Nonlinear resistance material, and discharge prevention structure
A zinc composite oxide-based nonlinear resistance material with conductive powder and resin addresses the challenge of discharge prevention in high frequency ranges by maintaining effective electric field relaxation, enhancing discharge prevention structures in rotating machine coil ends.
Patent Information
- Application Number
- JP2023043885
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing nonlinear resistance materials struggle to provide effective discharge prevention in high frequency ranges, such as frequencies of 400 Hz or higher, due to insufficient electric field relaxation characteristics.
A nonlinear resistance material comprising a base material with a nonlinear resistance layer made of zinc composite oxide, containing zinc oxide, bismuth oxide, antimony oxide, cobalt oxide, manganese oxide, and nickel oxide, along with conductive powder and resin, which maintains suitable electric field relaxation characteristics even at high frequencies.
The material exhibits stable electric field relaxation characteristics in high frequency ranges, effectively preventing discharge in applications like coil ends of rotating machines, particularly at frequencies above 400 Hz.
Smart Images

Figure 2024133883000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonlinear resistance material and a discharge prevention structure. [Background technology]
[0002] As shown in Fig. 4, for example, an insulation structure is known for a coil end of a rotating machine (generator), in which an insulating layer 52 is wound around the outer layer of a conductor 51 incorporated in an iron core 41, and a low-resistance layer 53 with a relatively low resistance value is provided on the outer layer of the insulating layer 52. In the insulation structure of the coil end 50, the electric field strength may become high near the end portion of the low-resistance layer 53. In order to alleviate this localized electric field concentration, there is, for example, an electric discharge prevention structure 4 in which an electric field alleviation layer 54 made of a nonlinear resistance material such as a corona discharge prevention tape is arranged to overlap part of the low-resistance layer 53.
[0003] For example, a material using silicon carbide is known as a nonlinear resistance material forming the electric field relaxation layer 54. Patent Document 1 describes that the electric field relaxation layer is formed by applying a paint using silicon carbide particles to the outer periphery of an insulating layer, or by wrapping a tape coated with such a paint around the insulating layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-217109 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, even with the above-mentioned corona discharge prevention tape, it may be difficult to obtain the desired discharge prevention effect in a high frequency range such as 400 Hz or more. For this reason, there is a demand for further improvement in the electric field relaxation characteristics of nonlinear resistance materials in the high frequency range.
[0006] Under these circumstances, an object of the present invention is to provide a nonlinear resistance material that has good electric field relaxation characteristics even in the high frequency region. [Means for solving the problem]
[0007] One aspect of the present invention that solves the above problem is to A substrate and a nonlinear resistance layer disposed on a main surface of the substrate, The nonlinear resistance layer is made of a nonlinear resistance powder of zinc complex oxide and a volume resistivity of 10 1 Ω cm or more 10 3 The conductive powder has a resistivity of Ω·cm or less, and a resin. The nonlinear resistance powder relates to a nonlinear resistance material that is a sintered body containing zinc oxide (ZnO), bismuth oxide (Bi2O3), antimony oxide (Sb2O3), cobalt oxide (Co2O3), manganese oxide (MnO2) and nickel oxide (NiO). Effect of the Invention
[0008] The nonlinear resistance material of the present invention exhibits favorable electric field relaxation characteristics even in high frequency ranges such as 400 Hz or more, making it particularly suitable for use as an electric field relaxation layer in discharge prevention structures such as the coil ends of rotating machines. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view of a nonlinear resistance material according to an embodiment. [Diagram 2] FIG. 4 is a schematic diagram of a coil end according to the embodiment. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a coil end according to the embodiment. [Figure 4] 1 is a schematic cross-sectional view of a conventional discharge prevention structure for a coil end. [Diagram 5] FIG. 1 is a diagram showing the results of surface resistivity in the examples. [Figure 6] FIG. 13 is a diagram showing the results of electrolytic relaxation characteristics in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0011] Fig. 1 is a schematic cross-sectional view of a nonlinear resistance material, Fig. 2 is a schematic view showing a coil end using a nonlinear resistance material in an electric field relaxation layer, and Fig. 3 is a cross-sectional view taken along line AA in Fig. 2.
[0012] [Nonlinear resistance materials] 1, the nonlinear resistance material includes a substrate 20 and a nonlinear resistance layer 10 disposed on a main surface of the substrate 20. The nonlinear resistance layer 10 is disposed on one or both main surfaces of the substrate 20, and is preferably disposed on both surfaces. The shape of the nonlinear resistance material is not particularly limited, but is preferably a tape-like material having a predetermined width.
