Polyamic acid and composition for low dielectric member therewith

A polyamic acid with a cage-like silsesquioxane and aliphatic structure addresses the challenge of high dielectric loss and low heat resistance in polyimide materials by forming a cured film with excellent dielectric properties and heat resistance, suitable for electronic devices.

JP2024134741AActive Publication Date: 2024-10-04JNC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023045088
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Existing polyimide materials used in electronic circuits and antennas face challenges in achieving low dielectric loss tangent and high heat resistance, leading to issues such as heat generation, signal attenuation, and delay, while methods to introduce cage-like silsesquioxanes have not effectively reduced dielectric loss tangent and often compromise mechanical strength and heat resistance.

Method used

A polyamic acid with a cage-like silsesquioxane and aliphatic structure is introduced into the main chain, combined with specific tetracarboxylic dianhydrides and diamines, to form a composition that achieves low dielectric loss tangent and high heat resistance, forming a cured film suitable for low dielectric members.

Benefits of technology

The composition results in a cured film with a dielectric loss tangent less than 0.01 at high frequencies and a 5% weight loss temperature of 450°C or higher, suitable for use in electronic devices and equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134741000001
    Figure 2024134741000001
  • Figure 2024134741000002
    Figure 2024134741000002
  • Figure 2024134741000003
    Figure 2024134741000003
Patent Text Reader

Abstract

To provide a polyamic acid having both high heat resistance and low dielectric loss tangent, and a composition for low dielectric members containing the same, low dielectric members such as a low dielectric substrate, an interlayer insulating film for a low dielectric substrate, or a low dielectric coating material, which are made of a cured film obtained by curing the low dielectric member composition of the present invention, and electronic devices such as electronic circuits, sensors, antennas, and radars using these, or electronic equipment using these low dielectric members and electronic devices.SOLUTION: A tetracarboxylic dianhydride including an aliphatic tetracarboxylic dianhydride is reacted with a diamine having a cage-shaped silsesquioxane (perfect) structure to obtain a polyamic acid having an aliphatic structure, preferably simultaneously having the aliphatic structure and a cage-shaped silsesquioxane (perfect) structure in a main chain. Furthermore, a composition for low dielectric member using the polyamic acid is provided.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamic acid and a composition for low dielectric components using the same, and more specifically to a polyamic acid having a cage-type silsesquioxane structure and an aliphatic structure, preferably an alicyclic structure, in the main chain, a composition for low dielectric components containing the polyamic acid, and a low dielectric component comprising a cured film having high heat resistance and low dielectric tangent properties obtained from the composition for low dielectric components, and electronic devices such as electronic circuits, sensors, antennas and radars having a low dielectric component comprising the cured film, or electronic equipment using these low dielectric components and electronic devices. [Background technology]

[0002] In recent years, signal frequencies have been increasing in response to the demand for ultra-high speed and large capacity information transmission. Higher frequencies increase the transmission loss of substrate materials for electronic circuits and antennas, resulting in problems such as heat generation in printed wiring boards and signal attenuation and delay. Transmission loss includes conductor loss caused by the conductors that form the transmission circuit and dielectric loss caused by the consumption of the electric field energy of the signal by insulators. In the high frequency range, the contribution of dielectric loss is large, and low dielectric loss materials with low dielectric loss are required as insulators for printed wiring boards of high frequency circuits. Since dielectric loss is proportional to the square root of the dielectric constant or dielectric loss tangent of the substrate material or resin, it is considered that the most effective way to reduce dielectric loss is to reduce the dielectric loss tangent of the substrate material or resin, which is a dielectric.

[0003] Polyimides, which have high insulating properties and reliability, have been widely used in electronic devices and electronic components such as circuit boards. Since polyimides contain many polar groups, it is very difficult to achieve low dielectric loss. Generally, methods to lower the dielectric constant and dielectric tangent by introducing fluorine or making the polyimide porous are used, but these methods have major issues such as reduced heat and solvent resistance, and a significant decrease in adhesion and mechanical strength.

[0004] Recently, various methods have been proposed to introduce polyhedral oligomeric silsequioxanes (POSS) into polyimides. In the reports by Nishiura et al. (see, for example, Patent Documents 1 and 2), a partially cleaved structure of POSS was mixed with polyimide to improve the problem of lack of uniformity in the thickness of the polyimide film in the conventional POSS and polyimide dispersion system, and thus succeeded in reducing the dielectric tangent. However, the partially cleaved structure of POSS is prone to thermal dissociation from the cleavage parts, and there are concerns about its heat resistance. In addition, it has been reported that giving a cage-shaped silsesquioxane a carbon-carbon double bond, a carbon-carbon triple bond, or a diallyl(iso)cyanurate skeleton is effective in improving heat resistance and dimensional stability (see, for example, Patent Documents 3 and 4). However, there have been no reports of successful reduction in the dielectric tangent, which significantly contributes to transmission loss. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-107121 A [Patent Document 2] JP 2013-18806 A [Patent Document 3] JP 2010-83917 A [Patent Document 4] JP 2004-196958 A Summary of the Invention [Problem to be solved by the invention]

[0006] In view of the problems of the prior art described above, the object of the present invention is to provide a polyamic acid having both high heat resistance and low dielectric loss tangent, and a composition for low dielectric members containing the same. It is also an object of the present invention to provide low dielectric members such as a low dielectric substrate, an interlayer insulating film for a low dielectric substrate, or a low dielectric coating material, which are made of a cured film obtained by curing the low dielectric member composition of the present invention, and electronic devices such as electronic circuits, sensors, antennas, and radars using these, or electronic equipment using these low dielectric members and electronic devices. [Means for solving the problem]

[0007] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by reacting an aliphatic tetracarboxylic dianhydride with a diamine having a cage-type silsesquioxane (perfect) structure to obtain a polyamic acid in which an aliphatic structure, preferably an alicyclic structure and a cage-type silsesquioxane structure, are introduced into the polyamic acid main chain, and by preparing a composition for low dielectric components containing the polyamic acid, and have completed the present invention.

[0008] The present invention includes the following configurations. [1] Polyamic acid (A) is obtained by reacting raw materials containing a tetracarboxylic dianhydride and a diamine, in which the tetracarboxylic dianhydride contains an aliphatic tetracarboxylic dianhydride in an amount of 2 mol % or more, and the diamine contains a diamine having a cage-shaped silsesquioxane structure.

[0009] [2] The polyamic acid (A) according to [1], wherein the content of the diamine having a cage-shaped silsesquioxane structure in the diamine is 0.5 mol % or more.

[0010] [3] The polyamic acid (A) according to [1] or [2], wherein the aliphatic tetracarboxylic dianhydride is at least one selected from the group consisting of tetracarboxylic dianhydrides represented by formulae (1-1) to (1-6). TIFF2024134741000001.tif2542 TIFF2024134741000002.tif2546 TIFF2024134741000003.tif2546 TIFF2024134741000004.tif2552 TIFF2024134741000005.tif41108 TIFF2024134741000006.tif41105 in formula (1-4), R 1 , R 2 , R 3 , and R 4 are independently hydrogen, methyl or fluorine. In formula (1-5) and formula (1-6), R is independently an alkyl having 1 to 45 carbon atoms, an aryl having 6 to 16 carbon atoms, or an arylalkyl having 7 to 16 carbon atoms; in the alkyl having 1 to 45 carbon atoms, at least one hydrogen may be replaced by fluorine; in the benzene ring in the aryl having 6 to 16 carbon atoms and the arylalkyl having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; in the alkylene in the arylalkyl having 7 to 16 carbon atoms, the number of carbon atoms is 1 to 10 and at least one -CH 2 - may be replaced by -O-; and R 5 is independently methyl or phenyl.

[0011] [4] The polyamic acid (A) according to any one of [1] to [3], wherein the diamine having a cage-shaped silsesquioxane structure is a diamine represented by formula (2-1): TIFF2024134741000007.tif4190In formula (2-1), X is independently an alkylene having 1 to 12 carbon atoms, an arylene having 6 to 16 carbon atoms, or an arylene alkylene having 7 to 16 carbon atoms; in this alkylene having 1 to 12 carbon atoms, at least one hydrogen may be replaced by fluorine, and in the benzene ring in the arylene having 6 to 16 carbon atoms and the arylene alkylene having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; R is independently an alkyl having 1 to 45 carbon atoms, an aryl having 6 to 16 carbon atoms, or an aryl alkyl having 7 to 16 carbon atoms; in this alkyl having 1 to 45 carbon atoms, at least one hydrogen may be replaced by fluorine, and at least one -CH 2 - may be replaced by -O- or -CH=CH-; in the benzene ring in the aryl having 6 to 16 carbon atoms and the arylalkyl having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; in the alkylene in the arylalkyl having 7 to 16 carbon atoms, the number of carbon atoms is 1 to 10 and at least one -CH 2 - may be replaced by -O-; and R 5 is independently methyl or phenyl.

[0012] [5] A composition for low dielectric members, comprising the polyamic acid (A) according to any one of [1] to [4].

[0013] [6] A composition for low dielectric components according to [5], wherein the composition for low dielectric components has a dielectric tangent of less than 0.01 at 10 GHz and 28 GHz when cured without adding an inorganic filler.

[0014] [7] The composition for a low dielectric member according to [5] or [6], further comprising a curing agent (C).

[0015] [8] The composition for a low dielectric member according to any one of [5] to [7], further comprising at least one additive (D) selected from the group consisting of a compound having a polymerizable double bond, a surfactant, an adhesion improver, and an antioxidant.

[0016] [9] A low dielectric member comprising a cured film obtained by curing the composition for a low dielectric member according to any one of [5] to [8].

