Substrate processing method, substrate processing apparatus, method for manufacturing semiconductor device and apparatus for manufacturing semiconductor
The substrate processing method efficiently forms a self-assembled monolayer with high density and protective performance by using a treatment liquid, removal, and annealing steps to repair defects, addressing the inefficiencies of conventional methods.
Patent Information
- Application Number
- JP2023044732
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods struggle to form a self-assembled monolayer (SAM) with high density and protective performance efficiently and in a short time, particularly due to issues with film defects and poor production efficiency.
A substrate processing method involving a film forming step with a treatment liquid, a removal step to eliminate unadsorbed molecules, and an annealing step to repair defects, including low and high-temperature annealing, and rapid cooling to form a dense and defect-free SAM.
The method enables the formation of a self-assembled monolayer with high film density and excellent protective performance in a shorter time, reducing film defects and improving production efficiency.
Smart Images

Figure 2024134431000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate processing method and substrate processing apparatus capable of efficiently forming a self-assembled monolayer having excellent density and protective performance in a short time, as well as a semiconductor device manufacturing method and semiconductor manufacturing apparatus. [Background technology]
[0002] In the manufacture of semiconductor devices, photolithography is widely used as a technique for selectively forming a film on a specific surface region of a substrate. For example, after forming a lower layer wiring, an insulating film is formed, and a dual damascene structure having trenches and via holes is formed by photolithography and etching, and a conductive film such as Cu is embedded in the trenches and via holes to form wiring.
[0003] However, in recent years, semiconductor devices have become increasingly miniaturized, and there are cases where the alignment accuracy of photolithography is insufficient. For this reason, there is a demand for an alternative to photolithography to selectively form a film in a specific region on the substrate surface with high accuracy.
[0004] For example, Patent Document 1 discloses a method for selectively etching a silicon nitride (SiN) film and a silicon oxide (SiO2) film on a substrate, in which a thermal phosphoric acid resistant material is formed as a SAM on the surface of the silicon oxide film in advance in order to selectively etch the silicon nitride film.
[0005] In order to adequately protect the silicon oxide film from the etching solution, it is necessary to form a highly dense SAM. However, with conventional SAM deposition methods, it is difficult to deposit such a highly dense SAM in a short time, resulting in poor production efficiency. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent No. 5490071 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a substrate processing method and substrate processing apparatus, as well as a semiconductor device manufacturing method and semiconductor manufacturing apparatus, which are capable of efficiently forming a self-assembled monolayer having excellent density and protective performance on a substrate surface in a short time by suppressing or reducing the occurrence of film defects. [Means for solving the problem]
[0008] In order to solve the above-mentioned problems, the substrate processing method according to the present invention is a substrate processing method for forming a self-assembled monolayer on a surface of a substrate, and is characterized by comprising a film formation step of contacting a processing liquid containing molecules capable of forming the self-assembled monolayer with the surface to chemically adsorb the molecules and form the self-assembled monolayer, a removal step of contacting a removal liquid with the surface of the substrate after the film formation step to remove at least a portion of the molecules that are not chemically adsorbed, and an annealing step of heating the substrate after the removal step.
[0009] According to the above-mentioned configuration, in the film formation step, molecules capable of forming a self-assembled monolayer (hereinafter, sometimes referred to as "SAM molecules") (hereinafter, sometimes referred to as "SAM molecules") are chemically adsorbed on the surface of the substrate and self-assembled to form a SAM. Then, in the removal step, a removal liquid is brought into contact with the surface of the substrate to remove at least a portion of the SAM molecules that are not chemically adsorbed. Here, in the SAM formed in the film formation step, film defects may occur because the SAM molecules cannot be locally chemically adsorbed on the surface of the substrate. In particular, when the contact time of the SAM molecules with the substrate surface is short, the frequency of occurrence of film defects in the surface increases, or the area of the film defects becomes large. However, in the above-mentioned configuration, since the substrate after the removal step is heated in the annealing step, such film defects can be repaired. As a result, unlike the conventional substrate processing method, even if the SAM molecules are not brought into contact with the substrate surface for a long time in order to form a dense SAM, the occurrence of film defects is suppressed, and a SAM with excellent denseness and protective performance can be efficiently formed in a short time.
[0010] In the above-mentioned configuration, the removal step is performed after the SAM film formation step and before the annealing step in order to prevent excess unadsorbed SAM molecules from remaining on the substrate surface. This prevents the formation of a good monolayer from being hindered. In other words, if the annealing step is performed in a state where excess unadsorbed SAM molecules remain on the substrate surface, a film made of unadsorbed SAM molecules will be formed on the SAM formed on the substrate surface. Therefore, by removing at least a portion of the unadsorbed SAM molecules with a removal solution, a good monolayer can be formed.
[0011] In the above configuration, the annealing process can include at least one of a low-temperature annealing process in which the substrate is heated to a temperature range higher than room temperature and not exceeding 100°C, and a high-temperature annealing process in which the substrate is heated to a temperature range higher than 100°C and not exceeding 200°C.
[0012] According to the above-mentioned configuration, the low-temperature annealing process rearranges the SAM molecules chemically adsorbed on the substrate surface. This allows the SAM molecules to be rearranged in the area of the film defect that occurs due to the lack of chemisorption, and the film defect can be repaired. In addition, the high-temperature annealing process promotes a dehydration condensation reaction between the SAM molecules that remain after the removal process and the SAM molecules chemically adsorbed on the substrate surface. This allows the SAM molecules to be re-chemically adsorbed in the area of the film defect that occurs due to the lack of chemisorption, and the film defect can be repaired.
[0013] In the above-described configuration, the annealing step may be a step performed in an atmosphere containing at least water.
[0014] The above-mentioned method may further include a cooling step of rapidly cooling the substrate to room temperature after the annealing step.
[0015] If the SAM formed on the substrate surface is in a crystalline state, grain boundaries will form within the SAM surface, and these grain boundaries will become film defects. However, by rapidly cooling the substrate to room temperature after the annealing process, the SAM can be made amorphous. This prevents grain boundaries from forming within the surface, further suppressing the occurrence of film defects.
[0016] In order to solve the above-mentioned problems, the manufacturing method of a semiconductor device of the present invention is a manufacturing method of a semiconductor device including processing a substrate having a laminate provided on its surface, the laminate including an alternately stacked protected layer to be protected during etching and an etched layer to be etched, the method including a step of selectively forming a self-assembled monolayer on at least the surface of the protected layer, and a step of selectively etching the etched layer using the self-assembled monolayer as a protective layer, the step of forming the self-assembled monolayer including a film formation step of contacting a treatment liquid including molecules capable of forming the self-assembled monolayer with the surface of the protected layer to chemically adsorb the molecules, a removal step of contacting a removal liquid with the surface of the protected layer after the film formation step to remove at least a portion of the molecules that are not chemically adsorbed, and an annealing step of heating the protected layer after the removal step.
[0017] According to the above-mentioned configuration, in the film formation step, the SAM molecules are chemically adsorbed on the surface of the protected layer and self-organized to form a SAM. Then, in the removal step, a removal liquid is brought into contact with the surface of the protected layer to remove at least a portion of the SAM molecules that are not chemically adsorbed. Here, in the SAM formed in the film formation step, the SAM molecules may not be able to be locally chemically adsorbed on the surface of the protected layer, and film defects may occur. In particular, when the contact time of the SAM molecules with the surface of the protected layer is short, the frequency of film defects in the surface increases, or the area of the film defects becomes large. However, in the above-mentioned configuration, since the substrate after the removal step is heated in the annealing step, such film defects of the SAM can be repaired. As a result, unlike the conventional semiconductor device manufacturing method, even if the SAM molecules are not brought into contact with the surface of the protected layer for a long time to form a dense SAM, the occurrence of film defects can be suppressed, and a SAM with excellent denseness and protective performance can be efficiently formed in a short time.
[0018] In the above-mentioned configuration, the removal step is performed after the SAM film formation step and before the annealing step in order to prevent excess unadsorbed SAM molecules from remaining on the surface of the protected layer. This prevents the formation of a good monolayer from being hindered. In other words, if the annealing step is performed in a state where excess unadsorbed SAM molecules remain on the surface of the protected layer, a film made of unadsorbed SAM molecules will be formed on the SAM formed on the surface of the protected layer. Therefore, by removing at least a portion of the unadsorbed SAM molecules with a removal solution, a good monolayer can be formed.
[0019] In the above configuration, the annealing process can include at least one of a low-temperature annealing process in which the protected layer is heated to a temperature range higher than room temperature and not higher than 100°C, and a high-temperature annealing process in which the protected layer is heated to a temperature range higher than 100°C and not higher than 200°C.
[0020] According to the above-mentioned configuration, the low-temperature annealing process rearranges the SAM molecules chemically adsorbed on the surface of the protected layer. This allows the SAM molecules to be rearranged in the area of the film defect that occurs due to the lack of chemisorption, and the film defect can be repaired. In addition, the high-temperature annealing process promotes a dehydration condensation reaction between the SAM molecules that remain after the removal process and the SAM molecules chemically adsorbed on the surface of the protected layer. This allows the SAM molecules to be re-chemically adsorbed in the area of the film defect that occurs due to the lack of chemisorption, and the film defect can be repaired.
[0021] In the above-described configuration, the annealing step may be a step performed in an atmosphere containing at least water.
[0022] The above-mentioned method may further include a cooling step of rapidly cooling the substrate to room temperature after the annealing step.
[0023] If the SAM formed on the surface of the protected layer is in a crystalline state, grain boundaries will form within the SAM's surface, and these grain boundaries will become film defects. However, by rapidly cooling the substrate to room temperature after the annealing process, the SAM can be made amorphous. This prevents grain boundaries from forming within the surface, further reducing the occurrence of film defects.
[0024] In order to solve the above-mentioned problems, the substrate processing apparatus of the present invention is a substrate processing apparatus that forms a self-assembled monolayer on a surface of a substrate, and is characterized by comprising: a supply unit that forms the self-assembled monolayer by supplying a processing liquid containing molecules capable of forming the self-assembled monolayer to the surface, a removal liquid supply unit that removes at least a portion of the molecules that are not chemically adsorbed by supplying a removal liquid to the surface of the substrate after the processing liquid has been supplied, and an annealing unit that heats the substrate after at least a portion of the molecules has been removed.
[0025] According to the above-mentioned configuration, the supply unit supplies a processing solution containing SAM molecules to the surface of the substrate, and the SAM molecules are chemically adsorbed to the substrate surface and self-organized to form a SAM. The remover supply unit removes at least a portion of the SAM molecules that are not chemically adsorbed by contacting the remover with the substrate surface. Here, in the SAM formed on the substrate surface, film defects may occur because the SAM molecules cannot be locally chemically adsorbed to the substrate surface. In particular, when the contact time of the SAM molecules with the substrate surface is short, the frequency of film defects in the surface increases, or the area of the film defects becomes large. However, the above-mentioned configuration further includes an annealing unit that heats the substrate after removing at least a portion of the SAM molecules. As a result, the above-mentioned configuration can repair the film defects of the SAM, and can suppress the occurrence of film defects and efficiently form a SAM with excellent density and protection performance in a short time without contacting the SAM molecules with the substrate surface for a long time to form a dense SAM, as in the conventional substrate processing apparatus.
