Hardmask composition, hardmask layer, and method of forming patterns

A hard mask composition with a self-polymer and solvent forms a dense, strong hard mask layer, addressing the challenge of forming fine semiconductor patterns by enhancing film strength and density for effective pattern transfer.

JP2024134514AActive Publication Date: 2024-10-03SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024000154
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-20
Filing Date
2024-01-04
Publication Date
2024-10-03
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

Existing lithographic techniques struggle to form fine patterns with good profiles as the size of semiconductor patterns decreases to several tens of nanometers, requiring improved film strength and density in hard mask layers.

Method used

A hard mask composition comprising a self-polymer of a specific compound and a solvent, which forms a hard mask layer through heat treatment, enhancing film density and strength by random cross-linking of structural units.

Benefits of technology

The hard mask layer exhibits improved film strength and density, enabling effective pattern transfer during etching processes, ensuring high-quality pattern formation in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134514000001
    Figure 2024134514000001
  • Figure 2024134514000002
    Figure 2024134514000002
  • Figure 2024134514000003
    Figure 2024134514000003
Patent Text Reader

Abstract

To provide a hardmask composition capable of forming a hardmask layer that may have excellent film strength and improved film density, thereby ensuring excellent pattern formation.SOLUTION: The invention relates to: a hardmask composition comprising a solvent and a self-polymer of a compound represented by chemical formula 1 in the figure; a hardmask layer produced from the hardmask composition; and a method of forming patterns from the hardmask composition. The definition of chemical formula 1 is as described in the specification.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hardmask composition, a hardmask layer including a cured product of the hardmask composition, and a patterning method using the hardmask composition. [Background technology]

[0002] In recent years, the semiconductor industry has been evolving from patterns of several hundred nanometers to ultrafine technology with patterns of several to tens of nanometers in size. Effective lithographic techniques are essential to realize such ultrafine technology.

[0003] A typical lithographic technique includes the steps of forming a material layer on a semiconductor substrate, coating a photoresist layer thereon, exposing and developing the material layer to form a photoresist pattern, and then etching the material layer using the photoresist pattern as a mask.

[0004] In recent years, as the size of a pattern to be formed decreases, it is difficult to form a fine pattern having a good profile using only the typical lithographic techniques described above. Therefore, a supplementary layer called a hard mask layer can be formed between a material layer to be etched and a photoresist layer to form a fine pattern. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Korean Patent Publication No. 10-2016-0145480 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a hard mask composition capable of forming a hard mask layer having excellent film strength and improved film density, thereby ensuring excellent pattern formability.

[0007] Another object of the present invention is to provide a hard mask layer comprising a cured product of the above hard mask composition.

[0008] It is still another object of the present invention to provide a pattern forming method using the above hard mask composition. [Means for solving the problem]

[0009] The hard mask composition according to the present invention includes a self-polymer of a compound represented by the following Chemical Formula 1, and a solvent.

[0010] [ka]

[0011] In the above chemical formula 1, The ring represented by A is a 5- or 6-membered ring formed through a saturated or unsaturated bond, and the skeleton of the ring is composed entirely of carbon atoms or of carbon atoms and one or more oxygen atoms or nitrogen atoms; L 1 and L 2 are each independently -(C=O)H; R 1 and R 2 each independently represents a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 30 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 30 carbon atoms, or a substituted or unsubstituted heterocycloalkyl group having 1 to 30 carbon atoms; m1 and m2 are each independently 0 or 1, and m1+m2=1; n1 is an integer from 0 to 3, and n2 is 0 or 1; k is 0 or 1, If k=0, then m1=1.

[0012] R in the above Chemical Formula 1 1 and R 2 are each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, and n1+n2 is preferably an integer of 1 to 4.

[0013] R in the above Chemical Formula 1 1 and R 2 are each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, and n1 is preferably an integer of 1 to 3.

[0014] The compound represented by the above Chemical Formula 1 is preferably at least one of the compounds represented by the following Chemical Formulas 2 to 5.

