments will be described with reference to FIG. This will be explained using:
[0102] The transistor 560 shown in FIG. 7A has a plurality of gates opposed to each other with a semiconductor film 406 interposed therebetween. The transistor 560 is characterized by having a substrate 400 having an insulating surface. A gate electrode 552 is provided on the gate electrode 552, and a base insulating film 401 is provided on the gate electrode 552. A semiconductor film 406 provided on the base insulating film 401, and a semiconductor film 406 formed on the base insulating film 401 and the semiconductor A source electrode 408a and a drain electrode 408b are provided on the film 406, and a source electrode A gate insulating film 51 covers the semiconductor film 406 and the drain electrode 408a. 2, a gate electrode 402 provided on the gate insulating film 512 and overlapping with the semiconductor film 406, In addition, an interlayer insulating film 414 covering the transistor 560 and a The drain electrode 40 is then electrically connected to the insulating film 412 via an opening provided in the insulating film 412 and the interlayer insulating film 414. An electrode 416 is provided which is electrically connected to 8b.
[0103] The material and manufacturing method of the gate electrode 552 are the same as those of the gate electrode 402 in the first embodiment. I can pour drinks.
[0104] The transistor 560 in this embodiment has a gate electrode facing the gate insulating film 406 therebetween. The gate electrode 552 and the gate electrode 402 are By applying different potentials, the threshold voltage of the transistor 560 can be controlled. Alternatively, the same potential may be applied to the gate electrode 552 and the gate electrode 402. The on-current of the transistor 560 can be increased.
[0105] The oxide insulating film 410 does not necessarily have to have a two-layer structure. The transistor 570 shown in FIG. 1 has the same structure as the transistor 450 in Embodiment 1 except that the oxide insulating film 41 0, an oxide insulating film 410c is further provided over the oxide insulating film 410b. In addition, in the transistor 580 illustrated in FIG. 7C, an oxide insulating film 410c is further provided over the oxide insulating film 410c. The insulating film 410d and the oxide insulating film 410e are stacked. The oxide insulating film 410c and the oxide insulating film 410e are similar to the oxide insulating film 410a. The oxide insulating film 410d can be formed using a material similar to that of the oxide insulating film 410b. There can be.
[0106] In addition, the oxide insulating film 410a formed at a lower power has a lower The film is dense, and the step on the side end surface of the source electrode 408a and the drain electrode 408b is By laminating as above, the step difference can be made gentler. do.
[0107] Then, an oxide insulating film that is denser than the oxide insulating film 410a is formed over the oxide insulating film 410a. By forming the insulating film 410b, the oxide insulating film 410b becomes a thin film of the oxide insulating film 410a. The effect of this is that the unevenness of the surface is flattened due to the high coverage of the unevenness. It becomes difficult to get into gaps.
[0108] The thickness of the semiconductor film 406 in a region in contact with the oxide insulating film 410a is The thickness of the semiconductor film 4 is smaller than that of the region in contact with the drain electrode 408a and the drain electrode 408b. In 06, the thin film region is a source electrode 408a and a drain electrode 408b. When processing the conductive film, a part of the conductive film is etched, or the source electrode 408 After forming the gate electrodes 408a and drain electrodes 408b, the exposed regions of the semiconductor film 406 are etched. The region is formed by performing a process on the transistor 570 and the transistor This region functions as a channel forming region of the transistor 580.
[0109] In the semiconductor film 406, the thickness of the channel forming region is reduced, so that the source electrode 4 The resistance of the region in contact with the drain electrode 408a and the drain electrode 408b is lower than that of the channel formation region. Therefore, the semiconductor film 406, the source electrode 408a, and the drain electrode This makes it possible to reduce the contact resistance with the electrode 408b.
[0110] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0111] (Embodiment 4) In this embodiment, an oxide semiconductor film is used as the semiconductor film 406 in the above embodiment. We will explain what happens when this happens.
[0112] A transistor including an oxide semiconductor film has a low current value in an off state (off-state current value). In addition, the field-effect mobility is relatively high, allowing high-speed operation. In the above embodiment, the oxide insulating film under the nitride insulating film is formed by removing oxygen. By making it possible to supply a film that can be used for a long time, the voids that were closed by the nitride insulating film during heating can be eliminated. The above-mentioned effect is more pronounced by releasing oxygen from the gaps and supplying oxygen to the oxide semiconductor film. A method for forming an oxide semiconductor film will be described below.
[0113] The oxide semiconductor film is formed by sputtering, MBE (Molecular Beam Induction), am Epitaxy) method, CVD (Chemical Vapor Depositi) method on method, Pulsed Laser Deposition (P LD method), ALD (Atomic Layer Deposition) method, etc. are used appropriately. It is possible.
[0114] In addition, when a large amount of hydrogen is contained in the oxide semiconductor film, hydrogen is bonded to the oxide semiconductor. As a result, some of the hydrogen atoms become donors and generate electrons, which act as carriers. The threshold voltage of the transistor is shifted in the negative direction. In this case, the hydrogen concentration is 5×10 18 atoms / cm 3 Less than 1 x 10 18 atoms / cm 3 Less than or equal to 5×10 17 atoms / cm 3 Further details are below. Preferably 1 x 10 16 atoms / cm 3 In addition, in the above-described oxide semiconductor film, The hydrogen concentration was measured by secondary ion mass spectrometry (SIMS). This is measured using a NMR Spectrometry (NMR Spectrometry).
[0115] For the above reasons, the gas used in forming the oxide semiconductor film is water, hydrogen, or water. It is preferable that impurities such as acid groups or hydrides are not included. In other words, the purity is 6N or more, preferably 7N or more (i.e., impurity concentration in the gas is 1 ppm or less, preferably 0 It is preferable to use a gas with a concentration of 0.1 ppm or less.
[0116] In addition, when the oxide semiconductor film is formed, moisture (water, water vapor, hydrogen, hydroxyl, etc.) in the film formation chamber is To remove the ions (including radicals or hydroxides), an adsorption-type vacuum pump, e.g., a cryopump It is preferable to use a pump, an ion pump, or a titanium sublimation pump. The evaporative means may be a turbomolecular pump plus a cold trap. The deposition chamber is evacuated using a pump, and contains hydrogen atoms, water (H2O), and other gases that contain hydrogen atoms. Since compounds (preferably compounds containing carbon atoms) and the like are exhausted, the deposition chamber is The concentration of impurities such as hydrogen and moisture contained in the oxide semiconductor film can be reduced.
[0117] The target used in the sputtering device should have a relative density of 90% or more and 100% or less. The relative density of the target is preferably 95% or more and 100% or less. By using the above-mentioned oxide semiconductor film, the formed oxide semiconductor film becomes dense.
[0118] The oxide semiconductor film may be made of, for example, an In-M-Zn-O-based material. Here, the metal element M is an element that has a higher bond energy with oxygen than In and Zn. Or, it is an element that has the function of suppressing the desorption of oxygen from In-M-Zn-O based materials. The metal element M acts to suppress the generation of oxygen vacancies in the oxide semiconductor film. This reduces the variation in the electrical characteristics of the transistors caused by oxygen vacancies, improving reliability. Therefore, a transistor with high performance can be obtained.
[0119] The metal element M is specifically Al, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, G a, Y, Zr, Nb, Mo, Sn, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta or W may be used, and preferably A The metal element M is one of the above elements. Alternatively, two or more kinds may be selected. Moreover, Ge may be used in place of the metal element M.
[0120] Here, the higher the In concentration, the more the oxide semiconductor represented by the In-M-Zn-O system material becomes. The carrier mobility and carrier density are increased. As a result, the higher the In concentration, the higher the electrical conductivity. It becomes an oxide semiconductor.
[0121] The structure of the oxide semiconductor film will be described below.
[0122] Oxide semiconductor films are roughly classified into single-crystal oxide semiconductor films and non-single-crystal oxide semiconductor films. The non-single-crystal oxide semiconductor film includes an amorphous oxide semiconductor film, a microcrystalline oxide semiconductor film, a polycrystalline oxide semiconductor film, and a polycrystalline oxide semiconductor film. Compound semiconductor film, CAAC-OS (C Axis Aligned Crystallin e Oxide Semiconductor film, etc.
[0123] The amorphous oxide semiconductor film has irregular atomic arrangement and does not contain crystalline components. The oxide semiconductor film does not have any crystal parts even in a microscopic region, and the entire film has a completely amorphous structure. A typical example is an oxide semiconductor film.
[0124] The microcrystalline oxide semiconductor film is, for example, a microcrystal (nanocrystal) having a size of 1 nm or more and less than 10 nm. Therefore, the microcrystalline oxide semiconductor film has a higher crystallinity than the amorphous oxide semiconductor film. The atomic arrangement is highly regular. Therefore, the microcrystalline oxide semiconductor film has a higher atomic order than the amorphous oxide semiconductor film. It has the advantage of having a lower density of defect states than silicon.
[0125] The CAAC-OS film is one of the oxide semiconductor films that has multiple crystal parts. The crystal part is small enough to fit inside a cube with one side less than 100 nm. The crystal parts contained in the OS film are cubes with one side less than 10 nm, 5 nm, or 3 nm. The CAAC-OS film has a smaller size than the microcrystalline oxide semiconductor film. The defect density is low. The CAAC-OS film is described in detail below. cormorant.
[0126] The CAAC-OS film was observed under a transmission electron microscope (TEM). When observed using a quartz crystal microscope, clear boundaries between the crystals were observed. It is not possible to confirm the grain boundary. It can be said that the AAC-OS film is less susceptible to the decrease in electron mobility caused by grain boundaries.
[0127] The CAAC-OS film was observed by TEM from a direction roughly parallel to the sample surface (cross-sectional TEM observation). When the metal atoms are observed, it can be confirmed that they are arranged in layers in the crystal part. Each layer of the CAAC-OS film is formed on a surface on which the film is to be formed (also called a surface on which the film is to be formed) or on a concave surface on the upper surface. The shape reflects a convexity, and is aligned parallel to the surface on which the CAAC-OS film is formed or the upper surface.
[0128] On the other hand, the CAAC-OS film was observed by TEM from a direction roughly perpendicular to the sample surface (plane T EM observation reveals that metal atoms are arranged in triangular or hexagonal shapes in the crystals. However, no regularity was observed in the arrangement of metal atoms between different crystal regions. do not have.
[0129] Cross-sectional and planar TEM observations revealed that the crystals in the CAAC-OS film had an orientation. It can be seen that...
[0130] X-ray diffraction (XRD) of CAAC-OS film When the structure was analyzed using the device, for example, CAAC-OS with InGaZnO4 crystals was In the out-of-plane analysis of the film, the diffraction angle (2θ) peaked at around 31°. This peak is attributed to the (009) plane of the InGaZnO4 crystal. Therefore, the crystals of the CAAC-OS film have a c-axis orientation, and the c-axis faces the surface on which the film is formed or the upper surface. It can be seen that it is oriented in a roughly vertical direction.
[0131] On the other hand, in-p X-rays are incident on the CAAC-OS film from a direction approximately perpendicular to the c-axis. In the lane method, a peak may appear at 2θ around 56°. is attributed to the (110) plane of the InGaZnO4 crystal. In the case of a nitride semiconductor film, 2θ is fixed at around 56°, and the normal vector of the sample surface is the axis (φ axis). When the sample is rotated and analyzed (φ scan), a crystal plane equivalent to the (110) plane is detected. In contrast, in the case of the CAAC-OS film, six peaks are observed, which are assigned to Even when φ is fixed at around 56° and scanned, no clear peak appears.
[0132] From the above, it is considered that the orientation of the a-axis and b-axis is uniform between different crystal regions in the CAAC-OS film. Although it is irregular, it has a c-axis orientation, and the c-axis is parallel to the normal vector of the surface on which it is formed or the upper surface. Therefore, the layered structure confirmed by the cross-sectional TEM observation mentioned above is consistent with the Each layer of arranged metal atoms is in a plane parallel to the ab plane of the crystal.
[0133] The crystalline part is formed when the CAAC-OS film is formed or after a crystallization process such as a heat treatment. As described above, the c-axis of the crystal is aligned to the surface on which the CAAC-OS film is to be formed. For example, in the CAAC-OS film, When the shape is changed by etching, the c-axis of the crystal is aligned with the CAAC-OS film. It may not be parallel to the face or top surface normal vector.