[0026] In the above configuration, the removal liquid supply unit is provided in order to prevent excess unadsorbed SAM molecules from remaining on the substrate surface. This prevents the formation of a good monolayer from being hindered. In other words, if annealing is performed with excess unadsorbed SAM molecules remaining on the substrate surface, a film made of unadsorbed SAM molecules will be formed on the SAM formed on the substrate surface. Therefore, by removing at least a portion of the unadsorbed SAM molecules with a removal liquid, a good monolayer can be formed.
[0027] In the above configuration, the annealing section can perform low-temperature annealing by heating the substrate after at least a portion of the molecules has been removed to a temperature range of higher than room temperature and not exceeding 100°C, and / or can perform high-temperature annealing by heating the substrate after at least a portion of the molecules has been removed to a temperature range of higher than 100°C and not exceeding 200°C.
[0028] According to the above configuration, the annealing unit performs low-temperature annealing on the substrate after removing at least a part of the SAM molecules at a temperature higher than room temperature and not higher than 100°C, thereby rearranging the SAM molecules chemically adsorbed on the substrate surface. This allows the SAM molecules to be rearranged in the region of the film defect where the SAM molecules are not chemically adsorbed, making it possible to form a SAM with the film defect repaired. In addition, by performing high-temperature annealing at a temperature higher than 100°C and not higher than 200°C, it is possible to promote a dehydration condensation reaction between the SAM molecules remaining without being removed by the removing solution and the SAM molecules chemically adsorbed on the substrate surface. This allows the SAM molecules to be re-chemically adsorbed in the region of the film defect where the SAM molecules are not chemically adsorbed, making it possible to form a SAM with the film defect repaired.
[0029] In the above-described configuration, the annealing section may heat the substrate in an atmosphere containing at least water.
[0030] The above-mentioned configuration may further comprise a cooling section for rapidly cooling the substrate to room temperature after heating in the annealing section.
[0031] If the SAM formed on the surface of the protected layer is in a crystalline state, grain boundaries will form within the SAM's plane, and these grain boundaries will become film defects. However, by providing a cooling section and enabling the substrate to be rapidly cooled to room temperature after annealing, an amorphous SAM can be formed. As a result, it is possible to form a SAM that suppresses the formation of grain boundaries within the plane and further suppresses the occurrence of film defects.
[0032] In order to solve the above-mentioned problems, the semiconductor manufacturing apparatus of the present invention is a semiconductor manufacturing apparatus that processes a substrate having a laminate provided on its surface, the laminate including an alternating layer of a protected layer that is to be protected by etching and an etched layer that is to be etched, and is characterized in that it comprises: a supply unit that forms the self-assembled monolayer by supplying a treatment liquid including molecules capable of forming a self-assembled monolayer to the surface; a removal liquid supply unit that removes at least a portion of the molecules that are not chemically adsorbed by supplying a removal liquid to the surface of the substrate after the treatment liquid has been supplied; an annealing unit that heats the substrate after at least a portion of the molecules has been removed; and an etching unit that selectively etches and removes the etched layer using the self-assembled monolayer as a protective layer.
[0033] The semiconductor manufacturing apparatus of the above configuration forms a SAM on at least the surface of the layer to be protected before etching the layer to be etched, thereby enabling excellent selective etching of the layer to be etched. In the above configuration, the supply unit supplies a processing liquid containing SAM molecules to the surface of the substrate, and the SAM molecules are chemically adsorbed to the substrate surface and self-organized to form a SAM. The remover supply unit removes at least a portion of the SAM molecules that are not chemically adsorbed by contacting the substrate surface with the remover. Here, in the SAM formed on the substrate surface, the SAM molecules may not be able to be locally chemically adsorbed to the substrate surface, resulting in film defects. In particular, when the contact time of the SAM molecules with the substrate surface is short, the frequency of film defects in the surface increases, or the area of the film defects becomes large. However, the above configuration further includes an annealing unit that heats the substrate after removing at least a portion of the SAM molecules. As a result, with the above configuration, film defects in the SAM can be repaired, and the occurrence of film defects can be suppressed without the need to keep the SAM molecules in contact with the substrate surface for a long period of time to form a dense SAM, as is the case with conventional semiconductor manufacturing equipment, and a SAM with excellent density and protective performance can be efficiently formed in a short period of time.
[0034] In the above configuration, the removal liquid supply unit is provided in order to prevent excess unadsorbed SAM molecules from remaining on the substrate surface. This prevents the formation of a good monolayer from being hindered. In other words, if annealing is performed with excess unadsorbed SAM molecules remaining on the substrate surface, a film made of unadsorbed SAM molecules will be formed on the SAM formed on the substrate surface. Therefore, by removing at least a portion of the unadsorbed SAM molecules with a removal liquid, a good monolayer can be formed.
[0035] In order to solve the above-mentioned problems, another semiconductor manufacturing apparatus of the present invention is a semiconductor manufacturing apparatus for processing a substrate having a laminate provided on its surface, the laminate including an alternately stacked protected layer to be protected by etching and an etched layer to be etched, the apparatus comprising: a substrate processing unit for selectively forming a self-assembled monolayer on at least the surface of the protected layer; and an etching processing unit for selectively etching and removing the etched layer using the self-assembled monolayer as a protective layer, the substrate processing unit comprising: a supply unit for forming the self-assembled monolayer by supplying a processing liquid containing molecules capable of forming the self-assembled monolayer to the surface of the substrate; a removal liquid supply unit for removing at least a portion of the molecules that are not chemically adsorbed by supplying a removal liquid to the surface of the substrate after the processing liquid has been supplied; and an annealing unit for heating the substrate after the removal of at least a portion of the molecules.
[0036] The semiconductor manufacturing apparatus of the above configuration includes at least a substrate processing unit for selectively forming a SAM on a layer to be protected, and an etching processing unit for selectively etching and removing the layer to be etched. Before etching the layer to be etched in the etching processing unit, a SAM is formed on at least the surface of the layer to be protected in the substrate processing unit to protect the layer to be etched, thereby enabling excellent selective etching of the layer to be etched. In the above configuration, the supply unit supplies a processing liquid containing SAM molecules to the surface of the substrate, thereby forming a SAM by chemically adsorbing the SAM molecules to the substrate surface and self-organizing the SAM. In addition, the removal liquid supply unit removes at least a portion of the SAM molecules that are not chemically adsorbed by contacting the substrate surface with the removal liquid. Here, in the SAM formed on the substrate surface, film defects may occur because the SAM molecules cannot be locally chemically adsorbed to the substrate surface. In particular, when the contact time of the SAM molecules with the substrate surface is short, the frequency of occurrence of film defects in the surface increases, or the area of the film defects becomes large. However, the above configuration further includes an annealing unit for heating the substrate after removing at least a portion of the SAM molecules. As a result, with the above configuration, film defects in the SAM can be repaired, and the occurrence of film defects can be suppressed without the need to keep the SAM molecules in contact with the substrate surface for a long period of time to form a dense SAM, as is the case with conventional semiconductor manufacturing equipment, and a SAM with excellent density and protective performance can be efficiently formed in a short period of time.
[0037] In the above configuration, the removal liquid supply unit is provided in order to prevent excess unadsorbed SAM molecules from remaining on the substrate surface. This prevents the formation of a good monolayer from being hindered. In other words, if annealing is performed with excess unadsorbed SAM molecules remaining on the substrate surface, a film made of unadsorbed SAM molecules will be formed on the SAM formed on the substrate surface. Therefore, by removing at least a portion of the unadsorbed SAM molecules with a removal liquid, a good monolayer can be formed.
[0038] In the above configuration, the annealing section can perform low-temperature annealing by heating the substrate after at least a portion of the molecules has been removed to a temperature range of higher than room temperature and not exceeding 100°C, and / or can perform high-temperature annealing by heating the substrate after at least a portion of the molecules has been removed to a temperature range of higher than 100°C and not exceeding 200°C.
[0039] According to the above configuration, the annealing unit performs low-temperature annealing on the substrate after removing at least a part of the SAM molecules at a temperature higher than room temperature and not higher than 100°C, thereby rearranging the SAM molecules chemically adsorbed on the surface of the protected layer. This allows the SAM molecules to be rearranged in the region of the film defect where the SAM molecules are not chemically adsorbed, making it possible to form a SAM with the film defect repaired. In addition, by performing high-temperature annealing at a temperature higher than 100°C and not higher than 200°C, it is possible to promote a dehydration condensation reaction between the SAM molecules remaining without being removed by the removing solution and the SAM molecules chemically adsorbed on the surface of the protected layer. This allows the SAM molecules to be re-chemically adsorbed in the region of the film defect where the SAM molecules are not chemically adsorbed, making it possible to form a SAM with the film defect repaired.
[0040] In the above-described configuration, the annealing section may heat the substrate in an atmosphere containing at least water.
[0041] The above-mentioned configuration may further comprise a cooling section for rapidly cooling the substrate to room temperature after heating in the annealing section.
