Ceramic member

A ceramic member with a zirconium phosphate-silver coating film addresses antibacterial and antiviral deficiencies by ensuring even distribution and maintaining design integrity, achieving effective antibacterial and antiviral performance.

JP2024134012APending Publication Date: 2024-10-03LIXIL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023044077
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing ceramic members lack both effective antibacterial and antiviral properties, and the use of conductive zinc oxide particles results in poor performance, ease of detachment, and significant color differences, making them unsuitable for desirable design and functionality.

Method used

A ceramic member with a heat-cured coating film containing dispersed zirconium phosphate particles carrying silver, with a silver concentration of 0.1 to 2 parts by mass per 100 parts of the total solid content, ensuring even distribution and maintaining design integrity while providing antibacterial and antiviral properties.

Benefits of technology

The ceramic member achieves excellent antibacterial and antiviral performance, maintaining design integrity with minimal color difference, as evidenced by ΔE<3.0, and withstands durability and light resistance tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134012000001
    Figure 2024134012000001
  • Figure 2024134012000002
    Figure 2024134012000002
Patent Text Reader

Abstract

To provide a ceramic member that balances design with antibacterial and antiviral properties.SOLUTION: A ceramic member has a ceramic substrate that is coated with a thermally cured coating layer with dispersed silver-carrying zirconium phosphate particles. The coating layer has a silver content of 0.1 pt.mass or more and 2 pts.mass or less relative to 100 pts.mass of the total solid in the coating layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to ceramic components. [Background technology]

[0002] The surfaces of ceramic members used in washstands, toilets, etc. are required to have antibacterial properties in order to prevent staining by bacteria. To date, antibacterial agents capable of imparting antibacterial properties to the surfaces of ceramic members have been proposed.

[0003] In Patent Document 1, 100 kg / cm 2 The volume resistivity measured under pressure is 10 5 An antibacterial and antifungal agent is disclosed, which is characterized by being composed essentially of zinc oxide fine particles having electrical conductivity of Ω·cm or less, and further, it is disclosed that this antibacterial and antifungal agent can be suitably used as an additive for imparting antibacterial and antifungal properties to various industrial materials and industrial products, such as natural fibers, synthetic fibers, natural leather, synthetic leather, paper, films, resins, and paints. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-104823 A Summary of the Invention [Problem to be solved by the invention]

[0005] Simply fixing conductive zinc oxide to the surface of the substrate results in only conductive zinc oxide particles being dispersed on the surface of the substrate, resulting in low antibacterial performance. In addition, the conductive zinc oxide particles are easily shed from the surface of the substrate. It is also known to apply antibacterial agents such as conductive zinc oxide to the surface of the tile by shot peening, but this method is not economical because of the large dust collection loss and the consumption of the antibacterial agent. Furthermore, the presence of conductive zinc oxide particles on the surface of the substrate increases the color difference ΔE before and after the antibacterial property is imparted, which may impair the design.

[0006] When conductive zinc oxide is mixed into synthetic resin or paint, the conductive zinc oxide present inside the substrate does not contribute to the antibacterial effect or contributes very little to the antibacterial effect. In order to enhance the antibacterial effect, it is necessary to add a large amount of conductive zinc oxide. However, adding a large amount of conductive zinc oxide in this way may increase the color difference ΔE before and after the formation of the coating film, which may impair the design or impair the properties of the substrate.

[0007] Furthermore, while the antibacterial and antifungal agent described in Patent Document 1 has antibacterial properties, it does not have antiviral properties.

[0008] The present disclosure has been made in consideration of the above circumstances, and an object of the present disclosure is to provide a ceramic member that combines designability with antibacterial and antiviral properties. [Means for solving the problem]

[0009] The ceramic member of the present disclosure includes a ceramic substrate and a coating film formed by dispersing silver-loaded zirconium phosphate particles therein and curing the coating film by heat. The silver concentration of the coating film is 0.1 parts by mass or more and 2 parts by mass or less per 100 parts by mass of the total solid content of the coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present disclosure will be described in further detail below.