[0015] [ka]

[0016] In the above Chemical Formula 2 to the above Chemical Formula 5, R a and R beach independently represents a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 30 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 30 carbon atoms, or a substituted or unsubstituted heterocycloalkyl group having 1 to 30 carbon atoms; X 3 -CR c R d -, -O-, or -NR e - and X 4 and X 5 are each independently -CR f -, or -N-, In this case, the above R c ~R f each independently represents a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, na is an integer between 0 and 3, nb is 0 or 1.

[0017] R in the above chemical formulas 2 to 5 a and R b are each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, and it is preferable that na+nb is an integer of 1 to 4.

[0018] R in the above chemical formulas 2 to 5 a and R bare each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, and na is preferably an integer of 1 to 3.

[0019] X in the above formula 3 3 is -O-, or -NR e -, and X in the above formula 4 4 and X in the above formula 5 5 are each independently -CR f - and Above R e and R f is preferably each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms.

[0020] The weight average molecular weight of the self-polymer is preferably 1,000 g / mol to 200,000 g / mol.

[0021] The self-polymer is preferably contained in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition.

[0022] The solvent is preferably propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, methylpyrrolidinone, acetylacetone or ethyl 3-ethoxypropionate.

[0023] According to another embodiment, there is provided a hardmask layer comprising the cured hardmask composition described above.

[0024] According to yet another embodiment, there is provided a method of forming a pattern, the method including the steps of providing a material layer on a substrate, applying the above-described hard mask composition on the material layer, heat-treating the hard mask composition to form a hard mask layer, forming a photoresist layer on the hard mask layer, exposing and developing the photoresist layer to form a photoresist pattern, selectively removing the hard mask layer using the photoresist pattern to expose portions of the material layer, and etching the exposed portions of the material layer.

[0025] The step of forming the hard mask layer preferably includes a step of performing a heat treatment at 100°C to 1,000°C. Effect of the Invention

[0026] According to the present invention, there is provided a hard mask composition capable of forming a hard mask layer having excellent film strength and improved film density, thereby ensuring excellent pattern formability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.

[0028] Unless otherwise defined in this specification, "substituted" means that a hydrogen atom in a compound is replaced with a halogen atom (F, Br, Cl, or I), a hydroxyl group, an alkoxy group, a nitro group, a cyano group, an amino group, an azide group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid group or a salt thereof, a vinyl group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a carbon atom, a substituted or unsubstituted alkyl group ... It means that the alkyl group is substituted with a substituent selected from an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an arylaryl group having 9 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, a heteroarylalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a cycloalkenyl group having 3 to 15 carbon atoms, a cycloalkynyl group having 6 to 15 carbon atoms, a heterocycloalkyl group having 3 to 30 carbon atoms, and combinations thereof.

[0029] Furthermore, two adjacent substituents among the above-mentioned substituted halogen atoms (F, Br, Cl, or I), hydroxy groups, nitro groups, cyano groups, amino groups, azide groups, amidino groups, hydrazino groups, hydrazono groups, carbonyl groups, carbamoyl groups, thiol groups, ester groups, carboxy groups and salts thereof, sulfonic acid groups and salts thereof, phosphoric acid and salts thereof, alkyl groups having 1 to 30 carbon atoms, alkenyl groups having 2 to 30 carbon atoms, alkynyl groups having 2 to 30 carbon atoms, aryl groups having 6 to 30 carbon atoms, arylalkyl groups having 7 to 30 carbon atoms, alkoxy groups having 1 to 30 carbon atoms, heteroalkyl groups having 1 to 20 carbon atoms, heteroarylalkyl groups having 3 to 20 carbon atoms, cycloalkyl groups having 3 to 30 carbon atoms, cycloalkenyl groups having 3 to 15 carbon atoms, cycloalkynyl groups having 6 to 15 carbon atoms, or heterocyclic groups having 2 to 30 carbon atoms may be bonded to form a ring.

[0030] Unless otherwise defined herein, the term "aryl group" refers to a group having one or more aromatic hydrocarbon moieties, and broadly includes aromatic hydrocarbon moieties linked by single bonds and non-aromatic fused rings to which aromatic hydrocarbon moieties are directly or indirectly fused. Aryl groups include monocyclic, polycyclic, or fused polycyclic (i.e., polycyclic groups containing rings which share adjacent pairs of carbon atoms) functional groups.