[0134] In addition, the crystallinity in the CAAC-OS film does not have to be uniform. When the crystalline part of the film is formed by crystal growth from the vicinity of the top surface of the CAAC-OS film, The area near the surface may have a higher crystallinity than the area near the surface on which it is formed. When impurities are added to the AC-OS film, the crystallinity of the region to which the impurities are added changes, resulting in a partial In some cases, regions of differing crystallinity may be formed.
[0135] In addition, the out-of-plane crystal structure of the CAAC-OS film with InGaZnO4 crystals In the analysis by the method, in addition to the peak at 2θ near 31°, a peak also appeared at 2θ near 36°. The peak at 2θ of around 36° may be due to the c-axis orientation in some parts of the CAAC-OS film. The CAAC-OS film contains crystals that do not have the 2θ value of about 31°. It is preferable that the spectrum shows a peak at 2θ of about 36° and does not show a peak at 2θ of about 36°.
[0136] The electrical characteristics of transistors using CAAC-OS films change when irradiated with visible or ultraviolet light. Therefore, the transistor has high reliability.
[0137] The oxide semiconductor film may be, for example, an amorphous oxide semiconductor film, a microcrystalline oxide semiconductor film, or a C The AAC-OS film may be a laminate film having two or more kinds of AAC-OS films.
[0138] The CAAC-OS film can be formed, for example, by sputtering a polycrystalline oxide semiconductor target. The film is formed by sputtering using the sputtering target. When the target is struck, the crystalline region of the sputtering target cleaves from the ab plane, The particles are peeled off as plate-like or pellet-like sputtered particles with a surface parallel to the b plane. In this case, the plate-like sputtered particles are deposited on the substrate while maintaining their crystalline state. By reaching this temperature, a CAAC-OS film can be formed.
[0139] In addition, the following conditions are preferably applied to form the CAAC-OS film.
[0140] By reducing the amount of impurities mixed in during film formation, it is possible to prevent the crystal state from being destroyed by impurities. For example, the concentration of impurities (hydrogen, water, carbon dioxide, nitrogen, etc.) present in the deposition chamber can be In addition, the impurity concentration in the deposition gas may be reduced. The temperature is -80°C or lower, preferably -100°C or lower, and more preferably -120°C or lower. A membrane gas is used.
[0141] In addition, by increasing the substrate heating temperature during film formation, the microstructure of sputtered particles is improved after they reach the substrate. Specifically, the substrate heating temperature is set to 100° C. or higher and 740° C. or lower, preferably The film is formed at a temperature between 200 and 500°C. By increasing the substrate heating temperature during film formation, When a flat sputtered particle reaches a substrate, migration occurs on the substrate. , the flat surface of the sputtered particle adheres to the substrate.
[0142] In addition, by increasing the oxygen ratio in the deposition gas and optimizing the power, plasma damage during deposition is reduced. The oxygen ratio in the deposition gas is preferably 30% by volume or more, and more preferably 100% by volume or more. Expressed as volume percent.
[0143] As an example of a sputtering target, an In-Ga-Zn oxide target is The details are shown below.
[0144] InO X powder, GaO Y Powder and ZnO Z The powders are mixed in a specified number of moles and pressurized. Then, it is heated at a temperature between 1000℃ and 1500℃ to produce polycrystalline In-G The target is a-Zn oxide. X, Y, and Z are any positive numbers. , the given molar ratio is, for example, InO X powder, GaO Y Powder and ZnO Z Powder, 2: 2:1, 8:4:3, 3:1:1, 1:1:1, 4:2:3 or 3:1:2. The type of powder and the molar ratio of the powder to be mixed are determined according to the sputtering target to be prepared. The amount may be appropriately changed depending on the application.
[0145] In addition, the oxide semiconductor film is in a supersaturated state immediately after deposition, in which oxygen is more than in the stoichiometric composition. For example, the oxide semiconductor film is preferably formed by a sputtering method. In this case, it is preferable to form the film under conditions in which the proportion of oxygen in the film forming gas is high, and particularly in an oxygen atmosphere. It is preferable to form the film using oxygen gas (100% oxygen gas). When the film is formed under the conditions of 100% oxygen gas, for example, the film formation temperature is 300°C or higher. Even if the film is heated, the release of Zn from the film is suppressed.
[0146] The oxide semiconductor film may have a structure in which a plurality of oxide semiconductor films are stacked. For example, The oxide semiconductor film is a stack of a first oxide semiconductor film and a second oxide semiconductor film. The oxide semiconductor film and the second oxide semiconductor film may be formed using metal oxides having different compositions. For example, a first oxide semiconductor film is made of an oxide containing three metal elements, and a second oxide semiconductor film is made of an oxide containing three metal elements. For example, an oxide including two metal elements may be used as the first oxide semiconductor film and the second oxide semiconductor film. The oxide semiconductor film 2 may be an oxide containing three metal elements.
[0147] In addition, the first oxide semiconductor film and the second oxide semiconductor film are made to contain the same elements. For example, the atomic ratio of the first oxide semiconductor film may be set to In:Ga:Zn= The atomic ratio of the first oxide semiconductor film is In:Ga:Zn=3:1:2. The atomic ratio of the first oxide semiconductor film may be In:Ga:Zn=1:3:2. The atomic ratio of In:Ga:Zn in the second oxide semiconductor film may be 2:1:3.
[0148] At this time, the first oxide semiconductor film and the second oxide semiconductor film, which are closer to the gate electrode, The content ratio of In and Ga in the oxide semiconductor film is preferably In>Ga. The content ratio of In and Ga in the oxide semiconductor film on the far side may be set to In≦Ga.
[0149] In oxide semiconductors, the s orbitals of heavy metals mainly contribute to carrier conduction, and the inclusion of In Increasing the ratio tends to increase the overlap of s orbitals, so In>Ga The oxide with this composition has a higher mobility than the oxide with In≦Ga composition. In addition, the formation energy of oxygen vacancies in Ga is larger than that in In, so oxygen vacancies are less likely to occur. In contrast, oxides with a composition of In≦Ga have more stable characteristics than oxides with a composition of In>Ga. To have sexuality.
[0150] An oxide semiconductor with a composition of In>Ga is applied to the channel side, and By applying an oxide semiconductor with a composition of In≦Ga to the other side of the panel, It is possible to further improve the mobility and reliability of the semiconductor device.
[0151] In addition, the first oxide semiconductor film and the second oxide semiconductor film are formed of oxide semiconductors having different crystallinity. That is, a single crystal oxide semiconductor film, a polycrystalline oxide semiconductor film, an amorphous oxide semiconductor film, A structure in which a nitride semiconductor film, a microcrystalline oxide semiconductor film, or a CAAC-OS film is appropriately combined. In addition, at least one of the first oxide semiconductor film and the second oxide semiconductor film may be When an amorphous oxide semiconductor is used for either one of the two, the internal stress of the oxide semiconductor film or the external stress This reduces the variation in transistor characteristics and further improves the reliability of the transistor. It is possible to increase the
[0152] On the other hand, amorphous oxide semiconductors are prone to absorbing impurities that act as donors, such as hydrogen. Oxygen vacancies are easily generated, so the oxide semiconductor film on the channel side is easily converted to n-type. It is preferable to use a crystalline oxide semiconductor film such as a CAAC-OS film.
[0153] In addition, the oxide semiconductor film has a stacked structure of three or more layers, and the amorphous semiconductor film is formed by stacking the multiple crystalline semiconductor films. A structure in which a conductor film is sandwiched may be used. Also, a structure in which a crystalline semiconductor film and an amorphous semiconductor film are alternately stacked may be used. A structure in which
[0154] In addition, in the case where the oxide semiconductor film has a stacked structure of a plurality of layers, the above structure may be formed by appropriately combining the layers. They can be used in combination.
[0155] In addition, the oxide semiconductor film has a stacked structure of multiple layers, and oxygen is added to each oxide semiconductor film after it is formed. The addition of oxygen can be performed by heat treatment in an oxygen atmosphere, ion implantation, ion doping, etc. Plasma immersion ion implantation method, plasma immersion ion implantation method, oxygen-containing atmosphere For example, a plasma treatment can be used.
[0156] By adding oxygen to each oxide semiconductor film, oxygen vacancies in the oxide semiconductor are reduced. This can enhance the effectiveness of the system.
[0157] In addition, the insulating film in contact with the oxide semiconductor film was measured using X-ray reflectometry (XRR). The preferred overall film density, as measured by flexometry, is 2.26 g / cm 3 More than 2.50g / cm 3 The insulating film having a film density in this range has a high It is possible to combine the amount of oxygen released.
[0158] When forming an insulating film, the active species of the source gas enters the surface on which the film is to be formed (here, the source electrode and the drain electrode). After being adsorbed on the insulating film (the upper surface of the rain electrode), it migrates on the surface on which it is to be formed. When the film is capable of supplying the active species of the source gas, the dangling bonds of the active species of the source gas are absorbed by the insulating film. The surface of the substrate is terminated with excess oxygen and stabilized, and the amount of surface migration of the activated species of the source gas on the substrate is reduced. As a result, there are some areas where it is difficult to form a film, such as steps, and voids are easily generated. Furthermore, it is difficult for the activated species of the source gas of the film to be formed thereafter to penetrate into the voids. The gap widens further.
[0159] In addition, the formation of the nitride insulating film allows the gap to be closed, and the closed space The voids can absorb a large amount of oxygen, so oxygen from the oxide insulating film is absorbed during heating. Therefore, oxygen defects in the oxide semiconductor film can be eliminated by the oxide insulating film. This allows oxygen to be replenished from the source, improving the reliability of the transistor. do.
[0160] In addition, when oxide insulating films are stacked as in the third embodiment shown in FIGS. 7B and 7C, In this case, the oxide insulating film 410b serves as a film that supplies oxygen to the oxide semiconductor film. When the nitride insulating film 411 is formed in contact with the insulating film 410b by applying high power, the oxide insulating film 4 There is a risk that excess oxygen contained in 10b will be released, decreasing the oxygen supply capacity.
[0161] Therefore, the oxide insulating film 410c and the oxide insulating film 410 are formed directly under the nitride insulating film 411. By providing the nitride insulating film 411, the oxide insulating film 410b In addition, a decrease in the oxygen supply ability of the oxide insulating film 410d can be suppressed.
[0162] Next, the oxide semiconductor film 31 and the oxide semiconductor film capable of supplying oxygen are formed by heat treatment. A model of the movement of nitrogen, hydrogen, and water in the insulating film 32 is described with reference to FIGS. 25 to 27. In addition, in Fig. 25 to Fig. 27, the dashed arrows indicate the movement of each atom due to heating. The solid arrows indicate the changes during or before and after the heat treatment. The insulating film 32 is an oxide insulating film containing more oxygen than the oxygen that satisfies the stoichiometric composition. I will use this to explain.
[0163] FIG. 25 shows a model of what may mainly occur in the oxide insulating film 32 due to heat treatment.
[0164] 25A shows the behavior of nitrogen atoms during heat treatment. Nitrogen atoms N (here, two nitrogen atoms) are converted into oxide insulating film 32 or surface This model shows that the nitrogen atoms bond to each other at the oxygen atom and become nitrogen molecules, which are then desorbed from the oxide insulating film 32.
[0165] FIG. 25B is a model showing the behavior of oxygen atoms due to heat treatment. 2 contains more oxygen atoms (exO, here 2 The heat treatment causes the oxygen atoms to bond to each other in the oxide insulating film 32 or on the surface. The atoms become atoms and are separated from the oxide insulating film 32 .
[0166] FIG. 25(C) is a model showing the behavior of hydrogen atoms and oxygen atoms due to heat treatment. The hydrogen atoms H (here, two hydrogen atoms) and the stoichiometric More oxygen atoms exO than satisfy the composition are formed in the oxide insulating film 32 or is bonded to the surface, becomes a water molecule, and is desorbed from the oxide insulating film 32.
[0167] FIG. 25D is a model showing the behavior of water molecules due to heat treatment. Water molecules contained in the oxide insulating film 32 are released from the oxide insulating film 32 by heat treatment.