[0017]

[10] [9] A low dielectric material according to the present invention; An electronic device having at least one capability selected from the group consisting of capabilities to generate, convert, transmit, and process radio frequency signals; electronic equipment. Effect of the Invention

[0018] The composition for low dielectric components of the present invention can be prepared by using a polyamic acid having a cage-shaped silsesquioxane structure and an aliphatic structure, preferably an alicyclic structure, in the polyamic acid main chain, and the cured film obtained by curing the composition has both a low dielectric tangent and high heat resistance. Therefore, the composition for low dielectric components containing the polyamic acid of the present invention can be used to produce low dielectric components such as low dielectric substrates, interlayer insulating films for low dielectric substrates, or low dielectric coating materials, and electronic devices such as electronic circuits, sensors, antennas, and radars using these, or electronic devices using these low dielectric components and electronic devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, the embodiments of the present invention will be described in detail, but the following description is an example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents. In addition, the embodiments of the present invention can be appropriately combined. 1. Polyamic acid (A) of the present invention The polyamic acid (A) of the present invention can be synthesized by polycondensation reaction of raw materials containing the following tetracarboxylic dianhydride and diamine.

[0020] 1-1.Tetracarboxylic dianhydride In the present invention, a tetracarboxylic dianhydride is used as a raw material for obtaining the polyamic acid (A). Examples of the tetracarboxylic dianhydride include aliphatic tetracarboxylic dianhydrides and aromatic tetracarboxylic dianhydrides. From the viewpoint of providing a low dielectric tangent, the polyamic acid (A) of the present invention is characterized in that the content of an aliphatic tetracarboxylic dianhydride, preferably an alicyclic tetracarboxylic dianhydride, more preferably at least one aliphatic tetracarboxylic dianhydride selected from the group consisting of the tetracarboxylic dianhydrides represented by the formulae (1-1) to (1-6), in the raw material tetracarboxylic dianhydride is 2 mol % or more, preferably 10 mol % or more. The preferred upper limit of the content of the aliphatic tetracarboxylic dianhydride in the raw material tetracarboxylic dianhydride is 50 mol %.

[0021] TIFF2024134741000008.tif2542 TIFF2024134741000009.tif2546 TIFF2024134741000010.tif2546 TIFF2024134741000011.tif2552 TIFF2024134741000012.tif41108 TIFF2024134741000013.tif4199

[0022] In formula (1-4), R 1 , R 2 , R 3 , and R 4 are independently hydrogen, methyl or fluorine. In formula (1-5) and formula (1-6), R is independently an alkyl having 1 to 45 carbon atoms, an aryl having 6 to 16 carbon atoms, or an arylalkyl having 7 to 16 carbon atoms; in the alkyl having 1 to 45 carbon atoms, at least one hydrogen may be replaced by fluorine; in the benzene ring in the aryl having 6 to 16 carbon atoms and the arylalkyl having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; in the alkylene in the arylalkyl having 7 to 16 carbon atoms, the number of carbon atoms is 1 to 10 and at least one -CH 2 - may be replaced by -O-; and R 5 is independently methyl or phenyl. "At least one -CH in the alkylene of the aryl alkyl 2 The meaning of the phrase "- may be replaced by -O-" is shown below as an example. 4 H 8 - at least one -CH 2 Some of the groups in which - is replaced with -O- are -C 3 H 6 O-, -CH 2 -O-(CH 2 ) 2 - and -CH 2 -O-CH 2 In this manner, the term "at least one" means "at least one selected without distinction." In consideration of the stability of the compound, the --CH 2 -OO-CH 2 -CH, where there are no adjacent oxygens 2 -O-CH 2 In the case of alkyl, the replacement of -O- is similar.

[0023] When an aliphatic tetracarboxylic dianhydride or a bulky tetracarboxylic dianhydride is used, a polyimide having a desired low dielectric constant is easily obtained, but the polyimide tends to become physically brittle. From the viewpoint of heat resistance and film formability, it is preferable to use one or more aromatic tetracarboxylic dianhydrides in combination within a range in which the effects of the polyamic acid (A) of the present invention can be maintained. Specific examples of aromatic tetracarboxylic dianhydrides that can be used in combination include 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 2,2',3,3'-diphenylsulfone tetracarboxylic dianhydride, 2,3,3',4'-diphenylsulfone tetracarboxylic dianhydride, 3,3',4,4'-diphenylether tetracarboxylic dianhydride, 2,2',3,3'-diphenylether tetracarboxylic dianhydride, 2,3,3',4'-diphenylether tetracarboxylic dianhydride, pyromellitic anhydride, biphenyl tetracarboxylic dianhydride, and the like. Examples of the dianhydride include phenyl-3,4,3',4'-tetracarboxylic dianhydride, biphenyl-2,3,2',3'-tetracarboxylic dianhydride, biphenyl-2,3,3',4'-tetracarboxylic dianhydride, meta-terphenyl-3,4,3',4'-tetracarboxylic dianhydride, para-terphenyl-3,4,3',4'-tetracarboxylic dianhydride, 2,2-[bis(3,4-dicarboxyphenyl)]hexafluoropropane dianhydride, 1,2,3,4-butanetetracarboxylic dianhydride, ethylene glycol bis(anhydrotrimellitate) (trade name: TMEG-100, manufactured by New Japan Chemical Co., Ltd.), and tetracarboxylic dianhydride having a cage-shaped silsesquioxane structure represented by formula (1-7). One or more of these can be used.

[0024] TIFF2024134741000014.tif4194

[0025] In formula (1-7), R is independently an alkyl having 1 to 45 carbon atoms, an aryl having 6 to 16 carbon atoms, or an arylalkyl having 7 to 16 carbon atoms; in the alkyl having 1 to 45 carbon atoms, at least one hydrogen may be replaced by fluorine; in the benzene ring in the aryl having 6 to 16 carbon atoms and the arylalkyl having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; in the alkylene in the arylalkyl having 7 to 16 carbon atoms, the number of carbon atoms is 1 to 10 and at least one -CH 2 - may be replaced by -O-; and R 5 is independently methyl or phenyl. Among these, pyromellitic anhydride is preferred from the viewpoint of less molecular rotation.

[0026] 1-2.Diamine In the present invention, a diamine having a cage-shaped silsesquioxane structure is used as a raw material for obtaining the polyamic acid (A). Examples of the diamine having a cage-shaped silsesquioxane structure include aliphatic diamines and aromatic diamines. The polyamic acid (A) of the present invention is characterized in that the content of diamine having a cage-shaped silsesquioxane structure, preferably represented by formula (2-1), in the raw material diamine is 0.5 mol % or more, from the viewpoint of suppressing the rotational motion of molecules and imparting a low dielectric tangent. TIFF2024134741000015.tif4190In formula (2-1), X is independently an alkylene having 1 to 12 carbon atoms, an arylene having 6 to 16 carbon atoms, or an arylene alkylene having 7 to 16 carbon atoms; in this alkylene having 1 to 12 carbon atoms, at least one hydrogen may be replaced by fluorine, and in the benzene ring in the arylene having 6 to 16 carbon atoms and the arylene alkylene having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; R is independently an alkyl having 1 to 45 carbon atoms, an aryl having 6 to 16 carbon atoms, or an aryl alkyl having 7 to 16 carbon atoms; in this alkyl having 1 to 45 carbon atoms, at least one hydrogen may be replaced by fluorine, and at least one -CH 2 - may be replaced by -O- or -CH=CH-; in the benzene ring in the aryl having 6 to 16 carbon atoms and the arylalkyl having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; in the alkylene in the arylalkyl having 7 to 16 carbon atoms, the number of carbon atoms is 1 to 10 and at least one -CH 2 - may be replaced by -O-; and R 5 is independently methyl or phenyl.

[0027] The content of the diamine having a cage-shaped silsesquioxane structure represented by formula (2-1) in the raw material diamine is preferably 2 mol% or more, and more preferably 5 mol% or more. The upper limit of the content of the diamine having a cage-shaped silsesquioxane structure represented by formula (2-1) in the raw material diamine is preferably 100 mol%, more preferably 50 mol%, and even more preferably 30 mol%.

[0028] As long as the effect of the polyamic acid (A) of the present invention can be maintained, it can be used in combination with any diamine other than the diamine having a cage-shaped silsesquioxane structure. The diamine to be used in combination may be either an aliphatic diamine or an aromatic diamine. From the viewpoint of low dielectric tangent characteristics, it is preferable to use an aliphatic diamine in combination. From the viewpoint of solubility and film-forming property, it is preferable to use an aromatic diamine in combination.

[0029] Examples of aliphatic diamines that can be used in combination include 1,2-bisaminomethylcyclohexane, 1,4-bisaminomethylcyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis(aminomethyl)norbornane, and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.

[0030] Examples of aromatic diamines that can be used in combination include 4,4'-diaminodiphenyl sulfone, 1,3-diaminobenzene, 2,4-diaminotoluene, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,7-diamino-dimethyldibenzothiophene-5,5'-dioxide, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-bis(4-aminophenyl)sulfide, 9,9-bis(4-aminophenyl)sulfide, and 1,2-dimethyl-1,2-diaminodiphenylether. nyl)fluorene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 3,3'-dihydroxy-4,4'-diaminobiphenyl, and 3,3',4,4'-tetraaminobiphenyl.

[0031] 1-3. Ratio of tetracarboxylic dianhydride to diamine The polyamic acid (A) used in the present invention is synthesized by reacting the above-mentioned tetracarboxylic dianhydride and diamine. If the difference in the number of moles of the tetracarboxylic dianhydride and diamine used is small, the molecular weight of the polymer increases and the amount of residual monomer decreases, leading to improved dielectric loss tangent characteristics. Therefore, it is preferable to set the ratio of the tetracarboxylic dianhydride and diamine in the raw materials to X moles of tetracarboxylic dianhydride and Y moles of diamine so that the relationship 0.8≦X / Y≦1.2 is satisfied. More preferably, 0.9≦X / Y≦1.1, and even more preferably, 0.95≦X / Y≦1.05.

