Method and device for manufacturing in-mold coated molded products
The method addresses air pocket issues in in-mold coating by using an air bleed gap to ensure seamless coating application, reducing manufacturing time and costs while enhancing the appearance and integrity of molded products.
Patent Information
- Application Number
- JP2023043667
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-19
- Publication Date
- 2024-10-02
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing in-mold coating methods face challenges such as air pocket formation near convex portions, leading to poor appearance and increased manufacturing costs due to the need for laser processing and thin film coatings, which are time-consuming and costly.
A method and apparatus for in-mold coating that forms a convex portion on the molding substrate with a height smaller than the coating gap, incorporating an air bleed gap to prevent air pocket formation by sweeping away air through this gap, ensuring seamless coating application.
Prevents air pocket formation, enhances coating integrity and peel strength, reduces manufacturing time and costs by eliminating the need for laser processing, and improves the overall appearance of the coated molded product.
Smart Images

Figure 2024133431000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and apparatus for manufacturing an in-mold coated molded product in which a coating gap is formed between the outer surface of a substrate sandwiched between a pair of molds and the inner surface of the molds, and a liquid coating agent is injected into the coating gap to adhere to the outer surface of the substrate. [Background technology]
[0002] As environmental issues have become a major concern in recent years, in-mold coating (IMC) has been attracting attention as an alternative painting technique that does not use organic solvents and is highly effective in reducing CO2 emissions. IMC is a technique in which a functional liquid coating agent (e.g., paint) is injected into the gap between the outer surface of the molded substrate and the inner surface of the mold using the mold used for molding, and a coating (e.g., paint) is formed on the outer surface of the molded substrate by heating (see Patent Document 1).
[0003] The features of IMC include: (1) it is environmentally and human-friendly because it does not use the organic solvents used in general spray painting; (2) it does not require equipment for the painting process (spraying, oven heat treatment); and (3) because the paint is not diluted with organic solvents, the rate at which the material (paint) before application is formed as a coating on the outer surface of the molded substrate (coating efficiency) is very high, resulting in extremely little waste.
[0004] The purpose of painting a resin molded product is to give the original outer surface of the material a vivid color, gloss, or metallic look that cannot be obtained by kneading, or to hide defects in appearance that occur during molding, thereby improving the design and giving the product a luxurious feel. Furthermore, there are many products in our daily lives that have functions that improve visibility and take operability into consideration. An example of this type of product is a computer keyboard with letters and symbols printed on the keys.
[0005] When printing or painting symbols or letters on the surface of computer keyboard keys, screen printing using silk mesh is usually used if the surface to be printed or painted is flat, and pad printing using elastic silicone rubber is used if the surface is curved. However, both of these methods use paint diluted with organic solvents and require oven treatment, which has a large impact on the environment.
[0006] On the other hand, as a highly functional switch part used in environments with little lighting such as indoors, in a car, or at night, for example, the one shown in FIG. 5 is known. FIG. 5(a) is a perspective view of the switch part, FIG. 5(b) is a cross-sectional view taken along line bb in FIG. 5(a), and FIG. 5(c) is a cross-sectional view taken along line cc in FIG. 5(a). This switch part has a generally black surface with a white pattern (mountain-shaped pattern) partially displayed, and a light-transmitting material is used for the white pattern (mountain-shaped pattern). In devices used in dark rooms, cars, or at night with little lighting, when the main power is turned on, a light (not shown) on the back of the switch part turns on, and the white area (the white pattern (mountain-shaped pattern) area) emits light and can be recognized, so that the switch part can be used even in dark environments.
[0007] This type of switch part is usually manufactured by forming a molded substrate from a transparent or translucent resin, first applying a black or other opaque paint to the entire outer surface of the molded substrate to form a coating, and then removing the coating only from the design area, which is the mountain-shaped pattern. A known method for partially removing this coating is the laser irradiation method, which uses a laser beam to vaporize and remove the black coating only from the design area (the mountain-shaped pattern) (see Patent Documents 2 and 3).
[0008] However, because the laser irradiation method is a high-heat treatment, in order to ensure the clearness of the boundary between the design area (white part of the mountain-shaped pattern) of the substrate exposed by removing the coating film by irradiation with a laser beam and the painted coating film part (black) in Fig. 5(a) while minimizing the thermal impact on the substrate itself, the spot diameter of the laser beam must be small, and there is a restriction that the irradiation energy cannot be large. Due to this restriction, in order to increase productivity, the coating film formed on the outer surface of the substrate must be as thin as possible (for example, 50 μm or less), and detailed control of the coating film thickness is required, which leads to increased costs.
[0009] In addition, the initial cost of installing laser processing equipment is high, and since processing is done by drawing a small spot in one stroke, it takes an extremely long time to process a large area, which is a factor that significantly increases manufacturing costs. Also, the laser irradiation method requires two processes: a process of painting the outer surface of the molding substrate and a process of removing part of the painted coating with a laser beam, so the number of steps increases and manufacturing time is required, making it inevitable that costs will increase. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Patent No. 3617807 [Patent Document 2] JP 2002-146558 A [Patent Document 3] JP 2005-7403 A Summary of the Invention [Problem to be solved by the invention]
[0011] Therefore, the present inventors have proposed a method for producing an in-mold coated molded product by mounting a molding substrate 2 in a first mold 1 as shown in Figs. 1(a) and 1(b), abutting the first mold 1 with the mounting substrate 2 mounted against a second mold 3 so as to cover the molding substrate 2 as shown in Figs. 2(a) and 2(b), forming a coating gap G1 (e.g., about 50 to 100 µm) between the inner surface of the second mold 3 and the outer surface of the molding substrate 2, and injecting a liquid coating agent (e.g., paint T) into the coating gap G1 to adhere to the outer surface of the molding substrate 2. In this method, as shown in Figs. 1(a) and 1(b), convex portions 4J corresponding to a desired pattern to be applied to the outer surface of the molding substrate 2 are formed on the outer surface of the molding substrate 2 as shown in Figs. 2(b), The molding substrate 2 is formed to a height H corresponding to the coating gap G1 shown in FIG. 1, and the first mold 1 with the molding substrate 2 attached is abutted against the second mold 3 so as to cover the molding substrate 2, so that the convex portion 4J formed on the outer surface of the molding substrate 2 comes into contact with the inner surface of the second mold 3. In this state, a liquid coating agent is injected into the coating gap G1, and the liquid coating agent (e.g., paint T) is adhered to the parts of the outer surface of the molding substrate 2 other than the convex portion 4J, so that the outer surface of the molding substrate 2 is coated with the liquid coating agent (e.g., paint T) except for the convex portion 4J (part of the desired pattern). A manufacturing method for an in-mold coated molded product has been developed and a patent application has been filed (Patent Application No. 2022-152771).
[0012] According to this manufacturing method for in-mold coated molded products, the molding substrate 2 on which a convex portion 4J (a portion of the desired pattern) having a height corresponding to the coating gap G1 as shown in FIG. 1(b) is formed is attached to the first mold 1 as shown in FIG. 1(a), and the first mold 1 is butted against the second mold 3 as shown in FIG. 2(b) to bring the top surface of the convex portion 4J of the molding substrate 2 into contact with the inner surface of the second mold 3. In this state, liquid coating agent is injected into the coating gap G1, so that the liquid coating agent is adhered to the outer surface of the molding substrate 2 except for the convex portion 4J (a portion of the desired pattern). Therefore, the process of coating the outer surface of the molding substrate 2 and the process of forming the desired pattern on the outer surface of the molding substrate 2 are carried out simultaneously, which shortens the manufacturing time and promotes cost reduction.
[0013] Moreover, unlike the conventional method, after coating the entire outer surface of the molding substrate 2, the coating in the desired pattern is not removed with a laser beam, so there is no initial cost for introducing laser processing equipment. In addition, when removing the coating in the desired pattern with a laser beam, it is necessary to make the coating as thin as possible (for example, 50 μm or less) to increase productivity, but in the above-mentioned method for producing an in-mold coated molded product, the coating is not removed with a laser beam, so there is no need to make the coating thin, and there is no cost for keeping the coating thin. Furthermore, since the above-mentioned production method is effective even if the coating is made to be somewhat thick, there is a possibility that the durability of the coating during long-term use will be improved by making the coating thicker depending on the usage environment.
[0014] In the manufacturing method of the above-mentioned in-mold coated molded product, as shown in FIG. 2(b), the first mold 1 with the molding substrate 2 attached thereto is abutted against the second mold 3, and a liquid coating agent (e.g., paint T) is injected into the injection port 5 formed on one side of the second mold 3. As the liquid coating agent passes through the coating gap G1 and is discharged from the discharge port 8 formed on the other side of the second mold 3, a coating film (paint film) is formed on the outer surface of the molding substrate 2, except for the protruding portion 4J, by the liquid coating agent.
[0015] However, in FIG. 2(b), the liquid coating agent (e.g., paint T) flowing from the injection port 5 through the coating gap G1 to the discharge port 8 flows while displacing the air in the coating gap G1. Depending on conditions such as the shape of the convex portion 4J, the viscosity of the liquid coating agent (hereinafter also referred to as paint T), the injection time, and the curing time, the displaced air may accumulate near the convex portion 4J without being discharged from the discharge port 8, forming air bubbles (air pockets).