[0168] As shown in the above model, nitrogen, hydrogen, and fluorine are released from the oxide insulating film 32 by heat treatment. The nitrogen, hydrogen, and water contents in the film can be reduced by desorbing one or more of the nitrogen, hydrogen, and water. can.
[0169] Next, a model that may occur in the oxide semiconductor film 31 due to heat treatment will be described with reference to FIG. Reveal.
[0170] 26A is a model showing behavior of nitrogen atoms due to heat treatment in an oxide semiconductor film. The nitrogen atoms N (two nitrogen atoms in this case) contained in 31 are converted into oxide semiconductors by heat treatment. the oxide semiconductor film 31, the interface between the oxide semiconductor film 31 and the oxide insulating film 32, or the interface between the oxide insulating film 32 and the oxide semiconductor film 31, Alternatively, the nitrogen atoms bond on the surface to become nitrogen molecules, which are then desorbed from the oxide semiconductor film 31 .
[0171] FIG. 26(B) is a model showing the behavior of hydrogen atoms and oxygen atoms due to heat treatment. The hydrogen atoms H (here, two hydrogen atoms) contained in the oxide semiconductor film 31 are converted into hydrogen atoms by the heat treatment. After moving to the oxide insulating film 32, the oxide insulating film 32 or its surface is stoichiometrically The oxygen atoms exO bond to more oxygen atoms than satisfy the composition, forming water molecules, and the oxide insulating film 3 Detach from 2.
[0172] FIG. 26(C) is a model showing different behavior of hydrogen atoms and oxygen atoms due to heat treatment. The amount of hydrogen atoms H contained in the oxide semiconductor film 31 is greater than the amount of oxygen that satisfies the stoichiometric composition. The oxide semiconductor film 31 or the oxide semiconductor film 3 1 and the oxide insulating film 32. To detach.
[0173] Figures 26(D) and 26(E) show different behaviors of hydrogen and oxygen atoms by heat treatment. The hydrogen atom H and the oxygen atom O contained in the oxide semiconductor film 31 are By the heat treatment, the oxide semiconductor film 31, the boundary between the oxide semiconductor film 31 and the oxide insulating film 32 The water molecules bond to the oxide insulating film 32 or its surface, and the water molecules are then bonded to the oxide insulating film 32 or its surface. At this time, the oxygen atoms are released from the insulating film 32. As shown in FIG. 26(E), the oxygen vacancy Vo occurs, but the compound contained in the oxide insulating film 32 More oxygen atoms exO than meet the stoichiometric composition move to the oxygen vacancy Vo, The oxygen deficiency Vo is filled and becomes an oxygen atom O.
[0174] From the above, it is considered that at least one of nitrogen, hydrogen, and water is removed from the oxide semiconductor film 31 by the heat treatment. By removing the top, the nitrogen, hydrogen, and water contents in the film can be reduced.
[0175] Next, a model of change in oxygen vacancies in the oxide semiconductor film 31 due to heat treatment will be described with reference to FIG. 7 will be used to explain.
[0176] When more oxygen than the stoichiometric composition is transferred to the oxide semiconductor film 31, the chemical More oxygen than meets the stoichiometric composition is added to the first oxygen atom from the position of the first oxygen atom. The first oxygen atom that was expelled moves to the position of the second oxygen atom, and the second 2 oxygen atoms are pushed out. Thus, more oxygen is added than is necessary to satisfy the stoichiometric composition. When the oxygen atoms move to the oxide semiconductor film 31, the oxygen atoms are pushed out from among the oxygen atoms. In FIG. 27, the pushing out of an oxygen atom between multiple oxygen atoms is The oxide semiconductor film 31 includes three oxygen vacancies (Vo_1 to Vo_3) and an oxygen The oxygen contained in the oxide insulating film 32 capable of supplying oxygen, specifically, the stoichiometric composition The oxygen vacancy is changed by using more oxygen atoms (exO_1~exO_3) than satisfy the condition. The oxide insulating film 32 is formed under low power conditions and has a coating A stack of an oxide insulating film 32a capable of supplying oxygen and an oxide insulating film 32b capable of supplying oxygen. It is a membrane.
[0177] In FIG. 27, three oxygen vacancies (Vo_1 to Vo_ 3) and oxygen contained in the oxide insulating film 32b capable of supplying oxygen, specifically, It shows more oxygen atoms (exO_1~exO_3) than satisfy the stoichiometric composition.
[0178] FIG. 27(A) shows the reaction between oxygen vacancies Vo_1 and oxygen atoms exO_1 due to heat treatment. The oxygen atom exO_1 is more than the stoichiometric oxygen atom, and the heat treatment The oxygen vacancy Vo_1 moves to the position of the oxygen vacancy Vo_1 included in the oxide semiconductor film 31. is filled in, resulting in an oxygen atom O_1.
[0179] Next, as shown in FIG. 27(B), more oxygen atoms than satisfy the stoichiometric composition are added. When exO_2 approaches the position of oxygen atom O_1 contained in the oxide semiconductor film 31, An oxygen atom O is removed from the position of the atom O_1. The removed oxygen atom O is an oxygen vacancy Vo_2 The oxygen vacancy Vo_2 is filled and an oxygen atom O_2 is formed. The position of the removed oxygen atom O_1 becomes an oxygen vacancy, but an oxygen atom ex O_2 moves and becomes oxygen atom O_1a.
[0180] Next, as shown in FIG. 27(C), more oxygen atoms than satisfy the stoichiometric composition are added. When exO_3 approaches the position of the oxygen atom O_1a included in the oxide semiconductor film 31, An oxygen atom O is removed from the position of atom O_1a. The removed oxygen atom O is an oxygen atom O_ The oxygen atom O moves to position 2. The oxygen atom O leaves the oxygen atom O_2. The released oxygen atom O is The oxygen vacancy Vo_3 is filled and becomes an oxygen atom O_3. The position of the atom O_1a becomes an oxygen vacancy, but the oxygen atom exO_3 moves to the oxygen vacancy, The oxygen atom O_1b is formed. The same is true for the oxygen atom O_2 from which the oxygen atom has been removed. In the oxygen vacancy, oxygen is released from the oxygen atom O_1a and moves to the oxygen vacancy. It becomes the elementary atom O_2a.
[0181] Through the above steps, oxygen contained in the oxide insulating film 32b capable of supplying oxygen is It is possible to compensate for oxygen vacancies in the oxide semiconductor film 31. Not only the oxygen vacancies on the surface of the body membrane 31 but also the oxygen vacancies in the membrane are filled by the heat treatment. From the above, the oxide insulating film 32b to which oxygen can be supplied while being heated is formed. Alternatively, after providing the oxide insulating film 32b capable of supplying oxygen, a heat treatment is performed. By performing the above-mentioned treatment, the amount of oxygen vacancies in the oxide semiconductor film 31 can be reduced. .
[0182] In addition, oxygen is provided in the back channel of the oxide semiconductor film 31 as the oxide insulating film 32a. Through the insulating oxide film, an oxide layer containing more oxygen than the stoichiometric composition is formed. By providing the oxide insulating film 32b, oxygen is moved to the back channel side of the oxide semiconductor film 31. This makes it possible to reduce oxygen deficiencies in the region.
[0183] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0184] (Embodiment 5) A semiconductor device having a display function (display) using the transistor shown as an example in the above embodiment In addition, a part of a driver circuit including a transistor can be manufactured. Alternatively, the entire display can be formed on the same substrate as the pixel section to form a system-on-panel. In this embodiment, a display device using the transistors shown as examples in the above embodiment will be described. An example of the device will be described with reference to Figs. 9 to 12. 11 is a cross-sectional view showing the cross-sectional configuration of the portion indicated by the dashed line MN in FIG. 9(B). It is.
[0185] In FIG. 9A, a pixel portion 902 provided on a first substrate 901 is surrounded by a A sealant 905 is provided and the substrate is sealed with a second substrate 906. In the above, a region different from the region surrounded by the sealant 905 on the first substrate 901 is In the signal line driving region, a signal line formed of a single crystal semiconductor or a polycrystalline semiconductor on a separately prepared substrate is A signal line driver circuit 903 and a scanning line driver circuit 904 are also mounted. 3. Various signals and potentials given to the scanning line driver circuit 904 or the pixel portion 902 are F PC(Flexible printed circuit)918a, FPC918b is supplied by
[0186] In FIG. 9B and FIG. 9C, a pixel portion 902 is provided on a first substrate 901. A sealant 905 is provided so as to surround the scanning line driver circuit 904. A second substrate 906 is provided on the pixel portion 902 and the scanning line driver circuit 904. The pixel portion 902 and the scanning line driver circuit 904 are formed by a first substrate 901, a sealant 905, and a third substrate 906. The display element is sealed by the second substrate 906. ) is different from the region surrounded by the sealant 905 on the first substrate 901. A signal line formed of a single crystal semiconductor or a polycrystalline semiconductor on a separately prepared substrate is placed in the region where the A driver circuit 903 is mounted. In FIG. 9B and FIG. 9C, the signal line driver Various signals and power supplies to the circuit 903, the scanning line driver circuit 904, or the pixel portion 902 The position is provided by FPC918.
[0187] In addition, in FIG. 9B and FIG. 9C, a signal line driver circuit 903 is separately formed. Although an example in which the first substrate 901 is mounted is shown, the present invention is not limited to this configuration. Alternatively, a driving circuit may be formed separately and mounted, or a part of a signal line driving circuit or a scanning line driving circuit may be mounted. Only a part of it may be formed separately and mounted.
[0188] The method of connecting the separately formed drive circuit is not particularly limited, and may be any method such as COG ( hip on glass method, wire bonding method, or TAB (Tape The Automated Bonding method can be used. This is an example of mounting a signal line driver circuit 903 and a scanning line driver circuit 904 by the COG method. FIG. 9(B) shows an example in which a signal line driver circuit 903 is mounted by the COG method, and FIG. 9 is an example in which a signal line driver circuit 903 is mounted by the TAB method.
[0189] The display device includes a panel in which a display element is sealed, and a controller for the panel. This includes modules in which ICs, etc., including lasers, are mounted.
[0190] In this specification, the term "display device" refers to an image display device, a display device, or Refers to light sources (including lighting devices) and connectors, such as FPC or TAB tape. Or a module with a TCP attached, a printed wiring board is provided beyond the TCP A module in which an IC (integrated circuit) is directly mounted on a module or display element using the COG method. All modules are included in the display device.
[0191] In addition, the pixel portion and the scanning line driver circuit provided on the first substrate include a plurality of transistors. The transistor described in the above embodiment can be applied to the semiconductor device.
[0192] Examples of display elements provided in the display device include liquid crystal elements (also called liquid crystal display elements), light-emitting elements, and the like. A light-emitting element (also called a light-emitting display element) can be used. This category includes elements whose brightness is controlled by a specific factor, such as inorganic EL (Electroluminescent) devices. These include organic EL elements, electronic inks, etc. A display medium whose contrast changes due to an electrical effect, such as a liquid crystal display, can also be used.
[0193] The display device shown in FIG. 10A has a connection terminal electrode 915 and a terminal electrode 916. The connection terminal electrode 915 and the terminal electrode 916 are anisotropically conductive with the terminals of the FPC 918. The electrodes are electrically connected via the electrode 919 .
[0194] The connection terminal electrode 915 is formed from the same conductive film as the first electrode 930, and the terminal electrode 916 are the source and drain electrodes of the transistor 910 and the transistor 911 (hereinafter, The pair of electrodes (also called a pair of electrodes) are formed of the same conductive film.
[0195] The display device shown in FIG. 10B includes a connection terminal electrode 915a, a connection terminal electrode 915b, and The terminal electrode 916 is connected to the connection terminal electrode 915a, the connection terminal electrode 915b, and the terminal The electrode 916 is electrically connected to a terminal of the FPC 918 via an anisotropic conductive material 919. It is being done.
[0196] The connection terminal electrode 915a is formed from the same conductive film as the first electrode 930. The terminal electrode 915b is formed from the same conductive film as the third electrode 941. The electrode of the first electrode 910 is formed from the same conductive film as that of the pair of electrodes of the transistor 911 .