[0013] [Nonlinear resistance layer] The nonlinear resistance layer 10 includes a nonlinear resistance powder, a conductive powder, and a resin. In the nonlinear resistance layer of this embodiment, the nonlinear resistance powder is a composite oxide mainly made of zinc oxide, and thus exhibits a nonlinear resistance characteristic in which a current flows when the applied voltage increases while a high resistance is exhibited when the applied voltage is low. On the other hand, when only the nonlinear resistance powder is used as the nonlinear resistance layer, the resistance remains high even when the voltage value increases, making it difficult to obtain the desired electric field relaxation characteristic. In response to this, it is conceivable to apply a nonlinear resistance material having a nonlinear resistance powder and a conductive powder, but the present inventors have found that, depending on the type of conductive powder, the resistance may become too low when the voltage value increases. For this reason, in the present invention, a nonlinear resistance material having a volume resistivity of 10 1 Ω cm or more 10 3 The nonlinear resistance layer contains a conductive powder with a resistivity of Ω·cm or less. A nonlinear resistance material having a nonlinear resistance layer containing the conductive powder described above tends to exhibit good electric field relaxation characteristics, without excessively decreasing resistance even when the voltage value increases, while maintaining a good dispersion state of the nonlinear resistance powder and the conductive powder.
[0014] The thickness of the nonlinear resistance layer is preferably 100 μm or more and 300 μm or less, and particularly preferably 150 μm or more and 250 μm or less. Within the above thickness range, the layer contains an appropriate amount of nonlinear resistance powder and conductive powder, which tends to exhibit good electric field relaxation characteristics and is less likely to cause cracks in the nonlinear resistance layer. Here, when the nonlinear resistance layer is present on both sides of the substrate, the thickness of the nonlinear resistance layer is preferably set to the above range as the total thickness of the nonlinear resistance layers on both sides.
[0015] Nonlinear resistance powder: The nonlinear resistance powder is a sintered body containing zinc oxide (ZnO), bismuth oxide (Bi2O3), antimony oxide (Sb2O3), cobalt oxide (Co2O3), manganese oxide (MnO2) and nickel oxide (NiO). The sintered body containing the above oxides is likely to become a nonlinear resistance powder that exhibits stable nonlinear resistance characteristics. In particular, by containing zinc oxide, bismuth oxide and antimony oxide, it becomes easier to have nonlinear resistance characteristics, and by containing cobalt oxide, manganese oxide and nickel oxide, it tends to be easier to exhibit stable nonlinear resistance characteristics. When cobalt oxide is contained, it is particularly easier to exhibit stable nonlinear resistance characteristics.
[0016] The reason why the nonlinear resistance powder of this embodiment stably exhibits nonlinear resistance characteristics is believed to be as follows: By sintering oxides such as bismuth oxide and antimony oxide together with zinc oxide to form a sintered body, a composite oxide in which at least a part of the multiple types of oxides combine to form spinel particles is formed, and segregates at the grain boundaries of the zinc oxide. This composite oxide of segregated spinel particles suppresses the growth of zinc oxide particles in the sintered body, making it easier for zinc oxide particles to have uniform and small particle sizes, which is believed to result in a nonlinear resistance powder with good nonlinear resistance characteristics.
[0017] The content of each oxide in the nonlinear resistance powder is preferably within the following ranges in terms of molar ratio when the total metal elements in the nonlinear resistance powder, calculated as oxides, is 100 mol %. The content of zinc oxide, which is the main material of the nonlinear resistance powder, is preferably 90.0 mol % or more, and more preferably 93.0 mol % or more. From the viewpoint of exhibiting stable nonlinear resistance characteristics, the content of zinc oxide is preferably 99.0 mol % or less, and more preferably 98.0 mol % or less.
[0018] From the viewpoint of easily becoming a nonlinear resistance powder exhibiting nonlinear resistance characteristics, the content of bismuth oxide is preferably 0.05 mol% or more and 3.0 mol% or less, and more preferably 0.1 mol% or more and 2.0 mol% or less. The content of antimony oxide is preferably 0.05 mol% or more and 4.0 mol% or less, and more preferably 0.1 mol% or more and 3.0 mol% or less. In particular, since it is easy to exhibit stable nonlinear resistance characteristics, the content of cobalt oxide is preferably 0.03 mol% or more and 3.0 mol% or less, and more preferably 0.05 mol% or more and 2.0 mol% or less. Since it is easy to exhibit stable nonlinear resistance characteristics, the content of manganese oxide is preferably 0.03 mol% or more and 3.0 mol% or less, and more preferably 0.05 mol% or more and 2.0 mol% or less. The content of nickel oxide is preferably 0.03 mol% or more and 3.0 mol% or less, and more preferably 0.05 mol% or more and 2.0 mol% or less.
