Cathode active material for lithium secondary batteries, lithium secondary battery, and manufacturing method of cathode active material for lithium secondary batteries

JP2024134400APending Publication Date: 2024-10-03HONDA MOTOR CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023044683
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Benefits of technology

【0012】 本発明のリチウム二次電池用正極活物質は、従来技術のLiNi0.5Mn0.5O2に構成元素としてチタン(Ti)を加え、Ni0.5Mn0.5の一部をLiとTiで置き換えることにより、電気化学特性を良好に維持しながら資源リスクのあるNiの使用量を低減することを可能にする。また、正極活物質が、前記一般式(1)で表されるリチウム遷移金属複合酸化物の化学組成の範囲、および格子定数の範囲を満たすことにより、遷移金属が均一に分散され、これによりリチウム二次電池の充放電容量を向上させることができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134400000001_ABST
    Figure 2024134400000001_ABST
Patent Text Reader

Abstract

To provide a cathode active material which does not use cobalt, which has the resource risk and is expensive, also reduces the amount of nickel to be used as further as possible and has excellent electrochemical characteristics.SOLUTION: A cathode active material for lithium secondary batteries contains a lithium transition metal composite oxide as a main component. The lithium transition metal composite oxide is a form of particles having a layered structure consisting of a lithium layer and a transition metal-lithium layer. The lithium transition metal composite oxide is expressed by the general formula (1): LimNixMnyTizO2 (in the formula, (m) leads 1.0<m≤1.1, (x) leads 0.4≤x<0.5, (y) leads 0.3<y<0.5, and (z) leads 0<z≤0.133). Regarding grating constants (a, c and c / a) of the lithium transition metal composite oxide, an a-axis length is 2.886 Å to 2.900 Å, a c-axis length is 14.29 Å to 14.35 Å and c / a is 4.940 to 4.960.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel positive electrode active material for a lithium secondary battery, a lithium secondary battery using the positive electrode active material, and a method for producing the positive electrode active material for a lithium secondary battery. [Background technology]

[0002] In recent years, research and development has been conducted on secondary batteries that contribute to energy efficiency. In particular, lithium secondary batteries are becoming increasingly important as a power source for electric vehicles (EVs) and hybrid electric vehicles (HEVs).

[0003] Positive electrode active materials have been attracting attention as important components that determine the capacity of lithium secondary batteries, and their development is underway. For example, nickel-manganese composite oxides have been reported as positive electrode active materials for use in lithium secondary batteries (see Non-Patent Document 1), and nickel-manganese-titanium composite oxides have been reported (see Non-Patent Document 2, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-60167 [Patent Document 2] JP 2008-12733 A [Non-patent literature]

[0005] [Non-Patent Document 1] Mitsuharu Tabuchi, Riki Kataoka, and Koji Yazawa, “High-Capacity Li-excess lithium nickel manganese oxide as a Co-free positive electrode material”, Materials Research Bulletin, 137 (2021) 111178 [Non-Patent Document 2] JSKim, CSJohnson, MMThackeray “Layered xLiMO2·(1-x)Li2M'O3 electodes for lithium batteries: a study of 0.95LiMn0.5Ni0.5O2·0.05Li2TiO3”, Electrochemistry Communications 4(2002)205-209 Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, in the technology relating to lithium secondary batteries, it is an issue to provide a positive electrode active material that does not use cobalt, which is expensive and has resource risks, and that uses as little nickel as possible, while having excellent electrochemical properties.

[0007] The technology described in the above Non-Patent Document 1 aims to develop a cobalt-free positive electrode material, but LiNi 0.5 Mn 0.5 In the XRD pattern of O2, the bimodal peaks around 2θ=65° are either tailed or not clearly separated. 7 In the Li-MAS-NMR data, peaks due to Ni, Mn-Li, and Mn-Li in the transition metal layer having a honeycomb structure are observed around 1350 ppm and 1500 ppm, respectively, and a shoulder peak due to Ni domains near Li in the Li layer near 533 ppm is observed in addition to a peak due to Mn domains near Li in the Li layer near 700 nm for the main peak. These indicate that in the lithium transition metal composite oxide described in Non-Patent Document 1, the transition metals (Ni, Mn) are not uniformly dispersed and phase separation or domain formation occurs. This suggests that the electrochemical properties of the lithium transition metal composite oxide disclosed in Non-Patent Document 1 are poor.

[0008] The technology described in Non-Patent Document 2 above is LiNi 0.5 Mn0.5 0.95LiMn with electrochemically inactive Li2TiO3 to enhance the stability of the O2 electrode 0.5 Ni 0.5 O2·0.05Li2TiO3 is used as the positive electrode material. However, 0.95LiMn 0.5 Ni 0.5 The XRD pattern of O2·0.05Li2TiO3 has the problem that the bimodal peak near 2θ = 65° is not clearly separated and the transition metals (Ni, Mn, Ti) are not uniformly dispersed.

[0009] The technology described in the above Patent Document 1 uses Li as a cobalt-free positive electrode material. 1+x (Ni y M z Mn 1-y-z ) 1-x However, in the XRD pattern of the lithium transition metal composite oxide described in the document, a peak due to the Li2MnO3 domain is observed near 2θ=22°, indicating that the transition metal is not uniformly dispersed. In addition, the technology described in the above Patent Document 2 proposes Li 1+x (M 1-n-m Ni m Ti n ) 1-x However, the lithium transition metal composite oxide described in this document is composed of a mixed phase of a crystal phase with a layered rock-salt structure and a crystal phase with a cubic rock-salt structure, and its chemical composition is not uniform.

[0010] The present invention provides a positive electrode material for lithium secondary batteries that is cobalt-free and uses a reduced amount of nickel, and further solves the problem of reduced electrochemical characteristics caused by non-uniform dispersion of transition metals as seen in the above-mentioned prior art. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention provides the following means. [1] A positive electrode active material for a lithium secondary battery, which contains a lithium transition metal composite oxide as a main component, wherein the lithium transition metal composite oxide is in the form of particles having a layered structure composed of a lithium layer and a transition metal-lithium layer, and the lithium transition metal composite oxide is represented by the general formula (1): Li m Ni x Mn y Ti z O2 (wherein m is in the range of 1.0 < m ≦ 1.1, x is in the range of 0.4 ≦ x < 0.5, y is in the range of 0.3 < y < 0.5, and z is in the range of 0 < z ≦ 0.133), and the lattice constants (a, c, c / a) of the lithium transition metal composite oxide are such that the a-axis length is 2.886 Å to 2.900 Å, the c-axis length is 14.29 Å to 14.35 Å, and c / a is 4.940 to 4.960. A positive electrode active material for a lithium secondary battery.

[0012] The positive electrode active material for a lithium secondary battery of the present invention adds titanium (Ti) as a constituent element to conventional LiNi 0.5 Mn 0.5 O2, and replaces a part of Ni 0.5 Mn 0.5 with Li and Ti, thereby making it possible to reduce the usage amount of Ni with resource risks while maintaining good electrochemical characteristics. Further, by satisfying the chemical composition range and the lattice constant range of the lithium transition metal composite oxide represented by the general formula (1), the transition metal is uniformly dispersed, and thereby the charge-discharge capacity of the lithium secondary battery can be improved.