[0032] 1-4.End-capping agent The polyamic acid (A) of the present invention may contain an end-capping agent as a raw material. Examples of the end-capping agent include a monohydroxy compound, a monoamine compound, and an acid anhydride.

[0033] When at least one selected from a monohydroxy compound and a monoamine compound is used as an end-capping agent, the acid anhydride functional group at the end of the polyamic acid can be blocked, and when an acid anhydride is used as an end-capping agent, the amino functional group at the end of the polyamic acid can be blocked. The polyamic acid (A) obtained by such end-capping improves the storage stability of the composition for low dielectric members.

[0034] Specific examples of monohydroxy compounds include benzyl alcohol, methanol, ethanol, 1-propanol, isopropyl alcohol, allyl alcohol, borneol, linalool, terpineol, and 3-ethyl-3-hydroxymethyloxetane. One or more of these may be used.

[0035] Among these, benzyl alcohol and 3-ethyl-3-hydroxymethyloxetane are more preferable.

[0036] The content of the monohydroxy compound in the raw material composition is preferably 1 to 10 parts by mole, more preferably 1 to 5 parts by mole, and even more preferably 1 to 2 parts by mole, based on 100 parts by mole of the total amount of diamines.

[0037] Examples of the monoamine compound include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine; and aminosilanes such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 4-aminobutyltrimethoxysilane, 4-aminobutyltriethoxysilane, 4-aminobutylmethyldiethoxysilane, p-aminophenyltrimethoxysilane, p-aminophenyltriethoxysilane, p-aminophenylmethyldimethoxysilane, p-aminophenylmethyldiethoxysilane, m-aminophenyltrimethoxysilane, and m-aminophenylmethyldiethoxysilane. One or more of these can be used.

[0038] Among these, butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, aniline, 3-aminopropyltrimethoxysilane, and 3-aminopropyltriethoxysilane are preferred.

[0039] When the content of the monoamine compound in the raw material composition is appropriate, the molecular weight of the polymer is extended, a polymer with a larger molecular weight is obtained, and the film-forming property and the dielectric loss tangent property are improved. The content of the monoamine compound in the raw material composition is preferably 1 to 10 parts by mole, more preferably 1 to 5 parts by mole, and further preferably 1 to 2 parts by mole, based on 100 parts by mole of the total amount of the diamines.

[0040] Specific examples of acid anhydrides include phthalic anhydride, trimellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, succinic anhydride, and dodecenylsuccinic anhydride. One or more of these may be used.

[0041] Among these, maleic anhydride, trimellitic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride are preferred.

[0042] As described above, the content of the acid anhydride in the raw material composition is preferably 1 to 10 parts by mole, more preferably 1 to 5 parts by mole, and even more preferably 1 to 2 parts by mole, relative to 100 parts by mole of the total amount of the tetracarboxylic dianhydride.

[0043] 1-5. Solvent (B1) used in the synthesis reaction of polyamic acid (A) The polyamic acid (A) can be synthesized by reacting a tetracarboxylic dianhydride with a diamine and, if necessary, an end-capping agent in a solvent. The solvent used in the synthesis reaction to obtain the polyamic acid (A) may be referred to as a reaction solvent (B1) below.

[0044] Specific examples of the reaction solvent (B1) include 4-hydroxy-2-butanone, diacetone alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol butyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, methyl 3-methoxypropionate, 3-ethoxypropionate, methyl 3-methoxy ... Examples of suitable dimethyl ethers include ethyl propionate, 3-methoxybutyl acetate, ethyl lactate, cyclopentanone, cyclohexanone, dipropylene glycol dimethyl ether, triethylene glycol dimethyl ether, tripropylene glycol dimethyl ether, γ-butyrolactone, 1-methyl-2-pyrrolidone, N,N-dimethylpropionamide, N,N-dimethylisobutyramide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylpropionamide, N-methylpropionamide, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, and dimethyl carbonate. One or more of these may be used.

[0045] Among these, from the viewpoint of the solubility of polyamic acid, γ-butyrolactone, 1-methyl-2-pyrrolidone, N,N-dimethylpropionamide, N,N-dimethylisobutyramide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylpropionamide, N-methylpropionamide, 3-methoxy-N,N-dimethylpropanamide, and 3-butoxy-N,N-dimethylpropanamide are preferred.

[0046] From the viewpoint of handling, the reaction solvent (B1) may be left as it is to be made into a polyamic acid solution or a gel-like substance. It is preferable to use the polyamic acid solution in the preparation of the composition for low dielectric members from the viewpoint of shortening the production time.

[0047] 1-6. Method for synthesizing polyamic acid (A) The order of adding the raw materials to the reaction system is not particularly limited. When the terminal blocking reaction is carried out using the monohydroxy compound, monoamine compound, and acid anhydride, the raw materials are added after the reaction of the tetracarboxylic dianhydride and the diamine, and the reaction is carried out at 10 to 40° C. for 0.1 to 12 hours.

[0048] The weight average molecular weight of the obtained polyamic acid (A) is preferably from 1,000 to 2,000,000, and more preferably from 8,000 to 500,000. Within these ranges, the solubility and film-forming properties are good.

[0049] As described above, the polyamic acid in the present invention is a polymer obtained by reacting raw materials containing a tetracarboxylic dianhydride and a diamine. In this specification, the polyamic acid also includes a form in which a part of the polyamic acid is cyclodehydrated and turned into a polyimide in the reaction process.

[0050] 2. Composition for low dielectric members according to the present invention The composition for low dielectric members of the present invention is a composition containing a polyamic acid (A) and, if necessary, a solvent (B2), and is preferably a composition for low dielectric members that, when cured without adding an inorganic filler to the composition, has a dielectric loss tangent of less than 0.01 at both 10 GHz and 28 GHz. The composition for low dielectric members of the present invention may further contain a curing agent (C), an additive (D), etc.

[0051] 2-1. Solvents used in compositions for low dielectric materials (B2) The solvent (B2) used as necessary in the composition for low dielectric members of the present invention is preferably a solvent capable of dissolving the polyamic acid (A), the curing agent (C), the additive (D), and the like.

[0052] In addition, in the case where the polyamic acid solution obtained by the synthesis of the polyamic acid (A) is used in the form of a polyamic acid solution for a composition for low dielectric components without extracting a polyamic acid solid from the polyamic acid solution, the reaction solvent (B1) contained in the polyamic acid solution is also included in the solvent (B2).

[0053] Specific examples of the solvent (B2) include 4-hydroxy-2-butanone, diacetone alcohol, 2-butanone, ethyl acetate, propyl acetate, butyl acetate, butyl propionate, ethyl lactate, methyl hydroxyacetate, ethyl hydroxyacetate, butyl hydroxyacetate, methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, methyl 3-oxypropionate, ethyl 3-hydroxypropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, methyl 3-methoxybutyl acetate, ethyl 3-ethoxypropionate, methyl 2-hydroxypropionate, propyl 2-hydroxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, 2-ethoxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, 2-ethoxypropionate, methyl 2-hydroxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, 2-ethoxypropionate, methyl 2-hydroxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxy ...ethyl 2-ethoxypropionate, ethyl 2-ethoxypropionate, ethyl Methyl pionate, ethyl 2-ethoxypropionate, methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, ethyl 2-oxobutanoate, 4-hydroxy-4-methyl-2-pentanone, 1,4-butanediol, cyclopentanone, cyclohexanone, tetrahydrofuran, acetonitrile, dioxane, toluene, xylene, γ-butyrolactone, 1-methyl-2-pyrrolidone, N,N-dimethylisobutyramide, N,N-diethylacetamide, N,N-diethylformamide, N,N-diethylpropionamide, 3-butoxy-N,N-dimethylpropanamide, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether, diethylene glycol Examples of the polypropylene glycol include polyethylene glycol having a weight average molecular weight of 1,000 or less, polypropylene glycol having a weight average molecular weight of 1,000 or less, poly(dipropylene glycol) having a weight average molecular weight of 1,000 or less, poly(tripropylene glycol) having a weight average molecular weight of 1,000 or less, and poly(tetrapropylene glycol) having a weight average molecular weight of 1,000 or less. At least one of these may be used.

[0054] Of these, cyclopentanone, cyclohexanone, γ-butyrolactone, 1-methyl-2-pyrrolidone, N,N-dimethylisobutyramide, N,N-diethylacetamide, N,N-diethylformamide, N,N-diethylpropionamide, 3-butoxy-N,N-dimethylpropanamide, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether, and diethylene glycol ethyl methyl ether are preferred.

[0055] When solubility is more important, cyclopentanone, cyclohexanone, γ-butyrolactone, 1-methyl-2-pyrrolidone, N,N-dimethylisobutyramide, N,N-diethylacetamide, N,N-diethylformamide, 3-butoxy-N,N-dimethylpropanamide, and N,N-diethylpropionamide are more preferable.

[0056] The content of the solvent (B2) is preferably 60 to 99% by weight, more preferably 70 to 96% by weight, based on the total amount of the composition for low dielectric members.

[0057] 2-2. Hardener (C) The composition for low dielectric members of the present invention may further contain a curing agent (C). By adding the curing agent (C), a crosslinking reaction occurs with the low molecular weight polyimide and the monomer components remaining after imidization during the curing process of the composition for low dielectric members, and adverse effects such as a decrease in heat resistance and a decrease in dielectric properties due to the residual monomers are suppressed, and a low dielectric member with higher heat resistance can be expected.

[0058] The curing agent (C) is not particularly limited as long as it is a compound having two or more functional groups reactive with a carboxyl group in one molecule.

[0059] Examples of functional groups which react with carboxyl groups are epoxy functional groups (oxirane, oxetane) and oxazoline functional groups.