[0197] As shown in FIG. 11, the semiconductor device has a connection terminal electrode 955 and a terminal electrode 916. The connection terminal electrode 955 and the terminal electrode 916 are different from the terminals of the FPC 918. They are electrically connected via isotropic conductive agent 919 .
[0198] The connection terminal electrode 955 is formed from the same conductive film as the second electrode 931, and the terminal electrode 916 The pair of electrodes of the transistor 910 and the transistor 911 are formed of the same conductive film. do.
[0199] A pixel portion 902 and a scanning line driver circuit 904 provided on a first substrate 901 are 10 and 11, the transistor included in the pixel portion 902 is 9 illustrates a transistor 910 and a transistor 911 included in the scan line driver circuit 904. In FIG. 10(A) and FIG. 10(B), a transistor 910 and a transistor 911 An insulating film 924 corresponding to the insulating film 412 in Embodiment 1 is provided on the insulating film 924. An interlayer insulating film 921 that functions as a flattening film is further provided on the insulating film. 923 is an insulating film that functions as a base film.
[0200] In this embodiment, the transistors 910 and 911 are the same as those in the above embodiment. The transistor shown in FIG.
[0201] In FIG. 11, the semiconductor of the transistor 911 for the driver circuit is formed over the insulating film 924. 9 shows an example in which a conductive film 917 is provided at a position overlapping with a channel forming region of the body membrane. Note that an oxide semiconductor film is used as the semiconductor film. By placing it in a position that overlaps with the channel formation area, the The variation in the threshold voltage of the transistor 911 can be further reduced. The potential of the gate electrode of the transistor 7 may be the same as or different from that of the gate electrode of the transistor 911. The conductive film 917 can also function as a second gate electrode. , GND, 0V, or may be floating.
[0202] The conductive film 917 also has a function of blocking an external electric field. (The circuit part including the transistor) The shielding function of the conductive film 917 prevents the device from being affected by external electric fields such as static electricity. This can prevent the electrical characteristics of the transistor from being changed. The above-described embodiment mode can be applied to any of the transistors.
[0203] The transistor 910 provided in the pixel portion 902 is electrically connected to a display element. The display element is not particularly limited as long as it can display an image. It can be used.
[0204] A first electrode and a second electrode (a pixel electrode, a common electrode, a counter electrode) for applying a voltage to a display element In the case of a photodiode, the direction of the light to be extracted, the location of the electrode, and the The light transmission or reflectivity can be selected depending on the pattern structure.
[0205] The first electrode 930, the second electrode 931, and the third electrode 941 include tungsten oxide. Indium oxide, indium zinc oxide with tungsten oxide, indium zinc oxide with titanium oxide Indium oxide, indium tin oxide containing titanium oxide, indium tin oxide (hereinafter referred to as I TO), indium zinc oxide, indium tin oxide with added silicon oxide, etc. A light-transmitting conductive material such as the above can be used.
[0206] The first electrode 930, the second electrode 931, and the third electrode 941 are made of tungsten (W ), Molybdenum (Mo), Zirconium (Zr), Hafnium (Hf), Vanadium (V ), Niobium (Nb), Tantalum (Ta), Chromium (Cr), Cobalt (Co), Nickel (Ni), titanium (Ti), platinum (Pt), aluminum (Al), copper (Cu), silver (A g) One or more of the following metals, their alloys, or their metal nitrides are used: It can be formed by:
[0207] The first electrode 930, the second electrode 931, and the third electrode 941 are made of a conductive polymer. The conductive layer can be formed using a conductive composition containing a conductive polymer. As the polymer, a so-called π-electron conjugated conductive polymer can be used. rianiline or its derivatives, polypyrrole or its derivatives, polythiophene or its derivatives or a copolymer or a copolymer of two or more of aniline, pyrrole and thiophene. or derivatives thereof.
[0208] FIG. 10 shows an example of a liquid crystal display device using a liquid crystal element as a display element. This is an example that employs the vertical electric field method.
[0209] In FIG. 10A, a liquid crystal element 913 which is a display element has a first electrode 930 and a second electrode 931. The liquid crystal layer 908 is sandwiched between an alignment film and an electrode 931. The second electrode 931 is provided with an insulating film 932 and an insulating film 933 which function as a second electrode. The first electrode 930 and the second electrode 931 are disposed on the second substrate 906 side, and are connected to the liquid crystal layer 908. The structure is such that they overlap through the
[0210] In FIG. 10B, a liquid crystal element 943, which is a display element, is formed on an interlayer insulating film 921. The liquid crystal layer 908 includes a first electrode 930, a third electrode 941, and a liquid crystal layer 908. 41 functions as a common electrode. An insulating layer is provided between the first electrode 930 and the third electrode 941. The insulating film 944 is formed using a silicon nitride film. Insulating films 932 and 933 are provided to sandwich the crystal layer 908 and function as alignment films. It is being done.
[0211] The spacer 935 is a columnar spacer obtained by selectively etching an insulating film. In order to control the distance (cell gap) between the first electrode 930 and the second electrode 931, It should be noted that a spherical spacer may also be used.
[0212] When liquid crystal elements are used as display elements, thermotropic liquid crystal, low molecular weight liquid crystal, high molecular weight liquid crystal, etc. Liquid crystal, polymer dispersed liquid crystal, ferroelectric liquid crystal, antiferroelectric liquid crystal, etc. can be used. These liquid crystal materials can exhibit cholesteric, smectic, cubic, and chromatic phases depending on the conditions. It shows an isotropic phase, an isotropic phase, etc.
[0213] Alternatively, a liquid crystal that exhibits a blue phase without using an alignment film may be used. When the temperature of the cholesteric liquid crystal is increased, the cholesteric phase transitions to the isotropic phase. The blue phase appears only in a narrow temperature range, so it is necessary to improve the temperature range. In order to improve the liquid crystal layer, a liquid crystal composition containing a chiral agent is used. The liquid crystal composition containing the liquid crystal and the chiral agent has a short response time of 1 msec or less, and is optically Since the display is isotropic, no alignment treatment is required and the viewing angle dependency is small. Since the rubbing process is unnecessary, the electrostatic breakdown caused by the rubbing process is eliminated. Therefore, defects and damage to the liquid crystal display device during the manufacturing process can be reduced. Therefore, the productivity of the liquid crystal display device can be improved.
[0214] The first substrate 901 and the second substrate 906 are fixed together by a sealant 925 . The sealant 925 can be made of an organic resin such as a thermosetting resin or a photocurable resin.
[0215] In the liquid crystal display device shown in FIG. 10A, the sealant 925 is a gate insulating film. The interlayer insulating film 921 is provided on the inside of the seal material 925. The insulating film 922 is formed by laminating a silicon nitride film and a silicon oxynitride film. When the insulating film 924 is selectively etched, the oxide / nitride silicon oxide film on the upper layer of the gate insulating film 922 is It is preferable to etch the silicon film to expose the silicon nitride film. The insulating film 922 is formed on the outer periphery of the insulating film 925. It is possible to prevent water from entering the inside of the sealant 925 from the outside.
[0216] In the liquid crystal display device shown in FIG. 10B, the sealant 925 is in contact with the insulating film 924. An interlayer insulating film 921 is provided on the inner side of the sealing material 925. Since the silicon nitride film on the surface of the insulating film 924 contacts the sealing material 925, water from the outside is prevented from entering the sealing material 924. It is possible to suppress the penetration of the ion exchange resin into the interior of 25.
[0217] The size of the storage capacitor provided in the liquid crystal display device is determined by the capacitance of the transistor arranged in the pixel portion. It is set so that the charge can be held for a certain period of time, taking into account the break current, etc. By using a transistor having a nitride semiconductor film, the liquid crystal capacitance in each pixel is It is sufficient to provide a storage volume having a size of 1 / 3 or less, preferably 1 / 5 or less, of the capacity of the Therefore, the aperture ratio of the pixel can be increased.
[0218] In addition, in display devices, black matrices (light-shielding films), polarizing members, phase difference members, reflectors, Optical members (optical substrates) such as anti-reflection members are provided as appropriate. For example, a polarizing substrate and a phase A circularly polarized light source such as a backlight or a sidelight may be used as the light source. may also be used.
[0219] In addition, the display method in the pixel section uses the progressive method, interlace method, etc. In addition, the color elements controlled by pixels when displaying colors are RGB (RGB=RGB). The color is not limited to the three colors RGBW (W stands for white, G stands for red, B stands for green, and B stands for blue). ) or RGB plus one or more colors such as yellow, cyan, or magenta The size of the display area may be different for each dot of the color element. The present invention is not limited to color display devices, but may be applied to monochrome display devices. It is also possible.
[0220] FIG. 12 shows a second electrode provided on the substrate 906 in the display device shown in FIG. An example in which a common connection part (pad part) for electrically connecting to 931 is formed on the substrate 901 Shows.
[0221] The common connection portion is disposed at a position overlapping with the seal material for bonding the substrate 901 and the substrate 906. and is electrically connected to the second electrode 931 via conductive particles contained in the sealing material. Or, provide a common connection part in a place that does not overlap with the sealing material (excluding the pixel part) and A paste containing conductive particles is provided separately from the sealing material so as to overlap the connection portion, and a second electrode 9 is formed. 31 may be electrically connected.
[0222] FIG. 12(A) is a cross-sectional view of the common connection portion, which corresponds to IJ in the top view shown in FIG. 12(B). Correct.
[0223] The common potential line 975 is provided on the gate insulating film 922 and is connected to the transistor 9 shown in FIG. 10. The source electrode 971 or the drain electrode 973 is made of the same material and in the same process. do.
[0224] The common potential line 975 is covered with the insulating film 924 and the interlayer insulating film 921. 24 and the interlayer insulating film 921 have a plurality of openings at positions overlapping the common potential line 975. The opening is provided for the source electrode 971 or the drain electrode 973 of the transistor 910. The contact hole connecting one of the first electrodes 930 and the second electrode 930 is fabricated in the same process.
[0225] In addition, the common potential line 975 and the common electrode 977 are connected at the opening. 77 is provided on the interlayer insulating film 921, and is connected to the connection terminal electrode 915 and the first electrode 9 of the pixel portion. It is made from the same materials and in the same process as 30.
[0226] In this manner, the common connection portion is formed in the same manufacturing process as the switching element of the pixel portion 902. It can be manufactured.
[0227] The common electrode 977 is an electrode that comes into contact with the conductive particles contained in the sealing material, and is disposed on the substrate 906. An electrical connection is made with the second electrode 931 of the first electrode 931 .
[0228] 12C, a common potential line 985 is connected to the gate of a transistor 910. They may be made of the same material and in the same process as the electrodes.
[0229] In the common connection portion shown in FIG. 12C, the common potential line 985 is A gate insulating film 922 and an insulating film 923 are provided below the insulating film 924 and the interlayer insulating film 921. 924 and the interlayer insulating film 921 have a plurality of openings at positions overlapping the common potential line 985. The opening is formed on the source electrode 971 or the drain electrode 973 of the transistor 910. The insulating film 924 and the contact hole connecting the first electrode 930 are formed in the same process. After etching the interlayer insulating film 921, the gate insulating film 922 is selectively etched. It is formed by
[0230] In addition, the common potential line 985 and the common electrode 987 are connected at the opening. 87 is provided on the interlayer insulating film 921, and is connected to the connection terminal electrode 915 and the first electrode 9 of the pixel portion. It is made from the same materials and in the same process as 30.
[0231] In the FFS mode liquid crystal display device shown in FIG. 10B, the common electrode 977, 987 each connects to the third electrode 941 .
[0232] Next, a light-emitting device using electroluminescence as a display element included in the display device The light-emitting element that utilizes electroluminescence can be applied to a light-emitting material They are classified according to whether the material is an organic compound or an inorganic compound. The latter is called an inorganic EL element.
[0233] In an organic EL element, electrons and positive electrodes are released from a pair of electrodes by applying a voltage to the light-emitting element. The holes are then injected into a layer containing a light-emitting organic compound, and a current is passed through them. The recombination of carriers (electrons and holes) causes light-emitting organic compounds to form excited states. When the excited state returns to the ground state, light is emitted. Such a light-emitting element is called a current-excitation type light-emitting element.