[0031] More specifically, the substituted or unsubstituted aryl group having 6 to 30 carbon atoms may be, but is not limited to, a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted naphthacenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted p-terphenyl group, a substituted or unsubstituted m-terphenyl group, a substituted or unsubstituted o-terphenyl group, a substituted or unsubstituted chrysenyl group, a substituted or unsubstituted triphenylene group, a substituted or unsubstituted perylenyl group, a substituted or unsubstituted fluorenyl group, a substituted or unsubstituted indenyl group, a substituted or unsubstituted furanyl group, or a combination thereof.

[0032] Unless otherwise defined in this specification, "hetero" means containing 1 to 3 heteroatoms selected from N, O, S, Se and P.

[0033] Unless otherwise defined in this specification, an "alkyl group" refers to a monovalent straight or branched chain hydrocarbon group consisting of carbon atoms linked by single bonds.

[0034] Unless otherwise defined in this specification, the term "alkenyl group" means a monovalent straight or branched chain hydrocarbon group containing at least one double bond between carbon atoms.

[0035] Unless otherwise defined in this specification, the term "alkynyl group" means a monovalent straight or branched chain hydrocarbon group containing at least one triple bond between carbon atoms.

[0036] Unless otherwise defined in this specification, a "cycloalkyl group" refers to a monovalent cyclic hydrocarbon group composed of carbon atoms linked by single bonds.

[0037] Unless otherwise defined in this specification, a "heteroalkyl group" refers to a monovalent linear or branched hydrocarbon group consisting of a single bond between carbon atoms in which at least one carbon atom is replaced with at least one heteroatom selected from N, O, S, Se, and P.

[0038] Unless otherwise defined in this specification, the term "heterocycloalkyl group" refers to a monovalent cyclic hydrocarbon group in which at least one carbon atom is substituted with at least one heteroatom selected from N, O, S, Se, and P, and is formed by linking carbon atoms with a single bond.

[0039] As used herein, polymers include both oligomers and polymers.

[0040] Unless otherwise specified in this specification, the "weight average molecular weight" is measured by dissolving a powder sample in tetrahydrofuran (THF) and then using Agilent Technologies' 1200 series gel permeation chromatography (GPC) (the column is Shodex's LF-804 and the standard sample is Shodex's polystyrene).

[0041] In the semiconductor industry, there is a constant demand to reduce the size of chips. To meet this demand, the line width of the resist patterned by lithography must be on the order of several tens of nanometers. Therefore, the height that can withstand the line width of the resist pattern is limited, and the resist may not be able to withstand the etching step. To compensate for this, an auxiliary layer called a hard mask layer is used between the material layer to be etched and the photoresist layer. This hard mask layer serves as an intermediate film that transfers the fine pattern of the photoresist to the material layer through selective etching. Therefore, the hard mask layer is required to have a high film density and improved film strength so that it can withstand the etching process required for pattern transfer.

[0042] The hard mask composition according to the present invention includes an autopolymer (homopolymer). The autopolymer has excellent crosslinking properties and the structural units are densely linked, so that when a composition including the autopolymer is heat-treated, a dense film structure can be formed due to the dense linkage between the polymers or structural units. Therefore, the hard mask layer formed from the hard mask composition according to the present invention can have high film density and improved film strength.

[0043] Specifically, the hard mask composition according to the present invention includes a self-polymer of a compound represented by the following Chemical Formula 1, and a solvent.

[0044] [ka]

[0045] In the above chemical formula 1, The ring represented by A is a 5- or 6-membered ring formed through a saturated or unsaturated bond, and the skeleton of the ring is composed entirely of carbon atoms or of carbon atoms and one or more oxygen atoms or nitrogen atoms; L 1 and L 2 are each independently -(C=O)H; R1 and R 2 each independently represents a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 30 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 30 carbon atoms, or a substituted or unsubstituted heterocycloalkyl group having 1 to 30 carbon atoms; m1 and m2 are each independently 0 or 1, and m1+m2=1; n1 is an integer from 0 to 3, and n2 is 0 or 1; k is 0 or 1, If k=0, then m1=1.