[0060] Compounds having two or more functional groups per molecule that react with carboxyl groups include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, glycidyl ether type epoxy compounds, glycidyl ester type epoxy compounds, biphenyl type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, bisphenol A novolac type epoxy compounds, aliphatic polyglycidyl ether compounds, cyclic aliphatic epoxy compounds, epoxy compounds having a siloxane bond site, glycidylamine type epoxy compounds, and other oxirane compounds having two or more epoxy groups (oxiranes) per molecule, 3,7-bis(3-oxetanyl)-5-oxa-nonane, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, and the like. Examples of the epoxy groups include oxetane compounds having two or more epoxy groups (oxetanes) per molecule, such as 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, triethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, 3-ethyl-3-(3-ethyl-3-oxetanylmethyloxymethyl)oxetane, and xylylene bisoxetane; compounds having two or more oxazoline functional groups per molecule; and polymers having two or more epoxy functional groups and at least one of oxazoline functional groups per molecule.

[0061] Specific examples of compounds having two or more epoxy groups (oxiranes) per molecule include bisphenol A type epoxy compounds jER 828, jER 1004, and jER 1009 (all trade names; manufactured by Mitsubishi Chemical Corporation), bisphenol F type epoxy compounds jER 806 and jER 4005P (all trade names; manufactured by Mitsubishi Chemical Corporation), glycidyl ether type epoxy compounds TECHMORE VG3101L (trade name; manufactured by Printec Co., Ltd.), EHPE3150 (trade name; manufactured by Daicel Corporation), EPPN-501H, EPPN-502H (all trade names; manufactured by Nippon Kayaku Co., Ltd.), and jER 1032H60 (trade name; manufactured by Mitsubishi Chemical Corporation), and glycidyl ester type epoxy compound Denacol. EX-721 (trade name; manufactured by Nagase ChemteX Corporation), diglycidyl 1,2-cyclohexanedicarboxylate (trade name; manufactured by Tokyo Chemical Industry Co., Ltd.), biphenyl-type epoxy compounds jER YX4000, jER YX4000H, jER YL6121H (all trade names; manufactured by Mitsubishi Chemical Corporation), NC-3000, NC-3000-L, NC-3000-H, NC-3100 (all trade names; manufactured by Nippon Kayaku Co., Ltd.), phenol novolac-type epoxy compound EPPN-201 (trade name; manufactured by Nippon Kayaku Co., Ltd.), jER 152, jER 154 (all trade names; manufactured by Mitsubishi Chemical Corporation), cresol novolac epoxy compounds EOCN-102S, EOCN-103S, EOCN-104S, and EOCN-1020 (all trade names; manufactured by Nippon Kayaku Co., Ltd.), bisphenol A novolac epoxy compounds jER 157S65 and jER 157S70 (all trade names; manufactured by Mitsubishi Chemical Corporation), cyclic aliphatic epoxy compounds Celloxide 2021P, Celloxide 3000, and Epolead GT401 (all trade names; manufactured by Daicel Corporation), epoxy compounds having siloxane bond sites 1,3-bis[2-(3,4-epoxycyclohexyl)ethyl]tetramethyldisiloxane (trade name; manufactured by Gelsest Incorporated), TSL9906 (trade name; manufactured by Momentive Performance Materials Japan, LLC), COATOSIL MP200 (product name;Examples of epoxy compounds include N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane (trade name; manufactured by Momentive Performance Materials Japan, LLC), Compocelan SQ506 (trade name; manufactured by Arakawa Chemical Industries, Ltd.), ES-1023 (trade name; manufactured by Shin-Etsu Chemical Co., Ltd.), which is a glycidylamine type epoxy compound, Sumiepoxy ELM-434 (trade name; manufactured by Sumitomo Chemical Co., Ltd.), and Sumiepoxy ELM-100 (trade name; manufactured by Sumitomo Chemical Co., Ltd.).

[0062] Specific examples of compounds having two or more epoxy groups (oxetanes) per molecule include ARON OXETANE OXT-121 (XDO) (product name; manufactured by Toagosei Co., Ltd.) and ARON OXETANE OXT-221 (DOX) (product name; manufactured by Toagosei Co., Ltd.).

[0063] A specific example of a compound having two or more oxazoline functional groups per molecule is 2,2'-(1,3-phenylene)-bis(2-oxazoline).

[0064] The content of the curing agent (C) is preferably from 0.5 to 60 parts by weight, and more preferably from 1 to 30 parts by weight, based on 100 parts by weight of the polyamic acid (A).

[0065] 2-3.Additives (D) Various additives (D) can be added to the composition for low dielectric members of the present invention in order to improve film properties such as scratch resistance, coating uniformity, adhesion, etc. Main examples of the additives (D) include compounds having a polymerizable double bond, surfactants, adhesion improvers such as silane coupling agents, antioxidants, and inorganic fillers.

[0066] 2-3-1. Compounds with polymerizable double bonds The composition for low dielectric members of the present invention may contain a compound having a polymerizable double bond. The compound having a polymerizable double bond used in the composition for low dielectric members of the present invention is not particularly limited as long as it has two or more polymerizable double bonds per molecule.

[0067] Among the above-mentioned compounds having a polymerizable double bond, specific examples of compounds having two polymerizable double bonds per molecule include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, epichlorohydrin-modified ethylene glycol di(meth)acrylate, epichlorohydrin-modified diethylene glycol di(meth)acrylate, epichlorohydrin-modified triethylene glycol di(meth)acrylate, epichlorohydrin-modified tetraethylene glycol di(meth)acrylate, epichlorohydrin-modified polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, epichlorohydrin-modified propylene glycol di(meth)acrylate, epichlorohydrin-modified dipropylene glycol di(meth)acrylate, epichlorohydrin-modified tripropylene glycol di(meth)acrylate, epichlorohydrin-modified tetrapropylene glycol di(meth)acrylate, epichlorohydrin-modified polypropylene glycol di(meth)acrylate, glycerol acrylate methacrylate, glycerol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, epichlorohydrin-modified 1,6-Hexanediol di(meth)acrylate, methoxylated cyclohexyl di(meth)acrylate, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, caprolactone-modified hydroxypivalic acid neopentyl glycol di(meth)acrylate, stearic acid-modified pentaerythritol di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, bis[(meth)acryloxyneopentyl glycol]adipate, bisphenol A di(meth)acrylate, ethylene oxide-modified bisphenol A di(meth)acrylate, bisphenol F di(meth)acrylate, ethylene oxide-modified bisphenol F di(meth)acrylate, Examples of the di(meth)acrylate include bisphenol S di(meth)acrylate, ethylene oxide modified bisphenol S di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, ethylene oxide modified phosphate di(meth)acrylate, caprolactone·ethylene oxide modified phosphate di(meth)acrylate, epichlorohydrin modified phthalic acid di(meth)acrylate, tetrabromobisphenol A di(meth)acrylate, triglycerol di(meth)acrylate, neopentyl glycol modified trimethylolpropane di(meth)acrylate, and isocyanuric acid ethylene oxide modified di(meth)acrylate. In the text, "(meth)acrylate" means acrylate or methacrylate, and "(meth)acryloxy" means acryloxy or methacryloxy.,

[0068] Among the above-mentioned compounds having a polymerizable double bond, specific examples of compounds having three or more polymerizable double bonds per molecule include trimethylolpropane tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, epichlorohydrin-modified trimethylolpropane tri(meth)acrylate, glycerol tri(meth)acrylate, epichlorohydrin-modified glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, alkyl-modified dipentaerythritol tri(meth)acrylate, ethylene oxide-modified phosphate tri(meth)acrylate, and caprolactone-ethylene oxide-modified phosphate tri(meth)acrylate. tri(meth)acrylate, caprolactone-modified tris[(meth)acryloxyethyl]isocyanurate, ditrimethylolpropane tetra(meth)acrylate, diglycerin tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, alkyl-modified dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, isocyanuric acid ethylene oxide-modified tri(meth)acrylate, and carboxyl group-containing polyfunctional (meth)acrylate.

[0069] The compound having a polymerizable double bond may be used alone or in combination of two or more.

[0070] From the viewpoint of scratch resistance, among the above-mentioned compounds having a polymerizable double bond, it is preferable to select from ethylene oxide-modified bisphenol F di(meth)acrylate, ethylene oxide isocyanuric acid-modified di(meth)acrylate, ethylene oxide isocyanuric acid-modified tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and carboxyl group-containing polyfunctional (meth)acrylate.

[0071] The content of the compound having a polymerizable double bond is preferably 1 to 60 parts by weight based on 100 parts by weight of the polyamic acid (A) in the composition for low dielectric members of the present invention from the viewpoint of a good balance between scratch resistance and dielectric loss tangent characteristics. When the dielectric loss tangent characteristics are more important, the content is more preferably 1 to 20 parts by weight.

[0072] 2-3-2.Surfactants In order to improve coating uniformity, an anionic, cationic, nonionic, fluorine-based or silicon-based leveling agent or surfactant may be added to the composition for low dielectric members of the present invention.

