Phenoxy resin ionomer, composition containing the same, resin film, powder, and method for producing phenoxy resin ionomer and method for producing resin film

By acid-modifying and ionomerizing phenoxy resin with metal ions, the resin's heat and solvent resistance are enhanced, addressing the limitations of conventional phenoxy resins and expanding its industrial applications.

JP2024134158APending Publication Date: 2024-10-03NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023044307
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional phenoxy resins lack sufficient heat resistance and solvent resistance, and their properties degrade in high-temperature environments, limiting their applications due to poor mechanical properties and adhesion.

Method used

The phenoxy resin is acid-modified and ionomerized by neutralizing part or all of its acidic functional groups with metal ions, forming ionic crosslinks that enhance heat and solvent resistance while maintaining flexibility and adhesion.

Benefits of technology

The resulting phenoxy resin ionomer exhibits improved heat resistance, solvent resistance, and mechanical strength, enabling applications in various industrial products such as insulating films, adhesive films, and composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134158000006
    Figure 2024134158000006
  • Figure 2024134158000007
    Figure 2024134158000007
  • Figure 2024134158000001
    Figure 2024134158000001
Patent Text Reader

Abstract

To improve heat resistance and solvent resistance without impairing features of a phenoxy resin.SOLUTION: There is provided a phenoxy resin ionomer in which a part or all of acidic functional groups contained in an acid-modified phenoxy resin having an acid modification ratio of 10 to 80% by the acidic functional groups are neutralized by metallic ions. The acidic functional group is preferably a carboxyl group, and the acid-modified phenoxy resin is preferably a carboxylic acid-modified phenoxy resin. As for the phenoxy resin ionomer, a neutralization ratio calculated by numeric expression (1) is preferably within a range of 10 to 80%. Expression (1): Neutralization rate (%)=[Vm×Mm÷Mf]×100. In the expression (1), Vm represents a valence of metallic ions, Mm represents a content (mol number) of metallic ions in a metallic compound, and Mf represents a content (mol number) of the acidic functional groups in the acid-modified phenoxy resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a phenoxy resin ionomer that can be used in various industrial products, a composition, a resin film, and a powder containing the same, as well as a method for producing the phenoxy resin ionomer and a method for producing a resin film. [Background technology]

[0002] Thermoplastic polyhydroxy polyether resins are known as phenoxy resins, and because of their excellent flexibility, impact resistance, and adhesion, they are used in a wide range of applications in the electronics field, such as insulating films and adhesive films. They have also been used as matrix resins for fiber-reinforced composite materials to improve their mechanical properties and adhesion to carbon fibers. However, conventional phenoxy resins have the disadvantage that, due to their characteristics as thermoplastic resins, they do not have sufficient heat resistance or mechanical properties, and their adhesion rapidly decreases in high-temperature environments. In addition, since phenoxy resins are easily dissolved by organic solvents, there has been a demand for improved solvent resistance.

[0003] Methods have been developed to solve these problems with phenoxy resin by forming crosslinks. For example, it is known that crosslinking phenoxy resin with excellent thermal stability can be obtained by using an acid anhydride as a crosslinking agent to crosslink the secondary hydroxyl groups of phenoxy resin.

[0004] In Patent Document 1, a crosslinked phenoxy resin with excellent heat resistance is synthesized by reacting an acid anhydride-modified phenoxy resin obtained by reacting a phenoxy resin with an acid anhydride with a crosslinking agent having two or more functional groups in the molecule that can react with the acid anhydride group to polymerize the acid anhydride-modified phenoxy resin.

[0005] In Patent Document 2, a solvent-free phenoxy resin composition obtained by dry blending a phenoxy resin with a crosslinking agent is molded in advance, and then heated to crosslink the hydroxyl groups of the phenoxy resin with the crosslinking agent, thereby synthesizing a crosslinked phenoxy resin with excellent heat resistance. In Patent Document 2, heat resistance is improved by crosslinking, but a crosslinked phenoxy resin is not obtained in a varnish containing an organic solvent.

[0006] By the way, ion-crosslinkable resins called ionomers, which crosslink polymers using metal compounds, are known. Patent Document 3 discloses an ionomer composition obtained by reacting an olefin polymer having at least one functional group selected from an acid group and an acid anhydride group with a metal compound. In addition, Non-Patent Document 1 discloses a phenoxy resin ionomer, but it examines the use of the ionomer as a curing catalyst for epoxy resin to make it Tg-less, and does not disclose adhesion or solvent resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 11-135901 [Patent Document 2] International Publication WO2014 / 157132 [Patent Document 3] JP 2020-158682 A [Non-patent literature]

[0008] [Non-Patent Document 1] Hirofumi Nishida, Satoshi Matsuda, Hajime Kishi, and Jun Murakami, "Tg-less epoxy resin using ion-containing polymer as a curing catalyst" Journal of the Adhesion Society of Japan Vol. 42 No. 1 (2006) Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to improve the heat resistance and solvent resistance of phenoxy resin without impairing the characteristics of the resin. [Means for solving the problem]

[0010] As a result of extensive research, the present inventors have found that heat resistance and solvent resistance can be improved by modifying a phenoxy resin with an acid and then ionomerizing it with a metal ion, and have thus completed the present invention.

[0011] That is, the phenoxy resin ionomer of the present invention is an acid-modified phenoxy resin having an acid modification rate of 10 to 80% by acidic functional groups, and the acidic functional groups contained therein are partially or entirely neutralized with metal ions.

[0012] In the phenoxy resin ionomer of the present invention, the acidic functional group may be a carboxyl group, and the acid-modified phenoxy resin may be a carboxylic acid-modified phenoxy resin.