[0013] [2] The positive electrode active material for a lithium secondary battery according to [1], wherein in the general formula (1), m is in the range of 1.05 ≦ m ≦ 1.066, x is in the range of 0.4 ≦ x ≦ 0.475, y is in the range of 0.4 ≦ y ≦ 0.475, and z is in the range of 0.05 ≦ z ≦ 0.133.

[0014] By optimizing the chemical composition of the lithium transition metal composite oxide represented by the general formula (1), the dispersibility of the transition metal is further improved, and the charge-discharge capacity of the lithium secondary battery can be further increased.

[0015] [3] The positive electrode active material for a lithium secondary battery according to [1] or [2], wherein a ratio of the number of Mn atoms to the number of Ni atoms (Mn / Ni ratio) on the surface of a particle of the lithium transition metal composite oxide is greater than 1.0 and less than 2.5.

[0016] By making the surface of the lithium transition metal composite oxide particles Mn-rich, when the lithium transition metal composite oxide is used as a positive electrode active material of a lithium secondary battery, it is possible to increase the charge / discharge capacity of the lithium secondary battery.

[0017] [4] Solid-state lithium nuclear magnetic resonance analysis using magic angle sample spinning ( 6 The positive electrode active material for a lithium secondary battery according to any one of [1] to [3], wherein in a spectrum of the lithium transition metal composite oxide measured by Li-MAS-NMR, a peak intensity ratio at 1500 ppm / 600 ppm is 0.15 or less.

[0018] By setting the peak intensity ratio at 1500 ppm / 600 ppm in the solid-state lithium nuclear magnetic resonance spectrum to 0.15 or less, phase separation of the transition metal is suppressed, that is, by uniformly dispersing the transition metal, when the lithium transition metal composite oxide is used as a positive electrode active material of a secondary battery, the charge / discharge capacity of the lithium secondary battery can be increased.

[0019] [5] Solid-state lithium nuclear magnetic resonance analysis ( 6 The positive electrode active material for a lithium secondary battery according to any one of [1] to [4], wherein in a spectrum of the lithium transition metal composite oxide measured by Li-MAS-NMR, a peak due to lithium contained in the transition metal-lithium layer does not exist at 1500 ppm.

[0020] As a result, when the lithium transition metal composite oxide is used as a positive electrode active material of a secondary battery, it is possible to further increase the charge / discharge capacity of the lithium secondary battery.

[0021] [6] A lithium secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, wherein the positive electrode contains the positive electrode active material for lithium secondary batteries according to any one of [1] to [5].

[0022] The lithium secondary battery of the present invention can have a high capacity because the positive electrode contains a positive electrode active material containing the above-mentioned lithium transition metal composite oxide as a main component.

[0023] [7] The lithium secondary battery according to [6], wherein the electrolyte is a solid electrolyte.

[0024] The positive electrode active material for a lithium secondary battery of the present invention can be applied to an all-solid-state lithium secondary battery.

[0025] [8] A method for producing a positive electrode active material for a lithium secondary battery according to any one of [1] to [5], A method for producing a positive electrode active material for a lithium secondary battery, comprising the steps of: heat-treating a mixture of a lithium compound, a titanium compound, and a nickel manganese compound at 1000°C or more and 1200°C or less for 1 minute or more and 7 hours or less; or heat-treating a mixture of a lithium compound and a nickel manganese titanium compound at 1000°C or more and 1200°C or less for 1 minute or more and 7 hours or less.

[0026] By using a method including the above steps, it is possible to produce a positive electrode active material for a lithium secondary battery that satisfies the range of the chemical composition and the range of the lattice constant of the lithium transition metal composite oxide represented by the general formula (1).

[0027] [9] The method for producing a positive electrode active material for a lithium secondary battery according to [8], further comprising the step of subsequently maintaining the obtained lithium transition metal composite oxide at 850° C. or higher and 950° C. or lower for 3 hours or longer and 12 hours or shorter after the heat treatment step.

[0028] By further providing a slow cooling step, the surface of the lithium transition metal composite oxide particles can be made Mn-rich. [Brief description of the drawings]

[0029] [Figure 1] FIG. 2 is a diagram showing 6Li-MAS-NMR spectra of the lithium transition metal composite oxides of Examples 1 and 2. [Diagram 2] FIG. 2 is a diagram showing 6Li-MAS-NMR spectra of the lithium transition metal composite oxides of Examples 3 and 4. [Diagram 3] FIG. 2 is a diagram showing powder X-ray diffraction patterns of the lithium transition metal composite oxides of Examples 1 and 2. [Figure 4] FIG. 2 is a diagram showing powder X-ray diffraction patterns of the lithium transition metal composite oxides of Examples 3 and 4. [Diagram 5] FIG. 2 is a graph showing charge / discharge curves in a lithium secondary battery using the lithium transition metal composite oxides of Examples 1 and 2. [Figure 6] FIG. 4 is a graph showing charge / discharge curves in lithium secondary batteries using the lithium transition metal composite oxides of Examples 3 and 4. [Figure 7] 3 is an electron microscope photograph of the lithium transition metal composite oxide particles of Example 3. [Figure 8] 1 is an electron microscope photograph of the lithium transition metal composite oxide particles of Example 4. [Figure 9] FIG. 1 is a cross-sectional view illustrating an example of a lithium secondary battery according to an embodiment of the present invention. [Figure 10] FIG. 1 is a diagram showing the 7Li-MAS-NMR spectrum of the lithium transition metal composite oxide (LiNi0.5Mn0.5O2) shown in Non-Patent Document 1. [Figure 11] FIG. 1 is a diagram showing an X-ray diffraction pattern of the lithium transition metal composite oxide (LiNi0.5Mn0.5O2) shown in Non-Patent Document 1. [Figure 12] FIG. 1 is a diagram showing an X-ray diffraction pattern of the titanium-containing lithium nickel manganese based composite oxide disclosed in Patent Document 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Preferred embodiments of the present invention will now be described in detail.

[0031] [Positive electrode active material for lithium secondary batteries] The positive electrode active material for lithium secondary batteries of the present invention is mainly composed of a lithium transition metal composite oxide and is used in the positive electrode of a lithium secondary battery. The term "mainly composed of" a lithium transition metal composite oxide means that the content of the lithium transition metal composite oxide is 75% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 99% by mass or more. The positive electrode active material for lithium secondary batteries may contain components other than the main component as long as the function of the present invention is not impaired.

[0032] The positive electrode active material for lithium secondary batteries of the present invention may contain only one type of lithium transition metal composite oxide or may contain two or more types of lithium transition metal composite oxide, so long as it contains a lithium transition metal composite oxide as a main component.

[0033] When a positive electrode active material is produced using a lithium transition metal composite oxide as a main component, the composition ratio (Li:Ni:Mn:Ti) of the entire lithium transition metal composite oxide is maintained in the obtained positive electrode active material. When a positive electrode active material obtained using a lithium transition metal composite oxide having such a composition as a main component is used in a secondary battery, a high capacity can be realized. In addition, the composition ratio of the lithium transition metal composite oxide is adjusted to be the same as the composition ratio required for the positive electrode active material to be obtained.