[0011] The ceramic member of the present disclosure comprises a coating film on a ceramic substrate, the coating film having silver-loaded zirconium phosphate particles dispersed therein and cured by heat, the silver concentration of the coating film being 0.1 to 2 parts by mass per 100 parts by mass of the total solid content of the coating film. In this ceramic member, the silver-loaded zirconium phosphate particles are dispersed in the coating film, the coating film is highly transparent, and the silver-loaded zirconium phosphate particles are evenly distributed on the substrate surface, so that the ceramic member has excellent designability, as well as excellent antibacterial and antiviral properties.

[0012] In the ceramic member of the present disclosure, the design is based on CIE1976 L * a * b * Color difference ΔE quantified using the color difference formula * The CIE1976 (also called CIELUV) is a color space adopted by the International Commission on Illumination (CIE) in 1976. In this specification and claims, ΔE * ab is sometimes simply written as ΔE.

[0013] In the ceramic member of the present disclosure, when ΔE<3.0, it is evaluated as having excellent design properties.

[0014] In the ceramic member of the present disclosure, the antibacterial properties are measured by carrying out a durability test (water resistance test and light resistance test) specified by SIAA (Society of Industrial Technology for Antibacterial Products), and then carrying out the antibacterial performance test method of ISO 22196:2011 (corresponding to JIS (Japanese Industrial Standard) JIS Z 2801:2012) to measure the antibacterial activity value R B The antibacterial activity value R is calculated and evaluated. B When the value is ≧2.0, it is evaluated as having excellent antibacterial properties.

[0015] In the ceramic member of the present disclosure, the antiviral property is measured by subjecting a ceramic member before or after treatment according to the durability test method specified by the SIAA to the antiviral test method of ISO 21702:2019 and measuring the antiviral activity value R after 24 hours of contact with a virus solution. V The antiviral activity value R is calculated and evaluated. V When the value is ≧2.0, it is evaluated as having excellent antiviral activity.

[0016] The water resistance test is a water resistance test of Category 1 (products that are subject to water splashes). Specifically, an accelerated test is performed under the test conditions of the water resistance test of the SIAA durability test method (2021 edition) (water temperature: room temperature, immersion time: 16 to 18 hours).

[0017] The light resistance test is a Category 1 (light resistance test for products with few opportunities for light exposure (products used indoors, etc.). Specifically, the test conditions for the light resistance test Category 1 of the SIAA durability test method (2021 edition) (xenon lamp (irradiance setting of 60 W / m in the wavelength range of 300 nm to 400 nm) 2 or equivalent setting) for 10±0.5 hours or sunlight (irradiance of 255 W / m in the wavelength range of 300 nm to 700 nm) 2 Accelerated testing is performed at 8 ± 0.4 hours exposure at 100 ± 10.0 °C.

[0018] In the ceramic member of the present disclosure, the post-abrasion antiviral property is measured by subjecting the ceramic member after the abrasion test to the antiviral test method of ISO 21702:2019 and measuring the antiviral activity value R after 24 hours of contact with a virus solution. V The antiviral activity value R is calculated and evaluated. V When the value is ≧2.0, it is evaluated as having excellent antiviral activity.

[0019] In the ceramic member of the present disclosure, the ceramic substrate is not particularly limited as long as it is a ceramic substrate such as a glass product (glass plate, glass craft, etc.), a fired tile base (glazed or unglazed), or an unglazed unfired tile base; however, any one selected from the group consisting of an unglazed fired tile base, a glazed fired tile base, and an unglazed unfired tile base is preferred, and a glazed fired tile base is more preferred.

[0020] In the ceramic member of the present disclosure, the coating film is a coating film in which silver-loaded zirconium phosphate particles are dispersed and which is cured by heat.

[0021] The silver-loaded zirconium phosphate particles (hereinafter also simply referred to as "silver-loaded zirconium phosphate particles") are obtained by substituting protons for lithium in crystalline lithium zirconium phosphate particles obtained by hydrothermal synthesis through acid treatment, further substituting protons for silver ions, drying, and firing at high temperature to load silver ions as part of the crystal structure. The silver-loaded zirconium phosphate particles have low oral acute toxicity and are negative for mutagenicity and skin irritation, making them extremely advantageous when the ceramic member of the present disclosure is used as an antibacterial and antiviral tile for a component of a washroom, bathroom, toilet, etc.