[0234] Inorganic EL elements are classified into dispersion type inorganic EL elements and thin film type inorganic EL elements depending on the element structure. Dispersion-type inorganic EL elements have a light-emitting layer in which particles of light-emitting material are dispersed in a binder. The emission mechanism is a donor-based ion exchange reaction that utilizes the donor and acceptor levels. This is an acceptor recombination type emission. Thin-film inorganic EL elements sandwich the light-emitting layer between dielectric layers. The structure is sandwiched between electrodes, and the light emission mechanism is the inner shell electron transition of metal ions. This is a localized light emission that utilizes organic EL elements. do.
[0235] The light emitting element only needs to have at least one of the pair of electrodes transparent in order to extract light. Then, a transistor and a light emitting element are formed on the substrate, and light is emitted from the opposite side of the substrate. Top emission, bottom emission, and side emission. There are light emitting devices with a double-sided emission structure that emits light from the side, and light emitting devices with any emission structure are suitable. It can be used.
[0236] FIG. 11 shows an example of a light-emitting device using a light-emitting element as a display element. The transistor 963 is electrically connected to a transistor 910 provided in the pixel portion 902. The light emitting element 963 is configured as follows: The layer structure is not limited to the configuration shown in FIG. Accordingly, the configuration of the light emitting element 963 can be changed as appropriate.
[0237] A silicon nitride film 950 is provided between the interlayer insulating film 921 and the first electrode 930. The silicon film 950 contacts the side surfaces of the interlayer insulating film 921 and the insulating film 924. Silicon nitride A partition 960 is provided on the edge of the membrane 950 and the first electrode 930. The partition 960 is made of an organic insulating material. In particular, the first electrode is formed of a photosensitive resin material. An opening is formed on the pole 930, and the sidewall of the opening is formed with a continuous curvature. It is preferable to form the surface so as to form a flat surface.
[0238] The light-emitting layer 951 may be composed of a single layer or a plurality of layers may be laminated. Either way is fine.
[0239] In order to prevent oxygen, hydrogen, moisture, carbon dioxide, and the like from entering the light-emitting element 963, the second electrode 9 A protective layer may be formed on the insulating film 31 and the partition wall 960. The protective layer may be formed of silicon nitride, nitride, or the like. Silicon oxide, aluminum oxide, aluminum nitride, aluminum oxide nitride, oxyaluminum nitride The first substrate 901 and the second substrate 902 can be formed with aluminum oxide, DLC film, etc. A filler 964 is provided in the space sealed by the substrate 906 and the sealant 936. This provides a highly airtight and low outgassing protection against exposure to the outside air. Packaging with film (lamination film, UV-curable resin film, etc.) and covering material It is preferable to enclose the
[0240] The sealant 936 is made of organic resin such as thermosetting resin or photocurable resin, or a free resin containing low melting point glass. Frit glass can be used. Frit glass is highly resistant to impurities such as water and oxygen. In addition, when frit glass is used as the sealant 936, In this case, as shown in FIG. 11, a frit glass is provided on the silicon nitride film 950 to form a silicon nitride film. This improves the adhesion between the silicon oxide film 950 and the frit glass, and also prevents the seal material 9 from being exposed from the outside. 36 It is possible to prevent water from entering the interior.
[0241] Filler 964 can be inert gas such as nitrogen or argon, or ultraviolet curing resin or Thermosetting resin can be used, and PVC (polyvinyl chloride), acrylic resin, poly Imide, epoxy resin, silicone resin, PVB (Polyvinyl Butyral) or EVA (ethylene vinyl acetate) can be used. For example, nitrogen can be used as a filler. Good.
[0242] If necessary, a polarizing plate or a circular polarizing plate (including an elliptical polarizing plate) may be attached to the light-emitting surface of the light-emitting element. ), retardation plates (lambda / 4 plates, lambda / 2 plates), color filters, and other optical films are appropriately installed. Alternatively, the polarizing plate or the circular polarizing plate may be provided with an anti-reflection film. It is possible to apply an anti-glare treatment that can diffuse reflected light and reduce glare.
[0243] In addition, since transistors are easily damaged by static electricity, etc., It is preferable to provide a protection circuit using a non-linear element.
[0244] As described above, by using the transistor described in the above embodiment, Therefore, a highly reliable semiconductor device can be provided.
[0245] This embodiment can be implemented in appropriate combination with the configurations described in other embodiments. It is Noh.
[0246] (Embodiment 6) The transistors according to the above-mentioned embodiments are used to provide an image sensor for reading information about an object. Therefore, a semiconductor device having a sensor function can be manufactured.
[0247] FIG. 13A shows an example of a semiconductor device having an image sensor function. FIG. 13(B) is a cross-sectional view showing a part of the photosensor. do.
[0248] The photodiode 602 has one electrode connected to a photodiode reset signal line 658. The other electrode is electrically connected to the gate of transistor 640. 0 indicates that either the source or the drain is connected to the photosensor reference signal line 672, The other of the drains is electrically connected to one of the source and drain of a transistor 656. The transistor 656 has a gate connected to a gate signal line 659 and a source or drain The other end is electrically connected to a photosensor output signal line 671.
[0249] Note that in the circuit diagrams in this specification, a transistor including an oxide semiconductor film is not clearly shown. In order to make it easier to understand, the symbol for a transistor using an oxide semiconductor film is written as “OS.” In FIG. 13A, transistors 640 and 656 are the same as in the previous embodiment. The transistor in accordance with the present invention can be applied to the present invention, which is a transistor including an oxide semiconductor film. In this embodiment, a transistor having a structure similar to that of the transistor 450 shown in the first embodiment is used. Here is an example of applying the register.
[0250] FIG. 13B shows a photodiode 602 and a transistor 603 in the photosensor. 40, a substrate 601 (element substrate) having an insulating surface is provided with a sensor. A functioning photodiode 602 and transistor 640 are provided. A substrate 613 is provided on the diode 602 and the transistor 640 using an adhesive layer 608. It is being done.
[0251] An insulating film 632, a planarizing film 633, and a planarizing film 634 are provided on the transistor 640. The photodiode 602 has an electrode 641b formed on the planarizing film 633 and a A first semiconductor film 606a, a second semiconductor film 606b, and and a third semiconductor film 606c, and a planarization film 634 are provided on the first to third semiconductor films. An electrode 642 electrically connected to the electrode 641b via a gate electrode 643 and provided in the same layer as the electrode 641b. , and an electrode 641 a electrically connected to the electrode 642 .
[0252] The electrode 641b is electrically connected to the conductive film 643 formed on the flattening film 634. 42 is electrically connected to the conductive film 645 via the electrode 641a. The photodiode 602 is electrically connected to the gate electrode of the transistor 640. The resistor 640 is electrically connected to the
[0253] Here, the first semiconductor film 606a is a semiconductor film having a p-type conductivity, and the second semiconductor film 606b is a semiconductor film having a p-type conductivity. The conductive film 606b is a high-resistance semiconductor film (i-type semiconductor film), and the third semiconductor film 606c is a In the example shown, a pin-type photodiode is used in which a semiconductor film having an n-type conductivity is laminated. .
[0254] The first semiconductor film 606a is a p-type semiconductor film, and is made of alumina containing an impurity element that imparts p-type conductivity. The first semiconductor film 606a can be formed of a ruthenium silicon film. Plasma CV is performed using semiconductor material gas containing Group 3 impurity elements (e.g., boron (B)). The semiconductor material gas used is silane (SiH4). Alternatively, Si2H6, SiH2Cl2, SiHCl3, SiCl4, SiF4, etc. may be used. In addition, after forming an amorphous silicon film that does not contain impurity elements, An impurity element may be introduced into the amorphous silicon film by ion implantation. By introducing impurity elements by a method such as a method of forming a semiconductor substrate, and then heating the semiconductor substrate, the impurity elements are diffused. In this case, the amorphous silicon film can be formed by LPCVD or vapor phase deposition. The first semiconductor film 606a may be formed by a deposition method, a sputtering method, or the like. It is preferable to form the insulating film so as to have a thickness of 50 nm or more.
[0255] The second semiconductor film 606b is an i-type semiconductor film (intrinsic semiconductor film) and is made of amorphous silicon. The second semiconductor film 606b is formed by using a semiconductor material gas. The amorphous silicon film is formed by the plasma CVD method. The semiconductor material gases are: Silane (SiH4) can be used. Alternatively, Si2H6, SiH2Cl2, SiHCl 3, SiCl4, SiF4, etc. may be used. The second semiconductor film 606b is formed by LPC The second semiconductor film 606b may be formed by a method such as a vapor deposition method, a vapor phase growth method, or a sputtering method. It is preferable that the film thickness is set to 200 nm or more and 1000 nm or less.
[0256] The third semiconductor film 606c is an n-type semiconductor film, and is an alumina film containing an impurity element that imparts n-type conductivity. The third semiconductor film 606c is formed of an amorphous silicon film. Using semiconductor material gas containing pure elements (e.g. phosphorus (P)), plasma CVD is used. Silane (SiH4) can be used as the semiconductor material gas. H6, SiH2Cl2, SiHCl3, SiCl4, SiF4, etc. may also be used. After forming an amorphous silicon film that does not contain impurity elements, the diffusion method or ion implantation method is used. An impurity element may be introduced into the amorphous silicon film by using an ion implantation method or the like. After the impurity element is introduced, the impurity element may be diffused by heating or the like. In this case, the method for forming the amorphous silicon film includes the LPCVD method, the vapor phase growth method, and The third semiconductor film 606c may be formed by sputtering or the like. It is preferable to form the insulating layer so that the thickness is 00 nm or less.
[0257] In addition, the first semiconductor film 606a, the second semiconductor film 606b, and the third semiconductor film 60 6c may be formed using a polycrystalline semiconductor instead of an amorphous semiconductor, or may be formed using a semi-crystalline semiconductor. Amorphous (Semi Amorphous Semiconductor: SAS) It may be formed using a semiconductor.
[0258] In addition, the mobility of holes generated by the photoelectric effect is smaller than that of electrons, so the pin type The photodiode exhibits better characteristics when the p-type semiconductor film side is used as the light receiving surface. From the surface of the substrate 601 on which the pin-type photodiode is formed, the photodiode 60 This shows an example of converting the light received by the semiconductor film 2 into an electrical signal. Since light from the semiconductor film side having a conductive type becomes disturbance light, the electrode uses a conductive film having a light-shielding property. In addition, the n-type semiconductor film side can be used as the light receiving surface.
[0259] The insulating film 632, the planarizing film 633, and the planarizing film 634 are made of an insulating material. Depending on the material, sputtering, plasma CVD, spin coating, dip coating, spray coating, etc. - Using coating, droplet ejection method (inkjet method), screen printing, offset printing, etc. The insulating film 632 can be formed similarly to the insulating film 412 in the first embodiment. of is used.
[0260] The planarization film 633 and the planarization film 634 may be made of, for example, polyimide, acrylic resin, or benzo Uses heat-resistant organic insulating materials such as cyclobutene resin, polyamide, and epoxy resin. In addition to the above organic insulating materials, low dielectric constant materials (low-k materials), Single layer of siloxane resin, PSG (phosphorus glass), BPSG (borophosphorus glass), etc. Alternatively, lamination may be used.
[0261] By detecting the light incident on the photodiode 602, information on the detected object is read. In addition, when reading the information of the detected object, a light source such as a backlight is used. It is possible.
[0262] The structures, methods, etc. described in this embodiment may be combined as appropriate with the structures, methods, etc. described in other embodiments. They can be used in combination.
[0263] (Embodiment 7) The semiconductor device disclosed in this specification can be applied to various electronic devices (including game machines). The electronic device can be a television device (television or television receiver) (also called "computer monitors"), digital cameras, digital video cameras, digital digital photo frames, mobile phones, portable game consoles, portable information terminals, audio playback devices, These electronic devices include gaming machines (pachinko machines, slot machines, etc.) and game cabinets. A specific example is shown in FIG.
[0264] FIG. 14A shows a table 9000 having a display section. A display unit 9003 is built into the housing 9001, and an image is displayed on the display unit 9003. It is possible to support the housing 9001 with four legs 9002. The housing 9001 also includes a power cord 9005 for supplying power.