[0034] (Lithium transition metal complex oxide) The lithium transition metal composite oxide used in the present invention is a layered rock-salt type oxide, and is in the form of particles having a layered structure of a lithium layer (Li layer) and a transition metal-lithium layer (TM-Li layer).

[0035] <Chemical composition> Conventional lithium transition metal composite oxides (e.g., LiNi 0.5 Mn 0.5 In the case of O2), when Li is dissolved in the transition element, Ni, which is involved in the redox reaction, 2+ Ni 3+In order to convert and improve the electrochemical properties as the cathode active material, it is necessary to increase the amount of Ni used. The present invention is based on the finding that by adding Ti as a constituent element to LiNi 0.5 Mn 0.5 O2 and replacing a part of Ni 0.5 Mn 0.5 with Li and Ti, it is possible to suppress the increase in the valence of Ni ions to 3. Accordingly, in the present invention, the amount of Ni used can be reduced while maintaining good electrochemical properties of the cathode active material.

[0036] The lithium transition metal composite oxide used in the present invention is represented by the general formula (1): Li m Ni x Mn y Ti z O2 (wherein m is in the range of 1.0 < m ≦ 1.1, x is in the range of 0.4 ≦ x < 0.5, y is in the range of 0.3 < y < 0.5, and z is in the range of 0 < z ≦ 0.133).

[0037] The lithium transition metal composite oxide used in the present invention is more preferably such that m in the general formula (1) is in the range of 1.05 ≦ m ≦ 1.066, x is in the range of 0.4 ≦ x ≦ 0.475, y is in the range of 0.4 ≦ y ≦ 0.475, and z is in the range of 0.05 ≦ z ≦ 0.133. Specifically, the lithium transition metal composite oxide used in the present invention has a chemical composition in the range from Li 1.05 Ni 0.475 Mn 0.475 Ti 0.05 O2 to Li 1.066 Ni 0.4 Mn 0.4 Ti 0.133 O2. This means that the molar ratio of Li / Ti in the transition metal-Li layer is in the range from Li:Ti = 1:1 [Li(Li 0.05 Ni 0.475 Mn 0.475 Ti 0.05 )O2] to Li:Ti = 1:2 [Li(Li 0.066 Ni 0.4 Mn 0.4 Ti 0.133 )O2].

[0038] The composition of the lithium transition metal composite oxide can be analyzed by inductively coupled plasma (ICP) optical emission spectrometry.

[0039] <Lattice constant> The lithium transition metal composite oxide used in the present invention is a layered compound of the rhombohedral system, and has a crystal structure of space group R-3m. The lattice constant of the lithium transition metal composite oxide is preferably an a-axis length of 2.886 Å to 2.900 Å, a c-axis length of 14.29 Å to 14.35 Å, and c / a of 4.940 to 4.960. With the lattice constant in the above range, the lithium transition metal composite oxide has low resistance because lithium ions are easily diffused within the primary particles. The lattice constant of the crystal can be determined by the least squares method using the X-ray diffraction pattern of the lithium transition metal composite oxide and each index and its interplanar spacing.

[0040] < 6 Li-MAS-NMR spectrum> 1 and 2 show solid-state lithium nuclear magnetic resonance (NMR) images of the lithium transition metal composite oxide according to an embodiment of the present invention. 6 The Li-MAS-NMR spectrum is shown. The solid line is the spectrum after heat treatment at 1050°C or 1100°C for 5 minutes, and the dashed line is the spectrum after heat treatment at 1050°C or 1100°C for 5 minutes and then holding at 850°C or 900°C for 6 hours. The spectrum shows a single peak near 600 ppm with no cracks (i.e., no phase separation or domain formation). This indicates that Ni, Mn, and Ti (transition metals) are uniformly dispersed. If the transition metals are not uniformly dispersed and Ni-rich or Mn-rich domains are formed, the peak near 600 ppm will be cracked and will not be a single peak.

[0041] In addition, the spectra shown in Figures 1 and 2 have no peaks other than the spinning side bands near 1500 ppm. If a Mn-rich domain is formed in the transition metal-Li layer, a peak appears near 1500 ppm.

[0042] For example, the above-mentioned non-patent document 1 describes a LiNi 0.5 Mn 0.5 O2 7 The Li-MAS-NMR spectrum is disclosed, and a main peak at 724 ppm due to the Mn-rich domain and a shoulder peak at 533 ppm due to the Ni-rich domain are observed, and are not a single peak. 0.5 Mn 0.5 In O2, it is shown that the transition metals (Ni, Mn) are not uniformly dispersed. In addition, near 1500 ppm, a peak at 1506 ppm due to Mn-Li and a peak at 1348 ppm due to Ni, Mn-Li are observed, which also indicates that the transition metals are not uniformly dispersed.

[0043] The lithium transition metal composite oxide used in the present invention has the following properties after heat treatment: 6 In the Li-MAS-NMR spectrum, there is no peak at 1500 ppm, or the peak intensity ratio of 1500 ppm / 600 ppm is 0.15 or less, 0.1 or less, or 0.05 or less. Preferably, the lithium transition metal composite oxide used in the present invention has no peak at 1500 ppm. In this specification, the absence of a peak at 1500 ppm means that no peak other than a ghost peak such as a spinning side band exists at 1500 ppm. The present inventors have found that the peaks in the spectra of FIGS. 1 and 2 are not present at 1500 ppm. 6 In the Li-MAS-NMR spectrum, it was confirmed by peak separation that there were no peaks other than a ghost peak at 1500 ppm.

[0044] The lithium transition metal composite oxide used in the present invention has transition metals uniformly dispersed therein, and therefore when used as a positive electrode active material in a lithium secondary battery, the charge / discharge capacity can be increased.

[0045] 6 The Li-MAS-NMR spectrum can be measured by a solid-state lithium nuclear magnetic resonance apparatus using the magic angle sample spinning method.

[0046] <X-ray diffraction (XRD) pattern> Figure 3 shows the XRD pattern of the lithium transition metal composite oxide (Li 1.05 Ni 0.475 Mn 0.475 Ti 0.05 O2) according to the embodiment. No peaks due to domain structure are observed in either the pattern (solid line) after heat-treating the raw material mixture at 1050°C for 5 minutes or the pattern (dashed line) after heat-treating at 1050°C for 5 minutes and then holding at 850°C for 6 hours. In particular, the two peaks at 2θ = 108° and 110° are clearly separated in both patterns, indicating that Ni, Mn, and Ti are uniformly dispersed without phase separation.

[0047] Figure 4 shows the XRD pattern of the lithium transition metal composite oxide (Li 1.066 Ni 0.4 Mn 0.4 Ti 0.133 O2) according to another embodiment. No peaks due to domain structure are observed in either the pattern (solid line) after heat-treating the raw material mixture at 1100°C for 5 minutes or the pattern (dashed line) after heat-treating at 1100°C for 5 minutes and then holding at 900°C for 6 hours. In particular, the two peaks at 2θ = 108° and 110° are clearly separated in both patterns, indicating that Ni, Mn, and Ti are uniformly dispersed without phase separation.