[0022] In the ceramic member of the present disclosure, the silver concentration of the coating film is from 0.1 to 2 parts by mass, preferably from 0.1 to 1.7 parts by mass, and more preferably from 0.1 to 1.4 parts by mass, relative to 100 parts by mass of the total solid content of the coating film. When the content of the silver-supported zirconium phosphate particles in the coating film is within the above range, the coating film has high transparency and does not impair the design, and can exhibit excellent antibacterial and antiviral properties.

[0023] The silver content of the silver-loaded zirconium phosphate particles (sometimes referred to as "silver loading amount") is not particularly limited, but is preferably 3 parts by mass or more and less than 20 parts by mass, more preferably 5 parts by mass or more and less than 18 parts by mass, and even more preferably 7 parts by mass or more and less than 16 parts by mass, relative to a total of 100 parts by mass of the silver-loaded zirconium phosphate particles, calculated as Ag2O. When the silver loading amount is within the above range, the design is less likely to be impaired, and more excellent antibacterial activity and antiviral activity tend to be exhibited.

[0024] The average particle size of the silver-supported zirconium phosphate particles is not particularly limited, but is preferably 0.3 μm to 10 μm, more preferably 0.3 μm to 5 μm, and even more preferably 0.3 μm to 1 μm. When the average particle size of the silver-supported zirconium phosphate is within the above range, the design is less likely to be impaired and more excellent antibacterial activity and antiviral activity tend to be exhibited.

[0025] The average particle size of the silver-supported zirconium phosphate particles is an average particle size measured by a laser diffraction / scattering type particle size distribution measuring instrument (NIKKISO Microtrack MT3000II).

[0026] The thickness of the coating film is not particularly limited, but is preferably 1 μm to 20 μm, more preferably 1 μm to 15 μm, and even more preferably 1 μm to 10 μm. When the thickness of the coating film is within the above range, the design is less likely to be impaired and more excellent antibacterial activity and antiviral activity tend to be exhibited.

[0027] A method for forming the coating film on the ceramic substrate, i.e., a method for producing a ceramic member according to the present disclosure, includes a method in which an organic composition for forming a thermosetting coating film, which contains the silver-supported zirconium phosphate particles and an organic binder, or an inorganic composition for forming a thermosetting coating film, which contains the silver-supported zirconium phosphate particles and an inorganic binder, is applied to the surface of the ceramic substrate to form a coating film, and the coating film is cured by heat.

[0028] The organic composition for forming a thermosetting coating film contains the silver-supported zirconium phosphate particles and an organic binder.

[0029] The organic binder is preferably a thermosetting polyurethane resin composition or a thermosetting polyester resin composition, more preferably a thermosetting polyurethane resin composition. The thermosetting polyurethane resin composition is, for example, a mixture containing a polyisocyanate compound and / or a urethane prepolymer and a polyol compound. The polyol is preferably a polyester polyol or a polyether polyol, more preferably a polyether polyol.

[0030] The content of the silver-supported zirconium phosphate particles in the organic composition for forming a thermosetting coating film is 10 parts by mass or more and 80 parts by mass or less, preferably 12 parts by mass or more and 75 parts by mass or less, and more preferably 15 parts by mass or more and 70 parts by mass or less, relative to 100 parts by mass of the total solid content of the organic composition for forming a thermosetting coating film. When the content of the silver-supported zirconium phosphate particles in the organic composition for forming a thermosetting coating film is within the above range, the coating film obtained by curing with heat has high transparency, does not impair design, and can exhibit excellent antibacterial and antiviral properties.

[0031] When the coating film is formed by thermal curing of the organic composition for forming a thermosetting coating film, the coating film has better abrasion resistance.

[0032] The inorganic composition for forming a thermosetting coating film contains the silver-supported zirconium phosphate particles and an inorganic binder.

[0033] The inorganic binder is preferably water glass, more preferably No. 3 or No. 4 sodium silicate water glass. Water glass is also called sodium silicate or soda silicate, and is not a single compound, but a liquid in which SiO2 (silicon dioxide) and Na2O (sodium oxide) are mixed in various ratios. The molecular formula is Na2O·nSiO2, where n is called the molar ratio and represents the number of moles of SiO2 per mole of Na2O.