[0042] If the SAM formed on the surface of the protected layer is in a crystalline state, grain boundaries will form within the SAM's plane, and these grain boundaries will become film defects. However, by providing a cooling section and enabling the substrate to be rapidly cooled to room temperature after annealing, an amorphous SAM can be formed. As a result, it is possible to form a SAM that suppresses the formation of grain boundaries within the plane and further suppresses the occurrence of film defects. Effect of the Invention
[0043] According to the present invention, it is possible to provide a substrate processing method and substrate processing apparatus, as well as a semiconductor device manufacturing method and semiconductor manufacturing apparatus, which are capable of forming a self-assembled monolayer on a substrate surface which has high film density and excellent compactness, in which the occurrence of film defects is effectively suppressed or reduced, and which has excellent protective performance, in a shorter time and more efficiently than conventional film formation methods. [Brief description of the drawings]
[0044] [Figure 1] 1A and 1B are cross-sectional views each showing a schematic representation of a laminate provided on a substrate, in which FIG. 1A shows the state before an etching step, and FIG. 1B shows the state after the etching step. [Diagram 2] FIG. 2(a) is a partial enlarged view of the portion surrounded by A in the laminate in FIG. 1(a), FIG. 2(b) is a partial enlarged view showing the formation of a SAM on the surface of the SiO2 layer, and FIG. 2(c) is a partial enlarged view of the portion surrounded by B in the laminate in FIG. 1(b), showing the etching of the SiN layer. [Diagram 3] 3 is a flowchart showing an example of an overall flow of a method for manufacturing a semiconductor device according to a first embodiment of the present invention. [Figure 4] FIG. 4(a) is a schematic diagram showing how a treatment liquid is supplied to the surface of a SiO2 layer in the first embodiment, FIG. 4(b) is a schematic diagram showing how a SAM molecule is chemically adsorbed onto the surface of the SiO2 layer, and FIG. 4(c) is a schematic diagram showing how the SAM molecule self-organizes on the surface of the SiO2 layer to form a SAM. [Diagram 5] Figure 5(a) is a schematic diagram showing how at least a portion of the excess SAM molecules are removed from the surface of the SiO2 layer in the removal process, Figure 5(b) is a schematic cross-sectional diagram showing how an annealing process is performed on the substrate W, and Figure 5(c) is a schematic diagram showing how the SAM is densified. [Figure 6] 1 is an explanatory diagram illustrating a schematic configuration of a semiconductor manufacturing apparatus according to a first embodiment of the present invention. [Figure 7] 1 is an explanatory diagram illustrating a schematic configuration of a processing liquid storage section provided in a supply section in a semiconductor manufacturing apparatus according to a first embodiment of the present invention. FIG. [Figure 8] 2 is an explanatory diagram illustrating a schematic configuration of a removing liquid reservoir provided in a removing liquid supply unit in the semiconductor manufacturing apparatus according to the first embodiment of the present invention. FIG. [Figure 9] 1 is a block diagram showing a schematic configuration of an inert gas reservoir in an inert gas supply unit in a semiconductor manufacturing apparatus according to a first embodiment of the present invention. [Figure 10] FIG. 2 is an enlarged view of a main part for explaining an annealing step performed by an annealing / cooling unit in the first embodiment of the present invention. [Figure 11] FIG. 4 is an enlarged view of a main part for explaining another annealing step by the annealing / cooling unit in the first embodiment of the present invention. [Figure 12] 1 is a block diagram showing a schematic configuration of a coolant reservoir in an annealing / cooling unit in a semiconductor manufacturing apparatus according to a first embodiment of the present invention. [Figure 13] 1 is an explanatory diagram illustrating a schematic configuration of an etching liquid storage unit in an etching liquid supply unit in a semiconductor manufacturing apparatus according to a first embodiment of the present invention. FIG. [Figure 14] FIG. 2 is an enlarged view of a main part for explaining a drying step of a rinsing liquid in the first embodiment of the present invention. [Figure 15] 10 is a flowchart showing an example of an overall flow of a method for manufacturing a semiconductor device according to a second embodiment of the present invention. [Figure 16] FIG. 11 is an explanatory diagram illustrating a schematic configuration of a substrate processing unit in a semiconductor manufacturing apparatus according to a second embodiment of the present invention. [Figure 17] FIG. 11 is a block diagram showing a schematic configuration of a water vapor reservoir in a water vapor supply unit in a semiconductor manufacturing apparatus according to a second embodiment of the present invention. [Figure 18] FIG. 11 is a cross-sectional view showing a state in which a plurality of substrates on which a SAM is formed are immersed in an etching solution in a second embodiment of the present invention. [Figure 19] 11 is a side view showing a schematic configuration of a lifter in a semiconductor manufacturing apparatus according to a second embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] (First embodiment) A first embodiment of the present invention will be described below.
[0046] [Substrate Processing Method (Semiconductor Device Manufacturing Method)] First, a substrate processing method according to the present embodiment will be described below with reference to the drawings. The substrate processing method of the present embodiment provides a technique for enabling good selective etching when forming a three-dimensional structure, such as a three-dimensional NAND structure, on the surface of a substrate.
[0047] The substrate processing method of this embodiment is applicable to a part of a process for forming a three-dimensional NAND structure on a substrate W made of silicon or the like. Therefore, hereinafter, an example in which the substrate processing method of this embodiment is applied to a manufacturing method of a semiconductor device, more specifically, a case in which processing is performed on a substrate W provided with a three-dimensional stack 3 as shown in Fig. 1 will be described. Fig. 1 is a cross-sectional view that shows a schematic representation of a stack provided on a substrate W, where Fig. 1(a) shows a state before an etching process and Fig. 1(b) shows a state after the etching process.
[0048] 2(a), the laminate 3 includes a structure in which SiO2 layers 1 functioning as interlayer insulating layers and SiN layers 2 functioning as sacrificial layers are alternately laminated on a substrate W. The laminate 3 also includes a plurality of memory trenches 4 extending through the laminate 3 in a direction perpendicular to the surface of the substrate W. FIG. 2(a) is a partial enlarged view of a portion surrounded by A in the laminate in FIG.
[0049] The method for manufacturing a semiconductor device according to this embodiment includes at least a self-assembled monolayer (hereinafter referred to as "SAM") formation step S1 and an etching step S2, as shown in Fig. 3, and enables selective etching of the SiN layer 2 through the memory trench 4 to form a recess on the side surface of the memory trench 4 in the stack 3. Fig. 3 is a flowchart showing an example of the overall flow of the method for manufacturing a semiconductor device according to this embodiment.
[0050] <SAM Formation Process> The SAM formation process S1 is a process of selectively forming a SAM as a protective layer on the surface of the SiO2 layer 1 which is the layer to be protected. As shown in FIG. 3, the SAM formation process S1 includes at least a film formation process S101, a removal process S102, a drying process S103, an annealing process S104, and a cooling process S105. Note that the SAM formation process S1 corresponds to the substrate processing method of the present invention.
[0051] 1. Film formation process The film formation process S101 is a process of bringing a treatment liquid containing a material capable of forming a SAM (hereinafter referred to as "SAM formation material") into contact with the surface of the substrate W to form a SAM.
[0052] The method of bringing the treatment liquid into contact with the substrate W is not particularly limited, and examples thereof include a method of applying the treatment liquid to the surface of the substrate W, a method of spraying the treatment liquid onto the surface of the substrate W, and a method of immersing the substrate W in the treatment liquid.
[0053] As a method of applying the treatment liquid to the surface of the substrate W, for example, there is a method of supplying the treatment liquid to the central portion of the surface of the substrate W while rotating the substrate W at a constant speed about its central portion. As a result, the treatment liquid supplied to the surface of the substrate W flows from near the center of the surface of the substrate W toward the peripheral portion of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and is diffused over the entire surface of the substrate W. As a result, the entire surface of the substrate W is covered with the treatment liquid, and a liquid film of the treatment liquid is formed.
[0054] The treatment liquid contains at least a SAM formation material. Further, in the treatment liquid, the SAM formation material may be dissolved or dispersed in a solvent. The SAM formation material is not particularly limited, and for example, octadecyltrichlorosilane (C 18 H 37Examples of the organic silane compounds include octadecyltrichlorosilane, which is a compound having a trichlorosilyl group as a functional group capable of forming a siloxane bond with a hydroxyl group. The solvent is not particularly limited, and examples thereof include ether solvents, aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, and fluorine-based solvents. The ether solvent is not particularly limited, and examples thereof include tetrahydrofuran (THF). The aromatic hydrocarbon solvent is not particularly limited, and examples thereof include toluene. The aliphatic hydrocarbon solvent is not particularly limited, and examples thereof include decane. The fluorine-based solvent is not particularly limited, and examples thereof include 1,3-bis(trifluoromethyl)benzene. These solvents can be used alone or in combination of two or more. From the viewpoint of being able to dissolve octadecyltrichlorosilane among the solvents exemplified above, aliphatic hydrocarbon solvents are preferred, and decane is particularly preferred.
[0055] The content of the SAM-forming material is preferably within the range of 0.005% by mass to 100% by mass, more preferably within the range of 0.05% by mass to 50% by mass, and particularly preferably within the range of 1% by mass to 10% by mass, relative to the total mass of the treatment liquid.
[0056] The treatment liquid may contain known additives as long as they do not impair the effects of the present invention. The additives are not particularly limited, and examples thereof include stabilizers and surfactants.
[0057] The conditions for contacting the treatment liquid with the substrate W are not particularly limited. However, the SAM formation step S1 of this embodiment can shorten the contact time of the treatment liquid compared to the case of forming a SAM film by a conventional method. Specifically, depending on the type of SAM formation material, its concentration, the type of solvent, etc., the time required for the SAM formation step S1 (the immersion time when the substrate W is immersed in the treatment liquid) can be appropriately set within the range of 1 minute to 1440 minutes, preferably 1 minute to 60 minutes, and more preferably 1 minute to 10 minutes.
[0058] Next, the process of forming a SAM will be described in more detail using an example in which the SAM-forming material is octadecyltrichlorosilane.
[0059] As shown in Fig. 4(a), when a processing liquid is supplied to the surface of a substrate W, molecules capable of forming a SAM (octadecyltrichlorosilane, hereinafter referred to as "SAM molecules") 5 are dispersed or dissolved in the processing liquid when it is first supplied. Fig. 4(a) is a schematic diagram showing how the processing liquid is supplied to the surface of a SiO2 layer.
[0060] Next, as shown in Fig. 4(b), if a hydroxyl group (OH group) 6 is present on the surface of the SiO2 layer 1, the SAM molecule 5 is chemically adsorbed onto the surface of the SiO2 layer 1 using the hydroxyl group 6 as a reaction site. More specifically, a siloxane bond is formed by reacting the trichlorosilyl group of the SAM molecule 5 with the hydroxyl group 6, and the SAM molecule 5 is chemically adsorbed onto the surface of the SiO2 layer 1. Fig. 4(b) is a schematic diagram showing the state in which the SAM molecule 5 is chemically adsorbed onto the surface of the SiO2 layer 1.
[0061] Next, when the SAM molecules 5 are chemically adsorbed at a high density on the surface of the SiO2 layer 1, an island-like structure of the SAM molecules 5 appears on the surface. Furthermore, in each island, the SAM molecules 5 self-organize and grow (expand) due to hydrophobic and electrostatic interactions between them, and finally form a SAM9 (see Figure 4(c)). However, film defects C occur in the SAM9 at the boundaries between adjacent islands where the SAM molecules 5 cannot penetrate, and in areas where the SAM molecules 5 are attached to the surface of the SiO2 layer 1 without being chemically adsorbed. Figure 4(c) is a schematic diagram showing how the SAM molecules 5 self-organize on the surface of the SiO2 layer 1 to form a SAM9.
[0062] 2.Removal process The removal step S102 is a step of removing the treatment liquid remaining on the surface of the SiO2 layer 1 after the film formation step S101. This makes it possible to remove excess SAM molecules 5 that do not contribute to the formation of the SAM 9, more specifically, at least a portion of the SAM molecules 5 that are not chemically adsorbed to the surface of the SiO2 layer 1, from the surface of the SiO2 layer 1. As a result, it is possible to prevent a film made of unadsorbed SAM molecules 5 from being formed on the SAM 9, and to form a good monolayer.
[0063] The method for removing the processing liquid from the surface of the SiO2 layer 1 is not particularly limited, and examples thereof include a method of applying the removal liquid to the surface of the substrate W, a method of spraying the removal liquid onto the surface of the substrate W, and a method of immersing the substrate W in the removal liquid.
[0064] An example of a method for applying the removing liquid to the surface of the substrate W is to supply the removing liquid to the center of the surface of the substrate W while rotating the substrate W at a constant speed around its center as an axis. In this way, the removing liquid supplied to the surface of the substrate W flows from near the center of the surface of the substrate W toward the peripheral edge of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and is spread over the entire surface of the substrate W. As a result, the processing liquid on the surface of the substrate W is replaced with the removing liquid, and the entire surface of the substrate W is covered with the removing liquid, forming a liquid film of the removing liquid.