[0046] The compound represented by Chemical Formula 1 contains aromatic rings and / or heterocycles with high carbon content, which can harden the film of the hard mask layer containing the self-polymer of the compound. In addition, the compound contains aromatic rings and / or heterocycles with relatively small size, which can be more densely connected to each other, thereby increasing the film density of the hard mask layer containing these self-polymers and further increasing the film strength.

[0047] The self-polymer according to one embodiment of the present invention is formed by the self-polymerization of the compound represented by Chemical Formula 1. The aldehyde group contained in the compound forms a bond between the compounds, and the bond formation may proceed randomly. Specifically, in one molecule, any carbon atom on an aromatic ring of another molecule is bonded to a carbon atom of an aldehyde, and thus the bond may occur randomly. That is, the self-polymer according to one embodiment may have a form in which the compounds represented by Chemical Formula 1 are randomly linked in a branched form. The initial reaction in which bonds between compounds occur randomly can be simply diagrammed as the following Reaction Scheme 1. However, the following Reaction Scheme 1 is merely an example of a bonding reaction between compounds, and is not limited thereto.

[0048] [ka]

[0049] When the compound self-polymerizes as shown in Reaction Scheme 1, the connections between the structural units can be denser than in a copolymer formed by linking two or more different structural units together. Therefore, the film strength of a hard mask layer formed from a composition including the self-polymer of the compound represented by Chemical Formula 1 can be improved.

[0050] The ring represented by A in the above chemical formula 1 is a 5- or 6-membered ring formed through a saturated or unsaturated bond, i.e., a single bond or a double bond, and the skeleton of the ring may be composed entirely of carbon atoms, or may be composed of carbon atoms and one or more oxygen atoms or nitrogen atoms. The number of atoms constituting the ring of A may be, for example, 5 or 6. When the number of atoms constituting the ring of A is 5, one of the elements may be oxygen (O) or nitrogen (N), and the ring represented by A may be, but is not limited to, a furan ring or a pyrrole ring.

[0051] R in the above Chemical Formula 1 1 and R 2 are each independently a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms. For example, each independently is a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, such as a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 5 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, but are not limited thereto.

[0052] In the above formula 1, n1+n2 is an integer of 0 to 4, for example, an integer of 1 to 4, for example, an integer of 1 to 3, but is not limited thereto. In this case, n1 is an integer of 0 to 3, for example, an integer of 1 to 3, but is not limited thereto.

[0053] In the above chemical formula 1, m1 and m2 are each independently 0 or 1, and m1 and m2 are not 0 at the same time, and m1+m2=1.

[0054] The compound represented by the above chemical formula 1 is preferably at least one of the compounds represented by the following chemical formulas 2 to 5.

[0055] [ka]

[0056] In the above Chemical Formula 2 to the above Chemical Formula 5, Above R a and R b are each independently a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 30 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 30 carbon atoms, or a substituted or unsubstituted heterocycloalkyl group having 1 to 30 carbon atoms.

[0057] For example, the above R a and R bare each independently a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms; for example, each independently a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, but are not limited to these.

[0058] As an example, R a and R b are each independently a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 5 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, for example, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 5 carbon atoms, or a substituted alkyl group having 1 to 5 carbon atoms, but are not limited to these.

[0059] Above X 3 -CR c R d -, -O-, or -NR e - and the above X 4 and X 5 are each independently -CR f = or -N = and the above R c ~R f are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms. For example, c ~R f are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 16 carbon atoms; for example, each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, but are not limited to these.

[0060] For example, X in the above formula 33 -CR c R d -, -O-, or -NR e - (where R e is a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms.) Examples thereof are -CH2-, -CH(CH3)-, -O-, or -NH-, for example, -O- or -NH-, but are not limited to these.