[0048] In contrast, for example, in Non-Patent Document 1 above, the XRD pattern of LiNi 0.5 Mn 0.5 O2 is disclosed. As shown in Figure 11, the peak at 2θ = 65° is not clearly separated or is tailing. In Non-Patent Document 1, this XRD pattern suggests that the disclosed lithium nickel manganese oxide is biphasic. Also, in the XRD pattern disclosed in Patent Document 1 above, as shown in Figure 12, a peak due to the Li2MnO3 domain structure is observed near 2θ = 20°.

[0049] <Surface composition> The lithium transition metal composite oxide particles may be primary particles or secondary particles, but secondary particles formed by agglomeration of a plurality of primary particles are preferred, as this gives relatively dense particles.

[0050] The lithium transition metal composite oxide particles have a multilayer structure of a lithium layer and a transition metal-Li layer, and preferably the composition of the outer surface has a higher Mn content than the composition of the center. The lithium transition metal composite oxide used in the present invention has a ratio of the number of Mn atoms to the number of Ni atoms on the lithium transition metal composite oxide surface (Mn / Ni ratio) preferably greater than 1.0 and less than 2.5, more preferably greater than 1.0 and less than 2.0. When the Mn / Ni ratio is within the above range, the movement of lithium ions is not inhibited, and when used as a positive electrode active material, the charge / discharge capacity of a lithium secondary battery becomes high.

[0051] The composition of the manganese-rich surface can be determined, for example, by quantitative analysis using X-ray photoelectron spectroscopy (XPS). XPS allows the composition of the manganese-rich surface of the entire particle to be analyzed. In other words, the analysis results obtained by XPS do not show the local composition of the entire surface of a particle, but show the composition of the entire surface of the particle.

[0052] [Method of manufacturing positive electrode active material for lithium secondary batteries] The positive electrode active material for lithium secondary batteries of the present invention contains the above-mentioned lithium transition metal composite oxide as a main component. As the lithium source of the lithium transition metal composite oxide, known compounds such as hydroxides such as lithium hydroxide monohydrate (LiOH·H2O), carbonates such as lithium carbonate (Li2CO3), acetates such as lithium acetate (CH3COOLi) and lithium acetate dihydrate (CH3COOLi·2H2O) can be used, and there is no particular limitation. As the compounds of the nickel source, manganese source, and titanium source of the transition metals, known oxides, hydroxides, or metal salts of nickel, manganese, and titanium can be widely used, and there is no particular limitation. For example, as the nickel compound, nickel hydroxide (Ni(OH)2), nickel(II) chloride (NiCl2), nickel(II) chloride hexahydrate (NiCl2·6H2O), nickel(II) nitrate hexahydrate (Ni(NO3)2·6H2O), etc. can be used, but are not limited to these. Examples of manganese compounds that can be used include, but are not limited to, manganese chloride (II) (MnCl2), manganese chloride (II) tetrahydrate (MnCl2·4H2O), manganese carbonate hexahydrate (MnCO3·6H2O), manganese nitrate (II) hexahydrate (Mn(NO3)2·6H2O), etc. Examples of titanium compounds that can be used include, but are not limited to, titanium dioxide (TiO2), titanium (IV) sulfate (Ti(SO4)2), etc. The above transition metal compounds can be used alone or as composite hydroxides (e.g., nickel manganese titanium composite hydroxide) by coprecipitation or the like.

[0053] The lithium transition metal composite oxide used in the present invention can be synthesized by using a known method. For example, a composite hydroxide or composite oxide of a nickel compound and a manganese compound is prepared as an intermediate compound, and this intermediate compound is mixed with a titanium compound and a lithium compound to form a raw material mixture, and this raw material mixture is heat-treated (for example, calcined) in a predetermined atmosphere at a predetermined temperature for a predetermined time, thereby synthesizing the oxide. In addition, a composite hydroxide or composite oxide of a nickel compound, a manganese compound, and a titanium compound is prepared as an intermediate compound, and this intermediate compound is mixed with a lithium compound to form a raw material mixture, and this raw material mixture is heat-treated (for example, calcined) in a predetermined atmosphere at a predetermined temperature for a predetermined time, thereby synthesizing the oxide.

[0054] The lithium transition metal composite oxide obtained in the heat treatment step is preferably further held at a predetermined temperature range for a predetermined time in a slow cooling step. The slow cooling conditions vary depending on the treatment conditions (e.g., heat treatment atmosphere such as oxygen atmosphere, nitrogen atmosphere, vacuum atmosphere, etc.), and are preferably adjusted appropriately. The present inventors have found that by appropriately selecting the heat treatment conditions and the slow cooling conditions, the transition metal of the lithium transition metal composite oxide can be uniformly dispersed and the Mn / Ni ratio of the particle surface can be increased. Hereinafter, the method for producing a positive electrode active material for lithium secondary batteries of the present invention will be described in more detail with reference to an embodiment.

[0055] "First step" In the first step, a predetermined amount of titanium compound and a predetermined amount of lithium compound are added to an intermediate nickel manganese compound, and the mixture is dispersed in a solvent such as ethanol. In addition to wet mixing using a solvent, a predetermined amount of the intermediate compound, a predetermined amount of titanium compound, and a predetermined amount of lithium compound may be mixed by dry mixing without using a solvent. For example, titanium dioxide (TiO2) is used as the titanium compound and lithium carbonate (Li2CO3) is used as the lithium compound, and Li 1.05 Ni 0.475 Mn 0.475 Ti 0.05When synthesizing O2, Li2CO3 is weighed out in an amount preferably 1 mass % to 5 mass %, for example 2 mass %, more than the stoichiometric ratio. 1.066 Ni 0.4 Mn 0.4 Ti 0.133 Similarly, when synthesizing O2, Li2CO3 is weighed out preferably 1 mass % to 5 mass %, for example 2 mass %, more than the stoichiometric ratio.

[0056] The nickel manganese compound can be synthesized by a known method. When the nickel manganese compound is a hydroxide, for example, nickel sulfate hexahydrate (NiSO4·6H2O) and manganese sulfate pentahydrate (MnSO4·5H2O) are weighed out so that the molar ratio of Ni:Mn is 1:1, and pure water is added to dissolve the compound. Then, an alkaline aqueous solution is dropped into the sulfate aqueous solution to co-precipitate the compound as a nickel manganese composite hydroxide.

[0057] Instead of using the nickel manganese compound as the intermediate compound, a nickel manganese titanium compound may be used. For example, a predetermined amount of a lithium compound is added to the nickel manganese titanium compound, and the mixture is dispersed in a solvent such as ethanol. In addition to wet mixing using a solvent, a predetermined amount of the nickel manganese titanium compound and a predetermined amount of a lithium compound may be mixed by dry mixing without using a solvent. For example, lithium carbonate (Li2CO3) is used as the lithium compound, and Li 1.05 Ni 0.475 Mn 0.475 Ti 0.05 When synthesizing O2, Li2CO3 is weighed out in an amount preferably 1 mass % to 5 mass %, for example 2 mass %, more than the stoichiometric ratio. 1.066 Ni 0.4 Mn 0.4 Ti 0.133 Similarly, when synthesizing O2, Li2CO3 is weighed out preferably 1 mass % to 5 mass %, for example 2 mass %, more than the stoichiometric ratio.