[0016] For example, let us consider the flow of paint T and air in the coating gap G1 when the protrusion 4J has a blocking portion 12 that is open on the upstream side in the flow direction of the liquid coating agent (paint T) flowing through the coating gap G1, as shown in part a1 of Fig. 2(a) and its cross section part a11 of Fig. 2(b). An enlarged view of part a11 is shown in Fig. 3(a11), and an enlarged view of part a1 is shown in Fig. 3(a1).
[0017] As shown in Figures 3(a11) and 3(a1), when paint T approaches the damming portion 12 of the convex portion 4J, the air inside the damming portion 12 cannot escape, so the pressure increases, and the paint T in front of the damming portion 12 is pushed by the pressure, causing the tip Ta of the flow to become concave. Thereafter, as the flow of paint T progresses, as shown in Figures 3(a12) and 3(a2), the air inside the damming section 12 is left behind as it has no way to escape, and as shown in Figures 3(a13) and 3(a3), the air inside the damming section 12 is compressed by the pressure of the flow of paint T, and the paint T, which has detoured around the outside of the damming section 12, wraps around to the back of the damming section 12, and finally, as shown in Figures 3(a14) and 3(a4), the air inside the damming section 12 is further compressed by the pressure of the flow of paint T, but the air does not escape and air bubbles (air pockets A) may form.
[0018] In addition, as shown in part b1 of Fig. 2(a), when the convex portion 4J has a rear roll-in portion 13 that is open on the downstream side in the flow direction of the liquid coating agent (paint T) flowing through the coating gap G1, as shown in Fig. 4(b1), the paint T flows and hits the front part of the rear roll-in portion 13 of the convex portion 4J, and then as shown in Fig. 4(b2), the paint T is rolled inward of the rear roll-in portion 13 at the left and right rear ends of the rear roll-in portion 13 as shown in Fig. 4(b2), and as shown in Fig. 4(b3), the roll-in progresses from the left and right rear ends to the inside of the rear roll-in portion 13, and finally, as shown in Fig. 4(b4), the left and right rolls are connected to form an air pocket A inside the rear roll-in portion 13. Once the air pocket A is formed, the periphery is surrounded by the paint T and the convex portion 4J, so that air does not escape from the air pocket A.
[0019] In addition, as shown in part c1 of FIG. 2(a), in the case where the protrusion 4J has a side roll-in portion 14 that is open on the side that intersects with the flow direction of the liquid coating agent (paint T) flowing through the coating gap G1 (for example, the side that is perpendicular to the flow direction), as shown in FIG. 4(c1), the paint T flows and hits the tip of the upstream part of the side roll-in portion 14 of the protrusion 4J, and then, as shown in FIG. 4(c2), the flow is divided into the outer surface and the inner surface of the side roll-in portion 14, and the flow on the inner surface side penetrates into the side roll-in portion 14 by being rolled inward, as shown in FIG. 4(c3), the flow that penetrated into the side roll-in portion 14 flows and hits the inner surface of the downstream part of the side roll-in portion 14, and air is trapped inside the side roll-in portion 14, and the flow on the outer surface and the flow on the inner surface of the side roll-in portion 14 merge, and finally, as shown in FIG. 4(c4), an air pocket A may be formed inside the side roll-in portion 14.
[0020] In this way, in the process of injecting a liquid coating agent (paint T) into the injection port 5 from the state of Figure 2(b) to coat the outer surface of the molding substrate 2, if the above-mentioned air pocket A occurs, when the first mold 1 is separated from the second mold 3 and the coated molding substrate (in-mold coated molded product 10J) is removed from the first mold 1, the areas of the air pocket A formed in contact with each convex portion 4J in the removed in-mold coated molded product 10J will become paint missing areas K, resulting in a poor appearance, as shown in Figure 5(a), which is an oblique view of the in-mold coated molded product 10J, Figure 5(b), which is a sectional view taken along line bb in Figure 5(a), and Figure 5(c), which is a sectional view taken along line cc in Figure 5(a). In addition, as shown in Figure 2(b), the top surface of the convex portion 4J is abutted against the inner surface of the second mold 3 and is masked therefrom. Therefore, as shown in Figures 5(b) and 5(c), no coating film is formed on the top surface of the convex portion 4J. It is therefore possible that with continued use, the coating film 11J will peel off from the boundary between the top surface of the convex portion 4J and the coating film 11J or from the above-mentioned paint missing portion K.
[0021] Next, as shown in Figures 6(a), 6(b), and 6(c), the flow of the paint T and air in the coating gap G1 will be considered for the case where the convex portion 4J formed on the outer surface of the molding substrate 2 has an enclosed portion 16 that is enclosed on the inside by the flow of the liquid coating agent (paint T) flowing through the coating gap G1. Examples of the enclosed portion 16 include the letters "A" and "O" as well as ring-shaped patterns. An enlarged view of a portion a21 in Figure 6(b) is shown in Figure 7(a21), and a cross-sectional view of line II in Figure 7(a21) is shown in Figure 7(a1). The time course of the coating process for Figure 7(a21) is shown in Figures 7(a22), 7(a23), and 7(a24), and the time course of the coating process for Figure 7(a1) is shown in Figures 7(a2), 7(a3), and 7(a4). As shown in each figure, the top surface of the protrusion 4J having the surrounding portion 16 is abutted against the inner surface of the second mold 3, so the liquid coating agent (paint T) flowing through the coating gap G1 is not guided to the inside of the surrounding portion 16, and the air inside the surrounding portion 16 is not discharged. Therefore, an air pocket A is finally formed inside the surrounding portion 16 in Figures 7(a24) and 7(a4).
[0022] As shown in Fig. 7(a24) and Fig. 7(a4), after the coating step is completed, the first mold 1 is separated from the second mold 3 to remove the coated molded substrate 2 (in-mold coated molded product 10J). Fig. 8(a) shows a perspective view of the removed in-mold coated molded product 10J, and Fig. 8(b) shows a cross-sectional view along line bb in Fig. 8(a). As shown in the figures, the removed in-mold coated molded product 10J has a missing part K of paint T in the inner part of the enclosed part 16 of the protruding part 4J, where the paint T is not guided and the air is not discharged, resulting in a defective appearance. As a countermeasure against this, it is possible to provide a cutout part (not shown) that communicates the inside and outside in a part of the enclosed part 16 of the protruding part 4J, and to guide the paint T from the cutout part to the inside of the enclosed part 16. However, even if paint T seeps into the enclosing portion 16 from the cutout, there may be cases where the air inside the enclosing portion 16 is not completely discharged from the cutout, in which case air pockets A will still form inside the enclosing portion 16, resulting in paint missing portions K. In addition, the cutouts will cause the enclosing portion 16 to become discontinuous, which may degrade the appearance of the product (in-mold coated molded product 10J).
[0023] The object of the present invention, which has been devised in consideration of the above circumstances, is to provide a method and apparatus for manufacturing an in-mold coated molded product which can prevent air pockets from forming near the various protrusions described above and which can prevent missing areas of the coating due to air pockets. [Means for solving the problem]
[0024] According to the present invention, which has been invented to achieve the above-mentioned object, there is provided a method for producing an in-mold coated molded product by mounting a molding substrate on a first mold, abutting the first mold with the molding substrate mounted against a second mold so as to cover the molding substrate, forming a coating gap between the inner surface of the second mold and the outer surface of the molding substrate, and injecting a liquid coating agent into the coating gap to adhere to the outer surface of the molding substrate, wherein convex portions corresponding to a desired pattern to be applied to the outer surface of the molding substrate are formed on the outer surface of the molding substrate with a height smaller than the dimensions of the coating gap, the molding substrate with the convex portions formed is mounted on the first mold, and the first mold is abutted against the second mold so as to cover the molding substrate, forming an air-vent gap between the top surfaces of the convex portions and the inner surface of the second mold that is narrower than the coating gap, and in this state, injecting the liquid coating agent into the coating gap, and as the injected liquid coating agent passes through the air-vent gap, it sweeps away air near the convex portions in the coating gap through the air-vent gap (claim 1).
[0025] There is also provided a method for producing an in-mold coated molded product as described in claim 1, characterized in that by thus pushing away the air in the vicinity of the convex portions in the coating gap through the air vent gap, a basic coating film is formed on the outer surface of the substrate using a liquid coating agent in accordance with the coating gap on the parts other than the convex portions of the substrate, and a pattern coating film that is thinner than the basic coating film is formed on the top surfaces of the convex portions of the substrate in accordance with the air vent gap, and the dimensions of the air vent gap through which the pattern coating film is formed are set to dimensions that enable the top surfaces of the convex portions to be visually observed from the outside through the pattern coating film (Claim 2).
[0026] Further, there is provided a method for producing an in-mold coated molded product as described in claim 1 or 2, characterized in that the convex portion has at least one of a damming portion that is open on the upstream side in the flow direction of the liquid coating agent injected into the coating gap and flowing within the coating gap, a rear roll-up portion that is open on the downstream side in the flow direction of the liquid coating agent, a side roll-up portion that is open on the side that intersects with the flow direction of the liquid coating agent, and an enclosed portion that is enclosed on the inside with respect to the flow of the liquid coating agent (Claim 3).