[0061] For example, X in the above formula 4 4 and X in the above formula 5 5 are each independently -CR f = where R f is a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, for example, R f is a hydrogen atom or a deuterium atom, but is not limited thereto.

[0062] In the above Chemical Formula 2 to Chemical Formula 5, na is an integer of 0 to 3, for example, an integer of 1 to 3, but is not limited thereto. In addition, in the above Chemical Formula 3 to Chemical Formula 5, nb is 0 or 1.

[0063] The self-polymer may have a weight average molecular weight of 1,000 g / mol to 200,000 g / mol. For example, the weight average molecular weight may be 1,000 g / mol to 150,000 g / mol, for example, 1,000 g / mol to 100,000 g / mol, for example, 1,200 g / mol to 50,000 g / mol, for example, 1,200 g / mol to 10,000 g / mol, but is not limited thereto. By having a weight average molecular weight in the above range, the carbon content and solubility in a solvent of the hard mask composition containing the self-polymer may be adjusted and optimized.

[0064] The self-polymer may be included in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition. For example, it may be 0.2% by mass to 30% by mass, for example, 0.5% by mass to 30% by mass, for example, 1% by mass to 30% by mass, for example, 1.5% by mass to 25% by mass, for example, 2% by mass to 20% by mass, but is not limited thereto. By including the polymer in the above range, the thickness, surface roughness, and flatness of the hard mask can be easily adjusted.

[0065] The hard mask composition according to one embodiment of the present invention may include a solvent, and in one embodiment, the solvent may include at least one selected from propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, methylpyrrolidinone, acetylacetone, or ethyl 3-ethoxypropionate, but is not limited thereto. The solvent is not particularly limited as long as it has sufficient solubility and / or dispersibility in the polymer.

[0066] The hard mask composition may further include additives such as a surfactant, a crosslinking agent, a thermal acid generator, and a plasticizer.

[0067] Examples of the surfactant that can be used include, but are not limited to, fluoroalkyl compounds, alkylbenzenesulfonates, alkylpyridinium salts, polyethylene glycols, and quaternary ammonium salts.

[0068] Examples of the crosslinking agent include melamine-based agents, substituted urea-based agents, and polymers thereof. Preferably, a compound such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, or butoxymethylated thiourea can be used as a crosslinking agent having at least two crosslink-forming substituents.

[0069] In addition, as the crosslinking agent, a crosslinking agent having high heat resistance can be used. As the crosslinking agent having high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (e.g., a benzene ring or a naphthalene ring) in the molecule can be used.

[0070] Examples of the thermal acid generator that can be used include, but are not limited to, acidic compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, and naphthalenecarboxylic acid, and / or 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, and other organic sulfonic acid alkyl esters.

[0071] According to another embodiment, there is provided a hardmask layer comprising the cured hardmask composition described above.

[0072] A method for forming a pattern using the above-described hard mask composition will now be described.

[0073] A patterning method according to one embodiment includes providing a material layer on a substrate, applying a hardmask composition on the material layer, the hardmask composition including the polymer and a solvent described above, heat treating the hardmask composition to form a hardmask layer, forming a photoresist layer on the hardmask layer, exposing and developing the photoresist layer to form a photoresist pattern, selectively removing the hardmask layer using the photoresist pattern to expose portions of the material layer, and etching the exposed portions of the material layer.

[0074] The substrate may be, for example, a silicon wafer, a glass substrate, or a polymer substrate. The material layer is the material that is ultimately to be patterned, and may be, for example, a metal layer such as aluminum, copper, etc., a semiconductor layer such as silicon, or an insulating layer such as silicon oxide, silicon nitride, etc. The material layer may be formed, for example, by a chemical vapor deposition method.

[0075] The hard mask composition may be prepared in the form of a solution and applied by a spin-on coating method, as described above. In this case, the coating thickness of the hard mask composition is not particularly limited, but may be, for example, 50 to 200,000 Å.

[0076] The step of heat treating the hard mask composition may be performed for 10 seconds to 1 hour at, for example, 100° C. to 1,000° C. For example, the step of heat treating the hard mask composition may include a plurality of heat treatment steps, for example, a first heat treatment step and a second heat treatment step.