[0065] When the SAM-forming material is octadecyltrichlorosilane, the surface of the SiO2 layer 1 in the removal step S102 is as shown in Fig. 5(a). As shown in the figure, at least some of the SAM molecules 5 that do not contribute to the formation of the SAM 9 are removed from the surface of the SiO2 layer 1 of the substrate W by the removal liquid. Fig. 5(a) is a schematic diagram showing how at least some of the excess SAM molecules 5 are removed from the surface of the SiO2 layer 1 in the removal step S102.
[0066] The removal liquid is preferably an organic solvent that dissolves the SAM-forming material, has low water solubility, and has a reduced water content. If the removal liquid is capable of dissolving the SAM-forming material, it can effectively remove excess SAM molecules 5 that do not contribute to the formation of the SAM 9 from the surface. The removal liquid is preferably one having a water solubility of about 0.033% (330 ppm) or less at 25° C., for example. More specifically, examples of the removal liquid include toluene, decane, and 1,3-bis(trifluoromethyl)benzene. These solvents can be used alone or in combination of two or more.
[0067] 3.Drying process The drying step S103 is intended to remove the removal liquid (at least a part of the SAM molecules 5) remaining on the surface of the substrate W by drying the surface of the substrate W. By removing the removal liquid from the surface of the substrate W before the annealing step, a SAM consisting of a good monolayer can be formed. The drying method is not particularly limited, and examples thereof include a method of spraying an inert gas such as nitrogen gas onto the surface of the substrate W. The drying conditions such as the drying time and drying temperature are not particularly limited as long as the removal liquid is removed, and can be set appropriately as necessary. The drying step S103 may be omitted.
[0068] 4. Annealing process The annealing step S104 is a step of heating the substrate W (SAM9) to repair film defects C occurring in the SAM9 after the removal step S102 or the drying step S103 (see FIG. 5(b)). FIG. 5(b) is a schematic cross-sectional view showing the state in which the annealing step is performed on the substrate W. The annealing step S104 is preferably performed in an atmosphere in which no oxygen molecules are present. If annealing is performed in the presence of oxygen molecules, the SAM9 and the like are oxidized, which causes a problem in that the protective performance of the SAM9 is reduced.
[0069] The annealing step S104 includes at least one of a low-temperature annealing step in which heating is performed in a low-temperature range and a high-temperature annealing step in which heating is performed in a high-temperature range.
[0070] In the low-temperature annealing step, annealing is preferably performed in a low-temperature range higher than room temperature and lower than 100°C, more preferably in the range of 35°C or higher and 100°C or lower, and even more preferably in the range of 59°C or higher and 100°C or lower. The probability of chemical adsorption of the SAM molecules 5 to the surface of the SiO2 layer 1 tends to decrease with time. Therefore, for example, in the film formation step S101, if the contact time of the treatment liquid with the SiO2 layer 1 is short, it becomes difficult to sufficiently chemically adsorb the SAM molecules 5 to the surface of the SiO2 layer 1, and film defects C may occur. However, by annealing in a low-temperature range, the SAM molecules 5 chemically adsorbed to the surface of the SiO2 layer 1 can be rearranged. As a result, the SAM molecules 5 can be chemically adsorbed to the region of the film defect C that occurs without the SAM molecules 5 being chemically adsorbed, and the film defect C can be repaired. As a result, as shown in FIG. 5(c), the film defect C is repaired, and a SAM 9' having excellent density and protective performance is formed. In this specification, "room temperature" means a temperature range of 5°C to 35°C. FIG. 5(c) is a schematic diagram showing how SAM9 is densified.
[0071] In addition, in the high-temperature annealing step, it is preferable to anneal in a high-temperature range higher than 100°C and lower than 200°C, and more preferably in the range of 150°C or higher and 200°C or lower. For example, when the unadsorbed SAM molecules present on the SiO2 layer 1 are octadecyltrichlorosilane, the chlorosilyl group (-SiCl group) of the octadecyltrichlorosilane reacts with water to become a silanol group (-SiOH group). Furthermore, the SAM molecule having a silanol group can be chemically adsorbed by a dehydration condensation polymerization reaction between the silanol group and a hydroxyl group (OH group) present on the surface of the SiO2 layer 1. Here, since the dehydration condensation polymerization is a rate-limiting step, for example, in the film formation step S101, if the contact time of the treatment solution with the SiO2 layer 1 is short, it becomes difficult to sufficiently chemically adsorb the SAM molecule 5 on the surface of the SiO2 layer 1, and film defects C may occur. However, by annealing at a high temperature, the SAM molecules 5 can be chemically adsorbed to the regions of the film defects C where the SAM molecules 5 are not chemically adsorbed, and the film defects C can be repaired. As a result, as shown in Fig. 5(c), the film defects C are repaired and a SAM 9' with excellent density and protective performance is formed.
[0072] The annealing time in the annealing step is preferably 5 minutes or more, more preferably 15 minutes or more, and even more preferably in the range of 30 minutes or more and 120 minutes or less. By setting the annealing time to 5 minutes or more, the above-mentioned dehydration condensation reaction can be further promoted, and the film defect C can be more effectively repaired.
[0073] The annealing step S104 may be a low-temperature annealing step followed by a high-temperature annealing step, which makes it possible to form a SAM 9' having better density and protective properties.
[0074] In addition, in Figures 4(a) to 4(c) and Figures 5(a) to 5(c), the circles of SAM molecule 5, SAM 9 and SAM 9' are schematic representations of either a silicon atom (Si atom), a chlorine atom (Cl atom) or a hydroxyl group (OH group).
[0075] 5. Cooling process The cooling step S105 is a step of rapidly cooling the substrate W after the annealing step S104 to room temperature. If the SAM 9' formed on the surface of the SiO2 layer 1 is in a crystalline state, grain boundaries are formed within the surface of the SAM 9', and these grain boundaries may become film defects. However, by rapidly cooling the SAM 9' to room temperature immediately after the annealing step S104, the SAM 9' can be made amorphous (non-crystalline). This prevents grain boundaries from being formed within the surface, and further prevents film defects from occurring.
[0076] In this specification, "rapid cooling" means that the substrate W immediately after the annealing step S104 is cooled (rapidly cooled) to room temperature.
[0077] As a result, in the SAM formation step S1, as shown in FIG. 2(b), a SAM 9' having excellent density and protective performance can be formed on the surface of the SiO2 layer 1. In the SAM formation step S1, in order to form a dense SAM 9', regions (film defects C) on the surface of the SiO2 layer 1 where SAM molecules cannot be chemically adsorbed are repaired. As a result, a SAM 9' having high film density and excellent density, in which the occurrence of film defects is suppressed or reduced, and which has excellent functionality as a protective film can be formed in a shorter time than with conventional methods. FIG. 2(b) is a partial enlarged view showing the state in which the SAM 9' has been formed on the surface of the SiO2 layer 1.
[0078] In the SAM formation step S1 of this embodiment, it is preferable not to heat the substrate W (more specifically, the SiO2 layer 1 (protected layer)) after the film formation step S101 and before the annealing step S104. If the substrate W is heated in a state where an excess of unadsorbed SAM molecules 5 remain on the surface of the substrate W, a film made of unadsorbed SAM molecules 5 may be formed on the SAM 9 formed on the surface of the substrate W. Therefore, by not heating the substrate W in a state where an excess of unadsorbed SAM molecules 5 remain on the surface of the substrate W before the annealing step S104, it is possible to prevent a film made of unadsorbed SAM molecules 5 from being formed on the SAM 9 formed on the surface of the substrate W. As a result, a SAM 9' made of a good monolayer can be formed.
[0079] <Etching process> The etching step S2 is a step of selectively etching the SiN layer 2, which is a sacrificial layer and a layer to be etched. More specifically, this is a step of bringing an etching solution into contact with the SiN layer 2 through the memory trench 4 and removing the SiN layer 2. In this step, the SAM 9' functions as a protective layer to protect the SiO2 layer 1. This makes it possible to effectively prevent the SiO2 layer 1 from being etched.
[0080] An example of a method for applying the etching liquid to the surface of the substrate W is to rotate the substrate W at a constant speed around its central portion as an axis and supply the etching liquid to the central portion of the surface of the substrate W. In this way, the etching liquid supplied to the surface of the substrate W flows from near the center of the surface of the substrate W toward the peripheral portion of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and is spread over the entire surface of the substrate W. As a result, the entire surface of the substrate W is covered with the etching liquid, and a liquid film of the etching liquid is formed.
[0081] The etching liquid can be appropriately set in consideration of the constituent material of the layer to be etched, the etching rate, etc. When the layer to be etched is a SiN layer 2 as in this embodiment, the etching liquid can be, for example, an aqueous solution of phosphoric acid (H3PO4) or hydrofluoric acid (for example, HF:DIW=1:100 in volume ratio). The concentration of the etching liquid can also be appropriately set in consideration of the constituent material of the layer to be etched, the etching rate, etc.
[0082] Furthermore, the etching temperature (that is, the temperature of the etching solution) and the etch rate for the layer to be etched can be appropriately set in consideration of the constituent material of the layer to be etched.
[0083] It is preferable to sequentially perform a rinsing step for removing the etching liquid and a drying step immediately after the etching step S2. The rinsing method in the rinsing step is not particularly limited, and examples thereof include a method of supplying a rinsing liquid to the surface of the substrate W and a method of immersing the substrate W in the rinsing liquid. The rinsing liquid is not particularly limited, and examples thereof include DIW. In addition, cleaning conditions such as the rinsing time and the temperature of the rinsing liquid are not particularly limited, and can be set appropriately as needed. The drying step is intended to remove the rinsing liquid remaining on the surface of the substrate W. The drying method is not particularly limited, and examples thereof include a method of spraying an inert gas such as nitrogen gas onto the surface of the substrate W, and a method of contacting a high-temperature gaseous organic solvent with the back surface Wb of the substrate W and heating it. Drying conditions such as the drying time and drying temperature are not particularly limited, and can be set appropriately as needed. Examples of the gaseous organic solvent include volatile organic solvents containing at least one selected from the group consisting of IPA (isopropyl alcohol), HFE (hydrofluoroether), methanol, ethanol, acetone, and trans-1,2-dichloroethylene.
[0084] As a result, in the etching step S2, only the SiN layer 2 can be selectively removed as shown in FIG. 2(c). In addition, the SAM 9', which has excellent density and protective performance, covers and protects the surface of the SiO2 layer 1, so that the SiO2 layer 1 can be prevented from being etched and the etched silicon component can be prevented from precipitating and adhering to the surface of the SiO2 layer 1. Furthermore, the tolerance range of the silicon concentration contained in the etching solution such as phosphoric acid can be increased. FIG. 2(c) is a partial enlarged view of the portion surrounded by B in the laminate in FIG. 1(b), showing the state in which the SiN layer 2 has been etched.
[0085] [Substrate processing equipment (semiconductor manufacturing equipment)] Next, the substrate processing apparatus according to this embodiment will be described below by taking as an example a case where it is applied to a semiconductor manufacturing apparatus.