[0027] According to the present invention, there is provided a method for producing an in-mold coated molded product by mounting a molding substrate on a first mold, abutting the first mold with the molding substrate mounted against a second mold so as to cover the molding substrate, forming a coating gap between the inner surface of the second mold and the outer surface of the molding substrate, and injecting a liquid coating agent into the coating gap to adhere to the outer surface of the molding substrate, the method comprising the steps of forming convex portions on the inner surface of the second mold corresponding to a desired pattern to be applied to the outer surface of the molding substrate, the convex portions having a height smaller than the dimensions of the coating gap, and abutting the first mold with the molding substrate mounted against the second mold with the convex portions formed thereon so as to cover the molding substrate, forming an air vent gap narrower than the coating gap between the top surfaces of the convex portions and the outer surface of the molding substrate, and injecting the liquid coating agent into the coating gap in this state, and as the injected liquid coating agent passes through the air vent gap, it sweeps away the air in the coating gap near the convex portions through the air vent gap (Claim 4).
[0028] There is also provided a method for producing an in-mold coated molded product as described in claim 4, characterized in that the air near the convex portion in the coating gap is pushed away through the air vent gap, so that a basic coating film corresponding to the coating gap is formed on the outer surface of the molded substrate by the liquid coating agent on the portion of the molded substrate that faces other than the convex portion of the second mold, and a pattern coating film thinner than the basic coating film corresponding to the air vent gap is formed on the portion of the molded substrate that faces the convex portion of the second mold, and the dimensions of the air vent gap through which the pattern coating film is formed are set to dimensions that allow the molded substrate to be visually observed from the outside through the pattern coating film (claim 5).
[0029] There is also provided a method for producing an in-mold coated molded product as set forth in claim 4 or 5, characterized in that the convex portion of the second mold has at least one of a damming portion that is open on the upstream side in the flow direction of the liquid coating agent injected into the coating gap and flowing within the coating gap, a rear roll-up portion that is open on the downstream side in the flow direction of the liquid coating agent, a side roll-up portion that is open on the side that intersects with the flow direction of the liquid coating agent, and an enclosed portion that is enclosed on the inside with respect to the flow of the liquid coating agent (Claim 6).
[0030] According to the present invention, there is provided an apparatus for manufacturing an in-mold coated molded product used in the method for manufacturing an in-mold coated molded product described in claim 1, characterized in that convex portions corresponding to a desired pattern to be applied to the outer surface of the molded substrate are formed on the outer surface of the molded substrate with a height smaller than the dimension of the coating gap, and when a first mold on which the molded substrate with the convex portions is attached is abutted against a second mold so as to cover the molded substrate, an air vent gap narrower than the coating gap is formed between the top surfaces of the convex portions formed on the outer surface of the molded substrate and the inner surface of the second mold (claim 7).
[0031] According to the present invention, there is provided an apparatus for manufacturing an in-mold coated molded product used in the method for manufacturing an in-mold coated molded product described in claim 4, characterized in that a convex portion corresponding to the desired pattern to be applied to the outer surface of the molding substrate is formed on the inner surface of the second mold with a height smaller than the dimension of the coating gap, and when the first mold with the molding substrate attached is abutted against the second mold with the convex portion formed thereon so as to cover the molding substrate, an air vent gap narrower than the coating gap is formed between the top surface of the convex portion formed on the inner surface of the second mold and the outer surface of the molding substrate (claim 8).
[0032] There is also provided an apparatus for manufacturing an in-mold coated molded product as described in claim 7 or 8, characterized in that the convex portion has at least one of a damming portion that is open on the upstream side in the flow direction of the liquid coating agent injected into the coating gap and flowing within the coating gap, a rear roll-up portion that is open on the downstream side in the flow direction of the liquid coating agent, a side roll-up portion that is open on the side that intersects with the flow direction of the liquid coating agent, and an enclosed portion that is enclosed on the inside with respect to the flow of the liquid coating agent (claim 9). Effect of the Invention
[0033] The method and apparatus for producing an in-mold coated molded product according to the present invention can provide the following effects.
[0034] (1) According to the invention of claim 1, convex portions corresponding to the desired pattern to be applied to the outer surface of the molding substrate are formed on the outer surface of the molding substrate with a height smaller than the dimensions of the coating gap, and an air release gap narrower than the coating gap is formed between the top surface of the convex portion and the inner surface of the second mold, so that the air near the convex portions in the coating gap is swept away through the air release gap, which prevents air pockets from forming near the convex portions and prevents loss of coating due to air pockets. This improves the appearance of the product (in-mold coated molded product).
[0035] (2) According to the invention of claim 1, the liquid coating agent flows between the top surface of the convex portion of the molding substrate and the inner surface of the second mold, so that the top surface of the convex portion of the molding substrate is coated with a thickness corresponding to the air release gap, and the liquid coating agent flows between the part of the molding substrate other than the convex portion and the inner surface of the second mold, so that the part of the molding substrate other than the convex portion is coated with a thickness corresponding to the coating gap. As a result, the convex portion and the other part of the molding substrate are coated integrally without interruption, and the peel strength of the coating is improved.
[0036] (3) According to the invention of claim 4, convex portions corresponding to the desired pattern to be applied to the outer surface of the molding substrate are formed on the inner surface of the second mold with a height smaller than the dimensions of the coating gap, and an air release gap narrower than the coating gap is formed between the top surface of the convex portion and the outer surface of the molding substrate, so that the air near the convex portions in the coating gap is swept away through the air release gap, which prevents air pockets from forming near the convex portions and prevents loss of the coating due to air pockets. This improves the appearance of the product (in-mold coated molded product).
[0037] (4) According to the invention of claim 4, the liquid coating agent flows between the top surface of the convex portion of the second mold and the outer surface of the molding substrate, so that the portion of the molding substrate facing the convex portion of the second mold is coated with a thickness corresponding to the air release gap, and the liquid coating agent flows between the portion other than the convex portion of the second mold and the outer surface of the molding substrate, so that the portion of the molding substrate facing the portion other than the convex portion of the second mold is coated with a thickness corresponding to the coating gap. As a result, the portion of the molding substrate facing the top surface of the convex portion of the second mold and the portion facing the portion other than the convex portion of the second mold are coated integrally and seamlessly, improving the peel strength of the coating. [Brief description of the drawings]
[0038] [Figure 1]FIG. 1 is an explanatory diagram of a manufacturing method and manufacturing apparatus for an in-mold coated molded product, illustrating an outline of an invention previously invented by the present inventor and related to a prior application of the present applicant, in which (a) is a side cross-sectional view of a first mold, a second mold, and a molding substrate, and (b) is a perspective view of the molding substrate. [Diagram 2] FIG. 2 is an explanatory diagram showing a state in which a molding substrate is sandwiched between the first mold and the second mold shown in FIG. 1(a), where (a) is a plan view and (b) is a side cross-sectional view of (a). [Diagram 3] Figure 3(a11) is an enlarged view of portion a11 in Figure 2(b), Figure 3(a1) is an enlarged view of portion a1 in Figure 2(a) and is a cross-sectional view taken along line II in Figure 3(a11), Figures 3(a12), 3(a13), and 3(a14) are explanatory views showing the coating process following Figure 3(a11), and Figures 3(a2), 3(a3), and 3(a4) are explanatory views showing the coating process following Figure 3(a1). [Figure 4] Figure 4(b1) is an enlarged view of portion b1 in Figure 2(a), Figures 4(b2), 4(b3), and 4(b4) are explanatory diagrams showing the coating process following Figure 4(b1), Figure 4(c1) is an enlarged view of portion c1 in Figure 2(a), and Figures 4(c2), 4(c3), and 4(c4) are explanatory diagrams showing the coating process following Figure 4(c1). [Diagram 5] 6A to 6C are explanatory diagrams of an in-mold coated molded product manufactured by the manufacturing method and manufacturing apparatus for an in-mold coated molded product related to the invention in the prior application of the present applicant which have been explained using FIGS. 1 to 5, in which (a) is a perspective view of the in-mold coated molded product, (b) is a cross-sectional view taken along line bb in (a), and (c) is a cross-sectional view taken along line cc in (a). [Figure 6] FIG. 1 is an explanatory diagram of a method and an apparatus for manufacturing an in-mold coated molded product, showing an application example of the invention related to the applicant's earlier application, in which (a) is a plan view showing a state in which a molded substrate is sandwiched between a first mold and a second mold, (b) is a side cross-sectional view thereof, and (c) is a perspective view of the molded substrate. [Figure 7]Figure 7(a21) is an enlarged view of portion a21 in Figure 6(b), Figure 7(a1) is a cross-sectional view taken along line II in Figure 7(a21), Figures 7(a22), 7(a23), and 7(a24) are explanatory views showing the coating process following Figure 7(a21), and Figures 7(a2), 7(a3), and 7(a4) are explanatory views showing the coating process following Figure 7(a1). [Figure 8] FIG. 8 is an explanatory diagram of an in-mold coated molded product manufactured by the in-mold coated molded product manufacturing method and manufacturing apparatus, which is an application example of the invention related to the applicant's prior application described with reference to FIGS. 6 to 7, in which (a) is a perspective view of the in-mold coated molded product, and (b) is a cross-sectional view taken along line bb in (a). [Figure 9] FIG. 1 is an explanatory diagram of a manufacturing method and manufacturing apparatus for an in-mold coated molded product according to a first embodiment of the present invention, where (a) is a side cross-sectional view of a first mold, a second mold, and a molding substrate, and (b) is a perspective view of the molding substrate. [Figure 10] 9(a) and 9(b) are explanatory views showing a state in which a molding substrate is sandwiched between the first mold and the second mold shown in FIG. 9(a), where (a) is a plan view and (b) is a side cross-sectional view of (a). [Figure 11] Figure 11(A11) is an enlarged view of portion A11 in Figure 10(b), Figure 11(A1) is an enlarged view of portion A1 in Figure 10(a) and is a cross-sectional view along line II in Figure 11(A11), Figures 11(A12), 11(A13), and 11(A14) are explanatory views showing the coating process following Figure 11(A11), and Figures 11(A2), 11(A3), and 11(A4) are explanatory views showing the coating process following Figure 11(A1). [Figure 12] Figure 12(B1) is an enlarged view of portion B1 in Figure 10(a), Figures 12(B2), 12(B3), and 12(B4) are explanatory diagrams showing the coating process following Figure 12(B1), Figure 12(C1) is an enlarged view of portion C1 in Figure 10(a), and Figures 12(C2), 12(C3), and 12(C4) are explanatory diagrams showing the coating process following Figure 12(C1). [Figure 13]13A to 13D are explanatory diagrams of an in-mold coated molded product manufactured by the in-mold coated molded product manufacturing method and manufacturing apparatus according to the first embodiment described with reference to FIGS. 9 to 12, in which (a) is a perspective view of the in-mold coated molded product, (b) is a cross-sectional view taken along line bb in (a), (c) is a cross-sectional view taken along line cc in (a), and (d) is an enlarged view of part d in (b). [Figure 14] 5A and 5B are explanatory diagrams of a manufacturing method and manufacturing apparatus for an in-mold coated molded product according to a second embodiment of the present invention, in which (a) is a plan view showing a molded substrate sandwiched between a first mold and a second mold, (b) is a side cross-sectional view thereof, and (c) is a perspective view of the molded substrate. [Figure 15] Figure 15(A21) is an enlarged view of portion A21 in Figure 14(b), Figure 15(A1) is a cross-sectional view taken along line II in Figure 15(A21), Figures 15(A22), 15(A23), and 15(A24) are explanatory views showing the coating process following Figure 15(A21), and Figures 15(A2), 15(A3), and 15(A4) are explanatory views showing the coating process following Figure 15(A1). [Figure 16] 16A and 16B are explanatory diagrams of an in-mold coated molded product manufactured by the in-mold coated molded product manufacturing method and manufacturing apparatus according to the second embodiment of the present invention described with reference to Figures 14 and 15, in which (a) is a perspective view of the in-mold coated molded product, and (b) is a cross-sectional view taken along line bb in (a). [Figure 17] FIG. 17(a31) is an explanatory diagram of a manufacturing method and manufacturing apparatus for an in-mold coated molded product, showing a comparative example (a convex portion is provided on the inner surface of the second mold) of the invention related to the applicant's prior application, which was previously invented by the present inventor. FIG. 17(a31) is a partially enlarged view of the manufacturing apparatus for an in-mold coated molded product in which a convex portion is provided on the inner surface of the second mold and the top surface of the convex portion abuts against the outer surface of the molding substrate. FIG. 17(a32), FIG. 17(a33), and FIG. 17(a34) are explanatory diagrams showing the coating process following FIG. 17(a31). FIG. 17(b) is a side cross-sectional view of an in-mold coated molded product manufactured through the processes of FIG. 17(a31) to FIG. 17(a34). [Figure 18]18(A31) is a partially enlarged view of the manufacturing apparatus for an in-mold coated molded product in which a convex portion is provided on the inner surface of the second mold and an air vent gap is formed between the top surface of the convex portion and the outer surface of the molding substrate; FIG. 18(A32), FIG. 18(A33), and FIG. 18(A34) are explanatory views showing the coating step following FIG. 18(A31); and FIG. 18(B) is a side cross-sectional view of an in-mold coated molded product manufactured through the steps of FIG. 18(A31) to FIG. 18(A34). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] A preferred embodiment of the present invention will be described in detail below with reference to the accompanying drawings. The dimensions, materials, and other specific numerical values shown in the embodiment are merely examples for facilitating understanding of the invention, and do not limit the present invention unless otherwise specified. In this specification and drawings, elements having substantially the same functions and configurations are given the same reference numerals to avoid repeated explanations, and elements not directly related to the present invention are not illustrated.
[0040] (Outline of manufacturing method for in-mold coated molded products) The manufacturing method of the in-mold coated molded product according to the present invention is based on the premise that a molding substrate 2 is attached to a first mold 1 as shown in Figures 9(a) and 9(b), the first mold 1 with the molding substrate 2 attached is butted against a second mold 3 so as to cover the molding substrate as shown in Figures 10(a) and 10(b), a coating gap G1 is formed between the inner surface of the second mold 3 and the outer surface of the molding substrate 2, and a liquid coating agent is injected into the coating gap G1 to adhere to the outer surface of the molding substrate 2. This premise is the same as the manufacturing method and manufacturing device of the in-mold coated molded product according to the invention of the applicant's prior application, which was explained using Figures 1 to 5.
[0041] (Overview of the first embodiment) The manufacturing method of the in-mold coated molded product according to the first embodiment of the present invention is characterized in that, as shown in Figs. 10(a) and 10(b), convex portions 4 corresponding to a desired pattern to be applied to the outer surface of the molding substrate 2 are formed on the outer surface of the molding substrate 2 at a height H1 smaller than the dimension of the coating gap G1, the molding substrate 2 on which the convex portions 4 are formed is attached to a first mold 1, and the first mold 1 is abutted against a second mold 3 so as to cover the molding substrate 2, thereby forming an air-release gap G2 (G2 = G1 - H1) narrower than the coating gap G1 between the top surfaces of the convex portions 4 and the inner surface of the second mold 3, and in this state, as shown in Figs. 11(A11) to 11(A14) and 11(A1) to 11(A4), a liquid coating agent is injected into the coating gap G1, and when the injected liquid coating agent passes through the air-release gap G2, the air in the vicinity of the convex portions 4 in the coating gap G1 is swept away through the air-release gap G2. The first embodiment of the present invention has a similar configuration to the invention of the applicant's earlier application described with reference to FIGS. 1 to 5, except that the height H1 of the protrusion 4 is different.
[0042] Hereinafter, a method and an apparatus for producing an in-mold coated molded product according to the first embodiment will be described.
[0043] (Coating Gap G1) 9(a), 9(b), 10(a), and 10(b) show a manufacturing device for an in-mold coated molded product according to the first embodiment of the present invention. This device includes a lower first mold 1 in which a convex core 1a is formed, and an upper second mold 3 in which a concave cavity 3a is formed. When the first mold 1 is butted against the second mold 3 and clamped with a molding substrate 2 attached to the core 1a of the first mold 1, a coating gap G1 (for example, 10 to 100 μm) is formed between the outer surface of the molding substrate 2 and the inner surface of the cavity 3a of the second mold 3. The first mold 1 and the second mold 3 are not limited to being arranged vertically (vertical type), but may be arranged left and right (horizontal type). Various mechanisms such as hydraulic or electric mechanisms are used for the actuator that butts the first mold 1 against the second mold 3 to clamp the mold, separates them to open the mold, and removes the molded product.
[0044] As shown in FIG. 9(a), FIG. 10(a), and FIG. 10(b), an injection port 5 for injecting a liquid coating agent (for example, thermosetting paint T) into the above-mentioned coating gap G1 is formed on one side of the second mold 3. The injection port 5 communicates with the cavity 3a through an injection passage 6 and a gate 7 formed inside the second mold 3. In addition, an outlet 8 for discharging the excess paint T from the liquid coating agent (hereinafter also referred to as paint T) injected into the coating gap G1 is formed on the other side of the second mold 3. The outlet 8 is one end of an outlet passage 9 formed in a groove shape from the side of the second mold 3 to the inner surface of the cavity 3a on the PL surface (parting line surface: abutting surface with the first mold 1) of the second mold 3, and communicates with the cavity 3a through the outlet passage 9 when the mold is clamped as shown in FIG. 10(b). According to this configuration, when paint T is injected into the injection port 5 provided on one side of the second mold 3 during mold closing as shown in Figure 10(b), the injected paint T flows through the coating gap G1 toward the discharge port 8 provided on the other side of the second mold, and the flow of the paint T causes the air in the coating gap G1 to be discharged from the discharge port 8, and the outer surface of the molding substrate 2 is coated with paint T as the paint T is discharged from the discharge port 8.