[0077] In one embodiment, the step of heat treating the hard mask composition may include a heat treatment step performed at, for example, 100° C. to 1000° C. for 10 seconds to 1 hour. For example, the heat treatment step may be performed in an air or nitrogen atmosphere, or in an atmosphere having an oxygen concentration of 1% by weight or less.

[0078] In one embodiment, the step of heat-treating the hard mask composition includes a first heat-treatment step performed at, for example, 100° C. to 1,000° C., for example, 100° C. to 800° C., for example, 100° C. to 500° C., for example, 150° C. to 400° C., for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes.

[0079] Also, it may include a second heat treatment step successively performed at, for example, 100° C. to 1,000° C., for example, 300° C. to 1,000° C., for example, 500° C. to 1,000° C., for example, 500° C. to 600° C., for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes. As an example, the first and second heat treatment steps may be performed in an air or nitrogen atmosphere, or in an atmosphere with an oxygen concentration of 1% by mass or less.

[0080] At least one of the steps of heat treating the hard mask composition is performed at a high temperature of 200° C. or more, thereby allowing the hard mask composition to exhibit high etching resistance that can withstand etching gases and chemical solutions to which the hard mask composition is exposed in subsequent processes including an etching process.

[0081] In one embodiment, forming the hard mask layer may include an ultraviolet-visible (UV / Vis) curing step and / or a near-infrared (near IR) curing step.

[0082] In an embodiment, the step of forming the hard mask layer may include at least one of the first heat treatment step, the second heat treatment step, the UV / Vis curing step, and the near IR curing step, or may include two or more of these steps consecutively.

[0083] In one embodiment, the method may further include forming a silicon-containing thin film layer on the hard mask layer, the silicon-containing thin film layer being formed of a material such as SiCN, SiOC, SiON, SiOCN, SiC, SiO, and / or SiN.

[0084] In an embodiment, before the step of forming the photoresist layer, a bottom anti-reflective coating (BARC) may be further formed on the silicon-containing thin film layer or the hard mask layer.

[0085] In one embodiment, the step of exposing the photoresist layer can be performed using, for example, ArF, KrF, or EUV, etc. After the exposure, a heat treatment process can be performed at 100°C to 700°C.

[0086] In one embodiment, the step of etching the exposed portions of the material layer can be performed by dry etching using an etching gas, which can be, for example, N2 / O2, CHF3, CF4, Cl2, BCl3, and mixtures thereof.

[0087] The etched material layer can be formed in a variety of patterns, which can be diverse, such as metal patterns, semiconductor patterns, insulating patterns, etc., and can be applied as various patterns within a semiconductor integrated circuit device, for example. EXAMPLES

[0088] The above-mentioned embodiments of the present invention will be described in more detail with reference to the following examples. However, the following examples are merely for illustrative purposes and are not intended to limit the scope of the present invention.

[0089] [Synthesis of self-polymer] (Synthesis Example 1) In a 1L three-neck flask, 122g of 4-hydroxybenzaldehyde and 19g of p-toluenesulfonic acid monohydrate were dissolved in 200g of propylene glycol monomethyl ether acetate to prepare a solution, and the solution was stirred in a thermostatic bath at 90℃ to 100℃ and reacted for 40 hours. After the polymerization reaction was completed, the intermediate product was gradually cooled to room temperature. The intermediate product was put into 400g of distilled water and 400g of methanol, stirred vigorously, and then allowed to stand. Next, the supernatant was removed and the precipitate was dissolved in 200g of propylene glycol monomethyl ether acetate (PGMEA). Then, the methanol and distilled water remaining in the solution were removed under reduced pressure to obtain self-polymer A. (Mw: 1,500g / mol)