[0058] The nickel manganese titanium compound of the above formula can be synthesized by using a known method. When the nickel manganese titanium compound is a hydroxide, for example, nickel sulfate hexahydrate (NiSO4·6H2O), manganese sulfate pentahydrate (MnSO4·5H2O), and titanium sulfate (Ti(SO4)2) are weighed out so that the molar ratio of Ni:Mn:Ti is 1:1:x (x is preferably 0.05 to 0.333), and pure water is added to dissolve the compound, and then an alkaline aqueous solution is dropped into the sulfate aqueous solution to co-precipitate the compound as a nickel manganese titanium composite hydroxide.

[0059] As the precursor, a mixture of a lithium compound, a titanium compound, and a nickel manganese compound, or a mixture of a lithium compound and a nickel manganese titanium compound, is crushed and mixed to a desired size, and then the mixture is filled into a crucible and heat-treated. As the crucible, an alumina sagger, an alumina crucible, a platinum crucible, a gold crucible, or the like is used. For example, a firing furnace or a roller hearth kiln is used for the heat treatment of the mixture.

[0060] The mixture placed in a sagger or crucible is heated at a temperature rise rate of 5°C / min to 25°C / min, preferably 10°C / min to 25°C / min, until the heat treatment temperature is reached. The heat treatment atmosphere is not particularly limited, and examples thereof include air (air atmosphere) and oxygen flow. The heat treatment atmosphere is preferably oxygen flow. The heat treatment time can be appropriately set depending on the heat treatment temperature. The heat treatment time means the time during which the heat treatment temperature is maintained.

[0061] When a mixture of a lithium compound (e.g., Li2CO3), a titanium compound (e.g., TiO2), and a nickel-manganese compound is heat-treated, the heat treatment temperature is preferably 1000° C. or more and 1200° C. or less, more preferably 1000° C. or more and 1100° C. or less. The heat treatment time is preferably 1 minute or more and 7 hours or less, more preferably 2 minutes or more and 6 hours or less, and even more preferably 3 minutes or more and 5 hours or less.

[0062] When a mixture of a lithium compound (e.g., Li2CO3) and a nickel manganese titanium compound is heat-treated, the heat treatment temperature is preferably 1000° C. or more and 1200° C. or less, more preferably 1000° C. or more and 1100° C. or less. The heat treatment time is preferably 1 minute or more and 7 hours or less, more preferably 2 minutes or more and 6 hours or less, and further preferably 3 minutes or more and 5 hours or less.

[0063] "Second step" In the second step, the powder obtained after the heat treatment in the first step is cooled to 900° C. at a temperature drop rate of 5° C. / min to 25° C. / min, preferably 10° C. / min to 25° C. / min, and then the powder is held at 900° C. for 0.5 to 12 hours. The atmosphere in which the powder is held at 900° C. is not particularly limited, and examples thereof include air (air atmosphere), nitrogen atmosphere, and oxygen flow.

[0064] The method for producing a positive electrode active material for a lithium secondary battery of the present invention may include a step of holding the powder at 850° C. for 12 hours after the second step. In this case, the powder held at 900° C. in the second step is cooled to 850° C. at a temperature drop rate of 10° C. / min, and then the powder is held at 850° C. for 12 hours. The atmosphere in which the powder is held at 850° C. is not particularly limited, and examples thereof include air (air atmosphere), nitrogen atmosphere, and oxygen flow.

[0065] "The third step" In the third step, the powder held at 900° C. in the second step is cooled to 800° C. at a temperature drop rate of 5° C. / min to 25° C. / min, preferably 10° C. / min to 25° C. / min, and then the powder is held at 800° C. for 0.5 to 12 hours. The atmosphere in which the powder is held at 800° C. is not particularly limited, and examples thereof include air (air atmosphere), nitrogen atmosphere, and oxygen flow.

[0066] "The fourth step" In the fourth step, the powder held at 800° C. in the third step is cooled to 750° C. at a temperature drop rate of 5° C. / min to 25° C. / min, preferably 10° C. / min to 25° C. / min, and then the powder is held at 750° C. for 0.5 to 12 hours. The atmosphere in which the powder is held at 750° C. is not particularly limited, and examples thereof include air (air atmosphere), nitrogen atmosphere, and oxygen flow.

[0067] "The fifth step" In the fifth step, the powder held at 750° C. in the fourth step is cooled to 600° C. at a temperature drop rate of 5° C. / min to 25° C. / min, preferably 10° C. / min to 25° C. / min, and then the powder is held at 600° C. for 0.5 to 20 hours. The atmosphere in which the powder is held at 600° C. is not particularly limited, and examples thereof include air (air atmosphere), nitrogen atmosphere, and oxygen flow.

[0068] "The sixth step" In the sixth step, the powder held at 600°C in the fifth step is cooled at a temperature drop rate of 10°C / min to reach 400°C to 500°C, and then the powder is held at 400°C to 500°C for 0.5 hours to 30 hours. The sixth step may be a step of holding the powder at 450°C for 30 hours, and then holding the powder at 400°C for 30 hours. Alternatively, the sixth step may be a step of holding the powder at 500°C for 20 hours.

[0069] The slow cooling steps of the second to sixth steps described above can be appropriately changed or omitted as necessary. In one embodiment, the slow cooling step is performed by holding the material after the heat treatment at a temperature of 850° C. or higher and 950° C. or lower, preferably for 3 hours or higher and 12 hours or lower, more preferably for 4 hours or higher and 8 hours or lower, and most preferably for 6 hours. The positive electrode active material for lithium secondary batteries of the present invention can increase the Mn / Ni ratio on the particle surface of the lithium transition metal composite oxide by appropriately selecting the slow cooling conditions.

[0070] [Lithium secondary battery] The lithium secondary battery of the present invention is a lithium secondary battery comprising a positive electrode, a negative electrode, an electrolyte, and, as necessary, other battery elements, and the positive electrode contains a positive electrode active material mainly composed of the lithium transition metal composite oxide of the above-described embodiment.

[0071] The lithium secondary battery of the present invention can use the battery elements of known lithium secondary batteries as they are, except that the positive electrode contains a positive electrode active material mainly composed of the lithium transition metal composite oxide described above. The lithium secondary battery of the present invention may be of any of the following types: coin type, button type, cylindrical type, square type, and laminate type. The lithium secondary battery of the present invention can be used in a wide range of applications, such as for mobile devices such as mobile phones and notebook computers, and for in-vehicle use.

[0072] Hereinafter, a lithium secondary battery using an electrolytic solution (coin-type lithium secondary battery) will be described as an embodiment of the lithium secondary battery of the present invention. Each battery element described below can be similarly applied to an all-solid-state lithium secondary battery that does not use an electrolytic solution.

[0073] Fig. 9 is a cross-sectional view showing a schematic example of a lithium secondary battery according to this embodiment. Fig. 9 shows an example of the lithium secondary battery according to this embodiment, which is a coin-type lithium secondary battery. The lithium secondary battery 1 shown in Fig. 9 includes a negative electrode can (negative electrode terminal) 20, a negative electrode 3, a separator 4 impregnated with an electrolyte, an insulating packing (gasket) 5, a positive electrode 2, and a positive electrode can 10.