[0019] The nonlinear resistance powder may contain oxide compounds such as chromium oxide (Cr2O3), silver oxide (Ag2O), silicon oxide (SiO2), boron oxide (B2O3), and tin oxide (SnO2) as minor components other than those mentioned above. It is known that these oxide compounds are dissolved in zinc oxide crystal particles during the firing process. The metal in the oxide compound that is dissolved in this way functions as a donor. As a result, the free electron density of the zinc oxide crystal particles becomes higher, and the resistance value of the zinc oxide crystal particles themselves decreases, so that the voltage rise in the overcurrent range tends to be suppressed low. From this viewpoint, it is preferable to contain the above-mentioned oxide compounds in the nonlinear resistance powder. The content of the oxide compounds as minor components mentioned above is preferably 0.01 mol% or more and 7.0 mol% or less, and more preferably 0.05 mol% or more and 2.0 mol% or less, in terms of a molar ratio when the total metal elements in the nonlinear resistance powder are 100 mol% in terms of oxide.
[0020] The nonlinear resistance powder may contain other additives as desired. For example, it may contain rare earth oxides for the purpose of increasing the resistance of the nonlinear resistance powder. The rare earth oxides may contain at least one oxide (R2O3) of a rare earth element (R), such as yttrium (Y), europium (Eu), erbium (Er), thulium (Tm), gadolinium (Gd), dysprosium (Dy), holmium (Ho), or ytterbium (Yb). The content of the rare earth oxide in the nonlinear resistance powder is preferably 0.01 mol% or more and 5.0 mol% or less, and more preferably 0.1 mol% or more and 1.0 mol% or less, in terms of metal elements.
[0021] Average particle size of nonlinear resistance powder D 50 The average particle diameter D is preferably 15 μm or more and 60 μm or less, and particularly preferably 20 μm or more and 50 μm or less. 50 When the nonlinear resistance powder has an average particle diameter D in this embodiment, the nonlinear resistance layer is easily dispersed in a good state with the conductive powder, and is easily able to exhibit good electric field relaxation characteristics. 50 is the particle size at 50% cumulative value in the particle size distribution obtained by the laser diffraction / scattering method, and is the particle size on a volume basis.
[0022] Conductive powder: The conductive powder in this embodiment has a volume resistivity of 10 1 Ω cm or more 10 3 From the viewpoint of easily preventing the resistance from dropping too much, the volume resistivity is preferably 50 Ω·cm or more and 800 Ω·cm or less, and more preferably 70 Ω·cm or more and 600 Ω·cm or less. In this regard, for example, a typical conductive powder has a volume resistivity of about 10 -1 Conductors with a resistance of less than Ω cm are approximately 10 -1 Ω cm or more 10 8 Examples of the range of the volume resistivity include semiconductors with a volume resistivity of Ω·cm or less. In contrast, in this embodiment, by applying a conductive powder within the above-mentioned range of volume resistivity, it is possible to achieve both a suitable dispersion state of each powder and good electric field relaxation characteristics as a nonlinear resistance layer. The conductive powder in this embodiment is a material different from the nonlinear resistance powder, and the conductive powder targets materials other than the nonlinear resistance powder. Specifically, the conductive powder is a material that exhibits linear resistance and can be specified by the volume resistivity as described above. In contrast, the nonlinear resistance powder exhibits nonlinear resistance and the volume resistivity changes depending on the level of the voltage. In this way, the conductive powder and the nonlinear resistance powder in this embodiment are distinguished by whether or not they exhibit nonlinear resistance. The volume resistivity in this embodiment can be measured by a constant current application method (JIS K 7194) or the like.
[0023] The conductive powder may be made of various materials without limitation as long as the volume resistivity is within the above-mentioned range. For example, it can be appropriately selected from materials such as tin oxide, phosphorus-doped tin oxide, antimony-doped tin oxide, ITO, ATO, and silver-coated resin powder, and in particular, tin oxide and phosphorus-doped tin oxide are preferred.