[0073] Specific examples of surfactants include Polyflow No. 75, Polyflow No. 90, Polyflow No. 95 (all trade names; manufactured by Kyoeisha Chemical Co., Ltd.), Disperbyk-161, Disperbyk-162, Disperbyk-163, Disperbyk-164, Disperbyk-166, Disperbyk-170, Disperbyk-180, Disperbyk-181, Disperbyk-182, BYK-300, BYK-306, BYK-310, BYK-320, BYK-330, BYK-342, BYK-346, BYK-361N, BYK-3560, BYK-UV3500, BYK-UV3570 (all trade names; manufactured by BYK Japan Co., Ltd.), KP-341, KP-368, KP-96-50CS, KP-50-100CS (all trade names; manufactured by Shin-Etsu Chemical Co., Ltd.), Surflon S611 (trade name; Ftergent 222F, Ftergent 208G, Ftergent 251, Ftergent 710FL, Ftergent 710FM, Ftergent 710FS, Ftergent 601AD, Ftergent 650A, FTX-218 (all trade names; manufactured by Neos Co., Ltd.), Megafac F-410, Megafac F-430, Megafac F-444, Megafac F-472SF ... Gafac F-475, Megafac F-477, Megafac F-552, Megafac F-553, Megafac F-554, Megafac F-555, Megafac F-556, Megafac F-558, Megafac F-559, Megafac R-94, Megafac RS-75, Megafac RS-72-K, Megafac RS-76-NS, Megafac DS-21 (all trade names; manufactured by DIC Corporation), TEGO Twin 4000, TEGO Twin 4100, TEGO Flow 370, TEGO Flow 375, TEGO Glide 440, TEGO Glide 450, TEGO Rad 2200N (all trade names; manufactured by DIC Corporation).(manufactured by Evonik Japan Co., Ltd.), fluoroalkylbenzenesulfonates, fluoroalkylcarboxylates, fluoroalkylpolyoxyethyleneethers, fluoroalkylammonium iodides, fluoroalkylbetaines, fluoroalkylsulfonates, diglycerol tetrakis(fluoroalkylpolyoxyethyleneether), fluoroalkyltrimethylammonium salts, fluoroalkylaminosulfonates, polyoxyethylenenonylphenylether, polyoxyethyleneoctylphenylether, polyoxyethylenealkylethers, polyoxyethylenelaurylether, polyoxyethyleneoleylether, polyoxyethylenetridecylether , polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene laurate, polyoxyethylene oleate, polyoxyethylene stearate, polyoxyethylene laurylamine, sorbitan laurate, sorbitan palmitate, sorbitan stearate, sorbitan oleate, sorbitan fatty acid ester, polyoxyethylene sorbitan laurate, polyoxyethylene sorbitan palmitate, polyoxyethylene sorbitan stearate, polyoxyethylene sorbitan oleate, polyoxyethylene naphthyl ether, alkylbenzene sulfonate, and alkyldiphenyl ether disulfonate. One or more of these can be used.;

[0074] Among these, from the viewpoint of high coating uniformity, BYK-306, BYK-342, BYK-346, BYK-361N, BYK-3560, KP-341, Surflon S611, Ftergent 710FL, Ftergent 710FM, Ftergent 710FS, Ftergent 650A, Megafac F-477, Megafac F-556, Megafac RS-72-K, Megafac DS-21, TEGO Twin 4000, TEGO Flow 375, fluoroalkylbenzenesulfonates, fluoroalkylcarboxylates, fluoroalkylpolyoxyethyleneethers, fluoroalkylsulfonates, fluoroalkyltrimethylammonium salts, and fluoroalkylaminosulfonates are preferred.

[0075] The content of the surfactant in the composition for low dielectric members of the present invention is preferably 0.005 to 1% by weight based on the total amount of the composition for low dielectric members.

[0076] 2-3-3. Adhesion improver The composition for low dielectric members of the present invention may further contain an adhesion improver such as a silane-based, aluminum-based or titanate-based coupling agent from the viewpoint of further improving the adhesion between the formed cured film and the substrate.

[0077] Examples of adhesion improvers include silane-based coupling agents such as 3-glycidyloxypropyldimethylethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane; aluminum-based coupling agents such as acetoalkoxyaluminum diisopropylate; and titanate-based coupling agents such as tetraisopropylbis(dioctylphosphite)titanate.

[0078] Of these, 3-glycidyloxypropyltrimethoxysilane is preferred.

[0079] The content of the adhesion improver is preferably 0.01 to 10% by weight based on the total amount of the composition for low dielectric members.

[0080] 2-3-4. Antioxidants The composition for low dielectric members of the present invention may further contain an antioxidant such as a phenol-based antioxidant, a phosphorus-based antioxidant, a sulfur-based antioxidant, an amine-based antioxidant, etc., from the viewpoint of improving transparency and preventing yellowing when the cured film is exposed to high temperatures. Among these, a phenol-based antioxidant is preferred from the viewpoint of stability.

[0081] Specific examples of phenol-based antioxidants include tert-butylhydroquinone, butylated hydroxytoluene (BHT: 2,6-di-tert-butyl-p-cresol), ANTAGE SP (trade name; manufactured by Kawaguchi Chemical Industry Co., Ltd.), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl]propionate, )propanamide], ethylene bis(oxyethylene)-bis(3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octyl-3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 4,6-bis(dodecyl 4,6-bis(octylthiomethyl)-o-cresol, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4,4'-butylidenebis(6-tert-butyl-3-methylphenol), 2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl acrylate, 1,3,5-tris[[4-(1,1-dimethylethyl)-3-hydroxy-2,6-di methylphenyl]methyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 4-[[4,6-bis(octylthio)-1,3,5-triazin-2-yl]amino]-2,6-di-tert-butylphenol, and 2,2'-dimethyl-2,2'-(2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diyl)dipropane-1,1'-diyl=bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propanoate].

[0082] Among these, from the viewpoint of thermal stability, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] are more preferable. From the viewpoint of solubility, butylated hydroxytoluene (BHT: 2,6-di-tert-butyl-p-cresol) and octyl-3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid are more preferable.

[0083] The content of the antioxidant is preferably from 0.01 to 5.0 parts by weight, and more preferably from 0.05 to 2.0 parts by weight, based on 100 parts by weight of the polyamic acid (A).

[0084] 2-3-5. Inorganic fillers The composition for low dielectric members of the present invention may further contain an inorganic filler from the viewpoints of improving thermal conductivity, improving mechanical strength, adjusting viscosity, and the like. In order to suppress dielectric loss, the silica may be a silicon compound such as spherical silica, pulverized silica, hollow silica, or fumed silica, a metal oxide such as magnesium oxide, zinc oxide, or titanium oxide, or a metal salt such as potassium titanate. Of these, spherical silica, hollow silica, magnesium oxide, and potassium titanate are preferred, and hollow silica is more preferred. A fibrous or whisker-like inorganic filler can be used as a fibrous reinforcing agent to increase the strength of a substrate or a resin part. Preferred are glass cloth, low dielectric glass cloth, inorganic fibers such as carbon fiber and carbon nanotubes, and inorganic whiskers such as silicate whiskers, magnesium oxide whiskers and zinc oxide whiskers, and more preferred is low dielectric glass cloth. In order to increase the mechanical strength, it is preferable to use a large amount of inorganic filler, but if it is too much, the resin such as polyamic acid (A) may not be able to fill the gaps of the inorganic filler. Also, if there is too much resin, the effect of increasing the mechanical strength may not be achieved. In addition, since increasing the inorganic filler tends to increase the dielectric constant and decrease the dielectric tangent, it is preferable to determine the composition while balancing the two. In addition to inorganic fibers, organic fibers can also be used. Examples of organic fibers with high mechanical strength include polyamide fibers, aramid fibers, polyparaphenylene benzobisoxazole fibers, and liquid crystalline polyester fibers. They are lighter than inorganic fibers and are preferable for substrates of portable devices. Inorganic fillers with high thermal conductivity may be nitride fillers made of powdered boron nitride, silicon nitride, and other metal nitrides, carbides such as diamond, graphite, and silicon carbide, metal oxides such as magnesium oxide, zinc oxide, silicon oxide, titanium oxide, tin oxide, holmium oxide, and calcium oxide, metal hydroxides such as magnesium hydroxide and aluminum hydroxide, and silicate compounds such as cordierite and mullite. Boron nitride and silicon oxide, which have low dielectric constants, are preferred, and hexagonal boron nitride (h-BN) is particularly preferred because it has a low dielectric constant and high thermal conductivity. The more inorganic fillers there are, the higher the thermal conductivity, etc., but inorganic fillers generally have a high relative dielectric constant and a low dielectric tangent compared to resin components, so increasing the filling amount increases the dielectric constant. Therefore, it is preferable to fill the required amount within a range that does not exceed the desired dielectric constant. The composition for low dielectric members of the present invention has high transparency and is not only low dielectric, but also has a low refractive index. When the composition is used for an optical material, the refractive index can be adjusted by adding powder of hollow silica, spherical silica, titanium oxide, zirconium oxide, or the like.

[0085] The shape of the inorganic filler may be spherical, amorphous, fibrous, whisker-like, cylindrical, plate-like, etc. The type, shape, size, content, etc. of the inorganic filler may be appropriately selected depending on the purpose. When the polymer molded product such as the cured film obtained from the composition for low dielectric members of the present invention requires insulation, the inorganic filler may be conductive as long as the desired insulation, mechanical strength, dielectric constant, and dielectric loss are maintained.

[0086] The average particle size of the spherical or irregular inorganic filler is preferably 0.1 to 200 μm. More preferably, it is 1 to 100 μm. If it is 0.1 μm or more, the thermal conductivity is good, and if it is 200 μm or less, the filling rate can be increased. As for the fibrous inorganic filler, the tensile strength improves as the fiber length increases, but kneading or dispersion may not be possible, so it is preferable to select the fiber length depending on the application. When dispersed, the average particle size of the fibrous inorganic filler is preferably 0.01 to 200 μm. More preferably, it is 0.1 to 100 μm. If it is 0.01 μm or more, the thermal conductivity is good, and if it is 200 μm or less, the mechanical strength can be increased. The content of the inorganic filler in the polymer molded product after curing is preferably 20 to 95% by weight, and more preferably 50 to 95% by weight. If it is 20% by weight or more, the thermal conductivity becomes high, which is preferable. If it is 95% by weight or less, the polymer molded product does not become brittle, which is preferable.

[0087] As the inorganic filler, commercially available products that have been surface-treated, such as affinity-treated, easily-adhesive-treated, dispersing-treated, or waterproof-treated, may be used as they are, or the commercially available products from which the surface treatment agents have been removed may be used. Also, untreated inorganic fillers may be used after being treated with a silane coupling agent, affinity agent, surface tension adjuster, anti-settling agent, anti-aggregation agent, etc.