[0074] As shown in Fig. 9, the positive electrode can 10 is disposed on the lower side and the negative electrode can 20 is disposed on the upper side, with the positive electrode can 10 and the negative electrode can 20 forming the outer shape of the lithium secondary battery 1. A positive electrode 2 and a negative electrode 3 are provided between the positive electrode can 10 and the negative electrode terminal 20 via a separator 4 impregnated with an electrolyte, and the positive electrode 2 and the negative electrode 3 are separated by the separator 4. The positive electrode can 10 and the negative electrode can 20 are electrically insulated by an insulating packing 5.

[0075] In the lithium secondary battery of this embodiment, a conductive agent, a binder, etc. are mixed with the positive electrode active material for lithium secondary batteries of the above embodiment as necessary to prepare a positive electrode mixture, which is then pressed onto a current collector (not shown) to produce a positive electrode. As the current collector, preferably, stainless steel mesh, aluminum foil, etc. can be used. As the conductive agent, preferably, acetylene black, Ketchen black, etc. can be used. As the binder, preferably, tetrafluoroethylene, polyvinylidene fluoride, etc. can be used.

[0076] The blending of the positive electrode active material, conductive agent, and binder in the positive electrode mixture is not particularly limited. The content of the conductive agent in the positive electrode mixture is preferably 1 mass% to 15 mass%, more preferably 0.1 mass% to 5 mass%. The content of the binder in the positive electrode mixture is preferably 0.1 mass% to 10 mass%, more preferably 0.1 mass% to 5 mass%. It is preferable to blend the positive electrode active material, conductive agent, and binder so that the remainder of the positive electrode mixture (a portion other than the positive electrode active material and conductive agent) becomes the positive electrode active material.

[0077] In the lithium secondary battery of this embodiment, as the counter electrode to the positive electrode, any known material that functions as a negative electrode active material and can absorb and release lithium can be used, for example, metallic lithium, lithium alloys, and other metal-based materials, graphite, MCMB (mesocarbon microbeads), and other carbon-based materials, Si, Si alloys, silicon oxide, and other silicon-based materials.

[0078] The separator, battery container, and the like may be made of known battery elements.

[0079] The electrolyte may be a known electrolytic solution, solid electrolyte, etc. The electrolytic solution may be, for example, a solution in which an electrolyte such as lithium perchlorate or lithium hexafluorophosphate is dissolved in a solvent such as ethylene carbonate (EC), dimethyl carbonate (DMC), propylene carbonate (PC), or diethyl carbonate (DEC).

[0080] Moreover, the all-solid-state lithium secondary battery can also have the same structure as known all-solid-state lithium secondary batteries, except that a positive electrode active material containing the above-mentioned lithium transition metal composite oxide as a main component is used.

[0081] In the case of an all-solid-state lithium secondary battery, the electrolyte may be, for example, a polymer-based solid electrolyte such as a polyethylene oxide-based polymer compound, a polymer compound containing at least one of a polyorganosiloxane chain or a polyoxyalkylene chain, a sulfide-based solid electrolyte, or an oxide-based solid electrolyte.

[0082] For the positive electrode of the all-solid-state lithium secondary battery, for example, a positive electrode mixture containing a solid electrolyte in addition to the above-mentioned positive electrode active material, conductive agent, and binder can be supported on a positive electrode current collector made of aluminum, nickel, stainless steel, or the like.

[0083] The lithium secondary battery of this embodiment can achieve a high capacity because the positive electrode contains the positive electrode active material containing the above-mentioned lithium transition metal composite oxide as a main component. EXAMPLES

[0084] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0085] [Example 1] (Synthesis of lithium nickel manganese titanium oxide: Li 1.05 Ni 0.45 Mn 0.45 Ti 0.05 O2) Li2CO3 (Kojundo Kagaku), Ni 0.5 Mn 0.5 (OH)2 and TiO2 (Kojundo Chemical Co., Ltd.) were weighed out so that the molar ratio of Li:Ni:Mn:Ti was 1.05:0.45:0.45:0.05, and Li2CO3 was weighed out so that there was 2% more by mass than Li2CO3 based on the stoichiometric ratio, taking into account the evaporation of Li. 0.5 Mn 0.5The total mass of (OH)2 and TiO2 (manufactured by Kojundo Chemical) was 2.1 g. These were dispersed in ethanol in a mortar and mixed. Then, the mixture was filled into a platinum crucible of JIS standard. Using a firing furnace, the mixture filled into the platinum crucible was heated in air at a temperature increase rate of 15°C / min and fired at 1050°C for 5 minutes to obtain the lithium nickel manganese titanium oxide of Example 1.

[0086] (analysis) The chemical composition of the obtained sample was analyzed using an ICP emission spectrometer (product name: Agilent5110 VDV, manufactured by Agilent Technologies), and the results are shown in Table 1. As shown in Table 1, it was confirmed that the composition was Li:Ni:Mn:Ti = 1.05:0.44:0.46:0.05. In addition, the X-ray diffraction pattern of the obtained sample was measured using a powder X-ray diffractometer (product name: SmartLab, manufactured by Rigaku), and the lattice constant was calculated by the least squares method using each index and its interplanar spacing. The space group of the obtained sample was set to R-3m, and the lattice constants were calculated to be a = 2.88758(7) Å, c = 14.3078(5) Å, and c / a = 4.9549. The powder X-ray diffraction pattern is shown in Figure 3. The lattice constants are shown in Table 1. We also have an X-ray photoelectron spectroscopy (XPS) analyzer (product name: K-Alpha + The composition of the surface layer of the obtained sample was analyzed by quantitative analysis using a Thermo Fisher Scientific (manufactured by Thermo Fisher Scientific), and the results are shown in Table 1. As shown in Table 1, the Mn / Ni ratio in the surface layer was 1.20.

[0087] [Example 2] (Synthesis of lithium nickel manganese titanium oxide: Li 1.05 Ni 0.45 Mn 0.45 Ti 0.05 O2) Li2CO3 (Kojundo Kagaku), Ni 0.5 Mn 0.5(OH)2 and TiO2 (Kojundo Chemical Co., Ltd.) were weighed out so that the molar ratio of Li:Ni:Mn:Ti was 1.05:0.45:0.45:0.05, and Li2CO3 was weighed out so that there was 2% more by mass than Li2CO3 based on the stoichiometric ratio, taking into account the evaporation of Li. 0.5 Mn 0.5 The total mass of (OH)2 and TiO2 (manufactured by Kojundo Chemical) was 2.1 g. These were dispersed in ethanol in a mortar and mixed. Then, the mixture was filled into a platinum crucible of JIS standard. Using a firing furnace, the mixture filled into the platinum crucible was heated in air at a temperature increase rate of 15°C / min and fired at 1050°C for 5 minutes to obtain the lithium nickel manganese titanium oxide of Example 1. The powder after the heat treatment was cooled to 850° C. at a temperature drop rate of 10° C. / min, and then the powder was held at 850° C. in air for 6 hours. Thereafter, the powder was left to stand until its temperature reached room temperature, thereby obtaining the lithium nickel manganese titanium oxide of Example 2.