[0013] In the phenoxy resin ionomer of the present invention, the metal ions may be derived from a metal compound, and the neutralization rate calculated by the following formula (1) may be within the range of 10 to 80%. Neutralization rate (%)=[V m ×M m ÷Mf]×100 … Formula (1) [Here, Vm means the valence of the metal ion, Mm means the content (number of moles) of the metal ion in the metal compound, and Mf means the content (number of moles) of the acidic functional group in the acid-modified phenoxy resin.]

[0014] The phenoxy resin ionomer composition of the present invention contains the above-mentioned phenoxy resin ionomer and an organic solvent.

[0015] The phenoxy resin ionomer composition of the present invention is characterized in that the organic solvent is capable of dissolving the carboxylic acid-modified phenoxy resin and satisfies the following condition (1) or condition (2): Condition (1): The metal carboxylate, which is a precursor of the metal ion, is soluble. Or, Condition (2): Compatible with alcohols having 1 to 3 carbon atoms. At least one of the above conditions may be satisfied.

[0016] The resin film of the present invention contains the above-mentioned phenoxy resin ionomer.

[0017] The powder of the present invention contains the above-mentioned phenoxy resin ionomer.

[0018] The method for producing the phenoxy resin ionomer of the present invention comprises the following steps i) and ii); i) a step of reacting a secondary hydroxyl group of a phenoxy resin with an acidic functional group donating compound in a polar solvent to produce an acid-modified phenoxy resin having an acid modification rate in the range of 10 to 80%; and ii) ionomerizing the acid-modified phenoxy resin by adding a metal compound dissolved in a polar solvent to the acid-modified phenoxy resin; Contains:

[0019] In the method for producing a phenoxy resin ionomer of the present invention, the acidic functional group-donating compound may be a carboxylic acid anhydride compound represented by the following general formula (1) or general formula (2).

[0020] [ka]

[0021] In general formula (1) and general formula (2), the groups R are each independently a hydrogen atom, a hydrocarbon group, a halogen atom, an alkoxy group, an ester group, a cyano group, an amide group, an imide group, a silyl group, a carboxyl group, or a hydrocarbon group substituted with a polar group, and the polar group is a halogen atom, an alkoxy group, an ester group, a nitro group, a cyano group, an amide group, an imide group, or a silyl group.

[0022] The method for producing a resin film of the present invention comprises the following steps I) and II); I) a step of casting the phenoxy resin ionomer composition to form a coating film; and II) drying the coating film; In this case, in the step II), vacuum drying may be carried out after the heat drying. Effect of the Invention

[0023] The phenoxy resin ionomer of the present invention has improved heat resistance and chemical resistance while maintaining the practically sufficient shear strength and transparency that are characteristic of phenoxy resins. In addition, the phenoxy resin ionomer of the present invention can be made into various forms such as a varnish-like composition, a resin film, and a powder. Therefore, it is easy to apply to various uses, and can be used in many industrial products such as insulating films, adhesive films, matrix resins for fiber-reinforced composite materials, composite materials of metals and resins suitable for automobile parts, vibration-damping members for steel materials, packaging films, containers, and sporting goods. [Brief description of the drawings]

[0024] [Figure 1] FIG. 2 is a diagram showing infrared absorption spectra (IR) of the resin films produced in the Examples and Comparative Examples before vacuum drying. [Diagram 2] FIG. 2 is a diagram showing infrared absorption spectra (IR) of the resin films produced in the Examples and Comparative Examples after vacuum drying. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Next, an embodiment of the present invention will be described.

[0026] [Phenoxy resin ionomer] The phenoxy resin ionomer of the present invention is an acid-modified phenoxy resin in which the acid modification rate by the acid functional groups is within the range of 10 to 80%, and a part or all of the acid functional groups contained therein are neutralized with metal ions. Here, the term "ionomer" refers to an ionic polymer material in which metal ions are introduced into the polymer chain. The ionomer has the characteristic that the introduced ions form ionic bond crosslinks, while at the same time, it has fluidity due to dissociation of the ionic bonds in the high temperature range.

[0027] <Acid-modified phenoxy resin> Acid-modified phenoxy resin is a phenoxy resin in which the secondary hydroxyl group has been modified with a compound capable of donating an acidic functional group (acidic functional group donating compound). Phenoxy resin, the raw material for acid-modified phenoxy resin, is an amorphous thermoplastic resin obtained by the condensation reaction of a dihydric phenol compound with epihalohydrin, or the polyaddition reaction of a dihydric phenol compound with a difunctional epoxy resin. Phenoxy resin is also known as polyhydroxy polyether resin or thermoplastic epoxy resin.

[0028] The raw material phenoxy resin can be obtained by a conventionally known method in solution or without solvent.

[0029] The weight average molecular weight (Mw) of the raw material phenoxy resin is usually within the range of 10,000 to 200,000, preferably within the range of 20,000 to 100,000, and more preferably within the range of 30,000 to 80,000. If Mw is too low, the strength when ionomerized is likely to be insufficient, and if it is too high, the workability and processability are likely to be poor. Note that Mw is a value measured by gel permeation chromatography (GPC) and converted using a standard polystyrene calibration curve.

[0030] The hydroxyl equivalent (g / eq) of the raw material phenoxy resin is usually within the range of 50 to 1000, preferably within the range of 50 to 750, and particularly preferably within the range of 50 to 500. If the hydroxyl equivalent is too low, the number of hydroxyl groups that can be acid-modified increases, so it is necessary to set the acid modification rate low, whereas if the hydroxyl equivalent is too high, the number of hydroxyl groups that can be acid-modified decreases, so it is necessary to set the acid modification rate high.