[0086] The semiconductor manufacturing apparatus 100 of this embodiment is a single-wafer processing unit used to form a SAM and etch a layer to be etched, and includes, as shown in FIG. 6, a substrate holding unit 110 for holding a substrate W, a supply unit 120 for supplying a processing liquid to the surface Wf of the substrate W, a removing liquid supply unit 130 for supplying a removing liquid, an inert gas supply unit 140 for supplying an inert gas, an annealing / cooling unit (annealing unit, cooling unit) 150, an etching liquid supply unit 170, a volatile organic solvent supply unit 180, a chamber 190 which is a container for accommodating the substrate W, a splash prevention cup 200 for collecting the processing liquid, a swivel drive unit 210 for independently swivel-driving the arms of each unit described later, and a control unit 300. The semiconductor manufacturing apparatus 100 may also include a loading / unloading unit (not shown) for loading or unloading the substrate W. FIG. 6 is an explanatory diagram showing a schematic configuration of the semiconductor manufacturing apparatus 100 according to this embodiment. In this figure, in order to clarify the directional relationships of the objects shown, XYZ orthogonal coordinate axes are displayed as appropriate. Here, the XY plane represents the horizontal plane, and the +Z direction represents the vertical upward direction.
[0087] <Substrate holding part> The substrate holding unit 110 is a means for holding the substrate W, and as shown in Fig. 6, holds and rotates the substrate W in a substantially horizontal position with the surface Wf of the substrate W facing upward. The substrate holding unit 110 has a spin chuck 113 in which a spin base 111 and a rotation support shaft 112 are integrally connected. The spin base 111 has a substantially circular shape in a plan view, and a hollow rotation support shaft 112 extending in a substantially vertical direction is fixed to the center of the spin base 111. The rotation support shaft 112 is connected to a rotation shaft of a chuck rotation mechanism 114 including a motor. The chuck rotation mechanism 114 is housed in a cylindrical casing 115, and the rotation support shaft 112 is supported by the casing 115 so as to be rotatable around a vertical rotation axis.
[0088] The chuck rotation mechanism 114 can rotate the rotation support shaft 112 around the rotation axis by being driven by a chuck drive unit (not shown) of the control unit 300. This causes the spin base 111 attached to the upper end of the rotation support shaft 112 to rotate around the rotation axis J1 at a constant speed. The control unit 300 can adjust the rotation speed of the spin base 111 by controlling the chuck rotation mechanism 114 via the chuck drive unit.
[0089] A plurality of chuck pins 116 for gripping the peripheral edge of the substrate W are provided upright near the peripheral edge of the spin base 111. The number of chuck pins 116 to be provided is not particularly limited, but it is preferable to provide at least three or more in order to reliably hold the circular substrate W. In this embodiment, three chuck pins 116 are arranged at equal intervals along the peripheral edge of the spin base 111. Each chuck pin 116 includes a substrate support pin that supports the peripheral edge of the substrate W from below, and a substrate holding pin that holds the substrate W by pressing against the outer circumferential end face of the substrate W supported by the substrate support pin.
[0090] <Supply section> The supply unit 120 according to this embodiment is a unit that supplies a processing liquid to the front surface Wf of the substrate W. The supply unit 120 includes a processing liquid storage unit 121, a nozzle 122, and an arm 123, as shown in FIG.
[0091] 7, the treatment liquid storage section 121 includes a pressurizing section 124 and a treatment liquid tank 125. Note that, Fig. 7 is an explanatory diagram showing a schematic configuration of the treatment liquid storage section 121 in the supply section 120.
[0092] The pressurizing unit 124 includes a nitrogen gas supply source 124a which is a supply source of gas for pressurizing the inside of the processing liquid tank 125, a pump (not shown) for pressurizing the nitrogen gas, a nitrogen gas supply pipe 124b, and a valve 124c.
[0093] The nitrogen gas supply pipe 124b is connected to the processing liquid tank 125. Furthermore, a valve 124c is provided in the middle of the nitrogen gas supply pipe 124b. The valve 124c is electrically connected to the control unit 300, and the opening and closing of the valve 124c can be controlled by an operation command from the control unit 300. When the valve 124c is opened by an operation command from the control unit 300, nitrogen gas can be supplied to the processing liquid tank 125.
[0094] The processing liquid tank 125 may include an agitation unit that agitates the processing liquid in the processing liquid tank 125, and a temperature adjustment unit that adjusts the temperature of the processing liquid (neither is shown). The agitation unit may include a rotation unit that agitates the processing liquid, and an agitation control unit that controls the rotation of the rotation unit. The agitation control unit is electrically connected to the control unit 300, and the rotation unit is provided with, for example, a propeller-shaped agitation blade at the lower end of the rotation shaft. The control unit 300 issues an operation command to the agitation control unit to rotate the rotation unit, thereby causing the agitation blade to agitate the processing liquid. As a result, the concentration and temperature of the processing liquid can be made uniform in the processing liquid tank 125.
[0095] Furthermore, a discharge pipe 125a for supplying the processing liquid to the nozzle 122 is connected to the processing liquid tank 125. A discharge valve 125b is provided midway along the discharge pipe 125a. The discharge valve 125b is also electrically connected to the control unit 300. This allows the opening and closing of these valves to be controlled by operation commands from the control unit 300. When the discharge valve 125b is opened by an operation command from the control unit 300, the processing liquid is pressure-fed to the nozzle 122 via the discharge pipe 125a.
[0096] The nozzle 122 is attached to the tip of an arm 123 that extends horizontally, and is disposed above the spin base 111 when discharging the treatment liquid. The arm 123 is connected to a rotation drive unit 210 via a rotation shaft (not shown). The rotation drive unit 210 is electrically connected to a control unit 300, and rotates the arm 123 in response to an operation command from the control unit 300. As the arm 123 rotates, the nozzle 122 also moves.
[0097] <Removal liquid supply section> The removing liquid supply unit 130 according to this embodiment is a unit that supplies a removing liquid to the front surface Wf of the substrate W. As shown in FIG. 6, the removing liquid supply unit 130 includes a removing liquid storage unit 131, a nozzle 132, and an arm 133.
[0098] 8, the removing liquid storage unit 131 has a function of supplying the removing liquid to the nozzle 132, and includes a pressurizing unit 134 and a removing liquid tank 135. Fig. 8 is an explanatory diagram showing a schematic configuration of the removing liquid storage unit 131 in the removing liquid supply unit 130.
[0099] The pressurizing unit 134 includes a nitrogen gas supply source 134a which is a supply source of gas for pressurizing the inside of the removal liquid tank 135, a pump (not shown) for pressurizing the nitrogen gas, a nitrogen gas supply pipe 134b, and a valve 134c.
[0100] The nitrogen gas supply pipe 134b is connected to the removal liquid tank 135. Furthermore, a valve 134c is provided in the middle of the nitrogen gas supply pipe 134b. The valve 134c is electrically connected to the control unit 300, and the opening and closing of the valve 134c can be controlled by an operation command from the control unit 300. When the valve 134c is opened by an operation command from the control unit 300, nitrogen gas can be supplied to the removal liquid tank 135.
[0101] The removal liquid tank 135 may include an agitation unit that agitates the removal liquid in the removal liquid tank 135, and a temperature adjustment unit that adjusts the temperature of the removal liquid (neither is shown). The agitation unit may include a rotation unit that agitates the removal liquid in the removal liquid tank 135, and an agitation control unit that controls the rotation of the rotation unit. The agitation control unit is electrically connected to the control unit 300, and the rotation unit is provided with, for example, a propeller-shaped agitation blade at the lower end of the rotation shaft. The control unit 300 issues an operation command to the agitation control unit to rotate the rotation unit, thereby agitating the removal liquid with the agitation blade. As a result, the concentration and temperature of the removal liquid can be made uniform in the removal liquid tank 135.
[0102] Furthermore, a discharge pipe 135a for supplying the removal liquid to the nozzle 132 is connected to the removal liquid tank 135. A discharge valve 135b is provided midway along the discharge pipe 135a. The discharge valve 135b is electrically connected to the control unit 300. This allows the opening and closing of the discharge valve 135b to be controlled by an operation command from the control unit 300. When the discharge valve 135b is opened by an operation command from the control unit 300, the removal liquid is pressure-fed to the nozzle 132 via the discharge pipe 135a.
[0103] The nozzle 132 is attached to the tip of an arm 133 that extends horizontally, and is positioned above the spin base 111 when discharging the removal liquid. The arm 133 is connected to a rotation drive unit 210 via a rotation shaft (not shown). The rotation drive unit 210 is electrically connected to a control unit 300, and rotates the arm 133 in response to an operation command from the control unit 300. As the arm 133 rotates, the nozzle 132 also moves.
[0104] <Inert gas supply section (drying section)> The inert gas supply unit 140 according to this embodiment is a means for supplying an inert gas to the surface Wf of the substrate W. By providing the inert gas supply unit 104, the surface of the substrate W can be dried and the remaining removing solution can be removed. By removing the removing solution from the surface of the substrate W before the annealing step S104, a SAM 9' made of a good monolayer can be formed. If the drying step S103 is not performed, the inert gas supply unit 140 can be omitted from the semiconductor manufacturing apparatus 100.
[0105] As shown in FIG. 6, the inert gas supply unit 140 includes an inert gas storage unit 141, a nozzle 142, and an arm 143.
[0106] 9, the inert gas storage unit 141 has a function of supplying an inert gas to the nozzle 142, and includes an inert gas tank 144 for storing the inert gas, an inert gas temperature adjustment unit 145 for adjusting the temperature of the inert gas stored in the inert gas tank 144, and a pipe 146. An example of the inert gas stored in the inert gas tank 144 is nitrogen gas. FIG. 9 is a block diagram showing a schematic configuration of the inert gas storage unit 141 in the inert gas supply unit 140.
[0107] The inert gas temperature adjustment unit 145 is electrically connected to the control unit 300, and adjusts the temperature by heating or cooling the inert gas stored in the inert gas tank 144 in response to an operation command from the control unit 300. The temperature adjustment is performed so that the inert gas stored in the inert gas tank 144 is at room temperature, for example. The inert gas temperature adjustment unit 145 is not particularly limited, and for example, a known temperature adjustment mechanism such as a Peltier element or a pipe through which temperature-adjusted water passes can be used.
[0108] The inert gas storage unit 141 is connected to the nozzle 142 via a pipe 146, and a valve 147 is inserted in the middle of the path of the pipe 146. The inert gas in the inert gas tank 144 is pressurized by a pressurizing means (not shown) and sent to the pipe 146. The pressurizing means can be realized by compressing and storing the inert gas in the inert gas tank 144, in addition to pressurization by a pump or the like.
[0109] The valve 147 is electrically connected to the control unit 300 and is normally closed. Opening and closing of the valve 147 is controlled by an operation command from the control unit 300. When the valve 147 is opened by an operation command from the control unit 300, an inert gas is supplied from the nozzle 142 through the pipe 146 to the front surface Wf of the substrate W.