[0024] Average particle size of conductive powder D 50 is preferably 0.001 μm or more and 10 μm or less, and particularly preferably 0.01 μm or more and 5 μm or less. When the conductive powder has the above average particle size, the nonlinear resistance layer is likely to be well dispersed with the nonlinear resistance powder, and is likely to exhibit good electric field relaxation characteristics. In addition, the average particle size D of the conductive powder 50is the average particle size of the nonlinear resistance powder, D 50 The average particle size of the nonlinear resistance powder is preferably smaller than D 50 Average particle size of conductive powder D 50 Ratio of the average particle size of the conductive powder D 50 ) / (average particle size of nonlinear resistance powder D 50 ) × 100) is preferably 0.01% or more and 0.15%, and particularly preferably 0.02% or more and 0.10% or less. When the average particle size of the conductive powder and the nonlinear resistance powder is within the above ratio range, the conductive powder and the nonlinear resistance powder are well dispersed when the nonlinear resistance layer is formed.
[0025] Resin: There are no particular limitations on the resin that can be applied to this embodiment, and the resin functions as a base material for forming a layer in which the nonlinear resistance powder and the conductive powder are dispersed. The resin is preferably heat resistant, and is particularly preferably class F (155°C or higher) or class H (180°C or higher). For example, the resin may be silicone resin, acrylic resin, epoxy resin, or the like.
[0026] Optional components: The nonlinear resistance layer 10 may contain optional components, such as a dispersant, in addition to the nonlinear resistance powder, conductive powder, and resin described above. The type of dispersant is not particularly limited, and may include, for example, a wetting dispersant.
[0027] Blend ratio: The content of each material in the nonlinear resistance layer 10 is preferably within the following range. The content of the nonlinear resistance powder is preferably 40% by mass or more and 80% by mass or less, and more preferably 50% by mass or more and 70% by mass or less. The content of the conductive powder is preferably 3% by mass or more and 15% by mass or less, and more preferably 5% by mass or more and 10% by mass or less. The content of the resin is preferably 15% by mass or more and 40% by mass or less, and more preferably 20% by mass or more and 30% by mass or less. The content of the dispersant is preferably 0% by mass or more and 3% by mass or less, and more preferably 0.5% by mass or more and 1.5% by mass or less. Within the above content ranges, the nonlinear resistance layer 10 tends to have a favorable dispersion state of the nonlinear resistance powder and the conductive powder.
[0028] The mass ratio of the content of the nonlinear resistance powder to the conductive powder in the nonlinear resistance layer 10 (mass of conductive powder / mass of nonlinear resistance powder) is preferably 0.05 to 0.2, and particularly preferably 0.07 to 0.15. If it is within the above range, it is easy to achieve a good electric field relaxation effect by preventing the resistance from becoming too low.
[0029] [Base material] There are no particular limitations on the material that can be used as the substrate 20, and the material may be selected from appropriate materials such as fiber-reinforced cloth, etc. As the substrate 20, for example, a Tetron cloth, a glass cloth, etc. can be used.
[0030] [Manufacturing method] In this embodiment, the method of laminating the nonlinear resistance layer 10 on the substrate 20 is not particularly limited, and may be laminated by any method. For example, the nonlinear resistance layer 10 may be manufactured by applying a composition or slurry obtained by mixing a nonlinear resistance powder, a conductive powder, a resin, and an arbitrary component as a nonlinear resistance material to the substrate 20 to form the nonlinear resistance layer 10. Instead of applying to the substrate 20, the nonlinear resistance layer 10 may be formed by impregnating the substrate 20 with the composition or slurry. The application of the nonlinear resistance layer 10 to the substrate 20 can be performed by any method, and for example, a microvaristor paint application device described in JP 2022-053780 A may be used.
[0031] Manufacturing method of nonlinear resistance powder: The nonlinear resistance powder can be manufactured by carrying out the steps (1) to (4) shown below. (1) A first mixing step of mixing bismuth oxide, antimony oxide, cobalt oxide, manganese oxide, and nickel oxide with an optional auxiliary component. (2) A second mixing step in which the mixture from the first mixing step is mixed with zinc oxide. (3) A calcination step of calcining the mixture from the second mixing step (4) A firing process for firing the calcined body after the calcination process. Steps (1) to (4) will be described in detail below.