[0034] The content of the silver-supported zirconium phosphate particles in the inorganic composition for forming a thermosetting coating film is 10 parts by mass or more and 80 parts by mass or less, preferably 12 parts by mass or more and 75 parts by mass or less, and more preferably 15 parts by mass or more and 70 parts by mass or less, relative to 100 parts by mass of the total solid content of the inorganic composition for forming a thermosetting coating film. When the content of the silver-supported zirconium phosphate particles in the inorganic composition for forming a thermosetting coating film is within the above range, the transparency of the coating film obtained by curing with heat is higher, the design is not impaired, and excellent antibacterial and antiviral properties can be exhibited.

[0035] When the coating film is formed by thermal curing of the inorganic composition for forming a thermosetting coating film, the coating film has better abrasion resistance.

[0036] The coverage of the surface of the ceramic substrate by the coating film is not particularly limited, but is preferably 5% or more, more preferably 25% or more, even more preferably 50% or more, and particularly preferably 90% or more. The higher the coverage, the easier it is for the ceramic member of the present disclosure to exhibit antibacterial and antiviral properties.

[0037] [Aspects of the present disclosure] The aspects of the present disclosure are as follows.

[0038] [1] A ceramic member comprising a ceramic substrate and a coating film, the coating film having silver-loaded zirconium phosphate particles dispersed therein, the coating film being cured by heat, the coating film having a silver concentration of 0.1 to 2 parts by mass per 100 parts by mass of the total solid content of the coating film.

[0039] [2] The ceramic member according to [1], wherein a content of the silver in the silver-loaded zirconium phosphate particles in the coating film, in terms of AgO, is 3 parts by mass or more and less than 20 parts by mass per 100 parts by mass of the silver-loaded zirconium phosphate particles in total.

[0040] [3] The ceramic member according to [1] or [2], wherein the coating film is formed by thermally curing an organic composition for forming a thermosetting coating film, the organic composition comprising the silver-loaded zirconium phosphate particles and an organic binder.

[0041] [4] The ceramic member according to any one of [1] to [3], wherein the coating film is formed by thermally curing an inorganic composition for forming a thermosetting coating film, the inorganic composition comprising the silver-loaded zirconium phosphate particles and an inorganic binder.

[0042] [5] The ceramic member according to any one of [1] to [4], wherein the average particle size of the silver-loaded zirconium phosphate particles is 0.3 μm or more and 10 μm or less.

[0043] [6] The ceramic member according to any one of [1] to [5], wherein the coating film has a thickness of 1 μm or more and 20 μm or less.

[0044] [7] The ceramic member according to any one of [1] to [6], wherein the coating film has a coverage of 5% or more of the surface of the ceramic substrate.

[0045] [8] The ceramic member according to any one of [1] to [7], wherein a color difference ΔE before and after forming the coating film on the ceramic base material is less than 3.

[0046] [9] Antiviral activity value R after 24 hours of contact with a virus solution containing one or more test viruses, either influenza virus or feline calicivirus, according to ISO 21702:2019 V ≧2.0.

[0047]

[10] Antiviral activity value R after 24 hours of contact with a virus solution containing at least one of the influenza virus or feline calicivirus test viruses according to ISO 21702:2019 after a water resistance test of water resistance test category 1 specified by the Japan Association of Antibacterial Products V≧2.0.

[0048]

[11] Antiviral activity value R after 24 hours of contact with a virus solution containing at least one of the influenza virus or feline calicivirus test viruses according to ISO 21702:2019 after light resistance test of light resistance test category 1 specified by the Japan Association of Antibacterial Products V ≧2.0.

[0049]

[12] The ceramic member according to any one of [1] to

[11] , which is a tile. EXAMPLES

[0050] The present disclosure will be described in more detail below by showing examples, but the present disclosure is not limited to the examples.