[0110] <Annealing and cooling section> The annealing / cooling unit 150 of this embodiment has a function of heating the substrate W to perform an annealing process, and a function of cooling the substrate W. More specifically, as shown in Fig. 6, the annealing / cooling unit 150 includes a plate body 151, a heater 152, a heater current supply unit 153, a lifting / rotating mechanism 154, and a lifting shaft 155. Each of these units functions as an annealing unit.
[0111] The plate body 151 has a circular planar shape slightly smaller than the diameter of the substrate W in plan view. A heater 152 is provided inside the plate body 151. The heater 152 is connected to a heater current supplying unit 153. The heater current supplying unit 153 is electrically connected to the control unit 300, and can supply power to the heater 152 to generate heat in response to an operation command from the control unit 300. The heater 152 generates heat, so that the upper surface 151a of the plate body 151 is heated uniformly within the surface, and the rear surface Wb of the substrate W can also be heated uniformly within the surface by the radiant heat (radiation heat). The lifting shaft 155 passes through the inside of the rotation support shaft 112 of the substrate holder 110. The lower end of the lifting shaft 155 is connected to the lifting and rotating mechanism 154. The lifting / rotating mechanism 154 is electrically connected to the control unit 300, and raises and lowers the plate body 151 in the vertical direction (Z direction shown in FIG. 6) via the lifting shaft 155 in response to an operation command from the control unit 300. This allows the plate body 151 to be brought into contact with or separated from the back surface Wb of the substrate W. Furthermore, the lifting / rotating mechanism 154 can rotate the plate body 151 around the rotation axis J1 at a constant speed in response to an operation command from the control unit 300. The control unit 300 can also adjust the rotation speed of the plate body 151 by controlling the lifting / rotating mechanism 154.
[0112] The annealing by the annealing / cooling unit 150 can be performed, for example, as follows. That is, as shown in FIG. 10, the lifting / rotating mechanism 154 is controlled by an operation command from the control unit 300 to lift and lower the plate body 151 to a position spaced apart from the rear surface Wb of the substrate W by an arbitrary distance. As a result, a space 156 is formed between the upper surface 151a of the plate body 151 and the rear surface Wb of the substrate W. The distance between the upper surface 151a of the plate body 151 and the rear surface Wb of the substrate W is not particularly limited, and may be, for example, such that the substrate W can be heated by radiant heat (radiation heat) from the plate body 151. Next, the lifting / rotating mechanism 154 is controlled by an operation command from the control unit 300 to rotate the plate body 151 at a constant speed around the rotation axis J1. Also, the chuck rotating mechanism 114 is controlled via the chuck driving unit by an operation command from the control unit 300 to rotate the spin base 111 at a constant speed around the rotation axis J1, thereby rotating the substrate W. Furthermore, the control unit 300 controls the heater power supply unit 153 to supply power to the heater 152 to generate heat, based on an operation command. As a result, the back surface Wb of the substrate W is heated by radiant heat radiated from the upper surface 151a of the plate body 151. Since the substrate W and the plate body 151 are both rotating, heating by radiant heat can be performed uniformly within the back surface Wb of the substrate W. The substrate W and the plate body 151 may rotate in the same direction around the rotation axis J1, or may rotate in opposite directions. FIG. 10 is an enlarged view of a main part for explaining the annealing step S104 by the annealing / cooling unit 150.
[0113] Also, the annealing by the annealing / cooling unit 150 may be performed by directly contacting the upper surface 151a of the plate body 151 with the rear surface Wb of the substrate W as shown in FIG. 11. FIG. 11 is an enlarged view of a main part for explaining another annealing step S104 by the annealing / cooling unit 150. In this case, the lifting / rotating mechanism 154 is controlled by an operation command from the control unit 300 to lift the plate body 151 to bring the upper surface 151a of the plate body 151 into contact with the rear surface Wb of the substrate W, and the substrate W is separated from the chuck pins 116. That is, the substrate W is held only by the plate body 151 from the rear surface Wb side. Furthermore, the heater current supplying unit 153 is controlled by an operation command from the control unit 300 to supply power to the heater 152 to generate heat, and the rear surface Wb of the substrate W is directly heated.
[0114] The annealing / cooling unit 150 also includes a supply pipe 157 attached to the center of the plate body 151 and extending vertically downward, a coolant storage unit 158 for storing a coolant, and a discharge unit 159 for discharging the fluid coolant toward the back surface Wb of the substrate W (see FIG. 6). Each of these units functions as a cooling unit.
[0115] 12, refrigerant storage unit 158 includes refrigerant tank 161 that stores the refrigerant, and refrigerant temperature adjustment unit 162 that adjusts the temperature of the refrigerant stored in refrigerant tank 161. Fig. 12 is a block diagram showing a schematic configuration of refrigerant storage unit 158.
[0116] The coolant temperature adjustment unit 162 is electrically connected to the control unit 300, and adjusts the temperature by heating or cooling the coolant stored in the coolant tank 161 in response to an operation command from the control unit 300. The temperature adjustment may be performed so that the coolant stored in the coolant tank 161 has a temperature that can rapidly cool the substrate W to room temperature after the annealing step S104. The coolant temperature adjustment unit 162 is not particularly limited, and any known temperature adjustment mechanism, such as a chiller using a Peltier element or piping through which temperature-adjusted water flows, may be used.
[0117] Refrigerant storage unit 158 is connected to supply pipe 157 via piping 163, and a valve 164 is inserted in the middle of the path of piping 163. The refrigerant in refrigerant storage unit 158 is pressurized by a pressurizing means (not shown) and sent to piping 163. Note that the pressurizing means can be realized by compressing and storing the refrigerant in refrigerant storage unit 158, in addition to pressurization by a pump or the like.
[0118] The valve 164 is electrically connected to the control unit 300 and is normally closed. Opening and closing of the valve 164 is controlled by an operation command from the control unit 300. When the valve 164 is opened by an operation command from the control unit 300, a coolant is supplied from the discharge unit 159 through the piping 163 and the supply pipe 157. The coolant supplied from the discharge unit 159 comes into contact with the back surface Wb of the substrate W, thereby rapidly cooling the substrate W.
[0119] Here, the substrate W may be cooled while being rotated about the rotation axis J1. In this case, the control unit 300 issues an operation command to the chuck rotation mechanism 114 to rotate the substrate W at a constant speed about the rotation axis J1. The coolant supplied toward the back surface Wb of the substrate W can flow from near the center of the back surface Wb of the substrate W toward the peripheral edge of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and can be diffused over the entire back surface Wb of the substrate W. As a result, the substrate W can be cooled more effectively.
[0120] The refrigerant is not particularly limited, but from the viewpoint of rapidly cooling the SAM 9', a liquid such as DIW is preferable.
[0121] <Etching solution supply unit> The etching liquid supply unit 170 according to this embodiment is a means for supplying an etching liquid to the front surface Wf of the substrate W. As shown in FIG. 6, the etching liquid supply unit 170 has an etching liquid storage unit 171, a nozzle 172, and an arm 173.
[0122] 13, the etching liquid storage unit 171 includes at least an etching liquid tank 174, a temperature regulator 175, a liquid delivery pump 176, and a particle filter 177. Note that, FIG. 13 is an explanatory diagram showing a schematic configuration of the etching liquid storage unit 171 in the etching liquid supply unit 170.
[0123] The etching solution tank 174 may include an agitation unit (not shown) that agitates the etching solution in the etching solution tank 174. The agitation unit may include a rotation unit that agitates the etching solution and an agitation control unit that controls the rotation of the rotation unit. The agitation control unit is electrically connected to the control unit 300, and the rotation unit includes, for example, a propeller-shaped agitation blade at the lower end of the rotation shaft. The control unit 300 issues an operation command to the agitation control unit to rotate the rotation unit, thereby agitating the etching solution with the agitation blade. As a result, the concentration and temperature of the etching solution in the etching solution tank 174 can be made uniform.
[0124] The etching solution tank 174 is provided with a mixer 178 that can mix chemicals and DIW from an external supply source (not shown) to prepare an etching solution of a predetermined concentration. The chemicals are solutes that function as etchants. Examples of chemicals include the aforementioned phosphoric acid and hydrogen fluoride.
[0125] Further, the etching solution tank 174 is connected to a discharge pipe 179 for supplying the etching solution to the nozzle 172. A temperature regulator 175, a liquid delivery pump 176, and a particle filter 177 are sequentially interposed in the middle of the discharge pipe 179 from upstream to downstream. The temperature regulator 175 and the liquid delivery pump 176 are electrically connected to the control unit 300. This allows the temperature of the etching solution to be supplied to the nozzle 172 to be controlled by an operation command from the control unit 300. Furthermore, when the liquid delivery pump 176 is controlled by an operation command from the control unit 300, the etching solution can be pressure-fed to the nozzle 172 through the discharge pipe 179. The particle filter 177 can remove foreign matter such as particles in the etching solution.
[0126] The nozzle 172 is attached to the tip of an arm 173 that extends horizontally, and is disposed above the spin base 111 when discharging the etching liquid. The arm 173 is connected to a rotation drive unit 210 via a rotation shaft (not shown). The rotation drive unit 210 is electrically connected to a control unit 300, and rotates the arm 173 in response to an operation command from the control unit 300. As the arm 173 rotates, the nozzle 172 also moves.
[0127] <Volatile organic solvent supply unit> The volatile organic solvent supply unit 180 according to this embodiment is a means used for drying and removing the rinsing liquid in a drying step performed after a rinsing step for removing the etching liquid, for example. The volatile organic solvent supply unit 180 is connected to a supply pipe 157, and is capable of supplying a volatile organic solvent (a high-temperature gaseous organic solvent) from a supply source of the volatile organic solvent (not shown). The volatile organic solvent supply unit 180 is electrically connected to the control unit 300, and the volatile organic solvent is supplied from the discharge unit 159 through the supply pipe 157 in response to an operation command from the control unit 300. The volatile organic solvent supplied from the discharge unit 159 can heat the substrate W by contacting the rear surface Wb of the substrate W (see FIG. 14). This allows the rinsing liquid remaining on the front surface Wf of the substrate W to be dried and removed. FIG. 14 is an enlarged view of a main part for explaining the drying step of the rinsing liquid.
[0128] Here, the volatile organic solvent may be supplied while rotating the substrate W around the rotation axis J1. In this case, the control unit 300 issues an operation command to the chuck rotation mechanism 114 to rotate the substrate W around the rotation axis J1 at a constant speed. The volatile organic solvent supplied toward the back surface Wb of the substrate W flows from near the center of the back surface Wb of the substrate W toward the peripheral edge of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and can be diffused over the entire back surface Wb of the substrate W. As a result, the substrate W can be heated more effectively.
[0129] Note that another supply pipe for supplying the volatile organic solvent to the back surface Wb of the substrate W may be provided separately from the supply pipe 157. In this case, it is preferable that a discharge part for discharging the volatile organic solvent is also provided in the other supply pipe.