[0045] (Air release gap G2) As shown in Fig. 9(a), Fig. 9(b), and Fig. 10(b), on the outer surface of the molding substrate 2, a convex portion 4 according to a desired pattern to be applied to the outer surface of the molding substrate 2 is formed at a height H1 (e.g., 5 to 80 µm) smaller than the dimension of the coating gap G1 (e.g., 10 to 100 µm). The molding substrate 2 on which the convex portion 4 is formed is attached to the core 1a of the first mold 1. Then, as shown in Fig. 10(b), the first mold 1 is butted against the second mold 3, and the molding substrate 2 attached to the first mold 1 is inserted into the cavity 3a of the second mold 3. At this time, an air release gap G2 (G2 = G1 - H1: e.g., 5 to 50 µm) narrower than the coating gap G1 is formed between the top surface of the convex portion 4 formed on the outer surface of the molding substrate 2 and the inner surface of the cavity 3a of the second mold 3. The dimension of the air release gap G2 is larger than the particle size of the pigment or glitter particles contained in the paint T as a liquid coating agent, and does not prevent the passage of the pigment or glitter particles.
[0046] As shown in FIG. 10(b), the first mold 1 with the molding substrate 2 attached thereto is butted against the second mold 3 and clamped, and then a liquid coating agent (paint T) is injected into the injection port 5 provided on one side of the second mold 3. Then, the injected paint T flows through the coating gap G1 toward the discharge port 8 provided on the other side of the second mold 3, and when the paint T passes through the air vent gap G2, the air in the vicinity of the protrusion 4 in the coating gap G1 is swept away through the air vent gap G2. This prevents air pockets A from being formed in the vicinity of the protrusion 4, and prevents the occurrence of missing portions K of the coating due to the air pockets A. Therefore, after the coating process is completed, the first mold 1 shown in FIG. 10(b) is separated from the second mold 3 to open the mold, and the product (in-mold coated molded product 10 (see FIG. 13(a))) taken out of the core 1a of the first mold 1 can be prevented from having poor appearance due to the air pockets A, and the appearance quality is improved.
[0047] In the first embodiment, in the mold clamping state shown in Fig. 10(b), the liquid coating agent (paint T) flows between the top surface of the convex portion 4 of the molding substrate 2 and the cavity 3a of the second mold 3, so that the top surface of the convex portion 4 of the molding substrate 2 is coated with a thickness corresponding to the air release gap G2, and the liquid coating agent flows between the portion of the molding substrate 2 other than the convex portion 4 and the cavity 3a of the second mold 3, so that the portion of the molding substrate 2 other than the convex portion 4 is coated with a thickness corresponding to the coating gap G1. As a result, the product (in-mold coated molded product 10) taken out after the mold is opened is coated integrally with the convex portion 4 and the other portion without interruption, as shown in Fig. 13(b) and its enlarged view Fig. 13(d), so that the coating film 11 (coating film: represented by dots in the figure) is formed, and the peel strength of the coating film 11 (coating film) is improved.
[0048] According to the first embodiment, as described above, the air in the coating gap G1 near the protrusions 4 is swept away through the air vent gap G2, so that a basic coating film 11a corresponding to the coating gap G1 is formed on the outer surface of the forming substrate 2 by the liquid coating agent on the portions of the forming substrate 2 other than the protrusions 4, and a pattern coating film 11b thinner than the basic coating film 11a is formed on the top surfaces of the protrusions 4 of the forming substrate 2 in accordance with the air vent gap G2, as shown in Figures 13(b), 13(c) and 13(d). The basic coating film 11a and the pattern coating film 11b integrally form the above-mentioned integrated coating film 11. Here, by setting the dimensions of the air vent gap G2 which forms the pattern coating film 11b to a dimension that allows the top surfaces of the convex portions 4 to be visible from the outside through the pattern coating film 11b, the pattern of the convex portions 4 can be recognized when the appearance of the product (in-mold coated molded article 10) is visually inspected, and it is possible to achieve both improved peel strength of the paint film by the integral coating film 11 and recognition of the pattern by the convex portions 4.
[0049] (Protruding part 4) As shown in FIG. 9(b), in this embodiment, four protrusions 4 are provided on the outer surface of the molding substrate 2. The protrusions 4 shown in part A1 of FIG. 10(a) have a damming section 12 that is open on the upstream side of the flow direction of the coating agent (paint T) flowing in the coating gap G1. The protrusions 4 shown in part B1 of FIG. 10(a) have a rear roll-in section 13 that is open on the downstream side of the flow direction of the coating agent (paint T) flowing in the coating gap G1. The protrusions 4 shown in part C1 of FIG. 10(a) have a side roll-in section 14 that is open on the side that intersects with the flow direction of the coating agent (paint T) flowing in the coating gap G1. The damming section 12, the rear roll-in section 13, and the side roll-in section 14 will be described below.
[0050] (Dam section 12) The protrusion 4 shown in part A1 of FIG. 10(a) has a blocking portion 12. The blocking portion 12 is arranged such that the open side of the mountain-shaped member faces the upstream side of the flow of the paint T, and when the paint T injected into the inlet 5 passes through the coating gap G1 and is discharged from the outlet 8, the upstream side of the flow direction of the paint T flowing from left to right in the coating gap G1 is open. The blocking portion 12 is not limited to the shape of the open side of the mountain-shaped member, and may be a U-shaped or C-shaped shape in which the open side faces the upstream side of the flow of the paint T. In addition, the open side of these mountain-shaped, U-shaped, C-shaped, etc. is not limited to being arranged directly at 90 degrees to the flow of the liquid coating agent (paint T: hereinafter represented by dots) flowing through the coating gap G1 as in this embodiment, but may also be arranged at an angle (for example, 45 to 90 degrees) to the flow of the paint T. Furthermore, the damming portion 12 may have any shape as long as the upstream side of the flow of paint T is open as described above, and the downstream side of the flow of paint T may have any shape.
[0051] (Rear wrap-around section 13) The convex portion 4 shown in part B1 of FIG. 10(a) has a rear roll-in portion 13. The rear roll-in portion 13 is arranged such that the open side of the mountain-shaped member faces the downstream side of the flow of the paint T, and is shaped so that the downstream side of the flow direction of the paint T flowing from left to right in the coating gap G1 is open. The shape of the open side of the mountain-shaped member of the rear roll-in portion 13 is not limited to the shape, and the open side of the mountain-shaped member may be U-shaped or U-shaped, etc., facing the downstream side of the flow of the paint T. In addition, the open side of these mountain-shaped, U-shaped, U-shaped, etc. is not limited to being arranged in the opposite direction at 90 degrees to the flow of the liquid coating agent (paint T) flowing through the coating gap as in this embodiment, but may also be arranged in the opposite direction at an angle (for example, 45 to 90 degrees) to the flow of the paint T. In addition, the rear roll-in portion 13 may have a shape in which the downstream side of the flow of the paint T is open as described above, and the upstream side of the flow of the paint T may have any shape.
[0052] (Side roll-up section 14) The convex portion 4 shown in part C1 of FIG. 10(a) has a side roll-in portion 14. The side roll-in portion 14 is arranged so that the opening side of the mountain-shaped member intersects (orthogonal in this embodiment) with the flow of the paint T, and the side that intersects (orthogonal) with the flow direction of the paint T flowing from left to right in the coating gap G1 is open. The side roll-in portion 14 is not limited to the shape of the opening side of the mountain-shaped member, and may be a U-shaped or C-shaped opening side that is oriented to intersect with the flow of the paint T. In addition, the opening side of these mountain-shaped, U-shaped, C-shaped, etc. is not limited to being arranged so as to be perpendicular to the flow of the liquid coating agent (paint T) flowing through the coating gap G1, i.e., to intersect at 90 degrees, but also includes those arranged to intersect obliquely (for example, 45 to 90 degrees) with the flow of the paint T. In addition, the side roll-in portion 14 may have a shape in which the side that intersects with the flow of the paint T is open as described above, and the opposite side (the apex side of the mountain-shaped in this embodiment) may have any shape.
[0053] (Flow of paint T and air near the damming section 12) As shown in part A1 of Fig. 10(a) and part A11 of Fig. 10(b), which is the corresponding cross section, the flow of paint T and air in the coating gap G1 will be described for the damming section 12 that is open on the upstream side in the flow direction of the liquid coating agent (paint T) flowing through the coating gap G1. An enlarged view of part A11 of Fig. 10(b) is shown in Fig. 11(A11), and an enlarged view of part A1 of Fig. 10(a) is shown in Fig. 11(A1).
[0054] As shown in Figures 11(A11) and 11(A1), when the paint T indicated by dots approaches the damming portion 12 of the convex portion 4, the air in front of the damming portion 12 (left side in the figure) gradually escapes through the air vent gap G2 to the right side in the figure. However, because the air vent gap G2 is narrower than the coating gap G1, the air pressure inside the damming portion 12 increases to a certain extent, and the paint T in front of the damming portion 12 is pushed by this pressure, causing the tip Ta of the flow to have a concave shape. Thereafter, as the flow of paint T progresses, the air inside the damming portion 12 escapes through the air vent gap, as shown in Figures 11(A12) and 11(A2), and the paint T passes over the air vent gap G2, as shown in Figures 11(A13) and 11(A3), and finally, as shown in Figures 11(A14) and 11(A4), the paint T is coated without forming air bubbles (air pockets) near the protrusions 4 having the damming portions 12.