[0265] The transistor described in any of the above embodiments can be used in the display portion 9003. This makes it possible to provide high reliability to electronic devices.
[0266] The display unit 9003 has a touch input function. By touching the display button 9004 displayed on the screen with a finger or the like, the screen can be operated or information can be input. It also allows communication with and control of other home appliances, The control device may be a device that controls other home appliances by operating the screen. If the semiconductor device having an image sensor function described in embodiment 6 is used, the display portion 9003 It is possible to provide touch input functionality.
[0267] In addition, the screen of the display unit 9003 can be fixed to the floor by a hinge provided in the housing 9001. It can also be placed vertically and used as a television set. A large-screen television set will take up a lot of free space, but it can be placed on a table. If the display unit is built into the device, the space in the room can be used more effectively.
[0268] FIG. 14B shows a television device 9100. A display unit 9103 is incorporated in a housing 9101, and an image is displayed on the display unit 9103. In this example, the housing 9101 is supported by a stand 9105. The configuration shown is as follows.
[0269] The television device 9100 can be operated using an operation switch provided on the housing 9101 or a separate remote control. This can be done by using a remote control operation device 9110. The channel and volume can be controlled by the 9109, and the display 9103 shows The remote control device 9110 can control the video. A display unit 9107 for displaying information output from the device 9110 may be provided.
[0270] A television device 9100 shown in FIG. 14(B) includes a receiver, a modem, and the like. The television device 9100 can receive general television broadcasts using a receiver. Furthermore, by connecting to a wired or wireless communication network via a modem, Either directional (from sender to receiver) or bidirectional (between sender and receiver, or between receivers, etc.) ) information communication is also possible.
[0271] The transistor described in any of the above embodiments is used in the display portion 9103 and the display portion 9107. This allows the use of a television set and a remote control unit with high reliability. It is possible.
[0272] FIG. 14C shows a computer, which includes a main body 9201, a housing 9202, a display portion 9203, Including a keyboard 9204, an external connection port 9205, a pointing device 9206, etc. nothing.
[0273] The transistor described in any of the above embodiments can be used in the display portion 9203. This makes it possible to provide a high level of reliability to the computer.
[0274] FIG. 15(A) and FIG. 15(B) show a tablet-type terminal that can be folded in two. A) is an open state of the tablet terminal. The tablet terminal includes a housing 9630, a display unit 9631a, and a display unit 9631b. display unit 9631b, a display mode changeover switch 9034, a power switch 9035, a power saving It has a mode changeover switch 9036, a fastener 9033, and an operation switch 9038.
[0275] The transistor described in any of the above embodiments is b), making it possible to create a highly reliable tablet-type terminal.
[0276] A part of the display unit 9631a can be used as a touch panel area 9632a. By touching the operation keys 9638 displayed on the display unit 96, data can be input. In 31a, as an example, half of the area has a display function only, and the other half In the figure, the display area 96 has a touch panel function, but is not limited to this. The entire area of the display unit 931a may have a touch panel function. The entire surface of 631a is made to display keyboard buttons to serve as a touch panel, and the display section 9631b is made to display It can be used as a display screen.
[0277] In addition, in the display unit 9631b, as in the display unit 9631a, The part of the touch panel can be the area 9632b of the touch panel. Touch the area where the mode display switch button 9639 is displayed with your finger or a stylus. A keyboard button can be displayed on the display portion 9631b.
[0278] In addition, the touch panel area 9632a and the touch panel area 9632b are simultaneously You can also use touch input.
[0279] A display mode changeover switch 9034 is used to change the display orientation, such as portrait or landscape. You can switch between black and white and color display. The switch 9036 is a switch that turns on and off when the tablet terminal is in use and is detected by a light sensor built into the tablet terminal. The brightness of the display can be optimized according to the amount of light. In addition to sensors, other detection devices such as gyros, acceleration sensors, etc. that detect tilt may be incorporated.
[0280] FIG. 15A shows an example in which the display area of the display portion 9631b is the same as that of the display portion 9631a. However, there is no particular limitation, and one size may be different from the other size. The quality of the display may also be different. For example, one display panel may provide a higher resolution display than the other. It may also be used as a rule.
[0281] FIG. 15B shows the tablet terminal in a closed state. The tablet terminal includes a housing 9630 and a solar cell 9 15B, the charge / discharge control circuit 96 As an example of the 34, a configuration having a battery 9635 and a DC-DC converter 9636 is described below. This is shown.
[0282] In addition, since the tablet device can be folded in half, the case 9630 can be folded when not in use. Therefore, the display portions 9631a and 9631b can be protected. This allows us to provide tablet devices that are highly durable and reliable for long-term use. .
[0283] In addition, the tablet terminals shown in Fig. 15(A) and Fig. 15(B) are used in various Functions that display important information (still images, videos, text images, etc.), calendars, dates or times A function to display time and other information on the display, and to operate or edit the information displayed on the display by touch input. Touch input function, function to control processing by various software (programs), etc. It is possible to have.
[0284] The solar cell 9633 attached to the surface of the tablet device supplies power to the touch panel. The solar cell 9633 can supply the light to a display unit, a video signal processor, or the like. The battery 9635 can be efficiently charged by providing a light-emitting diode (LED) on one or both sides of the housing 9630. If a lithium-ion battery is used as the battery 9635, This has the advantage of enabling miniaturization.
[0285] The configuration and operation of the charge / discharge control circuit 9634 shown in FIG. A block diagram is shown in (C) and explained. Figure 15(C) shows a solar cell 9633, a battery 9635, DC-DC converter 9636, converter 9637, switches SW1 to SW 3. Shows the display unit 9631, the battery 9635, and the DCDC converter 96 36, a converter 9637, and switches SW1 to SW3 are connected to the charge / discharge control circuit shown in FIG. This corresponds to the control circuit 9634.
[0286] First, an example of operation when power is generated by the solar cell 9633 due to external light will be described. The power generated by the solar cell is converted to a voltage to charge the Battery 9635. The CDC converter 9636 steps up or steps down the voltage. When power is supplied from the solar cell 9633, switch SW1 is turned on and the converter The voltage is increased or decreased by a voltage converter 9637 to a voltage required for the display unit 9631. When you do not want to display anything on the display unit 9631, turn SW1 off and SW2 on to turn on the battery. It is sufficient to configure it to charge the Lee 9635.
[0287] The solar cell 9633 is shown as an example of a power generating means, but is not limited thereto. , and other power generation methods such as piezoelectric elements and thermoelectric conversion elements (Peltier elements) For example, the battery 9635 may be charged. A non-contact power transmission module that transmits and receives power and charges, or a combination of other charging methods This may also be configured.
[0288] The structures, methods, etc. described in this embodiment may be combined as appropriate with the structures, methods, etc. described in other embodiments. They can be used in combination. EXAMPLES
[0289] In this embodiment, in a semiconductor device according to the disclosed invention, a source electrode and The results of cross-sectional observation of the step portion of the drain electrode will be described.
[0290] First, a method for manufacturing a transistor of an example sample will be described.
[0291] First, a gate electrode was formed on a glass substrate. A tungsten film is formed, and a mask is formed on the tungsten film by a photolithography process. A portion of the tungsten film was etched using the mask to form a gate electrode. .
[0292] Next, a gate insulating film was formed on the gate electrode. The silicon nitride film and the silicon oxynitride film having a thickness of 200 nm were laminated. The silicon film was formed in the treatment chamber of a plasma CVD device using 50 sccm of silane and 5,000 sccm of nitrogen. The pressure in the treatment chamber was controlled to 60 Pa, and a high frequency power source of 27.12 MHz was used. The silicon oxynitride film was formed by supplying 150 W of power. Nitrous oxide (3000 sccm) was supplied to the processing chamber of the plasma CVD device, and the pressure in the processing chamber was kept at 4 The pressure was controlled at 0 Pa and 100 W of power was supplied using a 27.12 MHz high frequency power supply. The silicon nitride film and the silicon oxynitride film were grown at a substrate temperature of 350° C. It was formed.
[0293] Next, an oxide semiconductor film was formed so as to overlap with the gate electrode with the gate insulating film interposed therebetween. The IGZO film, which is a CAAC-OS film, is formed on the gate insulating film by sputtering. A mask is formed on the IGZO film by a photolithography process, and the I A part of the IGZO film was etched. Then, the etched IGZO film was subjected to heat treatment. In this embodiment, an IGZO film having a thickness of 35 nm was formed. Ta.
[0294] The IGZO film was made by sputtering a target of In:Ga:Zn=1:1:1 (atomic ratio). ) target and 50sccm argon and 50sccm The oxygen was supplied to the processing chamber of the sputtering device, and the pressure in the processing chamber was controlled to 0.6 Pa. The substrate temperature during the formation of the IGZO film was 1 The temperature was set to 70°C.
[0295] Next, heat treatment was performed to release water, hydrogen, and the like from the oxide semiconductor film. After heat treatment at 450°C for 1 hour in a nitrogen atmosphere, Heat treatment was carried out at 50°C for 1 hour.
[0296] Next, a conductive film is formed over the gate insulating film and the oxide semiconductor film, and forming a mask on the conductive film and etching a part of the conductive film using the mask; A source electrode and a drain electrode were formed. The conductive film is a 400 nm thick aluminum film formed on a 50 nm thick tungsten film. A titanium film having a thickness of 100 nm was formed on the aluminum film.
[0297] Next, the substrate is moved to a reduced pressure processing chamber, heated to 220°C, and then filled with nitrous oxide. The substrate was then moved to a processing chamber in which a 27.12 M H The oxygen plasma was generated by supplying 150 W of radio frequency power using a 1000 Hz radio frequency power source. The semiconductor film was exposed.
[0298] Next, after the plasma treatment, the oxide semiconductor film and the source An insulating film was formed on the gate electrode and the drain electrode. The insulating film was formed under four conditions, A1 to A4. The samples formed under the respective conditions were designated as Samples A1 to A4. In all of the samples A1 to A4, the insulating film had a thickness of 400 nm.
[0299] Condition 1: A silicon oxynitride film was used as the insulating film, and silane and The source gas was nitrous oxide at a flow rate of 4000 sccm, the pressure in the processing chamber was 40 Pa, and the substrate temperature was The temperature was set at 220°C and 150 W of high-frequency power was supplied to the parallel plate electrodes. The film density was measured by XRR and found to be 2.26 g / cm 3 in there were.
[0300] Condition 2 is a silicon oxynitride film used as the insulating film, and silane and The source gas was nitrous oxide at a flow rate of 4000 sccm. The pressure in the treatment chamber was 200 Pa. Plasma CV was performed with a plate temperature of 220°C and 1500 W of high-frequency power supplied to the parallel plate electrodes. The film density was measured by XRR and found to be 2.31 g / cm2. m 3 It was.
[0301] Condition 3 is a silicon nitride film used as an insulating film, silane at a flow rate of 50 sccm, The raw gases were nitrogen at a flow rate of 100 sccm and ammonia at a flow rate of 100 sccm. The pressure was set to 200 Pa, the substrate temperature was set to 220°C, and 1000 W of high frequency power was applied to the parallel plate electrodes. The film was formed by plasma CVD using a 1000-millimeter-wavelength ferroelectric liquid crystal. The film density was measured by XRR. 2.50g / cm 3 It was.
[0302] Condition 4 is a silicon nitride film used as an insulating film, silane at a flow rate of 200 sccm, and The raw gases were nitrogen at a flow rate of 1000 sccm and ammonia at a flow rate of 100 sccm. The pressure was 200 Pa, the substrate temperature was 350°C, and 2000 W of high-frequency power was applied to the parallel plate electrodes. The film was formed by the plasma CVD method using a supply voltage of 100 V. The film density was measured by XRR. The density is set at 2.72 g / cm 3 It was.
[0303] The cross sections of the samples A1 to A4 were observed using a cross-sectional scanning transmission electron microscope (STEM). :Scanning Transmission Electron Microscope The cross-section was observed using a TEM microscope. Figure 16(A) shows a STEM image of sample A1, and Figure 16(B) shows a STEM image of sample A2. FIG. 17(A) shows a STEM image of sample A2, FIG. 17(B) shows a STEM image of sample A3, and FIG. 4 are shown in STEM images.