[0088] 2-4. Preparation of composition for low dielectric components The composition for low dielectric members of the present invention can be obtained by adding, to the polyamic acid (A) and, as necessary, selectively adding additives (D) such as a solvent (B2), a curing agent (C), a compound having a polymerizable double bond, a surfactant, an adhesion improver, an antioxidant, an inorganic filler, and other additives, and mixing or dissolving them uniformly.

[0089] 2-5. Storage of low dielectric material composition The composition for low dielectric members of the present invention is preferably stored at a temperature in the range of -30°C to 25°C, since the composition has good stability over time. Storage at a temperature in the range of -20°C to 10°C is more preferable.

[0090] 3. Low dielectric components and electronic devices made of cured films obtained from the composition for low dielectric components The method of applying the composition for low dielectric members prepared as described above onto a substrate is not particularly limited, and examples thereof include a method using an applicator, a comma motor, a doctor blade, a dispenser, or a squeegee, a method using a rotating device such as a spin coater, and a printing method such as screen printing or inkjet printing. In order to coat uniformly, it is preferable to use a wet coating method. Among the wet coating methods, when preparing a small amount, a spin coating method that is easy and allows for homogeneous film formation is preferable. When productivity is important, a microgravure coating method, a gravure coating method, a dip coating method, a die coating method, a wire bar coating method, a bar coating method, a reverse coating method, a roll coating method, a slit coating method, a dipping method, a spray coating method, a meniscus coating method, a kiss coating method, a reverse kiss coating method, an air knife coating method, a curtain coating method, a flow coating method, a printing method, an inkjet method, a flexographic printing method, a screen printing method, a rod coating method, and the like are preferable. The wet coating method can be appropriately selected from these methods depending on the required film thickness, viscosity, curing conditions, etc.

[0091] When producing a sheet, a cast molding method is used in which a low dielectric material composition solution is used to coat a substrate that has been subjected to a release treatment using the composition solution by the above-mentioned method or the like, and then peeled off. When producing a structure, a mixture of raw material powders or a resin that has been prepolymerized by reacting some polymerizable groups in advance can be used with a mold as necessary, and resin molding methods such as press molding, injection molding, and various 3D printer molding methods (ejection lamination methods) can be used. After molding, the mold can be removed and the mold can be fully cured, or the mold can be fully cured while still in the mold, or in the case of a molding method that does not use a mold, the molded body can be fully cured as is.

[0092] The pre-baking conditions vary depending on the types and mixing ratios of the components used in preparing the low dielectric material composition, but are usually performed in two stages of 1-60 minutes on a hot plate or in an oven at 60-100° C. and 5-90 minutes on a hot plate or in an oven at 120-180° C. to evaporate the solvent and dry the composition. The main curing (main baking) conditions vary depending on the types and mixing ratios of the components, but are usually performed in an oven at 180-400° C. for 5-240 minutes.

[0093] When the composition for low dielectric members contains a curing agent (C), a crosslinking reaction occurs between the carboxyl group of the polyamic acid and the epoxy or oxazoline functional group of the curing agent (C) in the main curing (baking) process, and the resulting cured film is very tough.

[0094] A low dielectric member made of the cured film of the present invention has excellent properties such as low dielectric tangent and high heat resistance, since the dielectric tangent at high frequencies (10 GHz and 28 GHz) is preferably lower than 0.01 and the 5% weight loss temperature is preferably 450° C. or higher. Using this low dielectric member made of the cured film, electronic devices such as electronic circuits, sensors, antennas, and radars, or electronic devices using these low dielectric members and electronic devices can be manufactured. EXAMPLES

[0095] The present invention will now be described in detail with reference to Synthesis Examples, Preparation Examples, Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0096] For the abbreviations used in the Synthesis Examples, Preparation Examples, Examples, and Comparative Examples, the corresponding compound names, trade names, etc. are listed below. <Solvent> NMP: 1-methyl-2-pyrrolidone EDM: Diethylene glycol ethyl methyl ether KJCMPA: 3-butoxy-N,N-dimethylpropanamide (KJCMPA (registered trademark)-100; product name; manufactured by KJ Chemicals Co., Ltd.) <Tetracarboxylic acid dianhydride> BT-100: 1,2,3,4-butanetetracarboxylic dianhydride (Rikacid BT-100; product name; manufactured by New Japan Chemical Co., Ltd.) PMDA: Pyromellitic anhydride CBDA: Cyclobutane-1,2,3,4-tetracarboxylic dianhydride <Diamine> BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane DDE: 4,4'-diaminodiphenyl ether TFMB: 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl XQ1251: A compound represented by formula (2-2) (XQ1251; trade name; manufactured by JNC Corporation) TIFF2024134741000016.tif4185<end capping agent> MA: Maleic anhydride <Hardening agent> 1,3-PBO: 2,2'-(1,3-phenylene)-bis(2-oxazoline) <Additives> F-477: Megafac F-477 (product name; manufactured by DIC Corporation)

[0097] The abbreviations for the measurement items in the examples are shown below. Mw: Weight average molecular weight Mn: Number average molecular weight

[0098] Next, the measuring apparatus and analysis conditions used in the examples are shown below. <gpc> Equipment: Waters 2695 Separation Module / 2414 Differential Refractometer Solvent: Phosphoric acid-DMF mixed solution (phosphoric acid / DMF=0.6 / 100 weight ratio) Flow rate: 0.40mL / min Column temperature: 50℃ Column used: Waters HSPgel RT MB-M Standard sample for calibration curve: TSK standard polystyrene manufactured by Tosoh Corporation <Dielectric tangent measurement> Equipment: AET, INC. Cavity resonator TE mode 10 GHz, 28 GHz and Anritsu Corporation Vector network analyzer MS46522B-043 <Pyrolysis temperature measurement> Equipment: Rigaku Corporation TG-DTA8120 / S Atmosphere: Nitrogen Temperature rise conditions: 40℃→800℃, 10℃ / min

[0099] [Synthesis of polyamic acid] [Synthesis Example 1] Synthesis of polyamic acid (A1) In a 300mL four-necked separable flask equipped with a thermometer, a stirrer, and a nitrogen inlet tube, XQ1251 (5.00g; 3.74mmol) and DDE (6.75g; 33.70mmol) were added as diamines, and dehydrated NMP (112.40g) was added as a reaction solvent (B1). After the solids were completely dissolved, the reaction system was placed under a nitrogen atmosphere, the temperature inside the reaction system was lowered to below 0°C, and PMDA (7.35g; 33.70mmol) and CBDA (0.73g; 3.74mmol) were further added as tetracarboxylic dianhydrides. After stirring for 16 hours, a uniform and transparent polyamic acid (A1) solution with a solid content of 15.0% by weight was obtained. The Mw of the polyamic acid (A1) was 107,500, and the Mn was 43,800.

[0100] [Synthesis Example 2] Synthesis of polyamic acid (A2) Except for changing DDE to BAPP (13.83 g; 33.70 mmol) as the diamine and changing the amount of dehydrated NMP to 152.56 g, the reaction was carried out in the same manner as in Synthesis Example 1, and a uniform and transparent polyamic acid (A2) solution with a solid content of 15.0 wt % was obtained. The Mw of the polyamic acid (A2) was 113,200 and the Mn was 48,000.

[0101] [Synthesis Example 3] Synthesis of polyamic acid (A3) Except for changing the diamine from DDE to TFMB (10.79 g; 33.70 mmol) and changing the amount of dehydrated NMP to 135.32 g, the reaction was carried out in the same manner as in Synthesis Example 1, and a uniform and transparent polyamic acid (A3) solution with a solid content of 15.0 wt % was obtained. The Mw of the polyamic acid (A3) was 126,300 and the Mn was 58,300.

[0102] [Synthesis Example 4] Synthesis of polyamic acid (A4) Except for changing DDE to m-TB (7.15 g; 33.70 mmol) as the diamine and changing the amount of dehydrated NMP to 114.70 g, the reaction was carried out in the same manner as in Synthesis Example 1, and a uniform and transparent polyamic acid (A4) solution with a solid content of 15.0 wt % was obtained. The Mw of the polyamic acid (A4) was 106,300 and the Mn was 46,500.

[0103] [Synthesis Example 5] Synthesis of polyamic acid (A5) Except for changing the amount of tetracarboxylic dianhydride CBDA to BT-100 (0.74 g; 3.74 mmol) and changing the amount of dehydrated NMP to 112.44 g, the reaction was carried out in the same manner as in Synthesis Example 1, and then a uniform and transparent polyamic acid (A5) solution with a solid content concentration of 15.0 wt % was obtained. The Mw of the polyamic acid (A5) was 105,400 and the Mn was 41,300.

[0104] [Synthesis Example 6] Synthesis of polyamic acid (A6) Except for changing the amount of tetracarboxylic dianhydride CBDA to BT-100 (0.74 g; 3.74 mmol) and changing the amount of dehydrated NMP to 152.60 g, the reaction was carried out in the same manner as in Synthesis Example 2, and a uniform and transparent polyamic acid (A6) solution with a solid content concentration of 15.0 wt % was obtained. The Mw of the polyamic acid (A6) was 99,400 and the Mn was 32,100.

[0105] [Synthesis Example 7] Synthesis of polyamic acid (A7) Except for changing the tetracarboxylic dianhydride CBDA to BT-100 (0.74 g; 3.74 mmol) and changing the amount of dehydrated NMP to 135.36 g, the reaction was carried out in the same manner as in Synthesis Example 3, and then a uniform and transparent polyamic acid (A7) solution with a solid content concentration of 15.0 wt % was obtained. The Mw of the polyamic acid (A7) was 89,400 and the Mn was 30,400.