[0032] (1) First mixing step: In this step, bismuth oxide, antimony oxide, cobalt oxide, manganese oxide, nickel oxide, and any optional subcomponent are mixed in any solvent, for example, pure water. The mixture is preferably pulverized. The pulverization is performed, for example, using a ball mill to obtain a slurry of the mixture with an average particle size D 50 It is preferable to grind the powder so that the particle size is 0.7 μm or less.
[0033] (2) Second mixing step: In this step, zinc oxide and, optionally, a solvent (e.g., pure water) are added to the slurry of the mixture obtained in the first mixing step, and then mixed. Optionally, a binder (organic resin) and trace components may be added to the mixture. The mixture is preferably classified after drying, for example, by sieve classification. As the trace components, an oxidizing agent for adjusting the pH of the slurry, etc. may be appropriately used.
[0034] (3) Calcination step: In this step, the mixture obtained in the second mixing step is calcined. Calcination is preferably performed by heat treatment at a maximum holding temperature of 800°C to 950°C for 3 hours to 20 hours. As a preliminary step to the heat treatment for calcination, it is preferable to perform heat treatment at 350°C to 700°C to remove the organic binder.
[0035] (4) Firing step: In this step, the calcined body after the firing step is sintered. The sintering was performed by heat treatment at a maximum holding temperature of 900° C. to 1200° C. for 1 hour to 15 hours.
[0036] The nonlinear resistance powder is preferably pulverized and classified after the firing step so that the powder has a suitable average particle size. The pulverization may be performed using a crusher, for example, and the classification may be performed using a sieve.
[0037] [Application] The nonlinear resistance material of this embodiment is suitable for use in a discharge prevention structure for a coil end, which will be described below. An example of the discharge prevention structure for the coil end 3 is a discharge prevention structure having a low resistance layer 33 arranged on the outer layer of the insulating layer 32 in the coil end 3, and an electric field relaxation layer 34 arranged on the outer layer of the insulating layer 32, overlapping a part including the end of the low resistance layer 33, and having a higher resistivity than the low resistance layer when the applied voltage is low, as shown in Fig. 2, in which the electric field relaxation layer 34 is the nonlinear resistance material of this embodiment.
[0038] The insulating layer 32 is not particularly limited as long as it has insulating properties, and may be, for example, a layer formed by wrapping a tape material (mica tape) made of a base material made of glass fiber or polyester sheet, sprinkled with mica powder, and bonded with an adhesive around the conductor 31. The low resistance layer 33 has a volume resistivity of 10 2 ~10 3There are no particular limitations on the layer as long as it has a relatively low resistivity of about Ω·m, and it may be a layer formed of a tape material (carbon tape) obtained by impregnating or coating a conductive paint made of a mixture of carbon black and epoxy resin, etc., on a substrate such as a woven Tetron fabric or a woven glass fabric, and then curing the same. As shown in FIG. 3, the low resistance layer 33 and the electric field relaxation layer 34 are arranged on the outer layer of the insulating layer 32 in an overlapping manner (so that there is a portion where both layers are laminated so as to overlap on the outer layer of the insulating layer 32). For convenience of explanation, FIG. 2 and FIG. 3 are shown as diagrams in which the electric field relaxation layer 34 and the insulating layer 32 are provided shorter on the low resistance layer 33 side than the length of the conductor, but the length of the electric field relaxation layer 34 and the insulating layer 32 on the opposite side to the low resistance layer 33 is not particularly limited, and may be a length that completely covers the conductor. The discharge prevention structure may have a second low resistance layer (not shown) disposed on the overlapping portion of the electric field relaxation layer 34 and on the outer layer of the low resistance layer 33 (in this case, the low resistance layer 33 is referred to as a first low resistance layer). The second low resistance layer may be a layer formed of a carbon tape or the like similar to the first low resistance layer. The discharge prevention structure 34 may have a protective insulating layer (not shown) disposed on the overlapping portion of the second low resistance layer and the electric field relaxation layer 34 and on the outer layer of the electric field relaxation layer 34. The protective insulating layer is made of a tape material constituted of, for example, a heat shrinkable film and a woven Tetron fabric or a woven glass fabric. This tape material may contain a cured (B-stage) epoxy resin. EXAMPLES
[0039] The present embodiment will be described in further detail with reference to the following examples.
[0040] <<Consideration of conductive powder>> As a preliminary experimental example, first, conductive powder was examined. The surface resistivity was measured for the nonlinear resistance layers of the experimental example and comparative experimental example, which contained the nonlinear resistance powder and conductive powder in the compounding ratio shown below. The reason why the surface resistivity was evaluated here is that when the surface resistivity decreases gradually as the electrolytic value increases, it shows a better electric field relaxation effect as an electric field relaxation layer, as opposed to when it decreases abruptly. The experimental example and comparative experimental example will be explained below.