[0130] <Shatterproof cup> The shatterproof cup 200 is provided to surround the spin base 111. The shatterproof cup 200 is connected to a lifting drive mechanism (not shown) and can be raised and lowered in the vertical direction. When supplying a processing liquid or the like to the front surface Wf of the substrate W, the shatterproof cup 200 is positioned at a predetermined position by the lifting drive mechanism and surrounds the substrate W held by the chuck pins 116 from a lateral position. This makes it possible to collect the processing liquid or the like that splashes from the substrate W and the spin base 111.
[0131] <Control Unit> The control unit 300 is electrically connected to each part of the semiconductor manufacturing equipment and controls the operation of each part. The control unit 300 is composed of a computer having an arithmetic unit and a storage unit. The arithmetic unit uses a CPU that performs various arithmetic processing. The storage unit also includes a ROM, which is a read-only memory that stores a substrate processing program and an etching processing program, a RAM, which is a readable and writable memory that stores various information, and a magnetic disk that stores control software, data, and the like. The magnetic disk stores processing conditions in advance, including supply conditions for the processing liquid, removal liquid, inert gas, etching liquid, coolant, and volatile organic solvent, rinsing conditions, drying conditions, SAM film formation conditions, and etching conditions. The CPU reads the processing conditions into the RAM and controls each part of the semiconductor manufacturing equipment according to the contents.
[0132] Second embodiment A second embodiment of the present invention will now be described. This embodiment is different from the first embodiment in that the etching process is performed in a batch manner instead of a single-wafer type. Also, in the annealing process, it is different in that annealing is performed while supplying water vapor. Even with such a configuration, a self-assembled monolayer with a high film density, excellent denseness, and good suppression or reduction of film defects can be efficiently formed on the substrate surface in a shorter time than conventional film formation methods, with excellent protection performance.
[0133] [Substrate Processing Method (Method for Manufacturing Semiconductor Device)] The substrate processing method (method for manufacturing a semiconductor device) according to this embodiment will be described below with reference to FIG. 15. FIG. 15 is a flowchart showing an example of the overall flow of the substrate processing method according to the second embodiment of the present invention. Note that the film formation step S101, removal step S102, drying step S103, and cooling step S105 shown in FIG. 15 are the same as in the case of the first embodiment, so the details of these steps will be omitted.
[0134] <SAM Formation Step> 1. Annealing process The annealing process is, as in the case of the first embodiment, a process of repairing the film defects C generated in SAM9 after the drying process S103 by heating the substrate W (SAM9) (see FIG. 5(b)). Also, the annealing process of this embodiment is performed by heating while supplying water vapor to the surface Wf of the substrate W. By supplying water vapor, the annealing process can be performed in the presence of water. Thereby, for example, when the unadsorbed SAM molecules present on the SiO2 layer 1 are octadecyltrichlorosilane, it is possible to promote the reaction of the chlorosilyl group (-SiCl group) of octadecyltrichlorosilane with water to form a silanol group (-SiOH group). Thereby, it facilitates the chemisorption by subjecting the SAM molecules having silanol groups to a dehydration condensation polymerization reaction between the silanol groups and the hydroxyl groups (OH groups) present on the surface of the SiO2 layer 1. Furthermore, although dehydration condensation polymerization is the rate-determining step, annealing promotes dehydration condensation polymerization, so that the repair of the film defects C generated in SAM9 can be further achieved.
[0135] The supply of water vapor is preferably started at least at the start of the annealing step and stopped at the end of the annealing step.
[0136] The annealing step may be performed at a low temperature range of 100°C or less, but in this embodiment, it is preferable to perform the annealing step at a high temperature range of 100°C or more and 200°C or less. This promotes a dehydration condensation polymerization reaction between the silanol groups and the hydroxyl groups (OH groups) present on the surface of the SiO2 layer 1, and allows the film defects C to be repaired well. The heating temperature in the annealing step is more preferably in the range of 150°C or more and 200°C or less.
[0137] In this embodiment, water may be supplied to the surface Wf of the substrate W instead of water vapor. Even in this embodiment, the dehydration condensation polymerization reaction between the silanol groups and the hydroxyl groups (OH groups) present on the surface of the SiO2 layer 1 is promoted, and the film defects C can be successfully repaired.
[0138] <Etching process> The etching step S2' is a step of selectively etching the SiN layer 2, which is the layer to be etched, by immersing the substrate W after the SAM formation in an etching solution.
[0139] The method of immersing the substrate W in the etching solution is, for example, performed with the substrate W in an upright position. Here, the "upright position" refers to a position in which the surface of the substrate W is aligned in a direction substantially perpendicular to a horizontal plane, and includes a vertical position. The etching solution may be the same as that described in the first embodiment. In addition, the etching temperature (i.e., the liquid temperature of the etching solution) and the etch rate for the layer to be etched may be appropriately set in consideration of the constituent material of the layer to be etched, as in the first embodiment.
[0140] [Substrate processing equipment (semiconductor manufacturing equipment)] Next, the substrate processing apparatus according to this embodiment will be described below by taking as an example a case where it is applied to a semiconductor manufacturing apparatus.
[0141] The semiconductor manufacturing apparatus of this embodiment differs from the semiconductor manufacturing apparatus of the first embodiment in that it at least includes a single-wafer substrate processing unit for forming a SAM and a batch-type etching processing unit for etching the layer to be etched.
[0142] <Substrate processing unit> As shown in FIG. 16, the substrate processing unit 400 is different from the semiconductor manufacturing apparatus 100 of the first embodiment in that it includes a water vapor supply unit 220 instead of the etching liquid supply unit 170. FIG. 16 is an explanatory diagram showing a schematic configuration of the substrate processing unit 400 in the semiconductor manufacturing apparatus of the second embodiment. In this figure, XYZ orthogonal coordinate axes are displayed as appropriate to clarify the directional relationship of the illustrated objects. Here, the XY plane represents the horizontal plane, and the +Z direction represents the vertical upward direction. Note that the same reference numerals are used for components having the same functions as those in the semiconductor manufacturing apparatus of the first embodiment, and detailed descriptions thereof will be omitted.
[0143] The water vapor supplying unit 220 is a unit for supplying water vapor to the front surface Wf of the substrate W. The water vapor supplying unit 220 includes a water vapor storage unit 221, a nozzle 222, and an arm 223, as shown in FIG.
[0144] 17, the water vapor storage unit 221 has a function of supplying water vapor to the nozzle 222, and includes a water vapor tank 224 for storing water vapor, a water vapor temperature adjustment unit 225 for adjusting the temperature of the water vapor stored in the water vapor tank 224, and a pipe 226. Note that FIG. 17 is a block diagram showing a schematic configuration of the water vapor storage unit 221 in the water vapor supply unit 220.
[0145] The water vapor temperature adjustment unit 225 is electrically connected to the control unit 300, and adjusts the temperature by heating or cooling the water vapor stored in the water vapor tank 224 according to an operation command from the control unit 300. The temperature adjustment is performed so that the water vapor stored in the water vapor tank 224 is within the above-mentioned temperature range, for example. The water vapor temperature adjustment unit 225 is not particularly limited, and for example, a known temperature adjustment mechanism such as a Peltier element or a pipe through which temperature-adjusted water flows can be used.
[0146] One end of the pipe 226 is connected to the water vapor storage unit 221, and the other end is connected to the nozzle 222. A valve 227 is inserted in the middle of the pipe 226. The water vapor in the water vapor tank 224 is pressurized by a pressurizing means (not shown) and sent to the pipe 226.
[0147] The valve 227 is electrically connected to the control unit 300 and is normally closed. Opening and closing of the valve 227 is controlled by an operation command from the control unit 300. When the valve 227 is opened by an operation command from the control unit 300, water vapor is supplied from the nozzle 222 through the pipe 226 to the front surface Wf of the substrate W.
[0148] <Etching processing unit> The etching processing unit 500 of this embodiment is a batch-type processing unit used for etching a layer to be etched, and performs an etching step S2 on a substrate W on which a SAM has been formed in the substrate processing unit 400. As shown in Fig. 18, the etching processing unit 500 at least includes a substrate transport unit (not shown), a lifter 510, and a processing tank 520 for storing an etching liquid. Fig. 18 is a cross-sectional view showing a state in which a plurality of substrates W on which a SAM has been formed according to this embodiment are immersed in an etching liquid.
[0149] The substrate transport unit transports the substrate W on which the SAM has been formed in the substrate processing unit 400 to the etching processing unit 500. The substrate transport unit includes, for example, an articulated robot capable of transporting the substrate W. The tip of the articulated robot includes a transport arm capable of loading the substrates W all at once in a horizontal position.
[0150] As shown in FIG. 19, the lifter 510 includes a flat back plate 511, a plurality of (three) holding rods 512, and a lifting mechanism (not shown). The back plate 511 stands upright, and at its lower end, the holding rods 512 extend in one direction so as to be perpendicular to the back plate 511. The holding rods 512 are provided with a plurality of grooves 513 arranged in the extending direction. The plurality of grooves 513 are arranged at equal intervals and spaced apart from each other. Furthermore, each groove 513 extends in a direction perpendicular to the extending direction of the holding rod 512, and can fit a plurality of substrates W in an upright position. As a result, the holding rods 512 can abut against and support the substrates W from below in an upright position, and can hold them collectively. The number of holding rods 512 is not particularly limited as long as it is plural. Furthermore, the number of grooves 513 provided in holding rod 512 is not particularly limited and may be set appropriately depending on the number of substrates W to be held. The lifting mechanism can raise or lower lifter 510 in the Z direction shown in Fig. 19. This allows lifter 510, which is collectively holding the group of substrates W, to be moved into or removed from processing bath 520. Fig. 19 is a side view showing a schematic configuration of the lifter in the semiconductor manufacturing apparatus of this embodiment.
[0151] 18, the treatment tank 520 includes an injection pipe 522 for supplying the etching liquid into the treatment tank 520, an inner tank 523 for storing the etching liquid, and an outer tank 524 provided on the periphery of the upper opening of the inner tank 523. The injection pipe 522 is provided on the bottom of the inner tank 523, and enables the etching liquid to be supplied in an upflow manner to the inner tank 523. In addition, the outer tank 524 enables the etching liquid overflowing from the inner tank 523 to be collected.
[0152] (Other matters) In the above description, the most preferred embodiment of the present invention has been described. However, the present invention is not limited to this embodiment. The configurations in the above-described embodiment and each modified example can be changed, modified, substituted, added, deleted, and combined within a range that does not contradict each other. EXAMPLES
[0153] Preferred examples of the present invention are described in detail below. However, the materials, amounts, conditions, etc. described in the examples are not intended to limit the scope of the present invention unless otherwise specified.
[0154] Example 1 A substrate with a SiO2 film (thickness 100 nm) formed on its surface was prepared and immersed in a hydrogen fluoride solution for 1 minute. The volume ratio of hydrogen fluoride to DIW was hydrogen fluoride:DIW=1:100.
[0155] Next, the substrate was removed from the hydrogen fluoride solution and immersed in a treatment liquid containing a SAM-forming material for 5 minutes to form a SAM (approximately 1 nm thick) on the SiO2 film surface of the substrate (film formation process). The treatment liquid used was a toluene solvent in which octadecyltrichlorosilane, a SAM-forming material, was dissolved. The content (concentration) of octadecyltrichlorosilane was 5% by mass relative to the total mass of the treatment liquid.