[0051] [material] Silver-loaded zirconium phosphate particles (Novalon AG1100, Toagosei Co., Ltd., silver content (Ag2O equivalent) 14.1% by mass, average particle size 1 μm) Ceramic base material (porcelain tile: LIXIL, Fosky exterior floor type) Urethane (TKA-260, Tokushiki) Water glass (No. 3 sodium silicate, Fuji Chemical Co., Ltd.) ·Silane coupling agent (KBE-903, Shin-Etsu Chemical Co., Ltd.) · Hardener (TKA CURING AGENT, manufactured by Tokushiki Co., Ltd.) Discoloration prevention agent (Discoloration prevention agent for Novalon, manufactured by Toagosei Co., Ltd.) Dispersant (Polysol AP-1100, manufactured by Resonac)

[0052] [Examples 1 to 6] Examples 1 and 6 are comparative examples, and Examples 2 to 5 are working examples.

[0053] Water, silver-loaded zirconium phosphate particles, urethane resin, curing agent, and silane coupling agent were mixed in the amounts shown in Table 1 to prepare an organic composition for forming a coating film.

[0054] The prepared organic composition for forming a coating was applied to the surface of each ceramic substrate at a rate of 33 g / m. 2 (solid content of 1.2% or more and 3.0% or less (by mass)) was spray-coated and dried to form a coating film. In this manner, each test specimen was prepared.

[0055] Using each of the prepared test specimens, antibacterial and antiviral tests, antiviral tests after abrasion, and color difference measurements were performed to evaluate the antibacterial and antiviral properties, antiviral properties before and after abrasion, and changes in appearance. The evaluation results are shown in Table 1.

[0056] (Antibacterial evaluation) Antibacterial activity value R according to the antibacterial test method of ISO 22196:2011 B was determined and evaluated according to the following criteria.

[0057] 4.0≦R B A (has particularly excellent antibacterial properties) 2.0≦R B <4.0 B (Excellent antibacterial properties) 0 <R B ≦2.0 ···C (has antibacterial properties) R B =0 ···D (no antibacterial properties)

[0058] (Antiviral evaluation) Antiviral activity value R according to the ISO 21702:2019 antiviral test method V was determined and evaluated according to the following criteria.

[0059] 4.0≦R V A (has particularly excellent antibacterial properties) 2.0≦R V <4.0 B (Excellent antibacterial properties) 0 <R V ≦2.0 ···C (has antibacterial properties) R V =0 ···D (no antibacterial properties)

[0060] (Evaluation of antiviral properties after abrasion) After the abrasion test, the test specimen was evaluated for antiviral activity R according to the ISO 21702:2019 antiviral test method. V was determined and evaluated according to the following criteria.

[0061] 4.0≦R V A (has particularly excellent antibacterial properties) 2.0≦R V <4.0 B (Excellent antibacterial properties) 0 <R V ≦2.0 ···C (has antibacterial properties) R V =0 ···D (no antibacterial properties)

[0062] (Evaluation of appearance changes) The ΔE before and after the formation of the coating film was determined by measuring the L*a*b* values ​​using a color difference meter (KONICA MINOLTA CR-400) and was evaluated according to the following criteria.

[0063] ΔE<3.0 ···A (Excellent design) ΔE≧3.0 D (poor design)

[0064] [Table 1]

[0065] [Results explanation] The specimens of Examples 2 to 5, which are working examples, were excellent in the evaluations of antibacterial property, antiviral property, antiviral property after abrasion, and appearance change. In contrast, the specimen of Comparative Example 1 had a silver concentration of the coating film less than 0.1 parts by mass relative to 100 parts by mass of the total solid content of the coating film, and was poor in the evaluations of antiviral property and antiviral property after abrasion. The specimen of Comparative Example 6 had a silver concentration of the coating film more than 2 parts by mass relative to 100 parts by mass of the total solid content of the coating film, and was poor in the evaluation of appearance change.

[0066] [Examples 7 to 12] Examples 7 and 12 are comparative examples, and Examples 8 to 11 are working examples.

[0067] Water, silver-supported zirconium phosphate particles, water glass, a discoloration inhibitor, and a dispersant were mixed in the amounts shown in Table 2 to prepare an inorganic composition for forming a coating film.