[0106] [Synthesis Example 8] Synthesis of polyamic acid (A8) Except for changing the tetracarboxylic dianhydride CBDA to BT-100 (0.74 g; 3.74 mmol) and changing the amount of dehydrated NMP to 114.75 g, the reaction was carried out in the same manner as in Synthesis Example 4, and then a uniform and transparent polyamic acid (A8) solution with a solid content concentration of 15.0 wt % was obtained. The Mw of the polyamic acid (A8) was 93,500 and the Mn was 38,600.

[0107] [Synthesis Example 9] Synthesis of polyamic acid (A9) In a 300mL four-necked separable flask equipped with a thermometer, a stirrer, and a nitrogen inlet tube, XQ1251 (5.00g; 3.74mmol) and DDE (6.20g; 30.94mmol) were added as diamines, and dehydrated NMP (105.78g) was added as a reaction solvent (B1). After the solids were completely dissolved, the reaction system was placed under a nitrogen atmosphere, the temperature in the reaction system was lowered to below 0°C, and PMDA (6.67g; 30.60mmol) and CBDA (0.67g; 3.40mmol) were further added as tetracarboxylic dianhydrides, and the mixture was stirred for 16 hours. MA (0.13g; 1.36mmol) was added as a terminal blocking agent at room temperature, and the mixture was stirred and reacted for another 3 hours, resulting in a uniform, transparent polyamic acid (A9) solution with a solid content of 15.0% by weight. The polyamic acid (A9) had an Mw of 75,000 and an Mn of 26,700.

[0108] [Synthesis Example 10] Synthesis of polyamic acid (A10) Except for changing DDE to BAPP (12.70 g; 30.94 mmol) as the diamine and changing the amount of dehydrated NMP to 142.64 g, the reaction was carried out in the same manner as in Synthesis Example 9, and a uniform and transparent polyamic acid (A10) solution with a solid content of 15.0 wt % was obtained. The Mw of the polyamic acid (A10) was 66,300 and the Mn was 23,800.

[0109] [Synthesis Example 11] Synthesis of polyamic acid (A11) Except for changing DDE to TFMB (9.91 g; 30.94 mmol) as the diamine and changing the amount of dehydrated NMP to 126.82 g, the reaction was carried out in the same manner as in Synthesis Example 9, and a uniform and transparent polyamic acid (A11) solution with a solid content of 15.0 wt % was obtained. The Mw of the polyamic acid (A11) was 54,500 and the Mn was 20,100.

[0110] [Synthesis Example 12] Synthesis of polyamic acid (A12) Except for changing DDE to m-TB (6.57 g; 30.94 mmol) as the diamine and changing the amount of dehydrated NMP to 107.89 g, the reaction was carried out in the same manner as in Synthesis Example 9, and a uniform and transparent polyamic acid (A12) solution with a solid content of 15.0 wt % was obtained. The Mw of the polyamic acid (A12) was 60,500 and the Mn was 23,800.

[0111] [Synthesis Example 13] Synthesis of polyamic acid (A13) The amount of XQ1251 as diamine was changed to 10.00g; 7.48mmol, the amount of DDE was changed to 5.99g; 29.93mmol, the amount of PMDA as tetracarboxylic dianhydride was changed to 7.34g; 33.67mmol, and the amount of dehydrated NMP was changed to 136.38g. The reaction was carried out in the same manner as in Synthesis Example 1, and a uniform and transparent polyamic acid (A13) solution with a solid content concentration of 15.0% by weight was obtained. The Mw of the polyamic acid (A13) was 82,400 and the Mn was 33,800.

[0112] [Synthesis Example 14] Synthesis of polyamic acid (A14) The amount of XQ1251 as diamine was changed to 15.00g; 11.23mmol, the amount of DDE was changed to 2.25g; 11.23mmol, the amount of PMDA as tetracarboxylic dianhydride was changed to 4.41g; 20.21mmol, the amount of CBDA was changed to 0.44g; 2.25mmol, and the amount of dehydrated NMP was changed to 138.60g. After reacting in the same manner as in Synthesis Example 1, a uniform and transparent polyamic acid (A14) solution with a solid content concentration of 15.0% by weight was obtained. The Mw of the polyamic acid (A14) was 90,300, and the Mn was 39,600.

[0113] [Synthesis Example 15] Synthesis of polyamic acid (A15) The amount of XQ1251 as diamine was changed to 20.00g; 14.97mmol, and the amount of DDE was changed to 0g; 0mmol, i.e., DDE was not used, the amount of PMDA as tetracarboxylic dianhydride was changed to 2.94g; 13.47mmol, the amount of CBDA was changed to 0.29g; 1.50mmol, and the amount of dehydrated NMP was changed to 131.62g, respectively. After the reaction was carried out in the same manner as in Synthesis Example 1, a uniform and transparent polyamic acid (A15) solution with a solid content concentration of 15.0% by weight was obtained. The Mw of the polyamic acid (A15) was 84,300, and the Mn was 34,500.

[0114] [Comparative Synthesis Example 1] Synthesis of polyamic acid (A16) In a 300mL four-necked separable flask equipped with a thermometer, a stirrer, and a nitrogen inlet tube, DDE (11.01g; 55.00mmol) as a diamine and dehydrated NMP (130.39g) as a reaction solvent (B1) were added, and after the solids were completely dissolved, the reaction system was placed under a nitrogen atmosphere, the temperature inside the reaction system was lowered to below 0°C, PMDA (12.00g; 55.00mmol) was further added as a tetracarboxylic dianhydride, and after stirring for 16 hours, a uniform and transparent polyamic acid (A16) solution with a solid content concentration of 15.0% by weight was obtained. The Mw of the polyamic acid (A16) was 168,300 and the Mn was 84,900.

[0115] [Comparative Synthesis Example 2] Synthesis of polyamic acid (A17) Except for changing DDE to BAPP (15.05 g; 36.66 mmol) as diamine, the amount of PMDA as tetracarboxylic dianhydride to 8.00 g; 36.66 mmol, and the amount of dehydrated NMP to 130.59 g, the reaction was carried out in the same manner as in Comparative Synthesis Example 1, and a uniform, transparent polyamic acid (A17) solution with a solid content concentration of 15.0 wt % was obtained. The Mw of the polyamic acid (A17) was 184,800, and the Mn was 97,600.

[0116] [Comparative Synthesis Example 3] Synthesis of polyamic acid (A18) Except for changing DDE to TFMB (14.69 g; 45.86 mmol) as diamine, the amount of PMDA as tetracarboxylic dianhydride to 10.00 g; 45.86 mmol, and the amount of dehydrated NMP to 139.90 g, the reaction was carried out in the same manner as in Comparative Synthesis Example 1, and a uniform, transparent polyamic acid (A18) solution with a solid content concentration of 15.0 wt % was obtained. The Mw of the polyamic acid (A18) was 124,500, and the Mn was 51,000.

[0117] [Comparative Synthesis Example 4] Synthesis of polyamic acid (A19) Except for changing DDE to m-TB (11.68 g; 55.00 mmol) as diamine, the amount of PMDA to 12.00 g; 55.00 mmol as tetracarboxylic dianhydride, and the amount of dehydrated NMP to 134.14 g, the reaction was carried out in the same manner as in Comparative Synthesis Example 1, and a uniform, transparent polyamic acid (A19) solution with a solid content concentration of 15.0 wt % was obtained. The Mw of the polyamic acid (A19) was 162,200 and the Mn was 43,700.

[0118] Tables 1-1 to 1-5 show the tetracarboxylic dianhydrides, diamines, end-capping agents, reaction solvents (B1) used, and the resulting polyamic acids and their molecular weights used in the respective syntheses. In Tables 1-1 to 1-5, the numbers in square brackets represent molar ratios. That is, the total amount of diamines and the total amount of end-capping agents each represent molar parts relative to 100 molar parts of the total amount of tetracarboxylic dianhydrides.

[0119] Table 1-1 TIFF2024134741000017.tif66168

[0120] Table 1-2 TIFF2024134741000018.tif66168

[0121] Table 1-3 TIFF2024134741000019.tif71168

[0122] Table 1-4 TIFF2024134741000020.tif74155

[0123] Table 1-5 TIFF2024134741000021.tif54168

[0124] [Preparation of composition for low dielectric members] [Preparation Example 1] Polyamic acid (A1) solution (10.0000 g), F-477 (0.0015 g), and KJCPMA (5.0000 g) were mixed and dissolved to obtain composition 1.

[0125] [Preparation Example 2] Composition 2 was obtained in the same manner as in Preparation Example 1, except that the polyamic acid (A1) solution was changed to a polyamic acid (A2) solution.

[0126] [Preparation Example 3] Composition 3 was obtained in the same manner as in Preparation Example 1, except that the polyamic acid (A1) solution was changed to a polyamic acid (A3) solution.

[0127] [Preparation Example 4] Composition 4 was obtained in the same manner as in Preparation Example 1, except that the polyamic acid (A1) solution was changed to a polyamic acid (A4) solution.

[0128] [Preparation Example 5] Polyamic acid (A5) solution (10.0000 g), 1,3-PBO (0.0300 g), F-477 (0.0015 g), and EDM (5.0000 g) were mixed and dissolved to obtain composition 5.

[0129] [Preparation Example 6] Composition 6 was obtained in the same manner as in Preparation Example 5, except that the polyamic acid (A5) solution was changed to the polyamic acid (A6) solution.

[0130] [Preparation Example 7] Composition 7 was obtained in the same manner as in Preparation Example 5, except that the polyamic acid (A5) solution was changed to the polyamic acid (A7) solution.

[0131] [Preparation Example 8] Composition 8 was obtained in the same manner as in Preparation Example 5, except that the polyamic acid (A5) solution was changed to a polyamic acid (A8) solution.