[0031] The glass transition temperature (Tg) of the raw material phenoxy resin is suitably within the range of, for example, 65° C. to 160° C., and preferably within the range of 70° C. to 150° C. The glass transition temperature can be measured by the method described in the Examples below.

[0032] Examples of the raw material phenoxy resin include, but are not limited to, bisphenol A type phenoxy resin (e.g., trade names Phenotohto YP-50, YP-50S, YP-55U manufactured by Nippon Steel Chemical & Material Co., Ltd., PKHH and PKHB manufactured by HUNTSMAN, and YX7200B35 manufactured by Mitsubishi Chemical Corporation), bisphenol F type phenoxy resin (e.g., trade name Phenotohto FX-316 manufactured by Nippon Steel Chemical & Material Co., Ltd.), copolymer type phenoxy resin of bisphenol A and bisphenol F (e.g., trade name YP-70 manufactured by Nippon Steel Chemical & Material Co., Ltd.), and special phenoxy resin (e.g., trade names Phenotohto YPB-43C, FX293, FX280S, etc. manufactured by Nippon Steel Chemical & Material Co., Ltd.), and these can be used alone or in combination of two or more kinds. In the present invention, it is preferable to use a polymerized polyhydroxypolyether resin generally called a phenoxy resin as the phenoxy resin, but it may also be an in-situ polymerization type phenoxy resin polymerized to the same average molecular weight as the above (for example, 40,000 to 50,000 in weight average molecular weight). Among these phenoxy resins, bisphenol A type phenoxy resin or copolymer type phenoxy resin of bisphenol A and bisphenol F is more preferably used.

[0033] The acid-modified phenoxy resin has an acidic functional group. Examples of the acidic functional group include a carboxyl group, a sulfo group, a phosphoric acid group, and a phenolic hydroxyl group, but considering industrial production, a carboxyl group is preferred. In addition, as the acidic functional group-donating compound, it is preferable to use a carboxylic acid anhydride compound such as maleic anhydride, acetic anhydride, and succinic anhydride. As the carboxylic acid anhydride compound, for example, phthalic anhydride and its derivatives represented by the following general formula (1), or cyclohexyl phthalic anhydride and its derivatives represented by the general formula (2) are preferred.

[0034] [ka]

[0035] In general formula (1) and general formula (2), the groups R are each independently a hydrogen atom, a hydrocarbon group, a halogen atom, an alkoxy group, an ester group, a cyano group, an amide group, an imide group, a silyl group, a carboxyl group, or a hydrocarbon group substituted with a polar group, and the polar group is a halogen atom, an alkoxy group, an ester group, a nitro group, a cyano group, an amide group, an imide group, or a silyl group.

[0036] The acid-modified phenoxy resin has an acid-modified ratio of, for example, 10 to 80%, preferably 20 to 60%. If the acid-modified ratio is less than 10%, the number of crosslinking points due to reaction with metal ions is reduced, so that the properties of the ionomer cannot be fully expressed. If the acid-modified ratio exceeds 80%, the acid-modified phenoxy resin is likely to gel in the varnish state, significantly reducing the handling properties, and the various properties inherent to the phenoxy resin, such as flexibility, impact resistance, and adhesion, may be impaired, and in particular, there is a concern that the shear strength of the phenoxy resin ionomer may be significantly reduced compared to that of the phenoxy resin.

[0037] The acid modification rate means the amount (mol%) of the acidic functional group donating compound added to the total amount (moles) of secondary hydroxyl groups in the phenoxy resin. Specifically, for example, an acid modification rate of "20%" means that the acidic functional group donating compound was added so that the acidic functional group is 20 mol% relative to the total amount (moles) of secondary hydroxyl groups in the phenoxy resin.

[0038] <Metal ions> The metal species constituting the metal ion can be appropriately selected from, for example, alkali metals, alkaline earth metals, transition metals, etc. In addition, preferred metal species include, for example, lithium, sodium, potassium, magnesium, calcium, strontium, aluminum, titanium, zirconium, zinc, copper, iron, barium, gold, etc. In addition, the metal ion may be either a monovalent ion or a polyvalent ion having a valence of two or more, and two or more kinds of metal ions having different types or valences may be used in combination.

[0039] The metal ions can be prepared from metal compounds such as metal salts, metal oxides, metal hydroxides, and metal complexes such as alkoxides. In particular, it is preferable to use metal carboxylates such as acetates, formates, and oxalates.

[0040] <Neutralization rate> In the phenoxy resin ionomer, a part or all of the acid functional groups of the acid-modified phenoxy resin are neutralized with metal ions derived from a metal compound. The neutralization rate can be calculated by the following formula (1). Neutralization rate (%)=[V m ×M m ÷Mf]×100 … Formula (1) Here, Vm means the valence of the metal ion, Mm means the content (number of moles) of the metal ion in the metal compound, and Mf means the content (number of moles) of the acidic functional group in the acid-modified phenoxy resin.

[0041] The neutralization rate is preferably within the range of 10 to 80%, more preferably within the range of 20 to 70%, and even more preferably within the range of 25 to 60%. In this case, the prerequisite acid modification rate is preferably within the range of 10 to 80%. Within this range of acid modification rate, if the neutralization rate is below 10%, the number of crosslinking points by metal ions decreases, and the properties as an ionomer cannot be fully expressed. Within the range of the acid modification rate, if the neutralization rate exceeds 80%, various properties inherent to the phenoxy resin, such as flexibility, impact resistance, and adhesion, may be impaired, and if the neutralization rate is 100%, a decrease in shear strength, a decrease in chemical resistance, and a poor appearance due to a decrease in transparency may occur.