[0090] (Synthesis Example 2) In a 1L three-neck flask, 174g of 4-trifluoromethylbenzaldehyde and 19g of p-toluenesulfonic acid monohydrate were dissolved in 200g of propylene glycol monomethyl ether acetate to prepare a solution, and the solution was stirred in a thermostatic bath at 90℃ to 100℃ for 10 hours. After the polymerization reaction was completed, the intermediate product was gradually cooled to room temperature. The intermediate product was put into 400g of distilled water and 400g of methanol, stirred vigorously, and then allowed to stand. Next, the supernatant was removed and the precipitate was dissolved in 200g of propylene glycol monomethyl ether acetate (PGMEA). Then, the methanol and distilled water remaining in the solution were removed under reduced pressure to obtain self-polymer B. (Mw: 2,000g / mol)

[0091] (Synthesis Example 3) In a 1L three-neck flask, 138g of 3,4-dihydroxybenzaldehyde and 19g of p-toluenesulfonic acid monohydrate were dissolved in 200g of propylene glycol monomethyl ether acetate to prepare a solution, and the solution was stirred in a thermostatic bath at 90℃~100℃ and reacted for 20 hours. After the polymerization reaction was completed, the intermediate product was gradually cooled to room temperature. The intermediate product was put into 400g of distilled water and 400g of methanol, stirred vigorously, and then allowed to stand. Next, the supernatant was removed and the precipitate was dissolved in 200g of propylene glycol monomethyl ether acetate (PGMEA). Then, the methanol and distilled water remaining in the solution were removed under reduced pressure to obtain self-polymer C. (Mw: 1,500g / mol)

[0092] (Comparative synthesis example) In a 1L three-neck flask, 160g of 1-naphthol, 30g (0.2mol) of paraformaldehyde, and 19g of p-toluenesulfonic acid monohydrate were dissolved in 200g of propylene glycol monomethyl ether acetate to prepare a solution, and then the solution was stirred in a thermostatic bath at 90℃ to 100℃ and reacted for 5 hours. After the polymerization reaction was completed, the intermediate product was gradually cooled to room temperature. The intermediate product was put into 400g of distilled water and 400g of methanol, stirred vigorously, and then allowed to stand. Next, the supernatant was removed and the precipitate was dissolved in 200g of propylene glycol monomethyl ether acetate (PGMEA). Then, the methanol and distilled water remaining in the solution were removed under reduced pressure to obtain a comparative polymer. (Mw: 2,000g / mol)

[0093] [Examples and Comparative Examples: Production of Hard Mask Composition] Example 1 A hard mask composition was prepared by stirring 5 g of the self-polymer A obtained in Synthesis Example 1 with 50 g of a mixture of cyclohexanone / propylene glycol monomethyl ether acetate (1:1 volume ratio) for 60 minutes and filtering through a 0.45 μm Teflon filter.

[0094] Example 2 A hard mask composition was prepared in the same manner as in Example 1, except that the self-polymer B was used instead of the self-polymer A.

[0095] Example 3 A hard mask composition was prepared in the same manner as in Example 1, except that the self-polymer C was used instead of the self-polymer A.

[0096] (Comparative Example) A hard mask composition was prepared in the same manner as in Example 1, except that the comparative polymer was used instead of the self-polymer A.

[0097] [Evaluation 1: Evaluation of film density] The hard mask compositions according to Examples 1 to 3 and Comparative Example were spin-coated on silicon wafers and then heat-treated on a hot plate at 400° C. for 2 minutes to form hard mask layers with a thickness of 1,000 Å. The film density of the formed hard mask layers was measured using an X-ray diffraction analyzer (PANalytical Co., Ltd.). The results are shown in Table 1 below.

[0098] [Table 1]

[0099] Referring to Table 1, it can be seen that the hard mask layers formed from the hard mask compositions according to Examples 1 to 3 have superior film density compared to the hard mask layers formed from the hard mask compositions according to the Comparative Examples.

[0100] [Evaluation 2: Evaluation of membrane strength] The hard mask compositions according to Examples 1 to 3 and Comparative Example were spin-on coated on a silicon wafer to a thickness of 5,000 Å and then heat-treated on a hot plate at 400° C. for 2 minutes to form thin films. The hardness (H) and modulus (E) of the thin films were then measured using a nanoindenter (cube corner tip, Pmax=300 μN).

[0101] The measurement results are shown in Table 2 below.