[0132] [Preparation Example 9] Polyamic acid (A9) solution (10.0000 g), F-477 (0.0015 g), and dehydrated NMP (5.0000 g) were mixed and dissolved to obtain composition 9.

[0133] [Preparation Example 10] Composition 10 was obtained in the same manner as in Preparation Example 9, except that the polyamic acid (A9) solution was changed to a polyamic acid (A10) solution.

[0134] [Preparation Example 11] Composition 11 was obtained in the same manner as in Preparation Example 9, except that the polyamic acid (A9) solution was changed to a polyamic acid (A11) solution.

[0135] [Preparation Example 12] Composition 12 was obtained in the same manner as in Preparation Example 9, except that the polyamic acid (A9) solution was changed to a polyamic acid (A12) solution.

[0136] [Preparation Example 13] Polyamic acid (A13) solution (10.0000 g), F-477 (0.0015 g), and dehydrated NMP (5.0000 g) were mixed and dissolved to obtain composition 13.

[0137] [Preparation Example 14] Composition 14 was obtained in the same manner as in Preparation Example 13, except that the polyamic acid (A13) solution was changed to a polyamic acid (A14) solution.

[0138] [Preparation Example 15] Composition 15 was obtained in the same manner as in Preparation Example 13, except that the polyamic acid (A13) solution was changed to a polyamic acid (A15) solution.

[0139] [Comparative Preparation Example 1] Polyamic acid (A16) solution (10.0000 g), F-477 (0.0015 g), and dehydrated NMP (5.0000 g) were mixed and dissolved to obtain composition 16.

[0140] [Comparative Preparation Example 2] Composition 17 was obtained in the same manner as in Comparative Preparation Example 1, except that the polyamic acid (A16) solution was changed to a polyamic acid (A17) solution.

[0141] [Comparative Preparation Example 3] Composition 18 was obtained in the same manner as in Comparative Preparation Example 1, except that the polyamic acid (A16) solution was changed to a polyamic acid (A18) solution.

[0142] [Comparative Preparation Example 4] Composition 19 was obtained in the same manner as in Comparative Preparation Example 1, except that the polyamic acid (A16) solution was changed to a polyamic acid (A19) solution.

[0143] [Example 1] to [Example 15], [Comparative Example 1] to [Comparative Example 4] The dielectric tangent and heat resistance of each of the compositions 1 to 19 obtained in the above Preparation Examples were evaluated as follows.

[0144] <Preparation of cured film for dielectric tangent evaluation> Each of compositions 1 to 19 was applied to a cleaned silicon substrate in a square of 10 cm x 10 cm or more using an applicator, the solvent was evaporated on a hot plate at 80°C for 30 minutes, and the substrate was heated in a 150°C oven for 15 minutes, after which the oven was heated to 350°C over an hour, and the substrate was further heated at 350°C for 30 minutes for main curing (main baking) to obtain a polyimide cured film with a thickness of 45 μm. The cured film was peeled off from the silicon substrate and used as a measurement sample for dielectric loss tangent evaluation. <Method of measuring dielectric tangent> In order to reduce the effect of moisture in the measurement sample, the measurement sample was left to stand for one day in an electronic desiccator with a relative humidity of 10% RH in advance. Evaluation of the dielectric loss tangent properties was started after the measurement sample was left to stand for 60 minutes or more in a laboratory with an air conditioner set to a temperature of 20°C. The resonant frequency shift and attenuation of the measurement sample were measured, and the dielectric loss tangent (Df) was calculated using software manufactured by AET, Inc. to obtain the dielectric loss tangent characteristics at 10 GHz and 28 GHz. The results are shown in Tables 2-1 to 2-5. <Heat resistance evaluation method> Heat resistance was evaluated using the 5% weight loss temperature. The measurement was performed using a TG-DTA TG-DTA8120 / S manufactured by Rigaku Corporation in a nitrogen atmosphere at a heating rate of 10°C / min, and the results are shown in Tables 2-1 to 2-5.

[0145] Table 2-1 TIFF2024134741000022.tif71169

[0146] Table 2-2 TIFF2024134741000023.tif77169

[0147] Table 2-3 TIFF2024134741000024.tif71169

[0148] Table 2-4 TIFF2024134741000025.tif75168

[0149] Table 2-5 TIFF2024134741000026.tif71169

[0150] Tables 2-1 to 2-5 show the polyamic acid (A) solution, additive (D), curing agent (C), and solvent (B2) used in the preparation of each of the compositions for low dielectric members, the resulting compositions for low dielectric members, and the low dielectric members formed of the cured films, as well as the evaluation results of their dielectric tangent and heat resistance. In Tables 2-1 to 2-5, the numbers for each component used in the preparation of the compositions for low dielectric members indicate the weight (unit: g). Compared with the dielectric loss tangents of the cured films of Comparative Examples 1 to 4 shown in Table 2-5, it was found that the cured films of Examples 1 to 15 obtained from the compositions of Tables 2-1 to 2-4, except for Example 5, exhibited excellent dielectric loss tangent properties, with the dielectric loss tangents at 10 GHz and 28 GHz both being lower than 0.01. [Industrial Applicability]

[0151] The polyamic acid having a cage-shaped silsesquioxane structure in the main chain of the present invention is obtained by reacting an aliphatic tetracarboxylic dianhydride with a compound having a cage-shaped silsesquioxane structure to which a diamine functional group (amino) has been added. Since the composition for low dielectric members of the present invention contains the polyamic acid having a cage-shaped silsesquioxane structure in the main chain, the low dielectric member made of the obtained cured film has a dielectric loss tangent at high frequencies (10 GHz and 28 GHz) preferably lower than 0.01, and therefore can be suitably used as an insulating member for electronic devices and electronic equipment that handle high frequencies of 10 GHz or higher.< / gpc>

Claims

1. Polyamic acid (A) is obtained by reacting raw materials containing a tetracarboxylic dianhydride and a diamine, in which the tetracarboxylic dianhydride contains an aliphatic tetracarboxylic dianhydride in an amount of 2 mol % or more, and the diamine contains a diamine having a cage-shaped silsesquioxane structure.

2. 2. The polyamic acid (A) according to claim 1, wherein the content of the diamine having a cage-shaped silsesquioxane structure in the diamine is 0.5 mol % or more.

3. The polyamic acid (A) according to claim 1, wherein the aliphatic tetracarboxylic dianhydride is at least one selected from the group consisting of tetracarboxylic dianhydrides represented by formulas (1-1) to (1-6): In formula (1-4), R 1 , R 2 , R 3 , and R 4 are independently hydrogen, methyl or fluorine. In formula (1-5) and formula (1-6), R is independently an alkyl having 1 to 45 carbon atoms, an aryl having 6 to 16 carbon atoms, or an arylalkyl having 7 to 16 carbon atoms; in the alkyl having 1 to 45 carbon atoms, at least one hydrogen may be replaced by fluorine; in the benzene ring in the aryl having 6 to 16 carbon atoms and the arylalkyl having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; in the alkylene in the arylalkyl having 7 to 16 carbon atoms, the number of carbon atoms is 1 to 10 and at least one -CH 2 - may be replaced by -O-; and R 5 is independently methyl or phenyl.

4. 2. The polyamic acid (A) according to claim 1, wherein the diamine having a cage-shaped silsesquioxane structure is a diamine represented by formula (2-1): In formula (2-1), X is independently an alkylene having 1 to 12 carbon atoms, an arylene having 6 to 16 carbon atoms, or an arylenealkylene having 7 to 16 carbon atoms; in this alkylene having 1 to 12 carbon atoms, at least one hydrogen may be replaced by fluorine, and in the benzene ring in the arylene having 6 to 16 carbon atoms and the arylenealkylene having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; R is independently an alkyl having 1 to 45 carbon atoms, an aryl having 6 to 16 carbon atoms, or an arylalkyl having 7 to 16 carbon atoms; in this alkyl having 1 to 45 carbon atoms, at least one hydrogen may be replaced by fluorine, and at least one -CH 2 In the benzene ring of the aryl having 6 to 16 carbon atoms and the arylalkyl having 7 to 16 carbon atoms, at least one hydrogen may be replaced by fluorine or an alkyl having 1 to 6 carbon atoms; in the alkylene of the arylalkyl having 7 to 16 carbon atoms, the number of carbon atoms is 1 to 10 and at least one -CH 2 - may be replaced by -O-; and R 5 is independently methyl or phenyl.

5. A composition for low dielectric members, comprising the polyamic acid (A) according to claim 1 .

6. 6. The composition for low dielectric members according to claim 5, wherein when the composition for low dielectric members is cured without adding an inorganic filler, the dielectric tangents of the cured product at 10 GHz and 28 GHz are both less than 0.

01.

7. The composition for a low dielectric member according to claim 5 , further comprising a curing agent (C).

8. The composition for low dielectric members according to any one of claims 5 to 7, further comprising at least one additive (D) selected from the group consisting of a compound having a polymerizable double bond, a surfactant, an adhesion improver, and an antioxidant.

9. A low dielectric member comprising a cured film obtained by curing the composition for low dielectric members according to claim 5.

10. The low dielectric member according to claim 9 ; An electronic device having at least one capability selected from the group consisting of capabilities to generate, convert, transmit, and process radio frequency signals; electronic equipment.

Citation Information

Patent Citations

  • Diamine having silsesquioxane skeleton and polymer using the same

    JP2005232024A

  • Polyimide, adhesive film, laminate, cover lay film, copper foil with resin, metal-clad laminate, circuit board, and multilayer circuit board

    JP2022101116A

  • Peripherally aromatic silsesquioxanes featuring reactive functionality: synthesis and application thereof

    US20150148497A1

  • Polymer production method, polymer film manufacturing method employing said method, and laminate manufacturing method

    WO2022118629A1

  • Poly(amic acid), polyimide, and uses thereof

    WO2023276887A1