[0042] The neutralization rate refers to the amount (mol%) of the metal compound added to the total amount (moles) of acidic functional groups in the acid-modified phenoxy resin. For example, when the valence of the metal ion is 1, a neutralization rate of "50%" means that the metal compound was added so that the metal ion is 50 mol% of the total amount (moles) of acidic functional groups contained in the acid-modified phenoxy resin. Therefore, for example, when the acid modification rate is "20%, " the neutralization rate is "50%", this means that the acid-modified phenoxy resin obtained by adding an acidic functional group-donating compound so that the acidic functional groups are 20 mol% relative to the total amount (number of moles) of secondary hydroxyl groups in the phenoxy resin is deemed to have 20 mol% acidic functional groups, and a metal compound was added so that the acidic functional groups are 50 mol% relative to the total amount (number of moles) of the acidic functional groups.

[0043] The weight ratio of the metal ions contained in the phenoxy resin ionomer of the present invention is preferably within the range of 0.1 to 20% by weight, more preferably within the range of 0.5 to 15% by weight. If the weight ratio of the metal ions is less than 0.1%, the crosslinking points due to the metal ions are reduced, and the properties of the ionomer cannot be fully expressed. If the weight ratio of the metal ions exceeds 20%, the various properties inherent to the phenoxy resin, such as flexibility, impact resistance, and adhesion, may be impaired.

[0044] <Production method of phenoxy resin ionomer> The phenoxy resin ionomer of the present invention can be produced by acid-modifying a phenoxy resin with an acidic functional group-donating compound and then reacting it with a metal compound. Here, an example is described in which a carboxylic anhydride compound is used as the acidic functional group-donating compound to modify the phenoxy resin.

[0045] Process i): In step i), a carboxylic acid-modified phenoxy resin having an acid modification rate of 10 to 80% is produced by reacting a secondary hydroxyl group of the phenoxy resin with a carboxylic anhydride compound in a polar solvent. If the acid modification rate is below 10%, the number of crosslinking points due to the reaction with metal ions in the next step ii) is reduced, and the properties of the ionomer cannot be fully expressed. On the other hand, if the acid modification rate exceeds 80%, the acid-modified phenoxy resin is likely to gel in the varnish state, significantly reducing the handleability, and various properties inherent to the phenoxy resin, such as flexibility, impact resistance, and adhesion, may be impaired. In particular, there is a concern that the shear strength of the phenoxy resin ionomer will be significantly reduced compared to that of the phenoxy resin.

[0046] Step i) is preferably carried out in the presence of a catalyst. The catalyst used in step i) is preferably a catalyst that does not have active hydrogen, such as a tertiary amine. If the catalyst becomes a crosslinking point or has too high nucleophilicity, the acid-modified phenoxy resin or the phenoxy resin ionomer may gel at high temperatures. Specific examples of preferred catalysts include dimethylaminopyridine (DMAP) and 9-azajulolidine.

[0047] Specific examples of the polar solvent used in step i) include diethylene glycol dimethyl ether (MDM; diglyme), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), dimethylsulfoxide (DMSO), tetrahydrofuran (THF), triglyme, dioxane, ethylene glycol monomethyl ether, acetone, etc. Two or more of these solvents can also be used in combination.

[0048] In step i), the reaction is preferably heated to, for example, within a range of 80 to 120° C. If the reaction temperature is less than 80° C., the reaction time will be extended, and if it exceeds 120° C., condensation of COOH groups and OH groups will proceed, which may cause gelation.

[0049] Step ii): In step ii), a metal compound dissolved in a polar solvent is added to the carboxylic acid-modified phenoxy resin synthesized in step i), thereby ionomerizing the carboxylic acid-modified phenoxy resin.

[0050] The polar solvent used in step ii) is preferably the same polar solvent as that in step i) or an alcohol-based solvent. Specific examples of the alcohol-based solvent are preferably lower alcohols having 1 to 4 carbon atoms, such as methanol, ethanol, propanol, and butanol.

[0051] In step ii), the reaction is preferably heated to, for example, within a range of 40 to 100° C. If the reaction temperature is less than 40° C., the reaction time will be too long, and if the reaction temperature exceeds 100° C., the alcohol will volatilize rapidly and the metal ions will precipitate as salts before reacting. Incidentally, step ii) can be carried out following step i). That is, a metal compound dissolved in a polar solvent such as an alcohol-based solvent can be added to a solution of the carboxylic acid-modified phenoxy resin containing the catalyst and solvent used in step i). However, since residual catalyst can cause gelation, a purification step for removing the catalyst may be carried out after step i) and before step ii).

[0052] A phenoxy resin ionomer can be synthesized by carrying out the above steps i) and ii). The outline of the synthesis reaction when using Phenotohto YP-50S (trade name), a bisphenol A type phenoxy resin manufactured by Nippon Steel Chemical & Material Co., Ltd., as the raw phenoxy resin is as follows. Here, n indicates the number of repeating units, M indicates a metal atom, M +means a metal ion.

[0053] [ka]

[0054] In step i), the reaction is carried out from the raw material Fenotote YP-50S to its carboxylic acid modified product YPS-COOH. The carboxylic acid modified product YPS-COOH may contain -OH groups that are not modified with carboxylic acid, but these are omitted here. In step ii), the phenoxy resin ionomer YPS-COO-M is synthesized from the carboxylic acid modified product YPS-COOH. In the phenoxy resin ionomer, the metal ion M + An ionic bridge is formed via the

[0055] The synthesized phenoxy resin ionomer can be confirmed by infrared absorption spectroscopy (IR) as shown in the examples below. Specifically, the C=O stretching vibration peak of -COOH (1715 cm -1 ) and -COO·M + C=O stretching vibration peak (1567cm -1 ) indicates the synthesis of phenoxy resin ionomer from carboxylic acid modified phenoxy resin.