[0088] (analysis) The chemical composition of the obtained sample was analyzed in the same manner as in Example 1. The results are shown in Table 1. As shown in Table 1, it was confirmed that Li:Ni:Mn:Ti=1.09:0.44:0.42:0.05. In the chemical composition, Mn is reduced compared to Example 1 because Mn migrated to the surface layer of the obtained sample by heat treatment and further reached the platinum crucible. Li is increased compared to Example 1 because the total phase of the chemical composition was calculated as 2, and the reduced amount of Mn was allocated to Li. The reduced amount of Mn depends on the amount of precursor filled in the crucible. The space group of the obtained sample was determined to be R-3m, and all peaks could be indexed, confirming that it was a single phase. The lattice constants were determined to be a = 2.88675(7) Å, c = 14.3067(8) Å, and c / a = 4.9560. The powder X-ray diffraction pattern is shown in Figure 3. The lattice constants are shown in Table 1. The composition of the surface layer of the obtained sample was analyzed, and the results are shown in Table 1. As shown in Table 1, the Mn / Ni ratio in the surface layer was 1.47.

[0089] [Preparation of lithium secondary batteries] The lithium nickel manganese titanium oxide of Example 1 or the lithium nickel manganese titanium oxide of Example 2 was used as the positive electrode active material, acetylene black (AB) as the conductive agent, polyvinylidene fluoride (PVDF) as the binder, and NMP (N-methyl-2-pyrrolidone) as the solvent were mixed in a weight ratio of 8:1:1 to prepare a slurry. The slurry was then applied to an aluminum foil with a thickness of 15 μm and dried to prepare a positive electrode with a diameter of 14 mm. The coating area density was 4.5 mg / cm. 2 , volume density is 2.3g / cm 3 A lithium metal with a thickness of 200 μm and a diameter of 16 mm was used as the counter electrode for the positive electrode, and a polyethylene microporous membrane with a thickness of 20 μm and a diameter of 18 mm was used as the separator. The electrolyte was a 1.2 mol / L solution in which lithium hexafluorophosphate (LiPF6) was dissolved in a mixed solvent (volume ratio 3:4:3) of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC), and a lithium secondary battery (2032 coin cell) with the structure shown in FIG. 9 was fabricated. The battery was fabricated according to the known cell configuration and assembly method.

[0090] [Charge / discharge test] The charge / discharge characteristics of the prepared lithium secondary battery were evaluated by performing a charge / discharge test under a temperature condition of 55° C., a constant current at a rate of 0.05 C, a current density of 12.5 mA / g, and a cutoff potential of 4.7 V to 2.5 V. The charge / discharge test started with charging.

[0091] Fig. 5 shows charge / discharge curves in Examples 1 and 2. Fig. 5 shows voltage changes during discharge, in which the cell voltage decreases as the capacity increases, and voltage changes during charge, in which the cell voltage increases as the capacity increases.

[0092] 5, it was found that the lithium secondary battery using the lithium nickel manganese titanium oxide of Example 1 as the positive electrode active material has a higher capacity than the lithium secondary battery using the lithium nickel manganese titanium oxide of Example 2 as the positive electrode active material. In Example 2, too, if the heat treatment conditions are appropriately performed, a higher capacity can be achieved than in Example 1.

[0093] Furthermore, the obtained samples of Example 1 and Example 2 were analyzed by Li-MAS-NMR (product name: AVANCE300, manufactured by Bruker). The results are shown in FIG. 1. From the results shown in FIG. 1, 6 In the Li-MAS-NMR spectrum, there was no peak in the range of 1495 to 1505 ppm.

[0094] [Table 1]

[0095] [Example 3] (Synthesis of lithium nickel manganese titanium oxide: Li 1.07 Ni 0.40 Mn 0.40 Ti 0.13 O2) Li2CO3 (Kojundo Kagaku), Ni 0.5 Mn 0.5 (OH)2 and TiO2 (Kojundo Chemical Co., Ltd.) were weighed out so that the molar ratio of Li:Ni:Mn:Ti was 1.066:0.40:0.40:0.133, and Li2CO3 was weighed out so that there was 2% more by mass than Li2CO3 based on the stoichiometric ratio, taking into account the evaporation of Li. 0.5 Mn 0.5 The total mass of (OH)2 and TiO2 (manufactured by Kojundo Chemical) was set to 2.1 g. These were dispersed in ethanol in a mortar and mixed. Then, the mixture was filled into a platinum crucible of JIS standard. Using a firing furnace, the mixture filled into the platinum crucible was heated in air at a temperature increase rate of 15°C / min and fired at 1100°C for 5 minutes to obtain the lithium nickel manganese titanium oxide of Example 3. An electron microscope photograph of the obtained lithium nickel manganese titanium oxide is shown in FIG.

[0096] (analysis) The chemical composition of the obtained sample was analyzed in the same manner as in Example 1, and the results are shown in Table 2. As shown in Table 2, it was confirmed that Li:Ni:Mn:Ti=1.09:0.40:0.38:0.13. In the chemical composition, Mn is reduced compared to the charged composition because Mn migrated to the surface layer of the obtained sample by heat treatment and further reached the platinum crucible. Li is increased compared to Example 1 because the total phase of the chemical composition was calculated as 2, and the reduced amount of Mn was allocated to Li. The reduced amount of Mn depends on the amount of precursor filled in the crucible. The space group of the obtained sample was determined to be R-3m, and all peaks could be indexed, confirming that it was a single phase. The lattice constants were determined to be a = 2.89293(12) Å, c = 14.3323(7) Å, and c / a = 4.9543. The powder X-ray diffraction pattern is shown in Figure 4. The lattice constants are shown in Table 2. Moreover, the composition of the surface layer of the obtained sample was analyzed, and the results are shown in Table 2. As shown in Table 2, the Mn / Ni ratio in the surface layer was 1.06.

[0097] [Example 4] (Synthesis of lithium nickel manganese titanium oxide: Li 1.07 Ni 0.40 Mn 0.40 Ti 0.13 O2) Li2CO3 (Kojundo Kagaku), Ni 0.5 Mn 0.5 (OH)2 and TiO2 (Kojundo Chemical Co., Ltd.) were weighed out so that the molar ratio of Li:Ni:Mn:Ti was 1.066:0.40:0.40:0.133, and Li2CO3 was weighed out so that there was 2% more by mass than Li2CO3 based on the stoichiometric ratio, taking into account the evaporation of Li. 0.5 Mn 0.5The total mass of (OH)2 and TiO2 (manufactured by Kojundo Chemical) was 2.1 g. These were dispersed in ethanol in a mortar and mixed. Then, the mixture was filled into a platinum crucible of JIS standard. Using a firing furnace, the mixture filled into the platinum crucible was heated in air at a temperature increase rate of 15°C / min and fired at 1100°C for 5 minutes to obtain the lithium nickel manganese titanium oxide of Example 3. The powder after the heat treatment was cooled to 900° C. at a temperature drop rate of 10° C. / min, and then the powder was held at 900° C. in air for 6 hours or less. The powder was then left to cool to room temperature to obtain the lithium nickel manganese titanium oxide of Example 4. An electron microscope photograph of the obtained lithium nickel manganese titanium oxide is shown in Figure 8. Comparing Figures 7 and 8, it was confirmed that the surface morphology had changed due to the slow cooling process.