[0055] (Flow of paint T and air in the vicinity of the rear wrap-around section 13) As shown in part B1 of Figure 10(a), the flow of the paint T and air in the coating gap G1 will be described for the rear wrap-around section 13, which is open downstream in the flow direction of the liquid coating agent (paint T) flowing through the coating gap G1. An enlarged view of part B1 is shown in Figure 12(B1).
[0056] As shown in Fig. 12(B1), before the paint T flows and hits the front part of the rear rolled-in part 13 of the convex part 4, the air in front of the rear rolled-in part 13 (left side in the figure) is pushed aside to both sides (up and down in the figure) along the slope of the mountain-shaped member constituting the rear rolled-in part 13, and passes through the air release gap G2 between the top surface of the rear rolled-in part 13 (convex part 4) and the cavity 3a of the second mold to escape into the rear rolled-in part 13. After that, as shown in Fig. 12(B2), the paint T flows from the air release gap G2 to the inside of the rear rolled-in part 13, and as shown in Fig. 12(B3), the paint T that has entered the inside of the rear rolled-in part 13 through the air release gap G2 joins with the paint T at the left and right rear ends of the rear rolled-in part 13, and the paint T is supplied little by little to the inside of the rear rolled-in part 13 through the air release gap G2 as shown by the small arrow. Therefore, ultimately, as shown in FIG. 12(B4), coating is performed without forming air bubbles (air pockets) near the protrusions 4 having the rear rolled-in portions 13.
[0057] (Flow of paint T and air near the side wrap-around portion 14) As shown in part C1 of Figure 10(a), the flow of paint T and air in the coating gap G1 is explained for the side wraparound portion 14 that is open on the side that crosses the flow direction of the liquid coating agent (paint T) flowing through the coating gap G1. An enlarged view of part C1 is shown in Figure 12(C1).
[0058] As shown in FIG. 12(C1), after the paint T flows and hits the tip of the upstream side of the side roll-in portion 14, as shown in FIG. 12(C2), the paint T is divided into a flow along the outer surface of the side roll-in portion 14 and a flow that is rolled into the inner surface of the side roll-in portion 14. At this time, the air in front of the side roll-in portion 14 (convex portion 4) (left side in the figure) is divided like the paint T and flows into the side roll-in portion 14 through the air vent gap G2. Then, as shown in FIG. 12(C3), the paint T rolled into the inner surface of the side roll-in portion 14 and the paint T at the rear end of the outer surface of the side roll-in portion 14 join together, and the paint T is supplied little by little into the side roll-in portion 14 through the air vent gap G2 as shown by the small arrow, so that the paint T is finally coated without forming air bubbles (air pockets) near the convex portion 4 having the side roll-in portion 14, as shown in FIG. 12(C4).
[0059] (The relationship between the size of the air release gap G2 of the blocking portion 12, the rear wrap-around portion 13, and the side wrap-around portion 14) As explained using Fig. 11, in the protrusion 4 having the damming portion 12, the air-release gap G2 is primarily for discharging air, so a relatively narrow gap is sufficient. On the other hand, as explained using Fig. 12, in the protrusion 4 having the rear roll-in portion 13 and the protrusion 4 having the side roll-in portion 14, the air-release gap G2 also allows air to flow but primarily allows paint T to flow, so it is preferable to set it wider than in the protrusion 4 having the damming portion 12. For example, if the air-release gap G2 of the protrusion 4 having the damming portion 12 is 10 µm, it is possible to set the air-release gap G2 of the protrusion 4 having the rear roll-in portion 13 and the side roll-in portion 14 to 30 µm.
[0060] (In-mold coated molded product 10) As described above, by injecting a liquid coating agent (paint T) from the injection port 5 and discharging it from the discharge port 8 while the first mold 1 shown in Fig. 10(b) is pressed against the second mold 3 and clamped, the outer surface of the molding substrate 2 is appropriately coated (painted) without forming air bubbles (air pockets A) near the convex portion 4 having the blocking portion 12, the convex portion 4 having the rear roll-up portion 13, and the convex portion 4 having the side roll-up portion 14. After the first mold 1 is separated from the second mold 3 and opened, this product (in-mold coated molded product 10) is released from the core 1a of the first mold 1 by an ejection mechanism (ejector pin, etc.) provided in the first mold 1, and the hardened paint T is removed as an unnecessary part in the discharge passage 9.
[0061] This in-mold coated molded product 10 is shown in Figures 13(a), 13(b), 13(c), and 13(d). Figure 13(d) is an enlarged view of part d in Figure 13(b). During coating, in-mold coated molded product 10, air bubbles (air pockets A) are not formed near protruding portion 4 having damming portion 12, protruding portion 4 having rear roll-in portion 13, and protruding portion 4 having side roll-in portion 14, so that no missing portions K of coating (paint) are generated near these damming portions 12, rear roll-in portion 13, and side roll-in portion 14, and no appearance defects due to this do not occur.
[0062] In contrast, in the comparison example shown in Figures 5(a), 5(b), and 5(c) (an in-mold coated molded product 10J manufactured by the in-mold coated molded product manufacturing method and manufacturing apparatus of the invention related to the applicant's earlier application), as already mentioned, depending on conditions such as the viscosity of the paint T, the injection time, and the hardening time of the paint T, a missing portion K of the paint T due to an air pocket A may be formed near the convex portion 4J, which may result in a poor appearance.
[0063] 13(b) and 13(c), the top surface of the protrusions 4 of the molding substrate 2 is coated with a thickness corresponding to the air release gap G2, and the portion of the molding substrate 2 other than the protrusions 4 is coated with a thickness corresponding to the coating gap G1, so that the protrusions 4 and the other portions are coated integrally without interruption to form the coating film 11 (coating film). This improves the peel strength of the coating film 11 (coating film).
[0064] In contrast, in the comparative example shown in Figures 5(b) and 5(c) (an in-mold coated molded product 10J manufactured by the manufacturing method and manufacturing apparatus for an in-mold coated molded product relating to the invention in the applicant's prior application), as already mentioned, no coating film is formed on the top surface of the convex portion 4J, and therefore it is conceivable that with continued use the coating film 11J may peel off from the boundary between the top surface of the convex portion 4J and the coating film 11J or from the missing portion K of the paint T described above.
[0065] In the first embodiment, as shown in Figures 13(b), 13(c), and 13(d), a basic coating film 11a is formed on the outer surface of the molding substrate 2 in a portion other than the protruding portions 4 of the molding substrate 2 according to the coating gap G1 shown in Figure 10(b), and a pattern coating film 11b that is thinner than the basic coating film 11a is formed on the top surfaces of the protruding portions 4 of the molding substrate 2 according to the air release gap G2 shown in Figure 10(b). Here, by setting the dimensions of the air release gap G2 that forms the pattern coating film 11b to a dimension that allows the top surfaces of the protruding portions 4 to be visible through the pattern coating film 11b from the outside, the pattern of the protruding portions 4 can be recognized when the appearance of the product (in-mold coated molded product 10) is visually inspected, and thus both the improvement of peel strength due to the integral coating film 11 and the recognition of the pattern due to the protruding portions 4 can be achieved.
[0066] In order to clearly distinguish the convex portion 4 below the pattern coating film 11b and the molding substrate 2 below the basic coating film 11a from the outside with the naked eye in Figures 13(b), 13(c), and 13(d), it is preferable to set the dimension of the coating gap G1 shown in Figure 10(b) that forms the basic coating film 11a to a dimension that makes it impossible to visually recognize the molding substrate 2 from the outside through the basic coating film 11a. However, even if the coating gap G1 is set slightly smaller than that dimension so that the molding substrate 2 can be slightly recognized from the outside through the basic coating film 11a, it does not matter as long as there is a difference in tone (degree of shading) that can be distinguished from the pattern part of the convex portion 4 recognized from the outside through the pattern coating film 11b.
[0067] Second embodiment A method and an apparatus for manufacturing an in-mold coated molded product according to the second embodiment of the present invention will be described with reference to Figs. 14 to 16. The method and apparatus for manufacturing an in-mold coated molded product according to the second embodiment is basically the same as the first embodiment described with reference to Figs. 9 to 13, and differs only in that the protruding portion 4 has an enclosed portion 16 that is enclosed on the inside with respect to the flow of the liquid coating agent (paint T). Therefore, the same components as those in the first embodiment are given the same reference numerals and their description is omitted, and only the enclosed portion, which is the difference, will be described. The second embodiment has the same configuration as the invention related to the applicant's prior application described with reference to Figs. 6 to 8, except that the height H1 of the protruding portion 4 is different. For example, the enclosed portion may be a ring-shaped pattern or the letters "A" and "O".
[0068] (Box 16) As shown in Figures 14(a), 14(b), and 14(c), the protrusion 4 formed on the upper surface of the molding substrate 2 has an enclosed portion 16 that is surrounded on the inside by the flow of the liquid coating agent (paint T). The height of the top surface of the enclosed portion 16 from the upper surface of the molding substrate 2 is set to a height H1 that is smaller than the dimension of the coating gap G1, and as shown in Figure 14(b), when the first mold 1 with the molding substrate 2 attached thereto is abutted against the second mold 3 to close the mold, an air release gap G2 narrower than the coating gap G1 is formed between the top surface of the enclosed portion 16 and the inner surface of the cavity 3a of the second mold 3.