[0056] In addition, if there is a large amount of unreacted -COOH in the phenoxy resin ionomer, it is likely to cause gelation, so it is preferable to reduce this amount. The amount of unreacted -COOH cannot be determined from the neutralization rate based on the amount of metal compound added. For example, the C=O stretching vibration peak of -COOH (1720 cm) in the infrared absorption spectrum (IR) is not known. -1 ) and -COO·M + C=O stretching vibration peak (1560cm -1 ) the remaining amount of unreacted -COOH can be estimated.

[0057] In addition, by vacuum drying the obtained solution containing the phenoxy resin ionomer, it is possible to reduce the unreacted -COOH in the phenoxy resin ionomer while maintaining the ionomer skeleton, which is effective in preventing gelation.

[0058] The phenoxy resin ionomer has a higher glass transition temperature (Tg) than the raw material phenoxy resin. For example, the Tg is higher within a range of +5 to +50°C than the raw material phenoxy resin. Therefore, the phenoxy resin ionomer has improved heat resistance compared to the raw material phenoxy resin. Furthermore, the phenoxy resin ionomer also improves chemical resistance by forming ion associations due to aggregation of ions.

[0059] <Phenoxy resin ionomer composition> The phenoxy resin ionomer composition contains the phenoxy resin ionomer of the present invention and an organic solvent. The organic solvent is one which can dissolve the carboxylic acid-modified phenoxy resin and which satisfies the following condition (1) or condition (2): Condition (1): The metal carboxylate, which is a precursor of the metal ion, is soluble. Or, Condition (2): Compatible with alcohols having 1 to 3 carbon atoms. It is preferable that at least one of the above conditions is satisfied.

[0060] Specific examples of organic solvents that dissolve the carboxylic acid-modified phenoxy resin and satisfy condition (1) include dimethyl sulfoxide (DMSO), N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and tetrahydrofuran (THF). Specific examples of organic solvents that dissolve the carboxylic acid-modified phenoxy resin and satisfy condition (2) include diethylene glycol dimethyl ether (MDM; diglyme), dimethyl sulfoxide (DMSO), N-methyl-2-pyrrolidone (NMP), ethanol, and methanol. Among the above organic solvents, dimethyl sulfoxide (DMSO) is particularly preferable since it satisfies both the condition (1) and the condition (2).

[0061] The phenoxy resin ionomer composition can be produced by mixing the phenoxy resin ionomer with an organic solvent. The organic solvent used in the polymerization reaction can be used as it is as the organic solvent. The content of the organic solvent is not particularly limited, but it is preferable to adjust the concentration of the phenoxy resin ionomer to about 10 to 60% by weight.

[0062] The phenoxy resin ionomer composition may contain, as optional components, for example, organic fillers, inorganic fillers, plasticizers, pigments, flame retardants, dyes, surfactants, coupling agents, UV absorbing agents, short fibers, nanocarbons, and the like.

[0063] <Resin film> The resin film of the present invention contains a phenoxy resin ionomer. The resin film also includes a sheet-shaped one. The resin film preferably contains more than 50% by weight of the phenoxy resin ionomer based on the total resin components, more preferably 70% by weight or more, and even more preferably 80% by weight or more. The entire resin components may be made of the phenoxy resin ionomer of the present invention.

[0064] The resin film may contain optional components, such as organic fillers, inorganic fillers, plasticizers, pigments, flame retardants, dyes, surfactants, coupling agents, UV absorbing agents, short fibers, and nanocarbons.

[0065] The thickness of the resin film can be appropriately set depending on the application, but for example, it can be in the range of 1 to 500 μm when used as an insulating film or an adhesive film. The resin film may be laminated on a substrate such as a metal foil, a glass plate, or a resin film made of a material other than phenoxy resin ionomer.

[0066] The resin film preferably has a shear strength of 15 MPa or more, more preferably in the range of 17 to 25 MPa, as measured by the method described in the Examples below. A shear strength of 15 MPa or more allows the film to be used in various industrial products, such as insulating films, adhesive films, matrix resins for fiber-reinforced composite materials, composite materials of metal and resin, packaging films, containers, and sporting goods.

[0067] <Method of manufacturing resin film> The resin film of the present invention can be produced by a known method. When a phenoxy resin ionomer composition is used, the resin film can be produced, for example, by carrying out the following steps I) and II).

[0068] Process I): In step I, the phenoxy resin ionomer composition is cast onto any supporting substrate to form a coating film. The method of coating onto the supporting substrate is not particularly limited, and can be performed using a coater such as a comma, die, knife, or lip coater.

[0069] Process II): In step II), the coating film obtained in step I) is dried. Drying can be performed by a known method, for example, drying with a hot plate, vacuum drying, hot air drying, or the like.

[0070] When heat drying is performed at normal pressure in step II), it is preferable to heat to a temperature in the range of, for example, 80 to 180° C. If the drying temperature is less than 80° C., it takes too long to dry, and if it exceeds 180° C., gelation may occur. To obtain a film with good appearance, vacuum drying is suitable. The vacuum drying is preferably carried out in a vacuum oven at a pressure of 0.095 MPa or less, a temperature of 50 to 180° C., and a time of 10 to 300 minutes. If the temperature is below 50°C, it will take too long to dry, and if it exceeds 180°C, gelation may occur.

[0071] In step II), the coating may be dried in two stages. For example, the coating may be dried by heating on a hot plate at normal pressure, followed by vacuum drying in a vacuum oven. The two-stage drying is effective for reducing the amount of unreacted -COOH remaining in the phenoxy resin ionomer and suppressing gelation.