[0156] Next, the substrate was pulled out of the treatment solution, and a removal solution was continuously supplied to the substrate for 1 minute to remove the unadsorbed SAM-forming material remaining on the substrate surface (removal step). Toluene was used as the removal solution.
[0157] Next, the surface of the substrate on which the SAM was formed was dried by blowing nitrogen gas onto it after it was removed from the removal solution (drying step). The temperature of the nitrogen gas was room temperature, and the drying time was 0.33 minutes.
[0158] Furthermore, the dried substrate was annealed at a heating temperature (annealing temperature) of 100° C. for a heating time (annealing time) of 60 minutes (annealing step). Subsequently, the substrate after the annealing step was allowed to cool naturally to room temperature, thereby producing a sample according to this embodiment.
[0159] Next, the obtained sample was subjected to an etching process. Specifically, the substrate was immersed in an etching solution, and the area on the substrate surface that was not protected by the SAM was etched. The etching conditions were set to 200 seconds for immersion in the etching solution (etching process time) so that the amount of SiO2 etched was about 10 nm. An aqueous hydrogen fluoride solution was used as the etching solution, and the volume ratio of hydrogen fluoride to DIW was hydrogen fluoride:DIW=1:100.
[0160] Next, the substrate was removed from the etching solution and immersed in DIW for 0.5 minutes, then removed from the DIW (DIW rinsing process), and the etched surface was dried by spraying nitrogen gas (drying process). The temperature of the nitrogen gas was room temperature, and the drying time was 0.33 minutes.
[0161] Example 2 In this example, the heating temperature (annealing temperature) in the annealing step was changed to 150° C. Except for that, samples were prepared in the same manner as in Example 1, and the obtained samples were subjected to an etching treatment.
[0162] Example 3 In this example, the heating temperature (annealing temperature) in the annealing step was changed to 200° C. Except for that, samples were prepared in the same manner as in Example 1, and the obtained samples were subjected to an etching treatment.
[0163] Comparative Example 1 This comparative example differs from Example 1 in that the annealing step was not performed. Except for that, a sample was prepared in the same manner as in Example 1, and the obtained sample was subjected to an etching treatment.
[0164] (SAM compactness evaluation) For each of the samples according to Examples 1 to 3 and Comparative Example 1, the area of film defects in the SAM was calculated to evaluate the denseness of the SAM.
[0165] That is, the SAM of each sample was imaged using an atomic force microscope (AFM) (trade name: Dimension Icon, manufactured by Bruker Japan Co., Ltd.), and an observation image (AFM image) of 500 nm square was obtained. Next, each obtained observation image was binarized, and then image processing was performed to map the film defects, and the site (region) of the film defect of the SAM was identified. In order to identify the site (region) of the film defect of the SAM by mapping, image processing was performed so that defects located at a depth of less than 1 nm from the SAM surface were mapped, taking into consideration that the film thickness of the SAM was about 1 nm. This ensured that the site (region) at a depth of more than 1 nm from the SAM surface, more specifically, the etched site, was not mapped as the region of the film defect of the SAM and was not included in the area. Next, the area of the film defect region of the SAM identified by image processing was calculated, and the ratio to the area of the entire region in the observation image was calculated. The results are shown in Table 1.
[0166] As can be seen from Table 1, the area ratios of film defects in the SAMs in Examples 1 to 3 were 31.7%, 0.54%, and 0%, respectively, which were all reduced compared to the area ratio of film defects of 54.6% in the SAM in Comparative Example 1. This confirmed that the SAMs in Examples 1 to 3 all had good denseness.
[0167] [Table 1] [Explanation of symbols]
[0168] 1 SiO2 layer 2 SiN layer 3. Laminate 4. Memory Trench 5 SAM (self-assembled monolayer) molecule 6 Hydroxyl groups 9, 9' SAM (self-assembled monolayer) 100 Semiconductor manufacturing equipment 110 Board holding part 120 Supply section 130 Removal liquid supply section 140 Inert gas supply section 150 Annealing and cooling section (Annealing section, cooling section) 151 Plate body 152 Heater 154 Lifting and Rotating Mechanism 155 Elevation shaft 156 Space 170 Etching solution supply unit 180 Volatile Organic Solvent Supply Section 220 Steam supply section 300 Control section 400 Substrate Processing Unit 500 Etching Processing Units 510 Lifter 520 Treatment tank S1 Self-assembled monolayer (SAM) formation process S2, S2' Etching process S101 Film formation process S102 Removal process S103 Drying process S104, S104' Annealing process S105 Cooling process W substrate Surface of Wf substrate Back side of Wb board
Claims
1. A substrate processing method for forming a self-assembled monolayer on a surface of a substrate, comprising the steps of: a film formation step of contacting a treatment liquid containing molecules capable of forming the self-assembled monolayer with the surface to chemically adsorb the molecules and form the self-assembled monolayer; a removing step of contacting a removing liquid with the surface of the substrate after the film forming step to remove at least a portion of the molecules that are not chemically adsorbed; an annealing step of heating the substrate after the removing step; A method for processing a substrate, comprising:
2. The annealing step includes: a low-temperature annealing step of heating the substrate at a temperature higher than room temperature and not higher than 100° C.; A high-temperature annealing step of heating the substrate at a temperature in the range of more than 100° C. and less than 200° C.; The substrate processing method according to claim 1 , further comprising at least one of the steps of:
3. 2. The substrate processing method according to claim 1, wherein the annealing step is performed in an atmosphere containing at least water.
4. The substrate processing method according to claim 1 , further comprising a cooling step of rapidly cooling the substrate to room temperature after the annealing step.
5. 1. A method for manufacturing a semiconductor device, comprising processing a substrate having a laminate provided on a surface thereof, the method comprising: The laminate includes a layer to be protected from etching and a layer to be etched that are alternately laminated, selectively forming a self-assembled monolayer on at least a surface of the layer to be protected; and selectively etching the layer to be etched using the self-assembled monolayer as a protective layer, The step of forming a self-assembled monolayer includes: a film formation step of contacting a treatment liquid containing molecules capable of forming the self-assembled monolayer with the surface of the layer to be protected to chemically adsorb the molecules; a removing step of contacting a removing liquid with the surface of the protection layer after the film forming step to remove at least a part of the molecules that are not chemically adsorbed; an annealing step of heating the protective layer after the removing step; A method for manufacturing a semiconductor device comprising the steps of:
6. The annealing step includes: a low-temperature annealing step of heating the protective layer at a temperature higher than room temperature and not higher than 100° C.; a high-temperature annealing step of heating the protective layer at a temperature in the range of more than 100° C. and less than 200° C.; 6. The method for manufacturing a semiconductor device according to claim 5, comprising at least one of the steps of:
7. The annealing step is carried out in an atmosphere containing at least water. The method for manufacturing a semiconductor device according to claim 5 .
8. The method for manufacturing a semiconductor device according to claim 5 , further comprising a cooling step of rapidly cooling said substrate to room temperature after said annealing step.
9. A substrate processing apparatus for forming a self-assembled monolayer on a surface of a substrate, comprising: a supply unit that supplies a treatment liquid containing molecules capable of forming the self-assembled monolayer to the surface to form the self-assembled monolayer; a removing liquid supplying unit that supplies a removing liquid to the surface of the substrate after the supply of the processing liquid, thereby removing at least a portion of the molecules that are not chemically adsorbed; an annealing section that heats the substrate after removing at least a portion of the molecules; The substrate processing apparatus includes:
10. The annealing section includes: performing low-temperature annealing on the substrate after removing at least a portion of the molecules by heating at a temperature higher than room temperature and not higher than 100° C.; And / or the substrate processing apparatus according to claim 9 , further comprising: performing high-temperature annealing on the substrate after removing at least a portion of the molecules by heating the substrate at a temperature in the range of more than 100° C. and not more than 200° C.
11. The substrate processing apparatus according to claim 9 , wherein the annealing section heats the substrate in an atmosphere containing at least water.
12. The substrate processing apparatus according to claim 9 , further comprising a cooling section that rapidly cools the substrate to room temperature after the substrate has been heated by the annealing section.
13. A semiconductor manufacturing apparatus for processing a substrate having a laminate on a surface thereof, comprising: The laminate includes a layer to be protected from etching and a layer to be etched which are alternately laminated, a supply unit that supplies a treatment liquid containing molecules capable of forming a self-assembled monolayer to the surface to form the self-assembled monolayer; a removing liquid supplying unit that supplies a removing liquid to the surface of the substrate after the supply of the processing liquid, thereby removing at least a portion of the molecules that are not chemically adsorbed; an annealing section that heats the substrate after removing at least a portion of the molecules; an etching unit that selectively etches and removes the layer to be etched using the self-assembled monolayer as a protective layer; A semiconductor manufacturing apparatus comprising:
14. A semiconductor manufacturing apparatus for processing a substrate having a laminate on a surface thereof, comprising: The laminate includes a layer to be protected from etching and a layer to be etched which are alternately laminated, a substrate processing unit for selectively forming a self-assembled monolayer on at least a surface of the layer to be protected; an etching processing unit that selectively etches and removes the layer to be etched using the self-assembled monolayer as a protective layer; The substrate processing unit includes: a supply unit that supplies a treatment liquid containing molecules capable of forming the self-assembled monolayer to the surface to form the self-assembled monolayer; a removing liquid supplying unit that supplies a removing liquid to the surface of the substrate after the supply of the processing liquid, thereby removing at least a portion of the molecules that are not chemically adsorbed; an annealing section that heats the substrate after removing at least a portion of the molecules; A semiconductor manufacturing apparatus comprising:
15. The annealing section includes: performing low-temperature annealing on the substrate after removing at least a portion of the molecules by heating at a temperature higher than room temperature and not higher than 100° C.; And / or the semiconductor manufacturing apparatus according to claim 13 or 14, further comprising: performing high-temperature annealing on the substrate after removing at least a portion of the molecules by heating the substrate at a temperature in the range of more than 100° C. and not more than 200° C.
16. 15. The semiconductor manufacturing apparatus according to claim 13, wherein the annealing section heats the substrate in an atmosphere containing at least water.
17. 15. The semiconductor manufacturing apparatus according to claim 13, further comprising a cooling section that rapidly cools the substrate to room temperature after heating by the annealing section.
Citation Information
Patent Citations
Etching method
JP2013062278A
A method for selective dielectric deposition using self-assembled monolayers
JP2018512504A
System and method for spin-on coating of periodic organosilicate or self-assembled monolayer on substrate
JP2019145792A
Substrate processing method and substrate processing device
JP2020126934A
Method of washing away acidic gas from gas mixture
JP1979090071A
Cited By
Cooling apparatus, substrate processing apparatus, and cooling method
CN122835066A
Cooling apparatus, substrate processing apparatus, and method for cooling processing liquid
CN122835167A
Cooling apparatus, substrate processing apparatus, and method for cooling processing liquid
CN122835168A
Cooling apparatus and substrate processing apparatus
CN122835169A
Substrate processing apparatus
CN122847092A