[0069] An enlarged view of part A21 in Fig. 14(b) is shown in Fig. 15(A21), and a cross-sectional view of line II in Fig. 15(A21) is shown in Fig. 15(A1). The coating steps following Fig. 15(A21) are shown in Fig. 15(A22), Fig. 15(A23), and Fig. 15(A24), and the coating steps following Fig. 15(A1) are shown in Fig. 15(A2), Fig. 15(A3), and Fig. 15(A4). These coating processes are basically the same as those of the first embodiment described above, so detailed explanations will be omitted, but as shown in Figures 15(A22) and 15(A2), paint T penetrates into the enclosed portion 16 from the air vent gap G2 on the upstream side of the flow direction, and as shown in Figures 15(A23) and 15(A3), the air inside the enclosed portion 16 is discharged from the air vent gap G2 on the rear side in the flow direction of the paint T. Ultimately, as shown in Figures 15(A24) and 15(A4), paint T is filled inside the enclosed portion 16 without any gaps, and air pockets A can be avoided.
[0070] A product (in-mold coated molded product 10a) thus coated without air pockets A inside the surrounding portion 16 is shown in Fig. 16(a) and Fig. 16(b). In this in-mold coated molded product 10a, a basic coating film 11a is formed on the outer surface of the molding substrate 2 in the portion other than the protruding portion 4 having the surrounding portion 16, including the inside of the surrounding portion 16, according to the coating gap G1, and a pattern coating film 11b thinner than the basic coating film 11a is formed on the top surface of the protruding portion 4 (enclosure portion 16) of the molding substrate 2, according to the air release gap G2. The effects of the in-mold coated molded product 10a according to the second embodiment in which the basic coating film 11a and the pattern coating film 11b are integrally formed in this way are similar to those of the first embodiment described above, and therefore detailed description will be omitted.
[0071] (Relationship between the size of the air release gap G of the enclosed portion 16) In the second embodiment, as shown in Figures 15(A22) and 15(A2), the paint T infiltrates into the enclosed portion 16 from the air vent gap G2 on the upstream side in the flow direction, and as shown in Figures 15(A23) and 15(A3), the air inside the enclosed portion 16 is discharged from the air vent gap G2 on the rear side in the flow direction of the paint T, so that the paint T fills the enclosed portion 16 without air pockets A, and therefore it is desired to actively flow the paint T into the enclosed portion 16. Therefore, the air vent gap G2 between the top surface of the enclosed portion 16 and the inner surface of the cavity 3a of the second mold 3 in the second embodiment is preferably set wider than the air vent gap G2 of the protruding portion 4 having the rear rolled-in portion 13 and the air vent gap G2 of the protruding portion 4 having the side rolled-in portion 14 described in the first embodiment. For example, if the air release gap G2 of the protrusion 4 having the rear roll-in portion 13 and the side roll-in portion 14 is set to 30 μm, the air release gap G2 of the protrusion 4 having the surrounding portion 16 may be set to 50 μm.
[0072] Third embodiment A manufacturing method and manufacturing device for an in-mold coated molded product according to a third embodiment of the present invention will be described with reference to Figures 17 to 18. Figures 17(a31) to 17(a34) are coating process diagrams showing a comparison of the third embodiment (the invention related to the applicant's earlier application), Figure 17(b) is an in-mold coated molded product 10J obtained thereby as a comparison, Figures 18(A31) to 18(A34) are coating process diagrams according to the third embodiment, and Figure 18(B) is an in-mold coated molded product 10b according to the third embodiment obtained thereby.
[0073] In the third embodiment, as shown in Fig. 18(A31), a convex portion 4 for forming an air release gap G2, which is the key point of the present invention, is provided on the inner surface of the second mold 3 (the inner surface of the cavity 3a), and compared with the first embodiment in which the convex portion 4 is provided on the outer surface of the molding substrate 2 as shown in Fig. 11(A11) and the second embodiment in which the convex portion 4 is provided on the outer surface of the molding substrate 2 as shown in Fig. 15(A21), the third embodiment has the same configuration except that the convex portion 4 is provided on the inner surface of the cavity 3a of the second mold 3 instead of the outer surface of the molding substrate 2. Therefore, the same reference numerals are used for the same components as in the first and second embodiments, and the description is omitted, and only the difference that the convex portion 4 is provided on the inner surface of the cavity 3a of the second mold 3 will be described.
[0074] In the third embodiment, as shown in Fig. 18 (A31), a convex portion 4 is formed on the inner surface of the cavity 3a of the second mold 3 with a height H1 smaller than the dimension of the coating gap G1, and when the first mold 1 with the molding substrate 2 attached thereto is butted against the second mold 3, an air release gap G2 (G2 = G1 - H1) is formed between the top surface of the convex portion 4 and the outer surface of the molding substrate 2. That is, compared to the first embodiment shown in Fig. 11 (A11) and the second embodiment shown in Fig. 15 (A21), in which a convex portion 4 is provided on the outer surface of the molding substrate 2, and when the first mold 1 with the molding substrate 2 attached thereto is butted against the second mold 3, an air release gap G2 is formed between the top surface of the convex portion 4 and the inner surface of the cavity 3a of the second mold 3, the target on which the convex portion 4 is provided has been changed from the outer surface of the molding substrate 2 to the inner surface of the second mold 3.
[0075] (Paint T and air flow in comparison) In order to clarify the points of the third embodiment, first, a coating process of a comparative example will be described with reference to Fig. 17. In the comparative example, as shown in Fig. 17(a31), a convex portion 4J is formed on the inner surface of the cavity 3a of the second mold 3 at a height H corresponding to the coating gap G1, and when the first mold 1 with the molding substrate 2 attached thereto as shown in Fig. 2(b) is abutted against the second mold 3 and the mold is closed, the top surface of the convex portion 4J abuts against the outer surface of the molding substrate 2. It is assumed that the convex portion 4J formed on the outer surface of the molding substrate 2 in Fig. 2(b) does not exist.
[0076] In this state, when a liquid coating agent (e.g., paint T) is poured into the coating gap G1 as shown in Fig. 17(a31), depending on the conditions such as the shape of the convex portion 4J, the viscosity of the liquid coating agent (paint T), the injection time, and the curing time, the air in front of the convex portion 4J (in front of the direction of flow of paint T) is trapped because it is partitioned by the convex portion 4J and has no escape route, and finally, as shown in Fig. 17(a34), there is a possibility that an air pocket A is formed. As a result, as shown in Fig. 17(b), in the product (in-mold coated molded product 10J) that is opened and taken out, a coating film (paint film) 11J corresponding to the coating gap G1 is formed on the outer surface of the molding substrate 2 that faces the convex portion 4J, and a missing portion K of paint T is formed in the part of the air pocket A formed in contact with the convex portion 4J, resulting in a poor appearance.
[0077] In addition, as shown in Fig. 17(a34), the top faces of the protrusions 4J are abutted against the outer surface of the forming substrate 2 and are masked, so that, as shown in Fig. 17(b), no coating film (coating film 11J) is formed on the parts of the forming substrate 2 where the top faces of the protrusions 4J abut, and the outer surface of the forming substrate 2 is exposed. As a result, with continued use, it is possible that the coating film 11J will peel off from the boundary between the exposed parts 2R of the forming substrate 2 and the coating film 11J, or from the missing parts K of the paint T described above.
[0078] (Flow of paint T and air in the third embodiment) On the other hand, in the third embodiment, as shown in Fig. 18(A31), a convex portion 4 is formed on the inner surface of the cavity 3a of the second mold 3 with a height H1 smaller than the dimension of the coating gap G1, and when the first mold 1 with the molding substrate 2 attached thereto is abutted against the second mold 3 with the convex portion 4 formed therein as shown in Fig. 10(b) and the mold is closed, an air release gap G2 (G2=G1-H1) narrower than the coating gap G1 is formed between the top surface of the convex portion 4 and the outer surface of the molding substrate 2. It is assumed that the convex portion 4 formed on the outer surface of the molding substrate 2 in Fig. 10(b) does not exist.
[0079] In this state, as shown in FIG. 18(A31), when a liquid coating agent (e.g., paint T) is poured into the coating gap G1, the air in front of the convex portion 4 is discharged backward through the air vent gap G2 as shown in FIG. 18(A32), and the air pressure in front of the convex portion 4 is released. As a result, as shown in FIG. 18(A33), the paint T also smoothly passes through the air vent gap G2 and infiltrates behind the convex portion 4. Therefore, as shown in FIG. 18(A34), no air pocket A is formed near the convex portion 4, and the coating can be performed properly. As a result, as shown in FIG. 18(B), the product (in-mold coated molded product 10b) taken out after opening the mold does not have a missing portion K of the paint T due to the air pocket A.
[0080] That is, in the third embodiment, protrusions 4 corresponding to the desired pattern to be applied to the outer surface of the molding substrate 2 are formed on the inner surface of the second mold 3 with a height H1 smaller than the dimension of the coating gap G1, and an air release gap G2 narrower than the coating gap G1 is formed between the top surface of the protrusions 4 and the outer surface of the molding substrate 2, so that the air near the protrusions 4 in the coating gap G1 is swept away through the air release gap G2, thereby preventing air pockets A from forming near the protrusions 4 and preventing loss of coating due to the air pockets A. This makes it possible to prevent poor appearance of the product (in-mold coated molded product 10b).