[0072] <Powder> The powder of the present invention contains a phenoxy resin ionomer. By forming it in a powder form, it becomes possible to attach it to a fiber material by, for example, powder coating, and it becomes easy to apply it as a matrix resin for fiber reinforced plastic (FRP). The powder of the present invention can be produced by pulverizing a solidified product obtained by removing the solvent from a varnish containing the synthesized phenoxy resin ionomer to a desired particle size, or by pulverizing the above-mentioned resin film to a desired particle size.

[0073] The powder may contain optional components, such as organic fillers, inorganic fillers, plasticizers, pigments, flame retardants, dyes, surfactants, coupling agents, UV absorbers, short fibers, and nanocarbons.

[0074] The average particle size of the powder can be appropriately set depending on the application. For example, when the powder is applied to a fiber material for use as a matrix resin in fiber reinforced plastic (FRP), the average particle size measured by a laser diffraction / scattering method is preferably within a range of 10 to 100 μm, more preferably within a range of 40 to 80 μm. EXAMPLES

[0075] The features of the present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to the examples. In the following examples, various measurements and evaluations are as follows, unless otherwise specified.

[0076] [Glass transition temperature (Tg)] The resin film was pressed under the conditions of temperature: 160°C, pressure: 3.5MPa, and time: 60 minutes, and cut into test pieces measuring 5mm x 20mm. Measurements were performed using a dynamic viscoelasticity measuring device (DMA: manufactured by TA Instruments, product name: RSA-G2) at a heating rate of 4°C / min from 30°C to 200°C and a frequency of 11Hz. The temperature at which the change in elastic modulus (tan δ) was maximum was defined as the glass transition temperature.

[0077] [Tensile shear strength] Measurements were performed using a universal testing machine with reference to JIS K6850 (Test method for tensile shear adhesive strength between adhesive and rigid adherend). Measurements were performed in an environment of 25°C, and the test specimens used were galvanized steel sheets (SGCC) with a thickness of 1.6 mm, width of 25 mm, and length of 100 mm, and a backing plate with a thickness of 1.6 mm was used.

[0078] [Chemical resistance] The resin film was cut into a test piece 10 mm wide and 10 mm long, which was then immersed in 1 g of toluene at room temperature and the condition of the film was observed after 60 minutes. If the film shape was maintained, it was rated as "good", and if the film shape was not maintained even in part, it was rated as "bad".

[0079] [exterior] The resin film was visually observed.

[0080] [Infrared absorption spectrum (IR)] The resin film was analyzed by IR analysis using the ATR method (Ge). The IR intensity used for structural identification was 1605 cm -1 is normalized to 1, and the value is 1715 cm -1 (-COOH peak) and 1567cm -1 (-COO·M +The intensity of the peak (peak) is read.

[0081] The abbreviations used in the examples represent the following compounds. YP-50S: Bisphenol A phenoxy resin (product name: Phenototo YP50S, manufactured by Nippon Steel Chemical & Material Co., Ltd.) PA: Phthalic anhydride (trade name: Phthalic Anhydride, manufactured by Tokyo Kasei Kogyo Co., Ltd.) TMA: Trimellitic Anhydride (trade name: Trimellitic Anhydride, manufactured by Tokyo Chemical Industry Co., Ltd.) DMAP: 4-dimethylaminopyridine (product name: 4-dimethylaminopyridine, manufactured by Koei Chemical Industry Co., Ltd.) MDM: Diethylene glycol dimethyl ether (trade name: Diethylene Glycol Dimethyl Ether, manufactured by Tokyo Chemical Industry Co., Ltd.) Na(AcO): Sodium acetate (product name: Sodium acetate, Fujifilm Wako Pure Chemical Industries, Ltd.) Mg(AcO)2: Magnesium acetate (trade name: magnesium acetate tetrahydrate, Fujifilm Wako Pure Chemical Industries, Ltd.)

[0082] (Synthesis Example 1) Synthesis of YPS-20COOH: A 100-mL recovery flask was charged with 10 g of YP-50S, 26 g of MDM as a solvent, and 0.1 g of DMAP as a catalyst. The resulting mixed solution was heated to 110° C. with stirring to dissolve the mixture. Next, 1 g of PA was added and reacted for 30 minutes or more to obtain 37.1 g of varnish containing 11 g of carboxylic acid-modified phenoxy resin YPS-20COOH with an acid modification rate of 20%.

[0083] (Synthesis Example 2) Synthesis of YPS-40COOH: A 100-mL recovery flask was charged with 10 g of YP-50S, 28.4 g of MDM as a solvent, and 0.1 g of DMAP as a catalyst. The resulting mixed solution was heated to 110° C. with stirring to dissolve the mixture. Next, 2.1 g of PA was added and reacted for 30 minutes or more to obtain 40.6 g of varnish containing 12.1 g of carboxylic acid-modified phenoxy resin YPS-40COOH with an acid modification rate of 40%.

[0084] (Synthesis Example 3) Synthesis of YPS-40COOH-TMA: A 100-mL recovery flask was charged with 10 g of YP-50S, 29.8 g of MDM as a solvent, and 0.1 g of DMAP as a catalyst. The resulting mixed solution was heated to 110° C. with stirring to dissolve the components. Next, 2.7 g of TMA was added and reacted for 30 minutes or more to obtain 42.6 g of varnish containing 12.7 g of carboxylic acid-modified phenoxy resin YPS-40COOH-TMA with an acid modification rate of 40%.