[0304] As shown in FIG. 16(A), FIG. 16(B) and FIG. 17(A), the source electrode and the drain electrode It was confirmed that a void had occurred in the insulating film covering the dotted line in the figure. On the other hand, in FIG. 17(B), the insulating film covering the source electrode and the drain electrode No voids were observed.
[0305] From this, in the samples A1 to A4, the source electrode and the drain electrode are covered with The insulating film has a film density of 2.26 g / cm 3 More than 2.50g / cm 3 If the value is less than 1, the insulating film It was shown that voids were formed. EXAMPLES
[0306] In this embodiment, the characteristics of a transistor in which a nitride insulating film is formed over an oxide insulating film are evaluated. The measurement results will now be described.
[0307] First, a method for manufacturing a transistor of an example sample will be described.
[0308] As in Example 1, a gate electrode, a gate insulating film, and an oxide semiconductor film were formed on a glass substrate. Then, heat treatment was performed to eliminate water, hydrogen, and the like contained in the oxide semiconductor film. After heat treatment at 450°C for 1 hour in a nitrogen atmosphere, Heat treatment was carried out at 50°C for 1 hour.
[0309] Next, a conductive film is formed over the gate insulating film and the oxide semiconductor film, and forming a mask on the conductive film and etching a part of the conductive film using the mask; Then, a source electrode and a drain electrode were formed.
[0310] Next, the substrate is moved to a reduced pressure processing chamber, heated to 220°C, and then filled with nitrous oxide. The substrate was then moved to a processing chamber in which a 27.12 M H The oxygen plasma was generated by supplying 150 W of radio frequency power using a 1000 Hz radio frequency power source. The semiconductor film was exposed.
[0311] Up to this point, Example 1 can be taken into consideration.
[0312] Next, after the plasma treatment, the oxide semiconductor film and the source An insulating film was formed on the electrode and the drain electrode. The insulating film was a nitride insulating film on an oxide insulating film. The oxide insulating film is a first oxide nitride silicon oxide film having a thickness of 50 nm. A silicon film and a second silicon oxynitride film having a thickness of 400 nm were laminated to form the silicon oxide film.
[0313] The first silicon oxynitride film was prepared by using silane at a flow rate of 30 sccm and SiO at a flow rate of 4000 s. The source gas was nitrous oxide (NO2) of ccm, the pressure in the processing chamber was 40 Pa, and the substrate temperature was 220°C. The film was formed by plasma CVD in which 150 W of high frequency power was supplied to parallel plate electrodes.
[0314] The second silicon oxynitride film was formed by mixing silane at a flow rate of 160 sccm and SiO2 at a flow rate of 4000 sccm. The source gas was dinitrogen monoxide at a flow rate of 100 sccm. The pressure in the processing chamber was set to 200 Pa, and the substrate temperature was set to 220 ℃, and a high-frequency power of 1500 W was supplied to parallel plate electrodes. The conditions were such that the mixture contained more oxygen than would be required for the stoichiometric composition, and the mixture was heated to As a result, a silicon oxynitride film from which part of oxygen is released can be formed.
[0315] Next, heat treatment was performed to remove water, hydrogen, and the like from the oxide insulating film. The specimen was then subjected to a heat treatment at 350° C. for 1 hour in an oxygen atmosphere.
[0316] Next, a nitride insulating film was formed on the oxide insulating film. The silicon nitride film was formed using silane at a flow rate of 200 sccm and fluorine at a flow rate of 100 sccm. Nitrogen at 2000sccm and ammonia at 100sccm were used as raw gases. The pressure was 100 Pa, the substrate temperature was 350°C, and 2000 W of high-frequency power was applied to the parallel plate electrodes. The film was formed by plasma CVD using a supply voltage of 100 V.
[0317] Next, a part of the insulating film (oxide insulating film and nitride insulating film) is etched to form a source Openings were formed to expose portions of the positive and drain electrodes.
[0318] Next, an interlayer insulating film was formed on the insulating film (nitride insulating film). After coating on the insulating film, exposure and development are performed to form a part of the source electrode or drain electrode. An interlayer insulating film having an opening exposing the insulating film was formed. After that, a heat treatment was performed. The heat treatment was performed at a temperature of 25 The temperature was set to 0° C. and the reaction was carried out in a nitrogen atmosphere for 1 hour.
[0319] Next, a conductive film was formed to connect to a part of the source electrode or the drain electrode. A 100 nm thick ITO film containing silicon oxide was formed by sputtering.
[0320] Through the above steps, a transistor of the example sample was fabricated.
[0321] As a comparative example, the insulating film of the example sample was an oxide insulating film only, and no nitride insulating film was formed. A comparative sample transistor that was not subjected to the treatment was fabricated.
[0322] In the above-mentioned example samples and comparative sample samples, cross sections of the samples were observed using a cross-sectional scanning transmission electron microscope. (STEM:Scanning Transmission Electron Mic The cross-section was observed by STEM. Figure 18(A) shows a STEM image of the sample. 8(B) shows a STEM image of the comparative sample.
[0323] As shown in FIG. 18(A) and FIG. 18(B), a layer covering the source electrode and the drain electrode is The first silicon oxynitride film and the second silicon oxynitride film are surrounded by dotted lines in the figure. It was confirmed that a void was generated in the second portion as shown in FIG. No voids are formed in the silicon nitride film on the silicon oxynitride film. It was thus confirmed that the voids were blocked.
[0324] Next, the Vg-Id characteristics of the transistors of the above example sample and comparative sample were measured. .
[0325] As an accelerated life test for evaluating humidity resistance, a pressure cooker test (PCT) is used. In this example, the PCT was performed at a temperature of 130°C and humidity of 100°C. The embodiment sample and the comparative sample were held for 1 hour under the conditions of 85% humidity and 0.23 MPa pressure. .
[0326] In the embodiment sample and the comparative sample, GBT (Gate Bias Temperature In this embodiment, a GBT stress test was performed in a dark room. Under the conditions of Vg=-30V, Vd=0V, Vs=0V, stress temperature 60℃, no light irradiation, The stress application time was 1 hour. The actual measurement values were a channel length (L) of 6 μm and The width (W) was 50 μm, and the thickness (Tox) of the oxide film (gate insulating film) was 280 nm.
[0327] FIG. 19(A) shows the results of the GBT stress test of the embodiment sample, and FIG. 19(B) shows the results of the comparative example sample. The results of the GBT stress test of the sample are shown. The dotted line in the figure shows the measurement results before PCT. As a result, the solid line in the figure shows the measurement results after PCT. The horizontal axis shows the measurement results when the drain voltage (Vd: [V]) is 1 V and 10 V. The vertical axis indicates the gate voltage (Vg: [V]), and the vertical axis indicates the drain current (Id: [A]). "Drain voltage (Vd: [V])" is the potential difference between the drain and source with respect to the source. The gate voltage (Vg: [V]) is the voltage between the gate and source with respect to the source. It is the rank difference.
[0328] As shown in FIG. 19(A), the transistor of the example sample did not change significantly before and after PCT. On the other hand, as shown in FIG. 19B, the transistor of the comparative sample was It is clear that the threshold value changes significantly around T, and that it shifts to the negative side after PCT. It was acknowledged.
[0329] The difference between the embodiment sample and the comparative sample is that a silicon nitride film is formed on the second silicon oxynitride film. Therefore, even after PCT, the characteristics do not change due to the effect of the silicon nitride film. It was found that it was possible to suppress the amount of movement.
[0330] Therefore, the gaps in the silicon oxynitride film are blocked by the silicon nitride film. In addition, the present invention provides a semiconductor device using an oxide semiconductor with stable electrical characteristics and high reliability. It can be realized. EXAMPLES
[0331] In this embodiment, the difference in the temperature at which a nitride insulating film is formed on an oxide insulating film is The measurement results of the characteristics will now be described.
[0332] First, a method for manufacturing a transistor of an example sample will be described.
[0333] The example sample is the same as the example sample in Example 2 except that the deposition temperature of the silicon nitride film is set to 220° C. The sample B1 is the same as the sample in Example 2 (the silicon nitride film was formed at a temperature of 350 °C) is designated as sample B2.
[0334] For the silicon nitride film of sample B1, silane with a flow rate of 50 sccm and a flow rate of 5000 sccm were used. The source gases were nitrogen at 100 m and ammonia at 100 sccm. The pressure in the treatment chamber was set to 200 The plate temperature was set at 220°C, and 1000W of high frequency power was supplied to the parallel plate electrodes. The silicon nitride film of sample B2 was formed by the Zuma CVD method. The sample was the same as sample B1, except that the substrate temperature of the silicon film was 350°C.
[0335] Next, the Vg-Id characteristics of the transistors of Samples B1 and B2 were measured.
[0336] A pressure cooker test (PCT) was conducted as an accelerated life test for evaluating humidity resistance. In this example, the PCT was performed under the conditions of a temperature of 130°C, humidity of 85%, and pressure of 0.20 MPa. Samples B1 and B2 were held for 1 hour.
[0337] A GBT stress test was performed on sample B1 and sample B2. For the T-stress test, Vg=-30V~30V, Vd=0V, Vs= The test was performed at 0V, at a stress temperature of 60°C, without light irradiation, and for a stress application time of 1 hour. The values are channel length (L) 6 μm, channel width (W) 50 μm, oxide film (gate insulating film) The film thickness (Tox) was 280 nm.
[0338] FIG. 20(A1) shows the results of the GBT stress test of sample B1 before PCT, and FIG. 20(A2) shows the results of the GBT stress test of sample B1 before PCT. ) shows the results of the GBT stress test after PCT for sample B1. Also, FIG. 20(B1) shows 20(B2) shows the results of the GBT stress test of sample B2 before PCT. The results of the GBT stress test after CT are shown in Fig. 20(A1), Fig. 20(A2), Fig. In Fig. 20(B1) and 20(B2), the drain voltage (Vd: [V]) is 1V. The horizontal axis shows the gate voltage (Vg: [V]) and the vertical axis shows the measurement results at 10V and 10V. are the drain current (Id: [A]) and the field effect mobility (μFE: [cm 2 / Vs]) 20(A3) and 20(B3) show the PCT results of samples B1 and B2. The amount of change in threshold voltage (ΔVth) before and after the shift value (ΔShift) is shown.
[0339] In this specification, the threshold voltage (Vth) is the gate voltage (Vg: [V]). on the horizontal axis, and the square root of the drain current (Id (1 / 2) :[A]) plotted on the vertical axis The line with the maximum slope Id (1 / 2) When the tangent of is extrapolated, the tangent and the Vg axis ( That is, Id (1 / 2) The gate voltage is defined as the intersection point between the gate In this case, the drain voltage Vd is set to 10 V and the threshold voltage is calculated.
[0340] In this specification, the shift value (Shift) is the gate voltage (Vg: [V]). On a curve plotting the logarithm of the drain current (Id: [A]) on the vertical axis, When the tangent of the slope Id is extrapolated, the straight line Id = 1.0 x 10 -12 Intersection with [A] In this specification, the drain voltage Vd is set to 10 V. , and calculate the shift value.
[0341] As shown in FIG. 20(A3) and FIG. 20(B3), the trans- formation of samples B1 and B2 The transistors showed slight changes in threshold voltage and shift value before and after PCT, indicating degradation. It was also confirmed that the trajectory of sample B2 (the silicon nitride film was formed at a temperature of 350°C) The transistor of sample B1 (the silicon nitride film deposition temperature is 220°C) is It was confirmed that the changes in the threshold voltage and shift value were small. EXAMPLES
[0342] In this embodiment, the RBS (Rutherford backscattering) of the silicon nitride film, which is a part of the insulating film, Backscattering Spectrometry (BS) analysis results and secondary ion Secondary Ion Mass Spectrometer (SIMS) The evaluation results using the ry method will be explained below.
[0343] First, the analyzed samples will be described.
[0344] The sample is a silicon wafer 11 on which a silicon nitride film 12 is formed by plasma CVD. The silicon nitride film 12 was fabricated under two conditions, condition C1 and condition C2. The samples formed under the respective conditions were designated as Sample C1 and Sample C2.