[0081] In addition, as shown in Figures 18(A31), 18(A34) and 18(B), the portion of the forming substrate 2 opposite to the protrusions 4 is coated with a basic coating film 11a having a thickness corresponding to the coating gap G1, and the portion of the forming substrate 2 opposite to the protrusions 4 is coated with a pattern coating film 11b having a thickness corresponding to the air release gap G2, so that the forming substrate 2 is coated integrally and seamlessly with the basic coating film 11a and the pattern coating film 11b to form the coating film 11 (coating film). This improves the peel strength of the coating (coating film).
[0082] (others) The basic effects of the third embodiment are similar to those of the first and second embodiments, and therefore a description thereof will be omitted. In addition, as a modification of the third embodiment, it is also possible to add the components described in the first and second embodiments. For example, as a modification of the third embodiment, there is an embodiment in which the protrusion 4 has at least one of the blocking portion 12, the rear rolled-up portion 13, the side rolled-up portion 14, and the surrounding portion 16 described in the second embodiment. In addition, as a modification of the third embodiment, there is an embodiment in which the dimensions of the air release gap G2 forming the pattern coating film 11b and the dimensions of the coating gap G1 forming the basic coating film 11a are set to the dimensions described in the first and second embodiments.
[0083] Although the preferred embodiment of the present invention has been described above with reference to the accompanying drawings, it goes without saying that the present invention is not limited to the above-mentioned embodiment, and various modified or altered examples within the scope of the claims also belong to the technical scope of the present invention. For example, the top surface of the convex portion 4 is shown as a flat surface in each of the above-mentioned embodiments, but it also includes a curved surface, a sloping surface, and an uneven surface. In addition, the present invention also includes an embodiment in which the convex portion 4 has at least one of the blocking portion 12, the rear roll-up portion 13, the side roll-up portion 14, and the surrounding portion 16 described in the second embodiment, which are described in the first embodiment. In addition, the present invention also includes an embodiment in which the type in which the convex portion 4 described in the third embodiment is provided on the inner surface of the second mold 3 and the type in which the convex portion 4 described in the first and second embodiments is provided on the outer surface of the molding substrate 2 are mixed. [Industrial Applicability]
[0084] The present invention can be used for a method and apparatus for manufacturing an in-mold coated molded product in which a coating gap is formed between the outer surface of a substrate sandwiched between a pair of molds and the inner surface of the molds, and a liquid coating agent is injected into the coating gap to adhere to the outer surface of the substrate. [Explanation of symbols]
[0085] 1. First Mold 2 Molding base material 3. Second mold 4 Convex 10 In-mold coated molded products 11a Basic coating film 11b Pattern coating film 12 Damming section 13 Rear wrap-around section 14 Side roll-up section 16 Enclosed section T Paint as a liquid coating agentT G1 Coating Gap G2 Air release gap
Claims
1. A method for producing an in-mold coated molded product, comprising the steps of: mounting a molding substrate in a first mold; abutting the first mold with the mounting substrate against a second mold so as to cover the molding substrate; forming a coating gap between an inner surface of the second mold and an outer surface of the molding substrate; and injecting a liquid coating agent into the coating gap to adhere the coating agent to the outer surface of the molding substrate, A convex portion corresponding to a desired pattern to be applied to the outer surface of the molding substrate is formed on the outer surface of the molding substrate with a height smaller than the dimension of the coating gap, the molding substrate on which the convex portion is formed is attached to the first mold, and the first mold is abutted against the second mold so as to cover the molding substrate, thereby forming an air release gap narrower than the coating gap between the top surface of the convex portion and the inner surface of the second mold; a step of injecting the liquid coating agent into the coating gap in this state, and as the injected liquid coating agent passes through the air vent gap, the air in the vicinity of the convex portion in the coating gap is pushed away through the air vent gap.
2. The air in the vicinity of the protrusion in the coating gap is purged through the air vent gap, A basic coating film is formed on the outer surface of the molding substrate by the liquid coating agent in a portion other than the protruding portion of the molding substrate in accordance with the coating gap, and a pattern coating film thinner than the basic coating film is formed on the top surface of the protruding portion of the molding substrate in accordance with the air release gap; 2. The method for producing an in-mold coated molded product according to claim 1, wherein the dimension of the air vent gap through which the pattern coating film is formed is set to a dimension that enables the top surfaces of the convex portions to be visually observed from the outside through the pattern coating film.
3. 3. The method for producing an in-mold coated molded product according to claim 1, characterized in that the convex portion has at least one of a blocking portion that is open on the upstream side in the flow direction of the liquid coating agent injected into the coating gap and flowing within the coating gap, a rear roll-up portion that is open on the downstream side in the flow direction of the liquid coating agent, a side roll-up portion that is open on the side intersecting the flow direction of the liquid coating agent, and an enclosed portion that is enclosed on the inside with respect to the flow of the liquid coating agent.
4. A method for producing an in-mold coated molded product, comprising the steps of: mounting a molding substrate in a first mold; abutting the first mold with the mounting substrate against a second mold so as to cover the molding substrate; forming a coating gap between an inner surface of the second mold and an outer surface of the molding substrate; and injecting a liquid coating agent into the coating gap to adhere the coating agent to the outer surface of the molding substrate, A convex portion corresponding to a desired pattern to be applied to the outer surface of the molding substrate is formed on the inner surface of the second mold with a height smaller than the dimension of the coating gap, and the first mold with the molding substrate attached is abutted against the second mold with the convex portion formed thereon so as to cover the molding substrate, thereby forming an air release gap narrower than the coating gap between the top surface of the convex portion and the outer surface of the molding substrate; a step of injecting the liquid coating agent into the coating gap in this state, and as the injected liquid coating agent passes through the air vent gap, the air in the vicinity of the convex portion in the coating gap is pushed away through the air vent gap.
5. The air in the vicinity of the protrusion in the coating gap is purged through the air vent gap, A basic coating film is formed on the outer surface of the molding substrate by the liquid coating agent in the portion of the molding substrate opposite to the convex portion in accordance with the coating gap, and a pattern coating film thinner than the basic coating film is formed in the portion of the molding substrate opposite to the convex portion in accordance with the air release gap; 5. The method for producing an in-mold coated molded product according to claim 4, characterized in that the dimensions of the air vent gap through which the pattern coating film is formed are set to a dimension that allows the molding substrate to be visually observed from the outside through the pattern coating film.
6. 6. The method for producing an in-mold coated molded product according to claim 4 or 5, characterized in that the convex portion has at least one of a blocking portion that is open on the upstream side in the flow direction of the liquid coating agent injected into the coating gap and flowing within the coating gap, a rear roll-up portion that is open on the downstream side in the flow direction of the liquid coating agent, a side roll-up portion that is open on the side intersecting the flow direction of the liquid coating agent, and an enclosed portion that is enclosed on the inside with respect to the flow of the liquid coating agent.
7. A manufacturing apparatus used in the method for manufacturing an in-mold coated molded product according to claim 1, The apparatus for manufacturing an in-mold coated molded product is characterized in that a convex portion corresponding to a desired pattern to be applied to the outer surface of the molding substrate is formed on the outer surface of the molding substrate with a height smaller than the dimension of the coating gap, and when the first mold on which the molding substrate with the convex portion is attached is abutted against the second mold so as to cover the molding substrate, an air vent gap narrower than the coating gap is formed between the top surface of the convex portion formed on the outer surface of the molding substrate and the inner surface of the second mold.
8. A manufacturing apparatus for use in the method for manufacturing an in-mold coated molded product according to claim 4, The apparatus for manufacturing an in-mold coated molded product is characterized in that a convex portion corresponding to a desired pattern to be applied to the outer surface of the molding substrate is formed on the inner surface of the second mold with a height smaller than the dimension of the coating gap, and when the first mold with the molding substrate attached is abutted against the second mold in which the convex portion is formed so as to cover the molding substrate, an air vent gap narrower than the coating gap is formed between the top surface of the convex portion formed on the inner surface of the second mold and the outer surface of the molding substrate.
9. 9. The device for manufacturing an in-mold coated molded product according to claim 7 or 8, characterized in that the convex portion has at least one of a damming portion that is open on the upstream side in the flow direction of the liquid coating agent injected into the coating gap and flowing within the coating gap, a rear wrap-around portion that is open on the downstream side in the flow direction of the liquid coating agent, a side wrap-around portion that is open on the side intersecting the flow direction of the liquid coating agent, and an enclosed portion that is enclosed on the inside with respect to the flow of the liquid coating agent.
Citation Information
Patent Citations
Display method for mark and its product
JP2002146558A
Surface machining method for auxiliary material of apparel by laser beam and auxiliary material of apparel obtained by the same
JP2005007403A
In-mold coating molding method
JP3617807B2
Cited By
Method and apparatus for manufacturing molded products with in-mold coating.
JP2026136491A
Method and apparatus for manufacturing molded products with in-mold coating.
JP7935190B2
Manufacturing method and manufacturing device for in-mold-coated molded article
WO2026172732A1