[0041] Experimental example: Nonlinear resistance powder was prepared using the following procedure, then mixed with conductive powder, resin, and dispersant, and applied to an insulating plate to form a nonlinear resistance layer.
[0042] [Preparation of nonlinear resistance powder] First, in the first mixing step, 1.00 mol% of bismuth oxide, 2.00 mol% of antimony oxide, 1.00 mol% of cobalt oxide, 1.00 mol% of manganese oxide, 0.3 mol% of nickel oxide, and 0.1 mol% of silver oxide (Ag2O) as a subcomponent (200 mass ppm with respect to the total amount of zinc oxide and the mixture of the first mixing step) were mixed in pure water. The mixture was pulverized in a ball mill with 3 mm zirconia balls to obtain a slurry. The average particle size D of the slurry was 1.00 mol%. 50 The particle size was 0.7 μm or less. Note that the molar percentage of the compounding ratio in this production method is a molar percentage when the total amount of metal elements calculated as oxides is taken as 100 molar percentage.
[0043] Next, in the second mixing process, the slurry obtained in the above process, 94.6 mol% zinc oxide, polyvinyl alcohol as an organic binder (1 mass% relative to the mass of zinc oxide), and aluminum nitrate aqueous solution (Al(NO3)3·9H2O) as a trace component were mixed. 3+ The mixture was mixed in pure water at 20 ppm by mass in terms of ions, and then granulated using a spray dryer and classified using a sieve with an opening of 120 μm. The granulated material obtained above had an average particle size D 50 was 49.1 μm.
[0044] The granulated material obtained above was heat-treated at a maximum holding temperature of 800°C to 950°C for 3 to 20 hours to carry out a calcination process. As a pretreatment, the material was heat-treated at 350°C to 700°C to remove the organic binder. After that, the material was heat-treated at a maximum holding temperature of 900°C to 1200°C for 1 to 15 hours to carry out a sintering process. The sintered material obtained was pulverized with a pulverizer (Wonder Crush Mill, manufactured by Osaka Chemical Co., Ltd.) and classified with a sieve with an opening of 64 μm. The average particle size D of the nonlinear resistance powder obtained by the above process was 1.0 μm. 50 was 30.65 μm.
[0045] [Formation of nonlinear resistance layer] The nonlinear resistance powder and conductive powder obtained above were mixed in the following compounding ratio and applied in tape form to a thickness of about 1 mm on a glass epoxy insulating board to form a nonlinear resistance layer. In the experimental example, phosphorus-doped tin oxide (SP-2, manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd., volume resistivity 5×10 2 Ω cm (average value), average particle diameter D 50 The resin used was a room temperature drying type methyl silicone resin (KR-251, manufactured by Shin-Etsu Chemical Co., Ltd.), and the dispersant used was a wet dispersant (DISPER BYK180, manufactured by BYK). Nonlinear resistance powder 66.0wt% ·Conductive powder SP-2 6.7wt% ·Resin (KR-251) 27.0wt% Dispersant (DISPER BYK180) 0.3wt%
[0046] Comparative Experimental Example: In the comparative experimental example, carbon black (Tokai Carbon's Toka Black #4400, volume resistivity 10 ―1 The other materials and the conditions for producing the nonlinear resistance layer were the same as in Experimental Example 1. The conductive powder content was made lower than in the experimental example because it was predicted that the surface resistivity would be significantly reduced by the carbon black. Nonlinear resistance powder 65.7wt% ·Conductive powder SP-2 1.3wt% Resin (KR-251) 32.8wt% Dispersant (DISPER BYK180) 0.2wt%
[0047] [Surface resistivity measurement] On the tape-shaped nonlinear resistance layer formed in the experimental example and comparative experimental example (opposite side to the insulating plate), two conductive pastes (Dotite, Fujikura Kasei Co., Ltd.) were formed as electrodes with a gap of 10 mm between them, so as to be parallel to the long side of the tape. The length of the conductive paste in the long side direction was 300 mm. The current value was measured between the two electrodes formed with the conductive paste while changing the DC current from 1 V to 1000 V. An ammeter (ADCMT 5450) was used for the measurement. The surface resistivity (Ω / □) was calculated based on the measured values of voltage, current, electrode distance, and electrode length. The measurement results are shown in Figure 5.