[0102] [Table 2]

[0103] Referring to Table 2, the hardmasks formed from the hardmask compositions according to Examples 1 to 3 exhibit much higher hardness and elastic modulus than the hardmask formed from the hardmask composition according to the Comparative Example. In other words, it can be seen that the hardmasks formed from the hardmask compositions according to the Examples exhibit superior film strength and provide hardmasks with excellent mechanical properties compared to the hardmask formed from the hardmask composition according to the Comparative Example.

[0104] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the claims also fall within the scope of the present invention.

Claims

1. A hard mask composition comprising a self-polymer of a compound represented by the following formula 1, and a solvent: 【Chemistry 1】 (In the above chemical formula 1, The ring represented by A is a 5- or 6-membered ring formed through a saturated or unsaturated bond, and the skeleton of the ring is composed entirely of carbon atoms or of carbon atoms and one or more oxygen atoms or nitrogen atoms; L 1 and L 2 are each independently -(C=O)H; R 1 and R 2 each independently represents a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 30 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 30 carbon atoms, or a substituted or unsubstituted heterocycloalkyl group having 1 to 30 carbon atoms; m1 and m2 each independently represent 0 or 1, and m1+m2=1; n1 is an integer from 0 to 3, and n2 is 0 or 1; k is 0 or 1; If k=0, then m1=1.

2. R in the above formula 1 1 and R 2 are each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, and n1+n2 is an integer of 1 to 4.

3. R in the above formula 1 1 and R 2 are each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, and n1 is an integer of 1 to 3.

4. The hard mask composition according to claim 1, wherein the compound represented by Chemical Formula 1 is at least one of compounds represented by Chemical Formulas 2 to 5 below. 【Chemistry 2】 (In the above chemical formulas 2 to 5, R a and R b each independently represents a deuterium atom, a halogen atom, a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 30 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 30 carbon atoms, or a substituted or unsubstituted heterocycloalkyl group having 1 to 30 carbon atoms; X 3 is -CR c R d -, -O-, or -NR e - and X 4 and X 5 Each independently represents -CR f -, or -N-, At this time, the R c ~R f each independently represents a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; n a is an integer from 0 to 3; nb is 0 or 1.)

5. R in the above chemical formulas 2 to 5 a and R b are each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, and na+nb is an integer of 1 to 4.

6. R in the above formulas 2 to 5 a and R b are each independently a deuterium atom, a halogen atom, a hydroxyl group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, and na is an integer of 1 to 3.

7. X in the above formula 3 3 is -O- or -NR e -, and X in the above formula 4 4 and X in the above formula 5 5 Each independently represents -CR f - and The above R e and R f The hard mask composition of claim 4, wherein each of the groups is independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms.

8. 2. The hard mask composition of claim 1, wherein the weight average molecular weight of the self-polymer is from 1,000 g / mol to 200,000 g / mol.

9. The hard mask composition of claim 1 , wherein the self-polymer is present in an amount of 0.1% by weight to 30% by weight based on the total weight of the hard mask composition.

10. 2. The hard mask composition of claim 1, wherein the solvent is propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, methylpyrrolidinone, acetylacetone, or ethyl 3-ethoxypropionate.

11. A hardmask layer comprising a cured product of the hardmask composition according to any one of claims 1 to 10.

12. providing a layer of material over a substrate; applying a hard mask composition according to any one of claims 1 to 10 onto said material layer; heat-treating the hard mask composition to form a hard mask layer; forming a photoresist layer over the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer utilizing the photoresist pattern to expose portions of the material layer; and etching exposed portions of the layer of material; A pattern forming method comprising the steps of:

13. The method of claim 12, wherein the step of forming the hard mask layer comprises a step of performing a heat treatment at a temperature of 100° C. to 1,000° C.

Citation Information

Patent Citations

  • Resist underlay film material and pattern forming method using the same

    JP2012118300A

  • Polymer, hardmask composition, and method of forming patterns

    JP2020105513A

  • Hardmask composition, hardmask layer and method of forming patterns

    JP2021063986A

  • Resist underlayer-forming composition

    JP2022132962A