[0085] Example 1 Synthesis of YPS-20COO-50Na: 2.973 g of YPS-20COOH obtained in Synthesis Example 1, 7 g of MDM as a solvent, and 10 g of varnish containing 0.03 g of DMAP as a catalyst were placed in a 100 mL eggplant flask, and the mixture was gradually heated to 80°C while stirring. 3.077 g of a methanol solution containing 77 mg of sodium acetate as a metal salt was added dropwise to the mixture and reacted at 80°C for 10 minutes or more to obtain 10.077 g of varnish containing 3.050 g of phenoxy resin ionomer YPS-20COO-50Na with a neutralization rate of 50%.

[0086] Example 2 Synthesis of YPS-40COO-50Na: 2.975 g of YPS-40COOH obtained in Synthesis Example 2, 7 g of MDM as a solvent, and 10 g of varnish containing 0.02 g of DMAP as a catalyst were placed in a 100 mL eggplant flask, and the mixture was gradually heated to 80°C while stirring. 3.141 g of a methanol solution containing 141 mg of sodium acetate as a metal salt was added dropwise to the mixture and reacted at 80°C for 10 minutes or more to obtain 10.141 g of varnish containing 3.117 g of phenoxy resin ionomer YPS-40COO-50Na with a neutralization rate of 50%.

[0087] Example 3 Synthesis of YPS-40COO-25Na: 2.975 g of YPS-40COOH obtained in Synthesis Example 2, 7 g of MDM as a solvent, and 10 g of varnish containing 0.02 g of DMAP as a catalyst were placed in a 100 mL eggplant flask, and the mixture was gradually heated to 80°C while stirring. 3.071 g of a methanol solution containing 71 mg of sodium acetate as a metal salt was added dropwise to the mixture and reacted at 80°C for 10 minutes or more to obtain 10.071 g of varnish containing 3.046 g of phenoxy resin ionomer YPS-40COO-25Na with a neutralization rate of 25%.

[0088] Example 4 Synthesis of YPS-40COO-TMA-50Na: 2.977 g of YPS-40COOH-TMA obtained in Synthesis Example 3, 7 g of MDM as a solvent, and 10 g of varnish containing 0.02 g of DMAP as a catalyst were placed in a 100 mL eggplant flask, and the mixture was gradually heated to 80°C while stirring. 3.269 g of a methanol solution containing 269 mg of sodium acetate as a metal salt was added dropwise to the mixture and reacted at 80°C for 10 minutes or more to obtain 10.269 g of varnish containing 3.246 g of phenoxy resin ionomer YPS-40COO-TMA-50Na with a neutralization rate of 50%.

[0089] Example 5 Synthesis of YPS-40COO-50Mg: 2.975 g of YPS-40COOH obtained in Synthesis Example 2, 7 g of MDM as a solvent, and 10 g of varnish containing 0.02 g of DMAP as a catalyst were placed in a 100 mL eggplant flask, and the mixture was gradually heated to 80°C while stirring. 3.370 g of a methanol solution containing 370 mg of magnesium acetate as a metal salt was added dropwise to the mixture and reacted at 80°C for 10 minutes or more to obtain 10.370 g of varnish containing 3.345 g of phenoxy resin ionomer YPS-40COO-50Na with a neutralization rate of 50%.

[0090] [Preparation of resin film] The viscosity of the varnish obtained in Examples 1 to 5 was adjusted, filtered using a 0.5 μm filter, and applied to a release-treated 50 μm-thick PET film with a bar coater to a thickness of 55 μm. After heating and drying on a hot plate at 100° C. for 5 hours, the resin films 1 to 5 were obtained by vacuum drying at 150° C. and 0.09 MPa for 5 hours in a vacuum dryer. The Tg, shear strength, chemical resistance, and appearance of the resin films 1 to 4 were evaluated. For Example 5, only the chemical resistance and appearance were evaluated. The results are shown in Table 1.

[0091] (Comparative Examples 1 to 4) Resin films R1 to R4 were produced in the same manner as in Examples 1 to 5, using the varnish of YP-50S as Comparative Example 1 and the varnishes of the carboxylic acid-modified phenoxy resins produced in Synthesis Examples 1 to 3 as Comparative Examples 2 to 4. The Tg, shear strength, chemical resistance and appearance of the resin films R1 to R4 were evaluated. The results are shown in Table 1.

[0092] Next, for the resin films 1 to 4 of Examples 1 to 4 and the resin films R1 to R4 of Comparative Examples 1 to 4, drying was performed on a hot plate and then vacuum drying in a vacuum dryer. The infrared absorption spectra (IR) were measured after drying on the hot plate but before vacuum drying, and after vacuum drying in the vacuum dryer. The results are shown in Table 1. The IR intensity in Table 1 is 1605 cm -1 is standardized as "1", and the value is 1715 cm -1 (-COOH peak) and 1567cm -1(-COO·M + The intensity of the peak (peak) was read.

[0093] In addition, for the resin films 1 to 4 of the examples and the resin films R1 to R4 of the comparative examples, the acid modification rate and neutralization rate before and after vacuum drying were estimated based on the IR intensity. These are referred to as "IR acid modification rate" and "IR neutralization rate" to distinguish them from the acid modification rate based on the charged amount added and the neutralization rate based on the charged amount added. The IR acid modification rate was estimated from the IR intensity of the other examples and comparative examples, assuming that the reaction rate was 88%, since it was confirmed by NMR (nuclear magnetic resonance) analysis that the reaction rate when YP-50S and TMA were reacted under the conditions of the examples and comparative examples. In addition, the IR neutralization rate was estimated from the IR intensity of each example and comparative example, assuming that the reaction rate of the neutralization reaction was 100%. The results are also shown in Table 1.