[0048] As shown in Figure 5, in the experimental example, even when the electric field was increased to 30 V / mm or more, the decrease in surface resistivity was suppressed and the decrease was gradual, whereas in the comparative experimental example, the surface resistivity decreased rapidly as the electric field increased. From this, it is considered that the nonlinear resistance layer of the experimental example exhibits a better electric field relaxation effect than the comparative experimental example. In addition, in the comparative experimental example, the surface resistance value increased in the early stage when the voltage was started to be increased because the conductive powder content was low and the influence of materials other than the conductive powder became prominent.
[0049] <<Example>> Next, the electric field relaxation effect was evaluated for the nonlinear resistance material using the nonlinear resistance powder of the experimental example.
[0050] [Creation of nonlinear resistance materials] A nonlinear resistance material was produced using the nonlinear resistance powder produced in the above experimental example. A mixture prepared in the same ratio as in the above experimental example was applied to both sides of a glass cloth (1280 (E06C) for electronic boards) as a base material, with a thickness of 100 μm on each side, so that the total thickness of the layers on both sides was 200 μm. The application was performed using a microvaristor paint application device.
[0051] [Creating a discharge prevention structure] Example: Using the above nonlinear resistance material, a measurement target having a discharge prevention structure as shown in Figures 2 and 3 was produced. After wrapping mica tape as insulating layer 32 around the outer periphery of a conductor copper square bar (25 mm x 25 mm), carbon tape was wrapped around part of the outer periphery of insulating layer 32 as low resistance layer 33. Then, as shown in Figure 3, the above nonlinear resistance material was wrapped around the outer layer of insulating layer 32 as electric field relaxation layer 34 so as to overlap part of low resistance layer 33.
[0052] Comparative Examples 1 and 2: The discharge prevention structure was fabricated using SiC tape instead of the nonlinear resistance material of the example, but was the same as the example. The SiC tape of Comparative Example 1 was CoronaShield SC217.31 from VonRoll Switzerland Ltd, and the SiC tape of Comparative Example 2 was EGSB-T2701.
[0053] [Measurement of electric field strength] For the discharge prevention structures of the examples and the comparative examples, a predetermined voltage (1 kVrms, 3.81 kVrms, 6 kVrms) and an AC voltage of a predetermined frequency (50 Hz, 400 Hz, 800 Hz) were applied between the conductor 31 and the low resistance layer 33. Then, an optical electric field sensor (Seiko Giken Co., Ltd. CS-1403) was used to measure the electric field intensity every 5 mm in the direction in which the electric field relaxation layer was formed (to the right in FIG. 3), with the boundary B between the low resistance layer 33 and the electric field relaxation layer 34 in FIG. 3 set at x=0 mm. The optical electric field sensor head was installed 30 mm away from the surface of the bar coil in the radial direction. The electric field intensity was measured by converting it into a voltage Vp-p (mV) and displaying it on an oscilloscope (Tektronix DPO4104B). For this conversion, the antenna factor was used as a conversion coefficient. The above measurements were performed at single-phase 200V using a test transformer (Tokyo Seiden Co., Ltd. AH1946) and an AC stabilized power supply (Kikusui Electronics Co., Ltd. PCR2000LA).
[0054] From the above measurement results, the electric field strength was calculated based on the following formula. Electric field strength (V / m) = [Voltage Vp-p (mV) × Antenna factor (1 / m)] / 10 3 *The antenna factors are as follows: [Frequency (Hz)] [Antenna factor (1 / m)] 50 275441 400 65575 800 42666
[0055] The measurement results of the electric field strength for the discharge prevention structures of the example and comparative example measured as described above are shown in Fig. 6 and Tables 1 to 3. Fig. 6 shows the results at frequencies of 50 Hz, 400 Hz, and 800 Hz at a voltage of 3.81 kVrms.