[0345] Condition C1 is a temperature for holding the silicon wafer 11 at 220° C. and a flow rate of 50 sccm. Silane, nitrogen at a flow rate of 5000 sccm, and ammonia at a flow rate of 100 sccm were used as raw gases. The pressure in the treatment chamber was set to 200 Pa, and 1000 W of high frequency power was supplied to the parallel plate electrodes. A silicon nitride film 12 having a thickness of 100 nm was formed by plasma CVD.
[0346] In condition C2, the temperature at which the silicon wafer 11 is held is 350° C. and the flow rate is 200 sccm. The raw gas was silane at a flow rate of 2000 sccm, nitrogen at a flow rate of 100 sccm, and ammonia at a flow rate of 100 sccm. The pressure in the treatment chamber was set to 200 Pa, and 2000 W of high-frequency power was supplied to the parallel plate electrodes. A silicon nitride film 12 having a thickness of 300 nm was formed by plasma CVD.
[0347] Samples C1 and C2 were then evaluated. The RBS results are shown in Table 1.
[0348] [Table 1]
[0349] Sample C1 contains 26.5 atomic % silicon, 45.5 atomic % nitrogen, It was confirmed that the hydrogen content was 28.1 atomic %. 40.0 atomic % of carbon, 49.2 atomic % of nitrogen, and 10.8 atomic % of hydrogen. It was confirmed that sample C2 contained ic% of Zn. Therefore, compared with sample C1, sample C2 contained ic% of Zn. It was confirmed that the proportion of hydrogen in the composition was reduced.
[0350] Next, the results of the SIMS analysis are shown in FIG.
[0351] FIG. 22(A) shows the concentration profiles of hydrogen, oxygen, fluorine, and carbon by SIMS for sample C1. The concentration of hydrogen, oxygen, fluorine and carbon by SIMS of sample C2 is shown in FIG. The degree profile is shown.
[0352] Moreover, details of the SIMS analysis results of FIG. 22 are shown in Table 2.
[0353] [Table 2]
[0354] Sample C1 contains 2.8×10 hydrogen. 22 atoms / cm 3 , oxygen is 1.0×10 19 atoms / cm 3 , fluorine is 2.3 × 10 19 atoms / cm 3 , carbon is 5.5 x 1 0 18 atoms / cm 3 It was confirmed that sample C2 contained 1. 6×10 22 atoms / cm 3 , oxygen is 6.8 × 10 17 atoms / cm 3 , Fluorine is 7.4×10 18 atoms / cm 3 , carbon is 7.4 × 1017 atoms / cm 3 Contains Therefore, as with the RBS results, sample C2 was found to have the same It was confirmed that the proportion of hydrogen in the composition was reduced compared to that of the sample. C2 has a lower concentration of impurities such as hydrogen, oxygen, fluorine, and carbon than sample C1. was confirmed. EXAMPLES
[0355] In this example, we verified whether the voids in the insulating film serve as paths for the infiltration of water, hydrogen, etc. The verification was carried out using SIMS.
[0356] First, the sample will be described with reference to FIG. 23. The sample is an oxide semiconductor shown in FIG. Sample D1 in which a gap is generated due to an electrode on the semiconductor film and sample D2 in which a gap is generated due to an electrode on the semiconductor film are shown in FIG. We prepared two types of sample: sample D1, which has no electrodes and no voids.
[0357] A gate insulating film 22 and an oxide semiconductor film 23 are formed on a glass substrate 21, and a heat treatment is performed. The oxidation was performed in a nitrogen atmosphere to remove water, hydrogen, and the like from the oxide semiconductor film 23. After heat treatment at 450℃ for 1 hour, the specimen was cooled in a nitrogen and oxygen atmosphere at 450℃ for 1 hour. The heat treatment was carried out.
[0358] Next, a conductive film is formed on the gate insulating film 22 and the oxide semiconductor film 23, and then photolithography is performed. A mask is formed on the conductive film by a lithography process, and a part of the conductive film is etched using the mask. Then, the electrode 24 was formed.
[0359] Next, the substrate is moved to a reduced pressure processing chamber, heated to 220°C, and then filled with nitrous oxide. The substrate was then moved to a processing chamber in which a 27.12 M H The oxygen plasma was generated by supplying 150 W of radio frequency power using a 1000 Hz radio frequency power source. The semiconductor film was exposed.
[0360] Up to this point, Example 1 can be taken into consideration.
[0361] Next, after the plasma treatment, the oxide semiconductor film 23 and the An insulating film 27 was formed on the electrodes 24. The insulating film 27 was a nitride insulating film formed on the oxide insulating film 25. The oxide insulating film 25 is a laminated structure in which a first oxide film 26 is formed. A silicon oxynitride film 25a and a second silicon oxynitride film 25b having a thickness of 400 nm are laminated. And it was formed.
[0362] The first silicon oxynitride film 25a is made of silane at a flow rate of 30 sccm and SiO2 at a flow rate of 40 The source gas was dinitrogen monoxide at 0.00 sccm, the pressure in the processing chamber was 40 Pa, and the substrate temperature was 22 Formed by plasma CVD method at 0℃ and supplying 150W of high frequency power to parallel plate electrodes. did.
[0363] The second silicon oxynitride film 25b is made of silane at a flow rate of 160 sccm and SiO at a flow rate of 4 The source gas was nitrous oxide at 0.000 sccm, the pressure in the processing chamber was 200 Pa, and the substrate temperature was The temperature was set at 220°C and 1500 W of high-frequency power was supplied to parallel plate electrodes by the plasma CVD method. The conditions were such that the mixture contained more oxygen than would be required for the stoichiometric composition. A silicon oxynitride film from which part of oxygen is released by heat can be formed.
[0364] Next, heat treatment was performed to remove water, hydrogen, and the like from the oxide insulating film. The specimen was then subjected to a heat treatment at 350° C. for 1 hour in an oxygen atmosphere.
[0365] Next, a nitride insulating film 26 was formed on the oxide insulating film 25. The nitride insulating film 26 had a thickness of A silicon nitride film of 50 nm was formed. The run was performed with nitrogen at a flow rate of 5000 sccm and ammonia at a flow rate of 100 sccm as the source gas. The pressure in the processing chamber was set to 200 Pa, the substrate temperature to 220°C, and the average high-frequency power was set to 2000 W. The film was formed by plasma CVD using a layer of silicon dioxide supplied to a row of flat electrodes.
[0366] In this manner, sample D1 was prepared. Sample D2 was prepared without forming electrodes. It was produced (see Figure 23).
[0367] Samples D1 and D2 were subjected to a pressure cooker test (PCT). is PCT, temperature 130℃, humidity 85% (volume ratio of water vapor in the gas is H2O (water):D2O (heavy water) = 4:1, 2.0 atmospheres (0.20 MPa), and sample D2 were held for 15 hours.
[0368] In this embodiment, the "D atom" expressed in heavy water is a hydrogen atom with a mass number of 2. child( 2 H).
[0369] SIMS analysis was performed using SSDP (Substrate Side Depth Profile) Using SIMS (backside SIMS measurement), the specimens D1 and D2 after the PCT test were The concentrations of H atoms and D atoms in each sample were measured for sample D1 and sample D2.
[0370] FIG. 24(A) shows the concentration profiles of H and D atoms measured by SIMS after the PCT test of sample D1. The profile of H and D atoms measured by SIMS after the PCT test of sample D2 is shown in FIG. The concentration profiles of atoms are shown in Fig. 24(A) and (B). The profile shows that the abundance of D atoms is 0.015%. This is the concentration profile of D atoms present in nature calculated from the profile of H atoms. Therefore, the amount of D atoms mixed into the sample by the PCT test is different from the actual measured D atom concentration and the natural concentration. This is the difference from the abundance value of D atom concentration.
[0371] When Sample D1 and Sample D2 are compared, as shown in FIG. 24A, the electrode formed on the oxide semiconductor film The concentration profile of D atoms in the oxide semiconductor film is affected by the presence of a pole and the generation of voids. The concentration of D atoms in the oxide semiconductor film was increased to a high level. Therefore, sample D1 has poor barrier properties against water (H2O, D2O) from the outside. It was confirmed that... [Explanation of symbols]
[0372] 11 Silicon wafer 12 Silicon nitride film 21 Glass substrate 22 Gate insulating film 23 Oxide semiconductor film 24 electrodes 25 Oxide insulating film 25a First silicon oxynitride film 25b Second silicon oxynitride film 26 Nitride insulating film 27 Insulating Film 31 Oxide semiconductor film 32 Oxide insulating film 32a Oxide insulating film 32b Oxide insulating film 400 Substrates 401 Undercoat insulating film 402 Gate electrode 404 Gate insulating film 404a Gate insulating film 404b Gate insulating film 406 Semiconductor Film 407a Conductive film 407b Conductive film 407c conductive film 408a Source electrode 408b Drain electrode 410 Oxide insulating film 410a Oxide insulating film 410b Oxide insulating film 410c oxide insulating film 410d oxide insulating film 410e Oxide insulating film 411 Nitride insulating film 412 Insulating film 413 Cavity 414 Interlayer insulating film 416 Electrode 450 Transistors 510 Oxide insulating film 510a Oxide insulating film 510b Oxide insulating film 511 Nitride insulating film 512 Gate insulating film 530 Insulating film 550 Transistor 552 Gate electrode 560 Transistor 570 Transistor 580 Transistor 601 Substrate 602 Photodiode 606a Semiconductor film 606b Semiconductor film 606c Semiconductor film 608 Adhesive layer 613 Substrate 632 Insulating film 633 Planarization film 634 Planarization film 640 Transistor 641a electrode 641b Electrode 642 Electrode 643 Conductive Film 645 Conductive Film 656 Transistor 658 Photodiode reset signal line 659 Gate signal line 671 Photo sensor output signal line 672 Photosensor reference signal line 901 Board 902 Pixel section 903 Signal line driver circuit 904 Scanning line driver circuit 905 Sealing material 906 Substrate 908 Liquid crystal layer 910 Transistor 911 Transistor 913 Liquid crystal element 915 Connection terminal electrode 915a Connection terminal electrode 915b Connection terminal electrode 916 Terminal electrode 917 Conductive Film 918 FPC 918a FPC 918b FPC 919 Anisotropic conductive agent 921 Interlayer insulating film 922 Gate insulating film 923 Insulating Film 924 Insulating film 925 Sealing material 930 electrode 931 Electrode 932 Insulating film 933 Insulating film 935 Spacer 936 Sealing material 941 Electrode 943 Liquid crystal element 944 Insulating film 950 Silicon nitride film 951 Light-emitting layer 955 Connection terminal electrode 960 Bulkhead 963 Light emitting element 964 Filling material 971 Source Electrode 973 Drain electrode 975 Common potential line 977 Common electrode 985 Common potential line 987 Common electrode 9000 Table 9001 Case 9002 Legs 9003 Display section 9004 Display button 9005 Power Cord 9033 Fastener 9034 Switch 9035 Power Switch 9036 Switch 9038 Operation switch 9100 Television equipment 9101 Case 9103 Display section 9105 Stand 9107 Display section 9109 Operation key 9110 Remote control device 9201 Main unit 9202 Case 9203 Display section 9204 Keyboard 9205 External connection port 9206 Pointing Device 9630 Case 9631 Display section 9631a Display section 9631b Display section 9632a area 9632b area 9633 Solar Cells 9634 Charge / discharge control circuit 9635 Battery 9636 DC-DC Converter 9637 Converter 9638 Operation key 9639 Button
Claims
[Claim 1] a semiconductor film at least partially overlapping with a gate electrode via a gate insulating film; a source electrode and a drain electrode having an area in contact with a part of the upper surface of the semiconductor film; a first insulating film covering the source electrode, the drain electrode and the semiconductor film, having a void in a step region formed by the source electrode and the drain electrode on the semiconductor film, and containing silicon oxide as a component; a second insulating film containing silicon nitride as a component and provided in contact with the first insulating film so as to fill the voids in the first insulating film.
Citation Information
Patent Citations
Formation of sio2 film of lower trailing shape
JP1999233510A
Liquid crystal display
JP2007183633A
Semiconductor device and manufacturing method thereof
JP2010056546A
Method for manufacturing active element substrate, active element substrate, and active type display device
JP2010191283A
Semiconductor device and method for manufacturing the same
JP2011054951A