[0094] [Table 1]

[0095] From Table 1, the resin films 1 to 4 of Examples 1 to 4 have a Tg that is +15°C or more higher than the resin film R1 made of phenoxy resin and the corresponding resin films R2 to R4 of the comparative examples, and the heat resistance is improved, and the shear strength is also improved. Furthermore, the resin films 1 to 5 of Examples 1 to 5 have improved chemical resistance while maintaining the transparency of the appearance, compared to the resin films R1 to R4 of the comparative examples. Therefore, it was confirmed that by ionomerizing the phenoxy resin, it is possible to improve the heat resistance, mechanical strength, and chemical resistance compared to the phenoxy resin film, without impairing the appearance.

[0096] In addition, referring to the IR intensity in Table 1, in all of Examples 1 to 4 and Comparative Examples 2 to 4, the IR intensity was 1715 cm after vacuum drying compared to before vacuum drying. -1It can be seen that the IR intensity of (-COOH peak) is greatly reduced, and the IR acid modification rate is also reduced. From this, it is considered that the unreacted -COOH remaining in the phenoxy resin ionomer without being neutralized can be reduced by vacuum drying. Since the unreacted -COOH causes gelation, it was confirmed that vacuum drying can prevent gelation. Therefore, when the phenoxy resin ionomer is applied to applications such as insulating films, adhesive films, matrix resins for fiber-reinforced composite materials, composite materials of metal and resin suitable for automobile parts, vibration-damping members for steel materials, packaging films, containers, and sporting goods, gelation must be prevented because gelation causes embrittlement of the film, changes in appearance, and deterioration of physical properties, and vacuum drying is effective in preventing gelation.

[0097] 1 and 2 show IR charts before and after vacuum drying for the resin film 2 of Example 2, the resin film R1 of Comparative Example 1, and the resin film R3 of Comparative Example 3. FIG. 1 shows the IR chart before vacuum drying, and FIG. 2 shows the IR chart after vacuum drying. As shown in FIGS. 1 and 2, in Example 2, the C=O stretching vibration peak of -COOH (1715 cm) is smaller than that in Comparative Example 3. -1 ) is decreasing, while -COO·M + C=O stretching vibration peak (1567cm -1 ) was increased, and it was confirmed that the carboxylic acid-modified phenoxy resin was converted to a phenoxy resin ionomer. In addition, from a comparison of FIG. 1 and FIG. 2, in both Example 2 and Comparative Example 3, the C=O stretching vibration peak of -COOH (1715 cm) was increased by vacuum drying. -1 ) decreases, and -COO M + C=O stretching vibration peak (1567cm -1 ) was confirmed to be increasing.

[0098] Although the embodiment of the present invention has been described in detail above for the purpose of illustration, the present invention is not limited to the above embodiment, and various modifications are possible.

Claims

1. A phenoxy resin ionomer in which a part or all of the acidic functional groups contained in an acid-modified phenoxy resin having an acid modification rate of 10 to 80% by acidic functional groups are neutralized with metal ions.

2. 2. The phenoxy resin ionomer according to claim 1, wherein the acidic functional group is a carboxyl group, and the acid-modified phenoxy resin is a carboxylic acid-modified phenoxy resin.

3. The phenoxy resin ionomer according to claim 1, wherein the metal ions are derived from a metal compound, and the neutralization rate calculated by the following formula (1) is within the range of 10 to 80%. Neutralization rate (%) = [V m ×M m ÷Mf] × 100 … Formula (1) [wherein Vm is the valence of the metal ion, Mm is the content (molar number) of the metal ion in the metal compound, and Mf is the content (molar number) of the acidic functional group in the acid-modified phenoxy resin]

4. The phenoxy resin ionomer according to any one of claims 1 to 3. And, Organic solvents, A phenoxy resin ionomer composition comprising:

5. The organic solvent dissolves the carboxylic acid-modified phenoxy resin and satisfies the following condition (1) or condition (2): Condition (1): A metal carboxylate, which is a precursor of a metal ion, is soluble. Or, Condition (2): compatibility with alcohols having 1 to 3 carbon atoms; 5. The phenoxy resin ionomer composition according to claim 4, which satisfies at least one of the above conditions.

6. A resin film comprising the phenoxy resin ionomer according to any one of claims 1 to 3.

7. A powder containing the phenoxy resin ionomer according to any one of claims 1 to 3.

8. The following steps i) and ii); i) reacting a secondary hydroxyl group of a phenoxy resin with an acidic functional group donor compound in a polar solvent to produce an acid-modified phenoxy resin having an acid modification rate in the range of 10 to 80%; and ii) ionomerizing the acid-modified phenoxy resin by adding a metal compound dissolved in a polar solvent to the acid-modified phenoxy resin; A method for producing a phenoxy resin ionomer comprising the steps of:

9. 9. The method for producing a phenoxy resin ionomer according to claim 8, wherein the acidic functional group donating compound is a carboxylic acid anhydride compound represented by the following general formula (1) or (2): 【Chemistry 1】 [In general formula (1) and general formula (2), the groups R are each independently a hydrogen atom, a hydrocarbon group, a halogen atom, an alkoxy group, an ester group, a cyano group, an amide group, an imide group, a silyl group, a carboxyl group, or a hydrocarbon group substituted with a polar group, and the polar group is a halogen atom, an alkoxy group, an ester group, a nitro group, a cyano group, an amide group, an imide group, or a silyl group.]

10. The following steps I) and II); I) a step of casting the phenoxy resin ionomer composition according to claim 4 to form a coating film; and II) drying the coating film; A method for producing a resin film comprising the steps of:

11. The method for producing a resin film according to claim 10, wherein in the step II), vacuum drying is carried out after heat drying.

Citation Information

Patent Citations

  • Wiring board material and printed wiring board

    JP1999135901A

  • Ionomer resin composition and molded article thereof

    JP2020158682A

  • Phenoxy resin composition and cured product thereof

    WO2014157132A1