[0098] (analysis) The chemical composition of the obtained sample was analyzed in the same manner as in Example 3, and the results are shown in Table 2. As shown in Table 2, it was confirmed that Li:Ni:Mn:Ti=1.09:0.40:0.38:0.13. In the chemical composition, the Mn content is reduced compared to the charged composition because Mn migrated to the surface layer of the obtained sample by heat treatment and further reached the platinum crucible. The Li content is increased compared to Example 1, presumably because the total phase of the chemical composition was calculated as 2, and the reduced amount of Mn was allocated to Li. The reduced amount of Mn depends on the amount of precursor filled in the crucible. In addition, the space group of the obtained sample was determined to be R-3m, and all peaks could be indexed, confirming that it was a single phase, in the same manner as in Example 3. Furthermore, the lattice constants were determined to be a = 2.89424(8) Å, c = 14.3366(6) Å, and c / a = 4.9535. The X-ray diffraction pattern is shown in Figure 4. The lattice constants are shown in Table 2. Moreover, the composition of the surface layer of the obtained sample was analyzed in the same manner as in Example 3, and the results are shown in Table 2. As shown in Table 2, the Mn / Ni ratio in the surface layer was 1.08.

[0099] [Preparation of lithium secondary batteries] The lithium nickel manganese titanium oxide of Example 3 or the lithium nickel manganese titanium oxide of Example 4 was used as the positive electrode active material, acetylene black (AB) as the conductive agent, polyvinylidene fluoride (PVDF) as the binder, and NMP (N-methyl-2-pyrrolidone) as the solvent were mixed in a weight ratio of 8:1:1 to prepare a slurry. The slurry was then applied to an aluminum foil with a thickness of 15 μm and dried to prepare a positive electrode with a diameter of 14 mm. The coating area density was 4.5 mg / cm. 2 , volume density is 2.3g / cm 3 A lithium metal with a thickness of 200 μm and a diameter of 16 mm was used as the counter electrode for the positive electrode, and a polyethylene microporous membrane with a thickness of 20 μm and a diameter of 18 mm was used as the separator. The electrolyte was a 1.2 mol / L solution in which lithium hexafluorophosphate (LiPF6) was dissolved in a mixed solvent (volume ratio 3:4:3) of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC), and a lithium secondary battery (2032 coin cell) with the structure shown in FIG. 9 was fabricated. The battery was fabricated according to the known cell configuration and assembly method.

[0100] [Charge / discharge test] The charge / discharge characteristics of the prepared lithium secondary battery were evaluated by performing a charge / discharge test under a temperature condition of 55° C., a constant current at a rate of 0.05 C, a current density of 12.5 mA / g, and a cutoff potential of 4.7 V to 2.5 V. The charge / discharge test started with charging.

[0101] Fig. 6 shows charge / discharge curves in Examples 3 and 4. Fig. 6 shows voltage changes during discharge, in which the cell voltage decreases as the capacity increases, and voltage changes during charge, in which the cell voltage increases as the capacity increases.

[0102] As shown in Fig. 6, it was found that the lithium secondary battery using the lithium nickel manganese titanium oxide of Example 4 as the positive electrode active material had a higher capacity than the lithium secondary battery using the lithium nickel manganese titanium oxide of Example 3 as the positive electrode active material. From the results shown in Fig. 6, it was confirmed that the lithium nickel manganese titanium oxide of Example 4 can increase the capacity of the lithium secondary battery.

[0103] Furthermore, the obtained sample was analyzed by Li-MAS-NMR (product name: AVANCE300, manufactured by Bruker). The results are shown in FIG. 2. From the results shown in FIG. 2, 6 In the Li-MAS-NMR spectrum, there was no peak in the range of 1495 to 1505 ppm.

[0104] [Table 2] [Explanation of symbols]

[0105] 1. Lithium secondary battery 2 Positive electrode 3 Negative electrode 4. Separator impregnated with electrolyte 5 Insulating packing (gasket) 10 Positive electrode can 20 Negative can (negative terminal)

Claims

1. A positive electrode active material for a lithium secondary battery, the positive electrode active material comprising a lithium transition metal composite oxide as a main component, The lithium transition metal composite oxide is in the form of particles having a layered structure consisting of a lithium layer and a transition metal-lithium layer, The lithium transition metal composite oxide has the general formula (1): Li m Ni x Mn y Ti z O 2 (wherein m is in the range of 1.0<m≦1.1, x is in the range of 0.4≦x<0.5, y is in the range of 0.3<y<0.5, and z is in the range of 0<z≦0.133), The lithium transition metal composite oxide has lattice constants (a, c, c / a) of an a-axis length of 2.886 Å to 2.900 Å, a c-axis length of 14.29 Å to 14.35 Å, and c / a of 4.940 to 4.

960.

2. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein, in the general formula (1), m is in the range of 1.05≦m≦1.066, x is in the range of 0.4≦x≦0.475, y is in the range of 0.4≦y≦0.475, and z is in the range of 0.05≦z≦0.

133.

3. 2. The positive electrode active material for lithium secondary batteries according to claim 1, wherein a ratio of the number of Mn atoms to the number of Ni atoms (Mn / Ni ratio) on the surface of a particle of the lithium transition metal composite oxide is greater than 1.0 and less than 2.

5.

4. Solid-state lithium nuclear magnetic resonance analysis using magic angle sample spinning ( 6 2. The positive electrode active material for lithium secondary batteries according to claim 1, wherein in a spectrum of the lithium transition metal composite oxide measured by Li-MAS-NMR, the peak intensity ratio at 1500 ppm / 600 ppm is 0.15 or less.

5. Solid-state lithium nuclear magnetic resonance analysis ( 6 2. The positive electrode active material for lithium secondary batteries according to claim 1, wherein in a spectrum of the lithium transition metal composite oxide measured by Li-MAS-NMR, a peak due to lithium contained in the transition metal-lithium layer does not exist at 1500 ppm.

6. A lithium secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, the positive electrode containing the positive electrode active material for lithium secondary batteries according to any one of claims 1 to 5.

7. 7. The lithium secondary battery according to claim 6, wherein the electrolyte is a solid electrolyte.

8. A method for producing a positive electrode active material for a lithium secondary battery according to any one of claims 1 to 5, A method for producing a positive electrode active material for a lithium secondary battery, comprising the steps of: heat-treating a mixture of a lithium compound, a titanium compound, and a nickel manganese compound at 1000° C. or more and 1200° C. or less for 1 minute or more and 7 hours or less; or heat-treating a mixture of a lithium compound and a nickel manganese titanium compound at 1000° C. or more and 1200° C. or less for 1 minute or more and 7 hours or less.

9. The method for producing a positive electrode active material for a lithium secondary battery according to claim 8, further comprising the step of subsequently holding the obtained lithium transition metal composite oxide at 850°C or higher and 950°C or lower for 3 hours or higher and 12 hours or lower after the heat treatment step.

Citation Information

Patent Citations

  • Preparation method for surface-modified lithium-manganese-rich cathode material of lithium ion battery

    CN104577101A

  • Lithium-containing transition metal multiple oxide and manufacturing method thereof

    JP2002145623A

  • Nonaqueous electrolyte secondary battery

    JP2003168430A

  • Positive electrode for lithium-ion secondary battery, and lithium-ion secondary battery

    JP2005085720A

  • Positive electrode for lithium secondary batteries, and lithium secondary battery

    JP2005235628A