[0056] From FIG. 6, it was shown that in the results for any of the frequencies of 50 Hz, 400 Hz, and 800 Hz at a voltage of 3.81 kVrms, the electric field intensity in the Example is maximized at a position farther away from the boundary B (x=0) than in Comparative Examples 1 and 2, or the electric field intensity at each measurement point from the electric field intensity at the boundary B (x=0) to the electric field intensity maximum is smaller than that in Comparative Examples 1 and 2. From this, it was shown that the Example has a superior electric field relaxation effect to Comparative Examples 1 and 2. Furthermore, from Tables 1 to 3, it was shown that in the Example, the electric field intensity is maximized at a position farther away from the boundary B (x=0) than in Comparative Examples 1 and 2, or the electric field intensity at each measurement point from the electric field intensity at the boundary B (x=0) to the electric field intensity maximum is smaller than that in Comparative Examples 1 and 2, under any of the conditions of voltages of 1 kVrms, 3.81 kVrms, and 6 kVrms. In addition, in Tables 1 to 3, the maximum value of the electric field intensity (V / m) under each condition (if there are multiple values, the value at the position closer to the boundary B) is underlined. Therefore, it was shown that the examples had an excellent electric field relaxation effect regardless of the voltage and frequency conditions. It was also shown that the examples had an excellent electric field relaxation effect even in a high frequency range of 400 Hz or more.
[0057] [Table 1]
[0058] [Table 2]
[0059] [Table 3]
[0060] Preferred embodiments of the present invention are described below. [1] A nonlinear resistive layer disposed on a main surface of a substrate; The nonlinear resistance layer is made of a nonlinear resistance powder of zinc complex oxide and a volume resistivity of 10 1 Ω cm or more 10 3 The conductive powder has a resistivity of Ω·cm or less, and a resin. The nonlinear resistance powder is a nonlinear resistance material that is a sintered body containing zinc oxide (ZnO), bismuth oxide (Bi2O3), antimony oxide (Sb2O3), cobalt oxide (Co2O3), manganese oxide (MnO2) and nickel oxide (NiO). [2] The nonlinear resistance material described in [1], wherein the mass ratio of the content of the nonlinear resistance powder to the conductive powder in the nonlinear resistance layer (mass of conductive powder / mass of nonlinear resistance powder) is 0.05 or more and 0.2 or less. [3] The nonlinear resistance material according to [1] or [2], wherein the thickness of the nonlinear resistance layer is 100 μm or more and 300 μm or less. [4] Average particle size D of the conductive powder 50 is the average particle size D of the nonlinear resistance powder 50 The nonlinear resistance material according to any one of [1] to [3], [5] A low resistance layer disposed on the outer layer of the insulating layer at the coil end; an electric field relaxation layer disposed on the outer layer of the insulating layer, the electric field relaxation layer overlapping a portion of the low resistance layer including an end of the low resistance layer; The discharge prevention structure, wherein the electric field relaxation layer is made of the nonlinear resistance material according to any one of [1] to [4]. [Explanation of symbols]
[0061] 1. Nonlinear resistance materials 10 Nonlinear resistance layer 20 Base material 31, 51 Conductor 32, 52 Insulation layer 33, 53 Low resistance layer 34, 54 Electric field relaxation layer
Claims
1. A substrate and a nonlinear resistance layer disposed on a main surface of the substrate, The nonlinear resistance layer is made of a nonlinear resistance powder of zinc complex oxide and a volume resistivity of 10 1 Ω・cm or more 10 3 The conductive powder has a resistivity of Ω cm or less, and a resin, The nonlinear resistance powder is made of zinc oxide (ZnO), bismuth oxide (Bi 2 O 3 ), antimony oxide (Sb 2 O 3 ), cobalt oxide (Co 2 O 3 ), manganese oxide (MnO 2 A nonlinear resistance material that is a sintered body containing nickel oxide (NiO).
2. 2. The nonlinear resistance material according to claim 1, wherein the mass ratio of the content of the nonlinear resistance powder to the content of the conductive powder in the nonlinear resistance layer (mass of conductive powder / mass of nonlinear resistance powder) is 0.05 or more and 0.2 or less.
3. 3. The nonlinear resistance material according to claim 1, wherein the nonlinear resistance layer has a thickness of 100 μm or more and 300 μm or less.
4. The average particle diameter D of the conductive powder 50 is the average particle size D of the nonlinear resistance powder 50 The nonlinear resistance material according to claim 1 or 2, wherein
5. a low resistance layer disposed on an outer layer of the insulating layer at the coil end; an electric field relaxation layer disposed on the outer layer of the insulating layer, the electric field relaxation layer overlapping a portion of the low resistance layer including an end of the low resistance layer; The discharge prevention structure, wherein the electric field relaxation layer is made of the nonlinear resistance material according to claim 1 or 2.
Citation Information
Patent Citations
JP1980082048U
Coil for rotary electrical machine
JP1980136839A
Manufacture of insulated coil
JP1987077040A
Electric field relaxing material, and electric field relaxing member and electromagnetic coil using the same