[0068] The prepared inorganic composition for forming a coating film was sprayed onto the surface of each ceramic substrate at room temperature and dried. After drying, the substrate was heated at 520°C in an air atmosphere for 30 minutes to form a coating film. In this manner, each test specimen was prepared.

[0069] Using each of the prepared test specimens, antibacterial tests, antiviral tests, antiviral tests after abrasion, and color difference measurements were performed in the same manner as in Examples 1 to 6, and the antibacterial properties, antiviral properties before and after abrasion, and changes in appearance were evaluated. The evaluation results are shown in Table 2.

[0070] [Table 2]

[0071] [Results explanation] The specimens of Examples 8 to 11, which are working examples, were excellent in the evaluations of antibacterial property, antiviral property, antiviral property after abrasion, and appearance change. In contrast, the specimen of Comparative Example 7 had a silver concentration of the coating film less than 0.1 parts by mass relative to 100 parts by mass of the total solid content of the coating film, and was poor in the evaluations of antibacterial property, antiviral property, and antiviral property after abrasion. The specimen of Comparative Example 12 had a silver concentration of the coating film more than 2 parts by mass relative to 100 parts by mass of the total solid content of the coating film, and was poor in the evaluation of appearance change.

Claims

1. A ceramic member comprising a ceramic substrate and a coating film, the coating film having silver-loaded zirconium phosphate particles dispersed therein and cured by heat, the coating film having a silver concentration of 0.1 parts by mass or more and 2 parts by mass or less per 100 parts by mass of a total of solid contents of the coating film.

2. The silver content of the silver-loaded zirconium phosphate particles in the coating film is Ag 2 2. The ceramic member according to claim 1, wherein the amount of silver-supporting zirconium phosphate particles is 3 parts by mass or more and less than 20 parts by mass, calculated as O, relative to a total of 100 parts by mass of the silver-supporting zirconium phosphate particles.

3. 3. The ceramic member according to claim 1, wherein the coating film is formed by thermally curing an organic composition for forming a thermosetting coating film, the organic composition comprising the silver-loaded zirconium phosphate particles and an organic binder.

4. 3. The ceramic member according to claim 1, wherein the coating film is formed by thermally curing an inorganic composition for forming a thermosetting coating film, the inorganic composition comprising the silver-loaded zirconium phosphate particles and an inorganic binder.

5. 3. The ceramic member according to claim 1, wherein the silver-loaded zirconium phosphate particles have an average particle size of 0.3 μm or more and 10 μm or less.

6. 3. The ceramic member according to claim 1, wherein the coating has a thickness of 1 μm or more and 20 μm or less.

7. 3. The ceramic member according to claim 1, wherein the coating film has a coverage of 5% or more of the surface of the ceramic substrate.

8. The ceramic member according to claim 1 or 2, wherein a color difference ΔE before and after forming the coating film on the ceramic substrate is less than 3.

9. Antiviral activity value R after 24 hours of contact with a virus solution containing one or more test viruses, either influenza virus or feline calicivirus, according to ISO 21702:2019 V 3. The ceramic part according to claim 1 or 2, wherein the σ is ≧2.

0.

10. Antiviral activity value R after 24 hours of contact with a virus solution containing at least one of the influenza virus or feline calicivirus according to ISO 21702:2019 after water resistance test of water resistance test category 1 specified by the Japan Association of Antibacterial Products V 3. The ceramic part according to claim 1 or 2, wherein the σ is ≧2.

0.

11. Antiviral activity value R after 24 hours of contact with a virus solution containing at least one of the influenza virus or feline calicivirus according to ISO 21702:2019 after light resistance test of light resistance test category 1 specified by the Japan Association of Antibacterial Products V 3. The ceramic part according to claim 1 or 2, wherein the σ is ≧2.

0.

12. 3. The ceramic part according to claim 1 or 2, which is a tile.

Citation Information

Patent Citations

  • Antimicrobial porcelain or enameled product

    JP1995165478A

  • Precursor composition for producing glassy membrane and its production

    JP1998036719A

  • Antistatic resin composition

    JP2017114927A

  • Coating composition, coating film, and article

    JP2022050830A

  • Antiviral agent, coating composition, resin composition and antiviral product

    WO2017150063A1